Cement composition for ground improvement
The use of anhydrous gypsum with high Blaine specific surface area and controlled particle size in cement compositions addresses the challenge of solidifying organic-rich soils and reducing hexavalent chromium elution, achieving improved strength and reduced chromium leaching.
Patent Information
- Application Number
- JP2020122519
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-07-17
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2040-07-17
AI Technical Summary
Existing cement compositions struggle to effectively solidify soils with a large amount of organic matter such as volcanic ash clay and humus, and they also increase the elution of hexavalent chromium when applied to such soils.
A cement composition using anhydrous gypsum with a high Blaine specific surface area and controlled particle size distribution is employed, which includes a Blaine specific surface area of at least 4500 cm²/g and a cumulative volumetric passing 50% particle size of 15 μm or less, along with other cementitious materials like Portland cement and blast furnace slag.
The composition achieves both good strength development and significant reduction in hexavalent chromium elution, with enhanced uniaxial compressive strength and reduced hexavalent chromium leaching.
Smart Images

Figure 0007570774000001 
Figure 0007570774000002 
Figure 0007570774000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a cement composition for ground improvement that can be applied to soils containing a large amount of organic matter, such as volcanic ash clayey soil and humus soil, and that can suppress the amount of elution of hexavalent chromium and the like. [Background technology]
[0002] Prior art relating to cement compositions containing gypsum anhydride includes the inventions described in, for example, Patent Documents 1 and 2 below.
[0003] In Patent Document 1, the powder size is 3000 cm 2 / g or more 13000cm 2 / g or less, 60% to 90% by mass of ground granulated blast furnace slag, fineness of 2,500 cm 2 / g or more 8,000cm 2 The present invention discloses a cement-containing composition comprising 100 parts by mass of a mixture containing 3% by mass to 20% by mass of anhydrous gypsum having a particle size of 100% by mass or less and 5% by mass to 37% by mass of Portland cement, and 5 parts by mass to 30 parts by mass of recycled fine powder, which is a classified product of powder generated after separating and recovering a filling material from a hardened cement body, and has an average particle size of 2.0 μm or more and 10.0 μm or less and a cumulative 90% particle size of 20.0 μm or less.
[0004] In addition, Patent Document 1 states that (A)(a-1) has a powder size of 3000 cm 2 / g or more 13000cm 2 / g or less, 60 mass% to 90 mass% of ground granulated blast furnace slag, (a-2) fineness of 2,500 cm 2 / g or more 8,000cm 2The present invention relates to a method for preparing a ground improvement slurry by adding water to a cement-containing composition containing 100 parts by mass of a mixture containing 3% to 20% by mass of anhydrous gypsum having a particle size of 100 to 37% by mass of (a-3) Portland cement, and (B) 5 to 30 parts by mass of recycled fine powder, which is a classified product of powder generated after separating and recovering a filling material from a hardened cement body, and has an average particle size of 2.0 μm or more and 10.0 μm or less and a cumulative 90% particle size of 20 μm or less, such that the water / solid ratio (by mass) is 40% to 250%, and the obtained ground improvement slurry is poured into soil for 1 m. 3 and adding 150 kg to 1,200 kg per slab.
[0005] Patent Document 2 describes a method for producing a gypsum waste material by heat treatment, which has a Blaine specific surface area of 8000 cm 2 The present invention also discloses an admixture for high-strength cement compositions, which contains type II anhydrous gypsum having a molecular weight of 100000000000000 / g or more, and which contains, per 100 parts by mass of the type II anhydrous gypsum, 30 to 400 parts by mass of a siliceous fine powder, 5 to 20 parts by mass of slag powder, and 0.1 to 2 parts by mass of a water retention agent; and a high-strength cement composition, which contains the admixture for high-strength cement compositions and cement, and in which the admixture for high-strength cement compositions is added in an amount of 5 to 30 parts by mass per 100 parts by mass of cement.
[0006] In addition, this high-strength cement composition has a strength of 100N / mm 2 The strength is over 100N / mm 2 It is stated that it is possible to obtain cement products such as high strength Hume pipes and box culverts. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Patent No. 5734756 [Patent Document 2] Patent No. 4999179 Summary of the Invention [Problem to be solved by the invention]
[0008] The invention described in Patent Document 1 mentioned above aims to reduce carbon dioxide emissions during production by minimizing the amount of cement mixed in the cement-containing composition, and describes producing a ground improvement slurry using a classified powder product generated after separating and recovering the filler material from the hardened cement body, and applying the slurry to ground improvement work, but does not take into consideration the characteristics of the soil to which the slurry is to be applied.
[0009] In addition, the invention described in the above-mentioned Patent Document 2 enhances the expressed strength of a high-strength cement composition by blending appropriate amounts of type II anhydrous gypsum obtained by heat-treating waste gypsum, siliceous fine powder, slag powder, etc., but is not intended for ground improvement.
[0010] However, regarding the cement composition for ground improvement, there is a problem that it is difficult to solidify soil containing a large amount of organic matter, such as volcanic ash clayey soil and humus soil, and therefore a large amount of cement-based solidification material must be added. In addition, when the composition is applied to soil containing hexavalent chromium, there is a problem that the amount of hexavalent chromium eluted is high.
[0011] The present invention aims to provide a cement composition for ground improvement that is applicable to soils containing a large amount of organic matter, such as volcanic ash clayey soil and humus soil, and that is capable of achieving both good strength development and suppression of the amount of elution of hexavalent chromium. [Means for solving the problem]
[0012] The present invention relates to a cement composition for ground improvement comprising cement and anhydrous gypsum, the anhydrous gypsum having a Blaine specific surface area of 4500 cm 2 / g or more or a cumulative volume passing 50% particle size of 15 μm or less.
[0013] Blaine specific surface area is 4500cm 2The cement composition uses anhydrous gypsum having a Blaine specific surface area of 4900 cm 2 / g or more, more preferably 6000cm 2 / g or more, more preferably 10,000 cm 2 / g or more. It is presumed that the strength is increased because the dissolution rate of anhydrous gypsum increases as the Blaine specific surface area of the anhydrous gypsum increases.
[0014] In addition, a cement composition using anhydrous gypsum having a cumulative volume passing 50% particle size of 15 μm or less is used. The cumulative volume passing 50% particle size of the anhydrous gypsum is preferably 12 μm or less, more preferably 8 μm or less, and even more preferably 5 μm or less.
[0015] In addition, a cement composition using anhydrous gypsum having a cumulative volume passing 99% particle diameter of 100 μm or less is used. The cumulative volume passing 99% particle diameter of the anhydrous gypsum is preferably 50 μm or less, more preferably 30 μm or less.
[0016] The crystallite size (crystal particle diameter) of anhydrous gypsum is preferably 133 nm or less, more preferably 110 nm or less, and even more preferably 90 nm or less, 60 nm or less, or 50 nm or less. It is presumed that the crystallite size becomes small due to the energy generated by grinding the anhydrous gypsum or the process of producing the anhydrous gypsum.
[0017] The method for producing anhydrous gypsum is not particularly limited. Natural anhydrous gypsum may be crushed or classified. Anhydrous gypsum may be synthesized from waste gypsum, or anhydrous gypsum produced as a by-product during the production of hydrofluoric acid may be used.
[0018] The proportion of anhydrous gypsum in the cement composition is not limited. It is preferably 5% to 20%. If it is less than 5%, the effect of anhydrous gypsum is limited. If it exceeds 20%, the proportion of Portland cement decreases relatively and strength may not be fully expressed. Also, if the proportion of anhydrous gypsum exceeds 20%, excessive expansion may occur when solidifying soil with a high sand content, such as sandy soil, if a large amount is added.
[0019] In addition, the cement composition other than anhydrous gypsum is not limited, and examples of the cement composition other than anhydrous gypsum include portland cement, ground granulated blast furnace slag, and fly ash. Effect of the Invention
[0020] The cement composition for ground improvement of the present invention can be applied to soils containing a large amount of organic matter, such as volcanic ash clayey soil and humus soil, and can achieve both good strength development and suppression of the amount of elution of hexavalent chromium.
[0021] For the same soil quality, amount of solidification material added, and solidification material mix, the higher the Blaine specific surface area of the anhydrous gypsum or the smaller the cumulative volume passing 50% particle size, the higher the unconfined compressive strength of the solidification material will be. Also, the amount of hexavalent chromium eluted will be smaller. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0022] Tests 1 and 2 were conducted to confirm the effects of the present invention. The effects of anhydrous gypsum with different particle sizes, the crystallite size of anhydrous gypsum, the ratio of anhydrous gypsum, the presence or absence of a combination with ground granulated blast furnace slag with different fineness, and sample soil with different wet densities and moisture contents were confirmed.
[0023] [Test 1] Materials used Ordinary Portland cement (symbol N): Blaine specific surface area 3350 cm 2 / g Blast furnace slag powder 1 (SL1): Blaine specific surface area 4450 cm 2 / g · Anhydrous gypsum (symbol CS)
[0024] The test conditions and test results of Test 1 are shown in Tables 1 to 4.
[0025] [Table 1]
[0026] [Table 2]
[0027] [Table 3]
[0028] [Table 4]
[0029] In comparing Levels No. 1 to No. 5, Levels No. 6 to No. 10, Levels No. 11 to No. 15, Levels No. 16 to No. 20, Levels No. 21 to No. 25, and Levels No. 26 to No. 30, with the same sample soil, amount of solidification material added, and solidification material mix, there is a general trend that the higher the Blaine specific surface area of the anhydrous gypsum or the smaller the cumulative volume passing 50% particle size, the higher the uniaxial compressive strength of the solidification material.
[0030] In addition, the Blaine specific surface area is 12980 cm 2 / g of anhydrous gypsum 4 (CS4) and a Blaine specific surface area of 10660 cm 2 In the case of anhydrous gypsum 5 (CS5) at 200 / g, the difference in the unconfined compressive strength of the solidification material is small and may be reversed.
[0031] In addition, the cumulative volume passing through the device is almost the same. rate Standard No. 19 (using 50% grain size anhydrous gypsum) Cumulative volume passing rate 50% particle size 3.1μm , crystallite size 88.7nm ) and Level No. 20 ( Cumulative volume passing rate 50% particle size 3.2μm , crystallite size 41.8 nm ) the crystallite size of anhydrous gypsum is small No. 20 has a higher uniaxial compressive strength and is almost the same as No. 4 (50% cumulative volume passing rate grain size 3.1 μm, crystallite size 88.7 nm) and No. 5, which use anhydrous gypsum with a cumulative volume passing rate of 50% grain size. So, level No. 5 Uniaxial compression Strength is level No. 4. Uniaxial compressive strength The results were higher than those of the control. Also, the amount of hexavalent chromium eluted tends to be smaller.
[0032] In addition, comparing levels No. 1 to No. 5 and levels No. 16 to No. 20, it was confirmed that the amount of hexavalent chromium leaching was smaller in the cases of anhydrous gypsum 2 to 5, which used finer anhydrous gypsum, than in the case of anhydrous gypsum 1 (CS1).
[0033] In the test soils of levels No. 1 to No. 20, which used the volcanic ash clayey soil (V1) in Table 2, the comparison of levels No. 1 to No. 5 with levels No. 6 to No. 10 and the comparison of levels No. 11 to No. 15 with levels No. 16 to No. 20 showed that the amount of solidification material added was 150 kg / m 3 from 250kg / m 3 When the concentration of Cr increases to 100%, the strength (unconfined compressive strength at ages 7 days and 28 days) generally more than doubles.
[0034] In the test soils No. 21 to No. 30, which used humic soil (C1) in Table 2, the addition amount of solidification material was 150 kg / m3. 3 to 300 kg / m 3 When the concentration of Cr increases to 100%, the strength (unconfined compressive strength at ages 7 days and 28 days) increases significantly.
[0035] [Test 2] Materials used Ordinary Portland cement (symbol N): Blaine specific surface area 3350 cm 2 / g Blast furnace slag powder 1 (SL1): Blaine specific surface area 4450 cm 2 / g Blast furnace slag powder 2 (symbol SL2): Blaine specific surface area 11020 cm 2 / g · Anhydrous gypsum (symbol CS)
[0036] The test conditions and test results of Test 2 are shown in Tables 5 to 8.
[0037] [Table 5]
[0038] [Table 6]
[0039] [Table 7]
[0040] [Table 8]
[0041] Comparing Levels No. 31 to No. 33, and Levels No. 34 to No. 36, if the same sample soil, amount of solidification material added, and solidification material mix are used, the higher the Blaine specific surface area of the anhydrous gypsum or the smaller the cumulative volume passing 50% particle size, the higher the uniaxial compressive strength of the solidification material. In addition, the amount of hexavalent chromium leaching tends to be smaller.
[0042] Standards No. 32 and No. 33, which use fine anhydrous gypsum, have higher strength than standard No. 31. Standard No. 32, which uses small anhydrous gypsum crystallite size, has higher strength than standard No. 33.
[0043] Standard No. 35, which used fine gypsum anhydride 5 (CS5), had twice the strength (unconfined compressive strength at 7 days of age) of standard No. 31, which used gypsum anhydride 1 (CS1). When CS5 was used, standard No. 36, which used half the amount of gypsum anhydride compared to standard No. 35, had the same strength as standard No. 34, which used CS1 anhydride.
[0044] The amount of solidification material added is 150 kg / m 3Comparing standard No. 37, which uses anhydrous gypsum 1 (CS1), with standard No. 39, which uses anhydrous gypsum 5 (CS5), it is found that the use of anhydrous gypsum 5 (CS5) results in more than twice the strength of the use of anhydrous gypsum 1 (CS1).
[0045] Similarly, when the amount of solidification material added is 300 kg / m 3 Comparing standard No. 38, which uses anhydrous gypsum 1 (CS1), with standard No. 40, which uses anhydrous gypsum 5 (CS5), it is found that the strength achieved using anhydrous gypsum 5 (CS5) is nearly twice that achieved using anhydrous gypsum 1 (CS1).
Claims
1. A cement composition for ground improvement comprising cement and anhydrous gypsum, or cement, anhydrous gypsum and ground granulated blast furnace slag, wherein the anhydrous gypsum has a Blaine specific surface area of 10,000 cm 2 / g or more and 12000 cm 2 / g or less, a cumulative volume passing rate of 50% particle size is 5 μm or less, a cumulative volume passing rate of 99% particle size is 100 μm or less, and the crystallite size is 50 nm or less.
2. 2. The ground improvement cement composition according to claim 1, wherein the proportion of said anhydrous gypsum is 5 to 20 mass %.
Citation Information
Patent Citations
JP1974099179A
Rotor for induction motor
JP1982034756A
Solidifier for organic soft ground
JP1994287555A
Injection material for lowering hexavalent chromium
JP2002097057A
Hardening material composition for viscous soil
JP2004137322A