Conductive Paste
The conductive paste with a polyvinyl acetal resin optimized for specific IR absorption and particle size addresses undissolved substance issues, enhancing filterability and printability to improve the quality and productivity of multilayer ceramic capacitors.
Patent Information
- Application Number
- JP2020556330
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-27
- Filing Date
- 2020-09-25
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2040-09-25
AI Technical Summary
Conventional polyvinyl acetal resins used in conductive pastes for multilayer ceramic capacitors generate undissolved substances during solvent dissolution, leading to voids and reduced dispersibility, which degrade electrical properties and hinder productivity in the manufacturing process.
A conductive paste containing a polyvinyl acetal resin with specific IR absorption spectrum characteristics and particle size distribution, optimized to minimize undissolved substances and enhance filterability, printability, and surface smoothness.
The optimized conductive paste reduces undissolved substances, improves filtration efficiency, ensures excellent printability, and achieves smooth surface finish, resulting in enhanced electrical properties and productivity of multilayer ceramic capacitors.
Smart Images

Figure 0007569217000006 
Figure 0007569217000007 
Figure 0007569217000008
Abstract
Description
[Technical field]
[0001] The present invention relates to a conductive paste which, when dissolved in an organic solvent, has a small amount of fine undissolved matter and is easy to filter, has excellent printability, and can exhibit excellent surface smoothness after printing. [Background technology]
[0002] 2. Description of the Related Art In recent years, electronic components mounted in various electronic devices have become smaller and more laminated, and laminated electronic components such as multilayer circuit boards, laminated coils, and laminated ceramic capacitors are widely used. Among them, multilayer ceramic capacitors are generally manufactured through the following steps. First, a plasticizer, a dispersant, etc. are added to a solution in which a binder resin such as polyvinyl butyral resin or poly(meth)acrylic acid ester resin is dissolved in an organic solvent, and then a ceramic raw material powder is added and mixed uniformly with a mixing device such as a bead mill or a ball mill to obtain a ceramic slurry composition having a certain viscosity after defoaming. This slurry composition is cast onto a support surface such as a release-treated polyethylene terephthalate film or a SUS plate using a doctor blade, reverse roll coater, etc., and the volatile matter such as the solvent is distilled off by heating, etc., and then peeled off from the support to obtain a ceramic green sheet. Next, a conductive paste that will become the internal electrodes is applied to the obtained ceramic green sheets by screen printing, and multiple sheets are alternately stacked and heated and pressed to produce a laminate. After that, a process to thermally decompose and remove the binder resin components and the like contained in the laminate, that is, a so-called degreasing process, is performed, and external electrodes are sintered onto the end faces of the ceramic sintered body obtained by firing to obtain a multilayer ceramic capacitor.
[0003] Polyvinyl acetal resins used in the preparation of conductive pastes are generally used as solutions dissolved in organic solvents such as alcohols, esters, ethers, hydrocarbons, and mixtures thereof. However, when conventional polyvinyl acetal resins are dissolved in organic solvents, a small amount of undissolved matter is generated. When such undissolved matter is present, when the resin is used in a conductive paste, voids tend to remain in the degreasing and firing processes, and the dispersibility of conductive powders and the like is reduced, resulting in reduced electrical properties of the resulting product. For this reason, when using polyvinyl acetal resin for multilayer ceramic capacitors, it was necessary to mix it with organic or inorganic compounds, dissolve it in an organic solvent, and then perform a filtration process to remove any undissolved materials.
[0004] In response to this, Patent Document 1 proposes a polyvinyl acetal resin in which a reduction rate of the filtration flow rate is less than 10% when a polyvinyl acetal resin solution, which is prepared by dissolving the polyvinyl acetal resin in a 1:1 mixed solvent of methyl ethyl ketone and / or toluene and ethanol to prepare a 5 wt % solution, is filtered using a filter with a mesh size of 5 μm under conditions of a filtration temperature of 25° C. and a filtration pressure of 10 mmHg. It is also proposed that the use of such a polyvinyl acetal resin results in less undissolved matter when dissolved in an organic solvent, and the filtration time can be shortened, thereby improving productivity. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2005-325342 A Summary of the Invention [Problem to be solved by the invention]
[0006] On the other hand, in recent years, with the increasing functionality and miniaturization of electronic devices, there is a demand for multilayer ceramic capacitors with larger capacitance and smaller size. In order to meet such demands, it is necessary to thoroughly remove finer undissolved matter, but even the polyvinyl acetal resin described in Patent Document 1 cannot thoroughly remove finer undissolved matter, and it is necessary to remove the undissolved matter by filtration or the like, which causes a problem of reduced productivity.
[0007] An object of the present invention is to provide a conductive paste which, when dissolved in an organic solvent, has a small amount of fine undissolved matter and is easy to filter, has excellent printability, and can exhibit excellent surface smoothness after printing. [Means for solving the problem]
[0008] The present invention relates to a conductive paste used for forming an electrode of a multilayer ceramic capacitor, the conductive paste comprising a polyvinyl acetal resin, an organic solvent, and a conductive powder, the polyvinyl acetal resin having an IR absorption spectrum measured by an infrared spectrophotometer having a wave number of 3100 to 3700 cm -1 The wave number A of the peak in the range of -1 ), and the amount of hydroxyl groups (mol %) satisfies the relationships of the following formulas (1) and (2). [(3470-A) / hydroxyl group content]≦5.0 (1) (3470-A)≦150 (2) A: Wave number 3100~3700cm -1 When the minimum transmittance of the peak in the range is X (%), the wavenumber that shows the transmittance a (%) that satisfies [100-(100-X) / 2] is 3470cm -1 Wavenumber on the lower wavenumber side The present invention will be described in detail below.
[0009] As a result of intensive research, the present inventors have found that a polyvinyl acetal resin having a specific relationship between the minimum transmittance and the wave number A of the peak showing the transmittance satisfying a predetermined relationship and a specific amount of hydroxyl groups has a small amount of undissolved matter when dissolved in an organic solvent, and can be used as a binder for a conductive paste for forming electrodes of a multilayer ceramic capacitor to improve productivity. Furthermore, the present inventors have found that high printability and coating strength can be obtained by using such a polyvinyl acetal resin as a binder resin for a conductive paste, and have completed the present invention.
[0010] The conductive paste of the present invention contains a polyvinyl acetal resin. An example of an IR absorption spectrum of the polyvinyl acetal resin according to the present invention measured by an infrared spectrophotometer at 20° C. is shown in Fig. 1. In Fig. 1, the vertical axis represents transmittance and the horizontal axis represents wave number. In the IR absorption spectrum shown in FIG. 1, the minimum transmittance X is 64.5%. The transmittance a that satisfies [100-(100-X) / 2] is 82.25%, and the transmittance a is 3470 cm -1 The wavenumber A of the peak showing transmittance a is 3325 cm -1 Furthermore, 3470cm -1 The wavenumber B of the peak showing transmittance a is 3555 cm -1 It is. In the above case, (3470-A) is 145(cm -1 For example, if the amount of hydroxyl groups is 30 mol%, [(3470-A) / amount of hydroxyl groups] is 4.83 (cm -1 / mol%). Also, (B-3470) is 85 (cm -1 ) and (3470-A) / (B-3470) is 1.70.
[0011] FIG. 2 shows another example of the IR absorption spectrum of the polyvinyl acetal resin according to the present invention measured at 20° C. using an infrared spectrophotometer. In the IR absorption spectrum shown in FIG. 2, the minimum transmittance X is 74%. The transmittance a that satisfies [100-(100-X) / 2] is 87%, and the transmittance a is 3470 cm -1 The wavenumber A of the peak showing transmittance a is 3390 cm -1 Furthermore, 3470cm -1 The wavenumber B of the peak showing transmittance a is 3570 cm -1 It is. In the above case, (3470-A) is 80(cm -1 For example, if the amount of hydroxyl groups is 22 mol%, [(3470-A) / amount of hydroxyl groups] is 3.64 (cm -1 / mol%). Also, (B-3470) is 100(cm -1 ) and (3470-A) / (B-3470) is 0.80. The IR absorption spectrum can be measured by a transmission method using a Fourier transform infrared spectrophotometer (such as HORIBA's "FT-720" or JASCO's "FT / IR-4000") at 20°C.
[0012] In the analysis of polyvinyl acetal resin using the above infrared spectrophotometer, the spectrum originating from the stretching vibration of the CH bond of polyvinyl acetal resin was observed at 2980 cm -1 The above peak analysis was carried out by first determining whether the minimum transmittance of the peak due to the stretching vibration of the C-H bond is 2500 cm -1 and 3050cm -1 The film thickness of the measurement sample is adjusted so that the film thickness is 20 to 30% of the baseline obtained by connecting the lines 100 and 1100 cm. Furthermore, the measurement results show that the wave number of 3100 to 3700 cm is -1 A baseline is drawn for peaks that appear within this range, and the data is corrected so that the transmittance at both ends of the peak is 100%.
[0013] In the above polyvinyl acetal resin, the wave number is 3100 to 3700 cm -1 The wave number A of the peak in the range of -1) and the amount of hydroxyl groups (mol %) satisfy the relationship of the following formula (1). [(3470-A) / hydroxyl group content]≦5.0 (1) By satisfying the above relationship, it is possible to reduce fine undissolved matter. The above [(3470-A) / hydroxyl group amount] is 4.5 cm -1 The lower limit is preferably 2.5 cm / mol % or less. -1 It is preferable that the content is 1 / mol % or more.
[0014] In the above polyvinyl acetal resin, the wave number is 3100 to 3700 cm -1 The wave number A of the peak in the range of -1 ) satisfies the relationship of the following formula (2). (3470-A)≦150 (2) The above wave number is 3470cm -1 and the wave number A (cm -1 ) (3470-A) is estimated to be larger as the number of associated OH groups increases. The more associated OH groups there are, the higher the polarity of that part becomes, making it less soluble in organic solvents. The above (3470-A) has a preferred upper limit of 120 cm -1 The lower limit of the difference is not particularly limited, and the smaller the difference, the more preferable. The preferred lower limit is 0 cm -1 It is.
[0015] The above minimum transmittance X (%) is derived from the amount of hydroxyl groups in the polyvinyl acetal resin, and since the amount of hydroxyl groups is preferably 16 to 25 mol % for reasons described later, the preferred lower limit is 53%, more preferably 58%, and the preferred upper limit is 85%, more preferably 83%.
[0016] It is estimated that the smaller the wave number B of the above peak, the more associated OH groups there are. If there are many associated OH groups, the polarity of that part becomes high and it becomes difficult to dissolve in an organic solvent. Therefore, the preferable lower limit is 3520 cm -1 , and a more preferable lower limit is 3540 cm -1The upper limit is not particularly limited, and the higher the better, but due to the principle of IR spectrum, the upper limit is 3800 cm -1 It is estimated that:
[0017] It is preferable that the wave number A of the peak and the wave number B of the peak satisfy the relationship of the following formula (3) so that the number of associated OH groups does not become too large. (3470-A) / (B-3470)≦1.4 (3) B: Wave number 3100~3700cm -1 When the minimum transmittance of the peak in the range is X (%), the wavenumber that shows the transmittance a (%) that satisfies [100-(100-X) / 2] is 3470cm -1 Wavenumber on the higher wavenumber side The lower limit of the above (3470-A) / (B-3470) is preferably 0.5, and the upper limit thereof is more preferably 1.1.
[0018] The wavenumber A of the peak and the wavenumber B of the peak can be adjusted by appropriately setting the crystallinity, degree of saponification, degree of polymerization of the raw material polyvinyl alcohol resin, acetalization reaction conditions such as reaction time and reaction temperature, and the amount of acetal groups, amount of hydroxyl groups, degree of crystallinity, Mw / Mn, etc. of the polyvinyl acetal resin.
[0019] The polyvinyl acetal resin is dissolved in dihydroterpenic acetate to a concentration of 0.2% by weight, and the particle size distribution of the polyvinyl acetal resin solution is measured using a particle counter. The ratio of particles having a diameter of 0.5 to 1.0 μm is 2.5 × 10 to 100% by volume of the resin solution. -8 The particle volume is determined by counting the number of particles having a diameter of 0.5 to 1.0 μm using a particle counter, calculating the volume of the particles having a diameter of 0.5 to 1.0 μm assuming that the particles have a diameter of 0.75 μm and are true spheres, and then calculating the proportion (volume %) of particles having a diameter of 0.5 to 1.0 μm based on the number and volume of the particles. The above ratio is 2.5 x 10 -8When the content is 0.05 volume % or less, the filtration time can be shortened, the uniformity of the conductive paste is improved, a smoother coating film of the conductive paste can be produced, and sheet defects such as cracks are less likely to occur, making dielectric breakdown less likely to occur, which is advantageous in that the reliability of the resulting multilayer ceramic capacitor is improved. The above ratio is 2.1 x 10 -8 The lower limit of the above ratio is not particularly limited, and the lower the ratio the better, with 0 volume % being preferred. As the particle counter, for example, "KS-42C" manufactured by Rion Co., Ltd. can be used.
[0020] The above-mentioned particles having a diameter of 0.5 to 1.0 μm are very fine, and therefore do not necessarily correspond to good or bad optical properties (for example, haze).
[0021] The volume ratio of the particles having a diameter of 0.5 to 1.0 μm can be adjusted by appropriately setting, for example, the crystallinity, degree of saponification, degree of polymerization of the raw material polyvinyl alcohol resin, conditions of the acetalization reaction, the amount of acetal groups, amount of hydroxyl groups, degree of crystallinity, Mw / Mn, etc. of the polyvinyl acetal resin.
[0022] From the viewpoint of ensuring both good printability and a viscosity suitable for printing, the average degree of polymerization of the above polyvinyl acetal resin is preferably 200 or more, and more preferably 250 or more, and is preferably 1900 or less, and more preferably 1750 or less. The average degree of polymerization can be measured in accordance with JIS K 6726.
[0023] The polyvinyl acetal resin preferably has a structural unit having an acetal group represented by the following formula (4), a structural unit having a hydroxyl group represented by the following formula (5), and a structural unit having an acetyl group represented by the following formula (6).
[0024] [ka]
[0025] In the above formula (4), R 1 represents a hydrogen atom or an alkyl group having 1 to 20 carbon atoms.
[0026] In the above formula (4), R 1 When is an alkyl group having 1 to 20 carbon atoms, examples of the alkyl group include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group, a sec-butyl group, a tert-butyl group, a pentyl group, a hexyl group, a heptyl group, a 2-ethylhexyl group, an octyl group, a nonyl group, a decyl group, an undecyl group, a dodecyl group, a tridecyl group, a tetradecyl group, a pentadecyl group, an octadecyl group, etc. Among these, a methyl group and an n-propyl group are preferable.
[0027] When the polyvinyl acetal resin contains an acetoacetal group, the amount of the acetoacetal group is preferably 27 mol % or less. When the amount of acetoacetal groups is 27 mol% or less, the effect of the steric hindrance of the polyvinyl acetal resin can be fully exhibited, and the polyvinyl acetal resin can have excellent cleaning properties. The amount of acetoacetal groups in the polyvinyl acetal resin is more preferably 22 mol% or less, and even more preferably 20 mol%. The acetoacetal group is an acetal group contained in the structural unit having an acetal group represented by the above formula (4), R 1 is a methyl group. In this specification, the amount of acetoacetal groups in a polyvinyl acetal resin means the apparent amount of acetoacetal groups in the entire polyvinyl acetal resin.
[0028] When the polyvinyl acetal resin contains butyral groups, the amount of butyral groups is preferably 40 mol % or more and 80 mol % or less. When the butyral content is 40 mol% or more, the amount of residual hydroxyl groups is in a suitable range, and the solubility of the polyvinyl acetal resin in a low polarity solvent can be sufficient.When the amount is 80 mol% or less, the amount of residual hydroxyl groups can be sufficient, and the viscosity of the obtained conductive paste can be made suitable, thereby improving the storage stability. The butyral group amount of the polyvinyl acetal resin is more preferably 50 mol % or more and more preferably 75 mol % or less. The butyral group is an acetal group contained in the structural unit having an acetal group represented by the above formula (4), R 1 is a propyl group. In this specification, the butyral group content of the polyvinyl acetal resin means the apparent butyral group content of the entire polyvinyl acetal resin.
[0029] In the polyvinyl acetal resin, the ratio of the amount of acetoacetal groups to the amount of butyral groups (amount of acetoacetal groups / amount of butyral groups) is preferably 0 or more, more preferably 0.05 or more, and is preferably 0.9 or less, more preferably 0.75 or less. When the ratio of the amount of acetoacetal groups to the amount of butyral groups is within the above range, the polyvinyl acetal resin can effectively exert steric hindrance, resulting in a paste with excellent cleaning properties.
[0030] The total amount of acetal groups in the polyvinyl acetal resin is preferably 60 mol % or more, more preferably 64 mol % or more, and is preferably 80 mol % or less, more preferably 76 mol % or less. In the polyvinyl acetal resin, the proportion of acetoacetal groups in all acetal groups is preferably 0 mol % in the lower limit and 35 mol % in the upper limit. The amount of acetal groups can be measured, for example, by NMR. Regarding the method for calculating the amount of acetal groups, since the acetal groups of polyvinyl acetal resin are obtained by acetalizing two hydroxyl groups of polyvinyl alcohol, the method of counting the two acetalized hydroxyl groups is used.
[0031] In the polyvinyl acetal resin, the content of the structural unit having a hydroxyl group represented by general formula (5) (hereinafter also referred to as "hydroxyl group amount") is preferably 16 mol % in lower limit and 25 mol % in upper limit. When the amount of hydroxyl groups is 16 mol % or more, aggregation of the conductive powder can be suppressed, and the dispersibility of the obtained conductive paste can be improved to form a smooth printed coating film. When the amount of hydroxyl groups is 25 mol % or less, the conductive paste can have excellent solubility in the low-polarity organic solvent used in the present invention. The lower limit of the hydroxyl group amount is more preferably 17 mol %, and the upper limit thereof is more preferably 23 mol %. The amount of hydroxyl groups can be measured, for example, by NMR.
[0032] In the polyvinyl acetal resin, the ratio of the content of structural units having a hydroxyl group with a chain length of 1 to the total amount of hydroxyl groups is preferably 45% at the lower limit, more preferably 50% at the lower limit, and preferably 75% at the upper limit, more preferably 70% at the upper limit. By setting it within the above range, the amount of undissolved matter can be reduced. The chain length of the structural unit having a hydroxyl group means the number of consecutive structural units having a hydroxyl group represented by the above formula (5). That is, a chain length of 1 means that the structural units having a hydroxyl group are not consecutive, and that a structural unit having a hydroxyl group is not adjacent to another structural unit having a hydroxyl group. The content ratio of the structural unit having a hydroxyl group and having a chain length of 1 is, for example, 13 It can be measured by C-NMR.
[0033] In the polyvinyl acetal resin, the content of the structural unit having an acetyl group represented by general formula (6) (hereinafter also referred to as "acetyl group amount") is preferably 0.1 mol % in lower limit and 12 mol % in upper limit. When the amount of acetyl groups is 0.1 mol% or more, the polyvinyl acetal resin obtained can obtain an appropriate steric hindrance in the resin, and can easily be wiped off or cleaned from working equipment, such as a three-roll mill used for kneading or a printing plate, or can easily change the paste, thereby improving the productivity of the coating film. When the amount of acetyl groups is 12 mol% or less, the resin can have excellent solubility in low polarity solvents, and can also be given appropriate flexibility to the coating film after drying, so that the coating film strength after drying can be excellent. The more preferred lower limit of the amount of acetyl groups in the polyvinyl acetal resin is 1 mol %, and the more preferred upper limit is 10 mol %. The amount of acetyl groups can be measured, for example, by NMR.
[0034] In the polyvinyl acetal resin, the ratio of the amount of acetyl groups to the amount of butyral groups (amount of acetyl groups / amount of butyral groups) preferably has a lower limit of 0.01, more preferably 0.02, and preferably has an upper limit of 0.35, more preferably 0.30.
[0035] The polyvinyl acetal resin preferably further contains a structural unit having a carboxyl group. By containing the above-mentioned structural unit having a carboxyl group, the compound can be dissolved in an organic solvent of low polarity and can improve compatibility with the conductive powder, which is one of the constituent materials of the conductive paste, thereby improving printability.
[0036] Examples of the structural unit containing a carboxyl group include a structural unit represented by the following formula (7-1) and a structural unit represented by the following formula (7-2).
[0037] [ka]
[0038] In the above formula (7-1), R 2 and R 3 each independently represents an alkylene group having 0 to 10 carbon atoms; X 1 and X 2 Each independently represents a hydrogen atom, a metal atom, or a methyl group. 4 , R 5 and R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R 7 is an alkylene group having 0 to 10 carbon atoms, X 3 represents a hydrogen atom, a metal atom, or a methyl group. 2 , R 3 or R 7 is an alkylene group having 0 carbon atoms, R 2 , R 3 or R 7 means that the group is a single bond.
[0039] The polyvinyl acetal resin preferably has a constitutional unit represented by the above formula (7-1). When the polyvinyl acetal resin has a structural unit represented by the above formula (7-1), the two carboxyl groups in the structural unit are located at positions sandwiching the carbon of the main chain, and therefore the obtained conductive paste has a moderate interaction with the conductive powder, and storage stability can be improved.
[0040] In the above formula (7-1), R 2 and R 3 each independently represents an alkylene group having 0 to 10 carbon atoms; X 1 and X 2 each independently represents a hydrogen atom, a metal atom, or a methyl group.
[0041] In the above formula (7-1), R 2 and R 3 When the alkylene group represented by the formula (I) has 0 to 10 carbon atoms, aggregation of the carboxyl groups can be suppressed, and the copolymer can have excellent solubility in low-polarity solvents. 2 and R3 The preferred lower limit for the number of carbon atoms in the alkylene group represented by the following formula (1) is 0, the preferred upper limit is 5, the more preferred lower limit is 1, and the more preferred upper limit is 3.
[0042] Above R 2 and R 3 may be the same or different, but are preferably different. Also, it is preferable that at least one of them is a single bond.
[0043] Examples of the alkylene group having 0 to 10 carbon atoms include linear alkylene groups such as a single bond, a methylene group, an ethylene group, a trimethylene group, a tetramethylene group, a pentamethylene group, a hexamethylene group, an octamethylene group, and a decamethylene group, branched alkylene groups such as a methylmethylene group, a methylethylene group, a 1-methylpentylene group, and a 1,4-dimethylbutylene group, and cyclic alkylene groups such as a cyclopropylene group, a cyclobutylene group, and a cyclohexylene group. Among these, linear alkylene groups such as a single bond, a methylene group, an ethylene group, an n-propylene group, and an n-butylene group are preferred, and a single bond, a methylene group, and an ethylene group are more preferred.
[0044] Above X 1 and X 2 When at least one of the groups is a metal atom, examples of the metal atom include a sodium atom, a lithium atom, a potassium atom, etc. Among these, a sodium atom is preferable.
[0045] The structural unit represented by the above formula (7-1) is preferably derived from an α-dicarboxy monomer. Examples of the α-dicarboxy monomer include dicarboxylic acids having a radical polymerizable unsaturated double bond, such as methylenemalonic acid, itaconic acid, 2-methyleneglutaric acid, 2-methyleneadipic acid, and 2-methylenesebacic acid, as well as metal salts and methyl esters thereof. Among these, itaconic acid, metal salts and methyl esters thereof are preferably used. In this specification, the term "α-dicarboxy monomer" refers to a monomer having two carboxyl groups at the α-carbon positions.
[0046] The polyvinyl acetal resin preferably has a constitutional unit represented by the above formula (7-2). When the polyvinyl acetal resin has a constitutional unit represented by the above formula (7-2), the solvent solubility can be made more excellent. In the above formula (7-2), R 4 , R 5 and R 6 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms; R 6 represents an alkylene group having 0 to 10 carbon atoms; X 3 represents a hydrogen atom, a metal atom or a methyl group.
[0047] In the above formula (7-2), R 4 , R 5 and R 6 When the alkyl group represented by the formula (I) has 1 to 10 carbon atoms, steric hindrance is unlikely to occur, and the polymerization reaction during the synthesis of the raw materials can proceed sufficiently. 4 , R 5 and R 6 The preferred lower limit for the number of carbon atoms in the alkyl group represented by the formula (I) is 1, the preferred upper limit is 5, and the more preferred upper limit is 3.
[0048] R 4 and R 5 may be the same or different, but is preferably the same. 4 , R 5 and R 6 is preferably a hydrogen atom.
[0049] Examples of the alkyl group having 1 to 10 carbon atoms include linear alkyl groups such as methyl, ethyl, propyl, n-butyl, n-pentyl, n-heptyl, n-octyl, n-nonyl, and n-decyl, branched alkyl groups such as isopropyl, isobutyl, sec-butyl, tert-butyl, isopentyl, 2,2-dimethylpropyl, 1,1,3,3-tetramethylbutyl, and 2-ethylhexyl, and cycloalkyl groups such as cyclopropyl, cyclopropylmethyl, cyclobutyl, cyclopentyl, and cyclohexyl. Of these, linear alkyl groups such as methyl, ethyl, propyl, and n-butyl are preferred, and methyl and ethyl are more preferred.
[0050] In the above formula (7-2), R 6 When the alkylene group represented by the formula (I) has 0 to 10 carbon atoms, aggregation of the carboxyl groups is unlikely to occur, and the solubility of the resulting resin in a low-polarity solvent can be made sufficient. 6 The preferred lower limit for the number of carbon atoms in the alkylene group represented by the following formula (1) is 0, the preferred upper limit is 5, the more preferred lower limit is 1, and the more preferred upper limit is 3.
[0051] R in the above formula (7-2) 7 As the R in the above formula (7-1), 2 and R 3 Among these, a single bond, and a linear alkylene group such as a methylene group, an ethylene group, a trimethylene group, or a tetramethylene group are preferred, a single bond, a methylene group, or an ethylene group is more preferred, and a single bond is even more preferred.
[0052] Above X 3 When is a metal atom, examples of the metal atom include a sodium atom, a lithium atom, a potassium atom, etc. Among these, a sodium atom is preferable.
[0053] The structural unit represented by the above formula (7-2) is preferably derived from a monocarboxy monomer. Examples of the monocarboxy monomer include monocarboxylic acids having a radical polymerizable unsaturated double bond such as acrylic acid, crotonic acid, methacrylic acid, and oleic acid, and metal salts or methyl esters thereof. Among them, crotonic acid, metal salts or methyl esters thereof are preferably used.
[0054] In the polyvinyl acetal resin, the content of structural units having a carboxyl group (hereinafter also referred to as "carboxyl group amount") is preferably such that the lower limit is 0.01 mol % and the upper limit is 1.0 mol %. When the amount of carboxyl groups is 0.01 mol% or more, the effect of the polyvinyl acetal resin having carboxyl groups can be fully exhibited, the printability of the conductive paste can be improved, the surface smoothness can be excellent, and the storage stability can be excellent. When the amount of carboxyl groups is 1 mol% or less, the solubility of the polyvinyl acetal resin in organic solvents can be improved. The lower limit of the amount of carboxyl groups in the polyvinyl acetal resin is preferably 0.07 mol%, the upper limit is preferably 0.8 mol%, the more preferable lower limit is 0.1 mol%, and the more preferable upper limit is 0.6 mol%. The amount of carboxyl groups can be measured, for example, by NMR.
[0055] In this specification, the amount of carboxyl groups in a polyvinyl acetal resin means the ratio of structural units having carboxyl groups to the total structural units of the polyvinyl acetal resin. For example, the structural unit represented by the above formula (7-1) has two carboxyl groups, but regardless of the number of carboxyl groups present in one structural unit, the ratio of structural units having carboxyl groups to the total structural units of the polyvinyl acetal resin is defined as the amount of carboxyl groups.
[0056] In the present specification, the carboxyl group amount of the polyvinyl acetal resin means the apparent carboxyl group amount of the entire polyvinyl acetal resin. That is, for example, when the polyvinyl acetal resin contains a plurality of resins having different carboxyl group amounts, the carboxyl group amount of the polyvinyl acetal resin is calculated by multiplying the carboxyl group amount of each resin by the content ratio of the resin, and then adding up the values obtained. In particular, for example, when the polyvinyl acetal resin contains a carboxylic acid-modified polyvinyl acetal resin and an unmodified polyvinyl acetal resin, the amount of carboxyl groups in the polyvinyl acetal resin is calculated by the following formula (8). E = F × (G / H) (8) In the above formula (8), E represents the content (mol%) of the structural unit having a carboxyl group in the polyvinyl acetal resin, F represents the content (mol%) of the structural unit having a carboxyl group in the polyvinyl acetal resin having a structural unit having a carboxyl group, G represents the weight of the polyvinyl acetal resin having a structural unit having a carboxyl group, and H represents the weight of the entire polyvinyl acetal resin.
[0057] In the polyvinyl acetal resin, the ratio of the amount of carboxyl groups to the amount of acetyl groups (amount of carboxyl groups / amount of acetyl groups) is preferably 0.01 in lower limit and 0.2 in upper limit. When the ratio of the amount of carboxyl groups to the amount of acetyl groups is in the above range, the polyvinyl acetal resin effectively generates steric hindrance, making it easy to clean. When the ratio of the amount of carboxyl groups to the amount of acetyl groups is 0.01 or more, the effect of steric hindrance can be fully exerted, and when it is 0.2 or less, the effect of the carboxyl groups can be fully exerted, improving printability. The more preferable lower limit of the ratio of the amount of acetyl groups to the amount of carboxyl groups in the polyvinyl acetal resin is 0.015, and the more preferable upper limit is 0.1.
[0058] The polyvinyl acetal resin preferably has an ethylene unit represented by the following formula (9).
[0059] [ka]
[0060] In the polyvinyl acetal resin, the lower limit of the content of the ethylene units (hereinafter also referred to as "ethylene content") is preferably 1 mol%, more preferably 3 mol%, and preferably 20 mol%, more preferably 10 mol%. The ethylene content can be measured, for example, by NMR.
[0061] In the present specification, the ethylene content of the polyvinyl acetal resin means the apparent ethylene content of the entire polyvinyl acetal resin. That is, for example, when the polyvinyl acetal resin contains a plurality of resins having different ethylene contents, the ethylene content of the polyvinyl acetal resin is calculated by multiplying the ethylene content of each resin by the content ratio of the resin, and then adding up the values obtained.
[0062] In the polyvinyl acetal resin, the ratio of the ethylene content to the hydroxyl group content (ethylene content / hydroxyl group content) is preferably 0.01 in the lower limit and 1.0 in the upper limit. When the ratio of the ethylene content to the hydroxyl group amount is within the above range, the polyvinyl acetal resin can have improved solvent solubility, making it possible to prepare a conductive paste with excellent printability. The ratio of the ethylene content to the hydroxyl group content of the polyvinyl acetal resin is more preferably 0.015 in the lower limit and 0.5 in the upper limit.
[0063] The polyvinyl acetal resin has a weight average molecular weight (Mw) of preferably 30,000 at its lower limit, more preferably 35,000 at its lower limit, and preferably 400,000 at its upper limit, more preferably 350,000 at its upper limit. The polyvinyl acetal resin has a number average molecular weight (Mn) of preferably 15,000 at its lower limit, more preferably 20,000 at its lower limit, and preferably 150,000 at its upper limit, more preferably 120,000 at its upper limit. The polyvinyl acetal resin has a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of preferably 2.0 lower limit, more preferably 2.2 lower limit, preferably 4.0 upper limit, more preferably 3.7 upper limit. The Mw and Mn can be measured, for example, by gel permeation chromatography (GPC) using an appropriate standard (e.g., polystyrene standard). Columns used for measuring the Mw and Mn include, for example, TSKgel SuperHZM-H.
[0064] The polyvinyl acetal resin can usually be produced by acetalizing polyvinyl alcohol.
[0065] As the polyvinyl alcohol resin, for example, a conventionally known polyvinyl alcohol resin such as a resin produced by saponifying a polyvinyl acetate resin with an alkali, an acid, aqueous ammonia or the like can be used. The polyvinyl alcohol resin may be fully saponified, but it does not need to be fully saponified as long as there is at least one unit having two consecutive hydroxyl groups at the meso and racemo positions at at least one position in the main chain, and may be a partially saponified polyvinyl alcohol resin. In addition, as the polyvinyl alcohol resin, a copolymer of vinyl alcohol and a monomer copolymerizable with vinyl alcohol, such as an ethylene-vinyl alcohol copolymer resin or a partially saponified ethylene-vinyl alcohol copolymer resin, may also be used. The polyvinyl acetate resin may be, for example, an ethylene-vinyl acetate copolymer.
[0066] The polyvinyl alcohol resin has a crystallinity of preferably 45% or less, more preferably 38% or less, even more preferably 37% or less, even more preferably 36% or less, and particularly preferably 33% or less. The lower limit is not particularly limited, but is preferably 3% or more. By using the above polyvinyl alcohol resin, the number of undissolved matters measured by the above method can be kept within a predetermined range. The crystallinity can be measured by differential scanning calorimetry (DSC) as described in the Examples below.
[0067] In this specification, the crystallinity of the polyvinyl alcohol resin means the apparent crystallinity of the entire polyvinyl alcohol resin. That is, for example, when the polyvinyl alcohol resin contains a plurality of resins having different crystallinity, the crystallinity of the polyvinyl alcohol resin is calculated by multiplying the crystallinity of each resin by the content ratio of the resin, and then adding up the values.
[0068] The polyvinyl alcohol resin preferably has a degree of saponification of 70 mol % or more and 99.4 mol % or less, and more preferably 78 mol % or more and 98 mol % or less. By using the above polyvinyl alcohol resin, the number of undissolved matters measured by the above method can be kept within a predetermined range.
[0069] The acetalization can be carried out by a known method, and is preferably carried out in a water solvent, in a mixed solvent of water and an organic solvent compatible with water, or in an organic solvent. As the organic solvent compatible with water, for example, an alcohol-based organic solvent can be used. Examples of the organic solvent include alcohol-based organic solvents, aromatic organic solvents, aliphatic ester-based solvents, ketone-based solvents, lower paraffin-based solvents, ether-based solvents, amide-based solvents, and amine-based solvents. Examples of the alcohol-based organic solvent include methanol, ethanol, n-propanol, isopropanol, n-butanol, and tert-butanol. Examples of the aromatic organic solvent include xylene, toluene, ethylbenzene, and methyl benzoate. Examples of the aliphatic ester solvent include methyl acetate, ethyl acetate, butyl acetate, methyl propionate, ethyl propionate, methyl butyrate, ethyl butyrate, methyl acetoacetate, and ethyl acetoacetate. Examples of the ketone solvent include acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, methylcyclohexanone, benzophenone, and acetophenone. Examples of the lower paraffin solvent include hexane, pentane, octane, cyclohexane, and decane. Examples of the ether solvent include diethyl ether, tetrahydrofuran, ethylene glycol dimethyl ether, ethylene glycol diethyl ether, and propylene glycol diethyl ether. Examples of the amide solvent include N,N-dimethylformamide, N,N-dimethylacetamide, N-methylpyrrolidone, and acetanilide. Examples of the amine solvent include ammonia, trimethylamine, triethylamine, n-butylamine, di-n-butylamine, tri-n-butylamine, aniline, N-methylaniline, N,N-dimethylaniline, and pyridine. These solvents may be used alone or in combination of two or more. Among these, ethanol, n-propanol, isopropanol, and tetrahydrofuran are particularly preferred from the viewpoints of solubility in the resin and ease of purification.
[0070] The acetalization is preferably carried out in the presence of an acid catalyst. The acid catalyst is not particularly limited, and examples thereof include mineral acids such as sulfuric acid, hydrochloric acid, nitric acid, and phosphoric acid, carboxylic acids such as formic acid, acetic acid, and propionic acid, and sulfonic acids such as methanesulfonic acid, ethanesulfonic acid, benzenesulfonic acid, and paratoluenesulfonic acid. These acid catalysts may be used alone or in combination of two or more compounds. Among them, hydrochloric acid, nitric acid, and sulfuric acid are preferred, and hydrochloric acid is particularly preferred.
[0071] In the method for producing a polyvinyl acetal resin of the present invention, it is preferable to start acetalization after stirring the polyvinyl alcohol resin at a temperature of 90° C. or higher for 2 hours or more. By setting the stirring time to 2 hours or more, the polyvinyl alcohol resin is sufficiently dissolved, the degree of acetalization is sufficiently high, and the generation of undissolved matter can be suppressed.
[0072] The aldehyde used in the acetalization reaction may be an aldehyde having a chain aliphatic group, a cyclic aliphatic group, or an aromatic group having 1 to 10 carbon atoms. Any known aldehyde may be used as the aldehyde. The aldehyde used in the acetalization reaction is not particularly limited, and may be, for example, an aliphatic aldehyde, an aromatic aldehyde, or the like. Examples of the aliphatic aldehyde include formaldehyde, acetaldehyde, propionaldehyde, n-butyraldehyde, isobutyraldehyde, n-valeraldehyde, n-hexylaldehyde, 2-ethylbutyraldehyde, 2-ethylhexylaldehyde, n-heptylaldehyde, n-octylaldehyde, n-nonylaldehyde, n-decylaldehyde, and amylaldehyde. Examples of the aromatic aldehyde include benzaldehyde, cinnamaldehyde, 2-methylbenzaldehyde, 3-methylbenzaldehyde, 4-methylbenzaldehyde, p-hydroxybenzaldehyde, m-hydroxybenzaldehyde, phenylacetaldehyde, and β-phenylpropionaldehyde. These aldehydes may be used alone or in combination of two or more. Among them, preferred aldehydes are formaldehyde, acetaldehyde, butylaldehyde, 2-ethylhexylaldehyde, and n-nonylaldehyde, which have excellent acetalization reactivity and can provide sufficient internal plasticizing effect to the resin produced, thereby imparting good flexibility. In addition, more preferred are formaldehyde, acetaldehyde, and butylaldehyde, which can provide an adhesive composition that is particularly excellent in impact resistance and adhesion to metals.
[0073] The amount of the aldehyde to be added can be appropriately set according to the amount of acetal groups in the target polyvinyl acetal resin. In particular, it is preferable to add 60 to 95 mol%, preferably 65 to 90 mol%, based on 100 mol% of polyvinyl alcohol, because this allows the acetalization reaction to proceed efficiently and makes it easy to remove unreacted aldehyde.
[0074] In addition, the method of synthesizing the polyvinyl acetal resin having the above-mentioned structural unit having a carboxyl group is not particularly limited. For example, a method of saponifying polyvinyl acetate obtained by copolymerizing an α-dicarboxy monomer which is a structural unit represented by the above formula (7-1) or a monocarboxy monomer which is a structural unit represented by the above formula (7-2) with vinyl acetate, and acetalizing the resulting polyvinyl alcohol resin by a conventionally known method can be mentioned. In addition, a method of reacting an unmodified polyvinyl alcohol resin with a compound having a carboxyl group such as mercaptopropionic acid to obtain a carboxylic acid-modified polyvinyl alcohol resin by a conventionally known method can be mentioned. In addition, a method of reacting an unmodified polyvinyl acetal resin with a compound having a carboxyl group such as mercaptopropionic acid to perform post-modification can be mentioned. Among them, a method of acetalizing a carboxylic acid-modified polyvinyl alcohol resin by a conventionally known method is preferred. That is, the carboxylic acid-modified polyvinyl acetal resin is preferably an acetalized product of a carboxylic acid-modified polyvinyl alcohol resin. In the case of the acetalization product of the carboxylic acid-modified polyvinyl alcohol resin, a carboxylic acid-modified polyvinyl acetal resin in which an acetyl group and a carboxyl group are located relatively close to each other can be used. Such a carboxylic acid-modified polyvinyl acetal resin can have excellent paste removability because the acetyl group, which generates steric hindrance, generates an appropriate space around the carboxyl group, which has the effect of improving compatibility with the conductive powder. On the other hand, in the case of a carboxylic acid-modified polyvinyl acetal resin in which a carboxyl group is introduced by post-modification of an unmodified polyvinyl acetal resin, the acetyl group and the carboxyl group are present farther apart than in the case of an acetalized product of a carboxylic acid-modified polyvinyl alcohol resin, and therefore the effect of the steric hindrance of the acetyl group is weakened, and sufficient paste removal properties may not be obtained. In addition, when the α-dicarboxy monomer or monocarboxy monomer used in preparing the polyvinyl acetate by copolymerization is a methyl ester, the acetyl group derived from the vinyl acetate is not hydrolyzed before saponification, so that the polyvinyl alcohol resin can be more highly saponified in the subsequent saponification step.Furthermore, since the amount of sodium hydroxide added in the saponification step can be reduced, it is possible to reduce the sodium ion content of the polyvinyl alcohol resin and, in turn, the carboxylic acid-modified polyvinyl acetal resin. Even if the above-mentioned α-dicarboxy monomer or monocarboxy monomer is a methyl ester, hydrolysis is carried out in the subsequent saponification step, so that the obtained polyvinyl alcohol resin has a carboxylic acid unit that does not contain an ester. In addition, among the α-dicarboxy monomers that are the structural units represented by the above formula (7-1), X 1 , X 2 When a monomer in which is a hydrogen atom or a metal atom is used, the amount of sodium hydroxide consumed for hydrolysis of the acetyl group derived from vinyl acetate during saponification increases, and therefore the resulting carboxylic acid-modified polyvinyl acetal resin may have a relatively high sodium ion content.
[0075] The conductive paste of the present invention may contain, in addition to the polyvinyl acetal resin, other resins such as acrylic resins and ethyl cellulose, as long as the effects of the present invention are not impaired.
[0076] The conductive paste of the present invention contains an organic solvent. The organic solvent may be any organic solvent generally used in conductive pastes. In particular, to prevent the sheet attack phenomenon, it is necessary to use an incompatible, low-polarity organic solvent that does not swell or dissolve the polyvinyl butyral resin contained in the ceramic green sheet and has a solubility parameter of 8.5 to 14.0 (cal / cm 3 ) 0.5 It is preferable that the solubility parameter is calculated by the Fedors method. Examples of the organic solvent include terpineol derivatives such as dihydroterpineol, terpinyl acetate, isobornyl acetate, dihydroterpinyl acetate, dihydroterpinyl methyl ether, and terpinyl methyl ether, hydrocarbon solvents such as mineral spirits, and ethers and esters such as dipropylene glycol monomethyl ether and dipropylene glycol monomethyl ether acetate. Among these, dihydroterpineol and dihydroterpinyl acetate are preferred. These organic solvents may be used alone or in combination of two or more.
[0077] The amount of the organic solvent is not particularly limited, but the preferred lower limit is 100 parts by weight and the preferred upper limit is 10,000 parts by weight relative to 100 parts by weight of the polyvinyl acetal resin. When the amount of the organic solvent is 100 parts by weight or more, the viscosity of the conductive paste can be set in a suitable range, and printability can be improved. When the amount of the organic solvent is 10,000 parts by weight or less, the performance of the polyvinyl acetal resin can be fully exhibited in the conductive paste. The more preferred lower limit of the amount of the organic solvent relative to 100 parts by weight of the polyvinyl acetal resin is 200 parts by weight and the more preferred upper limit is 5,000 parts by weight.
[0078] The conductive paste of the present invention contains a conductive powder. The conductive powder is not particularly limited, and examples thereof include powders made of nickel, aluminum, silver, copper, and alloys thereof. These conductive powders may be used alone or in combination of two or more. Among these, nickel is preferred because of its excellent conductivity.
[0079] The conductive powder preferably has an average particle size of 50 to 300 nm and is substantially spherical in shape. When the average particle size is 50 nm or more, the conductive powder has a suitable specific surface area and can improve the dispersibility of the conductive powder. When the average particle size is 300 nm or less, the surface smoothness after printing can be improved. Note that substantially spherical includes particles having a shape close to a sphere as well as a perfect sphere.
[0080] The amount of the conductive powder to be blended is not particularly limited, but a preferred lower limit is 100 parts by weight and a preferred upper limit is 10,000 parts by weight per 100 parts by weight of the polyvinyl acetal resin. When the amount of the conductive powder is 100 parts by weight or more, the density of the conductive powder in the conductive paste can be kept in a sufficient range, and the conductive paste can have excellent conductivity. When the amount of the conductive powder is 10,000 parts by weight or less, the dispersibility of the conductive powder in the conductive paste can be improved, and the conductive paste can have excellent printability. The amount of the conductive powder to be blended is more preferably 200 parts by weight at the lower limit and 5,000 parts by weight at the upper limit relative to 100 parts by weight of the polyvinyl acetal resin.
[0081] The conductive paste of the present invention preferably further contains a ceramic powder in addition to the conductive powder, which makes it easier to match the shrinkage behavior of the conductive powder during firing with that of the ceramic green sheet. The ceramic powder is not particularly limited, but is preferably barium titanate, which is used in the green sheet. The average particle size of the ceramic powder is not particularly limited, but is preferably smaller than the average particle size of the conductive powder, specifically, is preferably 30 nm to 200 nm.
[0082] The conductive paste of the present invention may contain appropriate additives such as plasticizers, lubricants, antistatic agents, dispersants, and surfactants within the scope of the invention.
[0083] Examples of the plasticizer include phthalic acid diesters such as dioctyl phthalate (DOP) and dibutyl phthalate (DBP), adipic acid diesters such as dioctyl adipate, and alkylene glycol diesters such as triethylene glycol-di-2-ethylhexanoate, tetraethylene glycol-di-2-ethylhexanoate, triethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-2-ethylbutyrate, tetraethylene glycol-di-heptanoate, and triethylene glycol-di-heptanoate.
[0084] The dispersant is not particularly limited, but for example, fatty acids, aliphatic amines, alkanolamides, and phosphoric esters are suitable. A silane coupling agent or the like may also be added. The fatty acid is not particularly limited, and examples thereof include saturated fatty acids such as behenic acid, stearic acid, palmitic acid, myristic acid, lauric acid, capric acid, caprylic acid, coconut fatty acid, etc., and unsaturated fatty acids such as oleic acid, linoleic acid, linolenic acid, sorbic acid, beef tallow fatty acid, and hardened castor fatty acid, etc. Among these, lauric acid, stearic acid, oleic acid, etc. are preferred. The aliphatic amine is not particularly limited, and examples thereof include laurylamine, myristylamine, cetylamine, stearylamine, oleylamine, alkyl(coconut)amine, alkyl(hardened beef tallow)amine, alkyl(beef tallow)amine, and alkyl(soybean)amine. The alkanolamide is not particularly limited, and examples thereof include coconut fatty acid diethanolamide, beef tallow fatty acid diethanolamide, lauric acid diethanolamide, and oleic acid diethanolamide. The phosphate ester is not particularly limited, and examples thereof include polyoxyethylene alkyl ether phosphate ester and polyoxyethylene alkyl allyl ether phosphate ester.
[0085] The surfactant is not particularly limited, but examples of the anionic surfactant include sodium salts of fatty acids as carboxylic acids, sodium linear alkylbenzenesulfonate, sodium lauryl sulfate, and alkyl polyoxysulfates as sulfonic acids, and monoalkyl phosphates as phosphoric acids. Examples of the cationic surfactant include alkyl trimethyl ammonium salts, dialkyl dimethyl ammonium salts, and alkyl benzyl dimethyl ammonium salts, while examples of the amphoteric surfactant include alkyl dimethyl amine oxides and alkyl carboxy betaines. Examples of the nonionic surfactant include polyoxyethylene alkyl ethers, fatty acid sorbitan esters, alkyl polyglucosides, fatty acid diethanolamides, and alkyl monoglyceryl ethers. The above-mentioned dispersants and surfactants are also effective in suppressing an increase in viscosity of the paste or resin solution over time.
[0086] The method for producing the conductive paste is not particularly limited, and examples thereof include a method in which the polyvinyl acetal resin, the conductive powder, the organic solvent, and various additives added as necessary are mixed using various mixers such as a ball mill, a blender mill, and a three-roll mill.
[0087] The conductive paste of the present invention is applied to a ceramic green sheet by a printing process, and a plurality of these sheets are stacked and heated and pressed to produce a laminate, which is then degreased and fired to produce a ceramic sintered body, and external electrodes are formed on the end faces of the ceramic sintered body to obtain a multilayer ceramic capacitor. As the printing process, screen printing, die coating, gravure offset, etc. can be used. Such a multilayer ceramic capacitor also constitutes the present invention.
[0088] Since the conductive paste of the present invention contains little undissolved matter, the film applied by the printing process can be made smooth. Therefore, even after degreasing, a smooth film with few voids can be obtained, and a ceramic capacitor with excellent electrical properties can be obtained.
[0089] The method for printing the conductive paste of the present invention is not particularly limited, but can be performed by a printing process such as screen printing, die coating, gravure printing, etc., as described above. The optimal viscosity in this case differs depending on the printing process, so it can be adjusted appropriately. For example, in the case of screen printing, the viscosity is preferably adjusted at a shear rate of 10,000 s -1 For example, for gravure printing, the shear rate is 10,000 s -1 The viscosity at this time is preferably 0.05 to 0.5 Pa·s. Effect of the Invention
[0090] According to the present invention, it is possible to provide a conductive paste which, when dissolved in an organic solvent, has a small amount of fine undissolved matter and is easy to filter, has excellent printability, and can exhibit excellent surface smoothness after printing. [Brief description of the drawings]
[0091] [Figure 1] 2 is an example of an IR absorption spectrum obtained by measuring the IR absorption spectrum of the polyvinyl acetal resin according to the present invention. [Diagram 2]2 is an example of an IR absorption spectrum obtained by measuring the IR absorption spectrum of the polyvinyl acetal resin according to the present invention. [Diagram 3] FIG. 1 is a schematic diagram of a DSC curve. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0092] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0093] Example 1 (Preparation of polyvinyl acetal resin) 100g of polyvinyl alcohol resin A (average polymerization degree 1750, saponification degree 88 mol%, crystallinity degree 16%) was added to 1000g of pure water and stirred at a temperature of 90°C for 2 hours to dissolve. This solution was cooled to 40°C, and 90g of hydrochloric acid (concentration 35% by weight), 30g of acetaldehyde, and 40g of n-butylaldehyde were added to the solution. The liquid temperature was lowered to 10°C, and the acetalization reaction was carried out while maintaining this temperature. After the reaction was completed, the mixture was neutralized, washed with water, and dried to obtain a white powder of polyvinyl acetal resin. The crystallinity of the polyvinyl alcohol resin was measured by the following method. Specifically, the polyvinyl alcohol resin was subjected to differential scanning calorimetry under the following measurement conditions using a thermal analyzer ("DSC6200R" manufactured by Hitachi High-Tech Science Corporation), and the heat of fusion during the second heating was measured to determine the degree of crystallinity. <Measurement conditions> 0℃ (5 min hold) → (1st heating at 10℃ / min heating rate) → 270℃ → (10℃ / min cooling rate) → 0℃ (5 min hold) → (2nd heating at 10℃ / min heating rate) → 270℃ The heat of fusion was calculated from the area of the peak appearing between 100°C and 270°C during the second heating. The peak area was defined as the area of the region surrounded by the straight line connecting points A and B and the DSC curve, as shown in Figure 3. Here, point A was defined as the point at which the DSC curve was separated from the straight line drawn along the linear approximation of the DSC curve from 170°C to the higher temperature side. Point B was defined as the point on the DSC curve that indicated the end temperature of melting. The degree of crystallinity was calculated assuming that the heat of fusion of a polyvinyl alcohol resin with a degree of crystallinity of 100% was 156 J / g.
[0094] (Preparation of conductive paste) A resin solution was obtained by dissolving 10 parts by weight of the obtained polyvinyl acetal resin in 90 parts by weight of dihydroterpineol. After mixing 180 parts by weight of nickel powder as conductive powder, 20 parts by weight of barium titanate, and 50 parts by weight of dihydroterpineol, the obtained resin solution was mixed and dispersed using a triple roll to obtain a conductive paste.
[0095] Example 2 A white powder of a polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of a carboxylic acid-modified polyvinyl alcohol resin B was used instead of 100 g of a polyvinyl alcohol resin A. The carboxylic acid-modified polyvinyl alcohol resin B is a structural unit having a carboxyl group represented by formula (7-1) (in formula (7-1), R 2 is a single bond, R 3 CH2, X 1 and X 2 is a hydrogen atom), the average polymerization degree is 1750, the saponification degree is 89.2 mol %, the amount of carboxyl groups is 0.8 mol %, and the crystallinity is 19%. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0096] Example 3 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that polyvinyl alcohol resin C (average polymerization degree 1750, saponification degree 99 mol%, crystallinity degree 29%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 25 g of acetaldehyde and 57 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0097] Example 4 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin D (average degree of polymerization 1750, degree of saponification 96 mol%, degree of crystallinity 22%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 90 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0098] Example 5 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of carboxylic acid-modified polyvinyl alcohol resin E was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 90 g of n-butyl aldehyde. The carboxylic acid-modified polyvinyl alcohol resin E is a structural unit having a carboxyl group represented by formula (7-1) (in formula (7-1), R 2 is a single bond, R 3 CH2, X 1 and X 2 is a hydrogen atom), the average polymerization degree is 1750, the saponification degree is 97.9 mol %, the amount of carboxyl groups is 0.1 mol %, and the crystallinity is 22%. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0099] Example 6 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin F (average polymerization degree 1750, saponification degree 98 mol%, crystallinity degree 26%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 95 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0100] Example 7 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin G (average polymerization degree 900, saponification degree 96 mol%, crystallinity degree 32%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 85 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0101] Example 8 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin H (average degree of polymerization 900, saponification degree 90 mol%, crystallinity degree 29%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 15 g of acetaldehyde and 70 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0102] Example 9 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin J (average degree of polymerization 600, saponification degree 98 mol%, crystallinity degree 38%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 30 g of acetaldehyde and 70 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0103] Example 10 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin K (average polymerization degree 600, saponification degree 99 mol%, crystallinity degree 38%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 90 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0104] Example 11 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin L (average degree of polymerization 600, saponification degree 96 mol%, crystallinity degree 35%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 20 g of acetaldehyde and 70 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0105] Example 12 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin M (average degree of polymerization 400, saponification degree 98 mol%, crystallinity degree 42%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 25 g of acetaldehyde and 70 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0106] Example 13 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin N (average degree of polymerization 400, degree of saponification 96 mol%, degree of crystallinity 38%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 30 g of acetaldehyde and 55 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0107] Example 14 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin P (average degree of polymerization 250, degree of saponification 88 mol%, degree of crystallinity 32%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 30 g of acetaldehyde and 45 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0108] Example 15 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of carboxylic acid-modified polyvinyl alcohol resin Q was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 15 g of acetaldehyde and 70 g of n-butyl aldehyde. The carboxylic acid-modified polyvinyl alcohol resin Q is a structural unit having a carboxyl group represented by formula (7-2) (in formula (7-2), R 4 CH3, R 5 and R 6 is a hydrogen atom, R 7 is a single bond, X 3 is a hydrogen atom), the average polymerization degree is 250, the saponification degree is 87 mol %, the amount of carboxyl groups is 1 mol %, and the crystallinity is 29%. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0109] (Example 16) A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin R (average degree of polymerization 250, degree of saponification 90 mol%, degree of crystallinity 32%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 30 g of acetaldehyde and 60 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0110] (Example 17) A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of carboxylic acid-modified polyvinyl alcohol resin S was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 95 g of n-butyl aldehyde. The carboxylic acid-modified polyvinyl alcohol resin S is a structural unit having a carboxyl group represented by formula (7-1) (in formula (7-1), R 2 is a single bond, R 3 CH2, X 1 and X 2 is a hydrogen atom), the average polymerization degree is 250, the saponification degree is 98.99 mol %, the amount of carboxyl groups is 0.01 mol %, and the crystallinity is 45%. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0111] (Example 18) A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin T (average polymerization degree 250, saponification degree 99 mol%, crystallinity degree 45%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 95 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0112] (Example 19) A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of carboxylic acid-modified polyvinyl alcohol resin Z was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 15 g of acetaldehyde and 80 g of n-butyl aldehyde. The carboxylic acid-modified polyvinyl alcohol resin Z is a structural unit having a carboxyl group represented by formula (7-1) (in formula (7-1), R 2is a single bond, R 3 CH2, X 1 and X 2 is a hydrogen atom), the average polymerization degree is 600, the saponification degree is 96 mol %, the amount of carboxyl groups is 0.1 mol %, and the crystallinity is 20%. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0113] (Example 20) A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin α (average degree of polymerization 1750, saponification degree 98 mol%, ethylene content 5 mol%, crystallinity degree 25%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 95 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0114] Example 21 Instead of 100g of polyvinyl alcohol resin A, 100g of polyvinyl alcohol resin β (average polymerization degree 400, saponification degree 96 mol%, ethylene content 10 mol%, crystallinity degree 25%) was used. In addition, the aldehyde used in the reaction was changed to 30g of acetaldehyde and 55g of n-butyl aldehyde. A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1 except for the above. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0115] Example 22 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 50 g of carboxylic acid-modified polyvinyl alcohol resin Z and 50 g of polyvinyl alcohol resin β were used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 10 g of acetaldehyde and 85 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0116] Comparative Example 1 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin U (average degree of polymerization 2000, degree of saponification 88 mol%, degree of crystallinity 35%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 15 g of acetaldehyde and 75 g of n-butylaldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0117] Comparative Example 2 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin V (average degree of polymerization 2000, saponification degree 99 mol%, crystallinity degree 38%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 40 g of acetaldehyde and 45 g of n-butylaldehyde. Using the obtained polyvinyl acetal resin, an attempt was made to prepare a conductive paste in the same manner as in Example 1, but the resin was not dissolved in dihydroterpineol, and a conductive paste could not be obtained. In addition, "the resin dissolves" means that no precipitate of 10% by weight or more is formed based on the weight of the added resin, and "the resin does not dissolve" means that a precipitate of 10% by weight or more is formed based on the weight of the added resin.
[0118] Comparative Example 3 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin W (average degree of polymerization 1750, degree of saponification 85 mol%, degree of crystallinity 13%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 40 g of acetaldehyde and 25 g of n-butylaldehyde. Using the obtained polyvinyl acetal resin, an attempt was made to prepare a conductive paste in the same manner as in Example 1, but the resin was not dissolved in dihydroterpineol, and a conductive paste could not be obtained.
[0119] Comparative Example 4 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin X (average degree of polymerization: 500, degree of saponification: 85 mol%, degree of crystallinity: 26%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 40 g of acetaldehyde and 25 g of n-butylaldehyde. Using the obtained polyvinyl acetal resin, an attempt was made to prepare a conductive paste in the same manner as in Example 1, but the resin was not dissolved in dihydroterpineol, and a conductive paste could not be obtained.
[0120] Comparative Example 5 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin Y (average degree of polymerization 1750, saponification degree 99.9 mol%, crystallinity degree 38%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 95 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0121] Comparative Example 6 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin Y (average degree of polymerization: 500, degree of saponification: 99.9 mol%, degree of crystallinity: 71%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 95 g of n-butyl aldehyde. A conductive paste was obtained in the same manner as in Example 1 using the obtained polyvinyl acetal resin.
[0122] Comparative Example 7 A white powder of polyvinyl acetal resin was obtained in the same manner as in Example 1, except that 100 g of polyvinyl alcohol resin γ (average degree of polymerization 1750, degree of saponification 99.2 mol%, degree of crystallinity 35%) was used instead of 100 g of polyvinyl alcohol resin A, and the aldehyde used in the reaction was changed to 70 g of n-butyl aldehyde. Using the obtained polyvinyl acetal resin, an attempt was made to prepare a conductive paste in the same manner as in Example 1, but the resin was not dissolved in dihydroterpineol, and a conductive paste could not be obtained.
[0123] (evaluation) The polyvinyl acetal resins or conductive pastes obtained in Examples 1 to 22 and Comparative Examples 1 to 7 were evaluated as follows. The results are shown in Tables 1 and 2.
[0124] (1) Evaluation of polyvinyl acetal resin (1-1) Amount of acetal groups, hydroxyl groups, and acetyl groups The obtained polyvinyl acetal resin was dissolved in DMSO-D6 at a concentration of 10% by weight. 13 The amounts of acetal groups, hydroxyl groups, and acetyl groups were measured using C-NMR.
[0125] (1-2) Number average molecular weight (Mn), weight average molecular weight (Mw), Mw / Mn The obtained polyvinyl acetal resin was dissolved in tetrahydrofuran at a concentration of 0.05% by weight, and measured using a GPC apparatus HLC-8220 (manufactured by Tosoh Corporation). From the measurement results, the number average molecular weight Mn, weight average molecular weight Mw, and Mw / Mn were calculated using a molecular weight calibration curve prepared using a monodisperse polystyrene standard sample. The column used was Shodex LF-804 (manufactured by Showa Denko KK).
[0126] (1-3)IR Absorption Spectrum The obtained polyvinyl acetal resin was dissolved in a 1:1 ethanol / toluene mixed solution, and then coated on a PET film. -1 The film thickness of the measurement sample was adjusted so that the minimum transmittance of the peak appearing around the wavelength of 22% was obtained, and a polyvinyl acetal resin sheet was obtained. The IR absorption spectrum of the obtained polyvinyl acetal resin sheet was measured at 20°C using an infrared spectrophotometer (HORIBA, FT-720). The measurement results showed that the IR absorption spectrum of the obtained polyvinyl acetal resin sheet was 0.01 to 0.01 at a wave number of 3100 to 3700 cm.-1 A baseline was drawn for the peaks that appeared within this range, and peak analysis was performed on the data corrected so that the transmittance at both ends of the peak was 100%, and the minimum transmittance X, transmittance a, and wavenumbers A and B of the peaks were measured.
[0127] (1-4) Number and percentage (volume%) of particles with diameters of 0.5 to 1.0 μm The obtained polyvinyl acetal resin was dissolved in dihydroterpinyl acetate to a concentration of 0.2% by weight. The particle size distribution of 10 ml of the obtained solution was measured using a particle counter (KS-42C, manufactured by Rion Co., Ltd.), and the number of particles with a diameter of 0.5 to 1.0 μm per 10 ml was measured. The volume of the particles with a diameter of 0.5 to 1.0 μm was calculated assuming that the particles were true spheres with a diameter of 0.75 μm, and the proportion (volume %) of particles with a diameter of 0.5 to 1.0 μm was calculated based on the obtained measurement results.
[0128] (2) Evaluation of conductive paste (2-1) Paste filterability 2 ml of the obtained conductive paste was placed in a 2.5 ml syringe, and a needle with an outer diameter of 0.81 mm, an inner diameter of 0.51 mm, and a length of 38 mm was attached to the tip of the syringe. A force of 5 kgf was applied, and the time it took for all the paste to come out of the tip of the needle was measured.
[0129] (2-2) Printability Using a screen printer, a screen plate, and a printed glass substrate, the conductive paste was printed in an environment of 23°C and 50% humidity, and the solvent was dried in a fan oven for 30 minutes at 100°C. The following screen printer, screen plate, and printed glass substrate were used. Screen printing machine (MT-320TV, manufactured by Microtec) Screen plate (Tokyo Process Services, ST500, emulsion 2μm, 2012 patterns, screen frame 320mm x 320mm) Printing glass substrate (soda glass, 150mm x 150mm, thickness 1.5mm) The printed pattern was observed visually or under a magnifying microscope to confirm the shape of the edges of the printed surface and evaluated according to the following criteria. ◯: Printing was performed according to the print pattern, and no thread-like irregularities were observed at the print edge. △: Printed according to the print pattern, with one area where the edge of the print was thread-like and irregular. ×: The print pattern was not printed according to the print pattern, such as the print being smudged, or two or more portions were observed in which the print edge was disordered like threads.
[0130] (2-3) Surface roughness Using the printed pattern of the conductive paste obtained in "(2-2) Printability", 10 points were measured with a surface roughness meter (Surfcom, manufactured by Tokyo Seimitsu Co., Ltd.) and evaluated according to the following criteria. ○: Average surface roughness Ra of 10 points is less than 0.100 μm △: The average surface roughness Ra of 10 points is 0.100 μm or more and less than 0.150 μm ×: Average surface roughness Ra of 10 points is 0.150 μm or more
[0131] [Table 1]
[0132] [Table 2] [Industrial Applicability]
[0133] According to the present invention, it is possible to provide a conductive paste which, when dissolved in an organic solvent, has a small amount of fine undissolved matter and is easy to filter, has excellent printability, and can exhibit excellent surface smoothness after printing.
Claims
1. A conductive paste used to form electrodes of a multilayer ceramic capacitor, comprising a polyvinyl acetal resin, an organic solvent, and a conductive powder, The polyvinyl acetal resin has an average degree of polymerization of 250 to 1750, a hydroxyl group content of 16 to 25 mol%, an acetoacetal group content of 27 mol% or less, and a ratio (Mw / Mn) of weight average molecular weight (Mw) to number average molecular weight (Mn) of 2.2 to 3.7; The polyvinyl acetal resin has a peak wave number A (cm) in the wave number range of 3100 to 3700 cm in an IR absorption spectrum measured by an infrared spectrophotometer. -1 ), and the amount of hydroxyl groups (mol %) satisfies the relationship of the following formulas (1) and (2). [(3470-A) / hydroxyl group amount]≦5.0 (1) (3470-A)≦150 (2) A: Wave number 3100-3700cm -1 When the minimum transmittance of the peak in the range is X (%), the wave number showing the transmittance a (%) that satisfies [100-(100-X) / 2] is 3470 cm -1 Wavenumber on the lower wavenumber side
2. The polyvinyl acetal resin has an IR absorption spectrum measured by an infrared spectrophotometer with a wave number of 3100 to 3700 cm -1 The wave number A (cm -1 ), and the wave number B of the peak (cm -1 2. The conductive paste according to claim 1 , wherein the relationship of the following formula (3) is satisfied: (3470-A) / (B-3470)≦1.4 (3) B: Wave number 3100-3700cm -1 When the minimum transmittance of the peak in the range is X (%), the wave number showing the transmittance a (%) that satisfies [100-(100-X) / 2] is 3470 cm -1 Wavenumber on the higher wavenumber side
3. 3. The conductive paste according to claim 1, wherein the polyvinyl acetal resin has an acetyl group content of 0.1 to 12 mol %.
4. 4. The conductive paste according to claim 1, wherein the polyvinyl acetal resin has a content of a structural unit having a carboxyl group of 0.01 to 1.0 mol %.
Citation Information
Patent Citations
Positive resistance-temperature characteristic resin composition
JP1997105679A
Polyvinyl acetal resin and method for producing polyvinyl acetal resin
JP2005325342A
Polyvinyl acetal resin and ceramic green sheet
JP2008133371A
Ceramic slurry composition and ceramic green sheet
JP2012193084A
Conductive paste
JP2017063196A