Composition and cured product thereof

The composition of an olefin-aromatic vinyl compound-aromatic polyene copolymer with polar monomers and fillers addresses the challenges of low dielectric properties and heat resistance in insulating materials, ensuring effective high-frequency signal transmission and adherence to copper foil in electronic boards.

JP7570901B2Active Publication Date: 2024-10-22DENKA CO LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020197380
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-11-27
Publication Date
2024-10-22
Estimated Expiration
2040-11-27

AI Technical Summary

Technical Problem

Existing insulating materials face challenges in achieving low dielectric properties, heat resistance, and processability for high-frequency signal transmission, particularly in electronic board applications where solder reflow processes are involved, limiting suitable materials for such applications.

Method used

A composition comprising an olefin-aromatic vinyl compound-aromatic polyene copolymer with specific molecular weight and monomer content, combined with polar monomers like maleimide and fillers, to achieve a dielectric constant of 2.7 or less and dielectric loss tangent of 1.5 × 10^-3 or less, along with a CTE of 130 ppm/K or less, suitable for high-frequency applications.

Benefits of technology

The composition provides excellent low dielectric properties and heat resistance, maintaining mechanical integrity and adhesion to copper foil, suitable for high-frequency signal transmission and electronic board applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007570901000001
    Figure 0007570901000001
  • Figure 0007570901000002
    Figure 0007570901000002
  • Figure 0007570901000003
    Figure 0007570901000003
Patent Text Reader

Abstract

To provide a composition capable of making a cured product having excellent low dielectric characteristics.SOLUTION: A composition includes: an olefin-aromatic vinyl compound-aromatic polyene copolymer; and a polar monomer, where the value in a measured frequency range of 27-42GHz of a dielectric constant of a cured product of the composition found by a resonator method is 2.7 or less, the value in a measured frequency range of 27-42GHz of a dielectric tangent of a cured product of the composition found by a resonator method is 1.5×10-3 or less, and the CTE (coefficient of linear thermal expansion) of the composition found on the basis of a JPCA standard "electronic circuit board standard third edition" Clause 16 "material standard for print circuit board" is 130 ppm / K or less.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a composition and a cured product thereof. [Background technology]

[0002] As communication frequencies move into the gigahertz range and higher, there is an increasing need for insulating materials with low dielectric properties. Polyolefins such as polyethylene and aromatic vinyl compound polymers such as polystyrene are known as materials that exhibit excellent low dielectric constants and low dielectric loss tangents because they do not have polar groups in their molecular structures. However, their heat resistance as electrical insulators is problematic because their heat resistance depends on their crystalline melting point or glass transition temperature, and furthermore, because they are thermoplastic resins, there are problems with the film formation process (Patent Document 1).

[0003] Fluorine-based resins such as perfluoroethylene have the characteristics of low dielectric constant, low dielectric loss, and excellent heat resistance, but are difficult to process and form into films, making them poorly suited for devices. There are also issues with the adhesive strength to the copper foil of wiring. On the other hand, substrates and insulating materials using post-curing resins such as epoxy resins, unsaturated polyester resins, polyimide resins, and phenolic resins have been widely used due to their heat resistance and ease of handling, but their dielectric constant and dielectric loss are relatively high, and improvements are needed as insulating materials for high frequencies (Patent Document 2).

[0004] An electrical insulating material made of a graft or block copolymer made of olefin-based and styrene-based polymer segments has been proposed (Patent Document 3). This material focuses on the inherent low dielectric constant and low dielectric loss of olefin-based and styrene-based hydrocarbon polymers. The manufacturing method involves general graft polymerization of commercially available polyethylene and polypropylene in the presence of styrene monomer, divinylbenzene monomer, and a radical polymerization initiator, and this method has the problem that the graft efficiency (crosslinking density) does not increase and the uniformity of the polymer is insufficient. Furthermore, the obtained polymer contains gel, and there are problems with poor processability and filling properties. This material is a thermoplastic resin and does not have sufficient heat resistance, so it is necessary to add a heat-resistant resin such as 4-methyl-1-pentene. Therefore, it is difficult to apply this material to a molding method in which it is applied or filled in a specified location and then cured.

[0005] Patent Documents 4 to 6 disclose cured products obtained from specific polymerization catalysts and made of ethylene-olefin (aromatic vinyl compound)-polyene copolymers with specific compositions and blends and non-polar vinyl compounds, and also disclose compositions with common fillers such as silica.

[0006] It is also known to add a filler when forming a resin sheet, and spherical silica is sometimes used as such a filler, as described in Patent Documents 7 and 8. However, the effects of combinations of resin types and filler types have not been fully studied. [Prior art documents] [Patent documents]

[0007] [Patent Document 1] Special Publication No. 52-031272 [Patent Document 2] Japanese Patent Application Publication No. 6-192392 [Patent Document 3] Japanese Patent Application Publication No. 11-060645 [Patent Document 4] JP 2010-280771 A [Patent Document 5] JP 2009-161743 A [Patent Document 6] JP 2010-280860 A [Patent Document 7] JP 2003-165718 A [Patent Document 8] Special Publication No. 2013-528558 Summary of the Invention [Problem to be solved by the invention]

[0008] Even for thermoplastic compositions that are easily moldable, there is a demand for cured products that have excellent low dielectric properties required for insulating materials for high-frequency signal transmission. In particular, for electronic substrate applications that involve a solder reflow process involving exposure to high temperatures, the suitability requirements are strict, and the number of materials that can withstand practical use is limited. For this reason, there is a demand for the provision of materials with such excellent low dielectric properties. [Means for solving the problem]

[0009] That is, the present invention can provide the following aspects.

[0010] Aspect 1. an olefin-aromatic vinyl compound-aromatic polyene copolymer; Polar monomers and A composition comprising: the dielectric constant of a cured product of the composition, as determined by a resonator method, is 2.7 or less in a measurement frequency range of 27 GHz to 42 GHz; The dielectric tangent of the cured product of the composition, as determined by a resonator method, is 1.5×10 -3 is as follows: The CTE (coefficient of linear expansion) of the composition is 130 ppm / K or less, as determined based on JPCA standard "Electronic Circuit Board Standard 3rd Edition", Section 16 "Material Standard for Printed Wiring Boards". A composition comprising:

[0011] Aspect 2. 2. The composition of claim 1, wherein the polar monomer is one or more selected from the group consisting of maleimide, bismaleimide, maleic anhydride, glycidyl (meth)acrylate, triallyl isocyanurate, tri(meth)acrylic isocyanurate, and trimethylolpropane tri(meth)acrylate.

[0012] Aspect 3. 3. The composition of claim 1 or 2, wherein the polar monomer is a bismaleimide having an aromatic ring, the aromatic ring having one or more groups having one or more carbon atoms thereon.

[0013] Aspect 4. Aspect 4. The composition according to any one of aspects 1 to 3, wherein the amount of the polar monomer is in the range of 0.1 to 30 parts by mass per 100 parts by mass of the total of the copolymer and the polar monomer.

[0014] Aspect 5. The copolymer satisfies the following conditions (1) to (4): (1) The number average molecular weight of the copolymer is 500 or more and 100,000 or less. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass or more and 70% by mass or less. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of vinyl groups and / or vinylene groups derived from aromatic polyene units is 1.5 or more and less than 20 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, the aromatic vinyl compound monomer units, and the aromatic polyene monomer units is 100 mass %. The composition according to any one of aspects 1 to 4, wherein all of the above is satisfied.

[0015] Aspect 6. 6. The composition of any one of aspects 1 to 5, wherein a storage modulus of a cured product of the composition at 25° C. divided by a storage modulus of a cured product of the composition at 250° C. is 20 or less.

[0016] Aspect 7. The composition according to any one of Aspects 1 to 6, further comprising a second monomer, which is one or more selected from the group consisting of an aromatic vinyl compound monomer and an aromatic polyene monomer, and / or a resin.

[0017] Aspect 8. 8. The composition of claim 7, comprising 300 parts by weight or less of the second monomer and / or resin per 100 parts by weight of the copolymer.

[0018] Aspect 9. The composition according to any one of aspects 1 to 8, further comprising a curing agent.

[0019] Aspect 10. The composition according to any one of aspects 1 to 9, which is curable.

[0020] Aspect 11. A molded article obtained by curing the composition according to any one of aspects 1 to 10.

[0021] Aspect 12. 12. The molded article according to embodiment 11, which is a sheet.

[0022] Aspect 13. 13. The molded article according to embodiment 11 or 12, which is an electrical insulating material.

[0023] Aspect 14. A laminate comprising a layer containing the composition according to any one of aspects 1 to 10 and a metal foil.

[0024] Aspect 15. A cured product obtained by curing the laminate according to embodiment 14.

[0025] Aspect 16. A single layer CCL, multilayer CCL, single layer FCCL, or multilayer FCCL substrate comprising the cured product of embodiment 15. Effect of the Invention

[0026] The present invention provides a composition, the cured product of which has excellent low dielectric properties. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] The present invention will be described in more detail below. In this specification, the olefin-aromatic vinyl compound-aromatic polyene copolymer may be simply referred to as a copolymer. Unless otherwise specified, the numerical range in this specification includes the upper and lower limit values. In this specification, the term sheet also includes the concept of a film. Furthermore, even if the term film is described in this specification, the term sheet also includes the concept of a sheet. In this specification, the term (meth)acrylate is a concept that includes acrylate and methacrylate.

[0028] <Composition> In this specification, the composition (curable composition) may be referred to as a resin composition or a curable resin composition. The composition of the present invention contains an olefin-aromatic vinyl compound-aromatic polyene copolymer having a certain range of composition and molecular weight range described below. The composition further contains a "polar monomer" described below. The composition may further contain one or more other components such as "other added resin components", "inorganic fillers", "monomers other than polar monomers", and "curing agents" described below.

[0029] <Olefin-aromatic vinyl compound-aromatic polyene copolymer> Examples of general methods for producing an olefin-aromatic vinyl compound-aromatic polyene copolymer that can be used in the present invention are described in JP 2009-161743 A, JP 2010-280771 A, WO 00 / 37517, etc. This olefin-aromatic vinyl compound-aromatic polyene copolymer satisfies all of the following conditions (1) to (4). (1) The number average molecular weight of the copolymer is 500 or more and 100,000 or less, preferably 5,000 or more and 100,000 or less, more preferably 20,000 or more and 100,000 or less, and further preferably 30,000 or more and 100,000 or less. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass or more and 70% by mass or less. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 to less than 20, preferably 1.5 to less than 7, and more preferably 2 to less than 5, per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having 2 to 20 carbon atoms, and the total of the olefin monomer units, the aromatic vinyl compound monomer units, and the aromatic polyene monomer units is 100 mass %.

[0030] The present olefin-aromatic vinyl compound-aromatic polyene copolymer (sometimes simply abbreviated as "copolymer" in this specification) is obtained by copolymerizing each of the monomers of an olefin, an aromatic vinyl compound, and an aromatic polyene.

[0031] The olefin monomer is at least one selected from α-olefins having 2 to 20 carbon atoms and cyclic olefins having 5 to 20 carbon atoms, and is a compound consisting of carbon and hydrogen without substantially containing oxygen, nitrogen, or halogen. Examples of α-olefins having 2 to 20 carbon atoms include ethylene, propylene, 1-butene, 1-hexene, 1-octene, 1-decane, 1-dodecane, 4-methyl-1-pentene, and 3,5,5-trimethyl-1-hexene. Examples of cyclic olefins having 5 to 20 carbon atoms include norbornene and cyclopentene. The olefin is preferably a combination of ethylene and an α-olefin or a cyclic olefin other than ethylene, or ethylene alone. When ethylene alone or the mass ratio of the α-olefin other than ethylene contained therein / ethylene is 1 / 7 or less, more preferably 1 / 10 or less, the peel strength of the obtained cured product with copper foil or copper wiring can be increased, which is preferable. More preferably, the content of α-olefin monomer units other than ethylene contained in the copolymer is 6% by mass or less, most preferably 4% by mass or less, or the olefin is ethylene alone. In this case, the peel strength with copper foil or copper wiring can be further increased, which is more preferable. In addition, in the preferred combination of ethylene and α-olefin other than ethylene, the glass transition temperature of the ethylene-α-olefin-aromatic vinyl compound-aromatic polyene sequence of the finally obtained cured product can be freely adjusted within the range of about -60°C to -10°C depending on the type and content of the α-olefin.

[0032] The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and examples thereof include styrene, paramethylstyrene, paraisobutylstyrene, various vinylnaphthalenes, and various vinylanthracenes.

[0033] The aromatic polyene monomer is a polyene having 5 to 20 carbon atoms and having multiple vinyl groups and / or vinylene groups in its molecule, preferably a polyene having 8 to 20 carbon atoms. The aromatic polyene monomer is preferably a polyene having 8 to 20 carbon atoms and having multiple vinyl groups in its molecule, more preferably a compound having an aromatic vinyl structure such as ortho-, meta-, or para-various divinylbenzenes or mixtures thereof, divinylnaphthalene, divinylanthracene, p-2-propenylstyrene, or p-3-butenylstyrene, which is substantially free of oxygen, nitrogen, or halogen and is composed of carbon and hydrogen. In addition, a bifunctional aromatic vinyl compound described in JP-A-2004-087639, for example, 1,2-bis(vinylphenyl)ethane (abbreviation: BVPE), can also be used. Among these, preferably, ortho-, meta-, or para-various divinylbenzenes or mixtures thereof are used, and most preferably, a mixture of meta- and para-divinylbenzene is used. In this specification, these divinylbenzenes are referred to as "divinylbenzenes." When divinylbenzenes are used as the aromatic polyene, they are preferred because they have high curing efficiency and are easy to cure when a curing treatment is carried out.

[0034] The above-mentioned olefin, aromatic vinyl compound, and aromatic polyene monomers may also contain polar groups, such as olefins containing oxygen atoms, nitrogen atoms, etc., aromatic vinyl compounds containing oxygen atoms, nitrogen atoms, etc., or aromatic polyenes containing oxygen atoms, nitrogen atoms, etc., but the total mass of these monomers containing polar groups is preferably 10 mass% or less of the total mass of the composition, more preferably 3 mass% or less, and most preferably does not contain any monomers containing polar groups. By making the monomer 10 mass% or less, it is possible to improve the low dielectric properties of the cured product obtained by curing the composition (low dielectric constant and low dielectric loss can be set to appropriate values). It should be noted that, just to be sure, the term "monomer containing a polar group" in this context refers only to a component in the above-mentioned copolymer, and does not refer to a "polar monomer" that the composition contains separately from the copolymer.

[0035] The number average molecular weight of the copolymer is 500 to 100,000, preferably 5,000 to 100,000, more preferably 20,000 to 100,000, and even more preferably 30,000 to 100,000. By adjusting the number average molecular weight to such a range, even if an additional component such as a resin is added in an uncured state, the composition is less sticky, and the effect of improving thermoplasticity is obtained, and further, good physical properties such as high strength at break and high elongation at break can be easily imparted to the finally obtained cured product. When the number average molecular weight is 500 or more, the mechanical properties of the composition in the uncured stage are high and the adhesiveness is low, so that the composition is easily molded as a thermoplastic resin. When the number average molecular weight is 100,000 or less, the moldability is improved. The content of aromatic vinyl compound monomer units contained in the copolymer is 0% by mass to 70% by mass, preferably 0% by mass to less than 70% by mass, more preferably 10% by mass to 60% by mass, and even more preferably 10% by mass to 55% by mass. When the content of aromatic vinyl compound monomer units is 70% by mass or less, the glass transition temperature of the cured product of the final composition is not near room temperature, and the toughness and elongation at low temperatures are improved. When the content of aromatic vinyl compound monomer units is 10% by mass or more, the aromaticity of the copolymer is improved, the compatibility with flame retardants and fillers is improved, the flame retardants do not bleed out, and the fillers can be easily filled. When the content of aromatic vinyl compound monomer units is 10% by mass or more, a cured product of the composition having high peel strength with copper foil or copper wiring is obtained.

[0036] In the present copolymer, the content of vinyl groups and / or vinylene groups derived from aromatic polyene units is 1.5 or more and less than 20, preferably 1.5 or more and less than 7, more preferably 2 or more and less than 5 per number average molecular weight. The content of vinyl groups and / or vinylene groups may be collectively referred to as "vinyl group content" below. If the vinyl group content is less than 1.5, the crosslinking efficiency is low, and it is difficult to obtain a cured product with sufficient crosslinking density. If the vinyl group content is increased, it becomes easier to improve the mechanical properties of the finally obtained cured product at room temperature and high temperature. The vinyl group content derived from aromatic polyene units per number average molecular weight in the present copolymer is calculated by the number average molecular weight (Mn) calculated in terms of standard polystyrene obtained by GPC (gel permeation chromatography) method known to those skilled in the art and the 1 It can be obtained by comparing the vinyl group content and vinylene group content derived from aromatic polyene units obtained by H-NMR measurement. For example, 1 By comparing the intensities of the peak areas obtained by H-NMR measurement, it was found that the content of vinyl groups derived from aromatic polyene units in the copolymer was 0.142% by mass, and the number average molecular weight calculated as standard polystyrene by GPC measurement was 70,927. The molecular weight of the vinyl groups derived from aromatic polyene units in the number average molecular weight was the product of these, 100.8, which was divided by the formula weight of the vinyl groups, 27, to be 3.7. In other words, the content of vinyl groups derived from aromatic polyene units per number average molecular weight in this copolymer is 3.7. 1 The assignment of peaks obtained by H-NMR measurement is known from the literature. 1 A method for determining the composition of a copolymer from a comparison of peak areas obtained by H-NMR measurement is also known. In this specification, the content of divinylbenzene units in a copolymer is determined based on the peak intensity ( 1 In other words, the content of divinylbenzene units is calculated from the content of vinyl groups derived from divinylbenzene units, assuming that one vinyl group is derived from one divinylbenzene unit in the copolymer.

[0037] In the present copolymer, the preferred olefin monomer unit content is 30% by mass or more, and particularly preferably 45% by mass or more. The total of the olefin monomer units, aromatic vinyl compound monomer units, and aromatic polyene monomer units is 100% by mass. When the olefin monomer unit content is 30% by mass or more, the toughness (elongation) of the finally obtained cured product is improved, and cracks during curing, a decrease in the impact resistance of the cured product, and cracks during a heat cycle test of the cured product do not occur. In the present copolymer, the preferred olefin monomer unit content is 90% by mass or less.

[0038] In the present copolymer, specific examples of suitable olefin-aromatic polyene copolymers not containing aromatic vinyl compound monomer units include ethylene-divinylbenzene copolymers, ethylene-propylene-divinylbenzene copolymers, ethylene-1-butene-divinylbenzene copolymers, ethylene-1-hexene-divinylbenzene copolymers, and ethylene-1-octene-divinylbenzene copolymers.

[0039] In the present copolymer, examples of the olefin-aromatic vinyl compound-aromatic polyene copolymer containing an aromatic vinyl compound monomer unit include ethylene-styrene-divinylbenzene copolymer, ethylene-propylene-styrene-divinylbenzene copolymer, ethylene-1-hexene-styrene-divinylbenzene copolymer, and ethylene-1-octene-styrene-divinylbenzene copolymer. The copolymer used in the present invention can be produced by the production methods described in, for example, International Publication No. 00 / 37517, JP 2009-161743 A, and JP 2010-280771 A. The amount of the copolymer that may be contained in the present composition can be arbitrarily set depending on the application. In a preferred embodiment, the amount of the copolymer may be in the range of 70 to 99.9 parts by mass, more preferably 80 to 99.9 parts by mass, and even more preferably 85 to 99.9 parts by mass, relative to 100 parts by mass of the total of the copolymer and the polar monomer. By setting the amount of the copolymer in this range, it becomes easier to appropriately control the dielectric constant and dielectric loss tangent of the obtained cured product.

[0040] <Polar monomer> The polar monomer contained in the composition of the present invention refers to a monomer that has polarity in its molecular structure due to the presence of a polar group or the like. Such a polar monomer not only imparts adhesiveness to other materials necessary as an insulating material to the cured product of the composition, but also makes it possible to keep both the dielectric constant and the dielectric dissipation factor of the cured product low. It is generally known that the increase or decrease in the dielectric constant and the increase or decrease in the dielectric dissipation factor of a certain material tend to be mutually exclusive. In other words, it is easy for the other to increase if one is lowered, and it has been conventionally thought that it is impossible to lower both. However, the present inventor has found that the crosslink density is improved in the cured product of a composition to which a polar monomer has been added, and thus both the dielectric constant and the dielectric dissipation factor can be kept low, and thus the present invention has been completed. According to the present invention, for example, the dielectric constant can be set to 2.7 or less (more preferably 2.5 or less) and the dielectric dissipation factor can be set to 1.5×10 -3 Less than or equal to 1.2×10 -3 This has the remarkable effect of suppressing the

[0041] Moreover, in the case of a composition containing a polar monomer, the CTE (coefficient of linear expansion) of the cured product can also be suppressed to a low value. It has been thought that it is difficult to achieve both of these effects, but the present invention overturns this idea and provides a very useful insulating material.

[0042] Examples of the polar monomer include various maleimides, bismaleimides, maleic anhydride, glycidyl (meth)acrylate, triallyl isocyanurate (TAIC), tri(meth)acryl isocyanurate, trimethylolpropane tri(meth)acrylate, and derivatives thereof. Maleimides and bismaleimides that can be used in the present invention are described in, for example, International Publication No. 2016 / 114287 and JP-A No. 2008-291227, and can be purchased, for example, from Daiwa Kasei Kogyo Co., Ltd. and Designer Molecules Inc. These maleimide group-containing compounds may be used as polyamino bismaleimide compounds from the viewpoints of solubility in organic solvents, high frequency characteristics, high adhesion to conductors, moldability of prepregs, and the like. Polyamino bismaleimide compounds can be obtained, for example, by subjecting a compound having two maleimide groups at the terminals to a Michael addition reaction with an aromatic diamine compound having two primary amino groups in the molecule. When attempting to obtain high crosslinking efficiency with the addition of a small amount, polar monomers having two or more functional groups, such as bismaleimides, triallyl isocyanurate (TAIC), trimethylolpropane tri(meth)acrylate, and derivatives thereof, are preferred.

[0043] In a preferred embodiment, a bismaleimide having one or more aromatic rings can be used as the polar monomer, and more preferably, a bismaleimide having one or more substituents having one or more carbon atoms (such as an aliphatic substituent such as an alkyl group or a cyclic aliphatic substituent such as a cycloalkyl group) on the aromatic ring can be used. In a more preferred embodiment, a bismaleimide having the following structural formula can be used. [ka] In the formula, R1 and R1' are each independently (may be the same or different) a hydrogen atom or a substituent having 1 or more carbon atoms (preferably 1 to 20 carbon atoms), and examples of such a substituent include a linear or branched alkyl group (methyl group, ethyl group, n-butyl group, tert-butyl group, hexyl group, etc.), a (meth)acryloyl group, an acyl group, a substituted or unsubstituted aryl group, etc. In addition, R2 in the formula is a bond (i.e., two aromatic rings are directly bonded) or a divalent linker group having 1 or more carbon atoms (preferably 1 to 20 carbon atoms) (for example, a linear or branched alkylene group, an ether group, etc.). It is considered that the presence of a plurality of R1 and R1' other than hydrogen atoms on the aromatic ring in this way improves the rigidity of the obtained crosslinked structure, which contributes to the effects of the present invention. Without wishing to be bound by any particular theory, it is believed that such bismaleimides having aromatic rings not only have high insulating properties, but also have a bulky substituent that prevents the molecular structure from easily twisting, allowing a rigid crosslinked structure to be formed with the copolymer, thereby resulting in particularly remarkable effects. R1 is preferably a methyl group. R1' is preferably an ethyl group. R2 is preferably a methylene group.

[0044] In another preferred embodiment, a polyfunctional (meth)acrylate derivative having a long-chain aliphatic substituent (e.g., an alkyl group having about 5 to 20 carbon atoms) can be used as the polar monomer. The polyfunctional (meth)acrylate refers to a compound having two or more (meth)acryloyl groups. It is believed that such a long-chain aliphatic substituent is bulky, and therefore the crosslinked structure between the polar monomer and the copolymer can be rigidly maintained.

[0045] The amount of the polar monomer that may be contained in the composition can be set arbitrarily depending on the application. In a preferred embodiment, the amount of the polar monomer may be in the range of 0.1 to 30 parts by mass, more preferably 0.1 to 20 parts by mass, and even more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of the total of the copolymer and the polar monomer. By setting the amount of the polar monomer in this range, it becomes easier to appropriately control the dielectric constant and dielectric loss tangent of the obtained cured product.

[0046] The molecular weight of the polar monomer is preferably less than 10,000, more preferably less than 6,000.

[0047] <Additive resin (resin other than the above copolymer that may be contained in the present composition)> The resin component in the present composition may further contain a resin compound other than the copolymer (hereinafter, also simply referred to as "additive resin"). Any additive resin may be used as long as it does not impair the effects of the present composition, and preferably one or more selected from a hydrocarbon-based elastomer, polyphenylene ether, and aromatic polyene resin described below may be used. Among these, polyphenylene ether or a hydrocarbon-based elastomer is more preferable. Among the hydrocarbon-based elastomers, a conjugated diene polymer is preferable. Among the conjugated diene polymers, 1,2-polybutadiene is preferable. By using one or more selected from a hydrocarbon-based elastomer, polyphenylene ether, and aromatic polyene resin, the effect of the polar monomer can be promoted. The amount of the additive resin may be preferably in the range of 1 to 500 parts by mass in total, more preferably 1 to 300 parts by mass in total, relative to 100 parts by mass of the copolymer.

[0048] <Hydrocarbon elastomer> The amount of the hydrocarbon-based elastomer is preferably 1 to 500 parts by mass, more preferably 1 to 200 parts by mass, based on 100 parts by mass of the copolymer. The hydrocarbon-based elastomer that can be suitably used in the composition of the present invention may have a number average molecular weight of 20,000 or more, preferably 30,000 or more. Examples of the hydrocarbon-based elastomer include a single or multiple elastomers selected from ethylene-based or propylene-based elastomers, conjugated diene-based polymers, block copolymers or random copolymers of aromatic vinyl compounds-conjugated dienes, and hydrogenated products thereof. Examples of the ethylene-based elastomers include ethylene-α-olefin copolymers such as ethylene-octene copolymers and ethylene-1-hexene copolymers, EPR, and EPDM. Examples of the propylene-based elastomers include atactic polypropylene, polypropylene with low stereoregularity, and propylene-α-olefin copolymers such as propylene-1-butene copolymer.

[0049] <Conjugated diene polymer> Examples of the conjugated diene polymer include polybutadiene and 1,2-polybutadiene. Examples of the aromatic vinyl compound-conjugated diene block or random copolymer and their hydrogenated products (hydrogenated products) include SBS, SIS, SEBS, SEPS, SEEPS, SEEBS, etc. Suitable 1,2-polybutadiene is available, for example, as a product of JSR Corporation, and is also available from Nippon Soda Co., Ltd. under the product names of liquid polybutadiene: B-1000, B-2000, and B-3000. Examples of the copolymer containing a 1,2-polybutadiene structure that can be used suitably include "Ricon 100" from TOTAL CRAY VALLEY. When the resin or resins selected from these hydrocarbon elastomers are liquid (approximately 300,000 mPa s or less) particularly at room temperature (25°C), from the viewpoints of the handleability and moldability (handleability as a thermoplastic resin) of the composition of the present invention in an uncured state, the amount used is preferably in the range of 1 to 30 parts by mass, and more preferably 1 to 20 parts by mass, per 100 parts by mass of the copolymer.

[0050] <Polyphenylene ether> As the polyphenylene ether, a commercially available known polyphenylene ether can be used. The number average molecular weight of the polyphenylene ether is arbitrary, and considering the moldability of the composition, the number average molecular weight is preferably 10,000 or less, and most preferably 5,000 or less. The number average molecular weight may be preferably 500 or more. In addition, when the polyphenylene ether is added for the purpose of curing the composition of the present invention, it is preferable that the molecular end is modified and / or that one molecule has multiple functional groups. Examples of the functional group include an allyl group, a vinyl group, and an epoxy group. As the functional group, a radically polymerizable functional group is preferable. As the radically polymerizable functional group, a vinyl group is preferable. As the vinyl group, a (meth)acrylic group or an aromatic vinyl group is preferable. In other words, in the composition of the present invention, a bifunctional polyphenylene ether in which both ends of the molecular chain are modified with a radically polymerizable functional group is particularly preferable. Examples of such polyphenylene ether include Noryl (trademark) SA9000 manufactured by SABIC, and particularly preferably, a bifunctional polyphenylene ether oligomer (OPE-2St) manufactured by Mitsubishi Gas Chemical Company, Inc. can be used. The amount of polyphenylene ether used in the composition of the present invention is preferably from 1 to 500 parts by mass, more preferably from 1 to 300 parts by mass, and even more preferably from 1 to 200 parts by mass, based on 100 parts by mass of the copolymer.

[0051] <Aromatic polyene resin> Aromatic polyene resins include divinylbenzene reactive hyperbranched copolymers (PDV) manufactured by Nippon Steel Chemical & Material Co., Ltd. Such PDVs are described, for example, in the literature "Synthesis of polyfunctional aromatic vinyl copolymers and development of new IPN-type low dielectric loss materials using them" (Kawabe Masanao et al., Journal of the Japan Institute of Electronics Packaging, p. 125, Vol. 12 No. 2 (2009)). Other examples of aromatic polyene resins include aromatic polyene polymer resins having the above-mentioned aromatic polyene monomer as the main constituent unit.

[0052] <Hardening agent> The curing agent that may be contained in the composition may be a known curing agent that can be used for the polymerization or curing of conventional aromatic polyenes and aromatic vinyl compounds. Examples of such curing agents include radical polymerization initiators, cationic polymerization initiators, and anionic polymerization initiators, and preferably radical polymerization initiators are used. Preferred are organic peroxides and azo polymerization initiators, which can be freely selected depending on the application and conditions. A catalog listing organic peroxides can be found on the NOF Corporation website, for example: https: / / www.nof.co.jp / business / chemical / product01a.html https: / / www.nof.co.jp / business / chemical / product01b.html https: / / www.nof.co.jp / business / chemical / product01c.html It can be downloaded from. Organic peroxides are also described in the catalogs of Fujifilm Wako Pure Chemical Industries, Ltd. and Tokyo Chemical Industry Co., Ltd. The curing agent used in the present invention can be obtained from these companies. Also, a known photopolymerization initiator using light, ultraviolet light, or radiation can be used as the curing agent. Examples of curing agents using a photopolymerization initiator include a photoradical polymerization initiator, a photocationic polymerization initiator, and a photoanionic polymerization initiator. Such photopolymerization initiators are available, for example, from Tokyo Chemical Industry Co., Ltd. Furthermore, curing by radiation or electron beam itself is also possible. It is also possible to perform crosslinking and curing by thermal polymerization of the raw materials contained without containing a curing agent.

[0053] There is no particular limit to the amount of the curing agent used, but generally, 0.01 to 10 parts by mass is preferred per 100 parts by mass of the composition (preferably excluding the curing agent and solvent). When using a curing agent such as a peroxide or azo polymerization initiator, the curing process is carried out at an appropriate temperature and time, taking into consideration its half-life. In this case, the conditions are arbitrary according to the curing agent, but generally, a temperature range of about 50°C to 180°C is appropriate.

[0054] <Other monomers> The composition may further include a monomer other than the polar monomer described above (hereinafter, also referred to as "second monomer" or "second monomer"). The amount of such a second monomer may be any amount, but may be preferably 300 parts by mass or less relative to 100 parts by mass of the copolymer. The composition may not substantially include the second monomer. When the second monomer is included, the amount is preferably 1 part by mass or more, more preferably 5 parts by mass or more. When the amount of the second monomer is 300 parts by mass or less, the uncured composition does not have a viscous property, and molding processing as a thermoplastic resin becomes easy. In addition, when the content of the second monomer, which is easily volatile, is below a certain level, odor at the uncured stage does not become a problem. When a solvent is added to the composition to make the product in a varnish form, the monomer is lost as the solvent evaporates during use, and there is a problem that the substantial content of the second monomer is easily reduced. In addition, when the product is in the form of an uncured sheet, when the second monomer is included in a certain amount or less, the content of the second monomer is less likely to change during storage. The second monomer that can be suitably used in the composition of the present invention preferably has a molecular weight of less than 1000, more preferably less than 500. The monomer that can be suitably used in the composition of the present invention is an aromatic vinyl compound monomer, an aromatic polyene monomer, and / or a polar monomer. The monomer is preferably a monomer that can be polymerized by a radical polymerization initiator, and more preferably one or more of the group consisting of aromatic vinyl compounds and aromatic polyenes. In addition, BVPE (1,2-bis(vinylphenyl)ethane) described in JP-A-2003-212941 can also be suitably used.

[0055] From the viewpoint of increasing the mechanical strength (elastic modulus) of the cured product at high temperatures, the aromatic vinyl compound is preferably 50 parts by mass or more and 250 parts by mass or less, more preferably 80 parts by mass or more and 200 parts by mass or less, relative to 100 parts by mass of the copolymer. From the viewpoint of increasing the mechanical strength (elastic modulus) of the cured product at high temperatures, the aromatic polyene is preferably 1 part by mass or more and 30 parts by mass or less, relative to 100 parts by mass of the copolymer. When an aromatic vinyl compound and an aromatic polyene are used, the mass ratio of the aromatic vinyl compound and the aromatic polyene is preferably 70 to 99: 1 to 30, more preferably 85 to 95: 5 to 15, relative to a total of 100 parts by mass of the aromatic vinyl compound and the aromatic polyene.

[0056] <Solvent> An appropriate solvent (solvent) may be added to the composition of the present invention as necessary. The solvent is used to adjust the viscosity and fluidity of the composition. As the solvent, a volatile one is preferable, and for example, cyclohexane, toluene, ethylbenzene, acetone, isopropanol, etc. are used. In addition, the amount of the solvent used is preferably 10 parts by mass or less per 100 parts by mass of the copolymer from the viewpoint of moldability and handling of the composition as a thermoplastic resin before curing, and from the viewpoint of removal during and after curing, it is more preferable that the solvent is not substantially used. By "not substantially used," it is preferable that the solvent is 5 parts by mass or less, more preferably 1 part by mass or less, and most preferably 0 parts by mass. In addition, when used as a varnish, it is preferable to add an appropriate solvent to the composition of the present invention. The solvent is used to adjust the viscosity and fluidity of the composition as a varnish. As the solvent, a solvent having a boiling point of a certain degree or more is preferable, because the thickness of the applied film becomes uniform when the boiling point at atmospheric pressure is high, that is, when the volatility is low. A preferable boiling point is 100°C or more at atmospheric pressure, more preferably 130°C or more and 300°C or less. Examples of solvents suitable for such varnishes include cyclohexane, toluene, xylene, mesitylene, tetralin, acetone, ethylbenzene, limonene, mixed alkanes, mixed aromatic solvents, ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, ethylene glycol monobutyl ether, etc. The amount of the solvent used is preferably in the range of 10 to 2000 parts by mass, more preferably 5 to 500 parts by mass, and even more preferably 10 to 300 parts by mass, relative to 100 parts by mass of the composition of the present invention.

[0057] In this specification, the number average molecular weight of the above-mentioned copolymers and other polymers is determined as follows. The molecular weight is determined as the number average molecular weight (Mn) converted to standard polystyrene using GPC (gel permeation chromatography). The measurement can be performed under the following conditions.

[0058] (Number average molecular weight of 1000 or more) Column: Two TSKgel MultiporeHxl-M φ7.8×300 mm (Tosoh Corporation) columns are connected in series. Column temperature: 40℃ Solvent: THF Flow rate: 1.0ml / min. Detector: RI detector (differential refractive index detector)

[0059] (Number average molecular weight less than 1000) Columns: one TSKgel G3000HXL φ7.8×300 mm (manufactured by Tosoh Corporation), one TSKgel G2000HXL φ7.8×300 mm (manufactured by Tosoh Corporation), and four TSKgel G1000HXL φ7.8×300 mm (manufactured by Tosoh Corporation) connected in series. Column temperature: 40℃ Solvent: THF Flow rate: 0.5ml / min. Detector: RI detector (differential refractive index detector)

[0060] <Filling agent> The composition may further contain any amount of filler depending on the application. Such a filler may be an inorganic filler, and may be added for the purpose of controlling the thermal expansion coefficient, controlling the thermal conductivity, and reducing the cost. The amount of filler used may be as much as 2000 parts by mass per 100 parts by mass of the copolymer and the polar monomer. In particular, when adding an inorganic filler, it is preferable to use a known surface modifier, such as a silane coupling agent. In particular, when the objective of the present invention is to obtain a composition excellent in low dielectric constant and low dielectric loss, boron nitride (BN) or silica, particularly fused silica, is preferable as the inorganic filler. From the viewpoint of low dielectric properties, since the dielectric constant becomes particularly high when a large amount is added, it is preferable to use less than 500 parts by mass, more preferably less than 400 parts by mass, per 100 parts by mass of the copolymer and the polar monomer. Furthermore, in order to improve and enhance the low dielectric properties (low dielectric constant, low dielectric loss tangent), a hollow filler or a filler having a shape with many voids may be added.

[0061] When silica is used as a filler, it is preferable to use spherical silica powder, and more preferably to use surface-treated silica. Hereinafter, silica may be referred to as spherical silica powder. The volume ratio of the total of the copolymer and the polar monomer to the spherical silica powder may be in the range of 95-50:5-50, more preferably in the range of 90-70:10-30, and even more preferably in the range of 85-75:15-25.

[0062] Surface-treated silica refers to raw silica whose dielectric tangent has been reduced by surface treatment. Examples of such surface treatments include heat treatment and various coupling agent treatments including silane coupling agents. Preferably, the methods described in International Publication No. 2020 / 195205 and pending Japanese Patent Application No. 2020-077291 by the present applicant can be used as such surface treatments. In a preferred embodiment, spherical silica powder may be used as silica, and the surface treatment to which the spherical silica powder is subjected may be a heat treatment of the raw spherical silica powder at a temperature of 500 to 1100 ° C, preferably at a temperature of 500 to 1000 ° C, for a predetermined time in which the heating temperature (° C) × heating time (h) is 1000 to 26400 (° C·h), preferably 1800 to 17600 (° C·h). The treatment is preferably performed while fluidizing the raw silica powder under an inert atmosphere (such as nitrogen or argon). The temperature and time of the treatment are preferably selected so that the resulting silica satisfies at least one of the following conditions (a) and (b). (a) When the temperature is raised to 1000°C at a rate of 25 to 30°C / min, the number of water molecules desorbed at 500°C to 1000°C is 0.01 mmol / g or less. (b) Specific surface area is 1 to 30 m 2 / g, preferably 3 to 10m 2 / g. If the above conditions are satisfied, mixing with the resin component becomes easy, and the effect of reducing the dielectric tangent can be obtained.

[0063] When a spherical silica powder is used as the silica, the average particle size (d50) of the spherical silica powder is preferably 0.01 to 100 μm, more preferably 0.1 to 10 μm, and most preferably 0.3 to 1 μm. d50 is the value at 50% cumulative volume.

[0064] The silica immediately after the surface treatment may be allowed to cool naturally in the furnace, and after cooling to 200° C. or less, may be dried in a vacuum dryer, and then collected in a moisture-proof aluminum bag.

[0065] Any method can be used to manufacture the raw silica, and examples of such methods include a powder melting method in which the raw silica is passed through a high-temperature region above the melting point to be spheroidized to obtain spherical silica powder. For the silica before surface treatment, the wave number of the silica measured by the diffuse reflectance FT-IR method is 3735 cm -1 ~3755cm -1 The peak intensity is A, and the wave number is 3660 cm -1 ~3680cm -1 When the peak intensity is B, it is preferable that B / A is 3.0 or less.

[0066] The density of silica is 1.8 to 2.4 g / cm 3 Within this range, the silica particles have an appropriate amount of voids, and the silica crystal structure is appropriate, so that the thermal expansion coefficient can be appropriately suppressed.

[0067] When using spherical silica powder as silica, the average circularity of the spherical silica powder is preferably 0.85 or more, more preferably 0.90 or more. If the average circularity is 0.85 or more, when mixed with a resin component, the viscosity does not increase too much and the flowability is not easily reduced, so that the processability and filling property are improved. In addition, it is also possible to use a combination of spherical silica powder and other silica (preferably fused silica) as silica.

[0068] <Other fillers> In addition, if necessary, known inorganic or organic fillers other than the above surface-treated silica may be further added. These fillers are added for the purpose of controlling the thermal expansion coefficient, controlling the thermal conductivity, and reducing the cost, and the amount used is arbitrary depending on the purpose. The composition of the present invention can contain a large amount of inorganic fillers, and the amount that can be added can reach 2000 parts by mass per 100 parts by mass of copolymer. In particular, when adding inorganic fillers, it is preferable to use known surface modifiers, such as silane coupling agents. In particular, when the objective of the present invention is to obtain a composition excellent in low dielectric constant and low dielectric loss, which is one of the objects of the present invention, boron nitride (BN) is preferred as the inorganic filler. From the viewpoint of low dielectric properties, since the dielectric constant becomes particularly high when a large amount is added, it is preferable to use less than 500 parts by mass, more preferably less than 400 parts by mass of fillers per 100 parts by mass of copolymer. Furthermore, in order to improve and enhance low dielectric properties (low dielectric constant, low dielectric loss tangent), hollow fillers or fillers with many voids may be added.

[0069] Instead of inorganic fillers, organic fillers such as high molecular weight polyethylene or ultra-high molecular weight polyethylene can be used. From the viewpoint of heat resistance, it is preferable that the organic fillers themselves are crosslinked, and they are preferably blended in the form of fine particles or powder. These organic fillers can also suppress increases in dielectric constant and dielectric loss tangent.

[0070] On the other hand, by mixing and dispersing a high dielectric constant insulating filler having a dielectric constant of preferably 3 to 10,000, more preferably 5 to 10,000 at 1 GHz in the composition of the present invention, it is possible to prepare an insulating cured product having a high dielectric constant insulating layer having a dielectric constant of 20 or less while suppressing an increase in dielectric loss tangent (dielectric loss). By increasing the dielectric constant of a film made of an insulating cured product, it is possible to miniaturize circuits and increase the capacity of capacitors, which can contribute to miniaturization of high frequency electrical components. High dielectric constant layers and low dielectric loss tangent insulating layers are suitable for applications such as capacitors, inductors for resonant circuits, filters, and antennas. Examples of the high dielectric constant insulating filler used in the present invention include inorganic fillers or metal particles that have been subjected to insulation treatment. Specific examples are known high dielectric constant inorganic fillers such as barium titanate and strontium titanate, and other examples are specifically described in, for example, JP-A-2004-087639.

[0071] <Other additives> The composition may further contain one or more selected from a flame retardant and a surface modifier. The composition of the present invention can become a matrix of a cured product, and when cured, has excellent filling properties for other materials. Therefore, the composition contains one or more selected from these fillers, flame retardants, and surface modifiers, and the cured product tends to exhibit impact resistance and toughness even after curing.

[0072] <Flame retardants> A known flame retardant can be used in the composition of the present invention. From the viewpoint of maintaining a low dielectric constant and a low dielectric loss tangent, preferred flame retardants are known organic phosphorus-based flame retardants such as phosphoric acid esters or condensates thereof, known bromine-based flame retardants, and red phosphorus. In particular, among phosphoric acid esters, compounds having multiple xylenyl groups in the molecule are preferred from the viewpoint of flame retardancy and low dielectric loss tangent.

[0073] In addition to the flame retardant, antimony compounds such as antimony trioxide, antimony tetraoxide, antimony pentoxide, and sodium antimonate, or nitrogen-containing compounds such as melamine, triallyl-1,3,5-triazine-2,3,4-(1H,3H,5H)-trione, and 2,4,6-triaryloxy-1,3,5-triazine may be added as a flame retardant assistant. The total amount of these flame retardants and flame retardant assistants is usually preferably 1 to 100 parts by mass per 100 parts by mass of the composition. In addition, 30 to 200 parts by mass of the polyphenylene ether (PPE) resin having a low dielectric constant and excellent flame retardancy may be used per 100 parts by mass of the flame retardant.

[0074] <Surface modifier> The composition of the present invention may contain various surface modifiers for the purpose of improving adhesion to fillers, copper plates, and wiring. The amount of the surface modifier used is preferably 0.01 to 10 parts by mass, more preferably 0.1 to 5 parts by mass, per 100 parts by mass of the composition of the present invention other than the surface modifier. Examples of the surface modifier include various silane coupling agents and titanate coupling agents. The various silane coupling agents and titanate coupling agents may be used singly or in combination.

[0075] In the present invention, the flow temperature of the curable resin or composition can be adjusted according to the purpose and molding method by changing the blending ratio of the copolymer, monomer, additive resin, and if necessary, solvent of the composition within the above range, or further by changing the blending ratio of the flame retardant, filler, and surface modifier. Specifically, the composition of the present invention can be in the form of a product such as a "thermoplastic composition," a "semi-cured state (such as a B-stage sheet)," or a "varnish."

[0076] The composition of the present invention can be obtained by mixing, dissolving or melting the copolymer and one or more other components as described above, and any known method can be used for mixing, dissolving or melting.

[0077] <Thermoplastic composition and molded article> The composition of the present invention can exhibit the properties of a thermoplastic resin when a copolymer having a molecular weight in a certain range or more is used and a specific additive resin is included. Therefore, it can be molded into a shape such as a sheet, tube, strip, pellet, etc. in a substantially uncured state by a known molding method for a thermoplastic resin under conditions that do not cause crosslinking. The molded product may then be crosslinked (cured).

[0078] In addition, preferred embodiments of the present composition are as follows. When the additive resin, excluding the resin that is liquid at room temperature, contains a certain proportion or more of one or more resins selected from the hydrocarbon-based elastomer, polyphenylene ether, olefin-aromatic vinyl compound-aromatic polyene copolymer oligomer, or aromatic polyene-based resin, the composition can be easily molded as a thermoplastic resin in an uncured state. Specifically, the hydrocarbon-based elastomer (excluding the liquid resin) and / or polyphenylene ether can be added in a range of 30 to 200 parts by mass per 100 parts by mass of the copolymer. When the additive resin is liquid at room temperature, the composition can be added in a range of preferably 1 to 30 parts by mass, particularly preferably 1 to 20 parts by mass, per 100 parts by mass of the copolymer. The amount of the polar monomer used in the present thermoplastic composition may be preferably 15 parts by mass or less per 100 parts by mass of the total of the copolymer and the polar monomer. The number average molecular weight of the copolymer used is 500 to 100,000, preferably 20,000 to 100,000, more preferably 30,000 to 100,000. The thermoplastic composition described above may be molded into various shapes such as a sheet in advance by utilizing its thermoplasticity at a temperature equal to or lower than the action temperature of the curing agent, and may be combined with a semiconductor element, wiring, or a substrate and laminate as necessary, and then heated to cure and bond.

[0079] The composition of the present invention may be provided as a sheet obtained by molding the composition, which is heated and melted at a temperature below the action temperature or decomposition temperature of the curing agent, by a known method. Molding into a sheet may be performed by extrusion molding using a T-die, a two-roll machine, or extrusion lamination onto a substrate film. In this case, the composition, the mass ratio of copolymer / monomer, or the solvent, additive resin, and flame retardant are selected and adjusted so that the composition melts at the action temperature or decomposition temperature of the curing agent or below and becomes solid at around room temperature. In this case, the sheet is substantially in an uncured state. After that, the sheet is processed through various processing and assembly steps, and finally treated at a temperature and time above the action temperature or decomposition temperature of the curing agent to completely cure. Such a method is a general technique used for ethylene-vinyl acetate resin-based crosslinking sealant sheets for solar cells (photovoltaic power generation devices).

[0080] <Molded body in semi-cured state (B-stage sheet, etc.)> The composition of the present invention can also be made into a molded product, such as a sheet or tube, in a partially crosslinked state, for example, a state in which a part of the curing agent contained therein is reacted and semi-cured (so-called B-stage state). For example, by adopting a plurality of curing agents and / or curing conditions with different curing temperatures, it is possible to semi-cur it and control the melt viscosity and fluidity to make it into a B-stage state. That is, it is also possible to mold the present curable resin or composition into an easy-to-handle B-stage sheet by the first-stage curing (partial curing), laminate it on an electronic device or substrate, and then perform the second-stage curing (complete curing) to make it into a final shape. In this case, the composition of the composition, i.e., the mass ratio of copolymer / monomer is selected, and if necessary, a solvent, an additive resin, and a flame retardant are added, and further the composition containing a curing agent such as a peroxide is partially cured, adjusted to a sheet shape (B-stage state), and after molding and assembling the device, it can be heated under pressure to completely cure. As a method for partially curing the composition, a known method can be adopted. For example, there is a method in which peroxides with different decomposition temperatures are used in combination, and treated for a predetermined period of time at a temperature at which only one of the peroxides is substantially active to obtain a semi-cured sheet, and finally treated for a sufficient period of time at a temperature at which all of the curing agents are active to completely cure the sheet.

[0081] Furthermore, the molded article may be a sheet. The sheet may be uncured (semi-cured) to the extent that it can maintain a sheet shape, or may be completely cured. The degree of curing of the composition can be quantitatively measured by a known dynamic viscoelasticity measurement method (DMA, Dynamic Mechanical Analysis).

[0082] <Varnish-like composition and molded body thereof> The composition of the present invention can be made into a viscous liquid varnish depending on its composition and blending ratio. For example, a sufficient amount of solvent and / or an appropriate amount of liquid monomer can be used to make the composition into a varnish. In particular, when the composition is used as a varnish, it is preferable to add an appropriate solvent to the composition of the present invention. The solvent is used to adjust the viscosity and fluidity of the composition as a varnish. As the solvent, a solvent having a boiling point of a certain level or higher is preferable because a high boiling point under atmospheric pressure, that is, a low volatility, leads to a uniform thickness of the applied film. A preferred boiling point is about 100 or more, preferably 110°C or more and 300°C or less, under atmospheric pressure. Examples of solvents suitable for such varnish include toluene, xylene, mesitylene, ethylbenzene, limonene, ethylene glycol methyl ether acetate, ethylene glycol monoethyl ether acetate, and ethylene glycol monobutyl ether. The amount of the solvent used is preferably in the range of 10 to 2000 parts by mass per 100 parts by mass of the composition of the present invention. The varnish-like composition of the present invention can also be made by using a polymerization liquid containing the copolymer of the present invention obtained by polymerization. For example, the polymerization liquid may be concentrated or treated to remove residual monomers, and if necessary, solvents, other resin components, various additives, etc. may be added to adjust the component concentrations and solution viscosity, etc., to produce the polymer.

[0083] The varnish can be applied to or impregnated into a substrate, and the solvent or the like can be removed by drying or the like to obtain an uncured or semi-cured molded article. Generally, this molded article has the form of a sheet, film, or tape. The obtained uncured or semi-cured molded article is then cured.

[0084] <Curing> The composition can be cured by a known method, taking into consideration the curing conditions (temperature, time, pressure) of the curing agent contained therein. When the curing agent used is a peroxide, the curing conditions can be determined by taking into consideration the half-life temperature and the like disclosed for each peroxide.

[0085] <Cured product of the composition> The dielectric constant and dielectric loss tangent of the cured product obtained from the composition of the present invention are measured by a known resonator method (such as a cavity resonator perturbation method or a balanced disk resonator method). In this specification, the resonator method is performed in a measurement frequency range of 27 GHz to 42 GHz. The dielectric constant of the cured product may be preferably 2.7 to 2.0, particularly preferably 2.5 to 2.0. The dielectric loss tangent of the cured product is 1.5×10 -3 or less, preferably 0.3×10 -3 More than 1.5 x 10 -3 The volume resistivity of the cured product is preferably 1×10 15Ω·cm or more. These values ​​are preferable values ​​for a high-frequency electrical insulating material of, for example, 3 GHz or more. The copolymer used in the composition of the present invention is relatively soft and has a high tensile elongation, so that the cured product obtained from the composition using the copolymer has a relatively high impact resistance while exhibiting sufficient mechanical properties, and can have the characteristic of being able to follow the thermal expansion of the substrate. That is, the tensile modulus of the cured product of the present invention measured at room temperature (23°C) is preferably less than 30 GPa and 0.5 GPa or more. In particular, when a relatively large amount of filler is blended, the tensile modulus may be 3 GPa or more and 20 GPa or less. In addition, the tensile strength at break is preferably less than 200 MPa, 3 MPa or more, and the tensile elongation at break is preferably 0.1% or more and less than 300%, more preferably 1% or more and less than 50%. In particular, when a relatively large amount of filler is blended, the tensile elongation at break may be less than 30%. Those skilled in the art can determine the blending of the composition having the above physical property parameters and prepare a cured product by referring to the information described in this specification and publicly known documents. The cured product obtained from the composition of the present invention can exhibit practically sufficient heat resistance and mechanical properties at high temperatures even under conditions in which the amount of polar monomer in the composition and the amount of aromatic polyene as a component of other monomers are suppressed to a certain ratio or less. As described above, suppressing the amount of monomer or aromatic polyene as a component of monomer to a certain ratio or less is important in order to maintain moldability as a thermoplastic resin even in an uncured state.

[0086] The storage modulus of the cured product at 250° C. may be in the range of 10 MPa to 10 GPa, and preferably 15 MPa to 1 GPa. By having such a storage modulus, the cured product has an effect of having a hardness suitable for use as a base material or substrate.

[0087] In a preferred embodiment, the cured product of the composition has a small ratio of the storage modulus at 25°C divided by the storage modulus at 250°C (i.e., does not lose viscoelasticity excessively even at high temperatures). This property indicates that the crosslink density of the composition is unlikely to decrease even at high temperatures. The ratio is preferably 20 or less, more preferably 2 or more, more preferably 10 or less, and even more preferably 2 or more and 10 or less. The storage modulus of the cured product of the composition can be measured using a known dynamic viscoelasticity measuring device.

[0088] <General uses of the composition> The composition of the present invention can be used as a base material or substrate, such as a single-layer or multi-layer printed circuit board, a flexible printed circuit board, a so-called single-layer or multi-layer CCL (copper clad laminate), or a single-layer or multi-layer FCCL (flexible copper clad laminate) substrate, etc. It can also be used as various insulating materials for wiring, preferably for wiring of high-frequency signals, such as coverlays, solder resists, build-up materials, interlayer insulating agents, bonding sheets, interlayer adhesives, and bump sheets for flip-chip bonders.

[0089] <Use of the composition as an uncured or partially cured sheet> The uncured or partially cured sheet of the composition of the present invention can be suitably used as a high-frequency electrical insulating material. For example, it can be suitably used as a build-up film, a bonding sheet, a coverlay sheet, a bump sheet for a flip chip bonder, or an insulating layer or adhesive layer for a substrate. The composition of the present invention is used as a replacement for conventionally used sheets of epoxy resin or silicone resin. The composition of the present invention can form a cured insulating layer or a cured matrix phase with a low dielectric constant and low dielectric loss by performing a curing treatment. The thickness of the sheet is generally 1 to 300 μm. The sheet may contain woven or nonwoven fabrics such as glass cloth or ceramic fibers. The sheet may be impregnated or may be multi-layered with these. In addition, as an antenna cable for a mobile phone or the like, a flexible and bendable wiring partially or entirely insulated with the sheet of the present invention can be used instead of a conventional coaxial cable. For example, a wiring is covered with the sheet of the present invention or the B-stage sheet (coverlay sheet) using LCP (liquid crystal polymer), PPE sheet, fluorine-based resin, or polyimide resin as a substrate, cured, and bonded to the substrate, and can be used as an insulating material.

[0090] A multilayer wiring board in which the cured product obtained by using the composition of the present invention is an insulating layer can be a wiring board with low dielectric loss and excellent high frequency characteristics. In this case, in addition to low dielectric loss, the advantages are heat resistance that can withstand soldering, and a certain degree of softness, elongation, and impact resistance that can withstand stress due to heat cycles or thermal expansion differences. For example, a wiring board can be produced by laminating and pressing a core material such as a cloth made of glass or quartz, a nonwoven fabric, a film material, a ceramic substrate, a glass substrate, a general-purpose resin plate such as epoxy, a general-purpose laminate, and a conductor foil with an insulating layer made of the present cured product. Also, a slurry or solution containing the present composition may be applied to a core material (for example, an inner layer), dried, and cured to form an insulating layer. The thickness of the insulating layer is generally 1 to 300 μm. Such a multilayer wiring board can also be used by multilayering and integrating.

[0091] The cured product obtained by curing the varnish-like composition of the present invention, in particular, can be suitably used as an electrical insulating material as described above, and in particular can be used as a potting material, surface coating agent, coverlay, solder resist, build-up material, underfill material, filling insulating agent, interlayer insulating agent, or interlayer adhesive, or as a cured product for printed circuit boards, flexible printed circuit boards, CCL (copper clad laminate, copper clad laminate) boards, FCCL (flexible copper clad laminate) boards, or as a build-up film, bonding sheet, coverlay sheet, or cured product for a bump sheet for a flip chip bonder, as an electrical insulating material, in particular an electrical insulating material for high frequency.

[0092] In another aspect, the present invention provides a composition comprising an olefin-aromatic vinyl compound-aromatic polyene copolymer, the composition having a storage modulus of 10 MPa or more and 10 GPa or less at 250° C., a dielectric constant of 3.5 or more and 2.0 or more at 23° C., 10 GHz or 25 GHz to 40 GHz, and a dielectric loss tangent of 1.2×10 -3 It is possible to provide an electrically insulating material which is:

[0093] The uncured or semi-cured thermoplastic composition of the present invention can be bonded to a metal foil, particularly a copper foil for wiring, by heat and pressure treatment to obtain a laminate, without applying an adhesive or performing an adhesive treatment. Here, the metal foil is a concept including metal wiring. In particular, when a copolymer having an aromatic vinyl compound content of 10% by mass or more is used in the olefin-aromatic vinyl compound-aromatic polyene copolymer, and / or the olefin is ethylene alone, or the mass ratio of the olefin monomer component other than ethylene to the ethylene monomer component contained in the olefin is 1 / 7 or less, a peel strength of 1 N / mm or more can be obtained as measured according to Japanese Industrial Standards (JIS) C6481:1996. Furthermore, it is more preferable to provide a peel strength of 1.3 N / mm or more. More preferably, in the above copolymer, the olefin is ethylene alone, or the olefin monomer component other than ethylene is 1 / 10 or less to the ethylene monomer component contained in the olefin, and most preferably, the content of α-olefin monomer units other than ethylene contained in the copolymer is 4% by mass or less, or the olefin is ethylene alone, the peel strength can be further improved. Generally, it is known that the dielectric properties of laminates such as copper-clad laminated sheets are deteriorated by performing an adhesive treatment, and it is preferable that the composition has a peel strength of 1 N / mm or more when measured according to Japanese Industrial Standards (JIS) C6481:1996 without performing such treatment. Thus, the uncured or semi-cured thermoplastic composition of the present invention can be bonded to metal foils such as copper foils for wiring by a curing treatment such as a heat and pressure treatment, without performing any adhesive coating or adhesive treatment. However, in the present invention, with regard to the adhesion to metal foils and other members, other adhesiveness-imparting measures (adhesive coating, adhesive treatment, etc.) including the addition of the above-mentioned "surface modifier" are not hindered in any way. It is also possible to obtain a cured product by curing the above-mentioned laminate.

[0094] The uncured or semi-cured composition of the present invention can also be cured together with an LCP (liquid crystal polymer) layer under relatively mild curing conditions to provide high adhesive strength. The LCP layer may specifically be an LCP sheet or film. Therefore, for example, it can be a laminate containing an LCP sheet, a metal foil, preferably a copper foil, and the composition of the present invention. The number of layers of the laminate and the order of lamination are optional. As an example of the present invention, the composition of the present invention is useful as an adhesive layer between a metal foil (copper foil) and an LCP sheet. The composition of the present invention can exhibit high adhesiveness to both the metal foil and the LCP sheet. Conventionally, the adhesion between an LCP sheet and a copper foil required heating to the melting point of the LCP (approximately 280°C to 330°C) or a temperature close to the melting point and pressure bonding. However, by using the composition of the present invention as an adhesive layer, it is possible to bond the LCP and the metal foil at a lower temperature, substantially by pressure bonding at a temperature close to the curing temperature of the composition of the present invention. In this case, the low dielectric constant and low dielectric loss tangent value of the cured product of the composition of the present invention impart usefulness to the laminate, particularly as wiring for high-frequency signal transmission. Another example of the laminate of the present invention is a structure in which a metal wiring, preferably a copper wiring, arranged on an LCP layer is covered with a cured layer of the composition of the present invention from the side opposite the LCP layer, as a so-called coverlay on the LCP substrate wiring.

[0095] Here, LCP (liquid crystal polymer) refers to a thermoplastic polymer that has a liquid crystal state or optically birefringent properties when melted. Examples of LCP include lyotropic liquid crystal polymers that exhibit liquid crystallinity in a solution state and thermotropic liquid crystal polymers that exhibit liquid crystallinity when melted. Liquid crystal polymers are classified into I type, II type, and III type depending on the heat distortion temperature, and any type may be used. Examples of liquid crystal polymers include thermoplastic aromatic liquid crystal polyesters, and thermoplastic aromatic liquid crystal polyester amides in which amide bonds are introduced therein. LCP may be a polymer in which an isocyanate-derived bond such as an imide bond, a carbonate bond, a carbodiimide bond, or an isocyanurate bond is further introduced into an aromatic polyester or an aromatic polyester amide. The melting point of the LCP is preferably 220 to 400°C, more preferably 260 to 380°C, as determined by the DSC method. When the melting point is within the above range, a film or sheet having excellent extrusion moldability and excellent heat resistance can be obtained. Such LCPs can be obtained, for example, from Ueno Pharmaceutical Co., Ltd., Sumitomo Chemical Co., Ltd., and Polyplastics Co., Ltd. Here, the LCP sheet refers to a known LCP sheet, and the thickness thereof is arbitrary. The LCP sheet can be obtained by a known method such as a T-die extrusion method, an inflation method, or an endless belt (double belt press) method.

[0096] The composition of the present invention, for example, the curable composition, has the properties of a thermoplastic resin. Furthermore, the cured product obtained by curing the curable composition has excellent low dielectric properties, a high storage modulus at high temperatures, and a small coefficient of thermal expansion (coefficient of thermal expansion, CTE), and is therefore particularly suitable for use in various electronic substrates. EXAMPLES

[0097] The present invention will be described below with reference to examples, but the present invention should not be construed as being limited to the following examples.

[0098] The copolymers obtained in the Synthesis Examples and Comparative Synthesis Examples were analyzed by the following methods.

[0099] The content of vinyl group units derived from ethylene, hexene, styrene, and divinylbenzene in the copolymer is determined by: 1 The measurements were performed using H-NMR from the peak area intensities assigned to each compound. The sample was dissolved in deuterated 1,1,2,2-tetrachloroethane, and the measurements were performed at 80 to 130°C.

[0100] <Number average molecular weight> The molecular weight was determined as a number average molecular weight (Mn) converted to standard polystyrene using GPC (gel permeation chromatography) under the following conditions. (Number average molecular weight of 1000 or more) Column: Two TSKgel MultiporeHxl-M φ7.8×300 mm columns (Tosoh Corporation) were connected in series. Column temperature: 40℃ Solvent: THF Flow rate: 1.0ml / min. Detector: RI detector (differential refractive index detector)

[0101] <Glass transition temperature (DSC measurement)> DSC measurements were performed under nitrogen flow using a Seiko Electronics DSC6200. That is, 10 mg of resin was used, 10 mg of α-alumina was used as a reference, and an aluminum pan was used. Under a nitrogen atmosphere, the temperature was raised from room temperature to 240°C at a heating rate of 10°C / min, and then cooled to -120°C at 20°C / min. DSC measurements were then performed while heating to 240°C at a heating rate of 10°C / min to determine the glass transition temperature. The glass transition temperature referred to here is the extrapolated glass transition onset temperature of JIS K7121:2012, and is the temperature at the intersection of a straight line extending the low-temperature side baseline to the high-temperature side and a tangent drawn at the point where the gradient of the curve of the stepwise change part of the glass transition is maximum.

[0102] <Average particle diameter (d50)> The volume particle size distribution curve was obtained from a laser diffraction particle size analyzer (Beckman Coulter Model LS-230).

[0103] <Specific surface area> A sample of 1 g was filled into the measurement cell, and the specific surface area was measured using a fully automatic specific surface area measurement device (BET single-point method), Macsorb HM model-1201 manufactured by Mountech. The degassing conditions before measurement were 200 °C for 10 minutes. Nitrogen was used as the adsorption gas.

[0104] <Dielectric Constant and Dielectric Loss (Dielectric Tangent)> The dielectric constant and dielectric tangent were evaluated in the same manner using an equilibrium disk resonator (manufactured by Keysight Technologies). For the method of evaluating dielectric properties with an equilibrium disk resonator, two samples cut out from the sheet (diameter 3 cm, thickness 0.2 - 0.6 mm) were prepared, a copper foil was sandwiched between them, and they were set in the resonator. The resonance frequency (f0) of the peak that appeared at 27 - 42 GHz and the unloaded Q value (Qu) were measured. The dielectric constant was calculated from f0, and the dielectric tangent (tanδc) was calculated from Qu using the analysis software attached to the resonator (Balanced type circular disk resonator (method) calculator, equilibrium disk resonator method analysis software). The measurement temperature was 23 °C, and the humidity was 50%RH.

[0105] <CTE (Coefficient of Thermal Expansion)> CTE was measured with reference to the 16th item, material standard for printed wiring boards, of the JPCA standard "Standard for Electronic Circuit Boards, 3rd Edition" using a thermomechanical analyzer (TMA: Thermomechanical Analyzer, manufactured by BRUKER AXS, currently manufactured by Netzsch Japan) under the conditions of a width of 3 - 5 mm, a thickness of 0.5 - 0.6 mm, a distance between chucks of 15 - 20 mm, a tensile load of 10 g, and a heating rate of 10 °C / min, and the average value between 25 °C and 150 °C was obtained. In the composition according to the present invention, the CTE is required to be 130 ppm / K or less.

[0106] <Measurement of Storage Modulus> A dynamic viscoelasticity measuring device (TA Instruments, formerly Rheometrics RSA-G2) was used to measure at a frequency of 1 Hz and at a temperature range of -60°C to +300°C. Measurement samples (3mm x 40mm) were cut out from films with a thickness of approximately 0.1 to 0.3mm and measured to determine the storage modulus. The main measurement parameters involved in the measurement are as follows: Measurement frequency 1Hz Heating rate: 3℃ / min Sample measurement length: 10 mm Distortion 0.1%

[0107] <Olefin-aromatic vinyl compound-aromatic polyene copolymer> Copolymer P-1 was obtained by appropriately changing the monomer amount, ratio, polymerization pressure, and polymerization temperature with reference to the manufacturing methods described in International Publication No. 00 / 37517, JP 2009-161743 A, and JP 2010-280771 A. The total of the olefin monomer unit, the aromatic vinyl compound monomer unit, and the aromatic polyene monomer unit was set to 100% by mass. Table 1 shows the composition and number average molecular weight of the copolymer.

[0108] The main raw materials are as follows: The divinylbenzene used was divinylbenzene (mixture of meta and para, divinylbenzene purity 81%) manufactured by Nippon Steel Chemical & Material Co., Ltd. The curing agent used was Perhexyne 25B (2,5-dimethyl-2,5-bis(t-butylperoxy)hexyne-3) manufactured by NOF Corporation. As polar monomers, BMI-5100 (3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide manufactured by Daiwa Chemical Industry Co., Ltd.) and TAIC (triallyl isocyanurate manufactured by Mitsubishi Chemical Corporation) were used. In addition, OPE-2St (bifunctional polyphenylene ether oligomer manufactured by Mitsubishi Gas Chemical Co., Ltd.) was used.

[0109] Silica was Denka SFP-130MC (d50 = 0.6 μm, specific surface area 6.2 m 2A dielectric tangent reduction treatment product ("treated SFP-130MC") having a dielectric tangent of 1000 nm / g was used. The SFP-130MC dielectric tangent reduction treatment product is a surface-treated spherical silica powder produced by the method described in International Publication No. 2020 / 195205 and pending Japanese Patent Application No. 2020-077291 by the present applicant. Specifically, a raw material spherical silica powder (SFP-130MC manufactured by Denka Co., Ltd.) was heat-treated at a temperature of 500 to 1000 ° C for a predetermined time in which the heating temperature (° C.) × heating time (h) was 1800 to 17600 (° C. h). The treatment was performed by fluidizing the raw material silica powder under an inert atmosphere.

[0110] [Table 1]

[0111] [Table 2]

[0112] Example 1 Using a vessel equipped with a heating and cooling jacket and stirring blades, 90 parts by mass of P-1 (ethylene-styrene-divinylbenzene copolymer) obtained in the synthesis example and 10 parts by mass of BMI-5100 (manufactured by Daiwa Chemical Industry Co., Ltd., 3,3'-dimethyl-5,5'-diethyl-4,4'-diphenylmethane bismaleimide) as a polar monomer were stirred and dissolved at about 40°C. Furthermore, 1 part by mass of a curing agent Perhexine 25B (manufactured by NOF Corporation) was added to 100 parts by mass of the above mixture, dissolved, and stirred and mixed to obtain a varnish-like composition.

[0113] The obtained composition was further stirred with a foam mixer (Thinky Corporation), then poured into a silicone rubber mold (frame thickness 0.5 mm or 1.0 mm) placed on a pre-heated cellophane-covered glass plate, and the pressure was reduced from atmospheric pressure to 10 hPa at 60°C over 22 hours, and then dried for another 3 hours to obtain a dried sheet. The composition was then sandwiched between glass plates and adhered with clips, and heated under a nitrogen atmosphere at 120°C for 30 minutes, 150°C for 30 minutes, and then 200°C for 2 hours. After completion of the heating, the glass plate and mold were removed to obtain a sheet-like cured product.

[0114] Example 2 The same procedure as in Example 1 was repeated, except that 20 vol % of silica filler (SFP-130MC treated to reduce dielectric tangent) was added to 80 vol % (volume %) of the composition of Example 1 obtained as a sheet-like cured product, and the mixture was stirred to form a slurry-like varnish.

[0115] Example 3 The same procedure was carried out as in Example 1, except that 85 parts by mass of P-1 and 15 parts by mass of BMI-5100 were mixed.

[0116] Comparative Examples 1 to 5 Sheet-shaped cured products according to each Comparative Example were obtained in the same manner as in Example 1, except that the component compositions shown in Table 2 were used.

[0117] The cured products of the composition sheets obtained in Examples 1 to 3 had very low dielectric constants and dielectric tangents measured at the above measurement frequencies, and also showed CTEs below 130 ppm / K. Furthermore, in all of the Examples, the value obtained by dividing the storage modulus at 25°C by the storage modulus at 250°C was low, demonstrating that the crosslink density was maintained even at high temperatures.

[0118] On the other hand, the cured sheets obtained in Comparative Examples 1 to 4 all had too high CTE and were not particularly suitable for CCL applications. Comparative Example 5 had a low CTE, but the dielectric tangent was too high, similar to Comparative Example 3. Comparative Example 1 generally had too low viscosity, causing the sample to stretch and making it impossible to measure the storage modulus. Comparative Examples 2 and 3 also had too low viscosity at 250°C, causing the sample to stretch and making it impossible to measure the storage modulus.

[0119] From the above results, the cured product of the composition exhibits excellent low dielectric properties and low CTE properties, and is practically sufficient for CCL. Therefore, it is confirmed that the present invention can provide an electrical insulating material, particularly for high frequencies. The cured product can be suitably used as a thin-film electrical insulating material or an electrical insulating material for high frequencies. The cured product is useful as a printed circuit board, a flexible printed circuit board, a single-layer or multi-layer CCL (copper clad laminate) board, or a single-layer or multi-layer FCCL (flexible copper clad laminate) board. It can also be suitably used as an interlayer adhesive layer or an interlayer insulating layer for these.

Claims

1. The following conditions (1) to (4) (1) The number average molecular weight of the copolymer is 500 or more and 100,000 or less. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass or more and 70% by mass or less. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 20 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, the aromatic vinyl compound monomer units, and the aromatic polyene monomer units is 100 mass %. an olefin-aromatic vinyl compound-aromatic polyene copolymer satisfying all of the above requirements; a polar monomer which is a bismaleimide having one or more aromatic rings; A composition comprising: the dielectric constant of a cured product of the composition, as determined by a resonator method, is 2.7 or less in a measurement frequency range of 27 GHz to 42 GHz; The dielectric tangent of the cured product of the composition, as determined by a resonator method, is 1.5×10 -3 is as follows: The CTE (coefficient of linear expansion) of the composition is 130 ppm / K or less, as determined from the average value between 25°C and 150°C measured using a thermomechanical analyzer (TMA: Thermomechanical Analyzer, manufactured by BRUKER AXS, currently manufactured by Netzsch Japan) under conditions of width 3 to 5 mm, thickness 0.5 to 0.6 mm, chuck distance 15 to 20 mm, tensile load 10 g, and heating rate: 10°C / min, based on JPCA standard "Electronic Circuit Board Standard, 3rd Edition," Section 16 "Material Standard for Printed Wiring Boards." A composition comprising:

2. The composition according to claim 1 , wherein the aromatic ring of the polar monomer has one or more groups having one or more carbon atoms on the ring.

3. The polar monomer is a bismaleimide having the following structural formula:

3. The composition according to claim 2, wherein R 1 and R 1 ' are each independently a hydrogen atom or a substituent having one or more carbon atoms.

4. The composition according to any one of claims 1 to 3, wherein the amount of the polar monomer is in the range of 0.1 to 30 parts by mass per 100 parts by mass of the total of the copolymer and the polar monomer.

5. The copolymer satisfies the following conditions (1) to (4): (1) The number average molecular weight of the copolymer is 500 or more and 100,000 or less. (2) The aromatic vinyl compound monomer is an aromatic vinyl compound having 8 to 20 carbon atoms, and the content of the aromatic vinyl compound monomer unit is 0% by mass or more and 70% by mass or less. (3) The aromatic polyene is one or more selected from polyenes having 5 to 20 carbon atoms and having a plurality of vinyl groups and / or vinylene groups in the molecule, and the content of the vinyl groups and / or vinylene groups derived from the aromatic polyene units is 1.5 or more and less than 7 per number average molecular weight. (4) The olefin is one or more olefins selected from olefins having from 2 to 20 carbon atoms, and the total of the olefin monomer units, the aromatic vinyl compound monomer units, and the aromatic polyene monomer units is 100 mass %. The composition according to any one of claims 1 to 4, wherein all of the above are satisfied.

6. The composition according to any one of claims 1 to 5, wherein a value obtained by dividing a storage modulus of a cured product of the composition at 25°C by a storage modulus of a cured product of the composition at 250°C is 20 or less.

7. The composition according to any one of claims 1 to 6, further comprising a second monomer, which is at least one selected from the group consisting of an aromatic vinyl compound monomer and an aromatic polyene monomer, and / or a resin.

8. The composition according to claim 7, comprising 300 parts by mass or less of the second monomer and / or resin relative to 100 parts by mass of the copolymer.

9. The composition according to any one of claims 1 to 8, further comprising a curing agent.

10. The composition according to any one of claims 1 to 9, which is curable.

11. A molded article obtained by curing the composition according to any one of claims 1 to 10.

12. The molded article according to claim 11, which is a sheet.

13. The molded article according to claim 11 or 12, which is an electrical insulating material.

14. A laminate comprising a layer comprising the composition according to any one of claims 1 to 10 and a metal foil.

15. A cured product obtained by curing the laminate according to claim 14.

16. A single layer CCL, multilayer CCL, single layer FCCL, or multilayer FCCL substrate comprising the cured product of claim 15.

Citation Information

Patent Citations

  • Method to form droppout preventive angle for speeddchange gear fitted to automobiles

    JP1977031272A

  • Thermosetting resin composition having low dielectric constant

    JP1994192392A

  • Heat-resistant low-permitivity polymer material, and film, substrate board, electronic part and heat-resistant resin molding prepared from the same

    JP1999060645A

  • Non-porous spherical silica and method for producing the same

    JP2003165718A

  • Post curing resin composition and high frequency electrical insulating material using the same

    JP2009161743A