Method for recovering desalted washed ash from chlorine-containing ash

The alkaline washing of chlorine-containing ash with a 1.0 mol/L alkali concentration effectively desalinated and recovered calcium hydroxide, addressing the inefficiencies of previous methods by minimizing chlorine elution and carbon emissions, allowing the ash to be used as a cement raw material.

JP7570596B2Active Publication Date: 2024-10-22MITSUBISHI MATERIALS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020165151
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-30
Publication Date
2024-10-22
Estimated Expiration
2040-09-30

AI Technical Summary

Technical Problem

Existing methods for desalinating chlorine-containing ash, such as acid washing and carbon dioxide treatment, fail to effectively recover calcium while maintaining low carbon emissions, as they either elute calcium with chlorine or convert it to sparingly soluble compounds like calcium carbonate, leading to high CO2 emissions during cement manufacturing.

Method used

An alkaline washing process with an alkali concentration of 1.0 mol/L or more is applied to chlorine-containing ash, converting calcium into calcium hydroxide, followed by solid-liquid separation to recover desalinated washed ash with a chlorine concentration of 0.6% by mass or less, using alkali solutions, powders, or granules in a closed atmosphere.

Benefits of technology

The method achieves efficient desalination and recovery of calcium as calcium hydroxide, enabling its use as a cement raw material with minimal carbon emissions, as the recovered ash can be used as a substitute for cement, reducing CO2 emissions during manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570596000002
    Figure 0007570596000002
  • Figure 0007570596000003
    Figure 0007570596000003
  • Figure 0007570596000004
    Figure 0007570596000004
Patent Text Reader

Abstract

To provide a treatment method for desalinating chlorine-containing ash, and fixing and effectively recovering a calcium component.SOLUTION: A method for recovering desalinated washed ash of chlorine-containing ash is provided, including: an alkali washing step in which alkali is added to chlorine-containing ash and the ash is subjected to alkali washing with fluidity at an alkali concentration of 1.0 mol / L or higher, so that desalination is performed and calcium included in the chlorine-containing ash is converted into calcium hydroxide; and a solid-liquid separation step in which solid-liquid separation is performed after the alkali washing step, so that a solid content including the calcium hydroxide is recovered.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for effectively recovering calcium by desalting and washing chlorine-containing ash. [Background technology]

[0002] The reuse of incineration ash (bottom ash, fly ash, cinders, soot) generated by incineration of general waste and industrial waste, incineration ash landfilled at final disposal sites, and clinker dust generated from cement plants as cement raw materials has been promoted. However, since these incineration ash etc. contain about 10% chlorine, in order to recycle the above-mentioned various incineration ash and clinker dust etc. that contain chlorine (hereinafter referred to as chlorine-containing ash), it is necessary to desalinate them to a degree appropriate for the intended use.

[0003] In addition, the chlorine-containing ash is rich in calcium, approximately 20% to 50% in terms of oxide, and if this calcium can be effectively recovered, it will be possible to expand the recycling of chlorine-containing ash.

[0004] Regarding the desalting of the above-mentioned chlorine-containing ash, most of the chlorine compounds contained in the chlorine-containing ash are water-soluble and can be desalted by washing with water. However, some of the chlorine compounds are poorly soluble in water and can be desalted by washing with water. 2 O 3 CaCl 2 10H 2 O), etc., and cannot be fully desalted by washing with water alone. On the other hand, a method of desalting is known in which Friedel's salt, etc. is added with acid to lower the pH. However, with this method, calcium is eluted along with chlorine as the pH drops, so calcium cannot be fully recovered by washing with acid alone.

[0005] Also known are a method of washing chlorine-containing ash by adding water containing carbonate (JP Patent Publication 2006-326462 A) and a method of washing chlorine-containing ash by blowing carbon dioxide gas into a water slurry (JP Patent Publication 3924822 A). However, when washing is performed using carbonate or carbon dioxide gas, Friedel's salt is decomposed and desalted, so that desalted washed ash can be obtained, but some of the calcium becomes calcium carbonate, which is poorly soluble in water, and this is recovered as a solid content together with the washed ash by solid-liquid separation after washing. If this washed ash containing calcium carbonate is used as a cement raw material, a large amount of CO will be emitted during the production process. 2 There is a problem that occurs.

[0006] Thus, in order to reuse chlorine-containing ash as a cement raw material, it is necessary to fully demineralize it and effectively recover calcium, which is a cement component. Furthermore, it is necessary to reduce carbon dioxide emissions during cement production (CO 2 To comply with the requirements of the EPA, calcium carbonate (CaCO 3 , CaMg(CO 3 ) 2 It is preferable that the format be something other than a. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] JP 2006-326462 A [Patent Document 2] Patent No. 3924822 [Patent Document 3] Patent No. 5561326 Summary of the Invention [Problem to be solved by the invention]

[0008] The present invention has been made to solve the above problems, and provides a treatment method capable of sufficiently desalting chlorine-containing ash and effectively recovering calcium contained in the ash. [Means for solving the problem]

[0009] The method of the present invention is a treatment method which solves the above problems by the following constitution, and which is a method for desalting chlorine-containing ash and recovering washed ash containing calcium hydroxide. [1] A method for recovering desalted washed ash, comprising: an alkali washing step in which chlorine-containing ash is desalted by adding an alkali to the chlorine-containing ash and washing the ash with an alkali concentration of 1.0 mol / L or more, and the calcium contained in the chlorine-containing ash is converted into calcium hydroxide; and a solid-liquid separation step in which, after the alkali washing step, a solid content containing the calcium hydroxide is recovered by solid-liquid separation. The chlorine-containing ash contains sparingly soluble chlorine compounds, and the chlorine concentration of the desalted washed ash is reduced to 0.6 mass% or less by performing alkaline washing with a liquid having a pH of 13.0 or more at a liquid temperature of 10°C or more and less than 40°C, and alkaline washing with a liquid having a pH of 12.5 or more at a liquid temperature of 40°C or more and 80°C or less. A method for recovering desalted washed ash. [2] A method for recovering desalted washed ash from chlorine-containing ash described in [1] above, in which an alkaline solution, alkaline powder or granular alkali is added to chlorine-containing ash or a water slurry of chlorine-containing ash under a sealed atmosphere or an inert gas atmosphere so that the alkali concentration is 1.0 mol / L or more to perform alkaline washing.

[0010] [Specific explanation] The treatment method of the present invention is a method for recovering desalted washed ash, comprising an alkali washing step in which an alkali is added to chlorine-containing ash and the chlorine-containing ash is desalted by alkali washing with a liquid having an alkali concentration of 1.0 mol / L or more, and the calcium contained in the chlorine-containing ash is converted into calcium hydroxide, and a solid-liquid separation step in which solids containing the calcium hydroxide are recovered by solid-liquid separation after the alkali washing step. The chlorine-containing ash contains sparingly soluble chlorine compounds, and the chlorine concentration of the desalted washed ash is reduced to 0.6 mass% or less by performing alkaline washing with a liquid having a pH of 13.0 or more at a liquid temperature of 10°C or more and less than 40°C, and alkaline washing with a liquid having a pH of 12.5 or more at a liquid temperature of 40°C or more and 80°C or less. The present invention relates to a method for recovering desalted washed ash. The process of the present invention is outlined in the flow chart of FIG.

[0011] The treatment method of the present invention is a treatment method for effectively recovering calcium by immobilizing it while desalination of chlorine-containing ash. In the treatment method of the present invention, the chlorine-containing ash broadly includes chlorine-containing ashes such as incineration ash of general waste or industrial waste, incineration ash disposed of in landfill sites, or dust generated from cement plants.

[0012] <Alkaline cleaning process> The treatment method of the present invention includes an alkali washing step in which the chlorine-containing ash is desalted by adding an alkali to the chlorine-containing ash so that the alkali concentration is 1.0 mol / L or more, and the calcium contained in the chlorine-containing ash is solidified in the form of calcium hydroxide.

[0013] The alkali to be added to the chlorine-containing ash may be in the form of a solution, powder, or granules. The type of alkali that can be used may be a common hydroxide of an alkali metal, such as sodium hydroxide or potassium hydroxide. After adding washing water to the chlorine-containing ash to form a slurry, an alkali solution, an alkali powder, or granular alkali may be added, or an alkali solution may be added directly to the chlorine-containing ash.

[0014] The liquid-solid ratio of the chlorine-containing ash slurry to which an alkali has been added is preferably 2 to 20 (liquid:solid=2:1 to 20:1), and more preferably 3 to 10 (liquid:solid=3:1 to 10:1). If the liquid-solid ratio exceeds 20, the amount of alkali added will be excessive. On the other hand, if the liquid-solid ratio is less than 2, the amount of liquid will be too small and washing will be insufficient. If the liquid-solid ratio is about 3 to 10, washing can be sufficiently performed to improve the desalting effect, and Friedel's salt and the like will also be eluted, so that calcium hydroxide can be sufficiently recovered.

[0015] Washing is performed by adding an alkali so that the alkali concentration is 1.0 mol / L or more. By washing with an alkali concentration of 1.0 mol / L or more, desalination of chlorine-containing ash progresses. This is because OH - Cl contained in ions and poorly soluble chloride compounds such as Friedel's salt - It is presumed that an ion exchange reaction occurs with the ion, promoting the dissolution of chlorine. Al(OH) 4- If ions (aluminate ions) are present, desalination will also proceed. It is also possible that strong alkali dissolves silicic acid compounds containing chlorine, which will promote desalination.

[0016] In addition, by washing with an alkali to an alkali concentration of 1.0 mol / L or more, the calcium contained in the chlorine-containing ash can be solidified in the form of calcium hydroxide. Calcium contained in chlorine-containing ash such as incineration ash and incineration fly ash exists in the form of calcium hydroxide, calcium carbonate, calcium sulfate, etc., but most of it becomes calcium hydroxide when washed with an alkali concentration of 1.0 mol / L or more.

[0017] If the alkali concentration during washing is less than 1.0 mol / L, desalination will be insufficient. Furthermore, at around pH 7, calcium hydroxide and calcium carbonate contained in the chlorine-containing ash will dissolve in the liquid due to the drop in pH, making it difficult to solidify and recover calcium, and the calcium recovery rate will drop significantly.

[0018] In a liquid having an alkali concentration of 1.0 mol / L or more, when the liquid temperature is 10°C or more but less than 40°C, alkaline washing is performed at a pH of 13.0 or more, and when the liquid temperature is 40°C or more but less than 80°C, alkaline washing is performed at a pH of 12.5 or more, whereby the chlorine concentration of the washed ash can be desalted to approximately 0.6 mass% or less, and calcium contained in the chlorine-containing ash can be converted to calcium hydroxide and solidified. Since the solubility of calcium hydroxide decreases with an increase in the liquid temperature, the amount of calcium hydroxide recovered can be increased by setting the liquid temperature within the above range. In addition, CO 2 Since the solubility of gas also decreases with increasing temperature, the above liquid temperature can suppress the carbonation of calcium. Note that it is not necessary to make the liquid temperature higher than 80°C.

[0019] The alkaline washing step is preferably carried out in a sealed atmosphere or in an inert gas atmosphere such as nitrogen gas in order to prevent carbonation of calcium due to contamination with carbon dioxide in the air.

[0020] <Solid-liquid separation process> The alkaline washed slurry is subjected to solid-liquid separation to recover the solids. The solids contain calcium hydroxide along with the desalted washed ash. By converting the calcium contained in the chlorine-containing ash into calcium hydroxide and immobilizing it, it is possible to recover approximately 85% by mass or more of the calcium.

[0021] As the solid-liquid separation device, a filter press, a vacuum belt filter, a centrifugal dehydrator, etc. can be used. A filter press is easy to use. For example, the desalination effect can be further improved by penetrating and washing the washed ash cake obtained by solid-liquid separation with a filter press with washing water. The water content of the washed ash cake obtained by the filter press is low at about 25 to 40%, and since there is no excess water attached, the weight is reduced and the handling properties are improved. The generated washing wastewater contains chlorine, so it is treated and discharged, but the washing wastewater generated by penetrating and washing the filter press has a low chlorine concentration, so it may be recycled and used as washing water during alkaline washing.

[0022] In the treatment method of the present invention, the chlorine-containing ash can be efficiently desalted by crushing it before washing with an alkali. Examples of crushing equipment include a vibration mill and a hammer mill. Crushing and washing with an alkali may be performed simultaneously. The washing treatment may be a multi-stage washing. For example, washing with water is first performed to remove water-soluble chlorine compounds (NaCl, KCl, CaCl(OH), CaCl 2 After removing the above-mentioned substances, alkaline washing may be performed.

[0023] [Treatment equipment] An example of a treatment facility for carrying out the method of the present invention is shown in FIG. 2. The treatment facility shown in the figure is provided with a vibration mill 1 for receiving chlorine-containing ash and washing water. The chlorine-containing ash is appropriately pulverized in the vibration mill 1. The chlorine-containing ash slurry discharged from the vibration mill 1 is sent to an agitation washing tank 2. An alkaline solution is supplied to the agitation washing tank 2 so that the alkali concentration is 1.0 mol / L or more, and the slurry is agitated and washed. The washed slurry is sent to a filter press 3. The slurry is dehydrated in the filter press 3, and the generated washing wastewater is sent to a wastewater treatment facility 4. This washing wastewater may be used as washing water for alkaline washing. Meanwhile, the dehydrated cake (demineralized washed ash) is sent to a cement production facility 5 and reused. Effect of the Invention

[0024] According to the method of the present invention, by washing with an alkali at an alkali concentration of 1.0 mol / L or more, it is possible to promote the dissolution of chlorine contained in poorly soluble chlorine compounds and enhance the desalting effect, and by solidifying calcium in the chlorine-containing ash in the form of calcium hydroxide, it is possible to recover desalted washed ash that is rich in calcium. This desalted washed ash can be used as a substitute for cement raw material. In addition, since the calcium contained in this desalted washed ash is in the form of hydroxide, when this desalted washed ash is used as a cement raw material, it is possible to reduce the amount of CO 2 This will contribute greatly to reducing carbon emissions during cement production. [Brief description of the drawings]

[0025] [Figure 1] 1 is a process diagram showing an outline of a processing method of the present invention. [Diagram 2] 1 is a schematic diagram of a processing facility for carrying out the processing method of the present invention. [Diagram 3] 4 shows XRD patterns of washed ashes of the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0026] Examples of the present invention will be described below together with comparative examples. The Cl concentration of the recovered washed ash was analyzed by dissolving the washed ash in acid and then measuring the Cl concentration in the solution using a coulometric titration device. The Ca concentration of the recovered washed ash was measured by X-ray fluorescence analysis (XRF). The results are shown in Table 1. The XRD pattern of the recovered washed ash is also shown in Figure 3.

[0027] [Example] Incineration fly ash (Cl concentration 12.5 mass%, Ca concentration 25.9 mass%) was dried at 105°C and then sieved, and 100mL of pure water was added to 10g of ash with a size of 1mm or less for primary washing. 100mL of 1.0mol / L to 3.0mol / L sodium hydroxide (NaOH) solution was added to 10g of this primary washed ash to make a slurry, and the slurry was shaken at a liquid temperature of 10°C to 80°C for alkaline washing. This alkaline washed slurry was filtered and the washed cake was collected. 50mL of pure water was added to this washed cake for cake washing, and the desalted washed ash was collected. This desalted washed ash was dried at 105°C and 6.14g to 6.58g of dried desalted washed ash was collected (No. A1 to A8).

[0028] Comparative Example The primary washed ash of the examples was subjected to alkaline washing at a liquid temperature of 25° C. by adding 0.1 mol / L to 0.8 mol / L of sodium hydroxide solution (Nos. B1, B2, and B3). The ash that had been subjected to the primary washing in the example was washed with water at 25°C under a pH of 12.3 by adding pure water instead of the sodium hydroxide solution (No. B4). The ash that had been subjected to the primary washing in the example was adjusted to pH 7.1 by adding 0.7 mol / L hydrochloric acid instead of the sodium hydroxide solution, and was then washed with hydrochloric acid at a liquid temperature of 25°C (No. B5). The ash that had been subjected to the primary washing in the embodiment was washed with sodium carbonate at a solution temperature of 25° C. and a pH of 12.8 by adding 0.1 mol / L sodium carbonate solution instead of the sodium hydroxide solution (No. B6).

[0029] As shown in Table 1, in all of the samples A1 to A8 of the present invention, which were washed with an alkali concentration of 1.0 mol / L, the Cl concentration of the washed ash was desalted to 0.6 mass% or less, the Ca concentration was 35 mass% or more, and the Ca recovery rate was 85% or more. On the other hand, in comparative samples B1 to B3, in which the alkali concentration during alkaline washing was less than 1.0 mol / L, the Ca concentration in the wash ash was 35.1 to 36.2 mass%, and the Ca recovery rate was 88% to 90%, but the Cl concentration was 0.69 to 0.86 mass%, indicating a significantly low desalination effect. Furthermore, in sample B4, which was washed with water instead of with alkali, the Ca concentration in the washed ash was 32.1 mass % and the Ca recovery rate was 86%, but the Cl concentration was 0.86 mass %, indicating a significantly low desalination effect. In addition, in sample B5, which was washed with hydrochloric acid instead of with alkali, the Cl concentration in the washed ash was 0.36 mass%, which was a high desalination effect, but the Ca concentration was 24.4 mass%, and the Ca recovery rate was 38%, which was significantly low. In sample B6, which was washed with sodium carbonate instead of alkali, the Cl concentration in the washed ash was 0.54 mass%, which is a high desalination effect. The Ca concentration in the washed ash was 33.9 mass%, and the Ca recovery rate was 90%. However, as shown in the XRD in Figure 3, most of the calcium is calcium carbonate, so if the recovered washed ash is used as a cement raw material, a large amount of CO will be generated in the manufacturing process. 2 occurs.

[0030] [Table 1]

Claims

1. A method for recovering desalted washed ash, comprising an alkali washing step of adding an alkali to chlorine-containing ash, and desalting the chlorine-containing ash by alkali washing with a liquid having an alkali concentration of 1.0 mol / L or more, while converting calcium contained in the chlorine-containing ash into calcium hydroxide, and a solid-liquid separation step of recovering a solid content containing the calcium hydroxide by solid-liquid separation after the alkali washing step, wherein the chlorine-containing ash contains sparingly soluble chlorine compounds, and the method for recovering desalted washed ash is characterized in that the chlorine concentration of the desalted washed ash is reduced to 0.6 mass% or less by performing alkali washing at a liquid temperature of 10°C or more and less than 40°C with a liquid having a pH of 13.0 or more, and by performing alkali washing at a liquid temperature of 40°C or more and less than 80°C with a liquid having a pH of 12.5 or more.

2. 2. A method for recovering desalted washed ash from chlorine-containing ash as described in claim 1, in which alkaline washing is carried out by adding an alkaline solution, alkaline powder or granular alkali to chlorine-containing ash or a water slurry of chlorine-containing ash in a sealed atmosphere or an inert gas atmosphere so that the alkali concentration is 1.0 mol / L or more.

Citation Information

Patent Citations

  • Pretreatment method for cooperatively treating fly ash by cement kiln

    CN109748525A

  • Bending method for austenitic stainless cast steel pipe by high frequency induction heating

    JP1980061326A

  • Treatment method of fly ash

    JP2003181413A

  • Waste treatment method

    JP2003236497A

  • Method and system for treating waste gas from heating furnace for treating waste