Silicon nanocomposite structure powder for cathode material and its manufacturing method
The silicon nanocomposite structure powder addresses the limitations of conventional cathode materials by forming a non-stoichiometric silicon oxide layer on nano-sized silicon powder and combining it with graphite, enhancing discharge capacity and efficiency while reducing volume expansion and charge transfer resistance.
Patent Information
- Application Number
- JP2023517918
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-10-16
- Filing Date
- 2021-10-07
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2041-10-07
AI Technical Summary
Existing cathode materials for lithium-ion batteries face challenges such as low theoretical capacity, volumetric expansion leading to cracks and short circuits, and poor charge/discharge efficiency due to irreversible oxide phases and high energy costs in conventional manufacturing processes.
A silicon nanocomposite structure powder is produced by milling micro-sized silicon powder to nano-sized powder, oxidizing the surface with a non-stoichiometric silicon oxide layer, and combining it with highly conductive graphite powder to form a nanocomposite structure, which mitigates volume changes and reduces charge transfer resistance.
The silicon nanocomposite structure powder exhibits improved discharge capacity, efficiency, and cycle characteristics, maintaining charge/discharge efficiency at 99% or higher, with lower energy costs and higher productivity, suitable for next-generation lithium-ion batteries.
Smart Images

Figure 0007570734000002 
Figure 0007570734000003 
Figure 0007570734000004
Abstract
Description
Technical Field
[0001] The present invention relates to a cathode material for a lithium secondary battery, and more specifically, to a silicon nano composite structure powder for a cathode material and a method for producing the same, in which a SiO x (1 < x < 2) layer is formed on the surface of ultrafine silicon powder by a low-temperature oxidation reaction, and then nano-composited by milling with graphite powder having excellent conductivity, thereby improving the discharge capacity, efficiency, and cycle characteristics.
Background Art
[0002] Carbon electrodes used as cathodes of lithium-ion batteries have the advantage of excellent charging and discharging efficiency of the battery, but there are limitations in using them as cathode materials for next-generation lithium-ion batteries that require high battery capacity due to their low theoretical capacity of 375 mAh / g.
[0003] In the case of silicon (Si) used as a cathode material, it has a high theoretical capacity of about 3600 mAh / g, but when the lithium-ion battery is charged, Li reacts with Si to form Li 44 Si, resulting in a large volume expansion of up to about 400%. Such volume expansion induces cracks or electrical shorts in the cathode material of the lithium-ion battery made of silicon material, leading to a decrease in charge and discharge life and efficiency.
[0004] SiO x nano powder has a high battery capacity of approximately 1500 mAh / g, which varies depending on the oxygen concentration of SiO x When nano-sized SiO x nano powder is used as a cathode material for a lithium-ion battery, volume expansion does not occur, so there is an effect of preventing problems such as cracks or shorts.
[0005] Non-stoichiometric amorphous silicon oxide SiO x(1 < x < 2) acts as a buffer material that can mitigate the volume change (about 300%) due to lithium insertion / extraction of silicon because oxides such as lithium oxide (Li2O) and lithium silicate (Li4SiO4) are preferentially produced during the charge / discharge process, and has the characteristic of reducing (stress relaxation) the stress inside the electrode. As a result, although the charge / discharge capacity is lower than that of pure silicon, it is known to have stable cycle characteristics with a long lifespan.
[0006] Known SiO x The reason why the discharge capacity of the powder material is relatively low is that the phase fraction of silicon for reacting with lithium is much less than that of pure silicon (Si), and SiO x forms irreversible phases such as lithium oxide (Li2O) preferentially when reacting with lithium ions.
[0007] Korean Patent No. 10-1081864 (Patent Document 1) (Method for manufacturing high-purity SiO x nano powder with excellent volatility and its manufacturing apparatus) is a method of melting silicon and injecting gas onto its surface to produce SiO powder with a size of several tens of nanometers (nm). This is difficult to expect high productivity by inducing surface reaction by contacting oxygen gas with the vapor generated on the surface of the silicon melt. There is also a problem that it is difficult to induce a uniform reaction with oxygen in the process of adjusting the amount of generated vapor by adjusting the melt temperature to increase the vapor pressure. x
[0008] Korean Patent No. 10-1999191 (Patent Document 2) and No. 10-1586816 (Patent Document 3) mix Si and SiO2 raw material powders, and then heat and pulverize them at high temperature to obtain SiO x powder, and react the powder surface with Mg to form composite oxides of Mg and Si (MgSiO3 (enstatite), Mg2SiO4 (foresterite)) on the surface of the SiO x powder.
[0009] Such surface modification of Patent Document 2 and Patent Document 3 is lithium oxide of an irreversible phase formed by reaction with lithium during the charge / discharge process (SiOx -> Li2O), which has the effect of suppressing the decrease in initial charge / discharge capacity. However, the methods of Patent Documents 2 and 3 have a problem in that it is difficult to form a uniform oxide layer on the powder surface, so there is a limit to the improvement of characteristics.
[0010] Korean Patent Publication No. 10-2007-0105874 (Patent Document 4) (SiO x The manufacturing method (x<1) is a method in which a precursor (starting material) that generates vapor of silicon oxide and metal is heated in an inert gas atmosphere at a temperature range of 1100 to 2400°C, and a mixed vapor of silicon oxide and metal is precipitated on the deposition surface and collected.
[0011] Patent Document 4 has technical and economic problems such as low productivity, difficulty in forming a surface oxide film of uniform and constant thickness, and high energy costs (electrical energy).
[0012] Korean Patent Publication No. 10-2005-0119214 (Patent Document 5) discloses a method for producing SiO by heating a mixture of silicon oxide and metal powder in a vacuum. x Gas is generated and this is used to form SiO x A method for producing a precipitate.
[0013] In addition, SiO, which has good dispersibility, is produced by using pulse plasma. x Research results on a method for producing nanopowder were reported in Thin Solid Films 518 (2010), in which the oxidation reaction was limited by controlling process variables such as the flow rate of reactive gas and oxygen. x Techniques for producing nanopowders have been reported.
[0014] Thus, the core of the conventional technology is the generation of nano-sized SiO by evaporation of silicon and reaction with the ambient gas. x Production of powder (Patent Document 1), mixing silicon and SiO2 powder and reacting at high temperature to produce SiO x Preparation and grinding of powder, reaction with active metals such as Mg to produce (Mg,Si)O xThese techniques can be summarized as techniques for forming a complex oxide such as LiO and suppressing the formation of an irreversible phase (Patent Document 2 and Patent Document 3).
[0015] However, there is a very large capacity drop (decrease in charge / discharge capacity per one cycle) due to the formation of irreversible oxides at the beginning of charging and discharging, and in the manufacturing process to obtain the vapor phase, the evaporation rate is slow, resulting in low productivity, the high-temperature heating process increases energy costs, and the process has technical limitations, making it difficult to control the microstructure, such as the fraction and thickness of the oxide film, making it difficult to achieve reproducibility.
[0016] In addition, SiO x The layered silicon powder generates electrons along with large volume changes during the charge and discharge process, but a highly conductive matrix is required to transfer these to the current collector (copper plate). Conventionally, the matrix was formed on amorphous carbon, which has low conductivity, resulting in high charge transfer resistance, which adversely affected the charge and discharge cycle characteristics (capacity maintenance, charge and discharge efficiency). [Prior art documents] [Patent documents]
[0017] [Patent Document 1] Korean Patent No. 10-1081864 [Patent Document 2] Korean Patent No. 10-1999191 [Patent Document 3] Korean Patent No. 10-1586816 [Patent Document 4] Korean Patent Publication No. 10-2007-0105874 [Patent Document 5] Korean Patent Publication No. 10-2005-0119214 [Non-patent literature]
[0018] [Non-Patent Document 1] Thin Solid Films 518(2010)
Summary of the Invention
Problems to be Solved by the Invention
[0019] The present invention has been made to solve the above problems, and its object is to produce ultrafine silicon powder by high-energy milling and form a SiO x (non-stoichiometric silicon oxide, 1 < x < 2) layer on the surface of the powder by a low-temperature oxidation reaction, and then mix this with highly conductive graphite powder to form a nano-composite structure, thereby improving the charge-discharge capacity, efficiency, and cycle characteristics. Finally, it is to provide a composite material composed of nano-silicon powder surface-treated with SiO x and a highly conductive graphite base, and a silicon nano-composite structure powder for cathode material and a method for producing the same.
[0020] Another object of the present invention is that the fraction of the silicon oxide SiO x (non-stoichiometric silicon oxide, 1 < x < 2) phase is 50% or more, preferably composed of a pure SiO x phase, precisely oxidized by low-temperature oxidation, excellent in reactivity with Li ions, and to provide a silicon nano-composite structure powder for cathode material and a method for producing the same that are effective in alleviating the volume change (expansion) generated by the reaction of silicon inside the powder with Li ions.
[0021] Still another object of the present invention is to utilize a carbon-based structure of graphite containing a graphene layer with excellent conductivity when electrons are generated along with a large volume change during the charge-discharge process from silicon powder with a SiO x layer formed and transmitted to a current collector (copper plate), thereby reducing the charge transfer resistance and improving the charge-discharge cycle characteristics (capacity maintenance, charge-discharge efficiency), and to provide a silicon nano-composite structure powder for cathode material and a method for producing the same.
Means for Solving the Problems
[0022] According to one embodiment of the present invention for achieving the above object, a method for manufacturing silicon nano-composite structure powder for a cathode material includes a step of refining micro-sized micro-silicon powder into nano-sized nano-silicon powder by milling, and surface-oxidizing the nano-silicon powder at a low temperature to form SiO x (1 < x < 2) layer on the surface of the nano-silicon powder, and a step of mixing the silicon powder with SiO x (1 < x < 2) layer formed on its surface with graphite powder and milling to disperse the silicon powder with SiO x (1 < x < 2) layer formed on the base surface of the graphite powder.
[0023] The size of the nano-silicon powder is preferably set in the range of 50 to 200 nm.
[0024] The milling can be performed in the range of 6 to 10 hours by mechanical milling.
[0025] Furthermore, in the step of forming the SiO x (1 < x < 2) layer on the surface of the nano-silicon powder, the preferable heat treatment conditions for obtaining the SiO x (1 < x < 2) phase are set in the range of 350°C to 450°C when the heat treatment time is 2 hours.
[0026] The thickness of the SiO x (1 < x < 2) layer is set in the range of 5 to 20 nm.
[0027] Also, when mixing and milling the silicon powder with SiO x (1 < x < 2) layer formed on its surface with graphite powder, the milling time can be set within the range of maintaining the crystallinity of the graphite powder. In this case, the milling time is 2 hours or less, and the crystallinity of the graphite powder can be set to 50% or more.
[0028] Furthermore, on the surface with SiO xWhen milling by mixing silicon powder with a (1 < x < 2) layer formed and graphite powder, due to the friction between the silicon powder and the graphite powder, SiO x A graphene layer can be formed on the surface of the (1 < x < 2) layer.
[0029] A method for manufacturing silicon nano-composite structure powder for a cathode material according to another embodiment of the present invention includes the steps of preparing tens to hundreds of micro silicon powders, and then performing a refinement process by high-energy milling to obtain nano silicon powder, and subjecting the nano silicon powder to oxidation heat treatment to form a silicon oxide film with a SiO x (1 < x < 2) chemical structure on the surface of the nano silicon powder, and mixing the silicon powder surface-modified with the silicon oxide film and highly conductive graphite powder to perform planetary milling to form a silicon nano-composite structure powder in which the silicon powder surface-treated with SiO x is dispersed in the matrix of the graphite powder.
[0030] The graphite powder mixed with the silicon powder surface-modified with the silicon oxide film is set at 25 wt%.
[0031] The silicon oxide film is at least 50% as a fraction, and preferably, it can be a pure SiO x (1 < x < 2) phase.
[0032] By the planetary milling, pressure contact is made between the silicon powder with a SiO x (1 < x < 2) layer formed and the plate-like graphite powder.
[0033] In this case, as the milling time becomes longer and the ratio of the milling balls to the powder increases, the graphite structure collapses (decomposes). Therefore, by adjusting the two variables, the decomposition rate of the graphite structure can be adjusted. As the decomposition rate of the graphite structure increases, the electrical conductivity decreases. The amount of the graphite powder can be adjusted in consideration of the theoretical capacity (about 3600 mAh / g) of silicon.
[0034] The silicon nano-composite structure powder for cathode material according to an embodiment of the present invention includes silicon powder and SiO formed by low-temperature oxidation on the surface of the silicon powder x (1 < x < 2) layer, and a graphite matrix in which the silicon powder surface-treated with the SiO x is dispersed.
[0035] The size of the silicon powder is set in the range of 50 to 200 nm, and the thickness of the SiO x (1 < x < 2) layer is set in the range of 5 to 20 nm.
[0036] The silicon nano-composite structure powder for cathode material according to an embodiment of the present invention may further include a graphene layer formed between the SiO x (1 < x < 2) layer and the graphite matrix.
Advantages of the Invention
[0037] As described above, in the present invention, ultrafine silicon powder is produced by high-energy milling having a particle size of about 50 to 200 nanometers (nm), and SiO is formed on the surface of the powder by a low-temperature oxidation reaction x (non-stoichiometric silicon oxide) layer, and then this is mixed with conductive graphite powder and subjected to planetary milling to provide silicon nano-composite structure powder with improved discharge capacity, efficiency, and cycle characteristics.
[0038] That is, since the silicon nano-composite structure powder is formed in a silicon oxide SiO x phase by low-temperature oxidation, it has better reactivity with Li ions compared to the composite oxides (SiO x + SiO2) produced by conventional high-temperature processes, and is effective in alleviating the volume change (expansion) generated by the reaction between silicon and Li ions inside the powder.
[0039] In particular, the present invention provides a method for forming a SiO layer having a thickness of several to several tens of nanometers on the surface of ultrafine silicon powder. x This has the effect of modifying the surface, and in the process, the size of the silicon powder can be further refined. Instead of the conventional SiO2 (silicon dioxide), SiO x This surface modification technology has the advantage of effectively mitigating the volume expansion caused by the reaction of silicon with lithium ions.
[0040] SiO x The layered silicon powder generates electrons with large volume changes during the charge and discharge process, and a matrix with excellent conductivity is required to transfer these electrons to the current collector (copper plate). Conventionally, the matrix was formed using amorphous carbon, which has low conductivity, but the present invention uses a carbon matrix composed of graphite structure and graphene, which has excellent conductivity, which reduces charge transfer resistance and is effective in improving charge and discharge cycle characteristics (capacity maintenance, charge and discharge efficiency).
[0041] In other words, the electrons produced by the reaction (lithiation / deliation) between silicon and lithium ions are transferred to the copper plate, which is the current collector, and the capacity can be maintained even at a fast charge / discharge rate if the charge transfer resistance is reduced during this process. The present invention uses conductive graphite powder as the matrix to reduce the charge transfer resistance, resulting in a charge / discharge efficiency of at least 99%. [Brief description of the drawings]
[0042] [Figure 1] 1 is a manufacturing process diagram illustrating a method for manufacturing a silicon nanocomposite powder according to the present invention. FIG. [Figure 2]Photographs of an electron microscope of silicon nano-composite structure (Si / SiOx@C) powder manufactured according to the present invention, showing (a) a scanning electron microscope photograph of the powder, (b) a magnified transmission electron microscope photograph of the powder, and (c) a magnified micrograph of the high-resolution electron microscope inside the powder. [Figure 3] It is a graph showing the result of irradiating the chemical structure of the surface with XPS (X-ray photoelectron spectrometer) after oxidizing the powder manufactured by high-energy milling for 10 hours in air at 450 °C for 2 hours. [Figure 4] Graph comparing the charge and discharge cycle characteristics (capacity and efficiency changes) of pure silicon powder (nano-Si) manufactured by high-energy milling, powder (Si / SiOx) with a 10-nm-thick SiOx layer formed on the silicon powder, and the final silicon nano-composite structure powder (Si / SiOx@C) manufactured by milling (graphite crystallinity 50%) with 25 wt% of graphite added and a SiOx layer thickness of 10 nm. [Figure 5] It is a graph showing the change in capacity due to the change in the charge and discharge rate of the final silicon nano-composite structure powder manufactured according to the present invention.
Mode for Carrying Out the Invention
[0043] Hereinafter, embodiments of the present invention will be described in detail with reference to the attached drawings. In this process, the size, shape, etc. of the components shown in the drawings can be exaggeratedly illustrated for clarity and convenience of explanation.
[0044] FIG. 1 is a manufacturing process diagram for explaining a method for manufacturing silicon nano-composite structure powder according to the present invention.
[0045] Referring to FIG. 1, silicon nano-composite structure powder 50 according to the present invention has a SiO x (non-stoichiometric silicon oxide, 1 < x < 2) layer 30 formed on the surface of nano-silicon powder 20 with a size of about 50 to 200 nm by low-temperature oxidation, and SiO xThe silicon powder 25 surface-treated with [substance] is mixed with graphite powder having excellent conductivity, and by planetary milling, a structure in which the silicon powder 25 surface-treated with [substance] is dispersed in a graphite powder matrix with excellent conductivity as shown in Fig. 2 is obtained. x has a structure in which the silicon powder 25 surface-treated with [substance] is dispersed.
[0046] The silicon nanocomposite structure powder 50 according to the present invention forms a SiO (non-stoichiometric silicon oxide, 1 < x < 2) layer 30 excellent in reaction with lithium ions instead of SiO2 (silicon dioxide) generated during high-temperature heating by a low-temperature oxidation reaction. The silicon nanocomposite structure powder 50 according to the present invention can effectively alleviate the volume expansion caused by the reaction between silicon (Si) and lithium ions by such a surface modification technique. x Prevent the formation of a SiO2 (silicon dioxide) film on the surface of the nanosilicon powder 20 as described above, and the heat treatment temperature for obtaining a 100% SiO phase is preferably in the range of 350°C to 450°C. When the heat treatment temperature is less than 350°C, the formation of SiO is substantially difficult to expect. When it exceeds 450°C, a 100% SiO phase cannot be obtained, and the production ratio of SiO2 (silicon dioxide) gradually increases.
[0047] When the heat treatment temperature (i.e., oxidation temperature) is in the range of 350°C to 450°C, the thickness of the SiO layer 30 formed on the surface of the nanosilicon powder 20 is formed in the range of 5 to 20 nm, and the thickness of the SiO layer 30 also increases with the increase in the heat treatment temperature. When the heat treatment temperature reaches 550°C, the fraction of SiO2 increases and the ratio of SiO / SiO2 becomes 70%. When the heat treatment temperature reaches 650°C, the ratio of SiO / SiO2 decreases to 50%. x The heat treatment temperature for obtaining a 100% SiO phase is preferably in the range of 350°C to 450°C. When the heat treatment temperature is less than 350°C, the formation of SiO is substantially difficult to expect. x When it exceeds 450°C, a 100% SiO phase cannot be obtained, and the production ratio of SiO2 (silicon dioxide) gradually increases. x When the heat treatment temperature (i.e., oxidation temperature) is in the range of 350°C to 450°C, the thickness of the SiO layer 30 formed on the surface of the nanosilicon powder 20 is formed in the range of 5 to 20 nm, and the thickness of the SiO layer 30 also increases with the increase in the heat treatment temperature. When the heat treatment temperature reaches 550°C, the fraction of SiO2 increases and the ratio of SiO / SiO2 becomes 70%. When the heat treatment temperature reaches 650°C, the ratio of SiO / SiO2 decreases to 50%.
[0048] When the heat treatment temperature (i.e., oxidation temperature) is in the range of 350°C to 450°C, the thickness of the SiO layer 30 formed on the surface of the nanosilicon powder 20 is formed in the range of 5 to 20 nm, and the thickness of the SiO layer 30 also increases with the increase in the heat treatment temperature. When the heat treatment temperature reaches 550°C, the fraction of SiO2 increases and the ratio of SiO / SiO2 becomes 70%. When the heat treatment temperature reaches 650°C, the ratio of SiO / SiO2 decreases to 50%. x layer 30 is formed in the range of 5 to 20 nm, and the thickness of the SiO layer 30 also increases with the increase in the heat treatment temperature. When the heat treatment temperature reaches 550°C, the fraction of SiO2 increases and the ratio of SiO / SiO2 becomes 70%. When the heat treatment temperature reaches 650°C, the ratio of SiO / SiO2 decreases to 50%. x layer 30 also increases. When the heat treatment temperature reaches 550°C, the fraction of SiO2 increases and the ratio of SiO / SiO2 becomes 70%. When the heat treatment temperature reaches 650°C, the ratio of SiO / SiO2 decreases to 50%. x / SiO2 ratio becomes 70%, and when the heat treatment temperature reaches 650°C, the SiO x / SiO2 ratio decreases to 50%.
[0049] It should be noted that the specific substance represented by "[substance]" in the original text is not clear, so it is translated as "[substance]" in the translation. If there is more specific information, a more accurate translation can be provided.In this case, the heat treatment of the nano-silicon powder 20 was carried out with the heat treatment time fixed at 2 hours. When the heat treatment time increases, an SiO layer 30 with a desired thickness is formed even at a low temperature. When the heat treatment temperature is high, an SiO layer 30 with a desired thickness is formed even in a short heat treatment time. x The SiO x layer 30 is formed.
[0050] The silicon nano-composite structure powder 50 according to the present invention can adjust the thickness of the SiO x layer 30. As the thickness increases or the oxidation temperature increases, the lithium oxide (Li2O) phase fraction during charge and discharge increases, leading to the consumption of Li ions, which is one of the factors reducing the capacity.
[0051] The silicon nano-composite structure powder 50 according to the present invention has the effect of simultaneously refining silicon because the size of the nano-silicon powder 20 inside the powder decreases as the thickness of the SiO x layer 30 increases.
[0052] As described above, in the present invention, a low-temperature oxidation heat treatment is performed to obtain a 100% SiO x (1 < x < 2) phase on the surface of the nano-silicon powder.
[0053] The silicon nano-composite structure powder 50 according to the present invention has a structure in which silicon powder 25 surface-treated with SiO x is dispersed in a matrix of graphite powder with excellent conductivity. Silicon powder 25 surface-treated with SiO x and graphite powder with excellent conductivity are mixed and planetary milling is performed.
[0054] Planetary milling is a method of applying relatively high mechanical energy to the milling object. When silicon powder 25 with an SiO x (1 < x < 2) layer 30 formed on the surface and plate-shaped graphite powder are mixed and planetary milling is performed, pressure contact between the powders can be induced.
[0055] The longer the milling time and the higher the ratio of milling balls to powder, the more the graphite structure collapses (decomposes). Therefore, by adjusting the two variables, the decomposition rate of the graphite structure can be adjusted. The electrical conductivity decreases as the decomposition rate of the graphite structure increases.
[0056] In the present invention, in consideration of electrical conductivity, the milling time is carried out within a range not exceeding 2 hours in order to maintain the crystallinity of the graphite powder at 50% or more.
[0057] The amount of plate-shaped graphite powder mixed with 25 of the surface-modified silicon powder can be adjusted in consideration of the theoretical capacity of silicon (about 3600 mAh / g). For example, it is preferable to mix 25 wt%.
[0058] Hereinafter, a method for manufacturing silicon nanocomposite structure powder according to an embodiment of the present invention will be described with reference to FIG. 1.
[0059] First, after preparing 10 of pure micro Si powder having a diameter of about 20 μm (S11), a micronization process of milling this with a horizontal high-energy milling device for up to 12 hours is performed to obtain 20 of nano silicon powder having an average diameter of about 50 to 200 nm (S12).
[0060] The micro Si powder 10 is gradually micronized as the milling time increases, and is not further micronized after 12 hours.
[0061] The nano silicon powder 20 produced by the high-energy milling is subjected to oxidation heat treatment at a temperature of 250 to 650 ° C for 2 hours to form an SiO x (1 < x < 2) layer 30 on the surface of the nano silicon powder 20, and surface-modified silicon powder 25 is obtained (S13). As the heat treatment temperature increases, the SiO2 phase with respect to SiO x increases. Since the SiO2 phase does not react with Li ions, it is preferably present in the SiOx phase for use as a cathode material of a lithium secondary battery.
[0062] On the surface of the nano-silicon powder 20, SiO x (1 < x < 2) layer 30 is formed, and the surface-modified silicon powder 25 is mixed with highly conductive graphite powder and planetary milling is performed (S14). When the surface-modified silicon powder 25 and the graphite powder are mixed and milled, while powder-to-powder pressure welding is performed, the SiO x (1 < x < 2) layer 30 on the surface is coated with graphite.
[0063] In this case, due to the friction and pressure welding between the graphite and the silicon powder, a graphene layer 40 of a thin film separated from the graphite is formed on the surface of the SiO x (1 < x < 2) layer 30. Generally, graphene is one of the allotropes of carbon, and it is known to conduct electricity more than 100 times better than copper and have an electron mobility more than 100 times faster than silicon.
[0064] Also, in order to secure the electron movement path generated in the silicon powder and reduce the charge transfer resistance, it is preferable to maintain the crystallinity of the graphite that forms a film on the surface of the silicon powder.
[0065] Hereinafter, the manufacturing process of the silicon nano-composite structure powder according to the present invention will be described in detail. Table 1 shows the test conditions for examining the manufacturing conditions of the silicon nano-composite structure powder for realizing the present invention.
[0066]
Table 1
[0067] (Micro-fineization process of micro-silicon powder) After preparing low-cost pure microsilicon powder (99.9%, Sigma-Aldrich, Co.) 10 with a diameter of about 20 μm, the ratio of stainless steel balls to microsilicon (Si) powder 10 was fixed at 15:1 in a horizontal high-energy milling device for high-energy milling, and the milling time was set to 2, 4, 6, 10, and 12 hours (h) as shown in Table 1 to perform the microsilicon (Si) powder 10 refinement process.
[0068] As a result of evaluating the size of the microsilicon (Si) powder 10 depending on the milling time, it was found that the diameter decreased to about 0.2 μm (200 nm) after 6 hours, was refined to 0.05 μm (50 nm) after 10 hours, and thereafter no further change in size occurred. Therefore, it is preferable that the milling time for refinement of the microsilicon (Si) powder 10 into nanosilicon (Si) powder 20 having a size range of 0.05 μm (50 nm) to 0.2 μm (200 nm) is 6 to 10 hours.
[0069] (Oxidation heat treatment process) The nanosilicon (Si) powder 20 thus produced, having a size of 0.05 to 0.2 μm (50 to 200 nm), was subjected to an oxidation heat treatment at a temperature range of 250 to 650° C. for 2 hours. As a result, at 250° C., SiO x At 350°C, the thickness of SiO2 was about 5 nm, at 450°C, about 10 nm, at 550°C, about 15 nm, and at 650°C, about 20 nm. x was confirmed to be formed.
[0070] Considering the charge / discharge capacity, the SiO x The upper limit of the thickness of the layer 30 is preferably 20 nm. If the thickness exceeds 20 nm, the mobility of lithium ions decreases, which may cause a decrease in capacity. The most preferable condition is SiO x The thickness can be adjusted by extending the heat treatment time within the appropriate temperature range based on the above embodiment.
[0071] SiO x Not only the thickness of the silicon oxide film but also the chemical structure of the silicon oxide formed in the oxidation reaction is important. As the heat treatment temperature increases, the SiO x As shown in Table 1, the amount of SiO2 phase increased at a heat treatment temperature of 550°C. x At a heat treatment temperature of more than 650°C, the SiO2 phase fraction increases rapidly to more than 50%, which is the main cause of the decrease in electrochemical capacity. Therefore, it is not preferable to exceed 650°C.
[0072] The SiO2 phase does not react with Li ions, so SiO x In addition, when the heat treatment temperature is 350° C. and 450° C., the surface of the nanosilicon (Si) powder 20 is preferably in the 100% SiO phase. x phase is obtained. Therefore, 100% SiO x The heat treatment temperature for obtaining the SiO phase is preferably 350°C to 450°C. x The most preferred heat treatment temperature for forming the thickest layer 30 is 450°C.
[0073] (Graphite matrix and composite process) The surface-modified silicon (Si) powder 25 is formed by pressing graphite onto the surface of the silicon (Si) powder 25 to secure a path for electrons generated by the electrochemical reaction of silicon (Si) and Li ions and to mitigate the volume change of silicon. The graphite powder matrix has excellent conductivity, and SiO x Thus, a silicon nanocomposite powder 50 was obtained in which the silicon powder 25 having the surface treatment thereon was dispersed.
[0074] In order to press the graphite onto the surface of the silicon powder 25, the surface-modified silicon (Si) powder 25 was mixed with the graphite powder and subjected to planetary milling for 0.5 to 4 hours.
[0075] The amount of graphite powder can be changed depending on the design capacity (discharge capacity), and was set to 25wt% in the example. The milling conditions were as follows: Zirconia was used as the milling bead, and the ratio of beads to powder was fixed at 10:1. After 2 hours of milling, the crystallinity of the graphite powder collapsed by 50% compared to the initial state, and after 4 hours, it decreased to about 10%.
[0076] The present invention was achieved based on a 2-hour milling condition where the crystalline fraction of graphite is 50%. If the crystalline fraction of graphite is less than 50%, the charge transfer resistance increases, leading to a decrease in charge / discharge capacity. However, the milling device used in the present invention can be a similar milling device other than planetary milling, and in this case, the condition is limited to a minimum crystalline fraction of graphite of 50%.
[0077] FIG. 2 is an electron microscope image of the silicon nanocomposite powder produced according to the present invention, in which (a) shows the shape of the final synthesized silicon nanocomposite powder 50, (b) is a high-magnification transmission electron microscope (TEM) image of the silicon nanocomposite powder 50, and (c) is a high-resolution electron microscope image of the silicon nanocomposite powder 50.
[0078] From the electron microscope image in Fig. 2(c), amorphous SiO x It was confirmed that a layer was formed, and a thin graphene layer was formed on the outer layer. The inside (center) of the powder was crystalline silicon, and the outside was SiO x , continuous graphene layers are observed, with the outermost layer being a carbon (graphite) matrix structure.
[0079] The silicon nanocomposite powder produced by the present invention has a structure in which SiO is formed on the surface of the silicon powder by an oxidation reaction. x The formation of the layer also has the additional effect of reducing the size of the silicon powder inside.
[0080] Figure 3 is a graph showing the result of irradiating the chemical structure of the surface of nano-silicon powder produced by high-energy milling for 10 hours with XPS (X-ray photoelectron spectrometer) after oxidative heat treatment in air at 450 °C for 2 hours.
[0081] Referring to Figure 3, peaks of the Si-O bond binding energy are observed around 102 eV and 104 eV, which means the formation of the SiO x (1 < x < 2) phase. Si 0+ is the binding energy of pure silicon. No peak of the binding energy indicating the formation of SiO2 was observed. However, SiO2 was observed under the heat treatment conditions of 550 °C and 650 °C, and the SiO2 phase fraction appeared at about 50% in the case of 650 °C. This means that the SiO2 phase that does not react with Li ions is 50%, indicating that it does not sufficiently play a role in alleviating the volume expansion occurring during the charge and discharge process of silicon. As a result, it can be confirmed that the oxidation heat treatment temperature at which a 100% SiO x phase is formed is preferably 450 °C as a condition for maintaining electrochemical properties.
[0082] Figure 4 shows the charge and discharge cycle characteristics (capacity and efficiency changes) of a coin cell using the silicon nano-composite structure powder produced according to the present invention.
[0083] In Figure 4, nano-Si is pure silicon powder produced by high-energy milling, Si / SiO x is powder with a SiO x layer having a thickness of 10 nm formed on silicon, Si / SiO x @C is powder of an example of the present invention in which after forming a SiO x layer to a thickness of 10 nm, 25 wt% of graphite is further added and pressure-bonded by milling, and coin cells are fabricated using each of them, and the result of comparative evaluation of electrochemical properties.
[0084] The coin cells were fabricated according to the coin-type half-cells (CR-2032) standard, and consisted of 80% active material (silicon), 10% SFG6 as a graphite-based conductive agent, 2% Ketjenblack as a conductive agent, and 8% polyacrylic acid (PAA) as a binder. After preparing the slurry, it was screen-printed, dried, and punched into a circular shape to fabricate a disk-shaped cathode plate. The coin cells were fabricated in a glove box filled with high-purity Ar gas using Li foil as the reference electrode, Celgard 2400 membrane as the separator, and a mixture of EC (ethylene carbonate), DEC (diethyl carbonate), and FEC (fluoroethylene carbonate) dissolved in LiPF6 (lithium hexafluorophosphate) in a volume ratio of 5:70:25.
[0085] Referring to FIG. 4, the first cycle (1 cycle) was performed at a 0.1C rate (1C rate means that the complete charge / discharge time is 1 hour), and from the fourth cycle onwards, the charge / discharge cycle was performed at a 1C rate for a total of 300 cycles.
[0086] As a result, compared to pure silicon powder (nano-Si), SiO x Silicon powder (Si / SiO x ) and silicon nanocomposite powder with graphene formed on its surface (Si / SiO x In particular, graphene-formed silicon nanocomposite powder (Si / SiO x In the case of @C), the initial one-cycle capacity was 1748mAh / g and the efficiency was 87%, and at 300 cycles the capacity was 1355mAh / g, the capacity retention rate was 88%, and the average efficiency was 99.4%, demonstrating excellent properties as a high-efficiency, high-capacity cathode material.
[0087] FIG. 5 shows the silicon nanocomposite powder (Si / SiO xCells were manufactured by @C), charge-discharge tests were conducted at various speeds, and the results are those of evaluating the effect of the charge-discharge speed on the capacity change (high-rate charge-discharge performance). In FIG. 5, 1C means the charge-discharge condition within 1 hour, and 3C means the charge-discharge condition within 20 minutes.
[0088] Referring to FIG. 5, excellent performance was exhibited in which the reproducibility of the capacity change was maintained even for repeated speed changes. There was almost no difference in capacity recovery even after high-rate charge-discharge, and a very excellent result was shown in which the capacity exceeded 1000 mAh / g under the condition of 5C. This is due to the fact that high-quality SiO x It is a result showing that the graphite powder characteristics excellent in formation and conductivity are well melt-compounded and a nano-composite structure is well formed.
[0089] As described above, the silicon nano-composite structure powder for cathode material according to the present invention is different from the conventional methods for manufacturing SiO x powder, such as evaporation, surface reaction, and condensation of conventional silicon. First, inexpensive micro-silicon powder is used to produce nano-silicon powder with a size of about 50 to 200 nm in a short time by a mechanical milling process. Second, by surface-oxidizing the nano-silicon powder at a low temperature, instead of SiO2, SiO x (1 < x < 2) A surface layer with a chemical structure is formed. Third, in the process of mixing and milling the silicon powder (Si / SiO x ) with the surface formed with SiO x and graphite powder, by adjusting the milling conditions, a highly conductive base structure can be complexed to obtain silicon nano-composite structure powder.
[0090] Therefore, in the present invention, the chemical structure is completely different from that of the conventional SiO x powder, and it has the effect of uniformly modifying the powder surface. In this process, it is also possible to expect an accompanying effect that the size of the silicon powder decreases as the SiO x layer is formed on the silicon powder surface by an oxidation reaction.
[0091] In addition, the present invention has the effect of reducing charge transfer resistance when electrons generated by the reaction between the active material silicon and lithium ions are transferred to the current collector (copper plate) by forming a nano-composite structure with a graphite matrix having excellent conductivity, and has the characteristics of excellent cycle characteristics and charge / discharge efficiency.
[0092] Furthermore, in the present invention, charge / discharge tests were performed at various rates to evaluate the effect of charge / discharge rate on capacity change (high-speed charge / discharge performance). As a result, the reproducibility of capacity change was maintained even after repeated rate changes. This is due to the high-quality SiO x This indicates that the graphite powder properties, excellent in formation and conductivity, are successfully blended and the nanocomposite structure is well formed.
[0093] In addition, from the economical point of view, the present invention uses SiO x Compared to the conventional manufacturing process, it has lower energy costs, higher productivity, and is easier to mass-produce, which has the effect of strengthening the price competitiveness of high-performance silicon cathode materials.
[0094] Although the present invention has been described above by way of examples of specific preferred embodiments, the present invention is not limited to the above embodiments, and various changes and modifications may be made by those having ordinary skill in the art to which the present invention pertains without departing from the spirit of the present invention. [Industrial Applicability]
[0095] The present invention provides a silicon nanocomposite powder for use as a cathode material with improved discharge capacity, efficiency and cycle characteristics, which has low energy costs, high productivity, is easy to mass-produce, and is cost-competitive with high-performance silicon cathode materials, and can be applied to the field of anode active materials for lithium secondary batteries. The invention described in the original claims of the present application is appended below. [1] The step of refining micro-sized microsilicon powder into nano-sized nanosilicon powder by milling, Surface-oxidizing the nanosilicon powder to form a non-stoichiometric amorphous silicon oxide SiO x (1 < x < 2) layer on the surface of the nanosilicon powder, thereby obtaining nanosilicon powder surface-treated with SiO x A method for manufacturing silicon nano-composite structure powder for cathode materials, comprising the steps of: [2] The method for manufacturing silicon nano-composite structure powder for cathode materials according to [1], wherein the size of the nanosilicon powder obtained by milling the silicon powder is in the range of 50 to 200 nm. [3] The method for manufacturing silicon nano-composite structure powder for cathode materials according to [2], wherein the milling is performed in the range of 6 to 10 hours by mechanical milling. [4] In the step of forming a SiO x (1 < x < 2) layer on the surface of the nanosilicon powder, the heat treatment conditions for obtaining the SiO x (1 < x < 2) phase are set in the range of 350°C to 450°C when the heat treatment time is 2 hours. The method for manufacturing silicon nano-composite structure powder for cathode materials according to [1]. [5] The thickness of the SiO x (1 < x < 2) layer is in the range of 5 to 20 nm. The method for manufacturing silicon nano-composite structure powder for cathode materials according to [1]. [6] After mixing the nanosilicon powder surface-treated with SiO x with graphite powder and then milling to disperse the nanosilicon powder surface-treated with SiO x in the base of the graphite powder, the method for manufacturing silicon nano-composite structure powder for cathode materials according to [1], further comprising the step of forming a graphene layer on the surface of the SiO x (1 < x < 2) layer of the nanosilicon powder surface-treated with SiO x (1 < x < 2). [7] The milling time is 2 hours or less. The method for manufacturing silicon nano-composite structure powder for cathode materials according to [6]. [8] When mixing and milling the nanosilicon powder surface-treated with SiO x with graphite powder, the milling time is set so that the crystallinity of the graphite powder is maintained at 50% or more. The method for manufacturing silicon nano-composite structure powder for cathode materials according to [6]. [9] After preparing microsilicon powder, a step of performing a refinement process by high-energy milling to obtain nanosilicon powder, Surface-oxidizing the nano-silicon powder to form a non-stoichiometric amorphous silicon oxide SiO x (1 < x < 2) layer on the surface of the nano-silicon powder to obtain nano-silicon powder surface-treated with SiO x ; and a step of obtaining nano-silicon powder surface-treated with SiO ; mixing the nano-silicon powder surface-treated with SiO x and graphite powder and performing planetary milling to disperse the nano-silicon powder surface-treated with SiO x in the matrix of the graphite powder, and forming a graphene layer on the surface of the SiO x (1 < x < 2) layer of the nano-silicon powder surface-treated with SiO x . A method for manufacturing silicon nano-composite structure powder for cathode material, comprising:
[10] The method for manufacturing silicon nano-composite structure powder for cathode material according to [9], wherein the graphite powder to be mixed is set at 25 wt%.
[11] Nano-silicon powder, On the surface of the nano-silicon powder, a non-stoichiometric amorphous silicon oxide SiO x (1 < x < 2) layer formed by surface oxidation, And a graphite matrix in which the nano-silicon powder surface-treated with SiO x is dispersed, A graphene layer is formed on the surface of the SiOx (1 < x < 2) layer of the nano-silicon powder surface-treated with SiO x . Silicon nano-composite structure powder for cathode material.
[12] The silicon nano-composite structure powder for cathode material according to
[11] , wherein the size of the nano-silicon powder obtained by milling the silicon powder is set in the range of 50 to 200 nm.
[13] The silicon nano-composite structure powder for cathode material according to
[11] , wherein the thickness of the SiO x (1 < x < 2) layer is set in the range of 5 to 20 nm.
[14] The silicon nano-composite structure powder for cathode material according to
[11] , wherein the crystallinity of the graphite matrix is set to 50% or more.
Claims
1. A step of milling the micro-sized microsilicon powder into a nano-sized nanosilicon powder; The nanosilicon powder is surface-oxidized to form non-stoichiometric amorphous silicon oxide (SiO) on the surface of the nanosilicon powder. x By forming a (1<x<2) layer, SiO x and mixing the nanosilicon powder surface-treated with SiO x with graphite powder and then milling the mixture to disperse the nanosilicon powder surface-treated with SiO x in the matrix of the graphite powder.
2. The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 1, wherein the size of the nanosilicon powder obtained by milling the silicon powder is in the range of 50 to 200 nm.
3. The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 2, wherein the milling is carried out by mechanical milling for a period of 6 to 10 hours.
4. The surface of the nanosilicon powder is coated with SiO x In the step of forming the (1<x<2) layer, SiO x The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 1, wherein the heat treatment conditions for obtaining the (1<x<2) phase are set in the range of 350°C to 450°C when the heat treatment time is 2 hours.
5. The SiO x The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 1, wherein the thickness of the (1<x<2) layer is in the range of 5 to 20 nm.
6. The SiO x The SiO of nanosilicon powder surface-treated with x The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 1, further comprising forming a graphene layer on a surface of the (1<x<2) layer.
7. The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 6, wherein the milling time is 2 hours or less.
8. The SiO x 7. The method for producing a silicon nanocomposite structure powder for a cathode material according to claim 6, wherein when the nanosilicon powder surface-treated with the above-mentioned method is mixed with graphite powder and milled, the milling time is set so that the crystallinity of the graphite powder is maintained at 50% or more.
9. preparing microsilicon powder and then performing a micronization process by high energy milling to obtain nanosilicon powder; The nanosilicon powder is surface-oxidized to form non-stoichiometric amorphous silicon oxide (SiO) on the surface of the nanosilicon powder. x (1<x<2) layers are formed to form SiO x obtaining a surface-treated nanosilicon powder; The SiO x The nanosilicon powder and graphite powder that have been surface-treated in the above step are mixed and subjected to planetary milling, and the SiO x The nanosilicon powder having been surface-treated with the above-mentioned SiO x The SiO of nanosilicon powder surface-treated with x and forming a graphene layer on the surface of the (1<x<2) layer.
10. The method for producing silicon nanocomposite structure powder for cathode material according to claim 9, wherein the graphite powder to be mixed is set at 25 wt% based on the total of the nanosilicon powder surface-treated with SiOx and the graphite powder.
11. Nanosilicon powder; The surface of the nanosilicon powder is formed with non-stoichiometric amorphous silicon oxide (SiO) by surface oxidation. x (1<x<2) layers, The SiO x and a graphite matrix having nanosilicon powder dispersed therein, the nanosilicon powder having been surface-treated with the above-mentioned method. The SiO x The SiO of nanosilicon powder surface-treated with x A silicon nanocomposite structure powder for cathode materials, in which a graphene layer is formed on the surface of the (1<x<2) layer.
12. The silicon nanocomposite structure powder for cathode material according to claim 11, wherein the size of the nanosilicon powder is set in the range of 50 to 200 nm.
13. The SiO x The silicon nanocomposite structure powder for cathode material according to claim 11, wherein the thickness of the (1<x<2) layer is set in the range of 5 to 20 nm.
14. The silicon nanocomposite structure powder for cathode material according to claim 11, wherein the crystallinity of the graphite matrix is set to 50% or more.
Citation Information
Patent Citations
Method for producing negative electrode material of lithium ion battery, lithium ion battery, method of manufacturing negative electrode material of lithium ion battery, and manufacturing apparatus thereof
JP2017188329A
Composite silicon anode material, preparation method and use
JP2019505948A
Manufacturing method of high purity siox NANO particle with excellent volatility and apparatus for manufacturing the same
KR101081864B1
Negative active material for non-aqueous electrolyte rechargeable battery, the preparation method thereof, and rechargeable battery including the same
KR101586816B1
Silicon oxide composite for anode material of secondary battery and method for preparing the same
KR101999191B1