Amine-Based Primer Coatings for Electrophotographic Printing
Amine-functionalized copolymers in primer compositions address the adhesion and stability issues in liquid electrophotographic printing by promoting strong chemical interactions and reducing water solubility, resulting in improved toner adhesion and resistance.
Patent Information
- Application Number
- JP2022502826
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-07-18
- Filing Date
- 2020-07-15
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-07-15
AI Technical Summary
Liquid electrophotographic printing faces challenges with insufficient adhesion of images to certain substrates, particularly due to weak chemical interactions between toner particles and primer coatings, which can lead to poor water resistance and discoloration over time.
Development of primer compositions featuring amine-functionalized copolymers with controlled amine content, formulated to promote strong chemical interactions with toner particles while minimizing water solubility and discoloration, using emulsion polymerization techniques to create a primer coating on various substrates.
The primer compositions enhance adhesion of toner to substrates, providing improved water resistance and stability, with consistent adhesion across different colored toners and substrates, as demonstrated by tape pull tests.
Smart Images

Figure 0007570707000001 
Figure 0007570707000002 
Figure 0007570707000003
Abstract
Description
[Technical field]
[0001] CROSS-REFERENCE TO RELATED APPLICATIONS
[0001] This application claims the benefit of priority under 35 U.S.C. § 119 from Luxembourg Patent Application No. 1,101,319, filed July 18, 2019, which is incorporated by reference in its entirety herein. [Background technology]
[0002] On-demand digital printing machines based on liquid electrophotography systems are widely used in modern laser printing and copier systems. Electrophotography systems form a latent image on a photosensitive drum, and then liquid toner is applied to the latent image on the drum to form a physical image for subsequent transfer. HP ELECTROINK, an ethylene / acrylic copolymer composition, is an example of a common liquid toner system. After toner exposure, the image is electrically transferred to an intermediate transfer blanket or belt for printing onto a fibrous substrate, such as paper or a polymeric film substrate. Although high quality images can be achieved with liquid electrophotography, the transferred image usually does not adhere well to a fibrous substrate unless the substrate has been previously treated with a suitable primer coating. The primer coating is usually selected to contain suitable functional groups to promote chemical interaction with complementary organic functional groups in the toner to promote strong chemical adhesion of the toner to the surface of the substrate. Proper substrate adhesion is also an important factor of the primer coating.
[0003]
[0003] Toner adhesion failure may occur for any number of reasons. In one example, incomplete fusion of toner particles to the surface of the substrate may lead to poor adhesion. And more commonly, toner particles within the transferred image may only weakly interact with the substrate or the primer coating thereon, resulting in poor surface adhesion. Limited chemical interaction between the toner particles and the primer coating may result in poor toner adhesion. Thus, functional groups present within the primer coating may be selected to promote strong chemical interactions, such as hydrogen bonding or salt bridge formation, with complementary functional groups within the toner. Functional groups such as carboxylic acids, amines and alcohols may be particularly suitable in this regard, since these types of functional groups can both donate and accept hydrogen bonds. If the primer coating is too hydrophilic due to the presence of excess functional groups that can donate or accept hydrogen bonds, the primer coating may have poor water resistance. In addition to poor water resistance, some polymers with excessive amounts of amine functionality may corrode gently over time and / or may be subject to discoloration (especially yellowing), thereby limiting the applicability of these polymers, even though they often provide good toner adhesion. Summary of the Invention [Problem to be solved by the invention]
[0004]
[0004] This disclosure relates generally to primer compositions for liquid electrophotographic printing, and more particularly to primer compositions and primer-coated substrates that are characterized by polymers having specific amine content and methods for making the same.
[0005]
[0005] As discussed above, liquid electrophotography is a very powerful imaging technology. However, transferring an electrophotographic image to certain substrates can be problematic due to poor adhesion of the image to the substrate surface. Similarly, substrate adhesion can be problematic in some instances. Primer coatings can be used to improve adhesion of the image to the substrate, but some primer coatings exhibit limited water resistance or may discolor over time, thereby limiting their practical use. [Means for solving the problem]
[0006]
[0006] The present disclosure describes primer compositions that can be used to form primer coatings on a variety of substrates, including polymeric and paper substrates. The primer compositions disclosed herein feature amine-functionalized copolymers having a sufficient number of amine groups on the side chains to promote adhesion of toners, particularly HP ELECTROINK toners, while limiting the amount of amine groups to loadings or below loadings where coating robustness (due to excessive water solubility) or discoloration over time becomes an issue. In particular, the primer compositions disclosed herein feature amine-functionalized copolymers having an amine value of about 10 to about 180 mg KOH / g copolymer. The amine-functionalized copolymers may be copolymers of two or more ethylenically unsaturated monomers, where the ethylenic unsaturation can undergo polymerization to produce a saturated polymer backbone resulting from each monomer, at least one of the monomers having an amine-containing side chain. The amine value can be calculated or determined experimentally, as specified below.
[0007] In the present disclosure, the "amine value" can be determined by taking the weight fraction of the amine-containing monomer in the amine-functionalized copolymer, dividing by the molecular weight of the amine-containing monomer, multiplying by the molecular weight of KOH, and finally multiplying the result by 1000. The empirical amine value can also be experimentally verified, for example, by performing a potentiometric titration. In calculating the amine value, the weight fraction of the amine-containing monomer can be corrected for the calculation if not all of the amine is present as a free amine. As used herein, a "free amine" is not an amine salt, but contributes to the "amine value". The term "free amine" refers to any primary, secondary, or tertiary amine in which a non-bonded lone pair of electrons is present, and the amine is not protonated or quaternized and has a positive charge. That is, the "free amine" maintains its basicity. However, it is understood that in addition to free amines, protonated, quaternized, and / or similarly functionalized amine groups can be present in the primer compositions disclosed herein, provided that the amount of free amine remains sufficient to designate the amine value in the aforementioned range. Protonation of the amine may result from externally added acid and / or from the presence of olefinically unsaturated monomers with acidic side chains, as discussed further below. The effect of acid or quaternizing groups in lowering the amine value can be determined by calculating the number of moles of acid or quaternizing groups present, subtracting from the number of moles of amine-containing monomer present, and then calculating the amine value as described above. Amine derivatives such as amides are similarly no longer basic and do not contribute to the amine value disclosed herein.
[0008]
[0008] As a non-limiting example, if none of the amine groups are protonated (e.g., from exogenously added acid and / or monomers with acidic side chains), then an amine number of about 10 mg KOH / g polymer to about 180 mg KOH / g polymer corresponds to a loading of about 3 wt.% to about 52 wt.% for an amine-functionalized copolymer with the amine-containing monomer dimethylaminoethyl methacrylate. In the absence of monomers with acidic side chains and / or functionalization to remove the basicity of the amino groups, if the pH is high enough for the amine groups to remain substantially unprotonated, there can be a direct correlation between the amine number and the weight percentage of amine-containing monomers present.
[0009] Monomers with acidic side chains, such as carboxylic or sulfonic acids, can be present in the amine-functionalized copolymer, provided that the amount of such acidic monomers is sufficiently low and the amine value remains within the aforementioned range (i.e., a sufficiently low number of amine groups are internally protonated by the acidic groups). If the amount of acidic monomers is too high relative to the number of amine groups present, the amine value may be reduced to such an extent that poor toner adhesion to the primer coating occurs. For example, it may be desirable to incorporate a limited amount of carboxylic acid groups into the amine-functionalized copolymer to promote adhesion of the primer coating itself to certain types of substrates, such as paper substrates. Carboxylic acid groups may also improve compatibility with additives commonly and conventionally used in the printing industry. Similarly, it may be desirable to limit the overall number of amine groups in the amine-functionalized copolymer to avoid discoloration and excessive hydrophilicity. Thus, finding a balance between substrate adhesion and toner adhesion can be achieved by judicious consideration of how to achieve a suitable amine value, as provided in the present disclosure.
[0010]
[0010] The primer compositions disclosed herein may offer several advantages over polyethyleneimine, which has previously been used in primer coatings to promote adhesion of toners, including HP INDIGO toner. The amine-functionalized copolymers of the present disclosure may be formulated to have significantly fewer amine groups than with polyethyleneimine, thereby reducing the susceptibility of the primer coating to water degradation and / or discoloration over time. Additionally, significant structural resistance exists in the amine-functionalized copolymers disclosed herein, provided the amine number remains within the aforementioned range.
[0011] The primer composition described herein can be easily prepared by emulsion polymerization techniques by combining one or more first ethylenically unsaturated monomers lacking an amine group with one or more second ethylenically unsaturated monomers containing at least one amine group. A variety of single monomers or a variety of multiple monomers can undergo polymerization in the present disclosure. The ratio (molar or weight ratio) between the first ethylenically unsaturated monomer and the second ethylenically unsaturated monomer can be easily varied to suit the amine value and / or hydrophobicity of the resulting copolymer in the primer composition, as a non-limiting example. The presence of both hydrophilic and hydrophobic monomers in the copolymer can help promote toner adhesion and chemical resistance, as a non-limiting example. Although polymerization techniques other than emulsion polymerization can be used to prepare the copolymers of the present disclosure, copolymer emulsions made in the same manner can be advantageous because they can be directly applied to the desired substrate to form a primer coating, optionally after combining with a polyvalent metal salt to promote inkjet printing. The copolymer emulsion is also compatible with various types of starches to promote adhesion of primer coatings on paper substrates, as a non-limiting example.
[0012] The primer compositions and primer coatings formed therefrom described herein may be particularly effective in promoting adhesion of HP INDIGO toner. Adhesion can be comparatively assayed using a tape pull test as specified in ASTM F2252 / F2252M and further described in modified form herein. Advantageously, the primer compositions described herein demonstrate fairly limited adhesion variability between different color HP INDIGO toners, in contrast to many other types of primer compositions. Primarily, the primer coatings of the present disclosure provide comparable adhesion between black and color toners. Other types of primer coatings may have difficulty passing the tape pull test with both types of toners.
[0013]
[0013] Thus, the primer composition of the present disclosure may include a fluid, particularly an aqueous fluid, and an amine-functionalized copolymer dispersed therein. The amine-functionalized copolymer comprises the polymerization reaction product of one or more first ethylenically unsaturated monomers lacking an amine group and one or more second ethylenically unsaturated monomers having at least one amine group, such that at least one amine group comprises a side chain of the amine-functionalized copolymer. The amine-functionalized copolymer further has an amine value of about 10 to about 180 mg KOH / g copolymer, or about 30 to about 160 mg KOH / g copolymer, or about 50 to about 60 mg KOH / g copolymer, or about 60 to about 80 mg KOH / g copolymer, or about 80 to about 100 mg KOH / g copolymer, or about 100 to about 115 mg KOH / g copolymer, or about 115 to about 130 mg KOH / g copolymer, or about 130 to about 150 mg KOH / g copolymer. Other examples of such amine-functionalized copolymers may have an amine value of about 70 to about 140 mg KOH / g copolymer. The amine value range represents a compromise between providing particularly effective toner and substrate adhesion at the lower end of the range and not providing an amine-functionalized copolymer that is overly hydrophilic (i.e., prone to being overly water soluble) at the upper end of the range. The primer compositions disclosed herein may be particularly suitable for use in liquid electrophotographic printing.
[0014] The amine-functionalized copolymer can be dissolved in an aqueous fluid or dispersed as an emulsion in an aqueous fluid. Emulsions prepared in an essentially organic medium (e.g., water-in-oil emulsions) are also within the scope of the present disclosure. Advantageously, the amine-functionalized copolymer can be readily prepared using emulsion polymerization to directly form the primer composition as an emulsion polymerization reaction mixture, as discussed in more detail below. Other polymerization techniques suitable for use in the present disclosure include, for example, bulk or solution polymerization. In any polymerization technique, the polymerization can be initiated with a suitable radical initiator, illustrative examples of which are provided herein below.
[0015] More specific examples of the primer compositions disclosed herein may include emulsion-polymerized amine-functionalized copolymers dispersed as an emulsion within an aqueous fluid. The amine-functionalized copolymers include the polymerization reaction product of one or more first ethylenically unsaturated monomers lacking an amine group and one or more second ethylenically unsaturated monomers having at least one amine group, such that at least one amine group constitutes a side chain of the amine-functionalized copolymer, and the amine-functionalized copolymers further have an amine value of about 70 to about 140 mg KOH / g copolymer and a glass transition temperature of about 0° C. to about 50° C. Other specific examples may include amine-functionalized copolymers having an amine value in the range of about 10 to about 180 mg KOH / g copolymer and a glass transition temperature of about 0° C. to about 50° C., or any other suitable range of amine values disclosed herein. The glass transition temperature (T g ) can be determined by differential scanning calorimetry using a DSC3+ instrument (Mettler Toledo) using a scan period consisting of an initial cooling to -60°C at a 20°C / min ramp, a 5 minute stabilization period at this temperature, heating at a 20°C / min ramp to a temperature of 120°C / min, and a second 5 minute stabilization period at this temperature.
[0016] Aqueous fluids suitable for use in the present disclosure may include water or water mixed with a water-miscible organic solvent such as an alcohol or glycol.
[0017] The aqueous fluids of the present disclosure may have a non-acidic pH to maintain the amine value of the amine-functionalized copolymer within the aforementioned range. That is, the aqueous fluids of the present disclosure may have a pH of about 7 or greater. In more specific examples, the aqueous fluids may have a pH in the range of about 7 to about 10, or about 7.5 to about 10, or about 8 to about 10, or about 8.5 to about 10, or about 9 to about 10, or about 9.5 to about 10, or about 7.5 to about 9.5, or about 7.5 to about 9, or about 7.5 to about 8.5, or about 7.5 to about 8, or about 8 to about 9.5, or about 8 to about 9, or about 8 to about 8.5, or about 8.5 to about 9.5, or about 8.5 to about 9.5. At the aforementioned pH values, the amine groups in the amine-functionalized copolymer may not be protonated at all, each contributing to the amine value. The pH values in this disclosure can be measured at room temperature with a glass electrode using 1 M KCl electrolyte solution, calibrated to pH 4, pH 7 and pH 10 standards before use. A SENSION+ PH3 instrument from Hach was used.
[0017]
[0018] At pH values below 7, a portion of the amine groups may be protonated, reducing the amine value below that theoretically possible based on the total number of amine groups present, although pH values below 7 are acceptable in this disclosure, provided that the amine value remains within the ranges specified above. Also, as specified below, ethylenically unsaturated monomers having acidic groups may be present in limited amounts, which may also reduce the amine value below that theoretically possible based on the total number of amine groups present.
[0018]
[0019] The ethylenically unsaturated monomer containing at least one amine group may contain any one or more of primary amines, secondary amines or tertiary amines as appropriate. At least one amine group may be added to the ethylenically unsaturated monomer so that when polymerized with an ethylenically unsaturated monomer lacking an amine group, at least one amine is incorporated as a side chain of the amine-functionalized copolymer. Specific examples of ethylenically unsaturated monomers containing at least one amine group that may be suitable for use in the present disclosure include, for example, 2-(dimethylamino)ethyl methacrylate, 3-(dimethylamino)propyl methacrylate, 2-(diethylamino)ethyl methacrylate, 3-(diethylamino)propyl methacrylate, 2-(ethylamino)ethyl methacrylate, 3-(ethylamino)propyl methacrylate, 2-(methylamino)ethyl methacrylate, 3-(methylamino)propyl methacrylate, 2-(tert-butylamino)ethyl methacrylate, 3-(tert-butyl ... Methacrylate, 2-(dimethylamino)ethyl methacrylamide, 3-(dimethylamino)propyl methacrylamide, 2-(diethylamino)ethyl methacrylamide, 3-(dimethylamino)propyl methacrylamide, 2-(methylamino)ethyl methacrylamide, 3-(methylamino)propyl methacrylamide, 2-(ethylamino)ethyl methacrylamide, 3-(ethylamino)propyl methacrylamide, 2-(tert-butylamino)ethyl methacrylamide, 3-(tert-butylamino)propyl methacrylamide, vinylamine, allylamine and any combination thereof. The corresponding acrylamide-based monomers may also be suitable in certain circumstances, especially 2-(dimethylamino)ethyl acrylate. Thus, in any embodiment of the present disclosure, the one or more second ethylenically unsaturated monomers having at least one amine group may include an acrylamide or methacrylamide monomer having at least one amine group. In certain examples, all of the one or more second ethylenically unsaturated monomers may be acrylate or methacrylate monomers having an amine group.
[0019]
[0020] Suitable examples of ethylenically unsaturated monomers lacking amine groups are not considered to be particularly limited.Specific examples may include, for example, esters of acrylic or methacrylic acid such as n-butyl (meth)acrylate, cycloalkyl (meth)acrylates such as methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate and cyclohexyl (meth)acrylate; styrene or its substituted variants; dienes such as 1,3-butadiene or isoprene; vinyl esters such as vinyl acetate, vinyl alkanoate or their derivatives; nitriles such as (meth)acrylonitrile; acrylamide or methacrylamide; olefinically unsaturated halides such as vinyl chloride; alpha-olefins; or any combination thereof. Still other examples of suitable ethylenically unsaturated monomers lacking amine groups that may be present in the amine-functionalized copolymers include, for example, hydroxy-functionalized monomers such as hydroxyethyl (meth)acrylate or hydroxypropyl (meth)acrylate; (meth)acrylamide derivatives such as N-methylol (meth)acrylamide and diacetone acrylamide; polyvinyl monomers such as allyl methacrylate, divinylbenzene, and various alkylene glycol di(meth)acrylates.
[0020]
[0021] When present, suitable alpha olefins that can be incorporated into the amine-functionalized copolymer include, but are not limited to, ethylene, propylene, isobutylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-octene, 1-decene, 1-dodecene, 1-tetradecene, or combinations thereof. Linear alpha olefins having an even number of carbon atoms are particularly suitable because they are readily available.
[0021]
[0022] Particularly suitable examples of amine-functionalized copolymers can contain from about 1 wt.% to about 60 wt.% of an olefinically unsaturated monomer comprising at least one amine group. In more specific examples, from about 5 wt.% to about 45 wt.%, or from about 10 wt.% to about 40 wt.%, or from about 10 wt.% to about 25 wt.%, or from about 25 wt.% to about 40 wt.% of an olefinically unsaturated monomer comprising at least one amine group can be present.
[0022]
[0023] Even more specific examples of suitable amine-functionalized copolymers may include about 60 wt.% to about 100 wt.% acrylate or methacrylate monomers and about 40 wt.% or less of an ethylenically unsaturated monomer that is not an acrylate or methacrylate monomer. Some amine-functionalized copolymers of the present disclosure may include all acrylate or methacrylate monomers, in which case a first portion of the acrylate or methacrylate monomers may contain at least one amine group and a second portion of the acrylate or methacrylate monomers may be devoid of amine groups. Optionally, a third portion of the acrylate or methacrylate monomers may have pendant carboxylic or sulfonic acids in amine-functionalized copolymers that include all acrylate or methacrylate monomers, as specified below.
[0023]
[0024] As mentioned above, the amine-functionalized copolymer may further include at least one monomer unit having a pendant carboxylic acid or sulfonic acid, provided that the amount of such acid-containing monomer unit remains within the range of amine value disclosed above. Suitable acid-containing monomers, when present, contain ethylenic unsaturation and are copolymerized with the first and second ethylenically unsaturated monomers discussed above. Illustrative examples may include, but are not limited to, acrylic acid, methacrylic acid, maleic acid, methyl hydrogen maleate, ethyl hydrogen maleate, itaconic acid, fumaric acid, crotonic acid, and citraconic acid. Suitable monomers containing sulfonic acid groups may include, for example, styrene sulfonic acid or 2-aminomethylpropane sulfonic acid derivatized with a vinyl group. It should be recognized that hydrolyzable monomers may be used similarly to introduce pendant carboxylic acid groups into the amine-functionalized copolymer. Suitable hydrolyzable monomers may include, for example, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, isobutyl acrylate, isobutyl methacrylate, methyl fumarate, vinyl acetate, vinyl propionate, vinyl benzoate, vinyl chloride, vinylidene chloride, acrylamide, acrylonitrile, methacryloamide, methacrylonitrile, fumaronitrile, etc. It will be appreciated that carboxylic acid or sulfonic acid functionalization of the polymer, if desired or synthetically suitable, can be accomplished by synthetic transformation of the polymer side chain followed by polymerization.
[0024]
[0025] When present, the acid-containing monomer having ethylenic unsaturation can be present in the amine-functionalized copolymer in an amount of 10 wt.% or less, for example, about 0.1 wt.% to about 1 wt.%, or about 1 wt.% to about 5 wt.%, or about 5 wt.% to about 10 wt.%. The acid-containing monomer that is acrylic acid, methacrylic acid, or any derivative thereof, can in some examples be copolymerized with other monomers that are all acrylates or methacrylates. In other examples, the acid-containing monomer that is not an acrylate or methacrylate can be copolymerized with other monomers that are all acrylates or methacrylates. In yet other examples, the acid-containing monomer that is not an acrylate or methacrylate can be copolymerized with other monomers that are not all acrylates or methacrylates, but preferably at least a portion of the other monomers are acrylates or methacrylates.
[0025]
[0026] The primer composition of the present disclosure may further comprise a surfactant or another suitable wetting agent. Suitable surfactants may include, for example, neutral surfactants (including zwitterionic surfactants and uncharged surfactants) and anionic surfactants. In contrast, cationic surfactants may prove to be difficult to synthesize during emulsion polymerization and may disrupt the adhesion between toner particles and primer coating. However, in certain circumstances, even cationic surfactants may be appropriately used in the present disclosure.
[0026]
[0027] Suitable neutral surfactants may include, for example, alkylaryl polyether alcohols, alkylphenol ethoxylates, alkyl ethoxylates, polyethylene sorbitan fatty acid esters, and mixtures thereof. When present, these types of neutral surfactants may be present in the primer composition of the present disclosure in an amount ranging from about 0.5 wt.% to about 2.0 wt.% based on total monomer. Other suitable neutral surfactants for use in the primer composition disclosed herein may include, for example, poloxamers, fatty acid esters, fatty acid glycerol esters, fatty acid sorbitol esters, and the like. Other neutral surfactants may include, for example, emulsifiers such as lecithin or glycerol esters, or polymer colloids such as polyvinyl alcohol, polyvinylpyrrolidone, hydroxyethyl cellulose, other cellulose derivatives, and the like. Zwitterionic surfactants that may be suitable for use in the present disclosure include, for example, betaines and sultaines.
[0027]
[0028] Suitable anionic surfactants for use in the present disclosure include, for example, alkyl ethoxylate sulfates and sulfonates, alkylphenol ethoxylate sulfates and sulfonates, alkyl sulfates, alkyl sulfonates, alkylaryl sulfonates, sulfosuccinates, and mixtures thereof. When present, these types of anionic surfactants can be present in the primer composition of the present disclosure in an amount ranging from about 0.02 wt.% to about 0.5 wt.% based on total monomer. Other anionic surfactants suitable for use in the primer composition disclosed herein include, for example, carboxylates of long-chain fatty acids, such as dodecanoic acid, stearic acid, oleic acid, palmitic acid, and the like, or phosphate esters of long-chain alcohols.
[0028]
[0029] The primer composition of the present disclosure is compatible with starch, and starch may be included in the primer composition, if desired, to promote bonding of the toner to the paper substrate. Suitable starches can include, for example, modified starches, such as ionic starches, oxidized starches, ethoxylated starches, hydroxyalkylated starches, carboxylated starches, aminated starches, and the like, or any mixture thereof. The starch can be chemically modified by oxidation, acid thinning, or functionalization or enzymatic modification. The starch can be derived from any plant source, including corn, potato, sweet potato, wheat, rice, sago, tapioca, waxy corn, sorghum, high amylose corn, and the like. When present, the starch can be included in the primer composition in a weight amount greater than that included in the amine-functionalized copolymer. In an illustrative example, the starch can be present in the primer composition in an amount ranging from about 50 wt.% to about 95 wt.% of the total solids of the primer composition. The selection of a particular starch may not be related to the primer composition itself, but may be dictated by other variables related to the printing process. The considerations for selecting a particular starch are familiar to those of skill in the art.
[0029]
[0030] Other adhesion promoters different from the amine-functionalized copolymer may also be suitably present in the primer composition disclosed herein. In addition to starch, other suitable adhesion promoters may include, for example, polyvinyl alcohol, styrene-butadiene rubber (SBR), polyethyleneimine, polyurethane, polyvinylpyrrolidone, carboxymethyl cellulose, guar gum, natural rubber, cellulose ether, urea, stearates, hydrogenated hydrocarbon rosin or rosin ester, acrylic polymer dispersions, and the like, and any combination thereof. The adhesion promoter may be present in an amount ranging from about 10 wt.% to about 90 wt.% on solids. If present, the adhesion promoter may be present such that the ratio of adhesion promoter:amine-functionalized copolymer is in the range of about 1:5 to 5:1, or about 1:1 to 5:1, or about 1:5 to 1:1. Without being bound by theory, the adhesion promoter may help promote adhesion of the primer coating to the substrate and / or promote adhesion of the toner to the primer coating.
[0030]
[0031] Still other additives that can be present in the primer compositions disclosed herein include, for example, pigments, dyes, fluorescent dyes, crosslinkers, defoamers, antistatic agents, dispersants, thickeners, waxes, fillers, biocides, rheology modifiers, preservatives, and any combination thereof.
[0031]
[0032] Provided that the amine value remains within the aforementioned range, the amine groups may include both protonated and non-protonated amines, and / or at least a portion of the amines may be functionalized to form quaternized amine groups or amine derivatives that no longer have lone pairs or electrons (e.g., amides, ureas, urethanes, etc.). In certain examples, the amine-functionalized copolymer may include a first portion of protonated amine groups and a second portion of non-protonated amine groups. In other examples, the amine-functionalized copolymer may include a first portion of quaternized or functionalized amine groups and a second portion of non-quaternized or non-functionalized amine groups. The total number of amine groups may be limited to avoid water solubility and discoloration, problems commonly encountered with amine-rich polymers such as polyethyleneimines.
[0032]
[0033] Suitable reagents for forming quaternary amine groups may include, for example, epoxides and electrophiles, such as alkyl halides or alkyl sulfonates. In some instances, suitable epoxides may be bifunctional compounds, such as glycidyl methacrylate, allyl glycidyl ether, and similar compounds that can further crosslink the amine-functionalized copolymer. Glycidyl methacrylate, for example, can cure the deposited primer coating by radiation. Additionally, reagents for forming quaternary amine groups can improve adhesion of substrates in certain conditions.
[0033]
[0034] The amine-functionalized copolymers of the present disclosure can have properties tailored for specific coating applications, which can be achieved by varying the monomers and the amount of monomers polymerized. Properties that can be varied include, for example, hydrophobicity / hydrophilicity, molecular weight, glass transition temperature, and the like. Certain desirable amine-functionalized copolymers of the present disclosure may have a glass transition temperature in the range of about 0° C. to about 50° C. Glass transition temperatures in this range can have good film-forming properties, in non-limiting examples. If the glass transition temperature is too low, excessive tackiness may result. The glass transition temperature can be determined by differential scanning calorimetry (DSC) under the conditions specified above.
[0034]
[0035] Depending on the polymerization conditions and other factors, the molecular weight of the polymers of the present disclosure can range from about 1×10 4 ~Approx. 1×10 7 , or about 2 × 10 4 ~Approx. 1×10 6 , or approximately 1 × 10 5 ~Approx. 1×10 6 The molecular weight may range from 0.1 to 1.0. Even higher molecular weights can be achieved if crosslinking occurs. It is understood that polymer molecular weights outside the aforementioned ranges may also be suitable for use in the present disclosure. The polymer molecular weights in this disclosure are weight average molecular weights (Mw) and can be determined by gel permeation chromatography (GPC) using refractive index (RI) detection. GPC analysis herein is performed by drying the polymer emulsion, redissolving the polymer in THF, filtering through a 0.45 μm filter, and then eluting the polymer on three consecutive columns (STYRAGEL HR2, STYRAGEL HR4 and STYRAGEL HR5). The analysis was carried out by injection into a Shimadzu LC-20AD GPC instrument equipped with a THF column (HR6, Waters) and a refractive index detector (Waters 2410). Chromatograms were acquired at 35° C. at a THF flow rate of 1 mL / min and molecular weights were calculated relative to polystyrene standards.
[0035]
[0036] Also provided herein is a substrate coated with a primer coating formed from the disclosed primer composition. Such a coated substrate may include a base substrate and a primer coating disposed on a surface of the base substrate. The primer coating includes an amine-functionalized copolymer having an amine value of about 10-180 mg KOH / g copolymer, or about 70-140 mg KOH / g copolymer, or about 30-160 mg KOH / g copolymer, or about 50-60 mg KOH / g copolymer, or about 60-80 mg KOH / g copolymer, or about 80-100 mg KOH / g copolymer, or about 100-115 mg KOH / g copolymer, or about 115-130 mg KOH / g copolymer, or about 130-150 mg KOH / g copolymer, the amine-functionalized copolymer comprising the polymerization reaction product of one or more first ethylenically unsaturated monomers lacking an amine group and one or more second ethylenically unsaturated monomers having at least one amine group. At least one amine group constitutes a side chain of the amine-functionalized copolymer. Any of the amine-functionalized copolymers identified above can be used in forming the primer coatings and coated substrates described herein.
[0036]
[0037] Once the primer composition has been applied to the surface of a suitable substrate, the aqueous fluid can be removed to leave a primer coating that includes the amine-functionalized copolymer disposed at the surface at the appropriate weight or viscosity. Any non-volatile components of the primer composition can also remain within the primer coating. Non-limiting examples of other components that may remain in the primer coating after application include, for example, surfactants, starch, or any of the other additives listed above.
[0037]
[0038] In a non-limiting example, a primer coating can be disposed on a suitable base substrate by a method that includes depositing a coating composition of the present disclosure onto the base substrate, particularly a coating composition that includes an amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid, and evaporating the aqueous fluid to leave a primer coating disposed on the base substrate. Application of heat and / or vacuum can be performed in some instances to facilitate removal of the aqueous fluid. In some instances, a gas flow can also be used to facilitate removal of the aqueous fluid from the surface of the substrate.
[0038]
[0039] Suitable base substrates that can be coated with the primer coating disclosed herein are not considered to be particularly limited. Exemplary base substrates that can be suitably coated include, for example, polymeric substrates, nonwoven substrates, and paper substrates. Specific examples of suitable base substrates can include, but are not limited to, paper (e.g., art paper, coated paper, paperboard, printer paper, cardboard, etc.), film (including polymeric film), nonwoven materials, etc. As used herein, the term "film" refers to a substrate made from organic polymeric materials, such as viscose, acetate, polyethylene, polypropylene, biaxially oriented polypropylene (BOPP) poly(vinyl chloride), polystyrene, polyamide, polycarbonate, or polyesters such as poly(ethylene terephthalate) or poly(butylene terephthalate). As used herein, the term "nonwoven" refers to a substrate made from fibrous materials such as wood cellulose, cotton, rayon, poly(ethylene terephthalate), poly(butylene terephthalate), polyacrylonitrile, polypropylene, etc., in which the individual fibers are at least partially fused together.
[0039]
[0040] As understood by those skilled in the art, BOPP and other polyolefin substrates are low surface energy materials and difficult to wet. Corona treatment of such substrates is often performed to introduce suitable functional groups to promote adhesion of primer coatings. The primer coatings disclosed herein can exhibit good adhesion to such corona-treated substrates due to the balance between hydrophilic and oleophilic monomers.
[0040]
[0041] When applied to a substrate surface, the primer coating has a coating weight of about 0.05 g / m 2 ~about 0.7g / m 2 , or about 0.1 g / m 2 ~about 0.6g / m 2 , or about 0.1 g / m 2 ~about 0.2g / m 2 , or about 0.2 g / m 2 ~about 0.3g / m 2 , or about 0.3 g / m 2 ~ approx. 0.4g / m 2 , or about 0.4 g / m 2 ~about 0.5g / m 2 , or about 0.5 g / m 2 ~about 0.6g / m 2 , or about 0.6 g / m 2 ~about 0.7g / m 2 When starch is present in the primer composition, the primer coating may have a coating weight ranging from 1.5 g / m 2 Thus, the coating weight containing starch can be about 0.05 g / m 2 ~Approx. 1.5g / m 2 , or about 0.1 g / m 2 ~about 0.5g / m 2 , or 0.5 g / m 2 ~ approx. 0.9g / m 2 , or 0.9 g / m 2 ~Approx. 1.2g / m 2 , or 1.2 g / m 2 ~Approx. 1.5g / m 2A primer coating lacking starch can also be present at these higher coat weights. Coating thicknesses of either type may range from about 0.1 microns to about 5 microns, or from about 0.3 microns to about 3 microns, or from about 0.5 microns to about 2 microns.
[0041]
[0042] The coated substrate of the present disclosure may further include HP INDIGO deposited on the primer coating, such as in the form of a toner, e.g., electrophotographic image. Electrophotographic images that can be formed on the primer coating include, but are not limited to, text, pictures, photographic images, and the like. The coated substrate including the toner can be formed by liquid electrophotographic printing, in a non-limiting example.
[0042]
[0043] Methods of forming the primer composition of the present disclosure are also contemplated herein. A suitable method of forming the primer composition may, in certain process configurations, feature an emulsion polymerization technique. The method may include: combining, in an aqueous fluid, one or more first ethylenically unsaturated monomers lacking an amine group with one or more second ethylenically unsaturated monomers having at least one amine group, and in an emulsion polymerization reaction of the one or more first ethylenically unsaturated monomers and the one or more second ethylenically unsaturated monomers carried out in the aqueous fluid, producing from about 10 to about 180 mg KOH / g copolymer, or from about 70 to about 140 mg KOH / g copolymer, or from about 30 to about 160 mg KOH / g copolymer, or from about 50 to about 60 mg KOH / g copolymer, or from about 60 to about 80 mg KOH / g copolymer, or from about 80 to about 100 mg KOH / g copolymer. forming an amine-functionalized copolymer having an amine number of about 100 to about 115 mg KOH / g copolymer, or about 115 to about 130 mg KOH / g copolymer, or about 130 to about 150 mg KOH / g copolymer, thereby providing a coating composition comprising the amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid. Anionic or nonionic surfactants can be used in the aqueous fluid, with the nonionic surfactants, after mixing with either the anionic or cationic additive, broadening the range of potential substrates on which the primer composition may be used.
[0043]
[0044] Radical initiators that can be used in emulsion polymerization include, for example, azo initiators such as alkali persulfate, ammonium persulfate, 4,4'-azobis-cyanovaleric acid or AIBN, and organic (hydro)peroxides such as t-butyl hydroperoxide. Azo initiators may be particularly desirable due to their ability to initiate polymerization without participating in an oxidation-reduction reaction with amine-containing monomers. The radicals can be formed by heating the reaction mixture or by using a reducing agent such as ascorbic acid or sodium formaldehyde sulfoxylate, among others. The polymerization reaction can occur at temperatures ranging from about 20°C to about 90°C. Organic chain transfer agents are also known as regulators, for example, 2-mercaptoethanol, tert-dodecyl mercaptan, among others, can also be implemented to control the molecular weight of the copolymer during its preparation.
[0044]
[0045] Depositing the primer composition on the base substrate can be accomplished by applying the primer composition to at least one surface of the base substrate and drying to remove the aqueous fluid. Applying the primer composition to the base substrate can be accomplished by any of a variety of methods, such as dipping, spraying, using rod or roller or equipment such as a size press, water box, blade coater, cast coater, rod coater, air knife coater, curtain coater, film press coater, flexo coater, etc. The primer composition can be applied in-line during the printing process or offline, and the coated substrate is then fed to the printing process in an offline configuration. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0045]
[0046] The embodiments of the present disclosure include:
[0047] A. Primer Composition Having an Amine Number of About 70 to About 140 mg KOH / g Copolymer. The primer composition comprises: an emulsion-polymerized amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid, the amine-functionalized copolymer having an amine number of about 70 to about 140 mg KOH / g Copolymer and a glass transition temperature of about 0° C. to about 50° C., and comprising the polymerization reaction product of one or more first ethylenically unsaturated monomers lacking an amine group and one or more second ethylenically unsaturated monomers having at least one amine group, the at least one amine group constituting a side chain of the amine-functionalized copolymer.
[0046]
[0048] B. Primer Composition Having an Amine Value of About 10 to About 180 mg KOH / g Copolymer. The primer composition comprises: a fluid; and an amine-functionalized copolymer dispersed in the fluid, the amine-functionalized copolymer having an amine value of about 10 to about 180 mg KOH / g Copolymer, the amine-functionalized copolymer comprising the polymerization reaction product of one or more first ethylenically unsaturated monomers lacking an amine group and one or more second ethylenically unsaturated monomers having at least one amine group, the at least one amine group comprising a side chain of the amine-functionalized copolymer.
[0047]
[0049] C. Coated Substrate. The coated substrate includes: a base substrate; and a primer coating disposed on a surface of the base substrate, the primer coating comprising an amine-functionalized copolymer having an amine value of from about 10 to about 180 mg KOH / g copolymer; the amine-functionalized copolymer comprises the polymerization reaction product of one or more first ethylenically unsaturated monomers lacking an amine group and one or more second ethylenically unsaturated monomers having at least one amine group, the at least one amine group comprising a side chain of the amine-functionalized copolymer.
[0048]
[0050] D. A method of making a primer composition comprising: combining, in an aqueous fluid, one or more first ethylenically unsaturated monomers lacking an amine group with one or more second ethylenically unsaturated monomers having at least one amine group; and in an emulsion polymerization reaction of the one or more first ethylenically unsaturated monomers and the one or more second ethylenically unsaturated monomers carried out in the aqueous fluid, forming an amine-functionalized copolymer having an amine value of from about 10 to about 180 mg KOH / g copolymer, thereby providing a coating composition comprising the amine-functionalized copolymer dispersed as an emulsion in the aqueous fluid.
[0049]
[0051] Each of embodiments A-D may have one or more of the following additional elements in any combination:
[0052] Element 1: The aqueous fluid has a pH of about 7 or greater.
[0050]
[0053] Element 2: The primer composition further comprises a neutral or anionic surfactant dispersed in the aqueous fluid.
[0054] Element 3: The primer composition further comprises a starch dispersed in the aqueous fluid.
[0051]
[0055] Element 4: The primer composition further comprises an adhesion promoter distinct from the amine-functionalized copolymer dispersed in the aqueous fluid.
[0056] Element 5: The primer composition further comprises an adhesion promoter distinct from the amine-functionalized copolymer dispersed in the fluid.
[0052]
[0057] Element 6: The amine-functionalized copolymer further comprises at least one monomer unit having a pendant carboxylic acid.
[0058] Element 7: The amine number is in the range of about 70 to about 140 mg KOH / g copolymer.
[0053]
[0059] Element 8: The amine-functionalized copolymer is dispersed as an emulsion in the fluid.
[0060] Element 9: The primer composition further comprises a neutral surfactant or an anionic surfactant dispersed in the fluid.
[0054]
[0061] Element 10: The one or more first ethylenically unsaturated monomers comprise at least one monomer selected from the group consisting of alkyl or cycloalkyl (meth)acrylates, n-butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, styrene, substituted styrenes, dienes, 1,3-butadiene, isoprene, vinyl esters, vinyl acetate, nitriles, (meth)acrylonitrile, olefinically unsaturated halides, vinyl chloride, vinyl bromide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate; (meth)acrylamide, substituted (meth)acrylamide, N-methylol (meth)acrylamide, diacetone acrylamide, allyl methacrylate, divinylbenzene, alkylene glycol di(meth)acrylate, and any combination thereof.
[0055]
[0062] Element 11: The one or more second ethylenically unsaturated monomers include at least one monomer selected from the group consisting of 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl methacrylate, and any combination thereof.
[0056]
[0063] Element 12: The amine-functionalized copolymer includes a first portion of protonated amine groups and a second portion of unprotonated amine groups.
[0064] Element 13: The primer composition further comprises a starch dispersed in the fluid.
[0057]
[0065] Element 14: The amine-functionalized copolymer has a glass transition temperature of about 0°C to about 50°C.
[0066] Element 15: The fluid comprises an aqueous fluid.
[0058]
[0067] Element 16: The base substrate comprises a polymeric substrate.
[0068] Element 17: The base substrate comprises a paper substrate.
[0069] Element 18: The primer coating further comprises starch.
[0059]
[0070] Element 19: Primer coating is approximately 0.05 g / m 2 ~Approx. 1.5g / m 2 The coating weight ranges from 0.1 to 100 g / g.
[0071] Element 20: The primer coating further comprises a neutral surfactant or an anionic surfactant.
[0060]
[0072] Element 21: The coated substrate further comprises a toner deposited on the primer coating.
[0073] Element 22: A primer coating is disposed on the base substrate by a method comprising the steps of: depositing a coating composition onto the base substrate, the coating composition comprising an amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid; and; allowing the aqueous fluid to evaporate, leaving the primer coating disposed on the base substrate.
[0061]
[0074] Element 23: The method further comprises the steps of: disposing the coating composition on a base substrate; and evaporating the aqueous fluid to leave the amine-functionalized copolymer disposed as a primer coating on the base substrate.
[0062]
[0075] Element 24: The amine-functionalized copolymer comprises from about 1 wt.% to about 60 wt.%, optionally from about 5 wt.% to about 45 wt.%, or from about 10 wt.% to about 40 wt.%, or from about 10 wt.% to about 25 wt.%, or from about 25 wt.% to about 40 wt.%, of one or more second olefinically unsaturated monomers having at least one amine group.
[0063]
[0076] Element 25: The amine-functionalized copolymer comprises about 60 wt.% to about 100% acrylate monomers and about 40 wt.% or less of ethylenically unsaturated monomers that are not acrylate or methacrylate monomers, optionally, the amine-functionalized copolymer comprises all acrylate or methacrylate monomers.
[0064]
[0077] Element 26: The amine-functionalized copolymer comprises up to about 10 wt.% of an acid-containing monomer, optionally from about 0.1 wt.% to about 10 wt.% of an acid-containing monomer, and further optionally, the acid-containing monomer is acrylic acid, methacrylic acid, or any derivative thereof.
[0065]
[0078] As non-limiting examples, exemplary combinations applicable to A include, but are not limited to, 1 and 2; 1 and 3; 1 and 4; 2 and 3; 2 and 4; 3 and 4; 1-3; 1-4; 2-4; 1 and 24; 1 and 25; 1 and 26; 2 and 24; 2 and 25; 2 and 26; 3 and 24; 3 and 25; 3 and 26; 1-3, and 24; 1-3, and 25; 1-3, and 26; 1-4, and 24; 1-4, and 25; 1-4, and 26; 24 and 25; 24 and 26; 25 and 26; and 24-26.As further non-limiting examples, exemplary combinations applicable to B include, but are not limited to, 5 and 6; 5 and 7; 5 and 8; 5 and 9; 5 and 10; 5 and 11; 5 and 12; 5 and 13; 5 and 14; 5 and 15; 6 and 7; 6 and 8; 6 and 9; 6 and 10; 6 and 11; 6 and 12; 6 and 13; 6 and 14; 6 and 15; 7 and 8; 7 and 9; 7 and 10; 7 and 11;7 and 12;7 and 13;7 and 14;7 and 15;8 and 9;8 and 10;8 and 11;8 and 12;8 and 13;8 and 14;8 and 15;9 and 10;9 and 11;9 and 12;9 and 13;9 and 14;9 and 15;10 and 11;10 and 12;10 and 13;10 and 14;10 and 15;11 and 12;11 and 13;11 and 14;11 and 15; 12 and 13; 12 and 14; 12 and 15; 13 and 14; 13 and 15; 14 and 15, and exemplary combinations include 24, 25, and / or 26; 5 and 24; 5 and 25; 5 and 26; 6 and 24; 6 and 25; 6 and 26; 7 and 24; 7 and 25; 7 and 26; 8 and 24; 8 and 25; 8 and 26; 9 and 24; 9 and 25; 9 and 26; 1 and further combinations of 0 and 24; 10 and 25; 10 and 26; 11 and 24; 11 and 25; 11 and 26; 12 and 24; 12 and 25; 12 and 26; 13 and 24; 13 and 25; 13 and 26; 14 and 24; 14 and 25; 14 and 26; 15 and 24; 15 and 25; 15 and 26; 24 and 25; 24 and 26; 25 and 26; and 24 to 26.Further non-limiting exemplary combinations applicable to C include, but are not limited to, 16 and 19; 16 and 20; 16 and 21; 16 and 22; 14 and 16; 17 and 18; 17-19; 17 and 19; 17 and 20; 17 and 21; 17 and 22; 14 and 17; 18 and 19; 18 and 20; 18 and 21; 18 and 22; 14 and 18; 19 and 20; 19 and 21; 19 and 22; 14 and 19; 20 and 21; 20 and 22; 14 and 20; 21 and 22; 14 and 21; 14 and 22 and any of the exemplary combinations may be in further combinations of 24, 24, and / or 26; 14 and 24; 14 and 25; 14 and 26; 16 and 24; 16 and 25; 16 and 26; 17 and 24; 17 and 25; 17 and 26; 18 and 24; 18 and 25; 18 and 26; 19 and 24; 19 and 25; 19 and 26; 20 and 24; 20 and 25; 20 and 26; 21 and 24; 21 and 25; 21 and 26; 24 and 25; 24 and 26; 25 and 26; and 24-26. Further non-limiting exemplary combinations applicable to D include, but are not limited to, 6 and 23; 7 and 23; 9 and 23; 10 and 23; 11 and 23; 12 and 23; 14 and 23; 6 and 7; 6 and 9; 6 and 10; 6 and 11; 6 and 12; 6 and 14; 7 and 9; 7 and 10; 7 and 11; 7 and 12; 7 and 14; 9 and 10; 9 and 11; 9 and 12; 9 and 14; 10 and 11; 10 and 12; 10 and 14; 11 and 12; 11 and 14; and 12 and 14 and any of the exemplary combinations may be in further combinations of 24, 24, and / or 26; 6 and 24; 6 and 25; 6 and 26; 7 and 24; 7 and 25; 7 and 26; 9 and 24; 9 and 25; 9 and 26; 10 and 24; 10 and 25; 10 and 26; 11 and 24; 11 and 25; 11 and 26; 12 and 24; 12 and 25; 12 and 26; 14 and 24; 14 and 25; 14 and 26; 24 and 25; 24 and 26; 25 and 26; and 24-26.
[0066]
[0079] In order to facilitate a better understanding of the present disclosure, the following examples of various representative embodiments are provided. In no event should the following examples be read as limiting or defining the scope of the present disclosure. EXAMPLES
[0067] Example 1
[0080] Exemplary Polymer Synthesis and Emulsion Blending Procedures. 1 kg of product was prepared by emulsion polymerization of the monomer mixture. The emulsion polymerization was carried out in a temperature-controlled double-glazed reactor equipped with an overhead condenser, stirrer and nitrogen inlet (20 mL / min N2 flow). A 7 mM solution of DOWFAX 2A1 (Dow Chemical) emulsifier in 211 g of pure water was added to the reactor and heated to 85° C. In a separate vessel, a monomer mixture containing 228 g of n-butyl acrylate, 146 g of styrene and 94 g of 2-(dimethylamino)ethyl methacrylate was emulsified in 247 g of water in the presence of 14 g of DISPONIL A 3065 (BASF) emulsifier. 5 g of an aqueous solution of 10 wt.% 4,4'-azobis(4-cyanovaleric acid) neutralized 1.5 times with ammonia was added to the reactor, followed 5 minutes later by 25 g of the previously prepared monomer emulsion. The reaction mixture was allowed to polymerize for 20 minutes, after which the remaining monomer emulsion was fed at a constant rate to the reaction mixture over a period of 4 hours. During this time, a parallel constant rate feed of 24 g of an aqueous solution of 4 wt.% 4,4'-azobis(4-cyanovaleric acid) neutralized 1.5 times with ammonia was also added to the reaction mixture. After addition of both feeds was completed, the reactor contents were held at 85°C under agitation conditions for an additional 60 minutes. High monomer conversions of over 80% were obtained under polymerization conditions.
[0068]
[0081] The resulting polymer dispersion was cooled to 50° C., and 14 g of an aqueous solution of 4 wt.% t-butyl hydroperoxide and 14 g of an aqueous solution of 6 wt.% BRUGGOLITE® FF6M reducing agent (Bruggemann GmbH & Co), 0.2 wt.% iron(II) sulfate heptahydrate and 0.5 wt.% tetrasodium ethylenediaminetetraacetate were fed in parallel to the reactor over a period of 2 hours. The reaction mixture was then held at 50° C. for 30 minutes and then cooled to room temperature. When room temperature was reached, 0.05 g of BYK-016 (BYK-Chemie) defoamer was slowly added to the reaction mixture under high speed stirring. The resulting emulsion was used directly for coating applications without further modification unless further modified as specified below.
[0069]
[0082] The other polymer emulsions in the following examples were similarly prepared by substituting the indicated ratios of ethylenically unsaturated monomers in the monomer mixture.
[0070] Example 2
[0083] Coating on polymer substrate and adhesion test. The polymer emulsion prepared in Example 1 was coated on a 48 ga PET polyester substrate, and after drying at 105° C. for 1 minute, the layer weight was 0.5 g / m 2 For the data in Table 1 below, a hot-nip laminator was used to transfer the HP color blocks from the untreated BOPP substrate to the PET substrate primed as described above. In this case, a hand drawdown was performed with a Meyer rod to deliver the primer composition on the substrate surface, followed by hot-nip lamination. For the data in Table 2 below, the primer coating was applied using an HP INDIGO 6000 press, and printing was performed on the press equipment using an HP INDIGO ELECTROINK under standard printing conditions. In particular, printing was performed using an HP INDIGO 6000 press operating in 4 shot mode, with a drying temperature of 80° C. and a corona power intensity of 800 W in the priming unit.
[0071]
[0084] The adhesion of the ink to the primer coating was evaluated by applying SCOTCH® 810 (3M) tape to the printed surface immediately after printing and removing the tape after 15 minutes. The test procedure was the same as that described in ASTM 2252 / 2252M, except that SCOTCH® 810 tape was used instead of SCOTCH® 610 tape, and the tape was pressed onto the coated substrate with four passes of a 2 kg roller. The percentage removal of the printed image was evaluated visually.
[0072]
[0085] The adhesion test results and selected physical property data are summarized in Tables 1 and 2 below. A value of "none" or 0% indicates complete removal of the printed image, and a value of 100% indicates no evident image removal. Control data for polymers having non-amine functionality and deposited under similar conditions is shown in Table 1. Data for polymers having various amounts of amine functionality is shown in Table 2. Percentages of monomers are by weight of the individual monomer relative to the total weight of monomers. Glass Transition Temperature (T g ) was determined by differential scanning calorimetry using a DSC3+ instrument (Mettler Toledo). The scan cycle consisted of an initial cooling to -60°C with a ramp of 20°C / min, followed by a 5 min stabilization period at this temperature. The samples were then cooled for 20 o 120 C / min ramp o C / min to a temperature of 100° C., followed by a second stabilization period of 5 minutes at this temperature. Two of the above cycles were performed on each sample, the first to remove the thermal history of the sample and the second to reduce the T g was used to determine the value.
[0073] [Table 1]
[0074] [Table 2-1]
[0075] [Table 2-2]
[0076] [Table 2-3]
[0077]
[0086] As shown in Table 1, coatings formulated with various copolymers containing carboxyl, epoxide or hydroxyl functionality provided ink transfer after lamination but did not promote image adhesion as measured by tape pull testing. Copolymers containing amide or urea functionality provided limited amounts of image adhesion as measured by tape pull testing, likely due to the formation of N-H hydrogen bonds or partial acid-base interactions between these functional groups and the carboxyl functionality in the toner.
[0078]
[0087] As shown in Table 2, several amine-containing copolymers provided both good image transfer and strong adhesion as measured by tape pull testing. In many cases, the adhesion percentage was greater than 80%. Although showing strong adhesion, a copolymer having a similar composition to the composition lacking the amine-containing monomer (entry 13) did not demonstrate measurable adhesion by tape pull testing. Copolymers having two different types of amine-containing monomers (entries 33 and 34) showed similar percentage adhesion values as copolymers having only a single type of amine-containing monomer.
[0079]
[0088] Primer coatings featuring copolymers containing monomers capable of internally protonating amine groups or copolymers with amine groups that were fully or partially quaternized or protonated after polymerization showed lower adhesion rates when a threshold level of amine modification was reached. Incorporation of carboxylic acid groups above a threshold level completely blocked image adhesion (entry 36), while significant image adhesion was still achieved when lesser amounts of carboxylic acid functionality were present (entry 35). The adhesion observed for the entry 35 copolymer was similar to or only slightly lower than that observed for copolymers with similar amounts of other monomers but lacking the carboxylic acid-containing monomer (entries 15 or 17). As with the incorporation of excess carboxylic acid functionality, post-synthesis acidification with mineral acid completely destroyed the ability of the copolymer to promote image adhesion (entry 37), while the non-acidified copolymer showed good image adhesion (entry 15). Partial epoxide functionalization of the amine groups retained good image adhesion (entry 38), with only a minimal decrease observed compared to the non-functionalized control copolymer (entry 22).
[0080] Example 3
[0089] Additional adhesion test data for coatings on plastic substrates. Polymer emulsions prepared as in Example 1 were coated onto a 48 ga PET polyester substrate or onto an 80 ga BOPP (biaxially oriented polypropylene) substrate. Coating was performed as in Example 2 using an HP INDIGO 6000 press. Coating weights were also different in this example. Adhesion test results and selected physical property data are summarized below in Table 3.
[0081] [Table 3-1]
[0082] [Table 3-2]
[0083] As shown, the incorporation of polyethyleneimine or polyurethane as an additional adhesion promoter into the coating did not significantly affect the observed image adhesion (entries 46-53). Polyethyleneimine or polyurethane was added to promote adhesion to the BOPP substrate.
[0084]
[0090] The water resistance of the coatings from entries 44 and 46 was tested by immersing the coated PET substrates for 30 minutes, 1 hour, 3 hours, and 24 hours. Tape pull tests were performed at each time after the coated substrates were removed from the water. The relatively hydrophilic copolymer coating (entry 46) showed significant delamination after just 30 minutes of immersion in water, while the more hydrophobic copolymer (entry 44) did not experience significant delamination over the test time.
[0085] Example 4
[0091] Adhesion test data for coatings on paper substrates. 8 wt.% aqueous starch solutions were held at 90°C for at least 25 minutes, after which the pH of the solution was adjusted to 8.5 using 1 wt.% aqueous potassium hydroxide solution. Each starch solution was blended with the polymer emulsion prepared as in Example 1 at a blend ratio of 75% starch and 25% copolymer on solids. The blends were held at 60°C for 1 hour, after which approximately 150 g / m 2 The coating was applied to a sheet of commercially available Starbrite Opaque Select Smooth 100T paper (Verity, caliper 7.4, brightness 96 and opacity 97) with a base weight of 2 g / m2 using a Meyer rod #4. 2 Coating was performed targeting a coating weight of dry material of 1000 g / g. Brookfield viscosity was determined immediately after compounding and after 24 hours storage at 60° C. to determine the colloidal stability of the blended coating emulsions. All of the amine-containing copolymers were colloidally stable with the starches tested; that is, the viscosity did not change appreciably over the 24 hour observation period.
[0086]
[0092] The coated paper sheets were prepared using an HP Indigo press WS 5500 Series3 operating in 4 shot mode, followed by standard screening procedures, with blanket temperatures of 110°C and impression cylinder temperatures of 42°C, respectively. HP 100% Black Liquid Toner and HP 290% Photo Black Toner (52% Yellow, 66% Magenta, 72% Cyan and 100% Black) were printed onto the coated paper sheets. Ink adhesion was evaluated by performing a tape pull test with SCOTCH® 234 (3M) tape after 10 minutes. Adhesion was evaluated using a flatbed scanner and processing the scanned image to determine the area removed by the tape. The adhesion of HP ELECTROINK to uncoated paper was found to be 65% for 100% Black Toner and 39% for 290% Photo Black Toner. Tables 4-7 show the results of the analysis of hydroxyethylated corn starch (INGREDION PEN-COTE®), oxidized corn starch (Douglas Figure 1 shows adhesion results obtained for blends of amine-containing copolymer emulsions with hydroxyethylated tapioca starch (EXCELSIZE 22) and hydroxyethylated potato starch (WESCOTE 3070). The amine-containing copolymers were colloidally stable with the starches tested and the viscosity did not change appreciably over the observation period.
[0087] [Table 4]
[0088] [Table 5]
[0089] [Table 6]
[0090] [Table 7]
[0091] As shown in Tables 4-7, image adhesion for the amine-containing copolymers was significantly stronger than the copolymers lacking amine functionality (entries 54, 60, 66, and 72). Furthermore, the amine-containing copolymers provided very high adhesion for both 100% black and 290% photo black toners. In contrast, the copolymers lacking amine functionality provided much lower image adhesion for the 290% photo black toner.
[0092]
[0093] All documents cited herein are incorporated herein by reference for all jurisdictions, and any priority documents and / or testing procedures are included to the extent not inconsistent with this document, where such practice is permitted. As is apparent from the summary and specific embodiments above, while the forms of the disclosure have been illustrated and described, various modifications can be made without departing from the spirit and scope of the disclosure. Accordingly, the disclosure is not intended to be limited thereby. For example, the compositions described herein may not include any component or composition not expressly listed or disclosed herein. Any method may lack any step not listed or disclosed herein. Similarly, the term "comprising" is considered synonymous with the term "including". Whenever a method, composition, element, or group of elements precedes the transition phrase "comprising", we also contemplate the same composition or group of elements with "consisting essentially of", "consisting of", "selected from the group consisting of" or "is" preceding the recitation of the composition or element(s), and vice versa.
[0093]
[0094] Unless otherwise indicated, all numbers expressing quantities of ingredients, properties such as molecular weight, reaction conditions, and the like used in the specification and the related claims are to be understood as being modified in all instances by the term "about." Accordingly, unless indicated to the contrary, the numerical parameters set forth in the following specification and appended claims are approximations that may vary depending upon the desired properties sought to be obtained by the embodiments of the present invention. At the very least, and without attempting to limit the application of the doctrine of equivalents to the scope of the claims, each numerical parameter should, at the very least, be construed in light of the number of reported significant digits and by applying ordinary rounding techniques.
[0094]
[0095] Whenever a numerical range with a lower limit and an upper limit is disclosed, any number and any range within that range is expressly disclosed. In particular, all ranges of values disclosed herein (in the form of "about a to about b" or equivalently "about a to b" or equivalently "about a to b") are understood to describe all numbers and ranges encompassed within the broader range of values. Also, the terms in the claims have their plain and ordinary meaning unless otherwise expressly and unambiguously defined by the patentee. Moreover, the indefinite article "a" or "an" used in the claims is defined herein to mean one or more of the element it introduces.
[0095]
[0096] One or more exemplary embodiments are presented herein. For the sake of brevity, not all features of a physical implementation are described or shown in this application. It should be understood that in developing a physical embodiment of the present disclosure, numerous implementation-specific decisions must be made to achieve the developer's goals, such as complying with system-related, business-related, government-related compliance and other constraints, and that these decisions will vary from implementation to implementation. Although the developer's efforts may be time-consuming and laborious, such efforts are nevertheless believed to be routine for those skilled in the art and having the benefit of the present disclosure.
[0096]
[0097] Thus, the present disclosure is well adapted to attain the ends and advantages mentioned as well as those inherent therein. The particular embodiments disclosed hereinabove are illustrative only, as the disclosure may be modified and practiced in different but equivalent manners apparent to those skilled in the art and having the benefit of the teachings herein. Moreover, no limitations are intended to be imposed on the details of construction or design shown herein, other than as set forth in the following claims. Thus, it is apparent that the particular exemplary embodiments disclosed hereinabove may be altered, combined or modified, and all such variations are deemed to be within the scope and spirit of the present disclosure. The embodiments illustratively disclosed herein may be suitably practiced in the absence of any element not specifically disclosed herein and / or the optional elements disclosed herein. Specific embodiments of the present invention are as follows. [Aspect 1] 1. A primer composition comprising: an emulsion-polymerized amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid, said amine-functionalized copolymer having an amine number of from about 70 to about 140 mg KOH / g copolymer and a glass transition temperature of from about 0° C. to about 50° C.; the amine-functionalized copolymer comprising: one or more first ethylenically unsaturated monomers lacking an amine group; and one or more second ethylenically unsaturated monomers having at least one amine group; wherein the at least one amine group constitutes a pendant chain of the amine-functionalized copolymer. [Aspect 2] 2. The primer composition of embodiment 1, wherein the aqueous fluid has a pH of about 7 or greater. [Aspect 3] 3. The primer composition of embodiment 1 or 2, further comprising a neutral surfactant or an anionic surfactant dispersed in the aqueous fluid. [Aspect 4] 4. The primer composition of any one of the preceding aspects, further comprising a starch dispersed in the aqueous fluid. [Aspect 5] The primer composition of any one of the preceding embodiments, further comprising an adhesion promoter different from the amine-functionalized copolymer dispersed in the aqueous fluid. [Aspect 6] 1. A primer composition comprising: Fluids; and an amine-functionalized copolymer dispersed in said fluid having an amine number of from about 10 to about 180 mg KOH / g copolymer; the amine-functionalized copolymer comprising: one or more first ethylenically unsaturated monomers lacking an amine group; and one or more second ethylenically unsaturated monomers having at least one amine group; wherein the at least one amine group constitutes a pendant chain of the amine-functionalized copolymer. [Aspect 7] 7. The primer composition of embodiment 6, further comprising an adhesion promoter different from the amine-functionalized copolymer dispersed in the fluid. [Aspect 8] The primer composition of any one of embodiments 6 to 7, wherein the amine-functionalized copolymer further comprises at least one monomer unit having a pendant carboxylic acid. [Aspect 9] 9. The primer composition of any one of aspects 6 to 8, wherein the amine value is in the range of about 70 to about 140 mg KOH / g copolymer. [Aspect 10]
[0023] Aspect 10. The primer composition of any one of aspects 6 to 9, wherein the amine-functionalized copolymer is dispersed in the fluid as an emulsion. [Aspect 11] 11. The primer composition of any one of embodiments 6 to 10, further comprising a neutral surfactant or an anionic surfactant dispersed in the fluid. [Aspect 12] 12. The primer composition of any one of aspects 6 to 11, wherein the one or more first ethylenically unsaturated monomers comprise at least one monomer selected from the group consisting of alkyl or cycloalkyl (meth)acrylates, n-butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, styrene, substituted styrenes, dienes, 1,3-butadiene, isoprene, vinyl esters, vinyl acetate, nitriles, (meth)acrylonitrile, olefinically unsaturated halides, vinyl chloride, vinyl bromide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate; (meth)acrylamide, substituted (meth)acrylamide, N-methylol (meth)acrylamide, diacetone acrylamide, allyl methacrylate, divinylbenzene, alkylene glycol di(meth)acrylates, and any combination thereof. [Aspect 13] A primer composition according to any one of aspects 6 to 12, wherein the one or more second ethylenically unsaturated monomers comprise at least one monomer selected from the group consisting of 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl methacrylate, and any combination thereof. [Aspect 14]
[0023] Aspects 6-14. The primer composition of any one of aspects 6 to 13, wherein the amine-functionalized copolymer comprises a first portion of amine groups that are protonated and a second portion of amine groups that are unprotonated. [Aspect 15] 15. The primer composition of any one of aspects 6 to 14, further comprising a starch dispersed in the fluid. [Aspect 16] 16. The primer composition of any one of aspects 6 to 15, wherein the amine-functionalized copolymer has a glass transition temperature of from about 0 °C to about 50 °C. [Aspect 17] 17. The primer composition of any one of the preceding aspects, wherein the fluid comprises an aqueous fluid. [Aspect 18] 1. A coated substrate comprising: A base substrate; and a primer coating disposed on a surface of the base substrate; the primer coating comprises an amine-functionalized copolymer having an amine value of from about 10 to about 180 mg KOH / g copolymer; the amine-functionalized copolymer comprising: one or more first ethylenically unsaturated monomers lacking an amine group; and one or more second ethylenically unsaturated monomers having at least one amine group; wherein the at least one amine group comprises a pendant chain of the amine-functionalized copolymer. [Aspect 19] 19. The coated substrate of embodiment 18, wherein the base substrate comprises a polymeric substrate. [Aspect 20] 19. The coated substrate of embodiment 18, wherein the base substrate comprises a paper substrate. [Aspect 21] 21. The coated substrate of embodiment 20, wherein the primer coating further comprises starch. [Aspect 22] The primer coating has a thickness of about 0.05 g / m 2 ~Approx. 1.5g / m 2 22. The coated substrate of any one of embodiments 18 to 21, having a coating weight in the range of [Aspect 23] 23. The coated substrate of any one of embodiments 18 to 22, wherein the amine-functionalized copolymer has a glass transition temperature of from about 0 °C to about 50 °C. [Aspect 24] 24. The coated substrate of any one of embodiments 18 to 23, wherein the primer coating further comprises a neutral surfactant or an anionic surfactant. [Aspect 25] 25. The coated substrate of any one of embodiments 18 to 24, further comprising a toner deposited on the primer coating. [Aspect 26] The primer coating comprising: applying to the base substrate a coating composition comprising the amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid; and Allowing the aqueous fluid to evaporate leaving the primer coating disposed on the base substrate. 26. The coated substrate of any one of embodiments 18 to 25, wherein the coated substrate is disposed on the base substrate by a method comprising: [Aspect 27] A method comprising: combining in an aqueous fluid one or more first ethylenically unsaturated monomers lacking an amine group with one or more second ethylenically unsaturated monomers having at least one amine group; and forming an amine-functionalized copolymer having an amine value of from about 10 to about 180 mg KOH / g copolymer in an emulsion polymerization reaction of the one or more first ethylenically unsaturated monomers and the one or more second ethylenically unsaturated monomers carried out in the aqueous fluid, thereby providing a coating composition comprising the amine-functionalized copolymer dispersed as an emulsion in the aqueous fluid. The method comprising: [Aspect 28] disposing the coating composition on a base substrate; and allowing the aqueous fluid to evaporate leaving the amine-functionalized copolymer disposed as a primer coating on the base substrate. 28. The method of embodiment 27, further comprising:
Claims
1. 1. A primer composition comprising: an emulsion-polymerized amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid, said amine-functionalized copolymer having an amine number of 70-140 mg KOH / g copolymer and a glass transition temperature of 0° C.-50° C.; and a starch dispersed in said aqueous fluid; Including, the amine-functionalized copolymer being one or more first ethylenically unsaturated monomers lacking an amine group; and one or more second ethylenically unsaturated monomers having at least one amine group wherein the at least one amine group constitutes a pendant chain of the amine-functionalized copolymer.
2. The primer composition of claim 1 , wherein the aqueous fluid has a pH of 7 or greater.
3. 3. The primer composition of claim 1 or 2, further comprising a neutral surfactant or an anionic surfactant dispersed in the aqueous fluid.
4. 4. The primer composition of claim 1, further comprising an adhesion promoter different from the amine-functionalized copolymer dispersed in the aqueous fluid.
5. 1. A primer composition comprising: fluid; a starch dispersed in said fluid; and an amine-functionalized copolymer dispersed in said fluid having an amine number of 10 to 180 mg KOH / g copolymer; the amine-functionalized copolymer being one or more first ethylenically unsaturated monomers lacking an amine group; and one or more second ethylenically unsaturated monomers having at least one amine group wherein the at least one amine group constitutes a pendant chain of the amine-functionalized copolymer.
6. The primer composition of claim 5 further comprising an adhesion promoter different from said amine-functionalized copolymer dispersed in said fluid.
7. The primer composition of claim 5 or 6, wherein the amine-functionalized copolymer further comprises at least one monomer unit having a pendant carboxylic acid.
8. The primer composition of any one of claims 5 to 7, wherein the amine value is in the range of 70 to 140 mg KOH / g copolymer.
9. The primer composition of claim 5 , wherein the amine-functionalized copolymer is dispersed in the fluid as an emulsion.
10. 10. The primer composition of claim 5, further comprising a neutral surfactant or an anionic surfactant dispersed in the fluid.
11. 11. The primer composition of claim 5, wherein the one or more first ethylenically unsaturated monomers comprise at least one monomer selected from the group consisting of alkyl or cycloalkyl (meth)acrylates, n-butyl (meth)acrylate, methyl (meth)acrylate, ethyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, isobornyl (meth)acrylate, cyclohexyl (meth)acrylate, styrene, substituted styrenes, dienes, 1,3-butadiene, isoprene, vinyl esters, vinyl acetate, nitriles, (meth)acrylonitrile, olefinically unsaturated halides, vinyl chloride, vinyl bromide, hydroxyethyl (meth)acrylate, hydroxypropyl (meth)acrylate; (meth)acrylamide, substituted (meth)acrylamides, N-methylol (meth)acrylamide, diacetone acrylamide, allyl methacrylate, divinylbenzene, alkylene glycol di(meth)acrylates, and any combination thereof.
12. 12. The primer composition of any one of claims 5 to 11, wherein the one or more second ethylenically unsaturated monomers comprise at least one monomer selected from the group consisting of 2-(dimethylamino)ethyl methacrylate, 2-(diethylamino)ethyl methacrylate, 2-(tert-butylamino)ethyl methacrylate, and any combination thereof.
13. 13. The primer composition of claim 5, wherein the amine-functionalized copolymer comprises a first portion of protonated amine groups and a second portion of unprotonated amine groups.
14. The primer composition of any one of claims 5 to 13, wherein the amine-functionalized copolymer has a glass transition temperature of from 0°C to 50°C.
15. The primer composition of claim 1 , wherein the fluid comprises an aqueous fluid.
16. 1. A coated substrate comprising: A base substrate; and a primer coating disposed on a surface of the base substrate; the primer coating comprises starch and an amine-functionalized copolymer having an amine value of 10 to 180 mg KOH / g copolymer; the amine-functionalized copolymer being one or more first ethylenically unsaturated monomers lacking an amine group; and one or more second ethylenically unsaturated monomers having at least one amine group wherein the at least one amine group comprises a side chain of the amine-functionalized copolymer.
17. The coated substrate of claim 16 , wherein the base substrate comprises a polymeric substrate.
18. The coated substrate of claim 16 , wherein the base substrate comprises a paper substrate.
19. The primer coating has a thickness of 0.05 g / m 2 ~1.5g / m 2 19. The coated substrate of claim 16 having a coating weight in the range of
20. The coated substrate of any one of claims 16 to 19, wherein the amine-functionalized copolymer has a glass transition temperature of from 0°C to 50°C.
21. 21. The coated substrate of any one of claims 16 to 20, wherein the primer coating further comprises a neutral surfactant or an anionic surfactant.
22. 22. The coated substrate of any one of claims 16 to 21, further comprising a toner deposited on the primer coating.
23. The primer coating comprises: applying to the base substrate a coating composition comprising the amine-functionalized copolymer dispersed as an emulsion in an aqueous fluid and the starch dispersed in the aqueous fluid; and Allowing the aqueous fluid to evaporate leaving the primer coating disposed on the base substrate.
23. The coated substrate of any one of claims 16 to 22, disposed on the base substrate by a method comprising:
24. 13. A method comprising: combining in an aqueous fluid one or more first ethylenically unsaturated monomers lacking an amine group with one or more second ethylenically unsaturated monomers having at least one amine group; forming an amine-functionalized copolymer having an amine value of 10 to 180 mg KOH / g copolymer in an emulsion polymerization reaction of said one or more first ethylenically unsaturated monomers and said one or more second ethylenically unsaturated monomers carried out in said aqueous fluid, thereby providing a coating composition comprising said amine-functionalized copolymer dispersed as an emulsion in said aqueous fluid; and blending starch into said emulsion; The method comprising:
25. disposing the coating composition on a base substrate; and allowing the aqueous fluid to evaporate leaving the starch and the amine-functionalized copolymer disposed on the base substrate as a primer coating.
25. The method of claim 24, further comprising:
Citation Information
Patent Citations
Suction air quantity controller for internal combustion engine
JP1989096436A
Recorded medium and manufacture thereof
JP2000043409A
Method of forming multilayer coating film
JP2010207654A
Primer compositions and articles made therefrom
JP2019502793A
Primer Coatings for Inkjet and Liquid Electrophotographic Printing
JP2022541237A