Negative electrode and secondary battery including the same
The combination of graphite, single-walled carbon nanotubes, and a cellulose-rubber binder in a silicon-based negative electrode addresses the expansion issues of silicon-based materials, enhancing both life and output characteristics by maintaining a stable conductive network and improving electrolyte wettability.
Patent Information
- Application Number
- JP2023540801
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2021-01-29
- Filing Date
- 2022-01-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2042-01-27
AI Technical Summary
Silicon-based active materials in negative electrodes of lithium secondary batteries experience significant volumetric expansion and contraction during charging and discharging, leading to electrical short circuits and reduced life and output characteristics due to inadequate binder tensile strength and electrolyte wettability.
A negative electrode design incorporating a silicon-based active material with a combination of graphite as a first conductive material, single-walled carbon nanotubes as a second conductive material, and a binder comprising cellulose and rubber compounds, where the materials are present in specific weight ratios to enhance electrolyte wettability and tensile strength, maintaining a conductive network despite volume changes.
The solution improves both the life and output characteristics of the negative electrode by suppressing volumetric expansion and contraction of silicon-based active materials, ensuring stable conductivity and enhanced tensile strength.
Smart Images

Figure 0007571304000001 
Figure 0007571304000002 
Figure 0007571304000003
Abstract
Description
[Technical field]
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0013020 filed on January 29, 2021, the entire contents of which are incorporated herein by reference.
[0002] The present invention relates to a negative electrode and a secondary battery including the same. [Background technology]
[0003] Recently, with the rapid spread of electronic devices using batteries, such as mobile phones, notebook computers, and electric vehicles, the demand for secondary batteries that are small, lightweight, and have a relatively high capacity is rapidly increasing. In particular, lithium secondary batteries, which are lightweight and have high energy density, are attracting attention as a driving power source for portable devices. As a result, research and development efforts to improve the performance of lithium secondary batteries are being actively carried out.
[0004] In general, a lithium secondary battery includes a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, an electrolyte, an organic solvent, etc. In addition, the positive electrode and the negative electrode may have an active material layer including a positive electrode active material or a negative electrode active material formed on a current collector. In general, a lithium-containing metal oxide such as LiCoO2 or LiMn2O4 is used as a positive electrode active material in the positive electrode, and a carbon-based active material or a silicon-based active material not containing lithium is used as a negative electrode active material in the negative electrode.
[0005] Among negative electrode active materials, silicon-based active materials have been attracting attention because they have a capacity about 10 times higher than that of carbon-based active materials and have excellent high-speed charging characteristics. However, silicon-based active materials have a large degree of volume expansion / contraction due to charging / discharging, and electrical short circuits between active materials are likely to occur due to repeated charging / discharging, which reduces the life characteristics of the negative electrode. In this regard, negative electrodes using silicon-based active materials together with binders containing styrene-butadiene rubber and carboxymethyl cellulose have been developed, but these binders do not have high tensile strength and cannot sufficiently suppress the volume expansion of the silicon-based active material. Meanwhile, negative electrodes using silicon-based active materials together with binders with high tensile strength such as polyvinyl alcohol and polyacrylic acid have been developed, but these binders such as polyvinyl alcohol and polyacrylic acid have poor electrolyte wettability, which reduces the conductivity of the active material, increases the resistance, and reduces the output characteristics of the negative electrode.
[0006] Korean Patent No. 10-0794192 relates to a method for manufacturing a carbon-coated silicon-graphite composite negative electrode material for a lithium secondary battery and a method for manufacturing a secondary battery including the same, but has limitations in solving the above-mentioned problems. [Prior art documents] [Patent documents]
[0007] [Patent Document 1] Korean Patent No. 10-0794192 Summary of the Invention [Problem to be solved by the invention]
[0008] An object of the present invention is to provide a negative electrode capable of simultaneously improving the life characteristics and output characteristics.
[0009] Another object of the present invention is to provide a secondary battery including the above-mentioned negative electrode. [Means for solving the problem]
[0010] The present invention provides a negative electrode comprising: a negative electrode current collector; and a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer comprising a silicon-based active material, a first conductive material containing graphite, a second conductive material containing single-walled carbon nanotubes, and a binder, the binder comprising a cellulose-based compound and a rubber-based compound, the first conductive material being contained in the negative electrode active material layer at 15 wt % to 25 wt %, the second conductive material being contained in the negative electrode active material layer at 0.15 wt % to 2.5 wt %, and the second conductive material and the binder being contained in the negative electrode active material layer at a weight ratio of 1.5:99.5 to 20.0:80.0.
[0011] The present invention also provides a secondary battery including the above-mentioned negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. Effect of the Invention
[0012] The negative electrode of the present invention is characterized in that, in a negative electrode using a silicon-based active material, a first conductive material containing graphite, a second conductive material containing single-walled carbon nanotubes, and a binder containing a cellulose-based compound and a rubber-based compound are used in combination, and the first conductive material, the second conductive material, and the binder are contained in specific contents. According to the present invention, by using a binder having excellent electrolyte wettability, the output characteristics of the negative electrode can be improved, and the second conductive material can be bound to the binder to improve the tensile strength of the binder, so that the volume expansion and contraction of the silicon-based active material can be suppressed, and the first conductive material can be present between the silicon-based active materials to maintain a conductive network. Therefore, the negative electrode and a secondary battery including the same can simultaneously improve the life characteristics and output characteristics to excellent levels. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The terms and words used in this specification and the claims should not be interpreted as being limited to their ordinary or dictionary meanings, but should be interpreted as having meanings and concepts that are consistent with the technical idea of the present invention, based on the principle that an inventor can appropriately define the concept of a term in order to best describe his / her invention.
[0014] The terms used in this specification are merely used to describe exemplary embodiments and are not intended to limit the present invention. A singular expression includes a plural expression unless the context clearly indicates otherwise.
[0015] In this specification, the terms "comprise", "comprise", or "have" are intended to specify the presence of embodied features, numbers, steps, components, or combinations thereof, and should be understood as not precluding the possibility of the presence or addition of one or more other features, numbers, steps, components, or combinations thereof.
[0016] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size that corresponds to 50% of the cumulative volume in the particle size distribution curve. 50 ) can be measured, for example, by using a laser diffraction method. The laser diffraction method generally allows measurement of particle sizes from the submicron range to about several mm, and can provide results with high reproducibility and high resolution.
[0017] <Negative electrode> The present invention relates to a negative electrode, specifically, to a negative electrode for a lithium secondary battery.
[0018] Specifically, the negative electrode of the present invention includes a negative electrode current collector and a negative electrode active material layer disposed on the negative electrode current collector. The negative electrode active material layer includes a silicon-based active material, a first conductive material including graphite, a second conductive material including single-walled carbon nanotubes, and a binder. The binder includes a cellulose-based compound and a rubber-based compound. The first conductive material is included in the negative electrode active material layer at 15 wt % to 25 wt %. The second conductive material is included in the negative electrode active material layer at 0.15 wt % to 2.5 wt %, and the second conductive material and the binder are included in the negative electrode active material layer at a weight ratio of 1.5:99.5 to 20.0:80.0.
[0019] Conventionally, silicon-based active materials have the advantages of having high capacity and rapid charging characteristics. However, silicon-based active materials have a large degree of volume expansion / contraction due to charging / discharging, which causes problems such as the active materials in the negative electrode losing contact with each other as charging / discharging continues. This makes it difficult to transfer lithium between the active materials, causing problems such as lithium precipitation, and a rapid decrease in life characteristics.
[0020] In order to solve these problems, the negative electrode of the present invention is characterized in that, in a negative electrode using a silicon-based active material, a first conductive material containing graphite, a second conductive material containing single-walled carbon nanotubes, and a binder containing a cellulose-based compound and a rubber-based compound are used in combination, and the first conductive material, the second conductive material, and the binder are contained in specific contents. According to the present invention, by using a binder having excellent electrolyte wettability, the output characteristics of the negative electrode can be improved, and the second conductive material can be bound to the binder to improve the tensile strength of the binder, thereby suppressing the volume expansion and contraction of the silicon-based active material, and the first conductive material can be present between the silicon-based active materials to maintain a conductive network. Therefore, the negative electrode and a secondary battery including the same can simultaneously improve the life characteristics and output characteristics to excellent levels.
[0021] The negative electrode current collector may include at least one selected from the group consisting of copper, stainless steel, aluminum, nickel, titanium, sintered carbon, and an aluminum-cadmium alloy, and may preferably include copper.
[0022] The negative electrode current collector may have a thickness of usually 3 μm to 500 μm, preferably 5 μm to 30 μm.
[0023] The negative electrode current collector may have a surface with fine projections and recesses to strengthen the binding force of the negative electrode active material. For example, the negative electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.
[0024] The negative electrode active material layer may be disposed on the negative electrode current collector. Specifically, the negative electrode active material layer may be disposed on at least one surface of the negative electrode current collector, specifically, on one or both surfaces of the negative electrode current collector.
[0025] The negative electrode active material layer includes a silicon-based active material, a first conductive material, a second conductive material, and a binder.
[0026] The silicon-based active material may include a compound represented by the following Formula 1:
[0027] [Chemical formula 1] SiO x
[0028] In the above Chemical Formula 1, 0≦x<2. In the case of SiO2, it is preferable that x is within the above range because SiO2 does not react with lithium ions and cannot store lithium.
[0029] Specifically, the silicon-based active material can contain Si. Conventionally, Si has been used in the form of silicon oxide (e.g., SiO xAlthough it is advantageous in that the capacity is about 2.5 to 3 times higher compared to (0 < x < 2), since the degree of volume expansion / contraction due to charge and discharge of Si is much larger than that of silicon oxide, commercialization is not easier. However, in the case of the secondary battery of the present invention, even when using a silicon-based active material containing Si, the charging potential of the active material can be lowered to a preferable level, so that while preventing a decrease in life characteristics, the high capacity and rapid charging characteristics of the silicon-based active material can be improved. Specifically, most of the silicon-based active material can be composed of Si, and more specifically, the silicon-based active material can be composed of Si.
[0030] The average particle diameter (D 50 ) of the silicon-based active material is 1 μm to 10 μm, preferably 2 μm to 6 μm, from the viewpoint of aiming for structural stability of the active material during charge and discharge, being able to more smoothly form a conductive network for maintaining electrical conductivity, or facilitating proximity to a binder for binding the active material and the current collector.
[0031] The silicon-based active material may be contained in the negative electrode active material layer at 60% by weight to 78% by weight, preferably 65% by weight to 75% by weight. When it is within the above range, while minimizing the influence of volume expansion / contraction of the silicon-based active material on the battery, the high capacity of the silicon-based active material can be sufficiently realized in the secondary battery.
[0032] The negative electrode active material layer contains a first conductive material containing graphite and a second conductive material containing single-walled carbon nanotubes.
[0033] In the negative electrode of the present invention, the first conductive material contains graphite and can continue to maintain a conductive network among the active materials even when the active materials expand / contract in volume due to charge and discharge. The second conductive material contains single-walled carbon nanotubes, has a large specific surface area, and can be well adsorbed on the surface of the active material, so that the conductivity of the silicon-based active material can be improved.
[0034] In addition, in the case of the second conductive material, the single-walled carbon nanotubes are bound to the binder in the negative electrode, thereby improving the tensile strength of the binder. Therefore, when the binder, first conductive material, and second conductive material of the present invention are used, the binder has excellent electrolyte wettability, which improves the output characteristics of the negative electrode, and a binder with excellent tensile strength can be realized, and the volume expansion and contraction of the silicon-based active material can be controlled to an excellent level. Therefore, the negative electrode containing the conductive material and binder of the present invention can simultaneously improve the output characteristics and life characteristics.
[0035] The specific surface area of the first conductive material is 5 m 2 / g~40m 2 / g, preferably 7m 2 / g~30m 2 / g, more preferably 10m 2 / g~20m 2 When the specific surface area of the first conductive material satisfies the above range, the viscosity of the negative electrode slurry for manufacturing the negative electrode can be prevented from becoming excessively high, and the dispersibility of the first conductive material can be improved, which is preferable, and thus the first conductive material can be uniformly distributed among the active materials, thereby improving the retention effect of the conductive network.
[0036] The specific surface area of the first conductive material can be defined as a value measured by a nitrogen adsorption method (BET specific surface area).
[0037] The first conductive material may include graphite, and more specifically, may include at least one selected from artificial graphite and natural graphite.
[0038] The graphite may be plate-shaped. When the graphite is plate-shaped, the graphite has excellent contact with the active materials when disposed between the active materials, and can more smoothly maintain the conductive network between the active materials. More specifically, the conductive material may include plate-shaped graphite.
[0039] The aspect ratio of the first conductive material may be 1.1 to 30.0, preferably 1.2 to 6.0. When the first conductive material has an aspect ratio in the above-mentioned range, the shape of the first conductive material can be well maintained even if the silicon-based active material expands / contracts in volume, so that the conductive network between the silicon-based active materials can be more preferably maintained. In this specification, the aspect ratio of the first conductive material can be defined as "long axis length of the first conductive material / short axis length of the first conductive material".
[0040] The average particle size (D 50 The average particle diameter (D 50 When the volume of the silicon-based active material is in the range, the conductive network between the active materials can be easily maintained even if the silicon-based active material expands / shrinks, and the life performance of the negative electrode can be improved.
[0041] The average particle size (D 50 ) and the average particle size (D 50 ) may be 1:1 to 1:5, preferably 1:1 to 1:2. When it is in this range, even if the silicon-based active material expands / contracts in volume in the negative electrode and the distance between the active materials increases, the first conductive material can maintain the conductive network between the active materials, which is preferable.
[0042] The first conductive material is contained in the negative electrode active material layer in an amount of 15% by weight to 25% by weight. When the first conductive material is used in the negative electrode active material layer in an amount of less than 15% by weight, it is difficult to sufficiently form a conductive network between silicon-based active materials. When the first conductive material is used in an amount of more than 25% by weight, the conductive network retention effect is improved, but the overall improvement in the conductivity in the negative electrode is slight due to the increased content of the first conductive material, which is a conductive material with a small specific surface area, and the content of the active material in the negative electrode is reduced, which is undesirable from the viewpoint of securing capacity.
[0043] The first conductive material may be preferably contained in the negative electrode active material layer in an amount of 17.5 wt % to 23.0 wt %. When the amount is within this range, the conductive network between the silicon-based active materials can be maintained even when charging and discharging are continued, and the life characteristics can be further improved, while the excellent rapid charging performance of the silicon-based active material can be more easily ensured.
[0044] The second conductive material has excellent electrical conductivity and excellent adsorption to the silicon-based active material, so that the electrical conductivity of the surface of the silicon-based active material can be improved. In addition, the second conductive material can be bonded to the binder to improve the tensile strength of the binder, so that the volume expansion and contraction of the silicon-based active material can be controlled.
[0045] The second conductive material may include a single-walled carbon nanotube (SWCNT). Specifically, the second conductive material may include a single-walled carbon nanotube aggregate formed by aggregating two or more single-walled carbon nanotubes.
[0046] The specific surface area of the second conductive material is 400 m 2 / g~1,500m 2 / g, preferably 600m 2 / g~1,200m 2 By having the specific surface area of the second conductive material satisfy the above range, the second conductive material can be favorably adsorbed onto the surface of the silicon-based active material, and the conductivity of the surface of the silicon-based active material can be imparted at an excellent level.
[0047] The specific surface area of the second conductive material can be defined as a value measured by a nitrogen adsorption method (BET specific surface area).
[0048] The diameter of the second conductive material may be 0.1 nm to 20 nm, preferably 1 nm to 5 nm, and when it is in the above range, it is preferable because the second conductive material can be stably adsorbed to the surface of the silicon-based active material.
[0049] In this specification, the diameter of the second conductive material is measured by the following method. A solution (solid content is 1% by weight based on the total weight of the solution) in which the second conductive material and carboxymethyl cellulose (CMC) are added to water in a weight ratio of 40:60 is diluted 1,000 times with water. One drop of the diluted solution is dropped onto a TEM grid, and the TEM grid is dried. The dried TEM grid is observed with a TEM device (product name: H7650, manufacturer: Hitachi) to measure the average diameter of the second conductive material.
[0050] The second conductive material may have a length of 1 μm to 50 μm, preferably 5 μm to 20 μm. When the length is within this range, the long fibers of the second conductive material can improve smooth adsorption or contact with the surface of the active material.
[0051] In this specification, the length of the second conductive material is measured by the following method. A solution (solid content is 1% by weight based on the total weight of the solution) in which the second conductive material and carboxymethyl cellulose are added to water in a weight ratio of 40:60 is diluted 1,000 times with water. Then, 20 ml of the diluted solution is filtered through a filter, and the filter from which the second conductive material has been filtered is dried. 100 images of the dried filter are taken with a scanning electron microscope (SEM), and the length of the second conductive material is measured using an imageJ program, and the average value of the lengths can be defined as the length of the second conductive material.
[0052] The aspect ratio of the second conductive material may be 5,000 to 15,000, preferably 6,000 to 12,000. When it is in this range, it is preferable in that the conductive network of the second conductive material can be stably maintained without being damaged by rolling of the electrode or volume expansion of the negative electrode active material, and can be smoothly attached to the surface of the silicon-based active material. The aspect ratio of the second conductive material can be defined as "the length of the second conductive material / the diameter of the second conductive material".
[0053] The second conductive material is included in the negative electrode active material layer in an amount of 0.15 wt % to 2.5 wt %. If the second conductive material is included in the negative electrode active material layer in an amount less than 0.15 wt %, the second conductive material is used too little, making it difficult to ensure the conductivity of the surface of the silicon-based active material, and the conductivity of the active material is reduced, and the content of the second conductive material bound to the binder is too small to sufficiently improve the tensile strength of the binder, which may cause a rapid deterioration in the life characteristics of the negative electrode. In addition, the second conductive material can contribute to the formation of a conductive network between the silicon-based active materials in addition to the surface of the silicon-based active materials, but if the content of the second conductive material is too small, it is difficult to expect such effects.
[0054] In addition, if the second conductive material is contained in the negative electrode active material layer in an amount exceeding 2.5 wt %, the second conductive material is used in excess, making it difficult to easily disperse during the manufacture of the negative electrode, and agglomeration occurs, making it difficult to ensure the conductivity of the silicon-based active material. Problems such as difficulty in uniformly distributing the second conductive material and localized increased resistance may occur. The conductivity of the surface of the silicon-based active material may decrease, and the large specific surface area of the second conductive material itself may cause problems such as side reactions of the electrolyte and gas generation, which may result in a decrease in the life characteristics of the negative electrode.
[0055] The second conductive material may be preferably contained in the negative electrode active material layer in an amount of 0.17% by weight to 2.0% by weight. When the amount is within this range, the surface conductivity of the silicon-based active material is improved, and the dispersibility of the second conductive material can be improved during the manufacture of the negative electrode, and the second conductive material can be distributed at a uniform level within the negative electrode, so that the life characteristics of the negative electrode are further improved and the excellent rapid charging performance of the silicon-based active material can be more easily exhibited.
[0056] The first conductive material and the second conductive material may be contained in the negative electrode active material layer in a weight ratio of 0.7:99.3 to 1.5:99.5, preferably 0.8:99.2 to 1.2:99.8. When the weight ratio is within this range, the conductivity of the surface of the silicon-based active material can be improved, and the conductive network between the silicon-based active materials can be maintained even when charging and discharging is continued, so that the life characteristics can be further improved and the excellent rapid charging performance of the silicon-based active material can be more easily secured.
[0057] The binder is a component that assists in binding the active material to the conductive material and the like and to the current collector.
[0058] The binder includes a cellulose-based compound and a rubber-based compound. The binder has improved electrolyte wettability by including the cellulose-based compound and the rubber-based compound. The binder including the cellulose-based compound and the rubber-based compound has a disadvantage of having a lower tensile strength than binders such as polyacrylic acid and polyvinyl alcohol. However, when used together with the second conductive material, the second conductive material is bound to the binder, thereby improving the tensile strength of the binder, and thus suppressing the volume expansion and contraction of the silicon-based active material.
[0059] The cellulose-based compound may include at least one selected from the group consisting of carboxy methyl cellulose (CMC), methyl cellulose (MC), hydroxypropyl cellulose (HPC), methyl hydroxypropyl cellulose (MHPC), ethyl hydroxyethyl cellulose (EHEC), methyl ethyl hydroxyethyl cellulose (MEHEC), and cellulose gum, and may preferably include carboxymethyl cellulose, which has good dispersibility and thickening properties.
[0060] The weight average molecular weight of the cellulose-based compound may be from 700,000 to 2,000,000, and preferably from 1,000,000 to 1,500,000, from the viewpoint of further improving dispersing power and thickening properties.
[0061] The rubber-based compound may include at least one selected from the group consisting of styrene butadiene rubber (SBR), acrylic rubber, butyl rubber, and fluoro rubber, and preferably includes styrene butadiene rubber from the viewpoint of excellent electrolyte wettability and excellent adhesive strength.
[0062] The binder may contain the cellulose-based compound and the rubber-based compound in a weight ratio of 5:95 to 80:20, preferably 15:85 to 50:50. When the weight ratio is within the above range, the electrolyte wettability is further improved, and the tensile strength improving effect by using the binder in combination with the second conductive material described above can be realized at an excellent level, which is preferable.
[0063] In the negative electrode of the present invention, the second conductive material and the binder are contained in the negative electrode active material layer in a weight ratio of 1.5:99.5 to 20.0:80.0. If the second conductive material is less than 1.5 wt % and the binder is more than 99.5 wt % with respect to the sum of the weights of the second conductive material and the binder, the effect of improving the tensile strength of the binder by the second conductive material is small, and it is difficult to smoothly control the volume expansion and contraction of the silicon-based active material. If the second conductive material is more than 20.0 wt % and the binder is less than 80.0 wt % with respect to the sum of the weights of the second conductive material and the binder, there is a possibility of a decrease in adhesive strength, and the second conductive material is not preferable because the dispersibility of the second conductive material is decreased, the binding force to the binder is decreased due to the occurrence of agglomeration phenomenon, etc., and the tensile strength cannot be improved. Specifically, the second conductive material and the binder may be contained in the negative electrode active material layer in a weight ratio of 1.5:99.5 to 5.0:95.0, specifically, a weight ratio of 1.5:98.5 to 5.0:95.0. When the weight ratio is within the above range, it is favorable from the viewpoints of improving the tensile strength of the binder, smoothly maintaining a conductive network, and improving the life characteristics of the negative electrode.
[0064] The binder may be included in the negative active material layer in an amount of 5 wt% to 20 wt%, preferably 7 wt% to 15 wt%. When the amount is within this range, the silicon-based active material can be smoothly bound to minimize the problem of volume expansion of the active material, and the binder can be easily dispersed during preparation of a slurry for forming the negative active material layer, thereby improving the coatability and phase stability of the slurry.
[0065] The thickness of the negative electrode active material layer may be 10 μm to 100 μm, preferably 20 μm to 50 μm. In this specification, the thickness of the negative electrode active material layer may be the thickness of one negative electrode active material layer formed on one surface of the negative electrode current collector.
[0066] <Secondary battery> The present invention provides a secondary battery, specifically a lithium secondary battery, which may include the above-mentioned negative electrode.
[0067] Specifically, the secondary battery may include a negative electrode, a positive electrode facing the negative electrode, a separator interposed between the negative electrode and the positive electrode, and an electrolyte. The negative electrode may be the above-mentioned negative electrode.
[0068] The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on the positive electrode current collector.
[0069] The positive electrode current collector is not particularly limited as long as it has high conductivity without inducing a chemical change in the battery. Specifically, the positive electrode current collector can be made of copper, stainless steel, aluminum, nickel, titanium, baked carbon, copper or stainless steel surface-treated with carbon, nickel, titanium, silver, or the like, or an aluminum-cadmium alloy.
[0070] The positive electrode current collector may typically have a thickness of 3 to 500 μm.
[0071] The positive electrode current collector may have a surface with fine projections and recesses to strengthen the bonding force of the positive electrode active material. For example, the positive electrode current collector may be used in various forms such as a film, a sheet, a foil, a net, a porous body, a foam, a nonwoven fabric, etc.
[0072] The positive electrode active material layer may be disposed on at least one surface of the positive electrode current collector, specifically, on one surface or both surfaces of the positive electrode current collector.
[0073] The positive electrode active material layer may include a positive electrode active material.
[0074] The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium transition metal composite oxide containing lithium and at least one transition metal selected from the group consisting of nickel, cobalt, manganese, and aluminum, preferably a lithium transition metal composite oxide containing lithium and a transition metal including nickel, cobalt, and manganese.
[0075] More specifically, examples of the lithium transition metal composite oxide include lithium-manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), lithium-cobalt-based oxides (e.g., LiCoO2, etc.), lithium-nickel-based oxides (e.g., LiNiO2, etc.), lithium-nickel-manganese-based oxides (e.g., LiNi 1-Y Mn Y O2 (where 0 < Y < 1), LiMn 2-z Ni z O4 (where 0 < Z < 2), etc.), lithium-nickel-cobalt-based oxides (e.g., LiNi 1-Y1 Co Y1 O2 (where 0 < Y1 < 1), etc.), lithium-manganese-cobalt-based oxides (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0 < Y2 < 1), LiMn 2-z1 Co z1 O4 (where 0 < Z1 < 2), etc.), lithium-nickel-manganese-cobalt-based oxides (e.g., Li(Ni p Co q Mn r1 )O2 (where 0 < p < 1, 0 < q < 1, 0 < r1 < 1, p + q + r1 = 1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0 < p1 < 2, 0 < q1 < 2, 0 < r2 < 2, p1 + q1 + r2 = 2), etc.), or lithium-nickel-cobalt-transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3 M S2)O2 (where M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are atomic fractions of independent elements, respectively, with 0 < p2 < 1, 0 < q2 < 1, 0 < r3 < 1, 0 < s2 < 1, and p2 + q2 + r3 + s2 = 1), etc., and one or more of these compounds can be included. Among them, in terms of enhancing the capacity characteristics and stability of the battery, the lithium transition metal composite oxide is LiCoO2, LiMnO2, LiNiO2, lithium nickel-manganese-cobalt oxide (e.g., Li(Ni 0.6 Mn 0.2 Co 0.2 )O2), Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., or lithium nickel cobalt aluminum oxide (e.g., Li(Ni 0.8 Co 0.15 Al 0.05 )O2, etc.). Considering the remarkable improvement effect by controlling the types and content ratios of the constituent elements forming the lithium transition metal composite oxide, the lithium transition metal composite oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O2, Li(Ni 0.5 Mn 0.3 Co 0.2 )O2, Li(Ni 0.7 Mn 0.15 Co 0.15 )O2 or Li(Ni 0.8 Mn 0.1 Co 0.1 )O2, etc., and one or more of these mixtures may be used.
[0076] Considering sufficient capacity display of the positive electrode active material, etc., it may be contained in the positive electrode active material layer at 80% to 99% by weight, preferably 92% to 98.5% by weight.
[0077] The positive electrode active material layer may further include a binder and / or a conductive material in addition to the positive electrode active material.
[0078] The binder is a component that assists in binding the active material and conductive material, etc., and binding to the current collector, and specifically includes at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethyl cellulose (CMC), starch, hydroxypropyl cellulose, regenerated cellulose, polyvinylpyrrolidone, tetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, and preferably includes polyvinylidene fluoride.
[0079] From the viewpoint of ensuring sufficient binding strength between components such as the positive electrode active material, the binder may be contained in the positive electrode active material layer in an amount of 1 to 20% by weight, preferably 1.2 to 10% by weight.
[0080] The conductive material can be used to supplement and improve the conductivity of the secondary battery, and is not particularly limited as long as it has conductivity without inducing chemical changes. Specifically, the conductive material may include at least one selected from the group consisting of graphite such as natural graphite and artificial graphite; carbon black such as carbon black, acetylene black, ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives, and preferably includes carbon black from the viewpoint of improving conductivity.
[0081] The conductive material has a specific surface area of 80 m2 or less, from the viewpoint of facilitating dispersion of the conductive material during preparation of a slurry for forming a positive electrode active material layer and further improving electrical conductivity. 2 / g~200m 2 / g, preferably 100m 2 / g~150m 2 / g.
[0082] From the viewpoint of ensuring sufficient electrical conductivity, the conductive material may be contained in the positive electrode active material layer in an amount of 1% by weight to 20% by weight, preferably 1.2% by weight to 10% by weight.
[0083] The thickness of the positive electrode active material layer may be 30 μm to 400 μm, preferably 50 μm to 110 μm.
[0084] The positive electrode may be prepared by coating a positive electrode slurry including a positive electrode active material, and optionally a binder, a conductive material, and a solvent for forming a positive electrode slurry, on the positive electrode current collector, followed by drying and rolling.
[0085] The positive electrode slurry forming solvent may contain an organic solvent such as NMP (N-methyl-2-pyrrolidone), and may be used in an amount that provides a preferred viscosity when the positive electrode active material, and optionally a binder and a conductive material, etc. are contained. For example, the positive electrode slurry forming solvent may be contained in the positive electrode slurry such that the concentration of solids including the positive electrode active material, and optionally a binder and a conductive material, is 50% by weight to 95% by weight, and preferably 70% by weight to 90% by weight.
[0086] The positive electrode active material layer may have a porosity of 20% to 35%. 。
[0087] The separator separates the negative electrode and the positive electrode to provide a path for lithium ions to move. Any separator that is generally used as a separator in a lithium secondary battery can be used without any particular limitation. In particular, a separator that has low resistance to ion movement of the electrolyte and has excellent humidification ability of the electrolyte solution is preferable. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, and an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof can be used. In addition, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting point glass fiber, polyethylene terephthalate fiber, etc., may be used. In addition, a coated separator containing a ceramic component or a polymeric material may be used to ensure heat resistance or mechanical strength, and may be selectively used in a single layer or multilayer structure.
[0088] In addition, examples of the electrolyte used in the present invention include organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the production of secondary batteries, but are not limited to these.
[0089] Specifically, the electrolyte may include an organic solvent and a lithium salt.
[0090] The organic solvent can be any organic solvent that can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, examples of the organic solvent that can be used include ester-based solvents such as methyl acetate, ethyl acetate, gamma-butyrolactone, and ε-caprolactone; ether-based solvents such as dibutyl ether and tetrahydrofuran; ketone-based solvents such as cyclohexanone; aromatic hydrocarbon-based solvents such as benzene and fluorobenzene; carbonate-based solvents such as dimethyl carbonate (DMC), diethyl carbonate (DEC), methyl ethyl carbonate (MEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (PC); alcohol-based solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (R is a C2 to C20 linear, branched, or cyclic hydrocarbon group that may contain a double bond aromatic ring or an ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; and sulfolanes. Among them, carbonate-based solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate, etc.) having high ionic conductivity and high dielectric constant capable of enhancing the charge / discharge performance of a battery and a low-viscosity linear carbonate-based compound (e.g., ethyl methyl carbonate, dimethyl carbonate, diethyl carbonate, etc.) is more preferred. In this case, a mixture of the cyclic carbonate and the linear carbonate at a volume ratio of about 1:1 to about 1:9 can provide superior electrolyte performance.
[0091] The lithium salt can be used without any particular limitation as long as it is a compound capable of providing lithium ions used in a lithium secondary battery. Specifically, the lithium salt can be LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2. The concentration of the lithium salt is preferably within the range of 0.1 to 2.0M. When the concentration of the lithium salt is within the above range, the electrolyte has appropriate conductivity and viscosity, so that it can exhibit excellent electrolyte performance and lithium ions can move effectively.
[0092] In the secondary battery of the present invention, the N / P ratio calculated by the following mathematical formula 1 may be 1.5 to 2.5, preferably 1.7 to 2.3.
[0093] [Mathematical formula 1] N / P ratio={(discharge capacity per unit area of the negative electrode) / (discharge capacity per unit area of the positive electrode)}.
[0094] Within this range, the silicon-based active material can exhibit high capacity and rapid charging characteristics, and the influence of the volume expansion / contraction of the silicon-based active material on the battery can be minimized, thereby further improving the life characteristics of the secondary battery.
[0095] Specifically, the discharge capacity per unit area of the negative electrode can be determined by the following method. First, a negative electrode sample that is the same as the negative electrode used is prepared. A coin-shaped half-cell is manufactured including the negative electrode sample, a lithium metal counter electrode facing the negative electrode, a separator interposed between the negative electrode and the lithium metal counter electrode, and an electrolyte, and the discharge capacity is determined. The discharge capacity per unit area of the negative electrode can be determined by dividing the discharge capacity by the area of the negative electrode sample.
[0096] The discharge capacity per unit area of the positive electrode can be determined by the following method. First, a positive electrode sample identical to the positive electrode used is prepared. A coin-shaped half-cell is manufactured including the positive electrode sample, a lithium metal counter electrode facing the positive electrode, a separator interposed between the positive electrode and the lithium metal counter electrode, and an electrolyte, and the discharge capacity is determined. The discharge capacity per unit area of the positive electrode can be determined by dividing the discharge capacity by the area of the positive electrode sample.
[0097] The secondary battery can be produced by inserting a separator between the negative electrode and the positive electrode and then injecting an electrolyte solution according to a typical method for producing a secondary battery.
[0098] The secondary battery according to the present invention is useful in the fields of portable devices such as mobile phones, notebook computers, and digital cameras, and electric vehicles such as hybrid electric vehicles (HEVs), and can be particularly preferably used as a constituent battery of a medium- to large-sized battery module. Accordingly, the present invention further provides a medium- to large-sized battery module including the above-mentioned secondary battery as a unit cell.
[0099] Such a medium- to large-sized battery module can be preferably applied to power sources that require high output and large capacity, such as electric vehicles, hybrid electric vehicles, and power storage devices.
[0100] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may be embodied in various different forms and should not be construed as being limited to the embodiments set forth herein, but the present invention is not limited to the embodiments set forth herein.
[0101] Working Example <Production of negative electrodes> Example 1: Preparation of negative electrode Silicon-based active material Si (average particle size (D 50The negative electrode slurry was prepared by mixing the first conductive material, the second conductive material, and the binder in a weight ratio of 70.0:19.8:0.2:10.0 (particle size: 2.3 μm), the first conductive material, the second conductive material, and the binder in a weight ratio of 70.0:19.8:0.2:10.0, and adding the mixture to distilled water as a solvent for forming the negative electrode slurry (solid concentration: 25 wt %).
[0102] The first conductive material is plate-shaped graphite (specific surface area: 17.0 m 2 / g, average particle size (D 50 : 3.5 μm, aspect ratio: 4.0), and the second conductive material is a single-walled carbon nanotube aggregate (specific surface area: 1,100 m 2 / g, diameter: 1.5 nm, length: 10-15 μm, aspect ratio: 6,667-10,000).
[0103] The binder used was a mixture of carboxymethyl cellulose (CMC, weight average molecular weight: 1,260,000) and styrene-butadiene rubber (SBR) in a weight ratio of 10:90.
[0104] The negative electrode current collector was a copper current collector (thickness: 8 μm) on both sides of which the negative electrode slurry was applied at 100 mg / 25 cm 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a negative electrode active material layer (thickness: 25 μm), which was used as a negative electrode (thickness of negative electrode: 58 μm).
[0105] Example 2: Preparation of negative electrode A negative electrode was prepared in the same manner as in Example 1, except that a mixture of carboxymethyl cellulose and styrene-butadiene rubber in a weight ratio of 30:70 was used as the binder.
[0106] Example 3: Preparation of negative electrode A negative electrode was prepared in the same manner as in Example 1, except that a mixture of carboxymethyl cellulose and styrene-butadiene rubber in a weight ratio of 60:40 was used as the binder.
[0107] Comparative Example 1: Production of negative electrode The binder used was a copolymer of polyvinyl alcohol and polyacrylic acid (a mixture of vinyl alcohol monomer and acrylic acid monomer in a weight ratio of 66:34 and polymerized), and the conductive material was carbon black (specific surface area: 63 m 2 / g, average particle size (D 50 A negative electrode was manufactured in the same manner as in Example 1, except that the first conductive material and the second conductive material were mixed in a weight ratio of 10.0:9.8:0.2, and the silicon-based active material, the conductive material, and the binder were mixed in a weight ratio of 70:20:10.
[0108] Comparative Example 2: Production of negative electrode Carbon black (specific surface area: 63 m2) is used as a conductive material. 2 / g, average particle size (D 50 A negative electrode was manufactured in the same manner as in Example 1, except that the first conductive material and the second conductive material were mixed in a weight ratio of 10.0:9.8:0.2, and the silicon-based active material, the conductive material, and the binder were mixed in a weight ratio of 70:20:10.
[0109] Comparative Example 3: Production of negative electrode A negative electrode was prepared in the same manner as in Example 1, except that the silicon-based active material, the first conductive material, the second conductive material, and the binder were mixed in a weight ratio of 80.0:9.8:0.2:10.
[0110] Comparative Example 4: Production of negative electrode A negative electrode was manufactured in the same manner as in Example 1, except that the first conductive material was not used, and the silicon-based active material, the second conductive material, and the binder were mixed in a weight ratio of 85:5:10.
[0111] Comparative Example 5: Production of negative electrode A negative electrode was manufactured in the same manner as in Example 1, except that the silicon-based active material, the first conductive material, the second conductive material, and the binder were mixed in a weight ratio of 60.0:29.8:0.2:10.0.
[0112] Comparative Example 6: Production of negative electrode A negative electrode was manufactured in the same manner as in Example 1, except that the silicon-based active material Si, the first conductive material, the second conductive material, and the binder were mixed in a weight ratio of 70.1:19.8:0.1:10.0.
[0113] Comparative Example 7: Production of negative electrode A negative electrode was manufactured in the same manner as in Example 1, except that the silicon-based active material Si, the first conductive material, the second conductive material, and the binder were mixed in a weight ratio of 67.2:19.8:3.0:10.0.
[0114] [Table 1]
[0115] <Secondary battery manufacturing> 1. Manufacturing of secondary batteries Li[Ni as a positive electrode active material 0.6 Co 0.2 Mn 0.2 ]O2(average particle size (D 50 ): 15 μm), carbon black (product name: Super C65, manufacturer: Timcal) as a conductive material, and polyvinylidene fluoride (PVdF) as a binder were added in a weight ratio of 97.5:1.0:1.5 to N-methyl-2-pyrrolidone (NMP) as a solvent for forming a positive electrode slurry to prepare a positive electrode slurry (solid concentration 72 wt%).
[0116] The positive electrode slurry was applied at 600 mg / 25 cm to both sides of an aluminum current collector (thickness: 15 μm) as a positive electrode current collector. 2 The coated layer was rolled and dried in a vacuum oven at 130° C. for 10 hours to form a positive electrode active material layer (thickness: 73.5 μm) to prepare a positive electrode (thickness: 162 μm).
[0117] A polyethylene separator was interposed between the positive electrode and the negative electrode of Example 1, and an electrolyte was injected to prepare the secondary battery of Example 1.
[0118] The electrolyte was an organic solvent made by mixing fluoroethylene carbonate (FEC) and diethyl carbonate (DMC) in a volume ratio of 30:70, to which vinylene carbonate was added at 3 wt% based on the total weight of the electrolyte, and LiPF6 was added as a lithium salt at a concentration of 1M.
[0119] Secondary batteries of Examples 2 and 3 and Comparative Examples 1 to 7 were manufactured in the same manner as in Example 1, except that the negative electrodes of Examples 2 and 3 and Comparative Examples 1 to 7 were used.
[0120] 2. Measurement and calculation of N / P ratio of secondary battery A negative electrode sample was prepared that was the same as the negative electrode of Example 1. A coin-shaped half-cell was manufactured containing the negative electrode sample, a lithium metal counter electrode facing the negative electrode, a polyethylene separator interposed between the negative electrode and the lithium metal counter electrode, and an electrolyte, and the discharge capacity was calculated (unit: mAh / g). The discharge capacity was divided by the unit area of the negative electrode sample to calculate the discharge capacity per unit area of the negative electrode of Example 1 (unit: mAh / cm 2 ).
[0121] A positive electrode sample was prepared that was the same as the positive electrode in Example 1. A coin-shaped half-cell was manufactured containing the positive electrode sample, a lithium metal counter electrode facing the positive electrode, a polyethylene separator interposed between the positive electrode and the lithium metal counter electrode, and an electrolyte, and the discharge capacity was calculated (unit: mAh / g). The discharge capacity was divided by the unit area of the positive electrode sample to calculate the discharge capacity per unit area of the positive electrode (unit: mAh / cm 2 ).
[0122] The N / P ratio of the secondary battery of Example 1 was calculated using the following formula (N / P ratio=2.00).
[0123] N / P ratio={(discharge capacity per unit area of the negative electrode) / (discharge capacity per unit area of the positive electrode)}.
[0124] The N / P ratios of the secondary batteries of Examples 2 to 3 and Comparative Examples 1 to 7 were determined in the same manner as in Example 1, except that the negative electrodes of Examples 2 to 3 and Comparative Examples 1 to 7 were used.
[0125] The results are shown in Table 2 below.
[0126] [Table 2]
[0127] Experimental Example Experimental Example 1: Evaluation of binder wettability and tensile strength 1. Manufacturing of binder film Binder films of Examples 1A to 3A and Comparative Examples 1A to 7A were produced, and their electrolyte wettability was evaluated.
[0128] Example 1A A binder film of Example 1A containing the conductive material and binder used in Example 1 in the same weight ratio as in Example 1 was prepared.
[0129] The method for manufacturing the binder film is as follows. A dispersion containing 3 g of the binder used in Example 1 was prepared. A solution was prepared by adding the conductive material used in Example 1 to the dispersion according to the weight ratio of Example 1. The solution was stirred at 2,500 rpm for 1 hour using a high-speed stirrer. The stirred solution was placed in a rectangular bowl with an area of 10 cm x 15 cm and a height of 3 cm, the inner surface of which was coated with Teflon (registered trademark), and allowed to air-dry in a hood to manufacture a binder film.
[0130] Example 2A A binder film of Example 2A was prepared containing the conductive material and binder used in Example 2 in the same weight ratio as in Example 2. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Example 2 were used in the same weight ratio as in Example 2, instead of the conductive material and binder used in Example 1.
[0131] Example 3A A binder film of Example 3A was prepared containing the conductive material and binder used in Example 3 in the same weight ratio as in Example 3. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Example 3 were used in the same weight ratio as in Example 3, instead of the conductive material and binder used in Example 1.
[0132] Comparative Example 1A A binder film of Comparative Example 1A was prepared containing the conductive material and binder used in Comparative Example 1 in the same weight ratio as in Comparative Example 1. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 1 were used in the same weight ratio as in Comparative Example 1, instead of the conductive material and binder used in Example 1.
[0133] Comparative example 2A A binder film of Comparative Example 2A was prepared containing the conductive material and binder used in Comparative Example 2 in the same weight ratio as in Comparative Example 2. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 2 were used in the same weight ratio as in Comparative Example 2, instead of the conductive material and binder used in Example 1.
[0134] Comparative example 3A A binder film of Comparative Example 3A was prepared containing the conductive material and binder used in Comparative Example 3 in the same weight ratio as in Comparative Example 3. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 3 were used in the same weight ratio as in Comparative Example 3 instead of the conductive material and binder used in Example 1.
[0135] Comparative example 4A A binder film of Comparative Example 4A was prepared containing the conductive material and binder used in Comparative Example 4 in the same weight ratio as in Comparative Example 4. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 4 were used in the same weight ratio as in Comparative Example 4 instead of the conductive material and binder used in Example 1.
[0136] Comparative example 5A A binder film of Comparative Example 5A was prepared containing the conductive material and binder used in Comparative Example 5 in the same weight ratio as in Comparative Example 5. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 5 were used in the same weight ratio as in Comparative Example 5 instead of the conductive material and binder used in Example 1.
[0137] Comparative Example 6A A binder film of Comparative Example 6A was prepared containing the conductive material and binder used in Comparative Example 6 in the same weight ratio as in Comparative Example 6. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 6 were used in the same weight ratio as in Comparative Example 6 instead of the conductive material and binder used in Example 1.
[0138] Comparative example 7A A binder film of Comparative Example 7A was prepared containing the conductive material and binder used in Comparative Example 7 in the same weight ratio as in Comparative Example 7. The method for preparing the binder film was the same as in Example 1A, except that the conductive material and binder used in Comparative Example 7 were used in the same weight ratio as in Comparative Example 7 instead of the conductive material and binder used in Example 1.
[0139] (2) Evaluation of electrolyte wettability The binder films produced in Examples 1A to 3A and Comparative Examples 1A to 7A were placed in an electrolyte at 60° C. for 24 hours, and then the electrolyte wettability was evaluated according to the following formula. The results are shown in Table 3 below.
[0140] Electrolyte wettability (%) = M / M0 x 100 (In the above formula, M is the weight of the binder film after it is placed in the electrolyte and then removed, and M0 is the weight of the binder film before it is placed in the electrolyte.)
[0141] (3) Evaluation of tensile strength The binder films manufactured in Examples 1A to 3A and Comparative Examples 1A to 7A were punched out into rectangular parallelepipeds with a width of 6.5 cm and a length of 1.5 cm. The punched out binder films were attached to a UTM (Universal Testing Machine) and then subjected to a tensile test in the horizontal direction. The tensile strength (unit: MPa) measured immediately before breakage was defined as the tensile strength of the binder film.
[0142] The tensile strength of the binder film is shown in Table 3 below.
[0143] [Table 3]
[0144] Referring to Table 3, the binder films of Examples 1A to 3A were evaluated to have high tensile strength while having excellent electrolyte wettability. This is believed to be because the second conductive material acts as a filler in the binder with excellent electrolyte wettability, thereby improving the tensile strength. Therefore, it can be predicted that the output characteristics and life characteristics can be improved simultaneously in the case of the negative electrodes of Examples 1 to 3.
[0145] However, in the case of Comparative Example 1A, both the electrolyte wettability and the tensile strength were evaluated as being poor. On the other hand, the binder films of Comparative Examples 2A to 7A were evaluated as having good electrolyte wettability to some extent, but low tensile strength. In other words, in the case of the negative electrodes used in Comparative Examples 1 to 7, it can be predicted that not only are the output characteristics poor, but also the capacity expression is not performed well during cycle charge and discharge.
[0146] Experimental example 2: Evaluation of output The discharge output characteristics of the secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 7 prepared as above were evaluated.
[0147] The secondary battery was charged and discharged for one cycle under the conditions of charge (1.0C CC / CV charge, 4.2V, 0.05C cut) and discharge (0.5C CC discharge, 3.2V cut), and the discharge capacity was measured. The results are shown in Table 4.
[0148] [Table 4]
[0149] Referring to Table 4, it can be seen that the secondary batteries of Examples 1 to 3, in which the contents of the first conductive material, the second conductive material, and the ratios of the second conductive material and the binder were adjusted to preferred levels, had a conductive network smoothly maintained in the negative electrode, and the wettability and tensile strength of the binder were secured, and thus exhibited excellent initial discharge capacity, compared to Comparative Examples 1 to 7.
[0150] Experimental Example 3: Evaluation of cycle cumulative capacity The cumulative cycle capacity of the secondary batteries of Examples 1 to 3 and Comparative Examples 1 to 7 prepared as above was evaluated.
[0151] The secondary battery was charged and discharged for 200 cycles under the conditions of charge (1.0C CC / CV charge, 4.2V, 0.05C cut) and discharge (0.5C CC discharge, 3.2V cut), and the discharge capacity for each cycle was measured and then added up. The results are shown in Table 5.
[0152] [Table 5]
[0153] Referring to Table 5, it can be seen that the secondary batteries of Examples 1 to 3, in which the contents of the first conductive material, the second conductive material, and the ratios of the second conductive material and the binder are adjusted to preferred levels, have a conductive network in the negative electrode that is smoothly maintained, the wettability and tensile strength of the binder are secured, and the capacity expression of the negative electrode and the secondary battery containing the silicon-based active material during charging and discharging of the cycle is realized at an excellent level, compared to Comparative Examples 1 to 7.
Claims
1. A negative electrode current collector; a negative electrode active material layer disposed on the negative electrode current collector, the negative electrode active material layer includes a silicon-based active material, a first conductive material including graphite, a second conductive material including single-walled carbon nanotubes, and a binder; The binder includes a cellulose-based compound and a rubber-based compound, the first conductive material is included in the negative electrode active material layer in an amount of 15% by weight to 25% by weight; the second conductive material is included in the negative electrode active material layer in an amount of 0.15 wt % to 2.5 wt %; The second conductive material and the binder are contained in the negative electrode active material layer in a weight ratio of 1.5:99.5 to 20.0:80.
0.
2. The negative electrode according to claim 1 , wherein the graphite is in a plate form.
3. The specific surface area of the first conductive material is 5 m 2 / g to 40m 2 The negative electrode according to claim 1 or 2, wherein the anode has a molecular weight of 1 / g.
4. The average particle size (D 50 4. The negative electrode according to claim 1, wherein the thickness of the first electrode is 1 μm to 20 μm.
5. The negative electrode according to any one of claims 1 to 4, wherein the first conductive material has an aspect ratio of 1.1 to 30.
0.
6. The specific surface area of the second conductive material is 400 m 2 / g~1,500m 2 The negative electrode according to claim 1 , wherein the anode mass ratio is 1:1 or more.
7. The negative electrode according to claim 1 , wherein the second conductive material has an average length of 5 μm to 30 μm.
8. The negative electrode according to any one of claims 1 to 7, wherein the second conductive material has an aspect ratio of 5,000 to 15,000.
9. The negative electrode according to claim 1 , wherein the first conductive material and the second conductive material are contained in the negative electrode active material layer in a weight ratio of 0.7:99.3 to 1.5:99.
5.
10. The negative electrode according to claim 1 , wherein the silicon-based active material is contained in the negative electrode active material layer in an amount of 60% by weight to 78% by weight.
11. The negative electrode according to claim 1 , wherein the binder contains the cellulose-based compound and the rubber-based compound in a weight ratio of 5:95 to 80:
20.
12. 12. The negative electrode according to claim 1, wherein the cellulose-based compound comprises at least one selected from the group consisting of carboxymethyl cellulose, methyl cellulose, hydroxypropyl cellulose, methyl hydroxypropyl cellulose, ethyl hydroxyethyl cellulose, methyl ethyl hydroxyethyl cellulose, and cellulose gum.
13. 13. The negative electrode according to claim 1, wherein the rubber-based compound includes at least one selected from the group consisting of styrene-butadiene rubber, acrylic rubber, butyl rubber, and fluororubber.
14. The negative electrode according to claim 1 , wherein the binder is contained in the negative electrode active material layer in an amount of 5% by weight to 20% by weight.
15. The negative electrode according to any one of claims 1 to 14, A positive electrode facing the negative electrode; a separator interposed between the negative electrode and the positive electrode; and an electrolyte.
Citation Information
Patent Citations
Binder for electrode of lithium cell and lithium cell employing the same
JP2013143382A
Electrode active material-carbon nanotube composite and manufacturing method thereof
JP2017084759A
Silicon-carbon composite anodes for lithium-ion batteries
JP2018514067A
Negative electrode active material, mixture negative electrode active material, water type negative electrode slurry composition, and manufacturing method of the negative electrode active material
JP2020077510A
Negative electrode
JP2020087653A