Printing method and printing device
The printing device and method address uneven gloss issues in inkjet systems by using clear ink with optimized interfacial energy to ensure uniform gloss and high-quality image output.
Patent Information
- Application Number
- JP2020154371
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-09-15
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-09-15
AI Technical Summary
Inkjet recording systems face issues with uneven gloss due to pigment particles remaining on the surface of the recording medium, leading to variations in image density and color, resulting in visually perceptible defects like areas with high and low glossiness coexisting within the same image.
A printing device and method that applies color inks with a clear ink containing polymer particles, optimizing interfacial energy to 50 mJ/m² with respect to each color ink layer, ensuring uniform gloss by enhancing the wettability and spreading of the clear ink on the color ink layer.
Achieves excellent gloss uniformity between color ink layers, producing printed matter with consistent gloss and image quality similar to silver halide photography.
Smart Images

Figure 0007571432000027 
Figure 0007571432000028 
Figure 0007571432000029
Abstract
Description
[Technical field]
[0001] The present invention relates to a printing method, and Printing Place Regarding. [Background technology]
[0002] In recent years, in the inkjet recording system, there has been a demand for images having high resolution and high color development, similar to those realized in silver halide photography and offset printing.
[0003] In such inkjet recording methods, aqueous color inks in which pigments as coloring materials and other additives are dispersed in water are generally used. The pigments have a composition similar to that of coloring materials used in general commercial printing inks, and are expected to bring the texture of printed matter closer to that of commercial printing. However, when recording is performed on coated paper for commercial printing or publication printing using aqueous color inks, the coloring materials exist as particles in the solvent, so there is a problem that they do not easily penetrate into the recording medium and the pigments tend to remain on the surface of the recording medium. In such cases, inkjet recording devices often combine four colors of ink: Y (yellow), M (magenta), C (cyan), and K (black) to produce full color; however, the amount of pigment used in the ink varies depending on the image density and color. In addition, printed matter has residual pigment on the surface of the recording medium, which results in differences in surface smoothness depending on the image density and color, resulting in diffuse reflection of light and resulting in uneven gloss.
[0004] Here, the term "uneven gloss" refers to a state in which a printed matter has a mixture of high gloss areas (gloss areas) and low gloss areas (matte areas). When uneven gloss occurs, gloss areas and matte areas are mixed in the same image, and in the case of a photographic image in particular, this is visually recognized as an image defect.
[0005] In order to solve the problem of uneven gloss, attempts have been made to use a substantially colorless and transparent ink (hereinafter sometimes referred to as "clear ink") that does not affect color reproducibility. For example, it has been proposed to improve the gloss of non-printed and low-duty areas of a color ink image by using a clear ink containing a cationic resin and polymer particles with a specific structure (see, for example, Patent Document 1). It has also been proposed to improve gloss by adjusting the dot diameter of the clear ink by controlling the ejection amount of the clear ink (see, for example, Patent Document 2).
[0006] In addition, an inkjet recording method has been proposed in which a high-gloss image quality similar to that of silver halide photography can be obtained by using a combination of a color ink and a clear ink, both of which have high permeability, on a recording medium that has a high surface gloss and low ink permeability (see, for example, Patent Document 3). Summary of the Invention [Problem to be solved by the invention]
[0007] An object of the present invention is to provide a printing apparatus that is excellent in gloss uniformity between color ink layers of each color and can produce printed matter with excellent gloss. [Means for solving the problem]
[0008] The printing apparatus of the present invention as a means for solving the above-mentioned problems includes a color ink applying means for applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer, and a clear ink applying means for applying a clear ink containing at least polymer particles onto the color ink layer, and the clear ink has an interface energy of 50 mJ / m for a solid image of each of the plurality of color inks. 2 The following is the result. Effect of the Invention
[0009] According to the present invention, it is possible to provide a printing apparatus which is excellent in gloss uniformity between color ink layers of each color and can produce printed matter with excellent gloss. [Brief description of the drawings]
[0010] [Figure 1] FIG. 1 is a perspective view illustrating an example of a printing device. [Diagram 2] FIG. 2 is a perspective view illustrating an example of a main tank in a printing apparatus. [Diagram 3] FIG. 3 is a diagram illustrating the interfacial energy of the clear ink with respect to the color ink layer. [Figure 4] FIG. 4 is a diagram illustrating the measurement of the contact angle between a solid and a liquid. [Diagram 5] FIG. 5 is an explanatory diagram of a method for determining the surface free energy of a color ink layer (solid) based on the Fowkes-Owens model. [Figure 6] FIG. 6 is a diagram illustrating a method for measuring the static surface tension of a liquid sample by the Wilhelmy method. [Figure 7] FIG. 7 shows an image including solid images of four colors each used in forming a color image in the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] (Printing method and printing device) The printing apparatus of the present invention has a color ink applying means for applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer, and a clear ink applying means for applying a clear ink containing at least polymer particles onto the color ink layer, and the clear ink has an interface energy of 50 mJ / m for a solid image of each of the plurality of color inks. 2 The following means are included, and other means may be included as necessary.
[0012] The printing method of the present invention includes a color ink applying step of applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer, and a clear ink applying step of applying a clear ink containing at least polymer particles onto the color ink layer, the clear ink having an interfacial energy of 50 mJ / m for each solid image of the plurality of color inks. 2 The process includes the following steps, and may further include other steps as necessary.
[0013] The printing method of the present invention can be suitably carried out by the printing apparatus of the present invention, and the color ink application step can be carried out by a color ink application means, the clear ink application step can be carried out by a clear ink application means, and the other steps can be carried out by other means.
[0014] In the conventional technologies described in the above Patent Document 1 (JP Patent No. 4096158) and Patent Document 2 (JP Patent Publication No. 2004-306557), from the standpoint of ejection stability, a surfactant is used to reduce the surface tension of the clear ink and promote the penetration of the clear ink into the recording medium, but a polymer coating cannot be formed on the surface of the recording medium, and uniform gloss cannot be obtained. Furthermore, in the conventional technology described in the above Patent Document 3 (Patent Publication No. 5509603), the wettability of the clear ink to the color ink layer is not optimized, so that when the clear ink lands on the color ink layer, repelling occurs or the clear ink does not wet and spread, and after drying, the polymer particles contained in the clear ink form fine irregularities, resulting in a printed product with uneven gloss.
[0015] In the present invention, the clear ink has an interface energy of 50 mJ / m for each solid image of the plurality of color inks. 2 less than or equal to 5 mJ / m 2 More than 50mJ / m 2 By adjusting the amount as described below, it is possible to obtain a print having excellent gloss uniformity between the color ink layers, excellent glossiness, and image quality that is close to that of a silver halide photograph. In the present invention, the color ink preferably includes at least a black ink, a yellow ink, a magenta ink, and a cyan ink, and the dispersion component of the surface free energy of the color ink layer of each color formed by the color ink is γ s d The polar component of the surface free energy of each color ink layer is γ s p Then, the dispersion component γ s d The maximum difference is 0.3 mJ / m 2 The polar component γ s p The maximum difference is 5mJ / m 2 By designing as described below, uneven gloss between the color ink layers of each color is eliminated, and a print with excellent uniformity and image quality close to that of a silver halide photograph can be obtained. Furthermore, even if the gloss uniformity between the color ink layers of each color decreases because the type and content of the pigment contained in the color ink varies depending on the image density and color, the clear ink has high wettability to the color ink layers, so the gloss of the image can be significantly improved by applying the clear ink to the color ink layers.
[0016] When discussing the wettability of the clear ink to the color ink layers of each color, the prior art documents adopted the static surface tension and / or dynamic surface tension of the color inks and clear ink in their respective liquid states. However, even if the physical properties of the color inks and / or clear ink in their liquid states were controlled, when images were actually formed, it was not possible to obtain a uniformly glossy image. Therefore, as a result of extensive research, the inventors introduced the concepts of wetting energy and interfacial energy of clear ink with respect to color ink layers of each color, and discovered a printing technology with excellent gloss uniformity based on a new design concept, which led to the creation of the present invention.
[0017] In order for the polymer particles contained in the clear ink to cover the surface of the color ink layer and form a uniform glossy surface, the clear ink must completely wet the surface of the color ink layer. Therefore, the inventors of the present invention have tried to bring the surface free energy of the color ink layer surface and the clear ink droplets closer together, and to set the interface energy as an index, and set this interface energy at 50 mJ / m 2 The following possible combinations of clear ink and color ink layers were thoroughly investigated.
[0018] First, there is Young's equation, shown in the following equation (1), which expresses the wettability of clear ink (liquid) on the surface of a color ink layer (solid).
[0019]
number
[0020] On the other hand, the surface tension of the color ink layer (solid) γ S can be indirectly measured by the two-liquid method based on the Fowkes-Owens model, which measures the contact angle of a solid using two probe liquids whose dispersive and polar components of the surface free energy are known. In the present invention, the two types of probe liquids used were pure water, which has a high polar component in the surface free energy, and methylene iodide, which has a high dispersive component in the surface free energy. Table A below shows the values of each component of the surface free energy of pure water and methylene iodide.
[0021] [Table A]
[0022] Here, the surface free energy of the solid γ S , the surface free energy of the liquid γ L The surface tension of each of these is expressed by the dispersion component γ d and the polar component γ p It can be expressed as the sum of
[0023]
number
[0024] In addition, the surface free energy of the solid, γ S To measure this, the concept of adhesion energy is required based on the Young-Dupre equation (1) above. First, the adhesive energy will be described with reference to FIG. As shown in Figure 3, when a liquid column and a solid column are separated, a liquid surface and a solid surface are created. Since a surface always has surface free energy, the energy in the system after separation is the surface free energy of the liquid, γ L and the surface free energy of the solid γ S It becomes harmony with. The energy that existed in the system before separation was the interfacial energy γ LS Therefore, the interfacial energy between the solid and the liquid, γ LS The adhesive work W required for peeling is the value obtained by subtracting (interfacial energy) aThis relationship is expressed by the Dupre equation, shown below in equation (3). Note that the adhesion energy (peeling energy) explained here is treated as "wetting energy" in the system between a solid surface and a liquid droplet.
[0025]
number
[0026] The above formula (3) is γ LS =γ S +γ L -Wa. Therefore, in FIG. 3, the interfacial energy γ LS The smaller the wetting energy Wa, the better the compatibility between the solid and the liquid. LS becomes smaller. Gamma S is the surface free energy of the color ink, and γ L is the surface free energy of the clear ink. These can be measured. Once the wetting energy Wa is determined, the interfacial energy γ LS can be sought.
[0027] On the other hand, when the substances are solid and liquid, if a droplet reaches equilibrium on the solid surface while maintaining a contact angle θ as shown in Figure 4, the Young's equation shown in the above equation (1) holds true.
[0028] Here, by combining the above Dupre equation (3) and Young equation (1), the value of the wetting energy (adhesion work) Wa can be obtained from the Young-Dupre equation shown in the following equation (4), which is composed of the surface free energy of the liquid and the contact angle θ at which the droplet reaches equilibrium on the solid surface. From this, the smaller the contact angle θ of the clear ink (i.e., the better it wets), the greater the wetting energy Wa.
[0029]
number
[0030] Therefore, from the above formula (4), γ L By calculating cosθ, the wetting energy Wa can be calculated. Surface free energy of liquid γ L For example, the surface free energy (static surface tension) of the clear ink can be measured. The contact angle θ at which the droplet reaches equilibrium on the solid surface can be determined, for example, by forming a solid image (color ink layer) of color ink on a recording medium and measuring the contact angle of the clear ink deposited on the color ink layer with a contact angle meter.
[0031] Here, the wetting energy Wa in the present invention can be obtained by the following method. The color ink image was formed under environmental conditions of 23°C ± 0.5°C and 50 ± 5% RH using an IPSiO GX e5500 (manufactured by Ricoh Co., Ltd.). A monochrome rectangular solid image of 5 cm × 20 cm was printed in advance on Superfine paper (manufactured by Epson Co., Ltd.), which is inkjet paper, with a resolution of 1,200 dpi and an ink deposition amount of 0.96 mg / cm. 2 Print and adjust the amount of ink adhesion by varying the drive voltage of the piezo element so that the ink adhesion amount becomes equal (600 mg / A4 size). At this time, individual settings are made for each color ink so that the ink adhesion amount is the same for each color. The amount of ink adhesion can be found by measuring the mass of the super fine paper before and after printing a rectangular solid image. For the print mode, select "Paper type: Glossy paper," "Print quality: Fine," and "Color matching: None" using the user settings of the driver that comes with the printer. Next, under the above set conditions, coated paper (OK top coat +, basis weight: 127.9 g / m 2 A four-color solid image set was created using Microsoft Word 2016 (Microsoft Corporation) on a paper tray (Oji Paper Co., Ltd.), and the four-color image was printed as a single image at a resolution of 1,200 dpi as shown in Figure 7. The image was then dried for 30 seconds in a thermostatic chamber set to an internal temperature of 90°C. Coated paper (OK topcoat +, basis weight: 127.9g / m 2 The arithmetic average roughness: Ra of a color ink image printed on a paper substrate (manufactured by Oji Paper Co., Ltd.) is 1.50 μm to 1.65 μm. The arithmetic mean roughness Ra was measured using a shape analysis laser microscope (VK-9510, manufactured by Keyence Corporation) at a magnification of 50. The average value of measurements taken at five locations on the same sample was used as the Ra value. The specific measurement conditions were lens magnification: 10x, filter: none, Z measurement pitch: 0.5 μm, and measurement mode: surface shape.
[0032] <Method for determining contact angle θ of clear ink> A method for determining the contact angle θ of the clear ink that has landed on the surface of a color ink image will be described in detail below. Here, using the printing conditions set above, a solid color image of each color created in Microsoft Word 2016 (Microsoft Corporation) is printed, and then clear ink is deposited onto this solid color image, and the contact angle is measured 1,000 ms after deposition. The contact angle was measured using a contact angle meter (DMo-501, manufactured by Kyowa Interface Science Co., Ltd.) This contact angle meter allows droplets of the measurement sample (clear ink) to be deposited on the surface of a color image, and the contact angle of the clear ink can be measured from the image of the deposited droplets. The contact angle is measured in an environment of 25°C. A droplet of the clear ink to be deposited is formed on the tip of the syringe needle, and the amount of the droplet is adjusted to 2.0 μL. The sample stage with the colored ink image on it is gently raised, and the droplet is deposited on the surface of the colored ink image. An image is captured 1,000 ms after the droplet has deposited on the surface of the colored ink image, and the contact angle is calculated using the θ / 2 method using the analysis software "FAMAS (interFAce Measurement & Analysis System)" that comes with the device. Measurements are also performed three or more times, and the average value is taken as the contact angle for that sample.
[0033] <Method to calculate static surface tension of liquid> A method for measuring the static surface tension of a liquid is described in detail below. Here, the static surface tension of the liquid γ L becomes smaller as the temperature of the liquid rises. This is because when the temperature of the liquid rises, the thermal motion of the liquid increases the intermolecular distance, thereby reducing the cohesive energy between the molecules. The measurement conditions for the static surface tension of clear ink are shown below. The static surface tension of clear ink is measured in a 25°C environment using an automatic surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.) in full automatic mode. Detailed measurement conditions are shown in Table B below.
[0034] [Table B]
[0035] A method for measuring the static surface tension of a liquid will now be described in detail. There are several methods for measuring the surface tension of a liquid, including creating a droplet of the sample on the tip of a needle and calculating the surface tension through image analysis from the state of a droplet of the liquid's maximum size (the pendant drop method); the ring method, in which a special ring is immersed in the liquid and the force applied to a balance is measured when the ring is released; and the Wilhelmy method (plate method), in which a platinum plate is immersed in the liquid sample and the force generated in the direction in which the liquid sample tries to pull the plate is measured using a balance weight sensor to calculate the surface tension. In the present invention, an automatic surface tensiometer (DY-300, manufactured by Kyowa Interface Science Co., Ltd.) is used to calculate the static surface tension: γL of a liquid sample by the Wilhelmy method according to the following formula (i).
[0036]
number
[0037] Since most liquids wet the platinum plate sufficiently, it can be assumed that the contact angle θ = 0°, i.e., cos θ = 1, and the surface tension is given by equation (ii) below.
[0038]
number
[0039] As mentioned above, when calculating the surface tension assuming that the contact angle between the platinum plate and the liquid is zero, the platinum plate needs to be completely wet. However, in reality, the platinum plate may not be sufficiently wet, so the platinum plate was immersed once (pre-wet) and then pulled out again. Under environmental conditions of 25°C, 10 mL of each color ink is placed in a 40 mm diameter dish, and after zero point adjustment, the platinum plate (the measuring element) is immersed once in the liquid sample in the dish (pre-wetting), and the series of operations starting from the start of measurement are carried out all automatically (see Figure 6). Static surface tension: γ L The average value of five measurements is used, and after each measurement, the platinum plate is washed with distilled water and then red-heat washed for about 30 seconds to remove any contaminants on the plate surface.
[0040] In the present invention, examples of a method for controlling the numerical range of the wetting energy Wa include adjusting the type of surfactant, the amount of surfactant added, and the mixing ratio of multiple types of surfactants.
[0041] Next, the color inks include at least a black ink, a yellow ink, a magenta ink, and a cyan ink, The dispersion component of the surface free energy of each color ink layer formed by applying the color ink is expressed as γ s d The polar component of the surface free energy of each color ink layer is γ s p Then, the dispersion component γs d The maximum difference is 0.3 mJ / m 2 The polar component γ s p The maximum difference is 5mJ / m 2 It is preferable that: Here, the dispersion component γ of the surface free energy in the color ink layer of each color is S d and the polar component γ S P can be measured as follows:
[0042] The above wetting energy (adhesion work) Wa can be expressed as the root mean square between the solid and liquid, as shown in the following formula (5).
[0043]
number
[0044] Therefore, from the above formula (4) and formula (5), the Young-Dupre formula shown in formula (6) below is obtained.
[0045]
number
[0046] Here, the Young-Dupre equation in the above formula (6) is expressed as 2√γ L d By dividing by this, it can be transformed into the following equation (7).
[0047]
number
[0048] From the above formula (7), the surface free energy γ S This will be described with reference to FIG. First, the two types of probe liquid, namely pure water and methylene iodide, shown in Table A above, are used to measure the contact angle on the color ink layer.
[0049] Next, based on the above formula (7), the dispersion component γ of the surface free energy of the color ink layer is calculated from the intercept of the graph in FIG. S d From the slope of the graph in FIG. 5, the polar component γ S P is obtained. Then, the obtained variance component γ S d and the polar component γ S p The surface free energy γ of the color ink layer is calculated as the sum of S can be sought.
[0050] The clear ink, color ink, and ink set used in the printing apparatus and printing method of the present invention will be described below.
[0051] <Clear ink> Clear ink refers to a colorless, transparent ink that does not substantially contain color materials. Here, "substantially free of color materials" means that the color material content is 0.5% by mass or less, and color materials may be contained on the order of impurities. The clear ink contains at least polymer particles, and preferably contains an organic solvent, water, and a surfactant, and further contains other components as necessary.
[0052] -Polymer particles- The polymer particles used in the color inks are dispersed in a solvent as a polymer emulsion, and may contain a dispersant or the like as necessary. The polymer emulsion is not particularly limited and can be appropriately selected depending on the purpose. Examples of the polymer emulsion include acrylic resins, urethane resins, vinyl acetate resins, styrene resins, butadiene resins, styrene-butadiene resins, vinyl chloride resins, acrylic-styrene resins, and acrylic-silicone resins. The polymer emulsion may be a synthesized one or a commercially available one, and may be used alone or in combination of two or more kinds of resin particles.
[0053] The cumulative 50% volume particle diameter of the polymer particles (D 50 ) is preferably such that no coarse particles of 0.5 μm (=500 nm) or more are observed, more preferably 200 nm or less, and even more preferably 100 nm or less. The lower limit is preferably 30 nm or more, and more preferably 50 nm or more. Cumulative 50% volume particle size (D 50 When the average particle diameter (nm) of the clear ink is 200nm or less, the ejection stability of the clear ink is good. Furthermore, when the polymer particles in the polymer emulsion do not have a crosslinked structure, the polymer particles are fused to each other while the aqueous medium in the clear ink permeates into the recording medium in the film-forming process after the clear ink is applied to the recording medium, and good glossiness is obtained. The cumulative 50% volume particle diameter (D 50 ) is the particle size equivalent to 50% of the cumulative volume distribution in the particle size distribution curve obtained by dynamic light scattering. Specifically, the polymer emulsion can be diluted to a solid content of 0.01% by mass or more and 0.1% by mass or less, and the solid content can be measured using a "Microtrac UPA" (manufactured by Leeds & Northrup).
[0054] The content of the polymer particles in the clear ink [the content of the polymer particles in the clear ink (solid content)] is preferably from 10% by mass to 30% by mass, and more preferably from 10% by mass to 20% by mass. When the content of the polymer particles is 10% by mass or more, gloss can be imparted to the image, and when the content is 30% by mass or less, the ejection stability of the clear ink is good. The content of the polymer particles in the polymer emulsion is not particularly limited and can be appropriately selected depending on the purpose, but is preferably from 10% by mass to 70% by mass.
[0055] -Surfactants- The surfactant content is set so that the interfacial energy of the clear ink against the color ink layer is 50 mJ / m 2 In order to adjust the amount as described below, appropriate adjustments can be made depending on the type of surfactant. The surfactant preferably contains a polyether-modified siloxane compound. By using the polyether-modified siloxane compound as a surfactant, the ink becomes less likely to wet the ink-repellent layer of the nozzle plate of the ink head, preventing ejection defects due to ink adhesion to the nozzles and improving ejection stability. The polyether-modified siloxane compound is preferably at least one selected from the compounds represented by the following general formulas (I) to (IV), in view of not impairing dispersion stability depending on the type of colorant or the combination with the organic solvent, having low dynamic surface tension, penetrability, and leveling property.
[0056] [ka] In the general formula (I), m represents an integer of 0 to 23, and n represents an integer of 1 to 10, a represents an integer of 1 to 23, and b represents an integer of 0 to 23. R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0057] [ka] In the general formula (II), m represents an integer of 1 to 8, and c and d represent integers of 1 to 10. 2 and R 3represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0058] [ka] In the general formula (III), e represents an integer of 1 to 8; 4 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0059] [ka] In the general formula (IV), f represents an integer of 1 to 8. 5 represents a polyether group represented by the following general formula (A). [ka] In the general formula (A), g represents an integer of 0 to 23, and h represents an integer of 0 to 23, and g and h cannot be 0 at the same time. 6 represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
[0060] As the polyether-modified siloxane compound, a compound appropriately synthesized or a commercially available product may be used. The method for synthesizing the polyether-modified siloxane compound is not particularly limited and can be appropriately selected depending on the purpose. For example, the descriptions in Japanese Patent No. 5101598, Japanese Patent No. 5032325, Japanese Patent No. 5661229, etc. can be referenced. Specifically, it can be synthesized by subjecting (A) a polyether and (B) an organohydrogensiloxane to a hydrosilylation reaction.
[0061] The polyether of the component (A) is -(C n H 2n O)-- (wherein, n is 2 to 4). The polyoxyalkylene copolymer units are preferably oxyethylene units -(C2 H 4 O)-, oxypropylene unit -(C 3 H 6 O)-, oxybutylene unit-(C 4 H 8 O)-, or a mixture thereof. The oxyalkylene units may be arranged in any manner to form either block or random copolymer structures, but preferably form a random copolymer group. More preferably, the polyoxyalkylene contains oxyethylene units (C 2 H 4 O) and oxypropylene units (C 3 H 6 O) in a random copolymer.
[0062] The organohydrogensiloxane of component (B) is an organopolysiloxane that contains at least one silicon-bonded hydrogen (SiH) per molecule. The organopolysiloxane may be, for example, 3 SiO 0.5 ), (R 2 SiO), (RSiO 1.5 ), (SiO 2 ) (wherein R is independently an organic group or a hydrocarbon group), any number or combination of siloxy units may be used. (R 3 SiO 0.5 ), (R 2 SiO), (RSiO 1.5 When R in (SiO 2 ) Siloxy units are designated as Q units. The organohydrogensiloxanes have a similar structure, but have at least one SiH present on the siloxy unit. The methyl-based siloxy unit in the organohydrogensiloxane is represented by "M H " Siloxy unit (R2 HSiO 0.5 ), "D H " Siloxy unit (RHSiO), "T H " Siloxy unit (HSiO 1.5 ) can be shown to include The organohydrogensiloxane may be any number of M, ... H , D, D H , T, T H , or Q siloxy units.
[0063] The component (A) and the component (B) are reacted by a hydrosilylation reaction. The hydrosilylation reaction is not particularly limited and may be appropriately selected depending on the purpose, but is preferably carried out in the presence of a hydrosilylation catalyst. The hydrosilylation catalyst is not particularly limited and can be appropriately selected depending on the purpose. Examples of the hydrosilylation catalyst include platinum, rhodium, ruthenium, palladium, osmium, and iridium metals, organometallic compounds thereof, and combinations of these. The content of the hydrosilylation catalyst is preferably 0.1 ppm or more and 1,000 ppm or less, and more preferably 1 ppm or more and 100 ppm or less, based on the mass of the components (A) and (B). The hydrosilylation reaction can be carried out neat or in the presence of a solvent, but is preferably carried out in the presence of a solvent.
[0064] Examples of the solvent include alcohols (e.g., methanol, ethanol, isopropanol, butanol, or n-propanol), ketones (e.g., acetone, methyl ethyl ketone, or methyl isobutyl ketone); aromatic hydrocarbons (e.g., benzene, toluene, or xylene); aliphatic hydrocarbons (e.g., heptane, hexane, or octane); glycol ethers (e.g., propylene glycol methyl ether, dipropylene glycol methyl ether, propylene glycol n-butyl ether, propylene glycol n-propyl ether, or ethylene glycol n-butyl ether), halogenated hydrocarbons (e.g., dichloromethane, 1,1,1-trichloroethane, methylene chloride, chloroform), dimethyl sulfoxide, dimethylformamide, acetonitrile, tetrahydrofuran, volatile oil, mineral spirits, or naphtha. These may be used alone or in combination of two or more.
[0065] The amounts of the component (A) and the component (B) used in the hydrosilylation reaction are not particularly limited and can be appropriately adjusted depending on the purpose, and are expressed as the molar ratio of the total unsaturated groups in the component (A) to the SiH content in the component (B). It is preferable to use a polyether unsaturated group amount of 20 mol % or less, and more preferably 10 mol % or less, based on the molar amount of SiH in the organohydrogensiloxane. The hydrosilylation reaction is not particularly limited and can be carried out in any known batch, semi-continuous, or continuous manner, for example, in a continuous manner using a plug flow reactor.
[0066] Examples of commercially available polyether-modified siloxane compounds include 71ADDITIVE, 74ADDITIVE, 57ADDITIVE, 8029ADDITIVE, 8054ADDITIVE, 8211ADDITIVE, 8019ADDITIVE, 8526ADDITIVE, FZ-2123, and FZ-2191 (all manufactured by TORAY Dow Corning Co., Ltd.); TSF4440, TSF4441, TSF4445, TSF4446, TSF4450, TSF4452, and TSF4460 (all manufactured by Momentive Performance Materials Co., Ltd.); Silface SAG002, Silface SAG003, Silface SAG005, Silface SAG503A, Silface SAG008, and Silface SJM003 (all manufactured by Nissin Chemical Industry Co., Ltd.); TEGO Wet KL245, TEGO Wet 250, TEGO Wet 260, TEGO Wet 265, TEGO Wet 270, TEGO Wet 280 (all manufactured by Evonik); BYK-345, BYK-347, BYK-348, BYK-375, BYK-377 (all manufactured by BYK Japan). These may be used alone or in combination of two or more. Among these, TEGO Wet 270 (manufactured by Evonik) and Silface SAG503A (manufactured by Nissin Chemical Industry Co., Ltd.) are preferred.
[0067] As the surfactant, in addition to the polyether-modified siloxane compound, a fluorine-based surfactant, a silicone-based surfactant, an acetylene glycol-based or acetylene alcohol-based surfactant, or the like may be used in combination.
[0068] The silicone surfactant is not particularly limited and can be appropriately selected according to the purpose. Among them, those that do not decompose even at high pH are preferable. Examples of silicone surfactants include side chain modified polydimethylsiloxane, both end modified polydimethylsiloxane, one end modified polydimethylsiloxane, and both end modified polydimethylsiloxane of side chain. Those having a polyoxyethylene group or a polyoxyethylene polyoxypropylene group as a modified group are particularly preferable because they show good properties as an aqueous surfactant. In addition, polyether modified silicone surfactants can also be used as silicone surfactants, and examples thereof include compounds in which a polyalkylene oxide structure is introduced into the Si part side chain of dimethylsiloxane.
[0069] As the fluorosurfactant, for example, perfluoroalkylsulfonic acid compounds, perfluoroalkyl carboxylic acid compounds, perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain are particularly preferred because they have low foaming properties. As the perfluoroalkylsulfonic acid compounds, for example, perfluoroalkylsulfonic acid, perfluoroalkyl sulfonate, etc. are included. As the perfluoroalkyl carboxylic acid compounds, for example, perfluoroalkyl carboxylic acid, perfluoroalkyl carboxylate, etc. are included. As the polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups on the side chain, for example, sulfate ester salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups on the side chains, salts of polyoxyalkylene ether polymers having perfluoroalkyl ether groups on the side chains, etc. are included. As the counter ions of the salts in these fluorosurfactants, Li, Na, K, NH 4 , N.H. 3 CH 2 CH 2 OH, NH 2 (CH 2 CH 2 OH) 2 , NH(CH 2 CH2 OH) 3 etc.
[0070] Examples of amphoteric surfactants include lauryl aminopropionate, lauryl dimethyl betaine, stearyl dimethyl betaine, and lauryl dihydroxyethyl betaine.
[0071] Examples of nonionic surfactants include polyoxyethylene alkylphenyl ethers, polyoxyethylene alkyl esters, polyoxyethylene alkylamines, polyoxyethylene alkylamides, polyoxyethylene propylene block polymers, sorbitan fatty acid esters, polyoxyethylene sorbitan fatty acid esters, and ethylene oxide adducts of acetylene alcohol.
[0072] Examples of the anionic surfactant include polyoxyethylene alkyl ether acetates, dodecylbenzene sulfonates, laurates, and polyoxyethylene alkyl ether sulfates. These may be used alone or in combination of two or more. Among these, fluorine-based surfactants are preferred.
[0073] As the fluorine-based surfactant, a compound having 2 to 16 fluorine-substituted carbon atoms is preferable, and a compound having 4 to 16 fluorine-substituted carbon atoms is more preferable. Examples of fluorine-based surfactants include perfluoroalkyl phosphate compounds, perfluoroalkyl ethylene oxide adducts, and polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in side chains, etc. Among these, polyoxyalkylene ether polymer compounds having perfluoroalkyl ether groups in side chains are preferred because they have low foaming properties, and fluorine-based surfactants represented by general formula (F-1) and general formula (F-2) are particularly preferred.
[0074] [General formula (F-1)] [ka] In the compound represented by the above general formula (F-1), m is preferably an integer of 0 to 10, and n is preferably an integer of 0 to 40 in order to impart water solubility.
[0075] [General formula (F-2)] C n F 2n+1- CH 2 CH(OH)CH 2 -O-(CH 2 CH 2 O) a -Y In the compound represented by the above general formula (F-2), Y is H or C m F 2m+1 m is an integer from 1 to 6, or CH 2 CH(OH)CH 2 -C m F 2m+1 where m is an integer between 4 and 6, or CpH 2p+1 where p is an integer from 1 to 19. n is an integer from 1 to 6. a is an integer from 4 to 14.
[0076] The fluorine-based surfactant may be a commercially available product, such as Surflon S-111, S-112, S-113, S-121, S-131, S-132, S-141, S-145 (all manufactured by Asahi Glass Co., Ltd.); Fullard FC-93, FC-95, FC-98, FC-129, FC-135, FC-170C, FC-430, FC-431 (all manufactured by Sumitomo 3M Limited); Megafac F-470, F-1405, F-474 (all manufactured by DIC Corporation); Zonyl TBS, FSP, FSA, FSN-100. , FSN, FSO-100, FSO, FS-300, UR, Capstone FS-30, FS-31, FS-3100, FS-34, FS-35 (all manufactured by Chemours); FT-110, FT-250, FT-251, FT-400S, FT-150, FT-400SW (all manufactured by Neos Co., Ltd.), Polyfox PF-136A, PF-156A, PF-151N, PF-154, PF-159 (manufactured by Omnova), Unidyne DSN-403N (manufactured by Daikin Industries, Ltd.), and the like. Among these, FS-3100, FS-34, and FS-300 manufactured by Chemours Corporation, FT-110, FT-250, FT-251, FT-400S, FT-150, and FT-400SW manufactured by Neos Co., Ltd., Polyfox PF-151N manufactured by Omnova, and Unidyne DSN-403N manufactured by Daikin Industries, Ltd. are particularly preferred, as they provide good printing quality, particularly improved color development, penetration into paper, wettability, and dye uniformity.
[0077] The content of the surfactant in the clear ink is not particularly limited and can be selected as appropriate depending on the purpose; however, from the viewpoints of achieving excellent wettability and ejection stability and improving image quality, the content is preferably from 0.001% by mass to 5% by mass, and more preferably from 0.05% by mass to 5% by mass.
[0078] -Organic solvents- The organic solvent used in the present invention is not particularly limited, and any water-soluble organic solvent can be used. Examples of the organic solvent include ethers such as polyhydric alcohols, polyhydric alcohol alkyl ethers, and polyhydric alcohol aryl ethers, nitrogen-containing heterocyclic compounds, amides, amines, and sulfur-containing compounds. Examples of polyhydric alcohols include ethylene glycol, diethylene glycol, 1,2-propanediol, 1,3-propanediol, 1,2-butanediol, 1,3-butanediol, 1,4-butanediol, 2,3-butanediol, 3-methyl-1,3-butanediol, triethylene glycol, polyethylene glycol, polypropylene glycol, 1,2-pentanediol, 1,3-pentanediol, 1,4-pentanediol, Examples of such glycerol include 2,4-pentanediol, 1,5-pentanediol, 1,2-hexanediol, 1,6-hexanediol, 1,3-hexanediol, 2,5-hexanediol, 1,5-hexanediol, glycerin, 1,2,6-hexanetriol, 2-ethyl-1,3-hexanediol, ethyl-1,2,4-butanetriol, 1,2,3-butanetriol, 2,2,4-trimethyl-1,3-pentanediol, and petriol. Examples of polyhydric alcohol alkyl ethers include ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether. Examples of polyhydric alcohol aryl ethers include ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether. Examples of the nitrogen-containing heterocyclic compound include 2-pyrrolidone, N-methyl-2-pyrrolidone, N-hydroxyethyl-2-pyrrolidone, 1,3-dimethyl-2-imidazolidinone, ε-caprolactam, and γ-butyrolactone. Examples of amides include formamide, N-methylformamide, N,N-dimethylformamide, 3-methoxy-N,N-dimethylpropionamide, and 3-butoxy-N,N-dimethylpropionamide. Examples of the amines include monoethanolamine, diethanolamine, and triethylamine. Examples of sulfur-containing compounds include dimethyl sulfoxide, sulfolane, and thiodiethanol. Other organic solvents include, for example, propylene carbonate, ethylene carbonate, and the like. It is preferable to use an organic solvent having a boiling point of 250° C. or less, since this not only functions as a wetting agent but also provides good drying properties.
[0079] As the organic solvent, polyol compounds having 8 or more carbon atoms and glycol ether compounds are also suitably used. Specific examples of polyol compounds having 8 or more carbon atoms include 2-ethyl-1,3-hexanediol and 2,2,4-trimethyl-1,3-pentanediol. Specific examples of the glycol ether compound include polyhydric alcohol alkyl ethers such as ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monobutyl ether, tetraethylene glycol monomethyl ether, and propylene glycol monoethyl ether; and polyhydric alcohol aryl ethers such as ethylene glycol monophenyl ether and ethylene glycol monobenzyl ether.
[0080] Polyol compounds having 8 or more carbon atoms and glycol ether compounds can improve the permeability of ink when paper is used as the recording medium.
[0081] The content of the organic solvent in the clear ink is not particularly limited and can be selected appropriately depending on the purpose. From the viewpoints of the drying property and ejection reliability of the clear ink, however, the content is preferably from 10% by mass to 60% by mass, and more preferably from 20% by mass to 60% by mass.
[0082] -water- The water is not particularly limited and can be appropriately selected depending on the purpose. Examples of the water include pure water such as ion-exchanged water, ultrafiltered water, reverse osmosis water, and distilled water, and ultrapure water. The water content in the ink is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of the drying property and ejection reliability of the ink, however, it is preferably from 10% by mass to 90% by mass, and more preferably from 20% by mass to 60% by mass.
[0083] -Other ingredients- The other components are not particularly limited and may be appropriately selected as necessary. Examples of the other components include antifoaming agents, pH adjusters, antiseptic and antifungal agents, and rust inhibitors.
[0084] --Antifoaming agent-- The defoaming agent is not particularly limited, and examples thereof include silicone-based defoaming agents, polyether-based defoaming agents, and fatty acid ester-based defoaming agents. These may be used alone or in combination of two or more. Among these, silicone-based defoaming agents are preferred because of their excellent foam breaking effect. As the defoaming agent, a compound represented by the following general formula (a) is preferably used.
[0085] [ka] In the above general formula (a), R 4 and R 5 are independently alkyl groups having 3 to 6 carbon atoms, R 6 and R 7 are independently an alkyl group having 1 to 2 carbon atoms, and n is an integer of 1 to 6.
[0086] Examples of the compound represented by the general formula (a) include 2,4,7,9-tetramethyldecane-4,7-diol and 2,5,8,11-tetramethyldodecane-5,8-diol. Among these, 2,5,8,11-tetramethyldodecane-5,8-diol is preferred because of its high defoaming effect and compatibility with the clear ink. The content of the defoaming agent is preferably from 0.01% by mass to 10% by mass, and more preferably from 0.1% by mass to 5% by mass, based on the total amount of the clear ink.
[0087] --Preservative and fungicidal agent-- The antiseptic and antifungal agent is not particularly limited, and examples thereof include 1,2-benzisothiazolin-3-one.
[0088] --Rust inhibitor-- The rust inhibitor is not particularly limited, and examples thereof include acid sulfite and sodium thiosulfate.
[0089] --pH adjuster-- There are no particular limitations on the pH adjuster, so long as it is capable of adjusting the pH to 7 or higher, and examples of the pH adjuster include amines such as diethanolamine and triethanolamine.
[0090] <Clear ink manufacturing method> The clear ink is produced by dispersing or dissolving the organic solvent, the polymer particles, and the surfactant, and further the other components as required, in water, and stirring and mixing them. The stirring and mixing can be carried out by using, for example, a sand mill, a homogenizer, a ball mill, a paint shaker, an ultrasonic disperser, a stirrer using a stirring blade, a magnetic stirrer, a high-speed disperser, or the like.
[0091] -Clear ink properties- The physical properties of the clear ink are not particularly limited and can be appropriately selected depending on the purpose. For example, it is preferable that the viscosity, surface tension, pH, etc. are within the following ranges. The viscosity of the clear ink at 25°C is preferably from 5 mPa·s to 30 mPa·s, more preferably from 5 mPa·s to 25 mPa·s, in order to improve print density and character quality and to obtain good ejection properties. Here, the viscosity can be measured using, for example, a rotational viscometer (RE-80L, manufactured by Toki Sangyo Co., Ltd.). The measurement conditions are 25°C, a standard cone rotor (1°34' x R24), a sample liquid volume of 1.2 mL, a rotation speed of 50 rpm, and 3 minutes. The surface tension of the clear ink is preferably 35 mN / m or less, and more preferably 32 mN / m or less at 25° C., in order to ensure that the ink is appropriately leveled on the recording medium and the drying time of the ink is shortened. The pH of the clear ink is preferably from 7 to 12, and more preferably from 8 to 11, from the viewpoint of preventing corrosion of metal members that come into contact with the ink.
[0092] <Color ink> The color ink contains at least one coloring material, and preferably contains an organic solvent, water, a surfactant, and polymer particles, and further contains other components as necessary.
[0093] -Coloring materials- The coloring material is not particularly limited, and pigments and dyes can be used. As the pigment, an inorganic pigment or an organic pigment can be used. These can be used alone or in combination of two or more. Also, mixed crystals can be used as the pigment. Examples of pigments that can be used include black pigments, yellow pigments, magenta pigments, cyan pigments, white pigments, green pigments, orange pigments, glossy pigments such as gold and silver pigments, and metallic pigments. As inorganic pigments, titanium oxide, iron oxide, calcium carbonate, barium sulfate, aluminum hydroxide, barium yellow, cadmium red, chrome yellow, as well as carbon black produced by known methods such as the contact method, furnace method, and thermal method can be used. As organic pigments, azo pigments, polycyclic pigments (e.g., phthalocyanine pigments, perylene pigments, perinone pigments, anthraquinone pigments, quinacridone pigments, dioxazine pigments, indigo pigments, thioindigo pigments, isoindolinone pigments, quinophthalone pigments, etc.), dye chelates (e.g., basic dye chelates, acid dye chelates, etc.), nitro pigments, nitroso pigments, aniline black, etc. can be used. Among these pigments, those having good affinity with the solvent are preferably used. In addition, resin hollow particles and inorganic hollow particles can also be used. Specific examples of pigments for black colors include carbon blacks (CI Pigment Black 7) such as furnace black, lamp black, acetylene black, and channel black; metals such as copper, iron (CI Pigment Black 11), and titanium oxide; and organic pigments such as aniline black (CI Pigment Black 1). In addition, for color, CI Pigment Yellow 1, 3, 12, 13, 14, 17, 24, 34, 35, 37, 42 (yellow iron oxide), 53, 55, 74, 81, 83, 95, 97, 98, 100, 101, 104, 108, 109, 110, 117, 120, 138, 150, 153, 155, 180, 185, 213, CI Pigment Orange Range 5, 13, 16, 17, 36, 43, 51, CI Pigment Red 1, 2, 3, 5, 17, 22, 23, 31, 38, 48:2 (Permanent Red 2B (Ca)), 48:3, 48:4, 49:1, 52:2, 53:1, 57:1 (Brilliant Carmine 6B), 60:1, 63:1, 63:2, 64:1, 81, 83, 88, 101 ( Red iron oxide), 104, 105, 106, 108 (Cadmium Red), 112, 114, 122 (Quinacridone Magenta), 123, 146, 149, 166, 168, 170, 172, 177, 178, 179, 184, 185, 190, 193, 202, 207, 208, 209, 213, 219, 224, 254, 264, CI Pigment Examples of pigments include CI Pigment Green 1, 4, 7, 8, 10, 17, 18, and 36.
[0094] The dye is not particularly limited, and acid dyes, direct dyes, reactive dyes, and basic dyes can be used. One type of dye may be used alone, or two or more types may be used in combination. Dyes such as CI Acid Yellow 17, 23, 42, 44, 79, 142, CI Acid Red 52, 80, 82, 249, 254, 289, CI Acid Blue 9, 45, 249, CI Acid Black 1, 2, 24, 94, CI Food Black 1, 2, CI Direct Yellow 1, 12, 24, 33, 50, 55, 58, 86, 132, 142, 144, 1 73, CI Direct Red 1, 4, 9, 80, 81, 225, 227, CI Direct Blue 1, 2, 15, 71, 86, 87, 98, 165, 199, 202, CI Directed Black 19, 38, 51, 71, 154, 168, 171, 195, CI Reactive Red 14, 32, 55, 79, 249, CI Reactive Black 3, 4, 35, etc.
[0095] The content of the color material in the color ink is preferably from 0.1% by mass to 15% by mass, and more preferably from 1% by mass to 10% by mass, from the viewpoints of improving image density, good fixing property, and ejection stability.
[0096] Methods for dispersing a pigment to obtain an ink include a method in which a hydrophilic functional group is introduced into the pigment to make it a self-dispersing pigment, a method in which the surface of the pigment is coated with a resin and then dispersed, and a method in which a dispersant is used to disperse the pigment. An example of a method for introducing a hydrophilic functional group into a pigment to make it a self-dispersing pigment is a method in which a functional group such as a sulfone group or a carboxyl group is added to a pigment (e.g., carbon) to make it dispersible in water. As a method for dispersing a pigment by coating its surface with a resin, there is a method in which the pigment is encapsulated in a microcapsule to make it dispersible in water. This can be called a resin-coated pigment. In this case, it is not necessary for all of the pigments blended in the ink to be coated with a resin, and uncoated or partially coated pigments may be dispersed in the ink as long as the effect of the present invention is not impaired. Examples of the method for dispersing using a dispersant include a method for dispersing using a known low molecular weight dispersant or a polymeric dispersant, typified by a surfactant. As the dispersant, for example, anionic surfactants, cationic surfactants, amphoteric surfactants, nonionic surfactants, etc. can be used depending on the pigment. As the dispersant, RT-100 (nonionic surfactant) manufactured by Takemoto Oil Co., Ltd. and sodium naphthalenesulfonate formalin condensate can also be suitably used. The dispersants may be used alone or in combination of two or more.
[0097] -Pigment dispersion- It is possible to obtain ink by mixing a pigment with materials such as water or an organic solvent, or it is also possible to manufacture ink by mixing a pigment with other materials such as water and a dispersant to prepare a pigment dispersion, and then mixing the resulting mixture with materials such as water or an organic solvent. The pigment dispersion is obtained by mixing and dispersing water, a pigment, a pigment dispersant, and other components as required, and adjusting the particle size. Dispersion is preferably performed using a dispersing machine. Cumulative 50% volume particle size of pigment in pigment dispersion (D 50 The thickness is not particularly limited and can be appropriately selected depending on the purpose, but is preferably 200 nm or less, more preferably 150 nm or less, in terms of improving the dispersion stability of the pigment and improving the image quality such as ejection stability and image density. The lower limit is preferably 10 nm or more, more preferably 50 nm or more. The cumulative 50% volume particle diameter of the pigment (D 50 ) can be measured, for example, using a particle size distribution measuring device (Nanotrac UPA-EX150, manufactured by Nikkiso Co., Ltd.). The pigment content in the pigment dispersion is not particularly limited and can be appropriately selected depending on the purpose. From the viewpoints of obtaining good ejection stability and increasing image density, the pigment content is preferably from 0.1% by mass to 50% by mass, and more preferably from 0.1% by mass to 30% by mass. It is preferable to filter out coarse particles from the pigment dispersion using a filter or a centrifugal separator, and degas the pigment dispersion, if necessary.
[0098] -Polymer particles- The type of polymer particles, cumulative 50% volume particle size, etc. are the same as those of the polymer particles in the clear ink. The content of the polymer particles is preferably from 0.5% by mass to 10% by mass, and more preferably from 1% by mass to 8% by mass, in terms of solid content, with respect to the total amount of the color ink.
[0099] The water, surfactants, organic solvents, and other components in the color inks are similar to the water, surfactants, organic solvents, and other components in the clear ink described above, and therefore a description thereof will be omitted.
[0100] (Ink set) The ink set of the present invention comprises color inks containing at least one coloring material and a clear ink containing at least polymer particles, and the clear ink has an interfacial energy of 50 mJ / m with respect to a color ink layer formed by the color inks. 2 The following is the result. The ink set includes a plurality of color inks, that is, inks of two or more colors having coloring materials, and preferably includes four colors: yellow, magenta, cyan, and black.
[0101] The color inks preferably include at least one type of ink selected from cyan ink, magenta ink, yellow ink, and black ink. The color inks constituting the ink set may be a plurality of inks each having the same hue as the above-mentioned color inks but each having a different pigment content. The combination of the plurality of inks may include, but is not limited to, inks having a black hue, such as black, light black, gray, and light gray.
[0102] <Pretreatment solution> The pretreatment liquid contains a flocculant, an organic solvent, and water, and may contain, as necessary, a surfactant, an antifoaming agent, a pH adjuster, an antiseptic / fungal agent, an antirust agent, and the like. The organic solvent, surfactant, defoamer, pH adjuster, antiseptic / fungal agent, and rust inhibitor may be the same as those used in ink, and other materials used in known treatment liquids may be used. The type of the flocculant is not particularly limited, and examples thereof include water-soluble cationic polymers, acids, and polyvalent metal salts.
[0103] <Post-processing solution> The post-treatment liquid is not particularly limited as long as it can form a transparent layer. The post-treatment liquid is obtained by selecting and mixing organic solvents, water, resins, surfactants, defoamers, pH adjusters, antiseptics, antifungals, rust inhibitors, etc. as necessary. The post-treatment liquid may be applied to the entire recording area formed on the recording medium, or may be applied only to the area where the ink image is formed.
[0104] <Recording Media> There are no particular limitations on the recording medium, and although plain paper, glossy paper, special paper, cloth, etc. can be used, good image formation is also possible using a non-permeable substrate. A non-permeable substrate is a substrate with a surface that has low water permeability and absorbency. It also includes materials that have many cavities inside but are not open to the outside. More quantitatively, in the Bristow method, 1 / 2 Water absorption up to 10mL / m 2 The term "substrate" refers to a substrate that is: As the impermeable substrate, for example, a plastic film such as a polyvinyl chloride resin film, a polyethylene terephthalate (PET) film, a polypropylene film, a polyethylene film, or a polycarbonate film can be suitably used.
[0105] The recording medium is not limited to those generally used as recording media, and may be wallpaper, flooring, building materials such as tiles, cloth for clothing such as T-shirts, textiles, leather, etc. By adjusting the configuration of the path for conveying the recording medium, ceramics, glass, metal, etc. may also be used.
[0106] <Printed material> The printed matter of the present invention is formed by forming a color ink layer on a recording medium and then forming a clear ink layer on the color ink layer. The arithmetic mean roughness R of the printed matter a is preferably 1.8 μm or less, and more preferably 0.5 μm or more and 1.5 μm or less. The arithmetic mean roughness R a is a value measured using a shape analysis laser microscope (VK-9510, manufactured by Keyence Corporation), and five areas of 100 μm × 100 μm are arbitrarily selected within the image area. The specific measurement conditions are: lens magnification: 10x, filter: none, Z measurement pitch: 0.5 μm, measurement mode: surface shape.
[0107] The maximum difference in color gloss between each printed matter formed using each ink of the ink set is preferably 10 or less, more preferably 7 or less, even more preferably 5 or less, and particularly preferably 3 or less. The inter-color gloss difference can be determined by measuring the 60° gloss of each printed matter formed using each ink of the ink set, and determining the value at which the gloss difference between each printed matter is maximum.
[0108] <Ink cartridges> The ink cartridge used in the present invention contains ink in a container, and further contains other members appropriately selected as necessary. The container is not particularly limited, and the shape, structure, size, material, etc. can be appropriately selected depending on the purpose.
[0109] <Printing method, printing device> The printing apparatus of the present invention has a color ink applying unit and a clear ink applying unit, and further has other units as required.
[0110] The printing method of the present invention includes a color ink applying step and a clear ink applying step, and may further include other steps as necessary.
[0111] -Color ink application process and color ink application means- The color ink applying step is a step of applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer, and is carried out by a color ink applying unit. The color ink applying means is not particularly limited, and examples thereof include an inkjet head. It is preferable that at least a part of the liquid chamber, the fluid resistance portion, the vibration plate, and the nozzle member of the inkjet head is formed from a material containing at least one of silicon and nickel. The nozzle diameter of the inkjet nozzle is preferably 30 μm or less, and more preferably from 1 μm to 20 μm.
[0112] -Clear ink application process and clear ink application means- The clear ink applying step is a step of applying a clear ink containing at least polymer particles onto the color ink layer, and is carried out by a clear ink applying unit. The clear ink applying means is not particularly limited, and examples thereof include an inkjet head.
[0113] The manner in which the ink is ejected is not particularly limited and varies depending on the type of the stimulus. For example, when the stimulus is "heat", thermal energy corresponding to a recording signal is applied to the ink in the recording head using, for example, a thermal head, and the thermal energy generates bubbles in the ink, and the pressure of the bubbles causes the ink to be ejected as droplets from the nozzle holes of the recording head. When the stimulus is "pressure", for example, a voltage is applied to a piezoelectric element attached to a position called a pressure chamber in an ink flow path in a recording head, causing the piezoelectric element to bend and the volume of the pressure chamber to decrease, thereby ejecting the ink as droplets from the nozzle hole of the recording head.
[0114] <Recording device and recording method> The color ink and clear ink used in the present invention can be suitably used in various recording devices using the inkjet recording method, such as printers, facsimile machines, copying machines, printer / fax / copier combination machines, and three-dimensional modeling devices. In the present invention, the recording apparatus and recording method refer to an apparatus capable of ejecting ink, various treatment liquids, etc. onto a recording medium, and a method of recording using the apparatus. The recording medium refers to an object onto which ink or various treatment liquids can be attached even temporarily. This recording device can include not only a head portion that ejects ink, but also means related to feeding, transporting, and discharging the recording medium, as well as other devices called pre-processing devices and post-processing devices. The recording apparatus and the recording method may have a heating means used in the heating step and a drying means used in the drying step. The heating means and the drying means include, for example, a means for heating and drying the printed surface and the back surface of the recording medium. The heating means and the drying means are not particularly limited, but for example, a hot air heater or an infrared heater can be used. Heating and drying can be performed before, during, or after printing. In addition, the recording device and recording method are not limited to those that visualize meaningful images such as characters and figures with ink. For example, those that form patterns such as geometric designs and those that create three-dimensional images are also included. Furthermore, unless otherwise specified, the recording apparatus includes both a serial type apparatus in which the ejection head moves and a line type apparatus in which the ejection head does not move. Furthermore, this recording device includes not only desktop types, but also wide-width recording devices capable of printing on A0-sized recording media, and continuous-feed printers that can use continuous paper wound into a roll as a recording medium.
[0115] An example of a recording device will be described with reference to Figs. 1 and 2. Fig. 1 is a perspective view of the device. Fig. 2 is a perspective view of a main tank. An image forming device 400 as an example of a recording device is a serial type image forming device. A mechanism unit 420 is provided inside an exterior 401 of the image forming device 400. Each ink storage unit 411 of the main tanks 410 (410k, 410c, 410m, 410y) for each color of black (K), cyan (C), magenta (M), and yellow (Y) is formed of a packaging material such as an aluminum laminate film. The ink storage unit 411 is stored in a storage container case 414 made of plastic, for example. As a result, the main tanks 410 are used as ink cartridges of each color. In the present invention, a clear ink is used in addition to the four types of ink described above. When the clear ink is added, a liquid storage unit having the clear ink and a liquid ejection head are added to the recording device. On the other hand, a cartridge holder 404 is provided at the back side of the opening when the cover 401c of the apparatus body is opened. A main tank 410 is detachably attached to the cartridge holder 404. As a result, each ink outlet 413 of the main tank 410 communicates with an ejection head 434 for each color via a supply tube 436 for each color, and ink can be ejected from the ejection head 434 to a recording medium.
[0116] This recording apparatus can include not only a portion that ejects ink, but also devices called pre-processing devices and post-processing devices. As an embodiment of the pre-treatment device and post-treatment device, a liquid storage section having a pre-treatment liquid and a liquid ejection head, similar to the case of inks such as black (K), cyan (C), magenta (M), and yellow (Y), and the like, are added, and the pre-treatment liquid and the post-treatment liquid are ejected by an inkjet recording method. As another embodiment of the pre-treatment device and the post-treatment device, there is an embodiment in which a pre-treatment device and a post-treatment device using a method other than the inkjet recording method, for example, a blade coating method, a roll coating method, or a spray coating method, are provided.
[0117] The uses of the color ink, clear ink, and ink set of the present invention are not particularly limited and can be appropriately selected according to the purpose, and can be applied to, for example, printed matter, paint, coating material, undercoat, etc. Furthermore, they can be used not only as inks to form two-dimensional characters and images, but also as materials for three-dimensional modeling to form three-dimensional solid images (three-dimensional objects). A known three-dimensional modeling device for forming a three-dimensional object can be used, and is not particularly limited. For example, a device equipped with an ink storage means, supply means, discharge means, drying means, etc. can be used. The three-dimensional object includes a three-dimensional object obtained by applying ink over and over. Also included is a molded product obtained by processing a structure to which ink is applied on a substrate such as a recording medium. The molded product is, for example, a recording material or structure formed in a sheet or film form, which is molded by heat stretching, punching, etc., and is preferably used for applications in which the surface is molded after decoration, such as meters and operation panel of automobiles, office automation equipment, electric and electronic equipment, cameras, etc.
[0118] In the present invention, the terms image formation, recording, printing, printing, etc. are all synonymous. Recording medium, media, and printed material are all synonymous. EXAMPLES
[0119] Examples of the present invention will be described below, but the present invention is not limited to these examples.
[0120] (Pigment Dispersion Preparation Example 1) <Preparation of Resin-Coated Black Pigment Dispersion> -Synthesis of polymer solution A- A 1 L flask equipped with a mechanical stirrer, a thermometer, a nitrogen gas inlet tube, a reflux condenser, and a dropping funnel was thoroughly purged with nitrogen gas, and then 11.2 g of styrene, 2.8 g of acrylic acid, 12.0 g of lauryl methacrylate, 4.0 g of polyethylene glycol methacrylate, 4.0 g of styrene macromer, and 0.4 g of mercaptoethanol were mixed and heated to 65°C. Next, a mixed solution of 100.8g of styrene, 25.2g of acrylic acid, 108.0g of lauryl methacrylate, 36.0g of polyethylene glycol methacrylate, 60.0g of hydroxylethyl methacrylate, 36.0g of styrene macromer, 3.6g of mercaptoethanol, 2.4g of azobismethylvaleronitrile, and 18g of methyl ethyl ketone was dropped into the flask over 2.5 hours. After the dropwise addition, a mixed solution of 0.8g of azobismethylvaleronitrile and 18g of methyl ethyl ketone was dropped into the flask over 0.5 hours. After aging at 65°C for 1 hour, 0.8g of azobismethylvaleronitrile was added and aged for another 1 hour. After the reaction was completed, 364g of methyl ethyl ketone was added to the flask, and 800g of polymer solution A with a concentration of 50% by mass was obtained.
[0121] -Preparation of pigment-containing polymer particle dispersion- 28 g of the above polymer solution A, 42 g of carbon black (FW100, manufactured by Degussa), 13.6 g of 1 mol / L potassium hydroxide aqueous solution, 20 g of methyl ethyl ketone, and 13.6 g of ion-exchanged water were thoroughly stirred and then kneaded using a roll mill. The obtained paste was poured into 200 g of pure water and thoroughly stirred, after which the methyl ethyl ketone and water were distilled off using an evaporator, and the dispersion was pressure-filtered with a polyvinylidene fluoride membrane filter with an average pore size of 5.0 μm to remove coarse particles, to obtain a resin-coated black pigment dispersion containing 15% by mass of carbon black and having a solid content concentration of 20% by mass. The volume-based cumulative 50% particle diameter (D 50 ) was measured and found to be 104 nm. The cumulative 50% particle size (D 50 ) was measured using a particle size distribution measuring device (Nanotrac UPA-EX150, manufactured by Nikkiso Co., Ltd.).
[0122] (Pigment Dispersion Liquid Preparation Example 2) <Preparation of Resin-Coated Cyan Pigment Dispersion> A resin-coated cyan pigment dispersion was prepared in the same manner as in Pigment Dispersion Preparation Example 1, except that the carbon black in Pigment Dispersion Preparation Example 1 was changed to a phthalocyanine pigment (CI Pigment Blue 15:3). The volume-based cumulative 50% particle diameter (D 50 ) was measured in the same manner as in Pigment Dispersion Liquid Preparation Example 1 and was found to be 93 nm.
[0123] (Pigment Dispersion Preparation Example 3) <Preparation of Resin-Coated Magenta Pigment Dispersion> A resin-coated magenta pigment dispersion was prepared in the same manner as in Pigment Dispersion Preparation Example 1, except that the carbon black in Pigment Dispersion Preparation Example 1 was changed to a magenta pigment (CI Pigment Red 122). The volume-based cumulative 50% particle diameter (D 50 ) was measured in the same manner as in Pigment Dispersion Liquid Preparation Example 1 and was found to be 127 nm.
[0124] (Pigment Dispersion Liquid Preparation Example 4) <Preparation of Resin-Coated Yellow Pigment Dispersion> In the pigment dispersion liquid preparation example 1, carbon black was replaced with monoazo yellow pigment (CI A resin-coated yellow pigment dispersion was prepared in the same manner as in Pigment Dispersion Preparation Example 1, except that C.I. Pigment Yellow 74) was used. The volume-based cumulative 50% particle diameter (D 50 ) was measured in the same manner as in Pigment Dispersion Liquid Preparation Example 1 and was found to be 76 nm.
[0125] (Color ink manufacturing example 1) -Preparation of color ink 1- The mixture of the following formulation was premixed and then filtered using a 25 mL needleless syringe equipped with a filter (acetyl cellulose membrane, outer diameter 2.5 cm, manufactured by Fuji Film Corporation) having an average pore size of 5.0 μm to remove coarse particles, thereby obtaining color ink 1. [Color ink 1 recipe] The resin-coated black pigment dispersion: 4.0% by mass TOCRYL W-6109 (acrylic resin emulsion, manufactured by Toyochem Co., Ltd.): 3.0% by mass (based on resin amount) Takelac W-6110 (urethane resin emulsion, manufactured by Mitsui Chemicals, Inc.): 3.0% by mass (based on resin amount) 3-Methyl-3-methoxybutanol: 4.0% by mass 3-Methyl-1,3-butanediol: 4.0% by mass 1,2-propanediol: 20% by mass 2-Ethyl-1,3-hexanediol: 1.5% by mass TEGO WET-270 (polyether modified siloxane copolymer, manufactured by Evonik): 0.5 mass% Proxel GXL (mold inhibitor, manufactured by Avecia): 0.05% by mass 2,4,7,9-Tetramethyldecane-4,7-diol: 0.4% by mass 2-Amino-2-ethyl-1,3-propanediol: 0.3% by mass Pure water: remaining amount (total: 100% by mass)
[0126] (Color ink manufacturing examples 2-12) -Production of color inks 2 to 12- Color inks 2 to 12 were prepared in the same manner as in Color Ink Production Example 1, except that the formulations in Color Ink Production Example 1 were changed to those shown in Tables 1 and 2 below. Note that the amount of resin added is shown.
[0127] Next, the static surface tension of each of the obtained color inks was measured by the Wilhelmy method (plate method, vertical plate method) in the same manner as in the above <Method of determining the surface tension of a liquid>. The results are shown in Tables 1 and 2.
[0128] [Table 1]
[0129] [Table 2]
[0130] (Clear ink manufacturing example 1) - Preparation of clear ink 1 - A mixture of the following formulation was premixed and then filtered using a 25 mL needleless syringe equipped with a filter (acetyl cellulose membrane, outer diameter 2.5 cm, manufactured by Fuji Film Corporation) with an average pore size of 5.0 μm to remove coarse particles, thereby obtaining clear ink 1. [Clear ink 1 formula] TOCRYL W-6109 (acrylic resin emulsion, manufactured by Toyochem Co., Ltd.): 15% by mass (based on resin amount) 3-Methyl-3-methoxybutanol: 4.0% by mass 3-Methyl-1,3-butanediol: 4.0% by mass 1,2-propanediol: 20% by mass 2-Ethyl-1,3-hexanediol: 1.5% by mass TEGO WET-270 (polyether modified siloxane copolymer, manufactured by Evonik): 1.0% by mass Proxel GXL (mold inhibitor, manufactured by Avecia): 0.05% by mass 2,4,7,9-Tetramethyldecane-4,7-diol: 0.4% by mass 2-Amino-2-ethyl-1,3-propanediol: 0.3% by mass Pure water: remaining amount (total: 100% by mass)
[0131] (Clear ink manufacturing examples 2 to 5) - Preparation of clear inks 2 to 5 - Clear inks 2 to 5 were prepared in the same manner as in Clear Ink Production Example 1, except that the clear ink formulation in Clear Ink Production Example 1 was changed to that shown in Table 3. Note that the amount of resin added is shown.
[0132] <Static surface tension measurement> Next, the static surface tension of each of the obtained clear inks was measured in the same manner as described above in <Method of determining static surface tension of liquid>. The results are shown in Table 3.
[0133] [Table 3]
[0134] Details of each component in the color inks and clear inks shown in Tables 1 to 3 above are as follows.
[0135] -resin- TOCRYL W-6109: Acrylic resin emulsion (cumulative 50% volume particle size (D 50 ) 80 nm, solid content concentration 41.1 mass%, manufactured by Toyochem Co., Ltd. TOCRYL W-4568: Acrylic resin emulsion (cumulative 50% volume particle size (D 50 ) 103 nm, solid content concentration 40.1 mass%, manufactured by Toyochem Co., Ltd. TOCRYL W-4657: Acrylic resin emulsion (cumulative 50% volume particle size (D 50 ) 53 nm, solid content concentration 40.3 mass%, manufactured by Toyochem Co., Ltd. Takelac W-6110: Urethane resin emulsion (cumulative 50% particle size (D 50 ) 47 nm, solid content 30.9 mass%, manufactured by Mitsui Chemicals, Inc.
[0136] -Surfactants- TEGO WET-270: Polyether modified siloxane copolymer (manufactured by Evonik) Silface SAG503A: Polyether modified siloxane compound (manufactured by Nissin Chemical Industry Co., Ltd.) TRITON(registered trademark) HW-1000: Polyoxyethylene alkyl ether (manufactured by The Dow Chemical Company)
[0137] - Anti-mold agent - · Proxel GXL (Avecia)
[0138] (Examples 1 to 7 and Comparative Example 1) <Color image formation> For color ink image formation, the ink sets of each color ink prepared in Color Ink Production Examples 1 to 12 according to the combinations shown in Table 5 were filled into IPSiO GX e5500 (manufactured by Ricoh Co., Ltd.) for each ink set under environmental conditions of 25°C ± 0.5°C and 50 ± 5% RH. In advance, a monochrome rectangular solid image of 5 cm x 20 cm was printed on Superfine paper (manufactured by Epson Corporation), which is a paper for inkjet printing, with a resolution of 1,200 dpi and an ink deposition amount of 0.96 mg / cm. 2 The drive voltage of the piezo element was varied to adjust the amount of adhesion so that the ink adhesion amount was 600 mg / A4 size. At this time, settings were made individually for each color ink so that the ink adhesion amount was the same. The amount of ink adhesion can be obtained by measuring the mass of the paper before and after printing a rectangular solid image. The print mode selected from the user settings of the driver attached to the printer was "Paper type: Glossy paper," "Print quality: Fine," and "Color matching: No." Next, under the above set conditions, coated paper (OK top coat +, basis weight: 127.9 g / cm 2 A four-color solid image set created using Microsoft Word 2016 (Microsoft Corporation) was printed as a single image at a resolution of 1,200 dpi as shown in Figure 7, and then dried for 30 seconds in a thermostatic chamber set to an internal temperature of 90°C. Coated paper (OK top coat +, basis weight: 127.9g / cm 2The arithmetic mean height: Ra of the color ink image printed on a paper sheet (manufactured by Oji Paper Co., Ltd.) was 1.50 μm to 1.65 μm. The arithmetic mean roughness: Ra was measured using a shape analysis laser microscope (VK-9510, manufactured by Keyence Corporation), and the average value of measurements taken at five arbitrary 100 μm × 100 μm areas within the image area was used as the value of Ra. Specific measurement conditions were lens magnification: 10x, filter: none, Z measurement pitch: 0.5 μm, and measurement mode: surface shape.
[0139] Next, the dispersion component γ of the surface free energy of each color ink layer is calculated as follows: S d and the polar component γ S P The dispersion component γ s d The maximum difference between the polar components γ s p The maximum difference was calculated, and the results are shown in Table 4.
[0140] <Dispersion component of surface free energy of color ink layer γ S d and the polar component γ S P Measurements > For the printed matter after drying, the contact angle was measured using two types of liquid (pure water, methylene iodide) with known values for each component of the surface free energy in the same manner as described above in <Method for determining contact angle θ of clear ink>, and the dispersion component γ of the surface free energy of each color ink layer was calculated from the Fowkes-Owens model. S d , polar component γ S P The dispersion component γ s d and the maximum difference between the polar components γ s p The maximum difference was calculated.
[0141] [Table 4]
[0142] <Formation of clear ink image> Next, according to the combinations shown in Table 5, each of the clear inks prepared in clear ink production examples 1 to 5 was printed on the color ink layer of the solid image prepared with each of the ink sets described above. The clear ink image was formed using IPSiO GX e5500 (manufactured by Ricoh Co., Ltd.) under environmental conditions of 25°C ± 0.5°C and 50 ± 5% RH. The clear ink layer was formed by printing a solid image chart created with Microsoft Word 2016 (manufactured by Microsoft) at a resolution of 600 dpi, and then drying for 120 seconds in a thermostatic chamber set to an internal temperature of 1,000°C. The amount of clear ink attached was 0.80 mg / cm. 2 The amount of the color ink applied was adjusted in the same manner as above so that the total amount was (500 mg / A4 size). For the print mode, I selected "Paper type: Plain paper", "Print quality: Fine", and "Color matching: No" from the user settings of the driver that came with the printer. Coated paper (OK top coat + 127.9g / m 2 After applying clear ink to the surface of a solid image of color ink formed on a paper (manufactured by Oji Paper Co., Ltd.), the clear ink was dried for 120 seconds in a thermostatic chamber set so that the internal temperature was 100° C. The color image obtained at this stage was the image shown in FIG.
[0143] Next, the interface energy γ of the clear ink with respect to the color ink layer is calculated as follows: LS The results are shown in Table 5.
[0144] <Interfacial energy γ LS Calculation of > The clear ink was deposited on the color ink layer in the combination shown in Table 5, and the contact angle θ of the clear ink with respect to the color ink layer was measured in the same manner as above. On the other hand, the static surface tension γ Lwas measured in the same manner as above. From these results, the wetting energy Wa was calculated by the Young-Dupre equation shown in the following formula (4).
[0145]
number
[0146] Next, for each of the obtained images, the 60° gloss and the arithmetic mean roughness Ra were evaluated as follows. Also, the ejection stability of each clear ink was evaluated as follows. The results are shown in Table 5.
[0147] <60° Gloss Measurement> The gloss level was measured using a gloss meter (BYK, micro-TRI-gloss) at an incidence / reflection angle of 60 degrees in accordance with JIS (Japanese Industrial Standards) Z 8741. The higher the gloss level, the higher the gloss level, and the unit is dimensionless. An image formed on A4 size paper was measured five times in both the conveying direction of the print and the direction perpendicular to the conveying direction, and the gloss level measured a total of 10 times was averaged to obtain the average gloss level. There was no difference in glossiness between the transport direction of the printed matter and the direction perpendicular to the transport direction, and there was no difference in glossiness in the in-plane direction of the solid image. A 60° gloss level of 60 or more indicates a high gloss level, with 75 or more being preferable. Furthermore, if the gloss level difference between the color inks is 10.0 or less, the gloss level can be perceived as uniform when visually recognized, with 7.0 or less being preferable, 5.0 or less being even more preferable, and 3.0 or less being particularly preferable.
[0148] <Measurement of arithmetic mean roughness Ra> For each image obtained, the arithmetic mean roughness R ais a value measured using a shape analysis laser microscope (VK-9510, manufactured by Keyence Corporation), and five areas of 100 μm × 100 μm were arbitrarily selected within the image area. Specific measurement conditions are lens magnification: 10x, filter: none, Z measurement pitch: 0.5 μm, measurement mode: surface shape. Note that the smaller the arithmetic mean roughness Ra, the higher the surface smoothness of the image.
[0149] <Clear ink ejection stability (intermittent ejection evaluation)> For each of the obtained clear inks, a solid image was created in Microsoft Word 2016 (Microsoft Corporation) so that the area ratio was 5% within an A4 size sheet of paper, and the solid image was printed on coated paper (OK top coat +, basis weight: 127.9 g / m 2 200 sheets were continuously printed onto a paper feed tray (Oji Paper Co., Ltd.), and the ink was visually inspected for irregularities in the ink discharge from each nozzle after printing, and rated according to the following criteria. A grade of B or higher is considered to be practically usable. The print mode used was "Glossy paper - Fine" mode and "No color correction" mode, modified from the plain paper user settings in the driver that came with the printer. [Evaluation Criteria] A: No disturbance in discharge B: Some irregular discharge C: Discharge is disturbed or there are areas where discharge is not performed
[0150] [Table 5]
[0151] For example, aspects of the present invention are as follows. <1> a color ink applying means for applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer; a clear ink applying means for applying a clear ink containing at least polymer particles onto the color ink layer, The clear ink has an interface energy of 50 mJ / m with respect to a solid image of each of the plurality of color inks. 2A printing device characterized in that: <2> The clear ink has an interface energy of 5 mJ / m with respect to a solid image of each of the plurality of color inks. 2 More than 50mJ / m 2 The above-mentioned <1> The printing apparatus according to the present invention is <3> the color inks include at least a black ink, a yellow ink, a magenta ink, and a cyan ink; The dispersion component of the surface free energy of each color ink layer formed by the color ink is γ s d The polar component of the surface free energy of each color ink layer is γ s p Then, the dispersion component γ s d The maximum difference is 0.3 mJ / m 2 The polar component γ s p The maximum difference is 5mJ / m 2 The above-mentioned <1> from <2> The printing apparatus according to any one of claims 1 to 5, <4> The content of the polymer particles is 10% by mass or more and 20% by mass or less. <1> from <3> The printing apparatus according to any one of claims 1 to 5, <5> The cumulative 50% volume particle diameter of the polymer particles (D 50 ) is 100 nm or less. <1> from <4> The printing apparatus according to any one of claims 1 to 5, <6> The clear ink contains a surfactant. <1> from <5> The printing apparatus according to any one of claims 1 to 5, <7> The surfactant is a polyether-modified siloxane compound represented by the following general formula (I): <6> The printing apparatus according to the present invention is [ka] In the general formula (I), m represents an integer of 0 to 23, and n represents an integer of 1 to 10, a represents an integer of 1 to 23, and b represents an integer of 0 to 23. R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. <8> The static surface tension of the color ink and the clear ink at 25° C. is 20 mN / m or more and 35 mN / m or less. <1> from <7> The printing apparatus according to any one of claims 1 to 5, <9> The ink jet recording medium is for use in ink jet recording. <1> from <8> The printing apparatus according to any one of claims 1 to 5, <10> a color ink applying step of applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer; a clear ink applying step of applying a clear ink containing at least polymer particles onto the color ink layer, The clear ink has an interface energy of 50 mJ / m with respect to a solid image of each of the plurality of color inks. 2 A printing method characterized in that: <11> A plurality of color inks containing color materials; and a clear ink containing at least polymer particles, The clear ink has an interface energy of 50 mJ / m with respect to a solid image of each of the plurality of color inks. 2 The ink set is characterized in that:
[0152] The above <1> from <9> The printing apparatus according to any one of the preceding claims, <10> The printing method according to claim 1, <11> According to the ink set described in the above, the conventional problems can be solved and the object of the present invention can be achieved. [Explanation of symbols]
[0153] 400 Image forming device 401 Exterior of image forming device 401c Device body cover 404 Cartridge Holder 410 Main Tank 410k, 410c, 410m, 410y Main tanks for black (K), cyan (C), magenta (M), and yellow (Y) 411 Ink storage unit 413 Ink outlet 414 Storage container case 420 Mechanism Department 434 Discharge Head 436 Supply Tube [Prior art documents] [Patent documents]
[0154] [Patent Document 1] Patent No. 4096158 [Patent Document 2] JP 2004-306557 A [Patent Document 3] Patent No. 5509603
Claims
1. a color ink applying means for applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer; a clear ink applying means for applying a clear ink containing at least polymer particles onto the color ink layer, the color inks include at least black ink, yellow ink, magenta ink, and cyan ink; The color ink contains at least three or more kinds of organic solvents of the same kind, the color inks and the clear ink contain at least one of a polyether-modified siloxane compound and a polyoxyethylene alkyl ether; the dispersion component of the surface free energy of each color ink layer formed with the color inks is γsd and the polar component of the surface free energy of each color ink layer is γsp, the maximum difference in the dispersion component γsd between the color ink layers of each color is 0.3 mJ / m2 or more, and the maximum difference in the polar component γsp between the color ink layers of each color is 5 mJ / m2 or less; The clear ink has an interface energy of 50 mJ / m with respect to each solid image of the plurality of color inks. 2 1. A printing device, comprising:
2. The clear ink has an interface energy of 5 mJ / m with respect to each solid image of the plurality of color inks. 2 50mJ / m or more 2 2. The printing apparatus of claim 1, wherein:
3. A printing device described in any one of claims 1 to 2, wherein the content of the polymer particles is 10 mass% or more and 20 mass% or less.
4. The printing device according to claim 1, wherein the polymer particles have a cumulative 50% volume particle diameter (D 50 ) of 100 nm or less.
5. A printing device described in any one of claims 1 to 4, wherein the polyether-modified siloxane compound is represented by the following general formula (I). 【Chemistry 1】 In the general formula (I), m represents an integer of 0 to 23, n represents an integer of 1 to 10, a represents an integer of 1 to 23, and b represents an integer of 0 to 23. R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms.
6. A printing device described in any one of claims 1 to 5, wherein the static surface tension of the color ink and the clear ink at 25°C is 20 mN / m or more and 35 mN / m or less.
7. A printing device described in any one of claims 1 to 6, which is for inkjet use.
8. A color ink applying step of applying a plurality of color inks containing color materials onto a recording medium to form a color ink layer; a clear ink applying step of applying a clear ink containing at least polymer particles onto the color ink layer, the color inks include at least black ink, yellow ink, magenta ink, and cyan ink; The color ink contains at least three or more kinds of organic solvents of the same kind, the color inks and the clear ink contain at least one of a polyether-modified siloxane compound and a polyoxyethylene alkyl ether; the dispersion component of the surface free energy of each color ink layer formed with the color inks is γsd and the polar component of the surface free energy of each color ink layer is γsp, the maximum difference in the dispersion component γsd between the color ink layers of each color is 0.3 mJ / m2 or more, and the maximum difference in the polar component γsp between the color ink layers of each color is 5 mJ / m2 or less; The printing method according to claim 1, wherein the clear ink has an interface energy of 50 mJ / m 2 or less with respect to a solid image of each of the plurality of color inks.
Citation Information
Patent Citations
Fluororesin composition having improved thermal stability
JP1980009603A
Ink jet recording method and clear ink composition used for the same
JP2004306557A
Inkjet recording method
JP2008229946A
Image forming method, inkjet printed matter, and active ray-curable type inkjet ink
JP2011025684A
Ink composition for clear layer formation, coating method for same, and printed article using same
JP2011177965A