Adaptive strap for brassiere products and manufacturing method thereof
The adaptive bra strap with silanol-terminated polydimethylsiloxane and boric acid transitions from low to high tensile strength, addressing the support and comfort issues in sports bras, providing stable breast support during exercise.
Patent Information
- Application Number
- JP2023523614
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-09-17
- Filing Date
- 2022-09-16
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-09-16
AI Technical Summary
Existing sports bras provide insufficient support during exercise, causing discomfort and pain due to high tensile strength in static conditions and inadequate vibration resistance, while proprietary solutions are expensive and pose safety risks.
An adaptive bra strap composed of silanol-terminated polydimethylsiloxane, a polymer matrix, boric acid, and a curing agent, which transitions from low tensile strength in static conditions to high strength during oscillatory movements, providing sufficient support and comfort.
The adaptive strap offers stable support during exercise by maintaining low tensile strength for comfort and high strength during vibrations, ensuring breast stability without causing pain or delamination.
Smart Images

Figure 0007571295000002 
Figure 0007571295000003 
Figure 0007571295000004
Abstract
Description
[Technical field]
[0001] CROSS REFERENCE TO RELATED APPLICATIONS: This application claims priority to U.S. Provisional Application No. 63 / 245,206, filed September 17, 2021, the disclosure of which is incorporated by reference in its entirety herein.
[0002] The present invention relates to an adaptive strap for a brassiere product that has low tensile strength during static extension to ensure comfort when worn, but produces relatively high strength during oscillation stretching to provide sufficient breast support. [Background technology]
[0003] Modern city dwellers pay more attention to their health to improve their quality of life, and exercise has become an important daily activity. One of the physiological characteristics of women is that breasts are glandular organs that hang down from the pectoral muscles and have no bone or muscle support. Exercise and daily movements inevitably cause vibration of the breasts, and if the vibration of the breasts is repeated over time, the breasts tend to sag, affecting movement during exercise and causing pain after exercise. As a result, sports underwear that can maintain the position of the breasts during exercise / daily movements and prevent their vibration has appeared.
[0004] Some women choose to wear regular bras when exercising because of the comfort they provide in daily life. However, such bras provide insufficient support during exercise. Sports bras provide more support than regular bras and can reduce breast slippage. Most sports bras use elastic fabrics with high tensile strength. Although such bras can provide adequate support to the breasts, they can cause problems such as shoulder straps digging into or rubbing against the skin. Unique products have been developed to alleviate these problems, but these products are expensive and have limited vibration resistance. As a result, there is a need for an adaptive strap for a bra that overcomes the aforementioned shortcomings. The present invention addresses this need.
[0005] US2020 / 0345082A1 describes a movement-responsive athletic apparel made by immersing fabric in a shear-thickening fluid (STF). The STF treatment involves immersing untreated fabric in a diluted STF bath, measuring the amount of liquid adhering to the fabric, and removing the diluent from the treated fabric. However, the ratio of diluent contained in the STF can be as high as 1:1 to 10:1. In addition, the diluent can include methanol, ethanol, isopropanol, and methyl ethyl ketone, which are flammable and easily vaporized. Depending on the dosage and type of diluent, the treatment can be dangerous to carry out.
[0006] CN111134409A discloses a self-adaptive apparel containing dynamic dilatancy based on strong dynamic covalent bonds or strong dynamic supramolecular interactions, or both strong dynamic covalent bonds and strong dynamic supramolecular interactions. However, the key performance parameters of the apparel, such as specific parameters of low and high speed, and the rate of tensile stress at low and high speed tension, are not disclosed. In one preferred embodiment, the elongation of the strap is high, up to 102% at high speed tensile stress, which will still cause great pain due to breast displacement. Furthermore, the movement of the breast during exercise is an oscillatory motion, not a simple linear displacement at a single constant speed. Therefore, the modulus evaluation at a constant speed may not match the actual usage scenario. Summary of the Invention
[0007] Therefore, there is a need for a material for application in adaptive brassiere straps that provides a brassiere with low tensile strength in static elongation to ensure comfort when worn while providing relatively high strength under vibration to adequately support the breasts during exercise and / or daily activities. In the present invention, the adaptive straps are made of a silanol-terminated polydimethylsiloxane, a polymer matrix, a filler, boric acid, and a curing agent. It is formed by reacting Elastic fabric and Adaptive MaterialsThe bra strap of the present invention exhibits adaptive capabilities to provide adequate support during different activities.
[0008] In one aspect, the invention provides an adaptive strap for a brassiere, comprising at least one adaptive material layer having a first strength modulus x during static loading and a second strength modulus of at least 2x during dynamic loading of at least about 3 Hz vibration, each of said adaptive material layers sandwiched between two elastic fabric layers such that said adaptive strap is stretchable to 100% of its initial length during lower wearer activity, but cannot stretch more than 50% during vigorous wearer activity.
[0009] In a further aspect, the adaptive strap has a thickness of less than 2 mm.
[0010] In a further aspect, the adaptive strap has a load strength of at least 7N at a static elongation of 10%.
[0011] In a further aspect, the adaptive strap has a load strength of at least 15N at a static elongation of 10% followed by a vibratory elongation at 3.0 Hz.
[0012] In a further aspect, the invention includes a method of preparing an adaptive strap for a brassiere. One or more silanol terminated polydimethylsiloxanes, a polymer matrix material, and boric acid are mixed at a reaction temperature for a reaction time to obtain a composite. The composite is mixed with a curing agent at room temperature to form an uncured adaptive material. The uncured adaptive material is filled into a temporary shell, inserted into one or more hollow structures, and worked into the hollow structures until it substantially fills the hollow spaces within the hollow structures. The temporary shell is removed from the hollow fabric structures and cured to form the adaptive strap.
[0013] The silanol terminated polydimethylsiloxane, polymer matrix, boric acid, and curing agent may be in the weight range of 5:100:0.02:0.5 to 100:100:1:3.
[0014] The silanol-terminated polydimethylsiloxane may be selected from one or more of silanol-terminated polydimethylsiloxane, silanol-terminated diphenylsiloxane-dimethylsiloxane copolymer, vinylmethylsiloxane-dimethylsiloxane copolymer, and may have a molar ratio of 0-18% phenyl and a molar ratio of 0-15% vinyl.
[0015] The silanol-terminated polydimethylsiloxane may have an average molecular weight of 650 to 139,000 g / mol.
[0016] The boric acid may be provided in an ethanol solution at a weight ratio of 1% to 10% by weight.
[0017] The curing agent may be one or more of a peroxide, a crosslinking agent, or a catalyst.
[0018] The composite may further include one or more fillers.
[0019] The filler may be silica dioxide, titanium dioxide, glyceryl oleate, or any combination thereof.
[0020] The polymer matrix may be silicone rubber, natural rubber, synthetic rubber, or a combination thereof, and may have a hardness of about 40 Shore A to 80 Shore A.
[0021] The curing agent may be a peroxide, which may be one or more of 2,4-dichlorobenzoyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, or dibenzoyl peroxide.
[0022] The curing agent may be a crosslinking agent, and the crosslinking agent may be selected from one or more silicon hydride compounds having at least two SiH groups.
[0023] The curing agent may be a catalyst, which may be one or more of palladium, rhodium, or platinum.
[0024] The reaction temperature for obtaining the complex may be about 80°C to 200°C.
[0025] The reaction time for obtaining the complex may be about 0.5 to 8 hours.
[0026] The curing temperature may be about room temperature or from 25°C to 200°C. The curing time may be from about 0.5 to 24 hours.
[0027] The adaptive strap for the brassiere may have a tensile strength of greater than 4 MPa after 960 circles and a static tensile strength of 1 MPa or greater under 10% strain. [Brief description of the drawings]
[0028] [Figure 1A]FIG. 1A shows a schematic structure of a material for an adaptive strap of a brassiere product. [Figure 1B] FIG. 1B shows a possible location of the material / adaptive straps of FIG. 1A in a sports bra. [Diagram 2] FIG. 2 shows a process flow diagram of the adaptive strap for brassiere of the present invention. [Diagram 3] FIG. 3 illustrates a fabrication process for producing an adaptive strap according to one embodiment of the present invention. [Figure 4] FIG. 4 is a tensile strain curve of the strap of Example 1. [Diagram 5] FIG. 5 shows the dynamic mechanical properties of the straps measured by DMA in Example 1. [Figure 6] FIG. 6 is a tensile strain curve of the strap of Example 2. [Figure 7] FIG. 7 shows the dynamic mechanical properties of the straps measured by DMA in Example 2. [Figure 8] FIG. 8 shows the tensile strength results of the adaptive straps for the brassiere tested by DMA in Example 3. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0029] The present invention provides an adaptive strap for a brassiere. In one aspect, a material 100 for an adaptive strap, as shown in FIG. 1, includes at least one adaptive material layer 10 and two elastic fabric layers 20. Each of the adaptive material layers 10 is sandwiched between two of the elastic fabric layers 20. The thickness of the material 100 in one embodiment is selected to be 2 millimeters or less. As used herein, the term "adaptive material" refers to a material that has low tensile strength under static loading conditions and high tensile strength during high speed vibration. In this way, the material "adapts" to the loading conditions, providing a high level of support to the breasts during vigorous exercise, since the material generally provides soft and stretchy comfort to the wearer during normal movement, while the elastic modulus increases in response to increased dynamic loading. In general, the adaptive material has a first strength modulus "x" during static loading and a second strength modulus of at least "2x" during dynamic loading of at least about 3 Hz vibration. Exemplary mechanical properties of material 100, in one aspect, are a load strength of 7 N or greater at a static elongation of 10%. In another aspect, material 100 exhibits a load strength of at least 15 N at a static elongation of 10% followed by oscillatory elongation at 3.0 Hz.
[0030] Because breasts move in approximately a figure-eight or "butterfly" pattern during exercise, the adaptive straps of the present invention can be used not only on the shoulder straps, but also on the side bands, across the back, and in a lower support band under the breasts, as shown in Figure IB. Other configurations for using the adaptive straps of the present invention are possible depending on the size of breasts to be supported by the bra (e.g., more adaptive straps / bands) and the intensity of the activity the bra is designed to be used for (running - more straps / bands, yoga or other activities with less breast movement - fewer straps / bands).
[0031] The adaptive material 10 comprises a reaction product formed by reacting silanol-terminated polydimethylsiloxane, a polymer matrix, boric acid, and optional fillers to obtain a cured composite, as described in more detail below. The elastic fabric layer 20 may be selected from one or more of fabrics made of elastane (polyether-polyurea copolymers, including brand names LYCRA and SPANDEX), nylon, polyester, polyurethane, and mixtures and blends of these polymers. Elastomeric materials including silicone, natural rubber / latex, and polyurethane-based elastomers (as well as mixtures / blends of the above elastic materials with elastomers) may also be used. Typically, the elastic portion 20 of the material 100 is selected to be longitudinally stretchable to 100% of its initial length under static load.
[0032] In one embodiment, the fabric 100 for making the adaptive straps of the present invention may be formed in situ, with the adaptive layer 10 cured with a shell formed by the elastic layer 20. Advantageously, this strengthens the bond between the elastic layer 20 and the adaptive layer 10, making the composite material 100 less susceptible to delamination. Additionally, this in-situ technique simplifies manufacturing of the garment, as the adaptive layer 10 can be difficult to assemble into a final garment if formed separately. As seen in FIG. 3, an exemplary method for preparing an adaptive strap for a brassiere includes: 1) mixing a silanol-terminated polydimethylsiloxane, a polymer matrix, boric acid, and optionally a filler together at a reaction temperature for a reaction time (discussed in more detail in the Examples below) to obtain a composite; 2) mixing the composite with a curing agent at room temperature to form an uncured adaptive material; 3) filling the uncured adaptive material into a tubular or other shaped removable shell 200 (e.g., a plastic tube as shown in FIG. 3); 4) dissolving the tubular The shell-filled uncured adaptive material is inserted into one or more hollow fabric structures formed into the shape of a support strap or band for use in a sports bra; 5) the tubular shell is slightly pushed in and pulled out of the hollow fabric structure until the uncured adaptive material substantially fills the hollow space within the hollow fabric structure; 6) the temporary tubular shell is removed from the hollow fabric structure; 7) the uncured adaptive material within the hollow fabric structure is allowed to cure in situ to form the adaptive straps.
[0033] In one embodiment, the silanol terminated polydimethylsiloxane, polymer matrix, boric acid, curing agent, and optional filler are in the weight range of 5:100:0.02:0.5:0 to 100:100:1:3:10.
[0034] The silanol-terminated polydimethylsiloxane may be selected from one or more of silanol-terminated polydimethylsiloxane, silanol-terminated diphenylsiloxane-dimethylsiloxane copolymer, or vinylmethylsiloxane-dimethylsiloxane copolymer, and may have a molar ratio of 0-18% phenyl and 0-15% vinyl. The average molecular weight of the silanol-terminated polydimethylsiloxane is 650-139,000 g / mol. Typically, the boric acid is provided in an ethanol solution at a weight ratio of 1% to 10% by weight. The curing agent may include a peroxide, a crosslinking agent, a catalyst, and combinations thereof. The peroxide may be one or more of 2,4-dichlorobenzoyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, and dibenzoyl peroxide. The crosslinking agent may be selected from silicon hydride compounds having at least two SiH groups. The catalyst may be one or more of palladium, rhodium, and platinum.
[0035] The reaction temperature for obtaining the composite is about 80° C. to 200° C., and the reaction time is about 0.5 to 8 hours. The curing temperature is room temperature or about 25° C. to about 200° C., and the curing time is about 0.5 to 24 hours. EXAMPLES
[0036] The following examples are presented to illustrate the present disclosure and are not intended to be limiting in any way. [Table 1]
[0037] Example 1 In this example, an adaptive strap was manufactured according to the method of the present invention as follows. 1) To ensure uniform mixing, boric acid was dissolved in ethanol to form a 10 wt.% solution. 2) Next, 9.974 g of silanol-terminated polydimethylsiloxane, 0.26 g of boric acid solution, and 100 g of vinyl silicone rubber (Shore A 60) as a polymer matrix were mixed and stirred at 120°C for 6 hours to form a composite. Here, the molecular weight of the silanol-terminated polydimethylsiloxane was 49,000 g / mol. 3) The above complex (110 g) and 2 g of platinum catalyst were mixed in an internal mixer at 50 rpm for 5 minutes. 4) The mixture was then poured into a tubular strap having an elastic fabric portion 20 made from spandex and polyester fibers. The strap was stored with the mixture at room temperature for 24 hours to cure and form an adaptive strap having a thickness of 1.46 mm.
[0038] The tensile strain curve of the strap is shown in Figure 4. As shown in Figure 4, the tensile force of the adaptive strap at 10% static strain is 6.49 N. The dynamic mechanical properties of the strap are measured by DMA as shown in Figure 5. The calculated tensile force at 10% static elongation at 8% amplitude of 3.0 Hz vibration is 16.32 N.
[0039] Example 2 In this example, an adaptive strap was manufactured according to the method of the present invention as follows. 1) 10 g of silanol-terminated polydimethylsiloxane (MW: about 650 g / mol), 10 g of silanol-terminated polydimethylsiloxane (MW: about 13,900 g / mol), 20 g of silanol-terminated diphenylsiloxane-dimethylsiloxane copolymer (18% diphenylsiloxane), 20 g of vinylmethylsiloxane-dimethylsiloxane copolymer (15% vinylmethylsiloxane), 2.88 g of boric acid, 17 g of silicon dioxide (filler), and 3 g of titanium dioxide (filler) were mixed and stirred at 200°C for 2 hours, and then 3 g of glyceryl oleate (filler) was mixed to form a complex. 2) Next, 100 g of vinyl silicone rubber (polymer matrix) (Shore A 60), 30 g of the above complex, and 1 g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (curing agent) were mixed for 5 minutes in an internal mixer at 50 r / min. 3) The mixture was injected into a tubular strap with an outer elastic material composition of spandex and nylon fibers. The strap was stored with the mixture at room temperature for 24 hours to cure and form an adaptive strap with a thickness of 1.46 mm.
[0040] The tensile strain curve of the strap is shown in Figure 6. As shown in Figure 6, the tensile force of the adaptive strap at 10% strain is 6.95N. The dynamic mechanical properties of the strap are measured by DMA as shown in Figure 7. The calculated tensile force at 10% static elongation at 8% amplitude with 3.0Hz vibration is 16.96N.
[0041] Example 3 In this example, an adaptive strap was manufactured according to the method of the present invention as follows. 1) 10 g of silanol-terminated polydimethylsiloxane (MW: about 650 g / mol), 10 g of silanol-terminated polydimethylsiloxane (MW: about 13,900 g / mol), 20 g of silanol-terminated diphenylsiloxane-dimethylsiloxane copolymer (18% diphenylsiloxane), 20 g of vinylmethylsiloxane-dimethylsiloxane copolymer (15% vinylmethylsiloxane), 2.88 g of boric acid, 17 g of silicon dioxide (filler), and 3 g of titanium dioxide (filler) were mixed and stirred at 200°C for 2 hours, and then 3 g of glyceryl oleate was mixed to form a complex. 2) Next, 100 g of vinyl silicone rubber (Shore A 60) (polymer matrix), 30 g of the above composite, and 1 g of 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane (curing agent) were mixed in an internal mixer at 50 rpm for 5 minutes. 3) The mixture was poured into a tubular strap having a fabric composition of spandex and nylon fibers. The strap was stored with the mixture at room temperature for 24 hours to cure and form an adaptive strap.
[0042] The adaptive straps of the bra are cut to a dimension of 4mm x 8mm. Dynamic Mechanical Analysis (DMA) is used to accurately analyze the mechanical properties of the vibration. As shown in Figure 8, the frequency can have a significant effect on the mechanical properties of the adaptive straps, while the effect of frequency is not obvious in the control sample. Even after 960 circles, the adaptive straps are very stable in terms of tensile strength.
[0043] advantage Advantages of the present invention include: 1) an adaptive strap for a brassiere with adaptive performance that provides adequate support during various activities; 2) a new formulation of material for the adaptive bra strap; 3) a simplified injection process for creating the adaptive bra strap; 4) fast recovery and stable performance of the adaptive bra strap.
[0044] As used herein, the terms "nearly," "essentially," "substantially," and "about" are used to describe and account for small variations. When used in conjunction with an event or circumstance, the term can refer to an event or circumstance occurring precisely or approximately. The term "about," as used herein with respect to a given value or range, generally means a range of ±10%, ±5%, ±1%, or ±0.5% of the given value or range. Ranges may be expressed herein as from one endpoint to another endpoint or between two endpoints. All ranges disclosed in this disclosure include the endpoints unless otherwise specified. The term "substantially coplanar" may refer to two surfaces that are disposed along the same plane within a few micrometers (μm), for example, within 10 μm, within 5 μm, within 1 μm, or within 0.5 μm, disposed along the same plane. When referring to "substantially" the same numerical value or characteristic, the term may refer to values within ±10%, ±5%, ±1%, or ±0.5% of the mean of the value.
[0045] The foregoing description of the present invention has been provided for purposes of illustration and description. It is not intended to be exhaustive or to limit the invention to the precise form disclosed. Many modifications and variations will be apparent to those skilled in the art.
[0046] Although the present disclosure has been described and illustrated with reference to specific embodiments thereof, these descriptions and illustrations are not limiting. Those skilled in the art should understand that various modifications can be made and equivalents can be substituted without departing from the true spirit and scope of the present disclosure as defined by the appended claims. The drawings are not necessarily drawn to scale. Due to manufacturing processes and tolerances, there may be distinctions between artistic renditions in the present disclosure and actual devices. There may be other embodiments of the present disclosure that are not specifically illustrated. The specification and drawings should be regarded as illustrative rather than restrictive. Changes can be made to adapt a particular situation, material, composition of matter, method, or process to the objective, spirit, and scope of the present disclosure. All such modifications are intended to be within the scope of the appended claims. Although the methods disclosed herein have been described with reference to certain operations performed in a particular order, it will be understood that these operations may be combined, sub-divided, or reordered to form equivalent methods without departing from the teachings of the present disclosure. Thus, unless specifically indicated herein, the order and grouping of operations are not limiting.
Claims
1. 1. An adaptive strap for a brassiere, comprising: at least one adaptive material layer having a first strength modulus, x, under static loading and a second strength modulus of at least 2x under dynamic loading of at least about 3 Hz vibration, the at least one adaptive material layer including an adaptive material formed by reacting a silanol-terminated polydimethylsiloxane, a polymeric matrix material, and boric acid; two or more elastic fabric layers; Including, each of the adaptive material layers is sandwiched between two of the elastic fabric layers such that the adaptive straps are stretchable to 100% of their initial length during low wearer activity, but cannot stretch more than 50% during vigorous wearer activity; Adaptive straps for bras.
2. 10. The adaptive strap for a brassiere of claim 1, wherein the adaptive strap has a thickness of less than 2 mm.
3. 2. The adaptive strap for a brassiere of claim 1, wherein the adaptive strap has a load strength of at least 7N at a static elongation of 10%.
4. 10. The adaptive strap for a brassiere of claim 1, wherein the adaptive strap has a load strength of at least 15N at a static elongation of 10% followed by a vibratory elongation at 3.0 Hz.
5. 10. A method for preparing an adaptive strap for a brassiere according to claim 1, comprising: i) mixing one or more silanol terminated polydimethylsiloxanes, a polymeric matrix material, and boric acid at a reaction temperature for a reaction time to obtain a composite; ii) mixing the composite with a curing agent at room temperature to form an uncured adaptive material; iii) filling the temporary shell with the uncured adaptive material; iv) inserting the temporarily filled uncured adaptive material into one or more hollow fabric structures; v) incorporating the uncured adaptive material into the hollow fabric structure until the uncured adaptive material substantially fills the hollow space of the hollow fabric structure; vi) removing the temporary shell from the hollow fabric structure; vii) curing the uncured adaptive material within the hollow fabric structure to form the adaptive strap; and A method including:
6. 6. The method of claim 5, wherein the silanol terminated polydimethylsiloxane, polymer matrix, boric acid, and curing agent are in the weight range of 5:100:0.02:0.5 to 100:100:1:
3.
7. 6. The method of claim 5, wherein the silanol terminated polydimethylsiloxane is selected from one or more of silanol terminated polydimethylsiloxane, silanol terminated diphenylsiloxane-dimethylsiloxane copolymer, vinylmethylsiloxane-dimethylsiloxane copolymer, wherein phenyl is in a molar ratio of 0-18% and vinyl is in a molar ratio of 0-15%.
8. The method of claim 5, wherein the silanol-terminated polydimethylsiloxane has an average molecular weight of 650 to 139,000 g / mol.
9. 6. The method of claim 5, wherein the boric acid is provided in an ethanol solution at a weight ratio of 1% to 10% by weight.
10. The method of claim 5 , wherein the curing agent comprises one or more of a peroxide, a crosslinking agent, and a catalyst.
11. The method of claim 5 , wherein the composite further comprises one or more fillers.
12. The method of claim 5, wherein the polymer matrix material is selected from silicone rubber, natural rubber, synthetic rubber, or a combination thereof and has a hardness of about 40 Shore A to 80 Shore A.
13. 11. The method of claim 10, wherein the curing agent is a peroxide, the peroxide being one or more of 2,4-dichlorobenzoyl peroxide, 2,5-dimethyl-2,5-di(tert-butylperoxy)hexane, or dibenzoyl peroxide.
14. The method of claim 10, wherein the curing agent is a crosslinking agent, the crosslinking agent being selected from one or more silicon hydride compounds having at least two SiH groups.
15. The method of claim 10, wherein the curing agent is a catalyst, the catalyst being one or more of palladium, rhodium, or platinum.
16. The method of claim 5, wherein the reaction temperature to obtain the complex is about 80°C to 200°C.
17. The method of claim 5, wherein the reaction time to obtain the complex is about 0.5 to 8 hours.
18. The method of claim 5, wherein the curing temperature is about room temperature or between 25°C and 200°C.
19. The method of claim 5, wherein the curing time is about 0.5 to 24 hours.
20. 12. The method of claim 11, wherein the filler is selected from silica dioxide, titanium dioxide, glyceryl oleate, or any combination thereof.
21. 5. The adaptive strap for a brassiere according to claim 1, wherein the adaptive strap has a tensile strength of greater than 4 MPa at a frequency of 2.0 Hz after 960 cycles of an 8 minute test and a tensile strength of greater than 1 MPa in a static state at 10% strain.
Citation Information
Patent Citations
Bra
CN113907450A
Brassiere having excellent swing-proofing property
JP2014163018A
Support suit for optimizing human posture and movement
JP2015519086A
Silicone rubber composition for coating
JP2018104560A
Elasticated bra band
KR200334389Y1