Textile products and manufacturing method thereof

The use of a silane coupling agent and zirconium phosphate layer on textile fibers addresses the issue of functional substance separation during washing, ensuring durable and efficient fixation of photocatalysts on textile surfaces.

JP7569520B2Active Publication Date: 2024-10-18SHINSHU UNIVERSITY +1
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2020096164
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-06-02
Publication Date
2024-10-18
Estimated Expiration
2040-06-02

AI Technical Summary

Technical Problem

Existing textile products face challenges in maintaining functional substance fixation and washing durability, particularly when functional substances are supported on the surface, as they tend to separate during washing due to friction, and conventional methods for fixing photocatalysts to fiber base materials are inefficient.

Method used

A method involving the use of a silane coupling agent with an amino group to form a surface treatment layer on the fiber base material, followed by a zirconium phosphate layer, which electrostatically fixes functional substances like photocatalysts, enhancing their adhesion and durability.

Benefits of technology

The method allows for firm fixation of functional substances, such as photocatalysts, on the textile surface, providing excellent washing durability and efficient manufacturing, even on chemical fibers like polyester, by utilizing electrostatic and covalent bonding.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007569520000002
    Figure 0007569520000002
  • Figure 0007569520000003
    Figure 0007569520000003
  • Figure 0007569520000004
    Figure 0007569520000004
Patent Text Reader

Abstract

To provide a textile product that allows a functional substance to be strongly fixed thereon and has excellent washing durability, and a method for producing a textile product that can efficiently produce the textile product.SOLUTION: A textile product has a fiber substrate, a surface-treated layer formed on at least part of the fiber substrate with a silane coupling agent, and a zirconium phosphate layer fixed on the surface-treated layer. The silane coupling agent includes a silane compound having an amino group.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a textile product and a method for producing a textile product. [Background technology]

[0002] In recent years, attempts have been made to impart functions such as flame retardancy, water repellency, UV protection properties, antibacterial properties, germicidal properties, stain resistance (self-cleaning properties), etc. to textile products such as woven fabrics, knitted fabrics, and nonwoven fabrics. Such functions are generally imparted to textile products by kneading a functional substance that imparts the desired function into the resin that constitutes the fiber.

[0003] However, depending on the functional substance, the functional substance embedded in the fiber may be in a state where it is difficult to exert the intended function. On the other hand, when the functional substance is supported on the surface of a textile product, the functional substance is likely to be removed from the textile product due to washing, friction during use, and the like.

[0004] Patent Document 1 proposes a textile product carrying a photocatalyst, characterized in that a zirconium phosphate layer is electrostatically fixed to a textile substrate, and a photocatalyst is electrostatically fixed to the surface of the zirconium phosphate layer. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] JP 2010-185158 A Summary of the Invention [Problem to be solved by the invention]

[0006] Meanwhile, textile products, including clothing, are washed (cleaned) frequently depending on their use. It is desirable for textile products imparted with functional substances to have washing durability, in which the functions of the functional substances are exhibited even after multiple washings. Although the textile product described in Patent Document 1 has a certain degree of washing durability, further improvement in washing durability is desired.

[0007] Furthermore, in the technology described in Patent Document 1, in order to firmly fix the photocatalyst to the fiber substrate, it is necessary to form a plurality of zirconium phosphate layers on the surface of the fiber substrate via aluminum ions or polyaluminum ions. There is a demand for a method for manufacturing a fiber product that can more efficiently and firmly fix a functional substance to a fiber substrate.

[0008] Therefore, an object of the present invention is to provide a textile product capable of firmly fixing a functional substance to the surface and having excellent washing durability, and a method for producing such a textile product that can efficiently produce the textile product. [Means for solving the problem]

[0009] As a result of intensive research to achieve the above object, the present inventors have found that a textile product capable of firmly fixing a functional substance can be obtained by treating the surface of a textile substrate with a silane coupling agent having an amino group to form a surface treatment layer, and then forming a zirconium phosphate layer on the surface of the textile substrate through the surface treatment layer. They also found that the above method is simpler and more efficient than conventional methods. Based on the above findings, the present inventors have further researched and arrived at the present invention.

[0010] The gist of the present invention is as follows. (1) a fiber base material; A surface treatment layer formed on at least a part of the surface of the fiber substrate using a silane coupling agent; a zirconium phosphate layer fixed on the surface treatment layer, The textile product, wherein the silane coupling agent comprises a silane compound having an amino group. (2) The fiber substrate has hydroxyl groups and / or carboxyl groups on its surface, The textile product according to (1), wherein the surface treatment layer is fixed to the textile substrate via the hydroxyl groups and / or the carboxyl groups. (3) The textile product according to (1) or (2), wherein the textile base material contains polyester-based fibers. (4) The textile product according to any one of (1) to (3), wherein the silane coupling agent contains an aminoalkyltrialkoxysilane. (5) The textile product according to any one of (1) to (4), further comprising a functional substance fixed to a surface of the zirconium phosphate layer. (6) The textile product according to (5), wherein the functional substance includes a photocatalyst. (7) The textile product according to (6), wherein the photocatalyst contains titanium oxide. (8) The textile product according to any one of (5) to (7), wherein the functional substance includes a protein or a sugar. (9) The textile product according to any one of (5) to (8), wherein the functional substance includes sericin. (10) The textile product according to any one of (5) to (9), wherein the functional substance contains cellulose. (11) treating at least a portion of a surface of a fiber substrate with a silane coupling agent to form a surface treatment layer on at least a portion of the surface of the fiber substrate; forming a zirconium phosphate layer on the surface treatment layer, The method for producing a textile product, wherein the silane coupling agent contains a silane compound having an amino group. (12) The method for producing a textile product according to (11), further comprising a step of introducing hydroxyl groups and / or carboxyl groups into the surface of the textile base material prior to the step of forming the surface treatment layer. (13) The method for producing a textile product according to (11) or (12), further comprising a step of fixing a functional substance on the zirconium phosphate layer. Effect of the Invention

[0011] With the above-mentioned configuration, it is possible to provide a textile product that can firmly fix a functional substance to the surface and has excellent washing durability, and a method for producing such a textile product that can efficiently produce the textile product. [Brief description of the drawings]

[0012] [Figure 1] FIG. 1 is a partially enlarged cross-sectional view of a textile product according to one embodiment of the present invention. [Diagram 2] FIG. 2 is a graph showing the results of a washing durability test of the textile products according to Example 1 and Comparative Example 1. [Diagram 3] FIG. 3 is a set of scanning electron microscope images of the fiber surface observed after each step of the method for producing a textile product according to Example 1. [Figure 4] FIG. 4 shows spectra obtained by observing the surfaces of the textile products according to Example 1 and Comparative Example 1 by energy dispersive X-ray microfluorescence analysis. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0013] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS Hereinafter, preferred embodiments of a textile product and a method for manufacturing a textile product according to the present invention will be described in detail with reference to the drawings.

[0014] <1. Textile products> First, the textile product according to the present embodiment will be described. Fig. 1 is a partially enlarged cross-sectional view of the textile product according to the present embodiment. Note that in the figure, the size of each component is appropriately exaggerated for ease of explanation, and the actual ratio and size of each component are not shown.

[0015] The textile product 1 shown in FIG. 1 includes a textile substrate 10, a surface treatment layer 20 disposed on at least a portion of the surface of the textile substrate 10, a zirconium phosphate layer 30 fixed on the surface treatment layer 20, and a functional substance 40 fixed on the surface of the zirconium phosphate layer 30.

[0016] (1.1. Fiber base material) The fiber substrate 10 is a substrate for a fiber product. The fiber substrate 10 is generally composed mainly of fibers such as natural fibers and / or synthetic fibers. The form of the fiber substrate 10 is not particularly limited and can be arbitrarily selected depending on the application of the fiber product. For example, it can be a single fiber, twisted yarn, composite yarn, hollow yarn, staple fiber, woven fabric, knitted fabric, net, nonwoven fabric, cotton, etc., and one of these can be used alone or two or more can be used in combination.

[0017] As described above, the fiber substrate 10 includes natural fibers and / or synthetic fibers. Examples of natural fibers include natural cellulose fibers such as cotton, hemp, kenaf, pulp (chemical pulp, mechanical pulp), and other plant fibers, particularly fibers derived from wood fibers, various cellulosic fibers such as regenerated cellulose fibers such as viscose rayon, cupra, and acetate, polysaccharide fibers having an amide group or an amino group such as chitin and chitosan, animal hair such as wool, cashmere, and angora, silk, and the like. One of these may be used alone or two or more may be used in combination. Examples of synthetic fibers include acrylic fibers such as acrylic fibers and modacrylic fibers, polyester fibers such as polyethylene terephthalate, polytrimethylene terephthalate, polyethylene naphthalate, and polybutylene terephthalate, polyether ester fibers, polyolefin fibers such as polyethylene and polypropylene, polyacrylate fibers, polyvinyl chloride fibers, nylon fibers such as nylon 6 and nylon 66, polyamide fibers, polyimide fibers, aramid fibers, polyetherimide fibers, polyphenylene sulfide fibers, polyurethane fibers, polyvinyl alcohol fibers, ethylene vinyl alcohol fibers, and polyarylate fibers. These may be used alone or in combination of two or more.

[0018] The fiber base material 10 may be made of only natural fibers or synthetic fibers, or may be made of a combination of natural and synthetic fibers. In these cases, it is of course possible to use multiple types of natural fibers or multiple types of synthetic fibers.

[0019] In addition, the fiber substrate 10 preferably has a hydroxyl group and / or a carboxyl group on its surface. Specifically, it is preferable that the hydroxyl group and / or the carboxyl group is exposed on the surface of the fiber constituting the fiber substrate 10. This allows the reactive group of the silane coupling agent constituting the surface treatment layer 20 described later to bond with the hydroxyl group or the carboxyl group on the surface of the fiber substrate 10, and the surface treatment layer 20 can be firmly fixed to the surface of the fiber substrate 10. For example, among the above-mentioned natural fibers, cellulosic fibers have a large number of hydroxyl groups originating from cellulose.

[0020] Alternatively, even in the case of fibers that do not have hydroxyl groups and / or carboxyl groups on their surface, hydroxyl groups and / or carboxyl groups can be generated on the fiber surface by the method described below, making it possible for the silanol groups of the silane coupling agent that constitutes the surface treatment layer 20 to bond with the hydroxyl groups or carboxyl groups on the surface of the fiber substrate 10, and the surface treatment layer 20 can be fixed more firmly to the surface of the fiber substrate 10.

[0021] The fiber substrate 10 preferably comprises one or more fibers selected from the group consisting of cellulose-based fibers, polysaccharide fibers, polyester-based fibers, and polyvinyl alcohol fibers, more preferably one or more fibers selected from the group consisting of natural cellulose fibers and polyester-based fibers, and particularly preferably one or more fibers selected from the group consisting of cotton, hemp, kenaf, and polyethylene terephthalate.

[0022] Due to the chemical structure of the components that compose the cellulose-based fiber, many hydroxyl or carboxyl groups are exposed on the surface, which improves the adhesion between the surface treatment layer 20 and the fiber substrate 10, and ultimately allows the functional substance to be more firmly fixed to the fiber substrate 10.

[0023] On the other hand, due to the chemical structure of the constituent components, polyester-based fibers such as polyethylene terephthalate have traditionally been difficult to support functional substances on their fiber surfaces. However, according to the present invention, it is possible to firmly support the functional substance 40 on the fiber surface. In addition, by generating hydroxyl groups and / or carboxyl groups on the fiber surface by the method described below, the adhesion between the surface treatment layer 20 and the fiber substrate 10 is improved, and the functional substance 40 is more firmly fixed to the fiber substrate 10.

[0024] (1.2. Surface Treatment Layer) The surface treatment layer 20 is a layer formed of a silane coupling agent on at least a part of the surface of the fiber substrate 10. The silane coupling agent constituting the surface treatment layer 20 contains a silane compound having an amino group. This makes it possible to firmly fix the zirconium phosphate layer 30 to the fiber substrate 10 via the surface treatment layer 20. As a result, it becomes possible to firmly fix the functional substance 40 supported on the zirconium phosphate layer 30 to the surface of the fiber product 1.

[0025] More specifically, the surface treatment layer 20 formed by the silane coupling agent has a siloxane bond as the main skeleton, which is generated by the reaction between reactive groups of the silane coupling agent, such as silanol groups and alkoxy groups bonded to silicon atoms. During the formation of the surface treatment layer 20, the reactive groups of the silane coupling agent also react with functional groups present on the surface of the fiber substrate 10, such as hydroxyl groups and carboxyl groups, to form covalent bonds. As a result, the surface treatment layer 20 formed is firmly fixed to the surface of the fiber substrate 10 by the covalent bonds.

[0026] On the other hand, as described above, the silane coupling agent contains a silane compound having an amino group. Therefore, the surface treatment layer 20 formed by the silane coupling agent has a large number of amino groups exposed on its surface. The nitrogen atoms in the amino groups can be converted into hydrogen ions (H +) and the like, and can be positively charged. The zirconium phosphate layer 30 can be fixed via the amino groups exposed on the surface treatment layer 20 and positively charged. Here, the amino groups exposed on the surface of the surface treatment layer 20 are fixed to the surface treatment layer 20 by covalent bonds, and the surface treatment layer 20 is fixed to the surface of the fiber substrate 10 by covalent bonds. Therefore, the amino groups are prevented from being detached from the surface of the fiber substrate 10, as compared with the conventional technology in which the zirconium phosphate layer 30 is supported by metal cations such as aluminum. Therefore, the zirconium phosphate layer 30 can be reliably fixed to the surface of the fiber substrate 10 via the surface treatment layer 20.

[0027] The surface treatment layer 20 formed by the silane coupling agent is mainly composed of relatively stable siloxane. Therefore, even if the textile product 1 carries a substance that has reactivity or catalyzes a reaction as a functional substance on the zirconium phosphate layer 30, the surface treatment layer 20 protects the fiber base material 10 from deterioration.

[0028] As described above, the silane coupling agent constituting the surface treatment layer 20 contains at least a silane compound having an amino group. Examples of the silane compound having an amino group include aminoalkyltrialkoxysilane, di-(aminoalkyl)-dialkoxysilane, and aminoalkyl-di-(alkoxy)-monoalkylsilane.

[0029] An example of the aminoalkyltrialkoxysilane is a silane compound represented by the following formula (1). Si(OR 1 )3R 2 NH2(1)

[0030] In formula (1), R 1 is a linear or branched alkyl group having 1 to 10 carbon atoms; R 2 is a linear or branched alkylene group having 1 to 10 carbon atoms.

[0031] R 1In the formula (I), examples of the linear alkyl group include a methyl group, an ethyl group, an n-propyl group, an n-butyl group, an n-pentyl group, an n-hexyl group, an n-heptyl group, an n-octyl group, an n-nonyl group, and an n-decyl group. 1 In the above formula, examples of the branched alkyl group include an i-propyl group, a t-butyl group, and an i-butyl group.

[0032] R 1 The number of carbon atoms in R is preferably 2 or more in order to suppress deterioration of the silane coupling agent during storage. 1 The number of carbon atoms in R is preferably 6 or less, and more preferably 4 or less, in order to maintain high reactivity of the silane coupling agent when the surface treatment layer 20 is formed. 1 is preferably an ethyl group, an n-propyl group, an n-butyl group, an i-propyl group, a t-butyl group or an i-butyl group, and particularly preferably an ethyl group, an n-propyl group or an n-butyl group.

[0033] R 2 Examples of the straight-chain alkylene group include straight-chain alkylene groups having 1 to 10 carbon atoms, such as methylene, ethylene, n-propylene, n-butylene, n-pentylene, n-hexylene, n-heptylene, and n-octylene. 2Examples of the branched alkylene group include a 1-methylpropylene group, a 2-methylpropylene group, a 1,1-dimethylpropylene group, a 1,2-dimethylpropylene group, a 1,3-dimethylpropylene group, a 2,2-dimethylpropylene group, a 1,2,3-trimethylpropylene group, a 1,1,2-trimethylpropylene group, a 1,2,2-trimethylpropylene group, a 1,1,3-trimethylpropylene group, a 1-methylbutylene group, a 2-methylbutylene group, a 1,1-dimethylbutylene group, and a 1,2-dimethylbutylene group. , 1,3-dimethylbutylene group, 1,4-dimethylbutylene group, 2,2-dimethylbutylene group, 2,3-dimethylbutylene group, 1,2,3-trimethylbutylene group, 1,2,4-trimethylbutylene group, 1,1,2-trimethylbutylene group, 1,2,2-trimethylbutylene group, 1,3,3-trimethylbutylene group, 1-methylpentylene group, 2-methylpentylene group, 3-methylpentylene group, 1-methylhexylene group, 2-methylhexylene group, and 3-methylhexylene group.

[0034] R 2 From the viewpoint of ensuring the stability of the silane coupling agent, the number of carbon atoms in R is preferably 2 or more. 2 The number of carbon atoms in R is preferably 6 or less, more preferably 4 or less. 2 is preferably an ethylene group, an n-propylene group, an n-butylene group or an n-pentylene group, particularly preferably an ethylene group, an n-propylene group or an n-butylene group.

[0035] Preferred aminoalkyltrialkoxysilanes include, for example, 2-aminoethyltriethoxysilane, 2-aminoethyltri-n-propoxysilane, 2-aminoethyltriisopropoxysilane, 2-aminoethyltri-n-butoxysilane, 2-aminoethyltrii-butoxysilane, 2-aminoethyltrisec-butoxysilane, 2-aminoethyltritert-butoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltri-n-propoxysilane, 3-aminopropyltriisopropoxysilane, 3-aminopropyltri-n-butoxysilane, 3-aminopropyltrii-butoxysilane, 3-aminopropyltrisec-butoxysilane, and 3-aminopropyltritert-butoxysilane.

[0036] An example of the di-(aminoalkyl)-dialkoxysilane is a silane compound represented by the following formula (2). Si(OR 3 )2(R 4 NH2)2(2)

[0037] An example of the aminoalkyl-di-(alkoxy)-monoalkylsilane is a silane compound represented by the following formula (3). Si(OR 5 )2(R 6 NH2)R 7 (3)

[0038] In the above formulas (2) and (3), R 3 , R 5 and R 7 R in the above formula (1), including its preferred embodiments. 1 In addition, in the above formulas (2) and (3), R 4 and R 6 R in the above formula (1), including its preferred embodiments. 2 is the same as:

[0039] Among the above, the silane coupling agent preferably contains an aminoalkyltrialkoxysilane, and more preferably contains one or more selected from the group consisting of 2-aminoethyltriethoxysilane, 2-aminoethyltri-n-propoxysilane, 2-aminoethyltriisopropoxysilane, 2-aminoethyltri-n-butoxysilane, 3-aminopropyltriethoxysilane, 3-aminopropyltri-n-propoxysilane, and 3-aminopropyltriisopropoxysilane.

[0040] The silane coupling agent may contain a silane compound other than the silane compound having an amino group. Examples of such silane compounds include alkoxysilane compounds such as methyltrimethoxysilane, dimethyldimethoxysilane, phenyltrimethoxysilane, dimethoxydiphenylsilane, n-propyltrimethoxysilane, hexyltrimethoxysilane, decyltrimethoxysilane, 1,6-bis(trimethoxysilyl)hexane, tetraethoxysilane, methyltriethoxysilane, dimethyldiethoxysilane, phenyltriethoxysilane, n-propyltriethoxysilane, hexyltriethoxysilane, and octyltriethoxysilane; vinyl group-containing silane compounds such as vinyltrimethoxysilane and vinylethoxysilane; 2-(3,4-epoxycyclohexyl)ethyltrimethoxysilane, 3-glycidoxypropylmethyldimethoxysilane, 3-glycidoxypropyltrimethoxysilane, 3-glycidoxypropyltrimethoxysilane, and 3-glycidoxypropyltrimethoxysilane. Examples of the silane compound include epoxy group-containing silane compounds such as glycidoxypropylmethyldiethoxysilane and 3-glycidoxypropyltrimethoxysilane; styryl group-containing silane compounds such as p-styryltrimethoxysilane; (meth)acryloxy group-containing silane compounds such as 3-methacryloxypropylmethyldimethoxysilane, 3-methacryloxypropyltrimethoxysilane, 3-methacryloxypropylmethyldiethoxysilane and 3-methacryloxypropyltriethoxysilane; ureido group-containing silane compounds such as 3-ureidopropyltrialkoxysilane; isocyanate group-containing silane compounds such as 3-isocyanatepropyltriethoxysilane; isocyanurate group-containing silane compounds such as tris-(trimethoxysilylpropyl)isocyanurate; hexamethyldisilazane; and hexamethyldisiloxane.

[0041] In such a case, the content of the silane compound having an amino group in the silane coupling agent is 10% by mass or more, and preferably 50% by mass or more.

[0042] The surface treatment layer 20 is formed by using the above-mentioned silane coupling agent. The details of the formation method will be described later.

[0043] The average thickness of the surface treatment layer 20 is not particularly limited, but is, for example, from 0.002 μm to 10 μm, and preferably from 0.1 μm to 1 μm.

[0044] The surface treatment layer 20 may have a relatively uniform thickness, or may have different thicknesses at different locations. When the thickness of the surface treatment layer 20 varies at different locations, the surface treatment layer 20 has irregularities. In this case, the surface treatment layer 20 can support a larger amount of zirconium phosphate polymer, and the substance adsorption ability of the zirconium phosphate layer 30 described later can be further improved.

[0045] (1.3. Zirconium phosphate layer) The zirconium phosphate layer 30 is fixed on the surface treatment layer 20. The zirconium phosphate layer 30 is formed by laminating one or more layers of plate-shaped inorganic polymers peeled off from zirconium phosphate having a layered structure. For example, the zirconium phosphate layer 30 is formed by laminating a layered inorganic polymer ([Zr((R 8 4N) x H 1-x PO4)2]) is composed of one or more laminated layers.

[0046] The zirconium phosphate layer 30 has a negative charge in the phosphate group in the plate-like polymer constituting the zirconium phosphate layer. On the other hand, the amino group exposed on the surface of the surface treatment layer 20 becomes a positively charged ammonium cation by receiving a hydrogen ion. Then, the phosphate group of the zirconium phosphate layer 30 and the ammonium cation of the surface treatment layer 20 are electrostatically bonded to fix the zirconium phosphate layer 30 to the surface treatment layer 20. Here, the zirconium phosphate layer 30 has a large number of phosphate groups on the contact surface with the surface treatment layer 20 due to its chemical structure. On the other hand, the surface treatment layer 20 also has a large number of ammonium cations on the contact surface with the zirconium phosphate layer 30. Therefore, electrostatic bonds (multipoint electrostatic bonds) between a large number of phosphate groups and ammonium cations are generated between the surface treatment layer 20 and the zirconium phosphate layer 30, and the surface treatment layer 20 and the zirconium phosphate layer 30 are fixed. In this case, even if the bonds between some of the phosphate groups and the ammonium cations are cut, the fixation between the surface treatment layer 20 and the zirconium phosphate layer 30 is maintained by other bonds. Furthermore, the once broken bond between the phosphate group and the ammonium cation will be re-bonded when they come close to each other again. As a result, the zirconium phosphate layer 30 is firmly fixed to the surface treatment layer 20.

[0047] On the other hand, the zirconium phosphate layer 30 has exposed phosphate groups even on the surface opposite to the surface treatment layer 20. Therefore, the zirconium phosphate layer 30 can electrostatically or chemically fix the functional substance 40 via the phosphate groups.

[0048] Furthermore, the zirconium phosphate layer 30 has an ion exchange ability similar to that of an ion exchange resin. Therefore, when the textile product 1 is used as clothing or the like, the zirconium phosphate layer 30 can adsorb ammonia or ammonium ions in sweat or urine. Since the ion exchange ability of the zirconium phosphate layer 30 is reversible, it can be regenerated by ion exchange with hydrogen ions in water during washing.

[0049] The thickness of the plate-like polymer constituting the zirconium phosphate layer 30 is about 0.75 nm. Therefore, even if many layers of polymer are laminated, for example several tens of layers, the zirconium phosphate layer 30 covers the fiber material relatively thinly and does not affect the texture of the fiber product 1.

[0050] Crystalline zirconium phosphate is known to be of the α type (Zr(HPO4)2·2H2O) and γ type (Zr(PO4)(H2PO4)·2H2O). The α type has a smaller interlayer distance of the polymer compared to the γ type, and Na + In addition, in terms of the structure of the phosphate group, the γ-type has a partial structure of a phosphate ion and a dihydrogen phosphate ion, whereas the α-type is composed of only a partial structure of a hydrogen phosphate ion, so that the charge density on the polymer surface is more uniform and the bonds with ammonium cations are also thought to be distributed uniformly and evenly, and stronger bonds can be expected. Therefore, it is preferable to use a polymer of zirconium phosphate peeled from α-type crystalline zirconium phosphate.

[0051] In addition, the layered inorganic polymer ([Zr((R 8 4N) x H 1-x PO4)2]), R 8 is independently H or a linear or branched alkyl group having 1 to 10 carbon atoms at each occurrence. The linear and branched alkyl groups are as described above for R 1 The same can be used. 8 is preferably a linear alkyl group having 1 to 6 carbon atoms, more preferably a linear alkyl group having 2 to 5 carbon atoms, and further preferably an n-propyl group, an n-butyl group, or an n-pentyl group. 8 are preferably identical.

[0052] The average thickness of the zirconium phosphate layer 30 is not particularly limited, but is, for example, 1 nm or more and 1000 nm or less, and preferably 10 nm or more and 500 nm or less.

[0053] The zirconium phosphate layer 30 may have a relatively uniform thickness or may have different thicknesses at different locations. Alternatively, the zirconium phosphate layer 30 may have irregularities due to the irregularities of the surface treatment layer 20. For example, when the zirconium phosphate layer 30 has irregularities on its surface, such irregularities on the zirconium phosphate layer 30 increase the surface area of ​​the zirconium phosphate layer 30 and promote adsorption of the functional substance 40 and other substances, such as ammonia and ammonium ions.

[0054] (1.4.Functional substances) The functional substance 40 is a substance for imparting a desired function to the fixed textile product 1. Examples of the desired functions that are imparted here include flame retardancy, water repellency, heat shielding, light shielding (blocking visible light and ultraviolet rays), antibacterial properties, germicidal properties, self-cleaning properties (stain resistance), and texture imparting properties.

[0055] The functional substance 40 is fixed on the zirconium phosphate layer 30. The mechanism for fixing the functional substance 40 to the zirconium phosphate layer 30 is not particularly limited, and may be electrostatic fixation using the negative charge of the phosphate group of the zirconium phosphate layer 30, or fixation by chemical bonding (e.g., ionic bonding, covalent bonding) between the zirconium phosphate layer 30 and the functional substance 40. The functional substance 40 is firmly fixed onto the fiber substrate 10 via the above-mentioned surface treatment layer 20 and zirconium phosphate layer 30 .

[0056] There are no particular limitations on the functional substance 40, so long as it can be fixed to the zirconium phosphate layer 30 and can exert a desired function. For example, the functional substance 40 may be a photocatalyst, a texture imparting agent, a water repellent, a moisturizing agent, a water absorbing agent, a light absorbing agent, a fluorescent agent, an adsorbent, etc., and one of these may be used alone or two or more may be used in combination.

[0057] Photocatalysts are substances that exhibit catalytic activity when irradiated with electromagnetic waves such as light. Examples of photocatalysts include metal compounds such as oxides, nitrides, hydroxides, and complex salts of metal elements. Depending on the type, such metal compounds can be excited by light irradiation (particularly ultraviolet irradiation) to exhibit oxidation-reduction ability and decompose organic matter. This allows the photocatalyst to exhibit antibacterial, bactericidal, and / or self-cleaning (anti-fouling) effects. Specific examples of metal oxides include titanium dioxide, titanic acid, titanates, niobic acid, niobic acids, titanoniobic acids, zinc oxide, copper oxide, silver oxide, iron oxide, tungsten oxide, nickel oxide, molybdic acid, and tantalic acids, metal oxynitrides such as tantalum oxynitrides, metal complex salts such as bismuth vanadates, and metal hydroxide complex salts such as copper hydroxyphosphates.

[0058] Among the above, the functional material 40 preferably contains a metal oxide, more preferably titanium oxide and / or silver oxide, as a photocatalyst. Titanium oxide has high photocatalytic activity and can impart a high self-cleaning function to the textile product 1. In addition, silver oxide has high germicidal and antibacterial functions. Titanium oxide is known to have various crystal types, such as anatase type, rutile type, brookite type, etc. Of these, the functional material 40 preferably contains the anatase type.

[0059] In addition, the metal oxide is usually supported on the zirconium phosphate layer 30 as a functional material 40 in the form of secondary particles formed by aggregation of primary particles. The average particle size of the primary particles of the metal oxide is not particularly limited, but is preferably less than 1 μm, more preferably 50 nm or less. This allows the metal oxide to exhibit high photocatalytic activity and strong binding power. In addition, if the average particle size of the primary particles of the metal oxide is too small, the band gap may widen due to the quantum size effect, making it impossible to effectively utilize near-ultraviolet light, thereby reducing reaction efficiency, so it is preferable that the average particle size of the primary particles of the metal oxide is 20 nm or more. The "average particle size of the primary particles" referred to here is the average particle size calculated from images observed under an electron microscope using an FE-SEM (field emission scanning electron microscope): Hitachi S-5000 type.

[0060] The particle size of the secondary particles of the metal oxide is not particularly limited, but is, for example, 50 to 5000 nm, preferably 1000 to 3000 nm, from the viewpoint of stable fixation to the zirconium phosphate layer 30 and maintaining the texture of the fiber. The particle size of the metal oxide dispersed in water is measured by a light scattering method in an aqueous dispersion of the metal oxide. Compared with the secondary particles in an aqueous dispersion of the metal oxide, the secondary particles (functional material 40) supported on the zirconium phosphate layer 40 tend to have a larger secondary particle size due to aggregation during the process of being supported on the surface, but the particle size of the secondary particles in the aqueous dispersion of the metal oxide is reflected in the particle size of the metal oxide (functional material 40) supported on the zirconium phosphate layer 40. Here, the aggregates formed by the particles coming into contact with each other on the supported surface will necessarily have a larger particle size than the secondary particles observed in the solution.

[0061] Most metal oxides as the functional material 40 are positively charged in an acidic solution and negatively charged in an alkaline solution due to the dissociation equilibrium of hydrophilic functional groups such as hydroxyl groups on the surface. In this embodiment, the charging tendency of metal oxides in water is utilized, and the functional material 40 (metal oxide) positively charged in water is electrostatically adsorbed to the negatively charged zirconium phosphate layer 30, and the functional material 40 is fixed to the outermost part of the fiber substrate. The phosphate group found in the partial structure of zirconium phosphate dissociates by protons to give the zirconium phosphate layer 30 a permanent negative charge, and has the property of specifically binding to metal oxides such as titanium oxide. The density of the phosphate structure of zirconium phosphate is 4.1 pieces / square nm, and exists at an extremely high density, so that even nanoparticle-shaped metal oxides can be firmly fixed by multipoint electrostatic bonds and specific covalent bonds.

[0062] The texture imparting agent imparts texture to the textile product 1. Examples of texture imparting agents include proteins such as sericin. Sericin is a component of silk, and by fixing sericin as the functional substance 40 to the zirconium phosphate layer 30, the textile product 1 can exhibit the texture of silk.

[0063] In addition, proteins have peptide bonds, and nitrogen atoms in the peptide bonds can become positively charged by receiving hydrogen ions, so proteins are fixed to the phosphate groups of the zirconium phosphate layer 30 via such positively charged portions.

[0064] The functional material 40 may also contain sugars. By using sugars as the functional material 40, it is possible to impart texture, water absorption, water retention, etc. similar to those of cotton or regenerated cellulose fibers. Examples of sugars include polysaccharides such as cellulose, hemicellulose, agarose, chitin, chitosan, alginic acid, etc., disaccharides such as sucrose, lactose, maltose, trehalose, turanose, cellobiose, etc., trisaccharides such as raffinose, melezitose, maltotriose, etc., tetrasaccharides such as acarbose, stachyose, etc., and other oligosaccharides, monosaccharides such as glucose, xylose, fructose, mannose, galactose, etc., and one of these can be used alone or two or more can be used in combination. The physical strength of the textile product 1 is guaranteed by the fiber base material 10 regardless of the degree of polymerization of the sugars as the functional material 40. Therefore, sugars with a low degree of polymerization such as monosaccharides and oligosaccharides can also be used as the functional material 40.

[0065] In addition, when sugars are difficult to fix to the zirconium phosphate layer 30, a layer of a silane compound may be further formed on the zirconium phosphate layer 30. This generates alkoxy groups derived from the silane compound on the surface of the zirconium phosphate layer 30, which can be firmly bonded to the hydroxyl groups of the sugars.

[0066] In FIG. 1, the functional material 40 is fixed on the zirconium phosphate layer 30 in a granular form, but the present invention is not limited to the illustrated embodiment, and the functional material 40 can be fixed on the zirconium phosphate layer 30 in any shape. For example, the functional material 40 is not limited to the illustrated embodiment, and may be particles having a heterogeneous shape and particle size, or may be secondary particles formed by agglomeration of a plurality of primary particles. For example, the functional material 40 may be in a layered form. In this case, the functional material 40 may be intercalated with the zirconium phosphate layer 30, or may have a porous structure.

[0067] According to the present embodiment described above, the zirconium phosphate layer 30 is fixed to the fiber substrate 10 via the surface treatment layer 20, so that the zirconium phosphate layer 30 is firmly fixed to the fiber product 1. Therefore, detachment of the functional substance 40 due to peeling of the zirconium phosphate layer 30 is suppressed. As a result, the functional substance 40 can be firmly fixed to the fiber product 1.

[0068] In the above description of the present embodiment, the textile product 1 has been described as having the functional substance 40, but the textile product according to the present invention does not have to have a functional substance. In this case, the textile product is distributed and used, for example, as an intermediate member, and any type of functional substance can be fixed thereto afterwards as necessary.

[0069] <2. Manufacturing methods of textile products> Next, a method for producing a textile product according to this embodiment will be described. The method for producing a textile product according to the present embodiment includes a step of treating at least a portion of a surface of a textile substrate with a silane coupling agent to form a surface treatment layer on at least a portion of the surface of the textile substrate (surface treatment step); and forming a zirconium phosphate layer on the surface treatment layer (zirconium phosphate layer forming step), The silane coupling agent includes a silane compound having an amino group.

[0070] The manufacturing method according to the present embodiment includes a preparation step of preparing a fiber substrate prior to the surface treatment step, and a step (pretreatment step) of introducing hydroxyl groups and / or carboxyl groups to the surface of the fiber substrate. Furthermore, the manufacturing method according to the present embodiment includes a step (functional substance fixing step) of fixing a functional substance on the zirconium phosphate layer after the zirconium phosphate layer formation step. Hereinafter, an example of the manufacturing method of the fiber product according to the present embodiment will be described in detail, taking the manufacturing of the above-mentioned fiber product 1 as an example.

[0071] (2.1. Preparation process) First, in this step, a fiber base material 10 is prepared. Examples of the fiber base material 10 include various fiber materials that can be used as the above-mentioned fiber base material 10. Furthermore, the fiber base material 10 may be subjected to known processing and cleaning treatments as necessary.

[0072] (2.2. Pretreatment process) In this step, hydroxyl groups and / or carboxyl groups are introduced onto the surface of the fiber substrate 10. This allows the surface treatment layer 20 to be more strongly formed and fixed onto the surface of the fiber substrate 10 in the surface treatment step.

[0073] The method for introducing hydroxyl groups and / or carboxyl groups is not particularly limited, and examples thereof include oxidation of a compound constituting the surface of the fiber substrate 10, solvolysis of an amide group (peptide bond) or an ester group present on the surface of the fiber substrate 10, and adsorption / bonding of a compound having a hydroxyl group and / or a carboxyl group to the surface of the fiber substrate 10. These methods may be carried out alone or in combination of two or more of them.

[0074] Specific methods for oxidizing the compound that constitutes the surface of the fiber substrate 10 include oxidation treatment with an oxidizing agent, irradiation with electromagnetic waves, or a combination of these. In the oxidation treatment using an oxidizing agent, the surface of the fiber substrate 10 is treated in the presence of an oxidizing agent such as ozone, hydrogen peroxide, chlorine, chlorine dioxide, or perchloric acid. Preferably, the treatment is performed in the presence of a liquid medium such as an aqueous solution. A relatively high concentration of the oxidizing agent can be retained in the liquid medium, enabling a uniform and efficient oxidation reaction. In this case, the liquid medium may be alkaline, acidic, or neutral, and can be appropriately changed depending on the constituent material of the fiber substrate 10, the type of oxidizing agent, the desired degree of oxidation, and the like.

[0075] The electromagnetic waves that can be used for the irradiation of electromagnetic waves are not particularly limited, and ultraviolet light, visible light, etc. can be used. Among them, ultraviolet light is preferably used in consideration of the efficiency of oxidation. Moreover, the irradiation of electromagnetic waves can be carried out in an atmosphere in which oxygen is present, for example, in an air atmosphere. In this case, ozone is generated from oxygen present in the atmosphere by the electromagnetic waves, and the ozone reacts and bonds on the surface of the fiber base material 10 to generate hydroxyl groups or carboxyl groups.

[0076] The solvolysis of the amide group (peptide bond) or ester group present on the surface of the fiber substrate 10 can be carried out by treating the fiber substrate 10 in a solution containing an acid or a base. Solvolysis can be suitably used for decomposing nitrile groups and ester groups.

[0077] Examples of the acid include inorganic acids such as hydrochloric acid, sulfuric acid, nitric acid, phosphoric acid, etc., and one of these may be used alone or two or more may be used in combination. Examples of the base include sodium hydroxide, potassium hydroxide, sodium carbonate, potassium carbonate, ammonia, etc., and one of these may be used alone or two or more may be used in combination.

[0078] Examples of the medium for the solution include various organic solvents such as water and alcohol-based solvents. When water is used as the medium, hydrolysis can be performed. Alternatively, when an alcohol-based solvent is used as the medium, alcoholysis can be performed. In addition, examples of the alcohol-based solvent include, but are not limited to, methanol, ethanol, n-propyl alcohol, 2-methylpropyl alcohol, 1-butanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, ethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,3-butanediol, 1,4-butanediol, 2-ethylhexanol, and benzyl alcohol.

[0079] The adsorption and binding of a compound having a hydroxyl group and / or a carboxyl group to the surface of the fiber substrate 10 is suitable for introducing a hydroxyl group or a carboxyl group to the surface of a protein-based fiber such as wool, or animal hair such as cashmere or angora. Specifically, for example, polyphenols having three or more hydroxyl groups in one molecule, such as tannin, tannic acid, Chinese gallnut, gall nut, and gallic acid, can be reacted with the fiber substrate 10. In this case, for example, the fiber substrate 10 can be immersed in a 1 to 100 mM aqueous solution of the polyphenols (temperature: about 10 to 100° C.) for about 0.25 to 2 hours. The reaction amount of the polyphenols is preferably about 1 to 10% by weight based on the fiber substrate 10.

[0080] Among the above, the introduction of hydroxyl groups and / or carboxyl groups to the surface of the fiber substrate 10 is preferably carried out by oxidation or solvolysis of the compound constituting the surface of the fiber substrate 10. Such a method makes it easy to introduce hydroxyl groups and / or carboxyl groups regardless of the type of fiber substrate 10. In particular, it is relatively difficult to subsequently introduce hydroxyl groups, carboxyl groups, etc. into chemical fibers such as acrylic fibers, polyester fibers, polyolefin fibers, and polyvinyl chloride fibers, but the above method makes it possible to suitably introduce these functional groups.

[0081] This step may be omitted. Specifically, this step is omitted if the surface treatment layer 20 is suitably formed in the surface treatment step described below even if this step is omitted. For example, this step may be omitted if the fiber substrate 10 has a sufficient amount of hydroxyl groups or carboxyl groups on the surface. An example of such a fiber substrate 10 is a fiber substrate made of cellulose-based fibers.

[0082] (2.3. Surface treatment process) In this step, at least a part of the surface of the fiber substrate 10 is treated with a silane coupling agent to form a surface treatment layer 20 on a part of the surface of the fiber substrate 10. Specifically, in this step, the above-mentioned silane coupling agent is applied to the target surface of the fiber substrate 10 and reacted to form the surface treatment layer 20.

[0083] The method of applying the silane coupling agent to the fiber substrate 10 is not particularly limited, and the agent can be applied by immersion, spraying, coating, printing (e.g., inkjet printing, screen printing), etc. Among the above methods, immersion is preferred from the viewpoint of being able to apply the agent uniformly to the fiber substrate 10 having irregularities.

[0084] The immersion can be performed by immersing the fiber substrate 10 in a treatment liquid containing a silane coupling agent. As the silane coupling agent contained in the treatment liquid, the silane coupling agent constituting the surface treatment layer 30 described above can be used.

[0085] The treatment liquid preferably contains an organic solvent. This dilutes the concentration of the silane coupling agent, and the amount of the silane coupling agent attached to the fiber substrate 10 is adjusted. The organic solvent is not particularly limited as long as it can dissolve the silane coupling agent. For example, alcohol-based solvents such as methanol, ethanol, n-propyl alcohol, 2-methylpropyl alcohol, 1-butanol, 2-methoxyethanol, 2-ethoxyethanol, 1-methoxy-2-propanol, 1,3-butanediol, 1,4-butanediol, 2-ethylhexanol, and benzyl alcohol; ketone-based solvents such as acetone, methyl ethyl ketone, methyl propyl ketone, methyl isobutyl ketone, diethyl ketone, dipropyl ketone, diisobutyl ketone, cyclohexanone, and diacetone alcohol; dimethyl ether, diethyl ether, di-n-propyl ether, diisopropyl ether, di-n-butyl ether, di-t-butyl ether, t-butyl methyl ether, 1,4-dioxane, ethylene glycol monomethyl ether ... Examples of suitable solvents include ether-based solvents such as ethyl acetate, methyl acetate, butyl acetate, sec-butyl acetate, methoxybutyl acetate, amyl acetate, n-propyl acetate, isopropyl acetate, methyl lactate, ethyl lactate, and butyl lactate; carbonate-based solvents such as dimethyl carbonate, diethyl carbonate, and ethyl methyl carbonate; halogen-based solvents such as methylene chloride, trichloroethylene, perchloroethylene, 1-bromopropane, chloroform, and carbon tetrachloride; 2-pyrrolidone, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, dimethylformamide, dimethylacetamide, sulfolane, morpholine, acetonitrile, and propionitrile; and these can be used alone or in combination of two or more.

[0086] Among the above, the treatment liquid preferably contains, as an organic solvent, one or more selected from the group consisting of alcohol-based solvents and ether-based solvents, and more preferably one or more selected from the group consisting of ethanol, n-propyl alcohol, 2-methylpropyl alcohol, and 1-butanol.

[0087] The concentration of the silane coupling agent in the treatment liquid is, for example, from 0.1% by mass to 10% by mass, and preferably from 0.2% by mass to 1% by mass.

[0088] The immersion time of the fiber substrate 10 in the treatment liquid is not particularly limited, but is from 30 seconds to 30 minutes, preferably from 1 minute to 15 minutes, so that an appropriate amount of the silane coupling agent can be attached to the fiber substrate 10.

[0089] The reaction of the silane coupling agent on the fiber substrate 10 can be carried out, for example, by drying in the air. In this case, air drying may be performed, or drying may be performed while heating at a temperature of 30° C. or higher and 150° C. or lower.

[0090] (2.4. Zirconium phosphate layer formation process) In this step, a zirconium phosphate layer 30 is formed on the surface treatment layer 20. The zirconium phosphate layer 30 can be formed by applying a zirconium phosphate dispersion to the surface treatment layer 20 and fixing the zirconium phosphate on the surface treatment layer 20.

[0091] More specifically, first, zirconium phosphate is dispersed in a dispersion medium to prepare a zirconium phosphate dispersion. The zirconium phosphate dispersion is prepared, for example, by dispersing crystalline zirconium phosphate having a layered structure in a dispersion medium by shaking, and then ion-exchanging the dispersion with an alkaline agent such as a hydroxide of tetraalkylammonium (e.g., tetraalkylammonium having an alkyl group having 1 to 6 carbon atoms, specifically tetramethylammonium, tetraethylammonium, tetrapropylammonium, tetrabutylammonium, etc.) to obtain individual zirconium phosphate polymers ([Zr n (PO4) 2n ] 2n- ) can be obtained by exfoliating and dispersing it.

[0092] The method of applying the zirconium phosphate dispersion to the surface treatment layer 20 is not particularly limited, and can be performed by immersion, spraying, coating, printing (e.g., inkjet printing, screen printing), etc. Among the above methods, immersion is preferred from the viewpoint of uniformly applying the zirconium phosphate polymer. In addition, by performing immersion, it is possible to simultaneously fix the zirconium phosphate polymer to the surface treatment layer 20 and form the zirconium phosphate layer 30.

[0093] The time for immersing the fiber substrate 10 carrying the surface treatment layer 20 in the zirconium phosphate dispersion is not particularly limited, but is, for example, from 1 minute to 60 minutes, preferably from 2 minutes to 15 minutes.

[0094] The fiber substrate 10 may be heated during or after immersion in the zirconium phosphate dispersion. This allows the zirconium phosphate polymer to be fixed to the surface treatment layer 20.

[0095] The heating method is not particularly limited and any method can be adopted, but microwave irradiation is preferable. By irradiating microwaves, the zirconium phosphate polymer can be fixed to the surface treatment layer 20 in a short time. For example, microwaves of 1 GHz to 5 GHz can be used, and the zirconium phosphate dispersion can be irradiated with the microwaves for 5 seconds to 200 seconds to perform heating.

[0096] When an external heat source such as a heater is used, the temperature of the zirconium phosphate dispersion can be set to 5° C. or more and 60° C. or less, and the heating can be performed by maintaining this temperature for 1 minute or more and 60 minutes or less.

[0097] After the fiber substrate 10 is immersed in the zirconium phosphate dispersion, excess zirconium phosphate dispersion that has adhered or permeated between the fibers of the fiber substrate 10 may be removed. This reduces unevenness in the adsorption of the zirconium phosphate layer 30 and enhances the binding strength of the zirconium phosphate layer 30 to the surface treatment layer 20 and the functional material 40. The zirconium phosphate dispersion can be removed by, for example, washing with a liquid medium such as water or an organic solvent.

[0098] Thereafter, drying is performed as necessary to obtain the fiber substrate 10 having the zirconium phosphate layer 30 fixed onto the surface treatment layer 20. In this case, air drying may be performed, or drying may be performed while heating at a temperature of 30° C. or higher and 150° C. or lower.

[0099] When the zirconium phosphate dispersion is applied to the surface treatment layer 20 by a method other than immersion, the zirconium phosphate layer 30 is fixed to the surface treatment layer 20 by drying or heating after application.

[0100] (2.5.Functional substance fixation process) Finally, the functional substance 40 is fixed on the zirconium phosphate layer 30. In this way, a textile product 1 is obtained in which the functional substance 40 is fixed on the zirconium phosphate layer 30. The functional substance 40 can be fixed by applying the functional substance 40 to the zirconium phosphate layer 30.

[0101] Although the method of applying the functional material 40 to the zirconium phosphate layer 30 is not particularly limited, it is preferable to apply a treatment liquid in which the functional material 40 is dispersed or dissolved to the zirconium phosphate layer 30. This allows the functional material 40 to be applied relatively uniformly.

[0102] The dispersion medium or solvent for the functional substance 40 is not particularly limited and can be appropriately selected according to the chemical and physical properties of the functional substance 40. For example, the above-mentioned organic solvents, water, etc. can be used.

[0103] The immersion time of the fiber substrate 10 having the zirconium phosphate layer 30 in the treatment liquid is not particularly limited, but is, for example, from 1 minute to 120 minutes, preferably from 2 minutes to 15 minutes.

[0104] The fiber substrate 10 may be heated during or after immersion in the treatment liquid. This allows the functional substance 40 to be fixed to the zirconium phosphate layer 30 via a chemical bond, depending on the type of functional substance 40. For example, when a photocatalyst is used as the functional substance 40, the photocatalyst is fixed to the zirconium phosphate layer 30 by a chemical bond such as a covalent bond, a coordinate bond, a hydrogen bond, or an ionic bond.

[0105] The heating method is not particularly limited and any method can be adopted, but microwave irradiation is preferable. By irradiating microwaves, the functional material 40 can be fixed to the zirconium phosphate layer 30 via chemical bonds in a short time. For example, microwaves of 1 GHz to 5 GHz can be used, and the treatment liquid can be irradiated with the microwaves for 5 seconds to 300 seconds to perform heating.

[0106] When an external heat source such as a heater is used, heating can be performed by setting the temperature of the treatment liquid to 5° C. or more and 90° C. or less and maintaining this temperature for 5 minutes or more and 120 minutes or less.

[0107] Thereafter, drying is performed as necessary to obtain the textile product 1 having the functional substance 40 fixed on the zirconium phosphate layer 30. In this case, air drying may be performed, or drying may be performed while heating at a temperature of 40° C. or higher and 150° C. or lower.

[0108] As described above, according to this embodiment, the functional substance 40 can be firmly fixed to the surface, and a textile product 1 with excellent washing durability can be efficiently manufactured. In particular, in this embodiment, by forming the zirconium phosphate layer 30 on a specific surface treatment layer 20, the functional substance 40 can be firmly fixed to the zirconium phosphate layer 30 without forming multiple zirconium phosphate layers, unlike the conventional method. Therefore, the step of forming multiple zirconium phosphate layers can be omitted.

[0109] In particular, it has not been easy to selectively fix functional substances to the surface of chemical fibers such as acrylic fibers, polyester fibers, polyolefin fibers, and polyvinyl chloride fibers, and it has been common to previously mix the functional substances into the materials constituting the chemical fibers. However, in this embodiment, the functional substance 40 can be firmly fixed to the surface of the fiber substrate 10 via the surface treatment layer 20 and the zirconium phosphate layer 30.

[0110] In the above description, the method for producing a textile product according to this embodiment has been described as including a functional substance fixing step, but this step may be omitted.

[0111] The present invention has been described in detail above based on a preferred embodiment, but the present invention is not limited to this, and each component can be replaced with any component that can perform a similar function, or any component can be added. EXAMPLES

[0112] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0113] <1. Manufacturing methods of textile products> Example 1 (1.1. Fiber base material preparation process) First, a sample cloth of 5 cm square (approximately 0.6 g) was cut out from a polyester cloth (manufactured by HAP Corporation) and used as the fiber substrate.

[0114] (1.2. Pretreatment process) Next, the sample fabric was irradiated with ultraviolet light from a low-pressure mercury lamp (output: 6 W, wavelength: 254 nm) for 5 minutes under air-tight conditions.

[0115] (1.3. Surface treatment process) First, 2.1 g of aminopropyltriethoxysilane (manufactured by Shin-Etsu Chemical Co., Ltd., product name LS3150) was weighed out in a glove box and mixed with 200 ml of ethanol to obtain a treatment solution. After immersing the sample fabric in the treatment solution for 10 minutes, it was air-dried in the air.

[0116] (1.4. Zirconium phosphate layer formation process) 400 ml of distilled water was added to 0.043 g of α-zirconium phosphate (Daiichi Kigenso Kagaku Kogyo, product name: CZP-100), and 2 ml of 10% by mass tetrabutylammonium hydroxide aqueous solution was gradually added dropwise while stirring at a constant speed to obtain a zirconium phosphate dispersion. During stirring, the pH of the mixture was kept in the range of 8 to 9 while the 10% by mass tetrabutylammonium hydroxide aqueous solution was added.

[0117] The sample fabric was then immersed in the zirconium phosphate dispersion for 15 minutes, and then removed from the dispersion and irradiated with microwaves in a microwave oven (650 W, 2.45 GHz) for 3 minutes. The sample fabric was then rinsed three times with tap water and air-dried in the air.

[0118] (1.5.Functional substance fixation process) 20 mL of distilled water was added to 0.90 g of titanium oxide (Nippon Aerosil Co., Ltd., product name: P25) and ground in a planetary ball mill at 450 rpm for 15 minutes. 1 mL of the resulting suspension was then diluted with 450 mL of distilled water and stirred with a stirrer for 30 minutes to obtain a TiO2 treatment solution.

[0119] The sample fabric was then immersed in the TiO2 treatment solution for 15 minutes, then removed from the solution and irradiated with microwaves in a microwave oven (650 W, 2.45 GHz) for 3 minutes, rinsed with tap water three times, and air-dried in the air. In this manner, a textile product according to Example 1 was obtained. Note that a plurality of textile products according to Example 1 were produced for the purpose of evaluation, which will be described later.

[0120] Comparative Example 1 A sample cloth of 5 cm square (approximately 0.6 g) was cut out from a polyester cloth (manufactured by HAP Corporation).

[0121] <2. Evaluation> (2.1. Washing durability test) The textile product according to Example 1 was washed 5, 10, 20, 30, and 40 times. Specifically, the textile product according to Example 1 was first sewn to the corner of a piece of cloth measuring about 20 cm x 30 cm, and placed in a laundry net. Next, the textile product was repeatedly washed 5, 10, 20, 30, and 40 times in accordance with the standard washing method described in the washing method for SEK mark textile products by the Japan Textile Evaluation Technology Council. Specifically, the washing cycle was repeatedly performed according to the following procedure.

[0122] 1) The washing machine tub was filled with water at 40°C up to the top water level line, and 40ml of "JAFET standard detergent blend" was added to this for every 30L of water to create the washing liquid. 2) The samples (textile products according to Example 1 and Comparative Example 1) and, if necessary, load fabrics were added to this washing liquid so that the liquor ratio became 1:30, and a washing operation was carried out. 3) After 5 minutes of treatment, the operation was stopped and the sample and the loaded fabric were dehydrated in a spin dryer. The washing liquid was then replaced with fresh water at room temperature and rinsed for 2 minutes using the same bath ratio. 4) The sample and the loaded fabric were dehydrated, rinsed again for 2 minutes, and dehydrated. 5) The washing cycles 1) to 4) were repeated the specified number of times.

[0123] The textile products according to Example 1 and Comparative Example 1, which had not been washed and had been washed 5, 10, 20, 30, and 40 times, were cut into pieces of 5 cm x 2.5 cm, and 0.3 ml of a 24.5 μM methylene blue solution was dropped onto the pieces and then dried. Next, 0.3 ml of water was dropped onto the part where the methylene blue solution had been dropped to moisten the pieces, and the pieces were exposed to ultraviolet light (0.6 mWcm) from a black lamp (NEC20S BL-B, 20 W). -2 After irradiating the fiber with 120 minutes of UV light, the diffuse reflection and absorption spectrum of the fiber surface with adsorbed methylene blue was measured using a UV-visible spectrophotometer (Shimadzu Corporation, UV-2400PC, integrating sphere unit: ISR-2200 (inner diameter: 60 mm)). The results are shown in Figure 2.

[0124] Fig. 2 is a graph showing the results of a washing durability test of the textile products according to Example 1 and Comparative Example 1. As shown in Fig. 2, the textile product according to Example 1 has a higher decomposition rate of methylene blue in an unwashed state (0 times) compared to the textile product according to Comparative Example 1, and it was found that the supported titanium dioxide functions as a photocatalyst. Furthermore, even when the textile product according to Example 1 is washed more frequently, the decrease in the decomposition rate of methylene blue is suppressed, and it can be seen that titanium dioxide is firmly fixed to the fiber surface.

[0125] (2.2. Scanning Electron Microscopy) Using a scanning electron microscope (Hitachi High-Tech Corporation, "S 3000N"), the fiber surface of the sample fabric was observed after (a) the fiber substrate preparation step, (b) the surface treatment step, (c) the zirconium phosphate layer formation step, and (d) the functional substance fixing step in Example 1. The results are shown in Figure 3.

[0126] Figure 3 shows scanning electron microscope images of the fiber surface after each step of the manufacturing method of the fiber product according to the present embodiment. As shown in Figure 3(b), compared to the untreated state (Figure 3(a)), the surface treatment layer with the silane coupling agent had irregularities of about 1 μm and was a layer covering the fiber substrate with irregularly shaped particles of 5 μm or less. The thickness of this surface treatment layer was estimated to be about 1 μm at most.

[0127] Furthermore, as shown in Figure 3(c), when the zirconium phosphate layer was formed, the unevenness derived from the surface treatment layer was no longer observed. After the functional substance fixing process, it was observed that titanium dioxide aggregates with sizes of about 200 nm to 1 μm were fixed, as shown in Figure 3(d).

[0128] (3.3. Energy dispersive X-ray microfluorescence analysis) The surfaces of the textile products according to Example 1 and Comparative Example 1 were observed using an energy dispersive X-ray microfluorescence analyzer (Shimadzu Corporation, model name: μEDX-1300). The results are shown in Fig. 4. Fig. 4(a) shows the EDX spectrum of the textile product according to Comparative Example 1, and Fig. 4(b) shows the EDX spectrum of the textile product according to Example 1.

[0129] When the untreated textile product according to Comparative Example 1 was observed, as shown in FIG. 4(a), TiK α The peak due to TiK is around 4.97 keV. β The peaks were observed due to titanium oxide, which was added to the polyester fabric (manufactured by HAP Corporation) as the fiber substrate to impart opacity. On the other hand, when the fiber product according to Example 1 was observed, as shown in FIG. 4(a), a TiK α The peak due to TiK is around 4.97 keV. βThe peaks derived from the titanium oxide particles were observed to be significantly larger than those in the textile product according to Comparative Example 1. This proves that in the textile product according to Example 1, titanium oxide is bound to the outermost layer of the textile product.

[0130] <3. Manufacturing methods of textile products> For the purpose of comparing a textile product in which a zirconium phosphate layer is formed using aluminum ions with a textile product according to the present disclosure, the following textile products were manufactured and prepared.

[0131] Example 2 In the same manner as in Example 1, a textile product according to Example 2 was produced.

[0132] Comparative Example 2 First, a sample cloth of 5 cm square (approximately 0.6 g) was cut from polyester cloth (manufactured by HAP Co., Ltd.) and used as the fiber substrate. Next, the sample cloth was washed with tap water and a neutral detergent, rinsed twice with tap water, centrifuged for dehydration, and then air-dried in the air.

[0133] Next, the sample fabric was irradiated with ultraviolet light from a low-pressure mercury lamp (output: 6 W, wavelength: 254 nm) for 5 minutes under air-tight conditions.

[0134] Next, the sample fabric was immersed in 15 ml of 3.67 mM potassium aluminum sulfate aqueous solution for 10 minutes, then rinsed twice with tap water and centrifuged for dehydration. The potassium aluminum sulfate used was a product manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0135] Next, 400 ml of distilled water was added to 0.043 g of α-zirconium phosphate (Daiichi Kigenso Kagaku Kogyo, product name: CZP-100), and 2 ml of 10% by mass tetrabutylammonium hydroxide aqueous solution was gradually added dropwise while stirring at a constant speed to obtain a zirconium phosphate dispersion. During stirring, the pH of the mixture was kept in the range of 8 to 9 while the 10% by mass tetrabutylammonium hydroxide aqueous solution was added. Thereafter, the sample fabric was immersed in the zirconium phosphate dispersion for 10 minutes, after which the sample fabric was rinsed twice with tap water and centrifuged for dehydration.

[0136] Next, the sample fabric was immersed in the titanium oxide treatment solution prepared in 1.5 above for 10 minutes, and then rinsed twice with tap water and centrifuged for dehydration. In this manner, a textile product according to Comparative Example 2 was obtained.

[0137] Comparative Example 3 First, a sample cloth of 5 cm square (approximately 0.6 g) was cut out from a polyester cloth (manufactured by HAP Corporation) and used as the fiber substrate. Next, the sample fabric was washed with tap water and a neutral detergent, rinsed twice with tap water, centrifuged for dehydration, and then air-dried in the air.

[0138] Next, the sample fabric was immersed in 15 ml of 3.67 mM potassium aluminum sulfate aqueous solution for 10 minutes, then rinsed twice with tap water and centrifuged for dehydration. The potassium aluminum sulfate used was a product manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.

[0139] Next, 400 ml of distilled water was added to 0.043 g of α-zirconium phosphate (Daiichi Kigenso Kagaku Kogyo, product name: CZP-100), and 2 ml of 10% by mass tetrabutylammonium hydroxide aqueous solution was gradually added dropwise while stirring at a constant speed to obtain a zirconium phosphate dispersion. During stirring, the pH of the mixture was kept in the range of 8 to 9 while the 10% by mass tetrabutylammonium hydroxide aqueous solution was added.

[0140] Next, the sample fabric was immersed in the prepared zirconium phosphate dispersion for 10 minutes, after which the sample fabric was rinsed twice with tap water and centrifuged for spin-drying.

[0141] Next, the sample fabric was immersed in the titanium oxide treatment solution prepared in 1.5 above for 10 minutes, and then rinsed twice with tap water and centrifuged for dehydration. In this manner, a textile product according to Comparative Example 3 was obtained.

[0142] Comparative Example 4 A sample cloth of 5 cm square (approximately 0.6 g) was cut out from a polyester cloth (manufactured by HAP Corporation), washed with tap water and a neutral detergent, rinsed twice with tap water, centrifuged for dehydration, and then air-dried in the air. This was the textile product according to Comparative Example 4.

[0143] <4. Evaluation> (4.1. Photocatalytic activity evaluation) For the textile product of Example 2 and the textile products of Comparative Examples 2 and 3, 0.3 ml of a 24.5 μM methylene blue solution was dropped onto the center of a 5 cm × 5 cm sample fabric and dried. Next, 0.3 ml of water was dropped onto the part where the methylene blue solution had been dropped to moisten it, and the sample was exposed to ultraviolet light (0.5 mWcm) from a black lamp (NEC20S BL-B, 20 W). -2 After irradiating the fiber with UV light for 120 minutes, the diffuse reflection and absorption spectrum of the fiber surface with adsorbed methylene blue was measured using a UV-visible spectrophotometer (Shimadzu Corporation, UV-2400PC, integrating sphere unit: ISR-2200 (inner diameter: 60 mm)). The decomposition rate of methylene blue was calculated from the diffuse reflection and absorption spectra before and after UV irradiation. The results are shown in Table 1.

[0144] (4.2. Washing durability test) The textile products according to Example 2 and Comparative Example 2 were washed 40 times by the method described in 2.1. Then, photocatalytic activity was evaluated by the same method as described in 4.1. The decomposition rate of methylene blue was calculated from the diffuse reflectance absorption spectrum before and after ultraviolet irradiation. The results are shown in Table 1.

[0145] [Table 1]

[0146] As shown in Table 1, the textile product of Example 2 had a higher decomposition rate of methylene blue both before and after washing, and exhibited significant photocatalytic activity, compared to the textile products of Comparative Examples 2 and 3. This suggests that when a zirconium phosphate layer is formed via a surface treatment layer formed with a silane coupling agent containing a silane compound having an amino group, a larger amount of titanium oxide can be supported, and the supported titanium oxide can be more firmly retained even during washing, compared to when a zirconium phosphate layer is formed via aluminum ions.

[0147] In addition, the textile product according to Comparative Example 2 had a higher decomposition rate of methylene blue before washing compared to Comparative Examples 3 and 4, and showed significant photocatalytic activity. This suggests that the affinity of the textile product according to Comparative Example 2 with aluminum ions is increased by the irradiation of the PET fiber surface of the textile substrate with ultraviolet light, and the amount of zirconium phosphate and subsequent titanium oxide supported is increased compared to the PET fiber of the textile substrate with no surface treatment shown in Comparative Example 3. However, after washing, the washing durability of the textile product according to Comparative Example 2 is significantly reduced, confirming that the washing durability is significantly lower than that of Example 2. Note that methylene blue absorbs ultraviolet light to a certain extent, and a certain amount is decomposed even by irradiation of ultraviolet light alone. For this reason, decomposition of methylene blue was observed even in the textile product according to Comparative Example 4, which does not support either zirconium phosphate or titanium oxide.

[0148] The decomposition rate before washing of the textile product of Comparative Example 3 was further decreased compared to Comparative Example 2. From this, it is presumed that the amount of titanium oxide supported on the textile product of Comparative Example 3 is even smaller.

[0149] The textile product of Example 2 showed a significantly higher decomposition rate of methylene blue even after washing than the textile product of Comparative Example 4 before washing. This suggested that the textile product of Example 2 still supported titanium oxide even after washing. On the other hand, the textile products of Comparative Examples 2 and 3 showed a decomposition rate of methylene blue after washing that was equal to or lower than the decomposition rate of methylene blue of the textile product of Comparative Example 4 before washing. This suggested that the textile products of Comparative Examples 2 and 3 no longer supported titanium oxide after washing. [Explanation of symbols]

[0150] 1. Textile products 10. Fiber substrate 20 Surface treatment layer 30 Zirconium phosphate layer 40 Functional substances

Claims

1. A fiber base material; A surface treatment layer formed of a silane coupling agent and fixed by a covalent bond to at least a portion of the surface of the fiber substrate; a zirconium phosphate layer fixed on the surface treatment layer; a functional substance electrostatically or chemically fixed to the surface of the zirconium phosphate layer via the phosphate group; the silane coupling agent contains a silane compound having an amino group, The functional substance includes a photocatalyst, a protein, or a sugar. Textile products.

2. The fiber substrate has a hydroxyl group and / or a carboxyl group on its surface, The textile product according to claim 1 , wherein the surface treatment layer is fixed to the textile substrate via the hydroxyl groups and / or the carboxyl groups.

3. The textile product according to claim 1 or 2, wherein the textile base material comprises a polyester fiber.

4. The textile product according to any one of claims 1 to 3, wherein the silane coupling agent comprises an aminoalkyltrialkoxysilane.

5. The textile product according to any one of claims 1 to 4, wherein the functional substance comprises titanium oxide.

6. The textile product according to any one of claims 1 to 5, wherein the functional substance comprises sericin.

7. The textile product according to any one of claims 1 to 6, wherein the functional substance comprises cellulose.

8. A step of treating at least a portion of a surface of a fiber substrate with a silane coupling agent to form a surface treatment layer fixed by a covalent bond to at least a portion of the surface of the fiber substrate; forming a zirconium phosphate layer on the surface treatment layer; and electrostatically or chemically immobilizing a functional substance on the zirconium phosphate layer via a phosphate group, the silane coupling agent contains a silane compound having an amino group, The method for producing a textile product, wherein the functional substance includes a photocatalyst, or a protein or a sugar.

9. The method for producing a textile product according to claim 8, further comprising a step of introducing hydroxyl groups and / or carboxyl groups into the surface of the textile base material prior to the step of forming the surface treatment layer.

Citation Information

Patent Citations

  • Flame-retardant composition and application thereof in polyester fabric

    CN111188192A

  • Functional fiber fabric

    JP2001040574A

  • Fibrous product having photocatalyst, and method for producing the same

    JP2010185158A

  • Allergen-reducing processing agent for fiber products

    JP2011246866A

  • Substrate for electronic device

    JP2012240356A