Glass article manufacturing method and manufacturing device thereof

The method addresses convex defects in glass ribbons by inspecting and adjusting transport speed, flow rate, and using MgO-free refractories to reduce defects, enhancing glass article quality.

JP7570600B2Active Publication Date: 2024-10-22NIPPON ELECTRIC GLASS CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
JP2021066436
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2020-04-16
Filing Date
2021-04-09
Publication Date
2024-10-22
Estimated Expiration
2041-04-09

AI Technical Summary

Technical Problem

The manufacturing process of glass articles often results in convex defects where both the front and back surfaces of the glass ribbon are convex, which can reduce the smoothness and transparency of the glass article, requiring measures different from those for general defects like foreign object defects.

Method used

A method involving an inspection step to detect convex defects in glass ribbons or articles, followed by a countermeasure step to adjust the transport speed of the glass ribbon, increase the flow rate of molten glass, and use refractories that do not contain MgO, or form an MgO-free layer on the molded body to reduce the occurrence of convex defects.

Benefits of technology

This method effectively reduces the occurrence of convex defects by managing the residence time of the glass ribbon in high-temperature regions and minimizing the diffusion of Mg ions, ensuring higher quality glass products.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570600000002
    Figure 0007570600000002
  • Figure 0007570600000003
    Figure 0007570600000003
  • Figure 0007570600000004
    Figure 0007570600000004
Patent Text Reader

Abstract

To reliably reduce the convex defects in which both sides of a glass ribbon become convex.SOLUTION: A method for producing a glass article has a molding step for molding a glass ribbon G from molten glass Gm and a transporting step for transporting the glass ribbon G. The method also includes a checking step for checking whether there is a convex defect in which both sides of the glass ribbon G become convex, and a control step for controlling the transport speed of the glass ribbon G in the transporting step depending on whether the convex defect has been detected or not in the checking step.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and an apparatus for manufacturing a glass article. [Background technology]

[0002] In a manufacturing process of glass products such as glass sheets and glass rolls, a glass ribbon is continuously formed from molten glass by a known forming method such as the overflow downdraw method or the float method. The formed glass ribbon is cooled to about room temperature while being transported downstream, and then cut into predetermined lengths to obtain glass sheets, or wound into a roll to obtain a glass roll (see, for example, Patent Document 1). [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2018-062433 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have come to find a new problem that, depending on the glass composition, a convex defect in which both the front and back surfaces of the glass ribbon are convex may be formed in the manufacturing process of the above-mentioned glass article. Since such convex defects may reduce the smoothness of the front and back surfaces of the glass article and may reduce the transparency, it is desirable to reduce them as much as possible.

[0005] However, in the case of foreign matter defects caused by the inclusion of bubbles, undissolved matter, or the like, defects in which only one of the front and back surfaces of the glass ribbon is convex are likely to be formed. In other words, convex defects in which both the front and back surfaces of the glass ribbon are convex are considered to have shapes and causes different from those of general defects such as foreign matter defects. Therefore, in order to reduce the occurrence of convex defects in which both the front and back surfaces of the glass ribbon are convex, measures other than those for general defects such as foreign matter defects are required.

[0006] An object of the present invention is to reliably reduce the occurrence of convex defects in which both the front and back surfaces of a glass ribbon are convex. [Means for solving the problem]

[0007] The present invention, which has been invented to solve the above problems, is a method for manufacturing a glass article, comprising a forming step of forming a glass ribbon from molten glass and a transporting step of transporting the glass ribbon that has been subjected to the forming step, and is characterized by comprising an inspection step of inspecting the glass ribbon for the presence or absence of a convex defect in which both the front and back surfaces are convex, and a countermeasure step of taking measures to reduce the convex defect. Here, the inspection object in the inspection step may be a glass ribbon, or may be a glass article (e.g., a glass sheet) obtained from the glass ribbon.

[0008] In this way, an inspection process and a countermeasure process are separately performed for a convex defect in which both the front and back surfaces of the glass ribbon are convex (hereinafter, may be simply referred to as a "convex defect"), so that the occurrence of the convex defect can be reliably reduced. The cause of the occurrence of the convex defect will be described later.

[0009] In the above configuration, the molten glass is preferably an aluminosilicate glass containing less than 1 mass% of MgO. Specifically, the molten glass preferably contains, in mass%, 50-80% SiO2, 5-25% Al2O3, 0-15% B2O3, 1-20% Na2O, 0-10% K2O, 0.5-10% P2O5, and 0-5% Li2O as a glass composition.

[0010] In this way, the glass composition is one in which convex defects are likely to occur, making the method for manufacturing a glass article according to the present invention particularly useful.

[0011] In the above configuration, the countermeasure step preferably includes a control step of adjusting a conveying speed of the glass ribbon in the conveying step according to the occurrence state of the convex defect detected in the inspection step.

[0012] As a result of intensive research, the present inventors have found that the occurrence rate of convex defects varies depending on the residence time of the glass ribbon in a high-temperature region near the forming process. In other words, when a convex defect in which both the front and back surfaces of the glass ribbon are convex is detected in an inspection process, the occurrence of convex defects can be reliably reduced by adjusting the conveying speed of the glass ribbon in accordance with the occurrence state of the convex defect in a control process and appropriately managing the residence time of the glass ribbon in a high-temperature region near the forming process.

[0013] In the above configuration, in the control step, it is preferable to increase the conveying speed of the glass ribbon when the occurrence of convex defects increases.

[0014] The inventors have confirmed that the occurrence of convex defects is reduced by increasing the conveying speed of the glass ribbon and shortening the residence time of the glass ribbon in the high-temperature region near the forming process. Therefore, when the occurrence of convex defects increases, it is preferable to increase the conveying speed of the glass ribbon and shorten the residence time of the glass ribbon in the high-temperature region near the forming process, as in the above configuration.

[0015] In the above configuration, in the control step, it is preferable to increase the flow rate of the molten glass in the forming step when the conveying speed of the glass ribbon is increased.

[0016] In this way, the flow rate of the molten glass increases even if the conveying speed of the glass ribbon increases, so that the thickness of the glass ribbon can be maintained constant.

[0017] In the above configuration, in the forming process, the molten glass is caused to flow down along the surface of the forming body by the down-draw method to form a glass ribbon, and in the control process, it is preferable to adjust the rotation speed of cooling rollers that sandwich both ends of the glass ribbon in the width direction from both sides directly below the forming body, depending on the occurrence status of convex defects detected in the inspection process.

[0018] In this way, the residence time of the glass ribbon in the high temperature region near the forming process, i.e., directly below the forming body, can be easily and reliably adjusted.

[0019] In the above configuration, the forming step preferably comprises a down-draw method in which molten glass is caused to flow down along the surface of the formed body to form a glass ribbon, and the countermeasure step preferably comprises a selection step of selecting a refractory material substantially free of MgO as the refractory material of the formed body in advance. Here, the "refractory material substantially free of MgO" means, for example, a refractory material having an MgO content of 1 mass % or less.

[0020] As a result of intensive research, the present inventors have found that the use of a shaped body made of a refractory material substantially free of MgO reduces convex defects in a glass ribbon. In other words, as described above, by selecting a refractory material substantially free of MgO as the refractory material of the shaped body, convex defects in a glass ribbon can be reliably reduced.

[0021] In the above configuration, the forming step preferably comprises a down-draw process in which molten glass is caused to flow down along the surface of the formed body to form a glass ribbon, and the countermeasure step preferably comprises a forming step of forming a non-MgO layer substantially free of MgO on the surface of the formed body in advance. Here, the "non-MgO layer substantially free of MgO" refers to a layer having an MgO content of 1 mass % or less, for example.

[0022] As a result of intensive research, the present inventors have found that if an MgO-free layer is present at the interface between a formed body and molten glass, convex defects in the glass ribbon are reduced. In other words, by forming an MgO-free layer on the surface of a formed body as described above, convex defects in the glass ribbon can be reliably reduced.

[0023] In the above configuration, the non-MgO-containing layer may be an alumina layer.

[0024] In the above configuration, when the MgO-free layer is an alumina layer, the formed body is preferably made of an alumina-based refractory material.

[0025] In this way, since the alumina-based refractory contains alumina, an alumina layer can be easily formed on the surface of the formed body.

[0026] In the above configuration, the convex defect has a height of, for example, 1 nm to 1 μm, a length of, for example, 0.1 to 100 mm, and a width of, for example, 0.1 to 10 mm.

[0027] The present invention, which has been invented to solve the above-mentioned problems, is a method for producing a glass article, which includes a forming step of forming a glass ribbon by causing molten glass to flow along the surface of a formed body by a down-draw method, wherein the molten glass is an aluminosilicate glass having an MgO content of less than 1 mass%, and the formed body is made of a refractory material that is substantially free of MgO.

[0028] According to this configuration, it is possible to obtain the same effects as those of the corresponding configuration already described.

[0029] The present invention, which was devised to solve the above-mentioned problems, is a glass article manufacturing apparatus comprising a forming zone for forming a glass ribbon from molten glass, and a conveying zone for conveying the glass ribbon downstream of the forming zone, and is characterized in that it comprises an inspection unit that inspects the glass ribbon for the presence or absence of convex defects in which both the front and back surfaces are convex, and a control unit that adjusts the conveying speed of the glass ribbon in the conveying zone depending on the occurrence status of convex defects detected by the inspection unit.

[0030] According to this configuration, it is possible to obtain the same effects as those of the corresponding configuration already described. Effect of the Invention

[0031] According to the present invention, it is possible to reliably reduce the occurrence of convex defects in which both the front and back surfaces of a glass ribbon are convex. [Brief description of the drawings]

[0032] [Figure 1] 1 is a longitudinal sectional view of a glass article manufacturing apparatus according to a first embodiment of the present invention. [Diagram 2] FIG. 2 is a front view showing an example of a glass plate on which a convex defect is formed. [Diagram 3] 3 is a cross-sectional view taken along line AA in FIG. 2. [Figure 4] FIG. 13 is a diagram showing an example of a temperature region in which a convex defect is formed. [Diagram 5] FIG. 13 is a diagram showing an example of a temperature region in which a convex defect is formed. [Figure 6] FIG. 13 is a diagram showing an example of a temperature region in which a convex defect is formed. [Figure 7] FIG. 13 is a diagram showing an example of a temperature region in which a convex defect is formed. [Figure 8] FIG. 4 is a vertical cross-sectional view showing a countermeasure step included in a manufacturing method of a glass article according to a second embodiment of the present invention. [Figure 9] FIG. 11 is a longitudinal cross-sectional view showing a countermeasure step included in a manufacturing method of a glass article according to a third embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0033] Hereinafter, an embodiment of the present invention will be described based on the attached drawings. XYZ in the drawings is an orthogonal coordinate system. The X and Y directions are horizontal directions, and the Z direction is vertical. While the glass ribbon G is transported in a vertical position, the X direction may be the sheet thickness direction of the glass ribbon G, the Y direction may be the width direction of the glass ribbon G, and the Z direction may be the transport direction (sheet drawing direction) of the glass ribbon G. Note that, by attaching the same reference numerals to corresponding components in each embodiment, duplicated explanations may be omitted. When only a part of the configuration is described in each embodiment, the configuration of the other embodiment described above may be applied to the other parts of the configuration. In addition to the combination of the configurations clearly stated in the description of each embodiment, the configurations of multiple embodiments may be partially combined even if not clearly stated, as long as there is no particular problem with the combination.

[0034] First embodiment 1, the manufacturing apparatus for a glass article according to the first embodiment is an apparatus for manufacturing a glass sheet Gp as a glass article. The manufacturing apparatus includes a processing apparatus 1 for a glass ribbon G, a cutting apparatus 2, an inspection unit 3, and a control unit 4.

[0035] The processing apparatus 1 includes a forming zone 11 for continuously forming a glass ribbon G, a heat treatment zone 12 for heat treating (slowly cooling) the glass ribbon G, a cooling zone 13 for cooling the glass ribbon G to approximately room temperature, and roller pairs 14 provided in multiple stages above and below in each of the forming zone 11, the heat treatment zone 12, and the cooling zone 13. In this embodiment, the region from the lower end 15c of the formed body 15 to the folding position (cutting position) P2 is the transport zone for the glass ribbon G. That is, in this embodiment, the transport zone includes the heat treatment zone 12 and the cooling zone 13.

[0036] The forming zone 11 and the heat treatment zone 12 are constituted by a furnace in which the periphery of the transport path of the glass ribbon G is surrounded by walls, and heating devices such as heaters for adjusting the temperature of the glass ribbon G are arranged at appropriate positions within the furnace. On the other hand, the cooling zone 13 is open to the external atmosphere at room temperature without the periphery of the transport path of the glass ribbon G being surrounded by walls, and no heating device such as a heater is arranged therein. By passing through the heat treatment zone 12 and the cooling zone 13, the glass ribbon G is given a desired thermal history.

[0037] In the internal space of the forming zone 11, a forming body 15 is disposed, which forms a glass ribbon G from molten glass Gm by an overflow downdraw method. The molten glass Gm supplied to the forming body 15 overflows from a groove (not shown) formed in a top 15a of the forming body 15, and the overflowing molten glass Gm flows along both side surfaces 15b, which have a wedge-shaped cross section, of the forming body 15 and joins at a lower end 15c, thereby continuously forming a plate-shaped glass ribbon G. The formed glass ribbon G is in a vertical position (preferably in a vertical position). The glass ribbon G and the glass sheet Gp have substantially the same glass composition as the molten glass Gm.

[0038] In this embodiment, the molded body 15 is made of an alumina-based refractory. The alumina-based refractory is preferably a refractory having an Al2O3 content of 90 mass% or more. The molded body 15 may be made of a zirconia-based refractory or the like. However, in the case of a zirconia-based refractory, when molten glass Gm having a specific tempered glass composition is allowed to flow down, zirconia derived from the molded body 15 may be mixed into the molten glass Gm, causing defects in the glass ribbon G and / or the glass sheet Gp. Therefore, from the viewpoint of preventing the occurrence of defects due to such zirconia, the molded body 15 is more preferably made of an alumina-based refractory.

[0039] The internal space of the heat treatment zone 12 has a predetermined temperature gradient downward. The glass ribbon G in the vertical position is heat treated (slowly cooled) so that the temperature decreases as it moves downward through the internal space of the heat treatment zone 12. This heat treatment reduces internal distortion of the glass ribbon G. The temperature gradient in the internal space of the heat treatment zone 12 can be adjusted, for example, by a heating device provided on the inner wall surface of the heat treatment zone 12.

[0040] The roller pairs 14 are configured to pinch both ends of the glass ribbon G in the width direction in a vertical position from both the front and back sides. Of the roller pairs 14, the roller pair arranged at the top is a cooling roller 14a equipped with a cooling mechanism therein. Note that, in the internal space of the heat treatment zone 12, the roller pairs 14 may include ones that do not pinch both ends of the glass ribbon G in the width direction. In other words, the opposing distance between the roller pairs 14 may be made larger than the plate thickness of both ends of the glass ribbon G in the width direction, and the glass ribbon G may pass between the roller pairs 14.

[0041] In this embodiment, both widthwise ends of the glass ribbon G obtained by the processing device 1 include portions (hereinafter also referred to as "ear portions") that are thicker than the widthwise central portion due to the influence of shrinkage during the forming process.

[0042] The cutting device 2 includes a scribe line forming device 21 and a breaking device 22, and is configured to cut the glass ribbon G in a vertical position that has descended from the processing device 1 in the width direction at predetermined lengths. In this way, glass plates Gp are sequentially cut out from the glass ribbon G.

[0043] The glass plate Gp is ​​a glass original plate (mother glass plate) from which one or more product glass plates are obtained. The thickness of the glass plate Gp is, for example, 0.2 mm to 10 mm, and the size of the glass plate Gp is, for example, 700 mm x 700 mm to 3000 mm x 3000 mm. The glass plate Gp is ​​used, for example, as a substrate or cover glass of a display. Note that the substrate or cover glass of a display is not limited to a flat panel.

[0044] The scribe line forming device 21 is a device that forms a scribe line S on one of the front and back surfaces of the glass ribbon G at a scribe line forming position P1 provided below the processing device 1. In this embodiment, the scribe line forming device 21 includes a wheel cutter 23 that forms a scribe line S along one of the front and back surfaces of the glass ribbon G in its width direction, and a support member 24 (e.g., a support bar or a support roller) that supports the other of the front and back surfaces of the glass ribbon G at a position corresponding to the wheel cutter 23.

[0045] The wheel cutter 23 and the support member 24 are configured to descend following the descending glass ribbon G, while forming a scribe line S over the entirety or part of the width direction of the glass ribbon G. In this embodiment, the scribe line S is also formed on both ends in the width direction, including the ear portions where the plate thickness is relatively large. The scribe line S may be formed by irradiating a laser or the like.

[0046] The slicing device 22 is a device that slicing the glass ribbon G along the scribe line S at a slicing position P2 provided below the scribe line formation position P1 to obtain a glass sheet Gp. In this embodiment, the slicing device 22 includes a slicing member 25 that abuts against the formation region of the scribe line S from the side where the scribe line S is not formed, and a chuck 26 that grips a lower region of the glass ribbon G below the slicing position P2.

[0047] The breaking member 25 is composed of a plate-like body (plate) having a flat surface that descends following the descending glass ribbon G and contacts the entire or part of the width direction of the glass ribbon G. The contact surface of the breaking member 25 may be a curved surface that is curved in the width direction.

[0048] A plurality of chucks 26 are provided at both ends of the glass ribbon G in the width direction at intervals in the longitudinal direction of the glass ribbon G. All of the plurality of chucks 26 provided at each end in the width direction are held by the same arm (not shown). By the operation of each arm, the plurality of chucks 26 follow the glass ribbon G as it descends while bending the glass ribbon G with the breaking member 25 as a fulcrum. This imparts bending stress to the scribe line S and its vicinity, and the glass ribbon G is broken in the width direction along the scribe line S. As a result, a glass sheet Gp is ​​cut out from the glass ribbon G. The cut glass sheet Gp is ​​transferred from the chuck 26 to a chuck 28 of another conveying device 27, and then conveyed in the width direction (Y direction) while remaining in a vertical position. The conveying direction of the glass sheet Gp by the conveying device 27 is not limited to the width direction and can be set to any direction. The chucks 26 and 28 may be changed to another holding form such as negative pressure adsorption.

[0049] The inspection unit 3 is a device for inspecting the presence or absence of convex defects F shown in FIG. 2 and FIG. 3. The convex defects F are minute convex portions in which both the front and back surfaces of the glass plate Gp are convex. That is, the convex defects F formed on one surface of the glass plate Gp and the convex defects F formed on the other surface of the glass plate Gp are formed at approximately the same positions. At the formation position of the convex defects F, there are no internal defects such as bubbles or foreign matter defects. Since the convex defects F are surface defects, the inspection unit 3 can use a known inspection device for inspecting the presence or absence of surface defects. In addition to the convex defects F, the surface defects include, for example, scratches, stains, and protruding defects formed only on one of the front and back surfaces of the glass plate Gp.

[0050] As shown in FIG. 1, the inspection unit 3 inspects a glass plate Gp cut out from a glass ribbon G to check for the presence or absence of a convex defect F. In this embodiment, the inspection unit 3 includes a light source 31 arranged at a fixed position on one surface side of the front and back surfaces of the glass plate Gp, and a sensor 32 arranged at a fixed position on the other surface side of the front and back surfaces of the glass plate Gp. The light source 31 irradiates light toward the glass plate Gp, and the sensor 32 receives the light irradiated from the light source 31 and transmitted through the glass plate Gp. The inspection unit 3 detects the presence or absence of a surface defect based on a change in the amount of light received by the sensor 32.

[0051] The area that can be inspected by the light source 31 and the sensor 32 of the inspection unit 3 is a line extending in the Z direction. The inspection area by the light source 31 and the sensor 32 is scanned over the entire surface of each of the front and back surfaces of the glass plate Gp by moving the glass plate Gp by the conveying device 27. This allows the presence or absence of surface defects, including the convex defect F, to be inspected. The glass plate Gp in which a surface defect has been detected is sampled from the conveying path of the conveying device 27 in order to identify the type of the surface defect. A white light interference microscope (such as VertScan (registered trademark) manufactured by Ryoka Systems Co., Ltd.) can be used to identify the type of surface defect. As a result, when the cross-sectional shape of the surface defect of the glass plate Gp is ​​observed with the white light interference microscope and a convex portion that satisfies a predetermined judgment criterion is detected on the front and back surfaces, it can be judged that the convex defect F is formed on the glass plate Gp. The judgment criterion is set to a value that takes into account the size of the detected convex portion, such as the height in the plate thickness direction, the length in the conveying direction, and the width in the direction perpendicular to the conveying direction, of the detected convex portion.

[0052] 2 and 3, the convex defect F has a streak shape extending along the conveying direction (sheet drawing direction) and has, for example, a height T in the sheet thickness direction of 1 nm to 1 μm, a length L in the conveying direction of 0.1 to 100 mm, and a width W in the direction perpendicular to the conveying direction of 0.1 to 10 mm. The length L of the convex defect F increases when the conveying speed of the glass ribbon G is increased, and decreases when the conveying speed of the glass ribbon G is decreased.

[0053] It is known that the incidence rate of convex defects F varies depending on the residence time of the glass ribbon G in the high-temperature region H (see FIGS. 4 to 7) near the forming body 15. In other words, as the residence time of the glass ribbon G in the high-temperature region H increases, the occurrence of convex defects F tends to increase (see Table 1 below).

[0054] The high temperature region H in which the convex defect F may be formed may have four modes as shown in Figs. 4 to 7. That is, in the first mode, the high temperature region H is from the middle position of the side surface 15b of the formed body 15 to the lower position of the cooling roller 14a as shown in Fig. 4. In the second mode, the high temperature region H is from the middle position of the side surface 15b of the formed body 15 to the lower position of the lower end 15c of the formed body 15 and above the cooling roller 14a as shown in Fig. 5. In the third mode, the high temperature region H is from the lower position of the lower end 15c of the formed body 15 to the upper position of the cooling roller 14a as shown in Fig. 6. In the fourth mode, the high temperature region H is from the lower position of the lower end 15c of the formed body 15 and above the cooling roller 14a to the lower position of the cooling roller 14a as shown in Fig. 7. In any mode, if the conveying speed (sheet drawing speed) of the glass ribbon G is increased, the temperature gradient in the vertical direction of the glass ribbon G is maintained constant, and therefore the residence time of the high temperature region H can be shortened.

[0055] Here, the convex defect F is thought to be caused by the following two reasons. That is, the first reason is thought to be due to the phase separation of glass occurring in the above-mentioned high temperature region H. This is because the convex defect F tends to increase when a glass composition that is likely to cause phase separation is selected. For this reason, the high temperature region H may be set based on the temperature at which the glass phase separates. The second reason is thought to be due to the diffusion (migration) of Mg ions from the molded body 15 to the molten glass Gm. This diffusion of Mg ions is more likely to occur as the temperature of the molten glass Gm increases, such as in the above-mentioned high temperature region H. The cause of the generation of the convex defect F has not yet been clearly elucidated, but the above-mentioned second cause is the most likely.

[0056] When the molten glass Gm (glass ribbon G) is an aluminosilicate glass with an MgO content of less than 1% by mass, the convex defect F is likely to occur in the glass ribbon G. Specifically, when the molten glass Gm contains, in mass%, SiO2 50-80%, Al2O3 5-25%, B2O3 0-15%, Na2O 1-20%, K2O 0-10%, P2O5 0.5-10%, and Li2O 0-5%, the convex defect F is likely to occur in the glass ribbon G. In this glass composition, the high temperature region H where the convex defect F can be formed is, for example, 800 to 1100°C. In addition, by restricting the glass composition range as described above, the glass ribbon G can easily achieve both ion exchange performance and devitrification resistance at a high level. Therefore, the glass ribbon G is obtained that is suitable for a chemically strengthened glass plate used for cover glass of mobile phones, digital cameras, PDAs (personal digital assistants), touch panel displays, and the like.

[0057] The lower the MgO content, the more likely the convex defect F is to occur, and the more pronounced the effect of the present invention in reducing the convex defect F. For this reason, the MgO content is more preferably 0.9% by mass or less, and even more preferably 0.5% by mass or less. The MgO content may be 0% by mass.

[0058] P2O5 is a component that enhances ion exchange performance when chemically strengthening glass, and in particular increases the stress depth of the compressive stress layer. As the content of P2O5 increases, glass becomes more susceptible to phase separation and convex defects F are more likely to occur. The lower limit of P2O5 is preferably 2%, more preferably 4%. On the other hand, the upper limit of P2O5 is preferably 8%, more preferably 6%.

[0059] Li2O is an ion exchange component, and also a component that reduces high-temperature viscosity and improves melting and moldability. It is also a component that increases Young's modulus. Furthermore, among alkali metal oxides, it has a large effect of increasing the compressive stress value. However, if the Li2O content is too high, the liquidus viscosity decreases and the glass becomes more susceptible to devitrification. In addition, the thermal expansion coefficient becomes too high, which reduces the thermal shock resistance and makes it difficult to match the thermal expansion coefficient of surrounding materials. Furthermore, if the low-temperature viscosity decreases too much and stress relaxation becomes more likely to occur, the compressive stress value may actually become smaller. Therefore, the Li2O content is preferably 0 to 3.5%, 0 to 2%, 0 to 1%, 0 to 2% or 0. ~0.5%, especially 0.01-0.2%.

[0060] 1, the control unit 4 is configured to adjust the conveying speed (sheet drawing speed) of the glass ribbon G depending on the occurrence status of the detected convex defects F. In detail, when the occurrence of the convex defects F increases, the control unit 4 increases the rotation speed of the cooling rollers 14a to increase the conveying speed of the glass ribbon G.

[0061] The control unit 4 is configured to increase the flow rate of the molten glass Gm supplied to the forming body 15 when increasing the conveying speed of the glass ribbon G. At this time, the flow rate of the glass ribbon G may be finely adjusted so as to prevent a decrease in the sheet thickness of the glass ribbon G associated with an increase in the conveying speed.

[0062] Next, a method for manufacturing a glass article using the glass article manufacturing apparatus configured as above will be described.

[0063] The method for manufacturing a glass article according to this embodiment includes a forming step, a heat treatment step, a cooling step, a cutting step, an inspection step, and a countermeasure step. Note that the heat treatment step, the cooling step, and a part of the cutting step also serve as a conveying step for conveying the glass ribbon G.

[0064] The forming step is a step of forming a glass ribbon G in a forming zone 11 .

[0065] The heat treatment step is a step in which the glass ribbon G that has been subjected to the forming step is subjected to a heat treatment in the heat treatment zone 12.

[0066] The cooling step is a step of cooling the glass ribbon G that has been subjected to the heat treatment step in the cooling zone 13.

[0067] The cutting step is a step in which the glass ribbon G that has been subjected to the cooling step is conveyed and cut in the width direction by a cutting device 2 to obtain a glass sheet Gp.

[0068] The inspection step is a step of inspecting the glass plate Gp for the presence or absence of a convex defect F by the inspection unit 3 or the like. In the inspection step, the presence or absence of a convex defect F is inspected according to a predetermined judgment criterion.

[0069] The countermeasure process is a process of taking measures to reduce the convex defect F of the glass ribbon. In the present embodiment, the countermeasure process includes a control process of adjusting the conveying speed of the glass ribbon G according to the occurrence state of the convex defect F detected in the inspection process.

[0070] In the control step, when the occurrence of the convex defect F increases, the conveying speed of the glass ribbon G is increased by the cooling roller 14a, and the occurrence of the convex defect F is controlled to a predetermined target value or less. Here, the target value can be set to any parameter related to the convex defect F, such as the occurrence rate of the glass sheet Gp having the convex defect F, the number of glass sheets Gp having the convex defect F, and the number of convex defects F per glass sheet Gp. In this way, when the occurrence of the convex defect F increases, the conveying speed of the glass ribbon G is increased, so that the residence time of the glass ribbon G in the high temperature region H near the forming body 15 is shortened. In this case, the contact time between the forming body 15 and the molten glass Gm is also shortened, so that the amount of Mg ions diffusing from the forming body 15 to the molten glass Gm is inevitably reduced, even if the refractory of the forming body 15 contains MgO. Therefore, the convex defect F of the glass ribbon G can be reliably reduced.

[0071] Conversely, if the conveying speed of the glass ribbon G is reduced, the residence time of the glass ribbon G in the high temperature region H near the forming body 15 becomes longer. As a result, the contact time between the forming body 15 and the molten glass Gm also becomes longer, and therefore, when the refractory material of the forming body 15 contains MgO, the amount of Mg ions diffusing from the forming body 15 to the glass ribbon Gm also inevitably increases. Therefore, the convex defect F of the glass ribbon G may increase.

[0072] Moreover, in the control process, when the occurrence of the convex defects F increases, in addition to increasing the conveying speed of the glass ribbon G, the flow rate of the molten glass Gm supplied to the forming body 15 is also increased. In this way, a decrease in the thickness of the glass ribbon G due to an increase in the conveying speed can be prevented, and the thickness of the glass ribbon G can be maintained constant.

[0073] Second Embodiment FIG. 8 is a diagram showing a countermeasure step included in the method for producing a glass article according to the second embodiment.

[0074] In the present embodiment, the countermeasure step includes a selection step of selecting a refractory material substantially free of MgO as the refractory material of the formed body 15 before forming the glass ribbon G that becomes the product.

[0075] The content of MgO in the molded body 15 is, for example, preferably 1 mass% or less, and more preferably 0.5 mass% or less. The content of MgO in the molded body 15 may be 0 mass%. When an alumina-based refractory is used as the refractory of the molded body 15, the content of MgO is less than the content of Al2O3.

[0076] If a refractory material substantially free of MgO is selected as the formed body 15 in this manner, the MgO concentration in the entire formed body 15 will be low or zero. As a result, an MgO-free layer R1 substantially free of MgO will be present in at least a surface layer portion including the surface of the formed body 15. Therefore, even if the glass ribbon G is an aluminosilicate glass with an MgO content of less than 1 mass %, the diffusion of Mg ions from the formed body 15 to the molten glass Gm is suppressed, and the convex defect F in the glass ribbon G can be reliably reduced.

[0077] Third embodiment FIG. 9 is a diagram showing a countermeasure step included in the method for producing a glass article according to the third embodiment.

[0078] In this embodiment, the countermeasure process includes a formation process of forming an MgO-free layer R2 that is substantially free of MgO on the surface of the molded body 15 (e.g., the top 15a and the side surface 15b) prior to the molding process of forming the glass ribbon G that will become the product.

[0079] The MgO content in the MgO-free layer R2 is, for example, preferably 1 mass % or less, and more preferably 0.5 mass % or less, and may be 0 mass %.

[0080] The thickness of the MgO-free layer R2 is preferably 100 μm or less, more preferably 20 μm to 100 μm, and most preferably 50 μm to 100 μm.

[0081] An example of the MgO-free layer R2 is an alumina layer. The alumina layer can be formed by flowing molten glass substantially free of MgO (e.g., MgO content is less than 0 to 1 mass %) down along the surface of the formed body 15 made of an alumina-based refractory material containing MgO. The molten glass substantially free of MgO used in the forming step preferably has the same or similar glass composition as the molten glass Gm substantially free of MgO used in the molding step.

[0082] By forming the MgO-free layer R2 on the surface of the formed body 15 in this manner, a layer that does not substantially contain MgO is interposed between the formed body 15 and the molten glass Gm. Therefore, the diffusion of Mg ions from the formed body 15 to the molten glass Gm is suppressed, and the convex defect F in the glass ribbon G can be reliably reduced.

[0083] In the forming step, it is preferable to flow the molten glass Gm while maintaining it at a temperature higher than the normal operating temperature (the temperature of the molten glass Gm in the forming step). This allows the MgO contained in the molded body 15 made of an alumina-based refractory to easily move from the surface of the molded body 15 to the molten glass Gm. As a result, the surface of the molded body 15 (strictly speaking, the surface layer including the surface) can be made into a refractory material that does not substantially contain MgO (MgO-free layer R2).

[0084] Here, the inventors of the present application have confirmed through extensive research that the time required for the MgO in the surface layer of the formed body 15 to be substantially completely transferred into the molten glass Gm is significantly shorter when the temperature of the molten glass Gm is 1250°C or higher than when the temperature of the molten glass Gm is less than 1250°C. Therefore, the temperature of the molten glass Gm in the forming step is preferably 1250°C or higher. In addition, the time of the forming step is preferably 72 hours or longer. However, if the temperature of the molten glass Gm is raised too high, creep of the formed body 15 may occur, so the temperature of the molten glass Gm in the forming step is preferably 1300°C or lower.

[0085] Furthermore, when the formed body 15 made of an alumina-based refractory contains MgO, spinel and alumina are often formed on the surface of the formed body 15, and in addition to the convex defect F, these may flow out as foreign matter into the glass ribbon G to be the product. However, by setting the temperature of the molten glass Gm in the forming step to 1250°C or higher, it is expected that the spinel and alumina formed on the surface of the formed body 15 can be washed away before the forming step of forming the glass ribbon G to be the product. In other words, it is expected that the effect of reducing the occurrence of defects originating from spinel, alumina, etc. in the glass ribbon G to be the product can be achieved.

[0086] The MgO-free layer R2 is not limited to an alumina layer, but may be any layer that can suppress the migration of Mg ions to the molten glass Gm. For example, a silica layer or a zirconia layer may be used as the MgO-free layer R2. The method for forming the MgO-free layer R2 is not limited to the above-mentioned method, but may be, for example, a sputtering deposition method.

[0087] Although a glass article manufacturing apparatus and a method for manufacturing the same according to an embodiment of the present invention have been described, the embodiment of the present invention is not limited thereto, and various modifications can be made without departing from the gist of the present invention.

[0088] In the above embodiment, the glass ribbon G is cut by scribe cleavage, but it may be cut by other methods such as laser cleavage or laser melting.

[0089] In the above embodiment, a cutting step of cutting the edge portions of the glass plate Gp may be further provided prior to the inspection step of inspecting for the presence or absence of the convex defect F.

[0090] In the above embodiment, in addition to the first inspection step of inspecting the presence or absence of the convex defect F, a second inspection step of inspecting the presence or absence of other defects such as bubbles or foreign matter in the glass plate Gp may be carried out.

[0091] In the above embodiment, the glass article is a glass sheet Gp. However, the glass article may be, for example, a glass roll obtained by winding a glass ribbon G into a roll.

[0092] In the above embodiment, a case has been described in which the control unit 4 automatically adjusts the conveying speed of the glass ribbon G according to the occurrence status of the detected convex defect F. However, an operator may manually adjust the conveying speed of the glass ribbon G or the flow rate of the molten glass Gm according to the occurrence status of the detected convex defect F.

[0093] In the above-described embodiment, the method for producing a glass article may further include a strengthening step of chemically strengthening the glass plate Gp (glass plate for chemical strengthening).

[0094] In the above embodiment, the case where the molten glass Gm is an aluminosilicate glass is illustrated, but the molten glass Gm is not limited to this. EXAMPLES

[0095] The results of the evaluation test show that the incidence of convex defects, in which both the front and back surfaces are convex, decreases when the conveying speed of the glass ribbon is increased. In the evaluation test, the flow rate of molten glass during forming was kept constant, and the conveying speed of the glass ribbon was changed to examine how the incidence of convex defects (number of glass sheets with convex defects / number of glass sheets inspected) changed. At this time, if there was even one convex defect in the glass sheet, it was counted as a glass sheet with a convex defect. The results are shown in Table 1. The conveying speed is shown as a relative value with the conveying speed of Example 3 as the reference (the conveying speed of Example 3 is 1).

[0096] The glass plate according to each example is an aluminosilicate glass that does not substantially contain MgO, and the glass composition includes, in mass%, SiO2 52%, Al2O3 27%, B2O3 0.1%, Na2O 7.0%, K2O 0.6%, MgO 0.1%, P2O 58.8%, Li2O 3.0%, and SnO2 0.1%. The size of the glass plate according to each example is 2350 mm x 2560 mm. In addition, an alumina molded body with an MgO content of 5 mass% was used as the molded body.

[0097] [Table 1]

[0098] According to Table 1, the incidence rate of convex defects is (Example 1)>(Example 2)>(Example 3), and it can be recognized that as the conveying speed (plate drawing speed) increases, the incidence rate of convex defects tends to decrease.

[0099] Next, Example 4 was carried out according to the third embodiment described above. In Example 4, a molded body similar to the molded body used in Examples 1 to 3 was used, and in the countermeasure step of Example 4, an MgO-free layer (alumina layer) substantially free of MgO was formed on the surface of the molded body. The alumina layer was formed by causing the above-mentioned aluminosilicate glass substantially free of MgO to flow down onto the surface of the molded body. The MgO content of the alumina layer was 0 mass %. Using this molded body 15, a glass plate was obtained under the conditions of Example 3 described above. As a result, in Example 4, the convex defect occurrence rate was lower than that of Example 1. [Explanation of symbols]

[0100] 1 Processing equipment 2 Cutting device 3. Inspection Department 4. Control Unit 11 Forming Zone 12 Heat Treatment Zone 13 Cooling Zone 14a Roller pair (cooling roller) 15 Molded body 21 Scribing line forming device 22 Folding device 23 Wheel Cutter 24 Support member 25 Folding material 27 Transport Equipment F Convex defect G Glass ribbon Gm Molten Glass Gp Glass Plate R1 MgO-free layer R2 MgO-free layer

Claims

1. A method for producing a glass article, comprising: a forming step of forming a glass ribbon from molten glass; and a conveying step of conveying the glass ribbon that has been subjected to the forming step, an inspection step of inspecting the glass ribbon for the presence or absence of a convex defect in which both the front and back surfaces are convex; and a countermeasure step of taking measures to reduce the convex defects, The countermeasure step includes a control step of adjusting a conveying speed of the glass ribbon in the conveying step according to an occurrence state of the convex defect detected in the inspection step, The method for manufacturing a glass article, characterized in that, in the control step, a conveying speed of the glass ribbon is increased when the occurrence of the convex defects increases.

2. The method for manufacturing a glass article according to claim 1 , characterized in that, in the control step, the flow rate of the molten glass in the forming step is increased when the conveying speed of the glass ribbon is increased.

3. In the forming step, the molten glass is caused to flow down along a surface of a forming body by a down-draw method to form the glass ribbon; The method for manufacturing a glass article as described in claim 1 or 2, characterized in that in the control process, the rotation speed of cooling rollers that clamp both ends of the glass ribbon in the width direction from both sides directly below the forming body is adjusted depending on the occurrence status of the convex defect detected in the inspection process.

4. A method for manufacturing a glass article, comprising: a forming step of forming a glass ribbon from molten glass; and a transporting step of transporting the glass ribbon that has been subjected to the forming step, an inspection step of inspecting the glass ribbon for the presence or absence of a convex defect in which both the front and back surfaces are convex; and a countermeasure step of taking measures to reduce the convex defects, In the forming step, the molten glass is caused to flow down along a surface of a forming body by a down-draw method to form the glass ribbon; The method for producing a glass article, wherein the countermeasure step comprises a forming step of forming, in advance, an MgO-free layer that is substantially free of MgO on a surface of the molded body.

5. The method for producing a glass article according to claim 4, wherein the MgO-free layer is an alumina layer.

6. The method for producing a glass article according to claim 5, wherein the formed body is made of an alumina-based refractory material.

7. The method for manufacturing a glass article according to any one of claims 1 to 6, characterized in that the molten glass is an aluminosilicate glass having an MgO content of less than 1 mass %.

8. The molten glass has a glass composition, in mass%, of SiO 2 50-80%, Al 2 O 3 5-25%, B 2 O 3 0-15%, Na 2 O 1-20%, K 2 O 0-10%, P 2 O 5 0.5-10%, Li 2 The method for producing a glass article according to claim 7, characterized in that it contains 0 to 5% of O.

9. The method for manufacturing a glass article according to any one of claims 1 to 8, characterized in that the convex defect has a height of 1 nm to 1 µm, a length of 0.1 to 100 mm, and a width of 0.1 to 10 mm.

Citation Information

Patent Citations

  • Method and apparatus for producing glass sheet

    JP2013151415A

  • Glass substrate manufacturing method, and glass substrate manufacturing apparatus

    JP2016190764A

  • Production method of glass substrate

    JP2017014054A

  • Coated, chemically strengthened, thin, flexible glass

    JP2017529305A

  • Method and equipment for manufacturing glass article

    JP2018062433A