Nonaqueous electrolyte secondary battery and method for manufacturing the same
By stacking electrodes with varying density patterns and injecting electrolyte from high to low density regions, the battery achieves even electrolyte distribution, addressing impregnation challenges and maintaining performance.
Patent Information
- Application Number
- JP2021561291
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-29
- Filing Date
- 2020-11-12
- Publication Date
- 2024-10-18
- Estimated Expiration
- 2040-11-12
AI Technical Summary
Existing non-aqueous electrolyte secondary batteries face challenges in evenly impregnating the electrode body with electrolyte, leading to uneven battery reactions and performance deterioration due to variations in electrolyte amount, particularly when grooves or low-density portions are used, which can reduce active material capacity.
The battery design alternately stacks positive and negative electrodes with separators, forming composite layers with varying densities, where the density away from the electrolyte injection point is lower than near it, allowing electrolyte to evenly distribute by injecting from the high-density to low-density regions.
This design ensures complete and even impregnation of the electrode body with non-aqueous electrolyte, preventing uneven reactions and performance deterioration, while maintaining or enhancing capacity by optimizing electrolyte distribution.
Smart Images

Figure 0007569801000003 
Figure 0007569801000004 
Figure 0007569801000005
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a nonaqueous electrolyte secondary battery and a method for manufacturing a nonaqueous electrolyte secondary battery. [Background technology]
[0002] Conventionally, non-aqueous electrolyte secondary batteries are widely known, which include an electrode assembly including a positive electrode, a negative electrode, and a separator, a non-aqueous electrolyte, and an exterior body that contains them. For example, Patent Document 1 discloses a cylindrical non-aqueous electrolyte secondary battery that includes a wound electrode assembly in which a positive electrode and a negative electrode are wound in a spiral shape with a separator interposed therebetween. In the non-aqueous electrolyte secondary battery of Patent Document 1, grooves are formed in at least one of the composite layers of the positive electrode and the negative electrode in order to improve the impregnation of the non-aqueous electrolyte in the electrode assembly and thereby improve the charge-discharge cycle characteristics of the battery.
[0003] Patent Document 2 discloses a cylindrical nonaqueous electrolyte secondary battery in which a low-density portion that is lower in density than other regions is formed along the axial direction of a wound electrode body in at least one of the composite layers of the positive electrode and the negative electrode. Patent Document 2 describes that the impregnation of the nonaqueous electrolyte is improved by providing a low-density portion in a part of the composite layer. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2001-176558 A [Patent Document 2] JP 2018-137187 A Summary of the Invention
[0005] Incidentally, the non-aqueous electrolyte is generally injected into the exterior body through an injection part provided in the exterior body after the electrode body is housed inside the exterior body. In this case, it is an important issue to impregnate the entire electrode body with the non-aqueous electrolyte. In this regard, the techniques disclosed in Patent Documents 1 and 2 still have room for improvement. In addition, in the non-aqueous electrolyte secondary battery of Patent Document 1, the amount of active material in the composite layer is reduced by forming a groove in the composite layer, so there is a problem in increasing the capacity of the battery.
[0006] The nonaqueous electrolyte secondary battery according to the present disclosure is a nonaqueous electrolyte secondary battery including an electrode assembly in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with separators interposed therebetween, a nonaqueous electrolyte, and an exterior body that contains the electrode assembly and the nonaqueous electrolyte, wherein the exterior body is provided with a liquid injection section for injecting the nonaqueous electrolyte, the plurality of positive electrodes include a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, and the plurality of negative electrodes include a negative electrode core and a negative electrode mixture layer formed on the surface of the negative electrode core, and the density of a first region away from the liquid injection section in at least one of the positive electrode mixture layer and the negative electrode mixture layer is lower than the density of a second region close to the liquid injection section.
[0007] A method for manufacturing a nonaqueous electrolyte secondary battery according to the present disclosure is a method for manufacturing a nonaqueous electrolyte secondary battery including an electrode assembly in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with separators interposed therebetween, a nonaqueous electrolyte solution, and an exterior body, the method including the steps of forming the positive electrode composite layer on a surface of a positive electrode core body to fabricate the positive electrode, forming the negative electrode composite layer on a surface of a negative electrode core body to fabricate the negative electrode, fabricating the electrode body using the plurality of positive electrodes and the plurality of negative electrodes, and housing the electrode body inside the exterior body and then injecting the nonaqueous electrolyte solution, characterized in that in at least one of the steps of forming the positive electrode composite layer and the negative electrode composite layer, the composite layer is formed such that the density of a region located on a first end side of the composite layer is lower than the density of a region located on a second end side opposite to the first end, and in the step of injecting the nonaqueous electrolyte solution, the nonaqueous electrolyte solution is injected into the interior of the exterior body from the second end side.
[0008] According to the nonaqueous electrolyte secondary battery of the present disclosure, when the nonaqueous electrolyte is injected into the exterior body, the entire electrode body can be impregnated with the nonaqueous electrolyte, and the nonaqueous electrolyte can be distributed evenly throughout the entire electrode body. For example, if the amount of electrolyte in the electrode body varies widely, the battery reaction becomes nonuniform, which can cause performance degradation. However, according to the nonaqueous electrolyte secondary battery of the present disclosure, the occurrence of such a problem can be suppressed. [Brief description of the drawings]
[0009] [Figure 1] FIG. 1 is a perspective view showing the appearance of a nonaqueous electrolyte secondary battery according to an embodiment. [Diagram 2] FIG. 2 is a perspective view of an electrode body and a sealing plate according to an example of the embodiment. [Diagram 3] FIG. 3 is an exploded perspective view of an electrode assembly according to an embodiment. [Figure 4] FIG. 4 is a cross-sectional view showing a part of an electrode assembly according to an embodiment, and a front view of a positive electrode. [Diagram 5] FIG. 5 is a diagram for explaining a manufacturing process of a positive electrode according to an embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an example of an embodiment of the present disclosure will be described in detail with reference to the drawings. It is assumed from the beginning that the following embodiments and modified examples will be selectively combined. In addition, in this specification, the expression "numerical value A to numerical value B" means "numerical value A or more and numerical value B or less" unless otherwise specified.
[0011] Fig. 1 is a perspective view showing the appearance of a nonaqueous electrolyte secondary battery 10 according to an embodiment, and Fig. 2 is a perspective view (showing a state in which an outer can 14 has been removed) of an electrode assembly 11 and a sealing plate 15 constituting the nonaqueous electrolyte secondary battery 10. The nonaqueous electrolyte secondary battery 10 shown in Fig. 1 has a rectangular container including an outer can 14 and a sealing plate 15 as an exterior body, but the exterior body is not limited thereto and may be, for example, an exterior body formed of a laminate sheet including a metal layer and a resin layer.
[0012] As illustrated in Figs. 1 and 2, the nonaqueous electrolyte secondary battery 10 includes an electrode assembly 11, a nonaqueous electrolyte, a bottomed rectangular cylindrical exterior can 14 that contains the electrode assembly 11 and the nonaqueous electrolyte, and a sealing plate 15 that closes the opening of the exterior can 14. The nonaqueous electrolyte secondary battery 10 is a so-called prismatic battery. The electrode assembly 11 is a laminated electrode assembly in which a plurality of positive electrodes 20 and a plurality of negative electrodes 30 are alternately laminated one by one with separators 40 interposed therebetween (see Fig. 3 described later for details). The exterior can 14 is a flattened, approximately rectangular parallelepiped metal container with one axial end open, and the sealing plate 15 has an elongated rectangular shape. The exterior can 14 and the sealing plate 15 are made of, for example, a metal material mainly composed of aluminum.
[0013] For ease of explanation, the height direction of the exterior can 14 will be referred to as the "vertical direction" of the nonaqueous electrolyte secondary battery 10, the sealing plate 15 side will be referred to as the "top", and the bottom side of the exterior can 14 will be referred to as the "bottom". In addition, the direction along the longitudinal direction of the sealing plate 15 will be referred to as the "lateral direction" of the nonaqueous electrolyte secondary battery 10.
[0014] The non-aqueous electrolyte solution includes, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. The non-aqueous solvent may be, for example, esters, ethers, nitriles, amides, or a mixture of two or more of these. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is replaced with a halogen atom such as fluorine. The electrolyte salt may be, for example, a lithium salt such as LiPF6.
[0015] The nonaqueous electrolyte secondary battery 10 includes a positive electrode terminal 12 electrically connected to the positive electrode 20 via a positive electrode current collector (not shown), and a negative electrode terminal 13 electrically connected to the negative electrode 30 via a negative electrode current collector (not shown). In this embodiment, the positive electrode terminal 12 is disposed at one end in the longitudinal direction of the sealing plate 15, and the negative electrode terminal 13 is disposed at the other end in the longitudinal direction of the sealing plate 15. The positive electrode terminal 12 and the negative electrode terminal 13 are external connection terminals electrically connected to other nonaqueous electrolyte secondary batteries 10, circuits, devices, etc., and are attached to the sealing plate 15 via insulating members.
[0016] The sealing plate 15 constituting the exterior body is provided with a liquid injection section 16 for injecting a non-aqueous electrolyte into the exterior can 14 in which the electrode body 11 is housed. As will be described in detail later, the non-aqueous electrolyte is injected from the liquid injection section 16 after the electrode body 11 is housed in the exterior can 14 and the opening of the exterior can 14 is closed with the sealing plate 15. The liquid injection section 16 is composed of, for example, a through hole formed in the sealing plate 15 and a rubber seal member that closes the through hole. In addition, the sealing plate 15 is provided with a gas exhaust valve 17 that opens to exhaust gas when an abnormality occurs in the battery, and a current interruption mechanism 18 that interrupts the current path when an abnormality occurs.
[0017] 1, a liquid injection part 16 and a gas exhaust valve 17 are provided between the positive electrode terminal 12 and the negative electrode terminal 13. The gas exhaust valve 17 is disposed in the longitudinal center of the sealing plate 15, and the liquid injection part 16 is disposed between the positive electrode terminal 12 and the gas exhaust valve 17. A current interrupt mechanism 18 is disposed on the back side of the positive electrode terminal 12.
[0018] As illustrated in FIG. 2, the electrode body 11 is divided into a first electrode group 11A and a second electrode group 11B. The first electrode group 11A and the second electrode group 11B have, for example, the same laminated structure and dimensions, and are laminated in the thickness direction of the electrode body 11. At the upper end of each electrode group, a plurality of positive electrode tabs 23 and a plurality of negative electrode tabs 33 extending toward the sealing plate 15 are formed. Each tab is a convex portion in which a composite layer, which will be described later, is not formed and the core surface is exposed. The positive electrode tab 23 is electrically connected to the positive electrode terminal 12 via the positive electrode current collector, and the negative electrode tab 33 is electrically connected to the negative electrode terminal 13 via the negative electrode current collector. The outer peripheral surface of each electrode group is covered with a separator 40.
[0019] FIG. 3 is an exploded perspective view of the electrode assembly 11. As illustrated in FIG. 3, the electrode assembly 11 includes a plurality of positive electrodes 20 and a plurality of negative electrodes 30. Each electrode group constituting the electrode assembly 11 includes, for example, one more negative electrode 30 than the positive electrode 20, and the negative electrode 30 is disposed on both sides of each electrode group in the thickness direction. FIG. 3 illustrates a plurality of separators 40 disposed one by one between the positive electrode 20 and the negative electrode 30, but each electrode group may include only one separator 40. In this case, the long separator 40 is folded zigzag and disposed between the positive electrode 20 and the negative electrode 30.
[0020] As described above, the electrode body 11 has a structure in which a plurality of positive electrodes 20 and a plurality of negative electrodes 30 are alternately stacked one by one with separators 40 interposed therebetween. The positive electrodes 20 and the negative electrodes 30 each include a positive electrode tab 23 and a negative electrode tab 33 protruding upward. In other words, the positive electrodes 20 and the negative electrodes 30 are stacked and arranged so that the tabs face the same direction. In addition, the positive electrode tab 23 is located at one lateral end side of the electrode body 11, the negative electrode tab 33 is located at the other lateral end side of the electrode body 11, and the positive electrode tabs 23 are arranged in the thickness direction of the electrode body 11, and the negative electrode tabs 33 are arranged in the thickness direction of the electrode body 11.
[0021] 4 is a cross-sectional view showing a part of the electrode body 11 and a front view of the positive electrode 20. As illustrated in FIG. 4, the positive electrode 20 includes a positive electrode core 21 and a positive electrode mixture layer 22 formed on the surface of the positive electrode core 21. The positive electrode mixture layer 22 is formed on both sides of the positive electrode core 21. Similarly, the negative electrode 30 includes a negative electrode core 31 and a negative electrode mixture layer 32 formed on the surface of the negative electrode core 31. The negative electrode mixture layer 32 is formed on both sides of the negative electrode core 31. The negative electrode 30 is one size larger than the positive electrode 20, and the negative electrode mixture layer 32 is disposed to face the range where the positive electrode mixture layer 22 of the positive electrode 20 is formed.
[0022] Hereinafter, the configurations of the positive electrode 20 and the negative electrode 30, in particular the configurations of the positive electrode mixture layer 22 and the negative electrode mixture layer 32, will be described in detail.
[0023] [Positive electrode] The positive electrode 20 has a structure in which a positive electrode composite layer 22 is formed on the entire surface of a positive electrode core 21 except for a positive electrode tab 23 (hereinafter referred to as a "base"). For the positive electrode core 21, a foil of a metal such as aluminum that is stable in the battery operating voltage range, or a film having the metal disposed on the surface layer, can be used. The thickness of the positive electrode core 21 is, for example, 5 μm to 20 μm, and preferably 8 μm to 15 μm. The base of the positive electrode core 21 has a rectangular shape when viewed from the front, and the positive electrode tab 23 protrudes from one side of the rectangle. In general, the positive electrode core 21 in which the base and the positive electrode tab 23 are integrally formed is obtained by processing one sheet of metal foil.
[0024] The positive electrode mixture layer 22 contains, for example, a positive electrode active material, a conductive material, and a binder, and is formed on both sides of the base of the positive electrode core 21. The positive electrode mixture layer 22 may be formed at the base of the positive electrode tab 23. The thickness of the positive electrode mixture layer 22 is, for example, 40 μm to 120 μm, and preferably 50 μm to 80 μm, on one side of the positive electrode core 21. The positive electrode 20 can be produced by applying a positive electrode mixture slurry containing a positive electrode active material, a conductive material, a binder, and the like onto the positive electrode core 21, drying and compressing the coating to form the positive electrode mixture layer 22 on both sides of the positive electrode core 21, and then cutting into a predetermined shape.
[0025] A lithium transition metal composite oxide is used as the positive electrode active material. Metal elements contained in the lithium transition metal composite oxide include Ni, Co, Mn, Al, B, Mg, Ti, V, Cr, Fe, Cu, Zn, Ga, Sr, Zr, Nb, In, Sn, Ta, W, etc. Among them, it is preferable to contain at least one of Ni, Co, and Mn. Examples of suitable composite oxides include lithium transition metal composite oxides containing Ni, Co, and Mn, and lithium transition metal composite oxides containing Ni, Co, and Al.
[0026] The volume-based median diameter (hereinafter, "D50") of the positive electrode active material is, for example, 2 μm to 30 μm. The volume-based D50 means a particle diameter at which the cumulative frequency is 50% from the smallest particle diameter in the volume-based particle size distribution, and is also called the median diameter. The D50 can be measured using a laser diffraction type particle size distribution measuring device (for example, Microtrack HRA, manufactured by Nikkiso Co., Ltd.) with water as the dispersion medium.
[0027] Examples of the conductive material contained in the positive electrode mixture layer 22 include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode mixture layer 22 include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide resins, acrylic resins, and polyolefin resins. These resins may also be used in combination with cellulose derivatives such as carboxymethylcellulose (CMC) or a salt thereof, and polyethylene oxide (PEO).
[0028] In the positive electrode 20, the positive electrode core 21 may be provided with a protective layer (not shown) adjacent to the positive electrode composite layer. The protective layer extends in a strip shape along the longitudinal direction of the positive electrode core 21. The protective layer has a function of preventing the negative electrode 30 from shorting with the positive electrode core 21 when the positive electrode 20 faces the negative electrode 30 via the separator 40 to form an electrode body. The protective layer includes, for example, inorganic material particles such as ceramics and a resin binder. The thickness of the protective layer formed on both sides of the positive electrode core 21 is, for example, 70 μm. In this embodiment, the positive electrode core 21 of the positive electrode 20 includes the positive electrode core 21 on which the protective layer is formed. In this embodiment, the protective layer is not an essential component and may be omitted.
[0029] The density of the positive electrode mixture layer 22 is not uniform, and it can have a high density region and a low density region. Specifically, the density of a first region away from the liquid injection part 16 is lower than the density of a second region close to the liquid injection part 16. That is, a low density region is formed in a portion of the positive electrode mixture layer 22 away from the liquid injection part 16, and a high density region is formed in a portion close to the liquid injection part 16. When the density of the positive electrode mixture layer is uniform, the nonaqueous electrolyte is less likely to penetrate into the first region away from the liquid injection part 16, but by lowering the density of the first region, the first region is more likely to be impregnated with the nonaqueous electrolyte.
[0030] In this embodiment, the liquid injection part 16 is provided at a position between the positive electrode terminal 12 and the gas exhaust valve 17 of the sealing plate 15 and overlapping with the positive electrode tab 23 in the vertical direction. For this reason, the density of the positive electrode mixture layer 22 may be highest in the vicinity of the positive electrode tab 23 and may decrease as it moves away from the positive electrode tab 23. However, from the viewpoint of productivity of the positive electrode 20, it is preferable that the density of the positive electrode mixture layer 22 is substantially constant along the lateral direction. In other words, it is preferable that the density of the positive electrode mixture layer 22 changes in the vertical direction, with the upper end side of the positive electrode mixture layer 22 close to the liquid injection part 16 being high density and the lower end side of the positive electrode mixture layer 22 away from the liquid injection part 16 being low density.
[0031] When the positive electrode mixture layer 22 is divided into thirds from the sealing plate 15 side toward the bottom side of the outer casing can 14 (the positive electrode mixture layer 22 formed at the base of the positive electrode core 21 is divided into thirds in the vertical direction), and the third region is defined as a second region 22B, an intermediate region 22C, and a first region 22A, in that order from the sealing plate 15 side, it is preferable that the density of the positive electrode mixture layer 22 satisfies the following relationship:
[0032] Density ρ of second region 22B 22B >Density ρ of intermediate region 22C 22C >Density ρ of the first region 22A 22A density ρ 22A is the density ρ 22C Lower, density ρ 22C is the density ρ 22B By forming such a density pattern in positive electrode mixture layer 22, it becomes possible to distribute the nonaqueous electrolyte evenly throughout electrode body 11 when the nonaqueous electrolyte is injected through injection part 16 provided in sealing plate 15.
[0033] The density of the positive electrode mixture layer 22 can be calculated from the specified area, the mass of the positive electrode mixture layer 22, and the average thickness of the positive electrode mixture layer 22, where the mass of the positive electrode mixture layer 22 is the mass of the positive electrode 20 with a specified area minus the mass of the positive electrode core 21 (the same applies to the density of the negative electrode mixture layer 32). 22B ,ρ 22C ,ρ 22A When measuring each of the density, positive electrode mixture layer 22 formed on the base of positive electrode core 21 may be divided into three equal parts in the vertical direction and used as sample pieces for density measurement.
[0034] The density of the positive electrode mixture layer 22 may decrease stepwise from the upper end to the lower end of the positive electrode mixture layer 22, or may change abruptly at the boundaries between the second region 22B, the intermediate region 22C, and the first region 22A. In this case, the density of each region may be constant throughout the entire region. The thickness of the positive electrode mixture layer 22 may change stepwise together with the density of the positive electrode mixture layer 22. For example, the thickness may increase stepwise from the upper end to the lower end of the positive electrode mixture layer 22 within a range that does not affect the battery performance.
[0035] The density of the positive electrode mixture layer 22 may change stepwise as described above, but preferably it gradually decreases from the upper end to the lower end of the positive electrode mixture layer 22. That is, it is preferable that the positive electrode mixture layer 22 does not have a boundary where the density changes abruptly. For example, there is no abrupt density difference at the boundary between the second region 22B, the intermediate region 22C, and the first region 22A, and the density of each region gradually decreases from the upper end to the lower end of each region. By forming a gradual density change in the vertical direction of the positive electrode mixture layer 22, the electrolyte moves more smoothly. In addition, the thickness of the positive electrode mixture layer 22 may gradually increase from the upper end to the lower end within a range that does not affect the battery performance.
[0036] The density pattern of the positive electrode mixture layer 22 may be applied only to the positive electrode mixture layer 22 formed on one side of the positive electrode core 21, but from the viewpoint of uniformity of the battery reaction, it is preferable that the density pattern be applied to each of the positive electrode mixture layers 22 formed on both sides of the positive electrode core 21. In addition, it is preferable that the density patterns are the same in both positive electrode mixture layers 22. The density pattern of the positive electrode mixture layer 22 is preferably applied to all of the positive electrodes 20 constituting the electrode body 11.
[0037] [Negative electrode] The negative electrode 30 has a structure in which a negative electrode composite layer 32 is formed on the entire area of the base, which is the portion of the surface of a negative electrode core 31 excluding a negative electrode tab 33. For the negative electrode core 31, a foil of a metal such as copper that is stable in the battery operating voltage range, or a film having such a metal disposed on the surface layer, can be used. The thickness of the negative electrode core 31 is, for example, 3 μm to 15 μm, and preferably 5 μm to 10 μm. As in the case of the positive electrode 20, the base of the negative electrode core 31 has a rectangular shape when viewed from the front, and the negative electrode tab 33 protrudes from one side of the rectangle.
[0038] The negative electrode mixture layer 32 contains, for example, a negative electrode active material and a binder, and is formed on both sides of the base of the negative electrode core 31. The negative electrode mixture layer 32 may be formed at the base of the negative electrode tab 33. The thickness of the negative electrode mixture layer 32 is, for example, 40 μm to 120 μm, and preferably 50 μm to 80 μm, on one side of the negative electrode core 31. The negative electrode 30 can be produced by applying a negative electrode mixture slurry containing a negative electrode active material and a binder, etc., onto the negative electrode core 31, drying and compressing the coating to form the negative electrode mixture layer 32 on both sides of the negative electrode core 31, and then cutting into a predetermined shape.
[0039] As the negative electrode active material, for example, a carbon-based active material that reversibly absorbs and releases lithium ions is used. Suitable carbon-based active materials include natural graphite such as flake graphite, lump graphite, and earthy graphite, and artificial graphite such as lump artificial graphite (MAG) and graphitized mesophase carbon microbeads (MCMB). In addition, as the negative electrode active material, a Si-based active material composed of at least one of Si and a Si-containing compound may be used, or a carbon-based active material and a Si-based active material may be used in combination.
[0040] As in the case of the positive electrode 20, the binder contained in the negative electrode mixture layer 32 may be a fluororesin, PAN, polyimide, acrylic resin, polyolefin, or the like, but it is preferable to use styrene-butadiene rubber (SBR). In addition, it is preferable that the negative electrode mixture layer 32 further contains CMC or a salt thereof, polyacrylic acid (PAA) or a salt thereof, polyvinyl alcohol (PVA), or the like. Among them, it is preferable to use SBR in combination with CMC or a salt thereof, or PAA or a salt thereof.
[0041] Negative electrode mixture layer 32 can have a high density region and a low density region, similar to positive electrode mixture layer 22. When negative electrode mixture layer 32 formed on the base of negative electrode core 31 is divided into three equal parts in the vertical direction, and these are defined as a second region, an intermediate region, and a first region, in that order from sealing plate 15 side, it is preferable that the density of negative electrode mixture layer 32 satisfies the following relationship:
[0042] Density ρ of the second region 32B 32B >Density ρ of the intermediate region 32C 32C>Density ρ of the first region 32A 32A The density of negative electrode mixture layer 32 may change stepwise, but preferably decreases gradually from the upper end to the lower end of negative electrode mixture layer 32 .
[0043] Since the density pattern of the positive electrode mixture layer 22 can also be applied to the negative electrode mixture layer 32 (as described above, the suitable density value is different), the above description of the negative electrode mixture layer 32 is used, and the overlapping description will be omitted below. In order to improve the impregnation of the non-aqueous electrolyte into the electrode body 11, the density of a first region away from the liquid injection part 16 may be made lower than the density of a second region close to the liquid injection part 16 in at least one of the positive electrode mixture layer 22 and the negative electrode mixture layer 32. Therefore, the above density pattern may be applied only to the positive electrode mixture layer 22, or may be applied only to the negative electrode mixture layer 32. The above density pattern may also be applied to both the positive electrode mixture layer 22 and the negative electrode mixture layer 32.
[0044] An example of a method for manufacturing the nonaqueous electrolyte secondary battery 10 having the above configuration will be described below. The manufacturing process of the nonaqueous electrolyte secondary battery 10 includes a step of preparing the positive electrode 20, a step of preparing the negative electrode 30, a step of preparing the electrode body 11 using the positive electrode 20 and the negative electrode 30, and a step of housing the electrode body 11 inside an exterior body and then injecting a nonaqueous electrolyte into the interior of the exterior body. Note that the constituent materials of the electrode body 11, such as the positive electrode active material, the negative electrode active material, and the separator 40, can be the same as conventional materials.
[0045] In this manufacturing process, in at least one of the steps of forming the positive electrode mixture layer 22 and the negative electrode mixture layer 32, the mixture layer is formed so that the density of the region located on the first end side of the mixture layer is lower than the density of the region located on the second end side opposite to the first end. Then, in the step of injecting the nonaqueous electrolyte, the nonaqueous electrolyte is injected from the second end side of the mixture layer into the exterior body. In other words, the nonaqueous electrolyte is injected so that it moves from the high density side to the low density side of the mixture layer.
[0046] When the exterior body is a rectangular metal container composed of exterior can 14 and sealing plate 15, injection part 16 exists even after the injection of the nonaqueous electrolyte, but the position of the injection part may not be clearly identified after the injection of the nonaqueous electrolyte. In either case, the nonaqueous electrolyte needs to be injected so that it moves from the high-density side to the low-density side of the composite layer.
[0047] The positive electrode 20 is produced by forming a positive electrode composite layer 22 on the surface of the positive electrode core 21 as described above. Similarly, the negative electrode 30 is produced by forming a negative electrode composite layer 32 on the surface of the negative electrode core 31. The electrode body 11 is produced by alternately stacking a plurality of positive electrodes 20 and a plurality of negative electrodes 30 one by one with separators 40 interposed therebetween. At this time, the positive electrodes 20 and the negative electrodes 30 are stacked so as to have an arrangement exemplified in FIG. 3. The separator 40 can be a zigzag-folded insulating porous sheet.
[0048] FIG. 5 is a diagram showing a manufacturing process of the positive electrode 20. As illustrated in FIG. 5, the positive electrode 20 is produced by applying a positive electrode composite slurry containing a positive electrode active material and the like to a long metal foil 50 that will become a positive electrode core 21, drying and rolling the coating film to form a positive electrode composite layer 22 on both sides of the metal foil 50, and then cutting the metal foil 50 into a predetermined shape. The metal foil 50 can be cut by a conventionally known method, such as laser irradiation or punching die processing. In FIG. 5, the cut portion is shown by an imaginary line. The long metal foil 50 has a width that allows two positive electrodes 20 to be formed in the width direction, for example, and has a width slightly larger than the vertical length of two positive electrodes 20.
[0049] The positive electrode composite slurry is applied to the metal foil 50 from both widthwise ends to the portions other than the fixed-width region, and exposed portions 51 are provided at both widthwise ends of the metal foil 50 where the surface of the metal foil 50 is exposed. The metal foil 50, on both sides of which the positive electrode composite layer 22 is formed by applying the positive electrode composite slurry, is cut in the center of the widthwise direction along the longitudinal direction, and is also cut in the widthwise direction at predetermined intervals corresponding to the lateral length of the positive electrode 20. The metal foil 50 is also cut in the longitudinal direction along the boundary between the positive electrode composite layer 22 and the exposed portions 51, and the exposed portions 51 are cut at predetermined intervals to form the positive electrode tabs 23.
[0050] The positive electrode composite slurry is applied to the surface of the metal foil 50 using a known application device such as a gravure coater, a slit coater, or a die coater. 22B >Density ρ of intermediate region 22C 22C >Density ρ of the first region 22A 22A There are no particular limitations on the method for forming positive electrode composite layer 22 having the density pattern. As an example, the density pattern can be formed by changing the amount of positive electrode composite slurry applied along the width direction of metal foil 50.
[0051] When the density pattern is formed by changing the amount of application of the positive electrode composite slurry, for example, the slurry is applied so that the amount of application gradually increases from the exposed portion 51 side toward the center side in the width direction of the metal foil 50. At this time, if the amount of application gradually increases from the center side in the width direction of the metal foil 50 toward the exposed portion 51 side, the composite slurry accumulates at the boundary between the exposed portion 51 and the positive electrode composite layer, causing the composite layer to swell, resulting in so-called "ridged edges." If the positive electrode sheet with raised edges is continued to be produced while being wound, it is undesirable because the raised edges may wrinkle and ultimately break. Then, the coating film of the positive electrode composite slurry is heated and dried to volatilize and remove the solvent in the slurry.
[0052] After the coating film is heated and dried, the coating film is compressed using a rolling roller or the like, and the rolling load of the rolling roller is increased from the center to the ends in the width direction of the metal foil 50 on which the coating film has been formed. For example, a method of compressing by applying a large load to both ends in the width direction of the rolling roller to bend the rolling roll into an inverted crown shape, or a method of compressing using a rolling roller with an inverted crown shape can be used. When the metal foil 50 coated with the slurry is compressed using these methods so that the coating amount gradually increases from the exposed portion 51 side toward the width direction center side of the metal foil 50, a positive electrode mixture layer 22 that gradually becomes denser from the width direction center side of the metal foil 50 toward the exposed portion 51 side is formed on both sides of the metal foil 50.
[0053] Next, metal foil 50 on which positive electrode mixture layer 22 has been formed is cut at a predetermined position, whereby positive electrode 20 having positive electrode mixture layer 22 with the above density pattern on both sides of metal foil 50 can be obtained.
[0054] In the manufacturing process of the nonaqueous electrolyte secondary battery 10, the electrode body 11 is accommodated in the exterior can 14 so that the second region 22B, which is a high-density region, is located on the upper end side of the positive electrode mixture layer 22 close to the sealing plate 15, and the first region 22A, which is a low-density region, is located on the lower end side of the positive electrode mixture layer 22 close to the bottom of the exterior can 14. When the above-mentioned density pattern is applied to the negative electrode mixture layer 32, the negative electrode 30 is also arranged so that the second region, which is a high-density region, is located on the sealing plate 15 side, and the first region, which is a low-density region, is located on the bottom side of the exterior can 14. At this time, the negative electrode 30 can be manufactured by applying a process approximately equivalent to that of the positive electrode 20 described above. The electrode body 11 is accommodated in the exterior can 14 after the positive electrode tabs 23 of the multiple positive electrodes 20 are connected to the positive electrode current collector and the negative electrode tabs 33 of the multiple negative electrodes 30 are connected to the negative electrode current collector by welding or the like.
[0055] After the electrode body 11 is housed in the exterior can 14 and the opening of the exterior can 14 is sealed with the sealing plate 15, the nonaqueous electrolyte is injected through the injection part 16 provided in the sealing plate 15. As a result, the nonaqueous electrolyte permeates into the electrode body 11 from the upper end of the positive electrode mixture layer 22 to impregnate the second region 22B, which is a high-density region, and then quickly permeates toward the lower end side of the positive electrode mixture layer 22, in that order of the intermediate region 22C and the first region 22A, and is impregnated into the entire positive electrode mixture layer 22.
[0056] The following description will be given with reference to an experimental example of the present disclosure, but the present disclosure is not limited to this experimental example. In at least one of the positive electrode composite layer of the positive electrode and the negative electrode composite layer of the negative electrode that constitute the electrode body, the density of a first region away from the liquid injection portion may be lower than the density of a second region close to the liquid injection portion.
[0057] First, for the positive electrode 20, the density ρ 22B , density ρ of intermediate region 22C 22C , and the density ρ 22AThe experimental examples are as follows. The following values are examples of average values of each density when lithium nickel cobalt manganese oxide (NCM) is used as the positive electrode active material, and the preferred range of each density varies depending on the type of positive electrode active material, etc.
[0058] (Experimental Example 1) Density ρ of second region 22B 22B 3.72g / cm 3 , density ρ of intermediate region 22C 22C 3.62g / cm 3 , density ρ of the first region 22A 22A 3.52g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0059] (Experimental Example 2) Density ρ of second region 22B 22B 3.67g / cm 3 , density ρ of intermediate region 22C 22C 3.57g / cm 3 , density ρ of the first region 22A 22A 3.47g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0060] (Experimental Example 3) Density ρ of second region 22B 22B 3.62g / cm 3 , density ρ of intermediate region 22C 22C 3.52g / cm 3 , density ρ of the first region 22A 22A 3.42g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0061] (Experimental Example 4) Density ρ of second region 22B 22B 3.59g / cm 3 , density ρ of intermediate region 22C 22C 3.57g / cm 3 , density ρ of the first region 22A 22A 3.55g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0062] (Experimental Example 5) Density ρ of second region 22B 22B 3.57g / cm 3 , density ρ of intermediate region 22C 22C 3.47g / cm 3 , density ρ of the first region 22A 22A 3.37g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0063] (Experimental Example 6) Density ρ of second region 22B 22B 3.52g / cm 3 , density ρ of intermediate region 22C 22C 3.42g / cm 3 , density ρ of the first region 22A 22A 3.32g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0064] (Experimental Example 7) Density ρ of second region 22B 22B 3.44g / cm 3 , density ρ of intermediate region 22C 22C 3.34g / cm 3 , density ρ of the first region 22A 22A 3.23g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0065] (Experimental Example 8) Density ρ of second region 22B 22B 3.37g / cm 3 , density ρ of intermediate region 22C 22C 3.27g / cm 3 , density ρ of the first region 22A 22A 3.16g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0066] (Experimental Example 9) Density ρ of second region 22B 22B 3.30g / cm 3 , density ρ of intermediate region 22C 22C 3.20g / cm 3 , density ρ of the first region 22A 22A3.08g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0067] (Experimental Example 10) Density ρ of second region 22B 22B 3.23g / cm 3 , density ρ of intermediate region 22C 22C 3.13g / cm 3 , density ρ of the first region 22A 22A 3.01g / cm 3 The positive electrode 20 was produced so as to satisfy the above conditions.
[0068] Next, for the negative electrode 30, the density ρ 32B , density ρ of the intermediate region 32C 32C , and the density ρ 32A The experimental examples are as follows: The following values are examples of average values of each density when graphite is used as the negative electrode active material, and the preferred range of each density varies depending on the type of negative electrode active material, etc.
[0069] (Experimental Example 11) Density ρ of the second region 32B 32B 1.70g / cm 3 , density ρ of the intermediate region 32C 32C 1.68g / cm 3 , density ρ32 of the first region 32A A 1.66g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0070] (Experimental Example 12) Density ρ of the second region 32B 32B 1.63g / cm 3 , density ρ of the intermediate region 32C 32C 1.57g / cm 3 , density ρ of the first region 32A 32A 1.52g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0071] (Experimental Example 13) Density ρ of the second region 32B 32B 1.58g / cm 3, density ρ of the intermediate region 32C 32C 1.52g / cm 3 , density ρ of the first region 32A 32A 1.47g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0072] (Experimental Example 14) Density ρ of the second region 32B 32B 1.53g / cm 3 , density ρ of the intermediate region 32C 32C 1.47g / cm 3 , density ρ of the first region 32A 32A 1.42g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0073] (Experimental Example 15) Density ρ of the second region 32B 32B 1.48g / cm 3 , density ρ of the intermediate region 32C 32C 1.47g / cm 3 , density ρ of the first region 32A 32A 1.46g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0074] (Experimental Example 16) Density ρ of the second region 32B 32B 1.48g / cm 3 , density ρ of the intermediate region 32C 32C 1.42g / cm 3 , density ρ of the first region 32A 32A 1.37g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0075] (Experimental Example 17) Density ρ of the second region 32B 32B 1.43g / cm 3 , density ρ of the intermediate region 32C 32C 1.37g / cm 3 , density ρ of the first region 32A 32A 1.32g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0076] (Experimental Example 18) Density ρ of the second region 32B 32B 1.39g / cm 3 , density ρ of the intermediate region 32C 32C 1.35g / cm 3 , density ρ of the first region 32A 32A 1.30g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0077] (Experimental Example 19) Density ρ of the second region 32B 32B 1.36g / cm 3 , density ρ of the intermediate region 32C 32C 1.31g / cm 3 , density ρ of the first region 32A 32A 1.26g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0078] (Experimental Example 20) Density ρ of the second region 32B 32B 1.32g / cm 3 , density ρ of the intermediate region 32C 32C 1.28g / cm 3 , density ρ of the first region 32A 32A 1.22g / cm 3 The negative electrode 30 was produced so as to satisfy the above requirements.
[0079] (Evaluation of impregnation speed of non-aqueous electrolyte) The impregnation speed of the non-aqueous electrolyte was measured for the positive electrodes 20 and negative electrodes 30 of Experimental Examples 1 to 20. The measurement method was to drip a fixed amount (1 μml) of the non-aqueous electrolyte onto the compressed positive electrode plate, and measure the time until the non-aqueous electrolyte was completely soaked in as the impregnation time with a stopwatch. These results are shown in Tables 1 and 2.
[0080] [Table 1]
[0081] [Table 2]
[0082] From the results of Experimental Examples 1 to 20, it can be seen that the impregnation time is shorter in the low density region than in the high density region of the positive electrode mixture layer or the negative electrode mixture layer. 22A Or ρ 32A is the density ρ 22C Or ρ 32C Lower, density ρ 22C Or ρ 32C is the density ρ 22B Or ρ 32B By forming a lower density pattern, the nonaqueous electrolyte injected from the injection part 16 provided in the sealing plate 15 can move smoothly toward the bottom of the can on the opposite side to the injection part. In other words, this means that the nonaqueous electrolyte can be distributed evenly throughout the entire electrode body.
[0083] As described above, according to the nonaqueous electrolyte secondary battery 10 having the above-mentioned configuration and including the electrode assembly 11 in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with separators interposed therebetween, when the nonaqueous electrolyte is injected into the exterior can 14, the entire electrode assembly 11 can be impregnated with the nonaqueous electrolyte, and the nonaqueous electrolyte can be distributed evenly throughout the entire electrode assembly 11. In addition, the nonaqueous electrolyte is pushed outward from the electrode assembly 11 due to the expansion of the electrode assembly 11 caused by charging and discharging the battery, but since the electrode assembly 11 has a structure in which the positive electrodes 20 and the negative electrodes 30 are alternately stacked one by one with separators 40 interposed therebetween, the nonaqueous electrolyte has better permeability than a wound electrode assembly. In other words, the nonaqueous electrolyte permeates the electrode assembly 11 from above, below, left and right. In the nonaqueous electrolyte secondary battery 10, the impregnation of the electrode body 11 with the nonaqueous electrolyte is greatly improved due to the synergistic effect of the density pattern of the composite layer and the laminated structure of the electrode body 11, thereby suppressing performance degradation caused by variations in the amount of nonaqueous electrolyte in the electrode body.
[0084] The above embodiment can be appropriately modified in design without impairing the purpose of the present disclosure. For example, in FIG. 2, the electrode body 11 including the first electrode group 11A and the second electrode group 11B is illustrated, but the electrode body 11 does not have to be divided into a plurality of electrode groups. In addition, a configuration in which a composite layer of the above density pattern is formed only on a portion of the plurality of positive electrodes 20 or only on a portion of the plurality of negative electrodes 30 is also assumed. [Explanation of symbols]
[0085] 10 Nonaqueous electrolyte secondary battery 11 Electrode body 11A First electrode group 11B Second electrode group 12 Positive terminal 13 Negative terminal 14 Outer can 15 Sealing plate 16 Injection section 17 Gas exhaust valve 18 Current interruption mechanism 20 positive electrode 21 Positive electrode core 22 Positive electrode mixture layer 22A 1st area 22B 2nd area 22C intermediate area 23 Positive tab 30 negative electrode 31 Negative electrode core 32 Negative electrode composite layer 33 Negative tab 40 Separator 50 Metal Foil 51 Exposed part
Claims
1. an electrode assembly in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked one by one with separators interposed therebetween; A non-aqueous electrolyte; an exterior body that accommodates the electrode assembly and the nonaqueous electrolyte; A non-aqueous electrolyte secondary battery comprising: The exterior body is provided with a liquid injection portion for injecting the nonaqueous electrolyte solution, The plurality of positive electrodes include a positive electrode core and a positive electrode mixture layer formed on a surface of the positive electrode core, The plurality of negative electrodes include a negative electrode core and a negative electrode mixture layer formed on a surface of the negative electrode core, the density of at least one of the positive electrode mixture layer and the negative electrode mixture layer decreases stepwise or gradually with increasing distance from the liquid injection portion.
2. The exterior body includes a bottomed rectangular cylindrical exterior can and a sealing plate that closes an opening of the exterior can, The liquid injection part is provided on the sealing plate, 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein when at least one of the positive electrode composite layer and the negative electrode composite layer is divided into thirds from the sealing plate side toward a bottom side of the exterior can, and the thirds are defined as a second region, an intermediate region, and a first region, in that order from the sealing plate side, the densities of the respective regions satisfy a relationship of density of the second region > density of the intermediate region > density of the first region.
3. A method for manufacturing a non-aqueous electrolyte secondary battery including an electrode assembly in which a plurality of positive electrodes and a plurality of negative electrodes are alternately stacked with separators interposed therebetween, a non-aqueous electrolyte, and an exterior body, comprising: forming the positive electrode mixture layer on a surface of a positive electrode core body to fabricate the positive electrode; forming the negative electrode mixture layer on a surface of a negative electrode core body to fabricate the negative electrode; producing the electrode assembly using the plurality of positive electrodes and the plurality of negative electrodes; a step of injecting the nonaqueous electrolyte after housing the electrode assembly inside the exterior body; Including, forming at least one of the positive electrode mixture layer and the negative electrode mixture layer such that a density of the at least one of the positive electrode mixture layer and the negative electrode mixture layer is stepwise or gradually decreased from a second end opposite to a first end of the at least one of the positive electrode mixture layer and the negative electrode mixture layer toward the first end; the step of injecting the nonaqueous electrolyte solution includes injecting the nonaqueous electrolyte solution into the exterior body such that the nonaqueous electrolyte solution moves from the second end side toward the first end side of at least one of the positive electrode mixture layer and the negative electrode mixture layer.
4. A method for manufacturing a nonaqueous electrolyte secondary battery as described in claim 3, wherein when at least one of the positive electrode composite layer and the negative electrode composite layer is divided into thirds from the second end toward the first end, and defined as a second region, an intermediate region, and a first region, in that order from the second end, the density of each of the regions satisfies the relationship: density of the second region > density of the intermediate region > density of the first region.
Citation Information
Patent Citations
Electrode and battery
EP0967672A1
Lithium secondary battery
JP2000090980A
Non-aqueous electrolyte secondary battery
JP2001176558A
Non-aqueous electrolyte rechargeable battery
JP2004207253A
Nonaqueous electrolyte secondary battery
JP2005209411A