Composition and hardened product
A varnish using an olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer addresses the challenges of high-frequency insulating materials by providing a cured product with low dielectric properties, mechanical strength, and adhesion to copper foil, suitable for electronic components.
Patent Information
- Application Number
- JP2023005482
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-05-20
- Filing Date
- 2023-01-17
- Publication Date
- 2024-10-17
- Estimated Expiration
- 2041-07-13
Smart Images

Figure 0007569392000001 
Figure 0007569392000002 
Figure 0007569392000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition and a cured product thereof. [Background technology]
[0002] As communication frequencies move into the gigahertz band and higher, there is an increasing need for insulating materials with low dielectric properties. Polyolefins such as polyethylene and aromatic vinyl compound polymers such as polystyrene have no polar groups in their molecular structures and are therefore known as materials that exhibit excellent low dielectric constants and low dielectric loss tangents. However, these materials have issues with their heat resistance as electrical insulators because their heat resistance depends on their crystalline melting point or glass transition temperature, and furthermore, because they are thermoplastic resins, there are issues with the film-forming process (Patent Document 1).
[0003] Fluorine-based resins such as perfluoroethylene have the characteristics of low dielectric constant, low dielectric loss, and excellent heat resistance, but are difficult to mold and form into films, and are therefore poorly suited for use in devices. There are also issues with adhesion to copper foil in wiring. On the other hand, substrates and insulating materials using post-curing resins such as epoxy resins, unsaturated polyester resins, polyimide resins, and phenolic resins have been widely used due to their heat resistance and ease of handling, but their dielectric constant and dielectric loss are relatively high, and improvements are needed as insulating materials for high frequencies (Patent Document 2).
[0004] An electrical insulating material made of a graft or block copolymer made of olefin-based and styrene-based polymer segments has been proposed (Patent Document 3). This material focuses on the inherent low dielectric constant and low dielectric loss of olefin-based and styrene-based hydrocarbon polymers. The manufacturing method is to carry out general graft polymerization on commercially available polyethylene and polypropylene in the presence of styrene monomer, divinylbenzene monomer, and a radical polymerization initiator. This method has the problem that the graft efficiency does not increase and the uniformity of the polymer is not sufficient. Furthermore, the obtained polymer contains gel, and there are problems with poor processability and filling properties. In addition, this material is a thermoplastic resin and does not have sufficient heat resistance, so it is necessary to add a heat-resistant resin such as 4-methyl-1-pentene. Furthermore, it is difficult to apply this material to a molding method in which it is applied or filled in a specified location and then cured.
[0005] Patent Document 4 describes an insulating layer made of a crosslinked structure containing a hydrocarbon compound having multiple aromatic vinyl groups as a crosslinking component. The cured product of this crosslinking component specifically described in the examples is rigid, and it is considered difficult to fill a large amount of filler.
[0006] Patent Document 5 shows a cured product obtained from a specific polymerization catalyst and made of an ethylene-olefin (aromatic vinyl compound)-polyene copolymer, a non-polar vinyl compound copolymer, and a specific composition and blending. The cured product specifically described in the examples of Patent Document 5 has the characteristics of a low dielectric constant and a low dielectric loss tangent, but is very soft, and therefore it is necessary to improve the mechanical strength such as the elastic modulus at room temperature and high temperature. For thin-film insulating materials, such as interlayer insulating materials for FPCs (flexible printed circuit boards) and FCCLs (flexible copper clad laminates) and coverlay applications, it is preferable to improve dimensional stability such as the thickness during the mounting process or during use after mounting. Patent Document 6 shows a cured product obtained from a similar specific polymerization catalyst and made of an ethylene-olefin (aromatic vinyl compound)-polyene copolymer, a non-polar vinyl compound copolymer, and a specific composition and blending. Patent Document 7 also shows a cured product of a composition containing a similar copolymer. However, the ethylene-olefin (aromatic vinyl compound)-polyene copolymers specifically described in Patent Documents 5 to 7 have high molecular weights, and therefore when dissolved in a solvent or monomer, the viscosity becomes high, and when used as a varnish, improvements in coatability and impregnation properties may be required. Furthermore, Patent Documents 5 to 7 do not describe a cured product containing only an ethylene-olefin (aromatic vinyl compound)-polyene copolymer or a product substantially containing the ethylene-olefin (aromatic vinyl compound)-polyene copolymer as the main component. Patent Document 8 discloses a method for producing a low molecular weight ethylene-styrene copolymer oligomer, but does not describe the production of an ethylene-styrene-divinylbenzene copolymer oligomer or its uses. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Special Publication No. 52-31272 [Patent Document 2] Japanese Patent Application Publication No. 6-192392 [Patent Document 3] Japanese Patent Application Publication No. 11-60645 [Patent Document 4] JP 2004-087639 A [Patent Document 5] JP 2010-280771 A [Patent Document 6] JP 2009-161743 A [Patent Document 7] JP 2010-280860 A [Patent Document 8] Japanese Patent Application Publication No. 9-040709 Summary of the Invention [Problem to be solved by the invention]
[0008] In contrast to the above-mentioned conventional techniques, it is desirable to provide a curable substance which is suitable for use as a varnish and which, when cured, has a high degree of crosslinking and exhibits excellent low dielectric properties and low water absorption. [Means for solving the problem]
[0009] That is, the present invention can provide the following: First, a varnish containing an olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the following conditions (1) to (4), one or more selected from the following (a) to (c), and (d) a solvent: (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000, preferably less than 10,000, and particularly preferably less than 5,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of aromatic vinyl compound monomer units is 0% by mass or more and 90% by mass or less, preferably 70% by mass or less. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass %. (a) Hardener (b) One or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, olefin-aromatic vinyl compound-aromatic polyene copolymers, and aromatic polyene resins. (c) Polar monomers
[0010] It is also possible to provide a cured product containing an olefin-aromatic vinyl compound-aromatic polyene copolymer that satisfies all of the following requirements (1) to (4): (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000, preferably less than 10,000, and particularly preferably less than 5,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass to 90% by mass, preferably 10% by mass to 70% by mass or 10% by mass to less than 70% by mass. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass %. Effect of the Invention
[0011] The varnish containing the olefin-aromatic vinyl compound-aromatic polyene copolymer of the present invention has low viscosity and excellent low dielectric properties, and can give a cured product having high mechanical strength (elastic modulus, etc.) at room temperature and especially at high temperatures. The cured product of the present invention also has excellent low dielectric properties and high mechanical strength (elastic modulus, etc.) at room temperature and especially at high temperatures. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0012] In this specification, the term "sheet" also includes the concept of "film." In addition, even if the term "film" is used in this specification, the term "sheet" also includes the concept of "sheet." The composition according to the present invention will be described in more detail below. In this specification, the term "composition" is a concept that includes varnish. That is, a composition that is particularly liquid is described as a varnish.
[0013] <Varnish> The varnish of the present invention contains an olefin-aromatic vinyl compound-aromatic polyene copolymer that satisfies all of the following conditions (1) to (4): (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000, preferably less than 10,000, and particularly preferably less than 5,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass to 90% by mass, preferably 10% by mass to 70% by mass, and more preferably 10% by mass to 60% by mass. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass %. At least one other (a) "hardening agent", (b) "One or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, olefin-aromatic vinyl compound-aromatic polyene copolymers, and aromatic polyene resins," (c) "Polar monomer" and (d) a solvent.
[0014] The olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer (hereinafter, sometimes simply referred to as "oligomer") can be obtained by copolymerizing each monomer of an olefin, an aromatic vinyl compound, and an aromatic polyene. In this specification, as a concept distinct from this "oligomer", when the number average molecular weight is 12000 or more, it is defined as an olefin-aromatic vinyl compound-aromatic polyene copolymer, or simply as a "copolymer". From the viewpoint of obtaining a suitable viscosity as a varnish, the varnish and the cured product thereof according to the present invention preferably contain 100 parts by mass or less of the olefin-aromatic vinyl compound-aromatic polyene copolymer relative to 100 parts by mass of the oligomer, more preferably contain 50 parts by mass or less, even more preferably contain 20 parts by mass or less, and even more preferably contain no olefin-aromatic vinyl compound-aromatic polyene copolymer.
[0015] The olefin monomer is at least one selected from α-olefins having 2 to 20 carbon atoms and cyclic olefins having 5 to 20 carbon atoms, and is a compound consisting of carbon and hydrogen without substantially containing oxygen, nitrogen, or halogen. Examples of α-olefins having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decane, 1-dodecane, 4-methyl-1-pentene, and 3,5,5-trimethyl-1-hexene. Examples of cyclic olefins having 5 to 20 carbon atoms include norbornene and cyclopentene. The olefin preferably used is a combination of ethylene and an α-olefin other than ethylene or a cyclic olefin, or ethylene alone. When ethylene alone or the mass ratio of the α-olefin component other than ethylene contained / ethylene component is preferably 1 / 7 or less, more preferably 1 / 10 or less, the peel strength of the obtained cured body with copper foil or copper wiring can be increased, which is preferable. More preferably, the content of α-olefin monomer components other than ethylene contained in the copolymer is 6 mass% or less, and even more preferably 4 mass% or less, or the olefin is ethylene alone. In the preferred combination of ethylene and α-olefin other than ethylene, the glass transition temperature of the finally obtained cured ethylene-α-olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer can be freely adjusted within the range of about -60°C to -10°C depending on the type and content of the α-olefin.
[0016] The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and examples thereof include styrene, paramethylstyrene, paraisobutylstyrene, various vinylnaphthalenes, and various vinylanthracenes.
[0017] The aromatic polyene monomer is a polyene having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in its molecule, preferably various ortho-, meta-, and para-divinylbenzenes or mixtures thereof, divinylnaphthalene, divinylanthracene, p-2-propenylstyrene, p-3-butenylstyrene, and other aromatic vinyl structures, substantially free of oxygen, nitrogen, and halogen, and composed of carbon and hydrogen. In addition, bifunctional aromatic vinyl compounds such as 1,2-bis(vinylphenyl)ethane (abbreviation: BVPE) described in JP-A-2004-087639 can also be used. Among these, various ortho-, meta-, and para-divinylbenzenes or mixtures thereof are preferably used, and a mixture of meta- and para-divinylbenzenes is most preferably used. In this specification, these divinylbenzenes are referred to as divinylbenzenes. When divinylbenzenes are used as aromatic polyenes, they are preferred because they have high curing efficiency and are easy to cure when subjected to a curing treatment.
[0018] The above-mentioned olefin, aromatic vinyl compound, and aromatic polyene monomers may contain other polar groups, such as olefins containing oxygen atoms, nitrogen atoms, etc., aromatic vinyl compounds containing oxygen atoms or nitrogen atoms, or aromatic polyenes containing oxygen atoms or nitrogen atoms, etc., but the total mass of these monomers containing polar groups is preferably 10 mass% or less of the total mass of the present resin composition, more preferably 3 mass% or less, and most preferably does not contain any monomers containing polar groups. By making it 10 mass% or less, the dielectric properties (low dielectric constant / low dielectric loss) of the cured body obtained by curing the present resin composition can be improved.
[0019] The number average molecular weight (Mn) of the copolymer oligomer is 500 or more and less than 12000, preferably less than 10000, and most preferably less than 5000. In the present invention, the number average molecular weight of 500 or more and less than 12000, preferably less than 10000, and most preferably less than 5000 means that the molecular weight calculated as standard polystyrene by GPC (gel permeation chromatography) falls within that range.
[0020] In the present copolymer oligomer, the content of vinyl groups and / or vinylene groups derived from aromatic polyene units, preferably the content of vinyl groups, is 1.5 or more and less than 10, preferably 2 or more and less than 7, per number average molecular weight. If the content of vinyl groups and / or vinylene groups is less than 1.5, the crosslinking efficiency is low, making it difficult to obtain a cured product with sufficient crosslinking density. The content of vinyl groups derived from aromatic polyene units (divinylbenzene units) per number average molecular weight in the copolymer oligomer is calculated by the number average molecular weight (Mn) calculated in terms of standard polystyrene obtained by a GPC (gel permeation chromatography) method known to those skilled in the art, and 1 The vinyl group content derived from the aromatic polyene unit obtained by H-NMR measurement can be compared. For example, 1 By comparing the intensities of the peak areas obtained by H-NMR measurement, if the content of vinyl groups derived from aromatic polyene units (divinylbenzene units) in the copolymer oligomer is 3.2% by mass, and the number average molecular weight converted into standard polystyrene by GPC measurement is 2100, then the molecular weight of the vinyl groups derived from aromatic polyene units in the number average molecular weight is the product of these, 67.5, which is divided by the formula weight of the vinyl groups, 27, to obtain 2.5. In other words, the content of vinyl groups derived from aromatic polyene units per number average molecular weight in this copolymer oligomer is found to be 2.5. 1 The assignment of peaks obtained by H-NMR measurement is known from the literature. 1 A method for determining the composition of a copolymer oligomer from a comparison of peak areas obtained by H-NMR measurement is also known. In this specification, the content of divinylbenzene units in a copolymer oligomer is determined based on the peak intensity ( 1 In other words, the content of divinylbenzene units is calculated from the content of vinyl groups derived from divinylbenzene units, assuming that one vinyl group is derived from one divinylbenzene unit in the copolymer.
[0021] When the copolymer oligomer satisfies the above other conditions and has a number average molecular weight of less than 12,000, preferably less than 10,000, most preferably less than 5,000, a cured product with a higher crosslinking degree (crosslinking density) can be obtained than when a copolymer with a higher molecular weight than the oligomer is used. The crosslinking degree can be determined by, for example, putting a cured product such as a sheet into xylene, heating it to the boiling point, refluxing for 1 hour, recovering it, and checking whether or not the cured product sheet (sometimes called a cured sheet) dissolves or swells. The less the cured product dissolves or swells, the higher the crosslinking degree is determined to be. Furthermore, the high-temperature mechanical properties of the cured product of the present copolymer oligomer can be improved. Specifically, the present cured product can exhibit a higher storage modulus at high temperatures than when a higher molecular weight copolymer is used. Even when a cured product of a composition containing other resins or monomers in addition to the copolymer oligomer is compared with a similar formulation, it can exhibit a higher storage modulus than when a higher molecular weight copolymer is used. This makes it possible to improve the durability and dimensional stability, for example, during a solder reflow process, of a single-layer or multi-layer CCL, FCCL, interlayer insulating layer, or interlayer adhesive layer that contains the present cured product. Specifically, from a practical standpoint, the cured product of the present invention has a storage modulus of 1×10 at 300°C. 6 Pa or more, preferably 2×10 6 Pa or more, most preferably 2.5×10 6 It can show values of Pa or more.
[0022] Furthermore, the present cured product can exhibit a lower coefficient of linear expansion (CTE) than when a higher molecular weight copolymer is used. Even if the cured product is a composition containing other resins or monomers in addition to the copolymer oligomer, it can exhibit a lower coefficient of linear expansion (CTE) when compared with similar formulations. Considering the use of the present cured product, the preferred CTE value for single-layer or multi-layer CCL, FCCL, interlayer insulating layer, or interlayer adhesive layer is in the range of 25 to 150°C, 200 ppm or less, preferably 100 ppm or less, and most preferably 75 ppm or less. Therefore, even if an electronic device, substrate, etc. containing the present cured product is subjected to heat treatment such as passing through a solder reflow furnace, it is preferable because warping, deformation, and exudation of the insulating layer can be suppressed.
[0023] Furthermore, by having a number average molecular weight (Mn) of 500 or more and less than 12000, preferably less than 10000, and most preferably less than 5000, it becomes easy to reduce the viscosity of a varnish containing the present copolymer oligomer. Specifically, even in a varnish containing the present copolymer oligomer at a practical concentration of 33 mass% or more, it becomes easy to adjust the viscosity to, for example, preferably 2000 mPa·s or less, more preferably 1000 mPa·s or less, more preferably 500 mPa·s or less, and most preferably 100 mPa·s or less. The lower the molecular weight of the copolymer oligomer, the easier it is to reduce the viscosity of the final varnish, and there is an effect of being able to widen the range of adjustment of the blend to obtain a particularly preferred viscosity of 100 mPa·s or less. The oligomer has a number average molecular weight of less than 12000, preferably less than 10000, and most preferably less than 5000, so that when it is made into a varnish, the viscosity can be relatively low, making it easy to handle, and in particular when a filler is added, the increase in the viscosity of the composition can be suppressed, and thus the oligomer has preferable properties different from those of higher molecular weight copolymers. In addition, the low number average molecular weight of the oligomer also makes it easy to impregnate glass and other nonwoven fabrics.
[0024] The content of aromatic vinyl compound monomer units contained in the present copolymer oligomer is 0% by mass or more and 90% by mass or less, more preferably 0% by mass or more and 70% by mass or less, or 0% by mass or more and less than 70% by mass, and even more preferably 10% by mass or more and 60% by mass or less. When the content of aromatic vinyl compound monomer units is less than 70% by mass, the glass transition temperature of the cured body of the finally obtained resin composition becomes lower than around room temperature, and the toughness and elongation at low temperatures can be improved, which is preferable. When the content of aromatic vinyl compound monomer units is 10% by mass or more, the aromaticity of the present copolymer oligomer is improved, the compatibility with the flame retardant and the filler is improved, the bleed-out of the flame retardant can be avoided, and the filling property of the filler can be improved. In addition, when the content of aromatic vinyl compound monomer units is 10% by mass or more, a cured body of the resin composition having high peel strength from copper foil or copper wiring can be obtained.
[0025] In the present copolymer oligomer, the content of the olefin monomer unit is preferably 20% by mass or more, more preferably 25% by mass or more, and most preferably 30% by mass or more. The total of the olefin monomer unit, aromatic vinyl compound monomer unit, and aromatic polyene monomer unit is 100% by mass. When the content of the olefin monomer unit is 20% by mass or more, the toughness (elongation) and impact resistance of the finally obtained cured body are improved, and cracks during curing or cracks during a heat cycle test of the cured body are less likely to occur. In the present copolymer oligomer, the content of the olefin monomer unit is preferably 90% by mass or less.
[0026] In the present copolymer oligomer, specific examples of suitable olefin-aromatic polyene copolymer oligomers not containing aromatic vinyl compound monomer units include ethylene-divinylbenzene copolymer oligomers, ethylene-propylene-divinylbenzene copolymer oligomers, ethylene-1-butene-divinylbenzene copolymer oligomers, ethylene-1-hexene-divinylbenzene copolymer oligomers, and ethylene-1-octene-divinylbenzene copolymer oligomers.
[0027] In the present copolymer oligomer, examples of the olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer containing an aromatic vinyl compound monomer unit include ethylene-styrene-divinylbenzene copolymer oligomer, ethylene-propylene-styrene-divinylbenzene copolymer oligomer, ethylene-1-hexene-styrene-divinylbenzene copolymer oligomer, and ethylene-1-octene-styrene-divinylbenzene copolymer oligomer.
[0028] The varnish of the present invention further contains, in addition to the present copolymer oligomer, (a) a curing agent, (b) one or more resins selected from a hydrocarbon-based elastomer, a polyphenylene ether-based resin, an olefin-aromatic vinyl compound-aromatic polyene copolymer, and an aromatic polyene-based resin, and (c) one or more polar monomers.
[0029] <Hardening agent> As a curing agent that can be used in the composition of the present invention, a known curing agent that can be used for polymerization or curing of conventional aromatic polyenes and aromatic vinyl compounds can be used. Examples of such curing agents include radical polymerization initiators, cationic polymerization initiators, and anionic polymerization initiators, and preferably radical polymerization initiators can be used. Preferred are organic peroxide-based and azo-based polymerization initiators, which can be freely selected depending on the application and conditions. A catalog listing organic peroxides can be found on the NOF Corporation website, for example. https: / / www.nof.co.jp / business / chemical / product01a.html https: / / www.nof.co.jp / business / chemical / product01b.html https: / / www.nof.co.jp / business / chemical / product01c.html It can be downloaded from. Organic peroxides are also described in the catalogs of Fujifilm Wako Pure Chemical Industries, Ltd. and Tokyo Chemical Industry Co., Ltd. The curing agent used in the present invention can be obtained from these companies. A known photopolymerization initiator using light, ultraviolet light, or radiation can also be used as the curing agent. Examples of curing agents using a photopolymerization initiator include a photoradical polymerization initiator, a photocationic polymerization initiator, and a photoanionic polymerization initiator. Such photopolymerization initiators can be obtained, for example, from Tokyo Chemical Industry Co., Ltd. Furthermore, curing by radiation or an electron beam itself is also possible. It is also possible to perform crosslinking and curing by thermal polymerization of the raw materials contained without containing a curing agent.
[0030] There is no particular limit to the amount of the curing agent used, but generally, 0.01 to 10 parts by mass is preferred relative to 100 parts by mass of the resin composition. The resin composition is preferably free of the curing agent and solvent. When using a curing agent such as a peroxide or azo polymerization initiator, the curing process is carried out at an appropriate temperature and time, taking into consideration its half-life. In this case, the conditions are arbitrary according to the curing agent, but generally, a temperature range of about 50°C to 200°C is appropriate.
[0031] The varnish of the present invention can contain component (b), i.e., "one or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, olefin-aromatic vinyl compound-aromatic polyene copolymers, and aromatic polyene resins," preferably in the range of 1 to 200 parts by mass per 100 parts by mass of the copolymerized oligomer. The addition of component (b) has the effect of improving the mechanical properties of the cured product obtained from the varnish.
[0032] <Hydrocarbon elastomer> The amount of the hydrocarbon-based elastomer used in the composition of the present invention is preferably 1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and most preferably 1 to 50 parts by mass, based on 100 parts by mass of the copolymer oligomer. The hydrocarbon-based elastomer that can be suitably used in the composition of the present invention preferably has a number average molecular weight of 100 or more and 100,000 or less, more preferably 1,000 or more and 4,500 or less. The hydrocarbon-based elastomer that can be suitably used in the composition of the present invention is preferably a single or multiple elastomers selected from ethylene-based or propylene-based elastomers, conjugated diene-based polymers, block copolymers or random copolymers of aromatic vinyl compounds-conjugated dienes, and hydrogenated products thereof. Examples of ethylene-based elastomers include ethylene-α-olefin copolymers such as ethylene-octene copolymer and ethylene-1-hexene copolymer, EPR, and EPDM, and examples of propylene-based elastomers include atactic polypropylene, low stereoregular polypropylene, and propylene-α-olefin copolymers such as propylene-1-butene copolymer.
[0033] Examples of the conjugated diene polymer include polybutadiene and 1,2-polybutadiene. Examples of the aromatic vinyl compound-conjugated diene block or random copolymer and their hydrogenated products (hydrogenated products) include SBS, SIS, SEBS, SEPS, SEEPS, SEEBS, etc. 1,2-polybutadiene that can be suitably used is available from Nippon Soda Co., Ltd. under the product names of liquid polybutadiene: B-1000, 2000, and 3000. In addition, an example of a copolymer containing a 1,2-polybutadiene structure that can be suitably used is "Ricon 100" from TOTAL CRAY VALLEY. When the resin or resins selected from these hydrocarbon elastomers are liquid (approximately 300,000 mPa s or less) particularly at room temperature (25°C), from the viewpoints of the handleability and moldability (handleability as a thermoplastic resin) of the composition of the present invention in an uncured state, the amount used is preferably 150 parts by mass or less, more preferably 1 to 30 parts by mass, and most preferably in the range of 1 to 20 parts by mass, per 100 parts by mass of the copolymer oligomer.
[0034] <Polyphenylene ether> As the polyphenylene ether (also referred to as "polyphenylene ether resin"), commercially available known polyphenylene ethers can be used. The number average molecular weight of the polyphenylene ether is arbitrary, and considering the moldability of the composition, the number average molecular weight is preferably 10,000 or less, and most preferably 5,000 or less. The number average molecular weight is preferably 500 or more.
[0035] In addition, when the composition of the present invention is added for the purpose of curing, it is preferable that the molecular end is modified with a functional group. In addition, when the composition of the present invention is added for the purpose of curing, it is preferable that one molecule has multiple functional groups. For example, it is preferable to use a modified polyphenylene ether. Examples of the functional group include radically polymerizable functional groups and functional groups such as epoxy groups, and preferably radically polymerizable functional groups. As the radically polymerizable functional group, a vinyl group is preferable. As the vinyl group, one or more of the group consisting of an allyl group, a (meth)acryloyl group, and an aromatic vinyl group are preferable, one or more of the group consisting of a (meth)acryloyl group and an aromatic vinyl group are more preferable, and an aromatic vinyl group is most preferable. That is, in the composition of the present invention, a bifunctional polyphenylene ether in which both ends of the molecular chain are modified with a radically polymerizable functional group is particularly preferable. Examples of such polyphenylene ether include Noryl (trademark) SA9000 (modified polyphenylene ether having methacryloyl groups at both ends, number average molecular weight 2200) manufactured by SABIC and bifunctional polyphenylene ether oligomer (OPE-2St, modified polyphenylene ether having vinylbenzyl groups at both ends, number average molecular weight 1200) manufactured by Mitsubishi Gas Chemical Company, Inc. Allylated PPE manufactured by Asahi Kasei Corporation can also be used. Among these, bifunctional polyphenylene ether oligomer (OPE-2St) manufactured by Mitsubishi Gas Chemical Company, Inc. can be preferably used. The amount of polyphenylene ether used in the composition of the present invention is preferably 1 to 200 parts by mass, more preferably 1 to 100 parts by mass, based on 100 parts by mass of the copolymerized oligomer.
[0036] <Olefin-aromatic vinyl compound-aromatic polyene copolymer> The olefin-aromatic vinyl compound-aromatic polyene copolymer (copolymer) in this specification is a copolymer having a number average molecular weight of 12000 or more. The amount of the olefin-aromatic vinyl compound-aromatic polyene copolymer used in the composition of the present invention is preferably 0 to 100 parts by mass, more preferably 0 to 50 parts by mass, and most preferably 0 to 20 parts by mass, relative to 100 parts by mass of the copolymerized oligomer. By using the olefin-aromatic vinyl compound-aromatic polyene copolymer in this range, a varnish having a good compatibility composition can be provided, and a cured product obtained from this varnish can exhibit good mechanical properties and good member adhesion (for example, adhesion to copper foil). The use of an amount of the olefin-aromatic vinyl compound-aromatic polyene copolymer that exceeds these ranges is not preferable because the viscosity of the toluene solution (varnish) increases. The use of an amount of the olefin-aromatic vinyl compound-aromatic polyene copolymer that exceeds these ranges is not preferable because it reduces the mechanical properties (storage modulus at 300°C) at high temperatures and increases the linear expansion coefficient (CTE).
[0037] <Aromatic polyene resin> The aromatic polyene resin includes a divinylbenzene reactive hyperbranched copolymer (PDV) manufactured by Nippon Steel Chemical & Material Co., Ltd. Such PDV is described, for example, in the document "Synthesis of polyfunctional aromatic vinyl copolymer and development of a new IPN type low dielectric loss material using the same" (Kawabe Masanao, Journal of Electronics Packaging Society, p. 125, Vol. 12 No. 2 (2009)). The amount of the aromatic polyene resin used in the composition of the present invention is preferably 1 to 200 parts by mass, more preferably 1 to 100 parts by mass, and most preferably 1 to 50 parts by mass, relative to 100 parts by mass of the copolymerized oligomer. The use of the aromatic polyene resin in an amount within these ranges is preferable in order to prevent a decrease in adhesion to other members and a decrease in toughness.
[0038] <Polar monomer> The polar monomer that can be used in the resin composition of the present invention is preferably 100 parts by mass or less per 100 parts by mass of the copolymerized oligomer. The resin composition may not substantially contain any monomer. The polar monomer is a monomer having one or more atoms selected from oxygen, nitrogen, phosphorus, and sulfur in the molecule, and the polar monomer that can be suitably used preferably has a molecular weight of less than 5000, more preferably less than 1000, and even more preferably less than 500. The polar monomer that can be suitably used in the resin composition of the present invention is preferably a polar monomer that can be polymerized by a radical polymerization initiator. Examples of the polar monomer include various maleimides, bismaleimides, maleic anhydride, triallyl isocyanurate, glycidyl (meth)acrylate, tri(meth)acryl isocyanurate, and trimethylolpropane tri(meth)acrylate. Maleimides and bismaleimides that can be used in the present invention are described in, for example, International Publication No. 2016 / 114287 and JP-A-2008-291227, and can be purchased from, for example, Daiwa Kasei Kogyo Co., Ltd., Nippon Kayaku Co., Ltd., and Designer Molecules Inc. Also, bismaleimide resin "SLK" manufactured by Shin-Etsu Chemical Co., Ltd. can be used. These maleimide group-containing compounds are preferably bismaleimides from the viewpoints of solubility in organic solvents, high frequency characteristics, high adhesion to conductors, moldability of prepregs, and the like. These maleimide group-containing compounds may be used as polyamino bismaleimide compounds from the viewpoints of solubility in organic solvents, high frequency characteristics, high adhesion to conductors, moldability of prepregs, and the like. Polyamino bismaleimide compounds can be obtained, for example, by subjecting a compound having two maleimide groups at the terminals to a Michael addition reaction with an aromatic diamine compound having two primary amino groups in the molecule. When attempting to obtain high crosslinking efficiency with a small amount of addition, it is preferable to use a polar monomer having a multifunctional group of two or more functional groups, and examples of such a monomer include bismaleimides, triallyl isocyanurate (TAIC), and trimethylolpropane tri(meth)acrylate. The amount of the polar monomer used in the resin composition of the present invention is preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, based on 100 parts by mass of the copolymerized oligomer.By using an amount within this range, the dielectric constant and dielectric dissipation factor of the obtained cured body are prevented from becoming too high; for example, the dielectric constant can be kept at 4.0 or less, preferably 3.0 or less, and the dielectric dissipation factor can be kept at 0.005 or less, preferably 0.002 or less.
[0039] The varnish of the present invention particularly preferably contains, in addition to the present copolymer oligomer, (a) a curing agent, (b) one or more resins selected from a hydrocarbon-based elastomer, a polyphenylene ether-based resin, and an aromatic polyene-based resin, and (c) one or more polar monomers.
[0040] The varnish of the present invention further comprises (d) a solvent.
[0041] <(d) Solvent> An appropriate solvent may be added to the resin composition of the present invention as necessary. The amount of the solvent is not particularly limited. The solvent is used to adjust the viscosity and fluidity of the composition. In particular, when the resin composition of the present invention is in the form of a varnish, a solvent is preferably used. As the solvent, if the boiling point under atmospheric pressure is too low, that is, if the volatility is too high, the thickness of the applied film may become uneven, so a solvent with a boiling point of a certain degree or higher is preferable. The preferred boiling point is about 100°C or higher under atmospheric pressure, more preferably 130°C or higher and 300°C or lower. Examples of the solvent include cyclohexane, toluene, ethylbenzene, xylene, mesitylene, tetralin, acetone, limonene, mixed alkanes, mixed aromatic solvents, etc. The amount of the solvent used in the composition of the present invention is arbitrary, but is preferably 5 to 500 parts by mass, more preferably 10 to 300 parts by mass, and most preferably 50 to 150 parts by mass, relative to 100 parts by mass of the copolymerized oligomer.
[0042] From another viewpoint, the present invention provides a cured product containing an olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the following conditions (1) to (4). Preferably, the present cured product is a cured product of a composition containing an olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the following conditions (1) to (4): (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000, preferably less than 10,000, and particularly preferably less than 5,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass or more and 90% by mass or less, preferably 10% by mass or more and less than 70% by mass. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass %. The cured product further comprises one or more selected from the following (a) to (c): (a) Hardener (b) One or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, olefin-aromatic vinyl compound-aromatic polyene copolymers, and aromatic polyene resins. (c) Polar monomers Here, (a) to (c) have the same meanings as described above. It is preferable that the above-mentioned (d) solvent is evaporated and removed in the cured product, but it does not matter if a part of it remains as long as it does not cause any practical problems. The cured product of the present invention can particularly preferably be obtained by curing a composition containing, in addition to the present copolymer oligomer, (a) a curing agent, (b) one or more resins selected from a hydrocarbon-based elastomer, a polyphenylene ether-based resin, and an aromatic polyene-based resin, and (c) one or more polar monomers.
[0043] The varnish or the cured product of the present invention may further contain one or more selected from (e) a filler, (f) a flame retardant, and (g) a surface modifier.
[0044] <Filling agent> Also, if necessary, a known inorganic or organic filler can be added. These fillers are added for the purpose of controlling the thermal expansion coefficient, controlling the thermal conductivity, and reducing the cost, and the amount used is arbitrary depending on the purpose. In particular, when adding an inorganic filler, it is preferable to use a known surface modifier, such as a silane coupling agent. In particular, when the object of the present invention is to obtain a resin composition excellent in low dielectric constant and low dielectric loss, the inorganic filler is preferably one or more of boron nitride (BN) or silica, and silica is more preferable. As the silica, fused silica is preferable. From the viewpoint of low dielectric properties, since the dielectric constant becomes particularly high when a large amount is added, it is preferable to use less than 500 parts by mass, more preferably less than 400 parts by mass of the filler per 100 parts by mass of the copolymerized oligomer. Furthermore, in order to improve and enhance the low dielectric properties (low dielectric constant, low dielectric loss tangent), a hollow filler or a filler having a shape with many voids may be added.
[0045] Alternatively, instead of inorganic fillers, organic fillers such as high molecular weight polyethylene or ultra-high molecular weight polyethylene can be used. From the viewpoint of heat resistance, it is preferable that the organic fillers themselves are crosslinked, and they are preferably blended in the form of fine particles or powder. These organic fillers can suppress increases in the dielectric constant and dielectric loss tangent.
[0046] On the other hand, by mixing and dispersing a high dielectric constant insulating filler having a dielectric constant of preferably 4 to 10,000, more preferably 5 to 10,000 at 1 GHz in the resin composition of the present invention, it is possible to produce an insulating cured body having a high dielectric constant insulating layer having a dielectric constant of preferably 4 to 20 while suppressing an increase in the dielectric loss tangent (dielectric loss). By increasing the dielectric constant of a film made of an insulating cured body, it is possible to miniaturize circuits and increase the capacity of capacitors, which can contribute to miniaturization of high frequency electrical components. A high dielectric constant, low dielectric loss tangent insulating layer is suitable for applications such as capacitors, inductors for resonant circuits, filters, and antennas. Examples of the high dielectric constant insulating filler used in the present invention include inorganic fillers or metal particles that have been subjected to insulation treatment. Specific examples are known high dielectric constant inorganic fillers such as barium titanate and strontium titanate, and other examples are specifically described in, for example, JP-A-2004-087639.
[0047] <Flame retardants> A flame retardant can be used in the resin composition of the present invention. From the viewpoint of maintaining a low dielectric constant and a low dielectric loss tangent, preferred flame retardants are known organic phosphorus-based flame retardants such as phosphoric acid esters or condensates thereof, known bromine-based flame retardants, and red phosphorus. In particular, among phosphoric acid esters, compounds having multiple xylenyl groups in the molecule are preferred from the viewpoint of flame retardancy and low dielectric loss tangent.
[0048] In addition to the flame retardant, antimony compounds such as antimony trioxide, antimony tetraoxide, antimony pentoxide, and sodium antimonate, or nitrogen-containing compounds such as melamine, triallyl-1,3,5-triazine-2,3,4-(1H,3H,5H)-trione, and 2,4,6-triaryloxy-1,3,5-triazine may be added as a flame retardant assistant. The total amount of these flame retardants and flame retardant assistants is usually preferably 1 to 100 parts by mass per 100 parts by mass of the resin composition. In addition, 30 to 200 parts by mass of the polyphenylene ether (PPE) resin having a low dielectric constant and excellent flame retardancy may be used per 100 parts by mass of the flame retardant.
[0049] <Surface modifier> The resin composition of the present invention may contain various surface modifiers for the purpose of improving adhesion to fillers, copper plates, and wiring. The amount of the surface modifier used is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the resin composition of the present invention other than the surface modifier. Examples of the surface modifier include various silane coupling agents and titanate coupling agents. The various silane coupling agents and titanate coupling agents may be used singly or in combination.
[0050] The composition and varnish of the present invention may contain additives that are usually used in resins, such as antioxidants, weathering agents, light stabilizers, lubricants, compatibilizers, antistatic agents, etc., within the scope of not impairing the effects and objects of the present invention. The composition and varnish of the present invention are obtained by mixing, dissolving or melting the various additives described above, and any known method can be used for mixing, dissolving and melting.
[0051] <Varnish> The varnish of the present invention can be made viscous liquid at room temperature or by heating to 100°C or less by adjusting the composition and molecular weight of the copolymerized oligomer used, adding a certain amount or more of a liquid monomer or solvent within the scope of the present invention, or adding a liquid flame retardant, and the viscosity at room temperature is, for example, several hundred thousand mPa·s or less, preferably 2000 mPa·s or less, more preferably 1000 mPa·s or less, and most preferably 500 mPa·s or less. Specifically, the varnish can be applied, impregnated, filled, or dropped into other materials by an appropriate method, and cured by heat or light to obtain the desired cured product. Such properties can be formed into insulating films or insulating layers by various transfer molding (pressure molding), applying on or between substrates or semiconductor device materials, extrusion lamination, or spin coating and then curing.
[0052] When the composition of the present invention is used for the present varnish, notwithstanding the above description, 10 parts by mass or more, 1000 parts by mass or less, preferably 200 parts by mass or less of a monomer and 10 parts by mass or more, 2000 parts by mass or less of a solvent can be used per 100 parts by mass of the copolymer oligomer of the present invention. Preferred solvents for varnish are as described above. After the varnish is applied or impregnated, the solvent (solvent) and the like can be removed by heating, air drying, or the like, and then the varnish can be cured, or the curing can be performed simultaneously with the removal of the solvent.
[0053] <Molded body> The shape of the molded product obtained from the composition of the present invention is arbitrary. For example, when the composition is a varnish containing a solvent, when the solvent is removed by heating, decompression, air drying, etc. after application on a substrate, the molded product generally becomes a sheet or film-like molded product. In addition, depending on the composition formulation, the composition itself may become a thermoplastic composition, in which case it can be molded into a sheet shape by a known resin processing method, for example, an extrusion method. Uncured sheets and films can be obtained by these methods. A composite can also be obtained by impregnating a porous substrate, woven fabric, or nonwoven fabric with the composition of the present invention and similarly removing the solvent. It can also be formed into, for example, a hemispherical shape by dropping it onto a substrate and removing the solvent. In addition, when the composition does not contain a solvent, a similar molded product can also be produced by heating and melting the composition under temperature conditions in which the curing agent does not act, molding it, and cooling it. The sheet may be uncured (semi-cured) to the extent that the sheet shape can be maintained, or may be completely cured. The degree of curing of the composition can be quantitatively measured by a known dynamic viscoelasticity measurement method (DMA, Dynamic Mechanical Analysis).
[0054] <Curing> The composition including the varnish of the present invention can be cured by a known method with reference to the curing conditions (temperature, time, pressure) of the curing agent contained therein. When the curing agent used is a peroxide, the curing conditions can be determined with reference to the half-life temperature and the like disclosed for each peroxide.
[0055] <Cured product obtained from the composition> In the measurement range of 10 to 30 GHz or 25 to 40 GHz, particularly preferably at 10 GHz, the dielectric constant of the cured product obtained from the composition including the varnish of the present invention is preferably 2.0 or more and 4.0 or less, more preferably 2.0 or more and 3.0 or less, and most preferably 2.0 or more and 2.5 or less. The dielectric loss tangent is preferably less than 0.005 and 0.0003 or more, more preferably 0.003 or less and 0.0005 or more. The volume resistivity of the obtained cured product is preferably 1×10 15 Ω·cm or more. These values are preferred values for high frequency electrical insulating materials of, for example, 3 GHz or more. The copolymerized oligomer used in the composition of the present invention is relatively soft and has a high tensile elongation, so that the cured product obtained from the composition using the copolymerized oligomer has a characteristic that it is relatively soft, has high impact resistance, and can follow the thermal expansion of the substrate while exhibiting sufficient mechanical properties. That is, the tensile modulus of the cured product of the present invention measured at room temperature (23°C) is preferably less than 3 GPa, 5 MPa or more, more preferably 10 MPa or more, and more preferably 50 MPa or more for substrate applications such as CCL. The tensile breaking strength is preferably less than 50 MPa, 5 MPa or more, more preferably 15 MPa or more, and the tensile breaking elongation is preferably 10% or more, and even more preferably 30% or more. The tensile breaking elongation is preferably less than 300%. The cured product of the composition of the present invention can have sufficient heat resistance for practical use.
[0056] <General uses of the resin composition or composition of the present invention> The resin composition or composition of the present invention can be used as a coverlay, a solder resist, a build-up material, an interlayer insulating agent, or an interlayer adhesive. It can also be used as a printed circuit board, a flexible printed circuit board, a CCL (copper clad laminate) board, or an FCCL (flexible copper clad laminate) board. It can also be used as a build-up film, a bonding sheet, a coverlay sheet, a bump sheet for a flip chip bonder, or an electrical insulating layer for a board.
[0057] <Use of the composition as an uncured or partially cured sheet> The uncured or partially cured sheet of the composition of the present invention can be suitably used as a high-frequency electrical insulating material. For example, it can be suitably used as a build-up film, a bonding sheet, a coverlay sheet, a bump sheet for a flip chip bonder, or an insulating layer for a substrate. Instead of conventionally used epoxy resins or silicone resins, the composition can be used as these films or sheets, and cured to form a cured matrix phase with a low dielectric constant and low dielectric loss. The thickness of the sheet is generally 1 to 300 microns. The sheet may contain or be impregnated with woven or nonwoven fabrics such as glass cloth or ceramic fibers, or may be multi-layered with these. In addition, as an antenna cable for a mobile phone or the like, a flexible and bendable wiring partially or entirely insulated with the sheet of the present invention can be used instead of a conventional coaxial cable. For example, the wiring can be covered and insulated with an LCP (liquid crystal polymer) or PPE sheet and the sheet of the present invention or a B-stage sheet (coverlay sheet).
[0058] A multilayer wiring board in which the cured product obtained by using the composition of the present invention is the insulating layer can be a wiring board with excellent high frequency characteristics with low dielectric loss. In this case, in addition to low dielectric loss, the advantages are heat resistance that can withstand soldering, and a certain degree of softness, elongation, and impact resistance that can withstand stress due to heat cycles or thermal expansion differences. For example, it can be produced by laminating and pressing a core material such as a cloth made of glass or quartz, a nonwoven fabric, a film material, a ceramic substrate, a glass substrate, a general-purpose resin plate such as epoxy, a general-purpose laminate, etc., and a conductor foil with an insulating layer made of the present cured product. Also, a slurry or solution containing a curable resin composition may be applied to the core material, dried, and cured to form an insulating layer. The thickness of the insulating layer is generally 1 to 300 microns. Such a multilayer wiring board can also be used by multilayering and integrating.
[0059] The cured product obtained by curing the curable resin or curable resin composition of the present invention can be suitably used as an electrical insulating material as described above, and in particular can be used as a cured product of a potting material, a surface coating agent, a coverlay, a solder resist, a build-up material, an underfill, a filling insulating agent, an interlayer insulating agent, or an interlayer adhesive, or as a cured product of a printed circuit board, a flexible printed circuit board, a CCL (copper clad laminate) board, an FCCL (flexible copper clad laminate) board, or as a build-up film, a bonding sheet, a coverlay sheet, or a bump sheet for a flip chip bonder, and can be used as an electrical insulating material, in particular an electrical insulating material for high frequency.
[0060] In another embodiment of the present invention, the present invention provides a method for producing an olefin-aromatic vinyl compound-aromatic polyene copolymer comprising the above-mentioned copolymer, the storage modulus at 300° C. being 5×10 5 It is also possible to provide an electrical insulating material having a dielectric constant of 2.0 to 2.5 and a dielectric tangent of 0.003 to 0.0005 in a measurement range of 10 to 30 GHz at 23° C. or more.
[0061] The uncured or semi-cured thermoplastic resin composition of the present invention can be bonded to copper foil for wiring by heat and pressure treatment, even without applying an adhesive or performing an adhesive treatment. Here, the copper foil is a concept including copper wiring. In particular, when a copolymer oligomer containing 10% by mass or more of aromatic vinyl compounds is used in the olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer as a raw material, and / or when the olefin is ethylene alone, or when the content of α-olefin relative to the ethylene contained is 6% by mass or less, preferably 4% by mass or less, a peel strength of 1.0 N / mm or more can be obtained in a measurement according to Japanese Industrial Standards (JIS) C6481:1996. It is generally known that the dielectric properties of laminates such as copper-clad laminate sheets are deteriorated by using adhesives or performing adhesive treatments, and it is preferable to provide a peel strength of 1.0 N / mm or more in a measurement according to Japanese Industrial Standards (JIS) C6481:1996 without performing such treatments. In this way, the uncured or semi-cured thermoplastic resin composition of the present invention can be bonded to copper foil for wiring by a curing treatment such as a heat and pressure treatment, without the need for any particular adhesive coating or adhesive treatment. However, in the present invention, there is no precluding the implementation of other measures for imparting adhesion to copper foil or other members (adhesive coating, adhesive treatment, etc.), including the addition of the above-mentioned "surface modifier."
[0062] <Method of producing copolymer oligomer> The present copolymer oligomer can be synthesized by copolymerizing each monomer of an olefin, an aromatic vinyl compound, and an aromatic polyene by any method. The polymerization solution obtained by the following production method can be used as a varnish or a raw material thereof as it is.
[0063] The use of a single-site coordination polymerization catalyst composed of a transition metal compound represented by the following general formula (1) and a cocatalyst is preferred because it enables the production of an olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying the number average molecular weight of the present invention at a lower polymerization temperature, i.e., under a lower polymerization pressure, without using a chain transfer agent such as hydrogen.
[0064] Formula (1) [ka] Here, M in the formula is zirconium or hafnium. Cp1 and Cp2 are cyclopentadienyl groups having no substituents, or cyclopentadienyl groups having one or two alkyl substituents (preferably having 1 to 3 carbon atoms) having no cyclic structure. One of Cp1 and Cp2 may be an indenyl group having no substituents, or an indenyl group having one or two alkyl substituents (preferably having 1 to 3 carbon atoms) having no cyclic structure. Cp1 and Cp2 may be the same or different. In order to produce an olefin-aromatic vinyl compound-aromatic polyene copolymerization oligomer having a lower molecular weight, it is preferable that both Cp1 and Cp2 are cyclopentadienyl groups having no substituents, or cyclopentadienyl groups having one or two alkyl substituents (preferably having 1 to 3 carbon atoms) having no cyclic structure. Y is a carbon, silicon, germanium, or boron atom having a bond with Cp1 and Cp2 and a hydrogen atom or a substituent, and the substituents may be different or the same, and may have a ring structure such as a cyclohexyl group. The substituent is preferably an alkyl group or a phenyl group. X may be the same or different and is preferably selected from the group consisting of hydrogen, halogens such as chlorine and bromine, alkyl groups such as methyl and ethyl, and aryl groups such as phenyl. The aryl group may include alkylaryl groups such as benzyl. Furthermore, two X's may be bonded to each other to form a diene group such as a butadiene group or an isoprene group.
[0065] Examples of such transition metal compounds include dimethylmethylenebiscyclopentadienylzirconium dichloride, diphenylmethylenebiscyclopentadienylzirconium dichloride, dimethylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride, and diphenylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride.
[0066] In the single-site coordination polymerization catalyst of the present invention, the cocatalyst may be a known cocatalyst that has been used in combination with a transition metal compound. As such a cocatalyst, alumoxanes such as methylaluminoxane (also referred to as methylalumoxane or MAO) or boron compounds are preferably used. If necessary, alkylaluminums such as triisobutylaluminum and triethylaluminum may be used together with these alumoxanes or boron compounds. Examples of such cocatalysts include the cocatalysts and alkylaluminum compounds described in EP 0872492A2, JP 11-130808 A, JP 9-309925 A, WO 00 / 20426 A, EP 0985689A2 A, and JP 6-184179 A.
[0067] The aluminum atom / transition metal atom ratio of the cocatalyst such as alumoxane to the metal of the transition metal compound is preferably 0.1 to 100,000, more preferably 10 to 10,000. If it is 0.1 or more, the transition metal compound can be effectively activated, and if it is 100,000 or less, it is economically advantageous. When a boron compound is used as the cocatalyst, the boron atom / transition metal atom ratio is preferably 0.01 to 100, more preferably 0.1 to 10, and most preferably 1. If it is 0.01 or more, the transition metal compound can be effectively activated, and if it is 100 or less, it is economically advantageous. The transition metal compound and the cocatalyst may be mixed and prepared outside the polymerization equipment, or may be mixed in the equipment during polymerization.
[0068] <Production of Copolymer Oligomer> The copolymer oligomer of the present invention is produced by contacting each of the raw material monomers, olefin, aromatic vinyl compound, and aromatic polyene, with a single-site coordination polymerization catalyst comprising the above-mentioned transition metal compound and co-catalyst. Any known method may be used for the order and method. For example, the copolymer oligomer can be produced by applying the copolymer production methods described in International Publication No. 00 / 37517, JP2009-161743A, and JP2010-280771A.
[0069] By using the single-site coordination polymerization catalyst comprising the above transition metal compound and cocatalyst, it is possible to produce the low molecular weight copolymer oligomer of the present invention without using a chain transfer agent, but there is no problem in using a chain transfer agent to produce a copolymer oligomer with a lower molecular weight, for example. As such a chain transfer agent, it is possible to use known chain transfer agents that are used together with the so-called single-site coordination polymerization catalyst, such as hydrogen, alkyl aluminums such as triisobutylaluminum, and 9-BBN described in Chung TC: Macromolecules, 26, 3467 (1993).
[0070] The production method may be a method of polymerization in liquid monomer without using a solvent, or a method of using a single or mixed solvent of saturated aliphatic or aromatic hydrocarbons or halogenated hydrocarbons such as pentane, hexane, heptane, cyclohexane, methylcyclohexane, benzene, toluene, ethylbenzene, xylene, mesitylene, limonene, chloro-substituted benzene, chloro-substituted toluene, methylene chloride, chloroform, etc. Preferably, mixed alkane solvents, cyclohexane, toluene, ethylbenzene, etc. are used. The polymerization form may be either solution polymerization or slurry polymerization. Also, known methods such as batch polymerization, continuous polymerization, prepolymerization, and multistage polymerization can be used as necessary.
[0071] It is also possible to use a single or multiple connected tank type polymerization vessel, or a linear or loop single or multiple connected pipe polymerization equipment. The pipe type polymerization vessel may have various known mixers such as a dynamic or static mixer or a static mixer also serving for heat removal, or various known coolers such as a cooler equipped with a thin tube for heat removal. It may also have a batch type prepolymerization vessel. Furthermore, a method such as gas phase polymerization can be used.
[0072] The polymerization temperature is preferably 0°C to 200°C. If it is 0°C or higher, the polymerization rate is fast and is industrially advantageous, and if it is 200°C or lower, decomposition of the transition metal compound does not occur. More industrially, it is preferably 30°C to 160°C, and particularly preferably 50°C to 160°C. The pressure during polymerization is generally preferably 1 atm to 100 atm, more preferably 1 atm to 30 atm, and industrially, it is most preferably 1 atm to 10 atm.
[0073] The oligomer is recovered from the polymerization solution obtained after the completion of the polymerization by a known method. From an industrial viewpoint, the steam stripping method or the crumb foaming method, which are the so-called raw rubber recovery methods, can be used. In a laboratory, a method of precipitating the oligomer in a large amount of methanol, the so-called methanol precipitation method, is generally convenient. Alternatively, without recovering the oligomer, the solvent and the residual monomer may be removed in whole or in part from the polymerization solution by evaporation using a rotary evaporator, a film evaporator, or the like, and the resulting solution may be diluted with a solvent, and these may be used as a varnish.
[0074] From another viewpoint, the present invention provides a cured product containing an olefin-aromatic vinyl compound-aromatic polyene copolymer obtained by using a single-site coordination polymerization catalyst composed of a transition metal compound represented by the above general formula (1) and a cocatalyst. The olefin-aromatic vinyl compound-aromatic polyene copolymer contained in this cured product preferably satisfies the above conditions (1) to (4). In addition, the present cured product preferably further contains one or more selected from the following (a) to (c): (a) Hardener (b) One or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, olefin-aromatic vinyl compound-aromatic polyene copolymers, and aromatic polyene resins. (c) Polar monomers Of the (b) resins, one or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, and aromatic polyene resins are preferred. EXAMPLES
[0075] The present invention will be described below with reference to examples, but the present invention should not be construed as being limited to the following examples.
[0076] The copolymers obtained in the Synthesis Examples and Comparative Synthesis Examples were analyzed by the following methods.
[0077] The content of vinyl group units derived from ethylene, hexene, styrene, and divinylbenzene in the copolymer is determined by: 1 The measurements were performed using H-NMR from the peak area intensities assigned to each compound. The sample was dissolved in deuterated 1,1,2,2-tetrachloroethane, and the measurements were performed at 80 to 130°C.
[0078] The molecular weight was determined as a number average molecular weight (Mn) converted to standard polystyrene using GPC (gel permeation chromatography) under the following conditions.
[0079] (Number average molecular weight of 1000 or more) Column: Two TSK-GEL MultiporeHXL-M φ7.8×300 mm (manufactured by Tosoh Corporation) were connected in series. Column temperature: 40℃ Solvent: THF Flow rate: 1.0ml / min. Detector: RI detector
[0080] (Number average molecular weight less than 1000) Columns: one TSKgel G3000HXL φ7.8×300 mm, one TSKgel G2000HXL φ7.8×300 mm, and four TSKgel G1000HXL φ7.8×300 mm (manufactured by Tosoh Corporation) connected in series. Column temperature: 40℃ Solvent: THF Flow rate: 0.5ml / min. Detector: RI detector
[0081] <Determination of degree of cross-linking> The sheet-shaped cured product was placed in xylene, heated to the boiling point, and refluxed for 1 hour before being collected. Samples in which no dissolution of the sheet was observed were judged to be "crosslinked" (marked with an O). Samples in which dissolution or partial dissolution was observed were judged to be "insufficiently crosslinked" (marked with an X).
[0082] <Measurement of storage modulus> A dynamic viscoelasticity measuring device (TA Instruments, formerly Rheometrics RSA-G2) was used to measure the storage modulus at 300°C at a frequency of 1Hz while increasing the temperature from room temperature. A measurement sample (3mm x 40mm) was cut out from a film of uniform thickness in the range of approximately 0.1 to 0.3mm that would not interfere with the measurement, and the thickness was accurately measured. Measurements were then performed to determine the storage modulus. The main measurement parameters involved in the measurement are as follows: Measurement frequency 1Hz Heating rate: 3℃ / min Sample measurement length: 10 mm Distortion 0.1%
[0083] <Water absorption rate> Measurements were performed in accordance with ASTM D570-98.
[0084] <Dielectric constant and dielectric loss (dielectric tangent)> The dielectric constant and dielectric loss tangent were measured using the cavity resonator perturbation method (Agilent Technologies 8722ES network analyzer, Kanto Electronics Application Development Co., Ltd. cavity resonator) at 23°C and 10 GHz using a 1 mm x 1.5 mm x 80 mm sample cut from the sheet. In addition, a balanced type circular disk resonator (Keysight Technologies) was used to evaluate the dielectric properties in the same way. The dielectric properties of the balanced type circular disk resonator were evaluated by preparing two identical samples (diameter 3 cm, thickness 0.3 mm), placing copper foil between them and setting them in the resonator, and measuring the resonance frequency (f0) and unloaded Q value (Qu) of the peak that appeared at 25 to 40 GHz. The dielectric constant was calculated from f0, and the dielectric loss tangent (tanδc) was calculated from Qu using the attached analysis software (Balanced type circular disk resonator (method) calculator, balanced type circular disk resonator method analysis software). The measurement temperature was 23°C and the humidity was 50% RH.
[0085] <Volume resistivity> The measurement was performed at room temperature using a film approximately 0.5 mm thick in accordance with JIS K6911:2006.
[0086] <Tensile test> In accordance with JIS K-6251:2017, a film sheet with a thickness of approximately 1 mm was cut into a No. 2 dumbbell 1 / 2 test piece shape and measured using an Orientec Co., Ltd. Tensilon UCT-1T model at 23°C and a tensile speed of 500 mm / min to determine the tensile modulus, tensile breaking strength, and tensile breaking elongation.
[0087] <Catalyst (transition metal compound)> In the following examples, dimethylmethylenebiscyclopentadienyl zirconium dichloride (isopropylidenebiscyclopentadienyl zirconium dichloride, see formula (2) below for structure) having a structure satisfying the above general formula (1) was used as the catalyst (transition metal compound).
[0088] Formula (2) [ka]
[0089] <Production of Copolymer Oligomer> Synthesis examples O-1, O-2, O-3 <Synthesis of ethylene-hexene-styrene-divinylbenzene copolymer oligomer and ethylene-styrene-divinylbenzene copolymer oligomer> With reference to the manufacturing methods described in JP-A-9-40709, JP-A-9-309925, JP-A-2009-161743, and JP-A-2010-280771, polymerization was carried out using dimethylmethylenebiscyclopentadienylzirconium dichloride as a catalyst, modified methylaluminoxane (Tosoh Finechem, MMAO-3A toluene solution) as a cocatalyst, cyclohexane as a solvent, styrene, divinylbenzene, ethylene, and 1-hexene as raw materials, if necessary, in an autoclave with a capacity of 10 L and a stirrer and a jacket for heating and cooling. 1-Isopropanol was added to the obtained polymerization liquid, and then a large amount of methanol was added to recover a copolymer oligomer. The copolymer oligomer was spread thinly in a large container and vacuum dried at 30°C for two days and nights. The raw material composition and polymerization temperature were changed to obtain copolymer oligomers O-1 to O-2 shown in Table 1. O-2 and O-3 were synthesized without using 1-hexene. The total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units was 100% by mass. Table 1 shows the composition and number average molecular weight of the copolymerized oligomer.
[0090] Synthesis example O-4 With reference to the manufacturing methods described in JP-A-9-309925, JP-A-2009-161743, and JP-A-2010-280771, polymerization was carried out using rac-diphenylmethylene(cyclopentadienyl)(1-indenyl)zirconium dichloride as a catalyst, modified methylaluminoxane (Tosoh Finechem, MMAO-3A toluene solution) as a cocatalyst, cyclohexane as a solvent, and styrene, divinylbenzene, and ethylene as raw materials in an autoclave with a capacity of 10 L and a stirrer and a jacket for heating and cooling. 1-Isopropanol was added to the obtained polymerization liquid, and then a large amount of methanol was added to recover a copolymer oligomer. This copolymer oligomer was vacuum dried at 30°C for two days and nights in the same manner as above. [ka]
[0091] Synthesis example P-1 As a comparative example, with reference to the manufacturing methods described in JP 2009-161743 A and JP 2010-280771 A, Rac-dimethylmethylenebis(4,5-benzo-1-indenyl)zirconium dichloride (see formula (3) below for structure) which does not satisfy the above general formula (1) was used as a catalyst, modified methylaluminoxane (Tosoh Finechem Corporation, MMAO-3A toluene solution) as a cocatalyst, cyclohexane as a solvent, and styrene, divinylbenzene, and ethylene as raw materials, and synthesis was performed in the same manner as the oligomers in Synthesis Examples O-1 to O-4, to obtain copolymer P-1. Table 1 shows the composition and number average molecular weight of the copolymer. Rac-dimethylmethylenebis(4,5-benzo-1-indenyl)zirconium dichloride does not satisfy the above general formula (1) because it does not have a cyclopentadienyl group.
[0092] Formula (3) [ka]
[0093] Synthesis example P-2 With reference to the manufacturing methods described in JP-A-9-309925, JP-A-2009-161743, and JP-A-2010-280771, polymerization was carried out using Rac-dimethylmethylenebis(1-indenyl)zirconium dichloride (see formula (4) below for structure) as a catalyst, modified methylaluminoxane (Tosoh Finechem, MMAO-3A toluene solution) as a cocatalyst, cyclohexane as a solvent, and styrene, divinylbenzene, and ethylene as raw materials, using an autoclave with a capacity of 10 L and equipped with a stirrer and a jacket for heating and cooling. 1-Isopropanol was added to the obtained polymerization liquid, and then a large amount of methanol was added to recover the copolymer. This copolymer oligomer was vacuum dried at 30°C for two days and nights in the same manner as above. Rac-dimethylmethylenebis(1-indenyl)zirconium dichloride does not satisfy the above general formula (1) because it does not have a cyclopentadienyl group.
[0094] Formula (4) [ka]
[0095] The raw materials were as follows: The 1,2-PBd used was Nippon Soda Co., Ltd. product B3000 (number average molecular weight 3200). A bifunctional polyphenylene ether oligomer (OPE-2St, number average molecular weight 1200) was used. A toluene solution product manufactured by Mitsubishi Gas Chemical Company, Inc. was further diluted with toluene, and a large amount of methanol was added to perform methanol precipitation, followed by air drying and drying under reduced pressure to obtain a powdered polyphenylene ether oligomer. The SEBS used was Asahi Kasei Chemicals Corporation's H-1041. The curing agent used was NOF Corporation's Percumyl D (dicumyl peroxide).
[0096] [Table 1]
[0097] [Table 2-1]
[0098] [Table 2-2]
[0099] Example 1 Using a vessel equipped with a heating and cooling jacket and stirring blade, O-1 (ethylene-hexene-styrene-divinylbenzene copolymer oligomer) obtained in the synthesis example and a solvent (toluene) were heated to about 60°C and stirred to dissolve the copolymer oligomer. Furthermore, 1 part by mass of a curing agent Percumyl D (dicumyl peroxide, manufactured by NOF Corporation) was added to 100 parts by mass of the resin composition (copolymer oligomer in Example 1) excluding the curing agent and solvent, dissolved, stirred and mixed to obtain a varnish-like composition. The obtained composition was poured into a Teflon (registered trademark) mold (frame length 7 cm, width 7 cm, thickness 0.2 mm, 0.5 mm, or 1.0 mm) on a PET sheet placed on a glass plate, air-dried on a hot plate at 50°C, and further dried in a vacuum dryer at 70°C for 1 hour to obtain an uncured sheet. A PET sheet was then placed on top of this, sandwiched between glass plates, and heated in a dryer for 30 minutes at 120° C., 30 minutes at 150° C., and then 120 minutes at 200° C. After completion of the heat treatment, the glass plates and the mold were removed, and a cured product was obtained as a flexible semi-rigid resin-like film.
[0100] Examples 2 to 9, Comparative Examples 1 to 6 Curable resin compositions were prepared according to the formulations in Table 2 (the units in the table are parts by mass) in the same manner as in Example 1, and heat treatment was carried out in the same manner to obtain film-like cured products of the compositions of the Examples and Comparative Examples. The state of the film-like cured products was observed.
[0101] <Materials used> 1,2-PBd B3000: Liquid polybutadiene, "B-3000" manufactured by Nippon Soda Co., Ltd., number average molecular weight 3200, viscosity 210 Poise (45°C) Bifunctional polyphenylene ether oligomer (OPE-2St): Modified polyphenylene ether having vinylbenzyl groups at both ends, manufactured by Mitsubishi Gas Chemical Company, Inc., number average molecular weight 1200 SEBS H-1041: Hydrogenated styrene-based thermoplastic elastomer (SEBS), Asahi Kasei Corporation's "Tuftec H1041", number average molecular weight 58,000
[0102] The uncured compositions obtained in Examples 1 to 9 were viscous liquids (varnish-like). Therefore, they could be easily made to flow at room temperature or by slightly heating, and could be applied or impregnated into porous materials.
[0103] The cured products of the curable resin compositions obtained in Examples 1 to 9 were evaluated. None of the cured sheets were dissolved in boiling xylene and maintained their shape, indicating that crosslinking had progressed sufficiently. The storage modulus (300°C) was also a desirable value of 2×10 6 Pa or higher.
[0104] Furthermore, the cured products of the copolymer oligomer alone (Examples 1, 2, 5, and 7) exhibited a higher storage modulus (300°C) than the cured product of the copolymer alone (Comparative Example 4). The storage modulus of Comparative Example 1, which is a cured product of another copolymer alone, was not measurable. The cured products of the compositions containing the copolymer oligomer exhibited a higher storage modulus (300°C) than the cured products of the compositions containing the same proportion of copolymer (Example 4 and Comparative Example 5, Examples 6 and 8 and Comparative Example 6).
[0105] Furthermore, when tensile tests were carried out on the examples in which component (b) was added, all of them showed a tensile modulus of elasticity of less than 3 GPa and 3 MPa or more. The tensile breaking strength of the sheets was in the range of 5 MPa or more and less than 50 MPa, and the tensile breaking elongation was in the range of 10% or more and less than 300%. This supports the improvement of mechanical properties by adding component (b). The dielectric constant of the cured body of the present invention was in the range of 2.0 or more and 3.0 or less, and the dielectric tangent was in the range of 0.003 or less and 0.0005 or more. The water absorption of the cured film was less than 0.1 mass%, and the volume resistivity was 1×10 15 It was Ω·cm or more.
[0106] The cured sheet of the composition obtained in Comparative Example 1 was partially dissolved in boiling xylene, and the degree of crosslinking was determined to be insufficient. Since the storage modulus of the cured sheet of Comparative Example 1 became too low at high temperatures, it broke near 250 °C during the measurement of the storage modulus, and the measurement at 300 °C was impossible.
[0107] The cured sheet of the composition obtained in Comparative Example 2 was hard and cracked, and various subsequent measurements were not performed.
[0108] The dielectric tangent of the sheet obtained in Comparative Example 3 did not satisfy the scope of the present invention. Therefore, the measurement of the storage modulus of the cured sheet of Comparative Example 3 was omitted.
[0109] The storage moduli (at 300 °C) of the sheets obtained in Comparative Examples 4, 5, and 6 did not satisfy the preferred range of the present invention.
[0110] <Viscosity of varnish> The resin concentration in the varnishes obtained in each Example and Comparative Example, and the viscosity of the varnishes were described in a table. The measurement was performed using a rotational rheometer (MCR302: manufactured by Anton Paar) at 25 °C and a shear rate of 1 sec -1 . In the table, ◎ (excellent) means less than 100 mPa·s, 〇 (good) means 100 or more and less than 500 mPa·s, △ (fair) means 500 or more and less than 2000 mPa·s, and × (NG) means 2000 mPa·s or more. The varnishes obtained in Examples 1 to 4 were ◎ at a resin concentration of 33% by mass or more, and were judged to have very excellent coating properties and impregnation properties. The varnishes obtained in Examples 5 to 9 were 〇 at a resin concentration of 33% by mass or more, and were judged to have excellent coating properties and impregnation properties. On the other hand, the varnishes containing the copolymer obtained in the Comparative Examples were relatively high in viscosity and were judged to be insufficient in coating properties and impregnation properties.
[0111] The linear expansion coefficient (CTE) of the cured sheet was measured. <CTE (Linear expansion coefficient)> CTE was measured using a thermomechanical analyzer (TMA: Thermomechanical Analyzer, manufactured by BRUKER AXS, now manufactured by Netzsch Japan) with reference to Section 16, Materials Standard for Printed Wiring Boards, of the JPCA Standard "Standard for Electronic Circuit Boards, 3rd Edition," and under conditions of width 3 to 5 mm, thickness 0.5 to 0.6 mm, chuck distance 15 to 20 mm, tensile load 10 g, and heating rate: 10°C / min, and the average value between 25°C and 150°C was calculated. The CTE values of the cured sheets obtained in Examples 2, 5, and 7, which were cured products of the oligomer alone, were 60 ppm, 85 ppm, and 100 ppm, respectively. On the other hand, the cured sheet obtained in Comparative Example 1, which was a cured product of the copolymer alone, had a CTE value of >500 ppm, and the sheet obtained in Comparative Example 4 had a CTE value of about 350 ppm.
[0112] From the above results, the cured product obtained by curing the curable resin composition of the present invention is sufficiently crosslinked, and has high mechanical properties at high temperatures. The composition exhibits excellent elongation (toughness) and strength at room temperature, a specific range of elastic modulus, and at the same time, excellent low dielectric constant and low dielectric tangent value, low water absorption, and high insulation. The uncured composition is in a varnish state having fluidity, has low viscosity and is easy to apply or impregnate, and can be easily formed into various shapes including sheets by molding and curing into various shapes, and can be suitably used as an electrical insulating material particularly for high frequency. The composition of the present invention can give a cured product having excellent moldability and molding processability such as film formability, low dielectric constant, low dielectric loss, high volume resistivity, high mechanical strength at room temperature and high temperatures, and excellent toughness (elongation), strength, heat resistance, and low water absorption.
[0113] The composition of the present invention can be used as a varnish by laminating with other members, applying coating, impregnating, etc., and curing, and can therefore be suitably used as an interlayer adhesive (interlayer adhesive layer) or an interlayer insulating agent (interlayer insulating layer). The composition of the present invention can be molded into various shapes in an uncured state by drying the varnish and removing the solvent, and can also be made into an uncured sheet, for example. The composition of the present invention can be cured and used as a printed circuit board, a flexible printed circuit board, an FCCL (flexible copper clad laminate) board, an interlayer adhesive layer, or an interlayer insulating layer. It can also be used as an insulating layer for a CCL (copper clad laminate) board or a PCB board. The cured product of the present invention can be suitably used as a thin-film electrical insulating material or an electrical insulating material for high frequencies. The cured product of the present invention can also be suitably used as a board, an antenna member, or a wiring material for a millimeter-wave radar.
Claims
1. A molded article obtained from a varnish containing an olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the following conditions (1) to (4), one or more of the following (a) to (c), and (d) a solvent: (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 10% by mass or more and 70% by mass or less. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin monomer is one or more selected from olefins having 2 to 20 carbon atoms, and is ethylene alone, a combination of ethylene and an α-olefin other than ethylene, or a combination of ethylene and a cyclic olefin, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass%. (a) Hardener (b) One or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, olefin-aromatic vinyl compound-aromatic polyene copolymers, and aromatic polyene resins. (c) Polar Monomer
2. The varnish has a resin content of at least 33% by mass or more, and is subjected to a drying process at 25° C. for 1 sec. -1 2. The molded article according to claim 1, having a viscosity of 2000 mPa·s or less as measured by a spectrometer.
3. A cured product obtained from the molded product according to claim 1 or 2, which is free of solvent.
4. The cured product according to claim 3, which is an electrical insulating material.
5. An electrical insulating material comprising the cured product according to claim 4.
6. A CCL substrate, an FCCL substrate, an interlayer insulating layer or an interlayer adhesive layer, comprising the cured product according to claim 3 or 4.
7. A method for producing a varnish, comprising the steps of: A step of obtaining an olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer having a number average molecular weight of 500 or more and less than 12,000 using a single-site coordination polymerization catalyst composed of a transition metal compound represented by the following general formula (1) and a cocatalyst; 【Chemistry 1】 (wherein M is zirconium or hafnium. Cp1 and Cp2 are cyclopentadienyl groups having no substituents, or cyclopentadienyl groups having one or two alkyl substituents not having a cyclic structure, and Cp1 and Cp2 may be the same or different from each other, or One of Cp1 and Cp2 is a cyclopentadienyl group having no substituent or a cyclopentadienyl group having one or two alkyl substituents not having a cyclic structure, and the other of Cp1 and Cp2 is an indenyl group having no substituent or an indenyl group having one or two alkyl substituents not having a cyclic structure. Y has bonds to Cp1 and Cp2 and is a hydrogen atom or a carbon atom having a substituent, and the substituents may be different or the same and may have a cyclic structure. X is selected from the group consisting of hydrogen, halogen, an alkyl group, and an aryl group, or two Xs combine to form a diene group. adding a solvent to the olefin-aromatic vinyl compound-aromatic polyene copolymer to obtain a varnish; Including, the olefin monomer in the olefin-aromatic vinyl compound-aromatic polyene copolymer is one or more olefin monomers selected from olefins having 2 to 20 carbon atoms, the aromatic vinyl compound monomer in the olefin-aromatic vinyl compound-aromatic polyene copolymer is an aromatic vinyl compound having from 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is from 10% by mass to 70% by mass, the aromatic polyene in the olefin-aromatic vinyl compound-aromatic polyene copolymer is one or more selected from polyenes having 5 to 20 carbon atoms and containing a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight, The total amount of the olefin monomer unit, the aromatic vinyl compound monomer unit and the aromatic polyene monomer unit in the olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer is 100 mass %. A manufacturing method comprising:
8. The method according to claim 7, wherein the olefin-aromatic vinyl compound-aromatic polyene copolymer contained in the obtained varnish satisfies all of the following conditions (1) to (4): (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 10% by mass to 60% by mass. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin monomer is one or more selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass %.
9. adding one or more selected from the following (a) to (c) to the olefin-aromatic vinyl compound-aromatic polyene copolymer: (a) Hardener (b) One or more resins selected from the group consisting of hydrocarbon elastomers, polyphenylene ether resins, and aromatic polyene resins. (c) Polar Monomer The method of claim 7 or 8, further comprising:
10. A method for producing a molded body, comprising the steps of: A step of obtaining an olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer having a number average molecular weight of 500 or more and less than 12,000 using a single-site coordination polymerization catalyst composed of a transition metal compound represented by the following general formula (1) and a cocatalyst; 【Chemistry 2】 (wherein M is zirconium or hafnium. Cp1 and Cp2 are cyclopentadienyl groups having no substituents, or cyclopentadienyl groups having one or two alkyl substituents not having a cyclic structure, and Cp1 and Cp2 may be the same or different from each other, or One of Cp1 and Cp2 is a cyclopentadienyl group having no substituent or a cyclopentadienyl group having one or two alkyl substituents not having a cyclic structure, and the other of Cp1 and Cp2 is an indenyl group having no substituent or an indenyl group having one or two alkyl substituents not having a cyclic structure. Y has bonds to Cp1 and Cp2 and is a hydrogen atom or a carbon atom having a substituent, and the substituents may be different or the same and may have a cyclic structure. X is selected from the group consisting of hydrogen, halogen, an alkyl group, and an aryl group, or two Xs combine to form a diene group. adding a solvent to the olefin-aromatic vinyl compound-aromatic polyene copolymer to obtain a varnish; Obtaining a molded body from the obtained varnish; Including, the olefin monomer in the olefin-aromatic vinyl compound-aromatic polyene copolymer is one or more olefin monomers selected from olefins having 2 to 20 carbon atoms, the aromatic vinyl compound monomer in the olefin-aromatic vinyl compound-aromatic polyene copolymer is an aromatic vinyl compound having from 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is from 10% by mass to 70% by mass, the aromatic polyene in the olefin-aromatic vinyl compound-aromatic polyene copolymer is one or more selected from polyenes having 5 to 20 carbon atoms and containing a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight, The total amount of the olefin monomer unit, the aromatic vinyl compound monomer unit and the aromatic polyene monomer unit in the olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer is 100 mass %. A manufacturing method comprising:
11. The method of claim 10 further comprising removing the solvent from the varnish.
12. A method for producing a cured body, comprising the steps of: A step of hardening the molded body obtained by the manufacturing method according to claim 10 or 11 by adding a peroxide to the molded body. A manufacturing method comprising:
13. The composition contains an olefin-aromatic vinyl compound-aromatic polyene copolymer having a number average molecular weight of 500 or more and less than 12,000, and has a storage modulus at 300° C. of 2.5×10 6 A cured product having a dielectric constant of 2.0 to 2.5 Pa and a dielectric loss tangent of 0.003 to 0.0005, measured at 23° C. and 10 GHz, the olefin monomer in the olefin-aromatic vinyl compound-aromatic polyene copolymer is one or more selected from olefins having 2 to 20 carbon atoms, and is ethylene alone, a combination of ethylene and an α-olefin other than ethylene, or a combination of ethylene and a cyclic olefin; the aromatic vinyl compound monomer in the olefin-aromatic vinyl compound-aromatic polyene copolymer is an aromatic vinyl compound having from 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is from 10% by mass to 70% by mass, the aromatic polyene in the olefin-aromatic vinyl compound-aromatic polyene copolymer is one or more selected from polyenes having 5 to 20 carbon atoms and containing a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight, The total amount of the olefin monomer unit, the aromatic vinyl compound monomer unit and the aromatic polyene monomer unit in the olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer is 100 mass %. A hardened body, characterized in that
14. The cured product according to claim 13, wherein the olefin-aromatic vinyl compound-aromatic polyene copolymer satisfies all of the following conditions (1) to (4): (1) The number average molecular weight of the copolymer oligomer is 500 or more and less than 12,000. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 10% by mass to 60% by mass. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 10 per number average molecular weight. (4) The olefin monomer is one or more selected from olefins having 2 to 20 carbon atoms, and is ethylene alone, a combination of ethylene and an α-olefin other than ethylene, or a combination of ethylene and a cyclic olefin, and the total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100 mass%.
15. The cured product according to claim 13 or 14, which does not contain a solvent.
16. The cured product according to any one of claims 13 to 15, which does not contain an olefin-aromatic vinyl compound-aromatic polyene copolymer having a number average molecular weight of 12,000 or more.
Citation Information
Patent Citations
Method to form droppout preventive angle for speeddchange gear fitted to automobiles
JP1977031272A
Thermosetting resin composition having low dielectric constant
JP1994192392A
Production of ethylene / Aromatic vinyl compound copolymer
JP1997040709A
Ethylene / aromatic vinyl compound copolymer and its production
JP1997309925A
Heat-resistant low-permitivity polymer material, and film, substrate board, electronic part and heat-resistant resin molding prepared from the same