Polar group-containing 2-alkenyl monomer copolymer, production method thereof, and oxygen barrier laminate
A novel radical copolymerization of polar group-containing 2-alkenyl and dialkenyl monomers addresses the challenge of low molecular weight oligomers, resulting in a high-molecular-weight, solvent-soluble copolymer with improved mechanical strength and applicability in film formation and packaging.
Patent Information
- Application Number
- JP2020175317
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-19
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-10-19
AI Technical Summary
Existing methods for polymerizing monomers with allyl groups result in low molecular weight oligomers due to degenerative chain transfer reactions, leading to poor moldability and mechanical strength, and require expensive catalysts or high acid usage, making industrial applications challenging.
A novel radical copolymerization process of polar group-containing 2-alkenyl and dialkenyl monomers, producing a high-molecular-weight copolymer that is soluble in various solvents, avoiding gelation and enabling applications in film formation and improved mechanical strength.
The copolymer achieves high molecular weight and solvent solubility, enhancing properties like adhesiveness and printability, and can be used in food packaging and other applications, overcoming the limitations of previous methods.
Smart Images

Figure 0007571456000018 
Figure 0007571456000019 
Figure 0007571456000020
Abstract
Description
[Technical field]
[0001] The present invention relates to a polar group-containing 2-alkenyl monomer copolymer, a production method thereof, and an oxygen barrier laminate. [Background technology]
[0002] Polymers of vinyl monomers with polar groups, such as acrylic acid esters, methacrylic acid esters, and vinyl acetate, are widely known. For example, polyvinyl alcohol (hereinafter sometimes abbreviated as PVOH) and ethylene-vinyl alcohol copolymer (hereinafter sometimes abbreviated as EVOH) are produced by saponifying polyvinyl acetate or ethylene-vinyl acetate copolymer obtained by radical polymerization of vinyl acetate or radical copolymerization of ethylene and vinyl acetate. PVOH and EVOH are used in a wide range of fields, including food packaging, taking advantage of their excellent gas barrier properties.
[0003] On the other hand, polymerization of monomers having allyl groups is more difficult than that of vinyl monomers such as vinyl acetate, and their polymers are hardly known. The main reason is that when monomers having allyl groups are radically polymerized, a degenerative chain transfer reaction to the monomer proceeds by abstraction of hydrogen atoms present on the allyl carbon atom, and only oligomers with a low degree of polymerization are obtained (Chem.Rev.58,808(1958) (Non-Patent Document 1)).
[0004] Japanese Patent Laid-Open Publication No. 58-49792 (Patent Document 1) describes ethylene-allyl acetate copolymer and ethylene-allyl acetate-vinyl acetate terpolymer as hydrocarbon oil compositions. The synthesis method is radical polymerization, and according to the examples, only low molecular weight substances with an intrinsic viscosity of about 0.12 dl / g are obtained.
[0005] JP 2004-256620 A (Patent Document 2) and Polym. Adv. Technol., 18, 953 (2007) (Non-Patent Document 2) describe a method of adding a Brønsted acid or Lewis acid in the radical polymerization of allyl acetate or allyl alcohol in order to increase the molecular weight of the resulting polymer. However, these polymerization methods require the addition of an equivalent amount of Brønsted acid or Lewis acid to the monomer, and there is room for improvement in terms of production costs and acid removal. In addition, these polymerization systems also produce low molecular weight oligomers as by-products, so dialysis membranes are used to isolate the polymer, leaving a major problem for industrial application.
[0006] JP 2011-68881 A (Patent Document 3) and J. Am. Chem. Soc., 133, 1232 (2011) (Non-Patent Document 3) describe copolymerization of ethylene with allyl acetate or allyl alcohol using an organometallic complex of Group 10 of the periodic table as a coordination polymerization catalyst. These polymerization methods have yielded ethylene-allyl acetate copolymers or ethylene-allyl alcohol copolymers with number average molecular weights Mn of about tens of thousands. However, these methods use expensive metal complexes as polymerization catalysts, and furthermore, only polymers incorporating only about a few mol % of allyl monomers have been obtained, leaving problems for industrialization.
[0007] In polymerization that only produces low molecular weight oligomers, a method of copolymerizing dialkenyl monomers and the like is known for the purpose of improving the molecular weight. The application of this method to allyl monomers is described in Pure & Appl. Chem., 61, 2051 (1989) (Non-Patent Document 4) and Chromatographia, 11, 137 (1978) (Non-Patent Document 5). However, in both documents, the copolymer is used as a stationary phase for gas chromatography, so it is clear that the copolymer is a polymer gel having a network structure in which the polymer chains are highly crosslinked and intricately entangled. Such polymer gels are poor in moldability in injection molding, cast molding, etc. because they are insoluble in solvents, and furthermore, the mechanical strength of the molded products is low. In addition, the allyl monomer content of the copolymers obtained in Non-Patent Document 4 and Non-Patent Document 5 is 40% or 10%, respectively. Copolymers with such a low allyl monomer content cannot exhibit useful physical properties derived from the allyl monomer, such as gas barrier properties. For this reason, industrial production of polar group-containing allyl polymers using this method has not been realized so far. [Prior art documents] [Patent documents]
[0008] [Patent Document 1] Japanese Patent Publication No. 58-49792 [Patent Document 2] JP 2004-256620 A [Patent Document 3] JP 2011-68881 A [Non-patent literature]
[0009] [Non-Patent Document 1] Chem. Rev. 58, 808 (1958) [Non-Patent Document 2] Polym.Adv.Technol.,18,953(2007) [Non-Patent Document 3] J. Am. Chem. Soc., 133, 1232 (2011) [Non-Patent Document 4] Pure & Appl. Chem., 61, 2051 (1989) [Non-Patent Document 5] Chromatographia, 11, 137 (1978) Summary of the Invention [Problem to be solved by the invention]
[0010] An object of the present invention is to provide a polar group-containing 2-alkenyl monomer copolymer which has a high molecular weight and is soluble in a predetermined solvent, and a method for producing the same. [Means for solving the problem]
[0011] As a result of intensive research aimed at solving the above problems, the present inventors have found that it is possible to provide a high molecular weight polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer having a novel structure and suitable for various applications by radical copolymerization of a polar group-containing 2-alkenyl monomer and a dialkenyl monomer, and have thus completed the present invention. Note that in this specification, the term "polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer" also includes ternary or higher copolymers containing other monomer units as minor components.
[0012] That is, the present invention relates to the following [1] to
[21] . [1] Equation (1), Equation (2), and Equation (3) [ka] (In the formula, R 1 , R 2 , R 3 and R 4each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom, and l, m, and n are numbers representing the molar ratios of the respective monomer structural units, and either l or m may be 0. A copolymer having a monomer structural unit represented by the following formula (A), (B), and (C): (A) the molar ratio 1 of the monomer structural unit represented by formula (1), the molar ratio m of the monomer structural unit represented by formula (2), and the molar ratio n of the dialkenyl monomer structural unit represented by formula (3) satisfy the following formula: The relationship 0.1≦[n / (l+m+n)]×100≦65 is satisfied. (B) The weight average molecular weight Mw is 10,000 to 1,000,000. (C) It does not gel and dissolves in a specified solvent. [2] The copolymer according to [1], which satisfies the relationship of 0.1≦[n / (l+m+n)]×100≦20. [3] The copolymer according to either one of [1] and [2], wherein X is -C6H4-. [4] R 1 , R 2 and R 4 The copolymer according to any one of [1] to [3], wherein [5] R 3 The copolymer according to any one of [1] to [4], wherein [6] The copolymer according to any one of [1] to [5], wherein either l or m is 0. [7] The copolymer according to any one of [1] to [6], wherein the predetermined solvent is at least one selected from the group consisting of benzene, toluene, xylene, chloroform, methylene chloride, carbon tetrachloride, dichloroethane, tetrachloroethane, chlorobenzene, dichlorobenzene, trichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, tetrahydrofuran, methanol, ethanol, isopropanol, n-propanol, 2-butanol, n-butanol, ethyl cellosolve, and butyl cellosolve. [8] Formula (4) [ka] (In the formula, R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. and a 2-alkenyl ester compound represented by formula (5): [ka] (In the formula, R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom. in the presence of a radical polymerization initiator, [ka] (In the formula, R 2 , R 3 , and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom, and m and n are numbers representing the molar ratio of each monomer structural unit. A method for producing a copolymer having a monomer structural unit represented by the following formula: [9] Formula (4) [ka] (In the formula, R 2 and R 3 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. and a 2-alkenyl ester compound represented by formula (5): [ka] (In the formula, R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom. in the presence of a radical polymerization initiator, and then saponifying the copolymer in an alcohol solvent in the presence of a catalyst. [ka] (In the formula, R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, provided that R 1 and R 2 are the same, X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom, l, m, and n are numbers representing the molar ratios of the respective monomer structural units, and m may be 0. A method for producing a copolymer having a monomer structural unit represented by the following formula:
[10] Formula (6) [ka] (In the formula, R 1 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms. and a 2-alkenyl alcohol compound represented by formula (5): [ka] (In the formula, R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom. In the presence of a radical polymerization initiator, a dialkenyl compound represented by the formula (1) and the formula (3) [ka] (In the formula, R 1 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom, and l and n are numbers representing the molar ratio of each monomer structural unit. A method for producing a copolymer having a monomer structural unit represented by the following formula:
[11] The method for producing a copolymer according to [9], wherein m is 0.
[12] R 1 , R 2 and R 4 The method for producing a copolymer according to any one of [8] to
[11] , wherein
[13] R 3 The method for producing a copolymer according to any one of [8] to
[12] , wherein
[14] The method for producing a copolymer according to any one of [8] to
[13] , wherein the radical polymerization initiator has a 10-hour half-life temperature of 50° C. or lower.
[15] The method for producing a copolymer according to any one of [8] to
[14] , wherein the polymerization temperature is in the range of 20 to 70°C.
[16] When the total molar amount of the 2-alkenyl ester compound represented by formula (4) and the 2-alkenyl alcohol compound represented by formula (6) is x and the molar amount of the dialkenyl compound represented by formula (5) is y, a reaction can be carried out according to the following formula: 0.1≦[y / (x+y)]×100≦65 The method for producing a copolymer according to any one of [8] to
[15] , wherein radical polymerization is carried out within the range.
[17] An oxygen barrier laminate comprising at least one plastic film layer and at least one oxygen barrier layer containing the copolymer according to any one of [1] to [7].
[18] The oxygen barrier laminate according to
[17] , wherein the plastic film is a polypropylene film.
[19] A method for producing an oxygen barrier laminate, comprising applying or casting a solution in which the copolymer according to any one of [1] to [7] is dissolved in a solvent onto a plastic film, and then drying the solution.
[20] The method for producing an oxygen barrier laminate according to
[19] , wherein the solvent is an alcohol. [twenty one] The method for producing an oxygen barrier laminate according to either
[19] or
[20] , wherein the solvent is ethanol and the plastic film is a polypropylene film. Effect of the Invention
[0013] According to the present invention, it is possible to obtain a polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer which has a high molecular weight and is soluble in a specific solvent, which has been difficult to produce in the past.
[0014] Since the polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer of the present invention has a polar functional structure such as an ester structure or a hydroxyl group, it can be used as a surface property modifier added to polyolefins, etc., for improving adhesion, printability, etc., a compatibilizer between non-polar polyolefins and other resins with high polarity, a dispersant for pigments, etc., as well as a paint, ink, adhesive, binder, plasticizer, lubricant, lubricating oil, surfactant, etc. In addition, since the copolymer of the present invention is soluble in a solvent, it can be easily formed into a film or sheet, and can be applied to food packaging materials, gasoline tanks, etc. [Brief description of the drawings]
[0015] [Figure 1] 1 is a 1H-NMR spectrum of the copolymer obtained in Example 3. [Diagram 2] 1 is a SEC chromatogram of the copolymer obtained in Example 3. [Diagram 3] 1 is a 1H-NMR spectrum of the saponified product obtained in Example 8. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0016] Preferred embodiments of the present invention will be described below, but the present invention is not limited to these embodiments.
[0017] 1. Polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer In one embodiment, the polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer is represented by the formula (1), the formula (2), and the formula (3): [ka] (In the formula, R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom, and l, m, and n are numbers representing the molar ratios of the respective monomer structural units, and either l or m may be 0. The copolymer has a monomer structural unit represented by the formula: The copolymer may optionally contain a fourth monomer structural unit.
[0018] R in formula (1), formula (2), and formula (3) 1 , R 2 , and R 4 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and may be different from each other.
[0019] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 1 , R 2 , and R 4 As the alkyl group, a hydrogen atom or a methyl group is preferable, and from the viewpoint of easy availability of raw materials, a hydrogen atom is particularly preferable.
[0020] R in Equation (2) 3 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0021] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 3 As the alkyl group, a methyl group or an ethyl group is preferable, and from the viewpoint of easy availability of raw materials, a methyl group is particularly preferable.
[0022] In formula (3), X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom.
[0023] Examples of the divalent organic group include an alkylene group and an arylene group. Examples of the divalent organic group containing an oxygen atom include an alkylene group or an arylene group to which two carbonyloxy groups (-C(=O)-O-) are bonded.
[0024] Examples of divalent organic groups include -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH(CH3)CH2-, -CH4-, -CH4-CH4-, -C(=O)-O-(CH2)2-OC(=O)-, -C(=O)-O-(CH2)2-O-(CH2)2-OC(=O)-, and -C(=O)-O-(C6H4)-OC(=O)-. Among these, X is preferably -C6H4- (phenylene group) or -C(=O)-O-(CH2)2-OC(=O)-, and particularly preferably -C6H4-. When X is -C6H4-, each X in the copolymer may be independently o-substituted, m-substituted, or p-substituted.
[0025] The copolymer of one embodiment satisfies the following requirements (A), (B), and (C). (A) the molar ratio 1 of the monomer structural unit represented by formula (1), the molar ratio m of the monomer structural unit represented by formula (2), and the molar ratio n of the dialkenyl monomer structural unit represented by formula (3) satisfy the following formula: The relationship 0.1≦[n / (l+m+n)]×100≦65 is satisfied. (B) The weight average molecular weight Mw is 10,000 to 1,000,000. (C) It does not gel and dissolves in a specified solvent.
[0026] (A) Molar ratio of monomer structural units The molar ratios l, m, and n satisfy the following relationship. 0.1≦[n / (l+m+n)]×100≦65
[0027] When [n / (l+m+n)] x 100 is 0.1 or more, the molecular weight of the copolymer is improved, and the strength of the molded product can be increased. When [n / (l+m+n)] x 100 is 65 or less, the copolymer can be made to have high solubility in a specified solvent without gelling. [n / (l+m+n)] x 100 is preferably 1 or more, and more preferably 5 or more. [n / (l+m+n)] x 100 is preferably 20 or less, and more preferably 15 or less. The value of [n / (l+m+n)] x 100 is described in the examples. 1 It is determined by H-NMR method. The l, m, and n in formula (1), formula (2), and formula (3) simply indicate the amount ratio of the corresponding monomers, and do not necessarily mean that the monomer structural units of formula (1), formula (2), and formula (3) are bonded consecutively in the number of l, m, and n, respectively.
[0028] In one embodiment, either l or m is 0.
[0029] (B) Weight average molecular weight The weight average molecular weight Mw of the copolymer in one embodiment is 10,000 to 1,000,000. From the viewpoint of the balance between moldability and strength of the molded article, Mw is preferably 10,000 to 500,000, and more preferably 10,000 to 100,000. If Mw is less than 10,000, the strength of the molded article decreases. If Mw exceeds 100,000, the solution viscosity or melt viscosity becomes too high, making molding difficult. Mw is determined by a method using GPC described in the examples.
[0030] (C) It does not gel and dissolves in a specified solvent. "Gelled" refers to a state in which the presence of a cross-linked structure results in the presence of components that are insoluble in any solvent. Even if the main chain of a gelled copolymer is dissolved in a good solvent, the cross-linked structure portion will only swell and will not dissolve. "Not gelled, soluble in a specified solvent" refers to the fact that all components of the copolymer will dissolve if an appropriate good solvent and temperature are selected. Whether or not the copolymer has dissolved is determined by visual observation.
[0031] The copolymer is preferably dissolved in a predetermined solvent at a temperature of 20 to 30° C. at a solid content concentration in the range of 0.1 to 10% by mass.
[0032] The predetermined solvent is a good solvent for the copolymer.Specific examples of the predetermined solvent include aromatic hydrocarbons such as benzene, toluene, and xylene, halogenated aliphatic hydrocarbons such as chloroform, methylene chloride, carbon tetrachloride, dichloroethane, and tetrachloroethane, halogenated aromatic hydrocarbons such as chlorobenzene, dichlorobenzene, and trichlorobenzene, nitrogen-containing solvents such as N,N-dimethylformamide and N,N-dimethylacetamide, sulfur-containing solvents such as dimethylsulfoxide, cyclic ether solvents such as tetrahydrofuran, alcohol solvents such as methanol, ethanol, isopropanol, n-propanol, 2-butanol, and n-butanol, and cellosolve solvents such as ethyl cellosolve and butyl cellosolve.
[0033] The good solvent as the predetermined solvent preferably includes benzene, toluene, xylene, chloroform, methylene chloride, N,N-dimethylformamide, or dimethylsulfoxide.
[0034] The predetermined solvent may be a single solvent or a mixed solvent of two or more kinds. In the case of a mixed solvent, the optimal solvent composition varies depending on the molar ratios l, m and n of the respective monomer structural units in the copolymer, but it is preferable to increase the ratio of the alcohol solvent or cellosolve solvent as l increases.
[0035] When dissolving the copolymer in a solvent, the solvent may be heated to promote dissolution. The heating temperature is preferably in the range of 40 to 200° C., more preferably in the range of 40 to 150° C., and particularly preferably in the range of 40 to 100° C., from the viewpoint of avoiding decomposition of the copolymer.
[0036] 2. Method for producing polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer The polar group-containing 2-alkenyl monomer-dialkenyl monomer copolymer of some embodiments can be produced by the following method. (A) The compounds represented by the formulas (4), (5), and (6), and, if necessary, other monomers corresponding to the fourth monomer unit, are copolymerized in the presence of a radical polymerization initiator described below. (B) The compounds represented by the formulas (4) and (5), and, if necessary, another monomer corresponding to the fourth monomer unit, are copolymerized in the presence of a radical polymerization initiator described below. (C) A copolymer obtained by copolymerizing the compounds represented by the formulas (4) and (5) and, if necessary, another monomer corresponding to the fourth monomer unit is subjected to a saponification reaction in an alcohol solvent in the presence of a catalyst described later. (D) The compounds represented by the formula (6) and the formula (5), and, if necessary, another monomer corresponding to the fourth monomer unit, are copolymerized in the presence of a radical polymerization initiator described below.
[0037] In one embodiment, in the copolymer produced by the method (C), the molar ratio m of the monomer structural unit represented by formula (2) is 0. In this embodiment, the saponification reaction proceeds completely.
[0038] In the copolymer, the monomer that is the source of the monomer structural unit represented by formula (2) is represented by formula (4): [ka] It is a 2-alkenyl ester compound represented by the formula:
[0039] R in Equation (4) 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0040] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 2 As the alkyl group, a hydrogen atom or a methyl group is preferable, and from the viewpoint of easy availability of raw materials, a hydrogen atom is particularly preferable.
[0041] R in Equation (4) 3 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0042] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 3 As the alkyl group, a methyl group or an ethyl group is preferable, and from the viewpoint of easy availability of raw materials, a methyl group is particularly preferable.
[0043] In the copolymer, the monomer that is the source of the monomer structural unit represented by formula (1) is represented by formula (6): [ka] It is a 2-alkenyl alcohol compound represented by the formula:
[0044] R in Equation (6) 1represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0045] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 1 As the alkyl group, a hydrogen atom or a methyl group is preferable, and from the viewpoint of easy availability of raw materials, a hydrogen atom is particularly preferable.
[0046] The monomer structural unit represented by formula (1) is represented by the above formula (4) [ka] The compound can also be obtained by polymerizing a 2-alkenyl ester compound represented by the following formula: and then hydrolyzing (saponification) the compound in an alcohol solvent using a catalyst described later.
[0047] R in Equation (4) 2 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and R 1 and R of the monomer unit represented by formula (2) 2 is R in Eq. (4). 2 Because it comes from R 1 and R 2 are identical.
[0048] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 2 As the alkyl group, a hydrogen atom or a methyl group is preferable, and from the viewpoint of easy availability of raw materials, a hydrogen atom is particularly preferable.
[0049] R in Equation (4) 3 represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0050] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 3As the alkyl group, a methyl group or an ethyl group is preferable, and from the viewpoint of easy availability of raw materials, a methyl group is particularly preferable.
[0051] The monomer represented by formula (4) and the monomer represented by formula (6) may be mixed and polymerized. From the viewpoint of improving the reaction rate, it is preferable to polymerize only the monomer represented by formula (4) without using the monomer represented by formula (6).
[0052] In the copolymer, the dialkenyl monomer which is the source of the monomer structural unit represented by formula (3) is represented by formula (5): [ka] It is a dialkenyl compound represented by the formula:
[0053] R in Equation (5) 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms.
[0054] Examples of the alkyl group having 1 to 3 carbon atoms include a methyl group, an ethyl group, an n-propyl group, and an isopropyl group. 4 As the alkyl group, a hydrogen atom or a methyl group is preferable, and from the viewpoint of easy availability of raw materials, a hydrogen atom is particularly preferable.
[0055] In the formula (5), X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom.
[0056] Examples of the divalent organic group include an alkylene group and an arylene group. Examples of the divalent organic group containing an oxygen atom include an alkylene group or an arylene group to which two carbonyloxy groups (-C(=O)-O-) are bonded.
[0057] Examples of divalent organic groups include -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2CH(CH3)CH2-, -CH4-, -CH4-CH4-, -C(=O)-O-(CH2)2-OC(=O)-, -C(=O)-O-(CH2)2-O-(CH2)2-OC(=O)-, and -C(=O)-O-(C6H4)-OC(=O)-. Among these, X is preferably -C6H4- (phenylene group) or -C(=O)-O-(CH2)2-OC(=O)-, and particularly preferably -C6H4-. When X is -C6H4-, it may be an o-substituted, m-substituted, or p-substituted.
[0058] The dialkenyl monomers may be used alone or in combination of two or more kinds.
[0059] Examples of the dialkenyl monomer represented by formula (5) include o-divinylbenzene, m-divinylbenzene, p-divinylbenzene, ethylene glycol dimethacrylate, and diethylene glycol diacrylate. Among these, p-divinylbenzene and ethylene glycol dimethacrylate are preferred.
[0060] In the method for producing a copolymer of one embodiment, other monomers corresponding to the fourth monomer unit may be copolymerized as necessary. Examples of other monomers include α-olefins such as propylene, 1-butene, 1-pentene, 1-hexene, 4-methyl-1-pentene, 1-heptene, 1-octene, 1-nonene, 1-decene, and styrene; cyclic olefins such as norbornene, cyclopentene, and cyclohexene; and olefins having polar groups such as acrylic acid esters, methacrylic acid esters, vinyl acetate, vinyl ether, acrylonitrile, and acrolein. Two or more of these may be polymerized in combination. The content of other monomers contained in the copolymer is preferably less than 5 mol%, and more preferably less than 2 mol%.
[0061] In the method for producing the copolymer of one embodiment, a known radical polymerization initiator can be used.
[0062] Examples of radical polymerization initiators include azo compounds such as 2,2'-azobisisobutyronitrile and 2,2'-azobis(2,4-dimethylvaleronitrile); ketone peroxide compounds such as methyl ethyl ketone peroxide and methyl isobutyl ketone peroxide; diacyl peroxide compounds such as benzoyl peroxide and lauroyl peroxide; dialkyl peroxide compounds such as dicumyl peroxide and t-butylcumyl peroxide; and peroxide compounds such as 1,1-di(t-hexylperoxy)-3,3,5-trimethylcyclohexane. Examples of the initiator include, but are not limited to, shiketal compounds; alkyl peroxyester compounds such as t-butyl peroxypivalate, t-butyl peroxy-2-ethylhexanoate, and t-butyl peroxyisobutyrate; peroxycarbonate compounds such as diisopropyl peroxydicarbonate, di-sec-butyl peroxydicarbonate, t-butyl peroxyisopropylcarbonate, and di(4-t-butylcyclohexyl) peroxydicarbonate; and thermal radical polymerization initiators such as hydrogen peroxide. These radical polymerization initiators may be used alone or in combination of two or more.
[0063] The 10-hour half-life temperature of the radical polymerization initiator is preferably 50° C. or less. In particular, the radical polymerization initiator is preferably di(4-t-butylcyclohexyl)peroxydicarbonate, which has a 10-hour half-life temperature of 48° C. If the 10-hour half-life temperature exceeds 50° C., the molecular weight of the copolymer may become too low.
[0064] The amount of radical polymerization initiator used can be determined based on the reaction temperature and the composition ratio of each monomer. The amount of radical polymerization initiator used is preferably 0.1 to 15 mol%, particularly preferably 0.5 to 10 mol%, based on the total amount of radically polymerizable monomers. If the amount of radical polymerization initiator added is 0.1 mol% or more, the progress of the polymerization reaction can be promoted. If the amount of radical polymerization initiator added is 15 mol% or less, a copolymer having a desired molecular weight can be economically produced.
[0065] In one embodiment of the method for producing a copolymer, the polymerization temperature is preferably in the range of 20 to 70° C., and particularly preferably in the range of 30 to 65° C. If the polymerization temperature is 20° C. or higher, the polymerization reaction can proceed at an economical rate. If the polymerization temperature is 70° C. or lower, the rate of chain transfer to the 2-alkenyl monomer can be suppressed, and a copolymer having a desired molecular weight can be produced.
[0066] In one embodiment of the method for producing a copolymer, when the total molar amount of the 2-alkenyl ester compound represented by formula (4) and the 2-alkenyl alcohol compound represented by formula (6) is x and the molar amount of the dialkenyl compound represented by formula (5) is y, a copolymer represented by the following formula: 0.1≦[y / (x+y)]×100≦65 It is preferable to carry out the radical polymerization in the range of 0.5≦[y / (x+y)]×100≦20 It is particularly preferable to carry out the radical polymerization within the range of 1 to 500° C.
[0067] By making the value of [y / (x+y)]×100 0.1 or more, the molecular weight of the copolymer can be increased to a desired level, and by making it 65 or less, gelation of the copolymer can be suppressed.
[0068] The polymerization method of the copolymer is not particularly limited, and a commonly used method such as bulk polymerization, solution polymerization, suspension polymerization, or gas phase polymerization can be used. Particularly, bulk polymerization and solution polymerization are preferable. The polymerization method may be a batch method, a continuous method, a single-stage polymerization, or a multi-stage polymerization. The monomer may be added within the above-mentioned monomer charge ratio range. A radical polymerization initiator may be added.
[0069] The polymerization time can be appropriately adjusted depending on the polymerization method and polymerization mode, the half-life of the initiator, etc. The polymerization time may be as short as a few minutes or as long as several thousand hours.
[0070] In order to prevent a decrease in initiation efficiency, the atmosphere in the polymerization system is preferably filled with an inert gas such as nitrogen gas or argon so as to prevent the inclusion of air, oxygen gas, moisture, etc. other than the monomer. It is also preferable to fill the gas phase with monomer vapor by charging the monomer or radical polymerization initiator in a glass ampoule or the like and performing freeze degassing.
[0071] In the case of solution polymerization, an inert solvent can be used in addition to the monomer.The inert solvent is not particularly limited, but examples thereof include aliphatic hydrocarbons such as isobutane, pentane, hexane, and cyclohexane, aromatic hydrocarbons such as benzene, toluene, and xylene, halogenated aliphatic hydrocarbons such as chloroform, methylene chloride, carbon tetrachloride, dichloroethane, and tetrachloroethane, halogenated aromatic hydrocarbons such as chlorobenzene, dichlorobenzene, and trichlorobenzene, aliphatic esters such as methyl acetate and ethyl acetate, aromatic esters such as methyl benzoate and ethyl benzoate, and aliphatic ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and t-butyl methyl ketone.
[0072] After the polymerization reaction is completed, the product copolymer may be isolated by post-treatment using known operations or treatment methods (e.g., neutralization, solvent extraction, washing with water, separation, solvent distillation, freeze-drying, reprecipitation, etc.).
[0073] The saponification reaction of the copolymer in an alcohol solvent can be carried out by a known method.
[0074] The saponification reaction can be carried out in a solvent containing an alcohol in the presence of an acidic or basic catalyst. Examples of the acidic catalyst include hydrochloric acid, sulfuric acid, phosphoric acid, acetic acid, trifluoroacetic acid, trichloroacetic acid, trifluoromethanesulfonic acid, methanesulfonic acid, and p-toluenesulfonic acid. From the viewpoint of industrial availability, hydrochloric acid, sulfuric acid, or acetic acid is preferred, and hydrochloric acid is more preferred. Examples of the basic catalyst include sodium hydroxide, potassium hydroxide, lithium hydroxide, sodium methoxide, and sodium ethoxide. From the viewpoint of industrial availability, sodium methoxide, sodium hydroxide, or potassium hydroxide is preferred, and sodium methoxide or sodium hydroxide is more preferred. Examples of the alcohol include methanol, ethanol, isopropanol, n-propanol, 2-butanol, and n-butanol. From the viewpoint of industrial availability, methanol or ethanol is preferred, and methanol is more preferred. The solvent containing the alcohol may be an alcohol alone or a mixture with another solvent. Examples of other solvents include toluene, xylene, cyclohexane, n-hexane, ethyl acetate, methyl acetate, n-propyl acetate, isopropyl acetate, n-butyl acetate, methyl ethyl ketone, tetrahydrofuran, methylene chloride, chloroform, dichlorobenzene, and water.
[0075] The copolymer can be molded into pellets, a film, a sheet, etc., using ordinary molding methods and conditions for thermoplastic resins.
[0076] The copolymer itself can be made into a product by molding such as injection molding, extrusion molding, and film molding. The copolymer can also be used as a surface property modifier added to polyolefins, such as adhesiveness and printability, a compatibilizer between non-polar polyolefins and other highly polar resins, and a dispersant for pigments. The copolymer can also be used as a paint, ink, adhesive, binder, plasticizer, lubricant, lubricating oil, surfactant, etc.
[0077] 3. Oxygen Barrier Laminate An oxygen barrier laminate can be produced by laminating at least one oxygen barrier layer containing the copolymer of one embodiment onto at least one plastic film.
[0078] From the viewpoint of improving the oxygen barrier property, the molar ratio 1 of the monomer structural unit represented by formula (1) and the molar ratio m of the monomer structural unit represented by formula (2) are preferably set to the following formula: 90≦[l / (l+m)]×100≦100 It is preferable that the relationship 95≦[l / (l+m)]×100≦100 It is more preferable that the relationship 98≦[l / (l+m)]×100≦100 It is particularly preferable that the following relationship is satisfied. If [l / (l+m)]×100 is less than 90, the oxygen barrier property is likely to decrease.
[0079] The oxygen barrier laminate of one embodiment can be produced by a molding method known in the field of general polymer molding and processing. Specifically, methods such as solution casting, T-die molding, inflation molding, dry lamination molding, extrusion coating, and co-extrusion molding can be used. Among these, solution casting is preferred from the viewpoints of ease of film formation and simplicity of process.
[0080] Solution casting is a method in which a solution of a copolymer dissolved in a solvent is applied or cast onto a plastic film, and then dried to form a laminate.
[0081] As the solvent, a good solvent for the copolymer can be used. From the viewpoint of ease of distillation in the drying step and safety, alcohol and glycol monoether are preferred, and ethanol and ethyl cellosolve are particularly preferred. These solvents may be used alone or in combination.
[0082] The solid content concentration of the solution (concentration of components other than the solvent) is not particularly limited, but is preferably 1 to 50% by mass, more preferably 3 to 30% by mass, and particularly preferably 5 to 20% by mass. If the solid content concentration is 1% by mass or more, the time required for distilling off the solvent in the drying step can be shortened, and the production cost can be reduced. If the solid content concentration is 20% by mass or less, the viscosity of the solution can be kept in an appropriate range, and the occurrence of thickness unevenness or streaks during coating or casting can be suppressed.
[0083] The copolymer solution may contain additives as necessary within the range that does not impair the oxygen barrier property. Examples of additives include stabilizers (antioxidants, heat stabilizers, ultraviolet absorbers, etc.), plasticizers, antistatic agents, lubricants, antiblocking agents, colorants, fillers, crystal nucleating agents, inorganic fillers, and plate-like inorganic compounds. These additives may be used alone or in combination of two or more.
[0084] The method for applying or casting the copolymer solution is not particularly limited, and known methods such as bar coater coating, Mayer bar coating, air knife coating, gravure coating, reverse gravure coating, microgravure coating, micro reverse gravure coater coating, die coater coating, slot die coater coating, vacuum die coater coating, dip coating, spin coat coating, spray coating, and brush coating can be used.
[0085] The drying method is not particularly limited, but known methods such as blowing hot air using a dryer or irradiating with infrared rays can be used.
[0086] The drying temperature depends on the heat resistance of the plastic film, but is preferably from room temperature to 150° C., more preferably from 50 to 120° C., and particularly preferably from 60 to 90° C. If the drying temperature is at or above room temperature, the time required for drying can be shortened. If the drying temperature is at or below 150° C., the generation of bubbles in the coating layer or the casting layer and the thermal deformation of the plastic film can be suppressed.
[0087] The drying time is not particularly limited, but is preferably 1 second to 30 minutes, more preferably 3 seconds to 15 minutes, and particularly preferably 5 seconds to 5 minutes. If the drying time is 1 second or more, the solvent can be sufficiently removed by distillation. If the drying time is 30 minutes or less, the manufacturing cost can be kept within an appropriate range.
[0088] The thickness of the oxygen barrier layer is not particularly limited, but is preferably 0.1 to 50 μm, more preferably 0.2 to 30 μm, and particularly preferably 0.5 to 10 μm. If the thickness of the oxygen barrier layer is 0.1 μm or more, the occurrence of pinholes or cracks in the oxygen barrier layer can be suppressed, and the deterioration of the oxygen barrier properties can be prevented. If the thickness of the oxygen barrier layer is 50 μm or less, the flexibility of the oxygen barrier laminate can be maintained.
[0089] Examples of plastic films include polyester films such as polyethylene terephthalate (PET) film, polybutylene terephthalate (PBT) film, and polynaphthalene terephthalate (PEN) film, polystyrene film, polycarbonate (PC) film, polyamide film, polyimide film, polyarylate film, polyacrylonitrile film, polyethylene film (including LLDPE: linear low-density polyethylene film, and HDPE: high-density polyethylene film), polyolefin films such as polypropylene film (including CPP: unstretched polypropylene film, and OPP: biaxially stretched polypropylene film), polycycloolefin film, polyvinylidene chloride (PVDC) film, polyvinyl chloride (PVC) film, and transparent vapor deposition films thereof. Surface treatment such as corona treatment may be applied to the plastic film.
[0090] From the viewpoints of improving the oxygen barrier property of the laminate and being easily available, the plastic film is preferably a polyethylene film, a polypropylene film, or a polyethylene terephthalate film, and particularly preferably a polypropylene film. By using these plastic films, a laminate having excellent water vapor barrier property and oxygen barrier property can be produced at low cost.
[0091] The oxygen permeability of the oxygen barrier laminate is 300cc / (m2) under low humidity conditions (0% RH). 2 ·day·atm) or less, and 250cc / (m 2 ·day·atm) or less is more preferable, and 200cc / (m 2 ·day·atm) or less. It is particularly preferable that the oxygen permeability under low humidity conditions (0% RH) is 300cc / (m 2 If the oxygen barrier laminate is used as a packaging bag, it is expected that the oxygen deterioration of the contents will be delayed if the oxygen barrier laminate is used as a packaging bag.
[0092] The oxygen permeability of the oxygen barrier laminate is preferably in a range in which the barrier properties are not reduced under high humidity conditions (90% RH) compared to low humidity conditions. Oxygen permeability ratio = Oxygen permeability at high humidity (90% RH) / Oxygen permeability at low humidity (0% RH) The oxygen transmission rate ratio represented by the following formula is preferably 5 or less, more preferably 4 or less, and particularly preferably 3 or less.
[0093] The oxygen barrier laminate of one embodiment may be stretched at least uniaxially. The stretching method is not particularly limited, and a known method can be used. For example, a tenter-type simultaneous biaxial stretching machine is used to simultaneously stretch an unstretched oxygen barrier laminate in the machine direction (MD) and the transverse direction (TD), thereby obtaining a simultaneously biaxially stretched oxygen barrier laminate.
[0094] The oxygen barrier laminate of one embodiment may be irradiated with high-energy rays such as ultraviolet rays, X-rays, electron beams, etc., as necessary. In this case, a component that crosslinks or polymerizes by high-energy irradiation may be blended in a layer that constitutes the oxygen barrier laminate, as long as the gas barrier property or flexibility is not impaired.
[0095] The oxygen barrier laminate of one embodiment may be subjected to a surface treatment such as a corona treatment, if necessary.
[0096] By laminating a sealant resin onto the oxygen barrier laminate of one embodiment, various laminate films can be produced.
[0097] Examples of the sealant resin include low-density polyethylene, medium-density polyethylene, high-density polyethylene, linear low-density polyethylene, polypropylene, ethylene-propylene copolymer, ethylene-vinyl acetate copolymer, ionomer resin, ethylene-acrylic acid copolymer, ethylene-methacrylic acid copolymer, ethylene-acrylic acid ester copolymer, ethylene-methacrylic acid ester copolymer, and polyvinyl acetate resin. Among these, polyolefins such as polyethylene, polypropylene, and ethylene-propylene copolymer, which have high heat seal strength or material strength, are preferred. The sealant resin may be used alone, or may be copolymerized or melt-mixed with other resins, and may further be acid-modified.
[0098] Examples of methods for forming a sealant layer on an oxygen barrier laminate include a method of laminating a film or sheet containing a sealant resin onto an oxygen barrier laminate via an adhesive, and a method of extrusion laminating a sealant resin onto an oxygen barrier laminate. In the former method, the film or sheet containing the sealant resin may be in an unstretched state or in a low-stretched state. For practical purposes, the film or sheet containing the sealant resin is preferably in an unstretched state.
[0099] The thickness of the sealant layer is not particularly limited, but is preferably from 20 to 100 μm, and more preferably from 40 to 70 μm.
[0100] A packaging bag can be produced using the oxygen barrier laminate of one embodiment. The packaging bag can be suitably used for filling and packaging food and beverage products such as fruits, juices, drinking water, alcohol, cooked foods, fish paste products, frozen foods, meat products, simmered foods, rice cakes, liquid soups, and seasonings, liquid detergents, cosmetics, and chemical products. EXAMPLES
[0101] The present invention will be described in more detail below with reference to examples and comparative examples, but the present invention is not limited to the following examples.
[0102] (1) Molecular weight of copolymer The molecular weight of the copolymer was analyzed by size exclusion chromatography (solvent: 0.1% by mass LiBr-DMF, temperature: 50°C, flow rate: 1.0 mL / min) using a GPC-120 “PolymerLabs” (Agilent Technologies) equipped with a PLgel 5 μm MIXED B column (two columns in series) with polystyrene as a molecular weight standard.
[0103] (2) Copolymerization ratio of polymer The content of each of the monomer structural units represented by formula (1), formula (2) and formula (3) was measured at room temperature using a nuclear magnetic resonance spectrometer VARIAN XR-400 or a nuclear magnetic resonance spectrometer JNM-ECS400 manufactured by JEOL Ltd. 1 This was determined by H-NMR analysis.
[0104] (3) Solubility of copolymer A specified solvent was added to the copolymer so that the solid content concentration became 5% by mass, and either (A) the mixture was left to stand at room temperature (20 to 30°C) for 24 hours, or (B) the mixture was heated at 40 to 70°C for 5 hours and then cooled to room temperature (20 to 30°C) after which the mixture was judged as "good" if no insoluble matter or components that had swollen into a gel were found by visual observation, and judged as "poor" if any insoluble matter or components that had swollen into a gel remained.
[0105] (4) Oxygen barrier properties The oxygen permeability was measured at 20°C and relative humidity of 0% and 90% according to JIS K 7126-2:2006 (Appendix A).
[0106] (5) Raw materials Allyl acetate (Showa Denko K.K.) and allyl alcohol (Aldrich) were distilled from commercial products. Divinylbenzene (Aldrich) was purified through an alumina column. 2,2'-azobisisobutyronitrile (Aldrich) was recrystallized from methanol. Di(4-t-butylcyclohexyl)peroxydicarbonate was synthesized according to the specification of U.S. Pat. No. 7,968,753 and used.
[0107] Example 1 A 100 mL glass flask was purged with argon gas, and divinylbenzene (0.7 mL, 4.9 mmol) and di(4-t-butylcyclohexyl)peroxydicarbonate (2 g, 5.0 mmol) were added as a solution in toluene (4 mL) to allyl acetate (45 mL, 418 mmol). The resulting mixture was heated at 40°C for 18 hours to carry out a polymerization reaction, then cooled to room temperature and purified by freeze-drying using benzene to obtain copolymer 1. The conversion of allyl acetate was 9%. Copolymer 1 was dissolved in benzene, chloroform, dimethyl sulfoxide, and dimethylformamide. The weight average molecular weight (Mw) of copolymer 1 measured by size exclusion chromatography was 26,000, and the polydispersity (Mw / Mn) was 15.8. The polymerization was carried out using deuterated chloroform as the solvent. 1From the H-NMR measurement, the molar ratios of the monomer structural units in copolymer 1 calculated from the integral ratio of methylene protons (-CH2-OC(O)-) derived from allyl acetate observed around 3.5 to 4.2 ppm and the integral ratio of protons (-C6H4-) derived from divinylbenzene observed around 6.2 to 7.7 ppm were l = 0 mol%, m = 80 mol%, and n = 20 mol%.
[0108] Example 2 After heating for 18 hours in the same manner as in Example 1, divinylbenzene (0.7 mL, 4.9 mmol) and di(4-t-butylcyclohexyl)peroxydicarbonate (2 g, 5.0 mmol) were dissolved in toluene (4 mL) and added again, and the mixture was heated at 40° C. for 18 hours. Thereafter, divinylbenzene and di(4-t-butylcyclohexyl)peroxydicarbonate were added again in the same manner, and the mixture was heated at 40° C. for 48 hours. This was repeated twice, and the mixture was heated for a total of 132 hours to carry out the polymerization reaction, and then copolymer 2 was obtained in the same manner as in Example 1. The analytical results are shown in Table 1.
[0109] Example 3 Allyl acetate (26 mL, 242 mmol) was mixed with divinylbenzene (0.34 mL, 2.4 mmol) and di(4-t-butylcyclohexyl)peroxydicarbonate (0.96 g, 2.4 mmol) in a glass ampoule to prepare a solution, which was then freeze-degassed (5 × 10 -3 After the ampoule was subjected to four pressure changes (pressures of 1000 mmHg) each, the ampoule was sealed. The ampoule was heated at 40°C for 46 hours, cooled to room temperature, and purified by freeze-drying using benzene to obtain copolymer 3. The conversion rate of allyl acetate was 17.0%. Analysis was performed in the same manner as in Example 1, and copolymer 3 was found to be soluble in benzene, chloroform, dimethyl sulfoxide, and dimethylformamide, and the weight average molecular weight (Mw) of copolymer 3 was 10,500, the polydispersity (Mw / Mn) was 7.8, and the molar ratios of the monomer structural units in copolymer 3 were l=0 mol%, m=89 mol%, and n=11 mol%. 1 The H-NMR spectrum is shown in FIG. 1, and the SEC chromatogram is shown in FIG.
[0110] Example 4 After heating for 46 hours in the same manner as in Example 3, divinylbenzene (0.34 mL, 2.4 mmol) and di(4-t-butylcyclohexyl)peroxydicarbonate (0.96 g, 2.4 mmol) were added again, and after freeze-degassing, the ampoule was sealed and heated at 40° C. for 24 hours. This operation was repeated three more times, and the polymerization reaction was carried out by heating for a total of 118 hours, and then Copolymer 4 was obtained by the same procedure as in Example 1. The analytical results are shown in Table 1.
[0111] Example 5 Except for changing the monomer from allyl acetate to allyl alcohol and changing the heating time to 18 hours, polymerization was carried out in the same manner as in Example 1 to obtain Copolymer 5. The analysis results are shown in Table 1.
[0112] Example 6 Allyl acetate (13 mL, 120 mmol), divinylbenzene (0.17 mL, 1.2 mmol), and di(4-t-butylcyclohexyl)peroxydicarbonate (0.48 g, 1.2 mmol) were mixed in a glass ampoule to prepare a solution, which was then freeze-degassed (5 × 10 -3 After the ampoule was heated at 60° C. for 4 hours, divinylbenzene (0.17 mL, 1.2 mmol) and di(4-t-butylcyclohexyl)peroxydicarbonate (0.048 g, 0.12 mmol) were added, and the mixture was heated again at 60° C. for 16 hours to carry out a polymerization reaction, and the same procedure as in Example 1 was used to obtain Copolymer 6. The analytical results are shown in Table 1.
[0113] Example 7 Polymerization was carried out in the same manner as in Example 6, except that the amount of di(4-t-butylcyclohexyl)peroxydicarbonate added was changed to 0.24 g (0.60 mmol), to obtain Copolymer 7. The analytical results are shown in Table 1.
[0114] Comparative Example 1 Polymerization was carried out in the same manner as in Example 1, except that divinylbenzene was not added, to obtain polymer C1. The analytical results are shown in Table 1.
[0115] Comparative Example 2 Polymerization was carried out in the same manner as in Example 1, except that the temperature was changed to 80° C. and 2,2′-azobisisobutyronitrile was used as the radical polymerization initiator, to obtain a copolymer C2. The analytical results are shown in Table 1.
[0116] Comparative Example 3 Except for changing the amount of divinylbenzene to 1.9 mL (12.9 mmol), polymerization was carried out in the same manner as in Example 1. The obtained copolymer C3 was insoluble in benzene, chloroform, etc., and the weight average molecular weight and the molar ratio of the monomer structural units could not be calculated.
[0117] Table 1 shows the polymerization conditions and the measured values of the obtained copolymer or polymer.
[0118] [Table 1]
[0119] In Examples 1 to 7, copolymers having high weight average molecular weight and high solubility in solvents could be produced. As shown in Comparative Examples 1 and 2, when no dialkenyl monomer is added or when radical polymerization is performed at high temperature, the molecular weight of the copolymer is low. As shown in Comparative Example 3, when the amount of dialkenyl monomer charged is increased too much, the copolymer gels.
[0120] (Purification Example 1) The copolymer obtained in Example 4 was dissolved in benzene, and the solution obtained was dropped into methanol to reprecipitate, and the precipitate was collected by filtration and analyzed in the same manner as in Example 1. The produced copolymer was dissolved in benzene, chloroform, dimethyl sulfoxide, dimethylformamide, and tetrahydrofuran, and the weight average molecular weight (Mw) of the copolymer was 24,000, the polydispersity (Mw / Mn) was 3.0, and the molar ratios of the monomer structural units were l=0 mol%, m=87 mol%, and n=13 mol%.
[0121] (Example 8) Saponification The copolymer 3 (2 g) obtained in Example 3 was dissolved in a mixed solvent of methanol (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., 30 mL) and tetrahydrofuran (manufactured by FUJIFILM Wako Pure Chemical Industries, Ltd., 5 mL), and after adding a 10% by mass solution of sodium methoxide in methanol, the mixture was heated in an oil bath at 60°C for 20 hours. The mixture was cooled to room temperature, and an ion exchange resin (Dowex) was added and stirred, followed by filtration. The obtained filtrate was reprecipitated with acetone, and the obtained solid was dried to obtain a saponified product (copolymer 8). The mixture was dissolved in methanol-d4 as the solvent. 1 From the H-NMR measurement, the molar ratios of the monomer structural units in copolymer 8 calculated from the integral ratio of methylene protons (-CH2-OH) derived from allyl alcohol found in the vicinity of 3.3 to 3.8 ppm and the integral ratio of protons (-CH4-) derived from divinylbenzene found in the vicinity of 6.0 to 7.5 ppm were 1 = 85 mol%, m = 0 mol%, and n = 15 mol%. 1 The H-NMR spectrum is shown in Figure 3.
[0122] (Film production example 1) The copolymer 8 obtained in Example 8 was dissolved in ethanol (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) so that the solid content concentration was 5 mass %, and filtered through a membrane filter with a pore size of 0.45 μm. The obtained filtrate was applied to a 60 μm corona-treated biaxially oriented polypropylene (OPP) film using a bar coater, and then heated and dried for 10 minutes in a hot air drying oven set at 40° C. Then, it was heated and dried for another 10 minutes in a hot air drying oven set at 80° C., to obtain a laminate in which the surface of the OPP film was coated with copolymer 8 to a thickness of 5 μm. The oxygen transmission rate of this laminate at a temperature of 20° C. and a relative humidity of 0% RH was 150 cc / (m 2 ·day·atm), and 360cc / (m at 90% RH 2 ·day·atm), and the formula is: Oxygen permeability ratio = Oxygen permeability at high humidity (90% RH) / Oxygen permeability at low humidity (0% RH) The oxygen transmission rate ratio, expressed as:
[0123] Comparative Example 4 The oxygen permeability of a 21 μm thick (barrier layer thickness 1 μm) PVA (Tg = 71.0°C) coated OPP film (manufactured by Mitsui Chemicals Tohcello Co., Ltd.) is 0.1 cc / (m) at 0% RH. 2 / day / atm), and 600cc / (m at 90% RH 2 / day / atm), and the ratio of oxygen transmission rates at high and low humidity was 6000.
Claims
1. Formula (1), Formula (2), and Formula (3) 【Chemistry 1】 (In the formula, R 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, X represents a divalent organic group having 1 to 20 carbon atoms which may contain an oxygen atom, l, m, and n are numbers representing the molar ratios of the respective monomer structural units, and either l or m may be 0. A copolymer having a monomer structural unit represented by the following formula (A), (B), and (C) which satisfies the following requirements (A), (B), and (C). (A) the molar ratio 1 of the monomer structural unit represented by formula (1), the molar ratio m of the monomer structural unit represented by formula (2), and the molar ratio n of the dialkenyl monomer structural unit represented by formula (3) satisfy the following formula: The relationship 0.1≦[n / (l+m+n)]×100≦65 is satisfied. (B) The weight average molecular weight Mw is 10,000 to 1,000,000. (C) It is not gelled and dissolves in a specified solvent.
2. The copolymer according to claim 1, which satisfies the relationship: 0.1≦[n / (l+m+n)]×100≦20.
3. X is -C 6 H 4 3. The copolymer according to claim 1, wherein
4. R 1 , R 2 and R 4 The copolymer according to any one of claims 1 to 3, wherein is a hydrogen atom.
5. R 3 The copolymer according to any one of claims 1 to 4, wherein is a methyl group.
6. The copolymer according to any one of claims 1 to 5, wherein either l or m is 0.
7. The copolymer according to any one of claims 1 to 6, wherein the predetermined solvent is at least one selected from the group consisting of benzene, toluene, xylene, chloroform, methylene chloride, carbon tetrachloride, dichloroethane, tetrachloroethane, chlorobenzene, dichlorobenzene, trichlorobenzene, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, tetrahydrofuran, methanol, ethanol, isopropanol, n-propanol, 2-butanol, n-butanol, ethyl cellosolve, and butyl cellosolve.
8. 8. An oxygen barrier laminate comprising at least one plastic film layer and at least one oxygen barrier layer comprising the copolymer according to claim 1.
9. 9. The oxygen barrier laminate according to claim 8, wherein the plastic film is a polypropylene film.
Citation Information
Patent Citations
Hydrocarbon oil composition
JP1983049792A
Low-yellowness polymer composition, polymerizable composition and lens made from same
JP1995238120A
Anion selective electrode
JP1998274632A
Process for preparing allyl acetate polymer and allyl alcohol polymer
JP2004256620A
Method for producing composite absorbent material for chromatographic separation of biopolymers