Printing method, thermal transfer printing device, and printed matter
The thermal transfer printing method and device address the challenge of distinguishing genuine prints from copies by using a protective layer with a filler to create an uneven surface, ensuring easy identification of counterfeit copies.
Patent Information
- Application Number
- JP2021025350
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-19
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-02-19
AI Technical Summary
Existing printed materials, such as securities and admission tickets, can be easily forged using color copying machines, and it is difficult to distinguish genuine prints from counterfeit copies due to the challenge of reproducing the glossy silver color of silver ink as a dull grayish color.
A thermal transfer printing method and device that includes a thermal transfer sheet with a protective layer containing a filler, which is transferred only to specific areas of the print, creating an uneven surface that reduces specular gloss in the copy-permitted regions, while maintaining design flexibility.
The method allows easy identification of color-copied copies by changing the specular gloss, making it evident whether the print is genuine or a copy, without affecting the design.
Smart Images

Figure 0007571608000002 
Figure 0007571608000003 
Figure 0007571608000004
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a method for producing a printed matter, a thermal transfer printing device, and a printed matter. [Background technology]
[0002] Due to technological advances in color copiers, printed materials such as securities and admission tickets can easily be counterfeited. As a countermeasure against counterfeiting, a method is known in which some information on a printed material is printed with silver ink. When such a printed material is color-copied, the shiny silver color of the silver ink on the printed material is not reproduced in the copy and becomes gray, making it possible to identify the copied counterfeit.
[0003] However, some people may not notice the change from the shiny silver to a dull light gray and may mistake the color-copied counterfeit for a genuine print. In addition, the area (printing pattern) used for authenticity determination had to be printed in silver ink, which placed restrictions on the design of the image to be printed. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 10-850 Summary of the Invention [Problem to be solved by the invention]
[0005] The present disclosure aims to provide a method for producing a printed matter that allows easy verification of the authenticity of a color-copied copy, and a thermal transfer printing device. Another aim of the present disclosure is to provide a printed matter that allows easy verification of the authenticity of a color-copied copy. [Means for solving the problem]
[0006] The method for manufacturing a printed matter disclosed herein includes the steps of: receiving an input of a copying-permitted area of an image; forming the image on a receiving layer of an image receiving sheet having a substrate, a metal-containing layer provided on the substrate, and a receiving layer provided on the metal-containing layer; and transferring the protective layer containing a filler from a thermal transfer sheet having the protective layer provided thereon to an area on the receiving layer on which the image has been formed, the area corresponding to the copying-permitted area.
[0007] The thermal transfer printing device disclosed herein comprises an input unit that accepts input of a copying-permitted area of an image, a supply unit that supplies a thermal transfer sheet having a colorant layer containing a colorant and a protective layer containing a filler, and a thermal head that heats the colorant layer of the thermal transfer sheet, forms the image on the receiving layer of an image receiving sheet having a substrate, a metal-containing layer provided on the substrate, and a receiving layer provided on the metal-containing layer, heats the protective layer, and transfers the protective layer to an area on the receiving layer where the image has been formed, which corresponds to the copying-permitted area.
[0008] The printed matter of the present disclosure comprises a substrate, a metal-containing layer provided on the substrate, a receiving layer provided on the metal-containing layer and having an image formed thereon, and a protective layer containing a filler provided in an area on the receiving layer corresponding to an area permitted for image copying. Effect of the Invention
[0009] According to the present disclosure, it is possible to produce a printed matter that allows easy verification of the authenticity of a color-copied copy. [Brief description of the drawings]
[0010] [Figure 1] 1 is a schematic configuration diagram of a thermal transfer printing device according to an embodiment of the present disclosure. [Diagram 2] FIG. [Diagram 3] FIG. [Figure 4] FIG. [Diagram 5] FIG. [Figure 6] FIG. [Figure 7] FIG. 13 is a diagram showing a color copy of a printed matter. [Figure 8] FIG. [Figure 9] FIG. [Figure 10] FIG. [Figure 11] FIG. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] Hereinafter, an embodiment of the present disclosure will be described based on the drawings. In order to clarify the description, the drawings may show the width, thickness, etc. of each part in a schematic manner compared to the actual embodiment, but these are merely examples and do not limit the interpretation of the present disclosure. In addition, in the present specification and each drawing, elements similar to those described above with respect to the previous drawings are given the same reference numerals, and detailed descriptions may be omitted as appropriate.
[0012] Fig. 1 is a schematic diagram of a thermal transfer printing device, and Fig. 2 is a plan view of a thermal transfer sheet 5 used in the thermal transfer printing device. The thermal transfer printing device prints an image by transferring color materials such as yellow, magenta, and cyan dyes onto an image receiving sheet 7. The image to be printed is, for example, a human image such as a face image, or text such as an address and name.
[0013] The thermal transfer sheet 5 has a Y layer 51 containing a yellow dye (Y), an M layer 52 containing a magenta dye (M), a C layer 53 containing a cyan dye (C), and a surface protective layer 54 (hereinafter referred to as a protective layer 54) arranged in surface sequence. In other words, when an assembly consisting of four panels, the Y layer 51, the M layer 52, the C layer 53, and the protective layer 54, is defined as "one unit (50)", the thermal transfer sheet 5 has this "one unit (50)" arranged in surface sequence (repeatedly).
[0014] A rotatable platen roll 2 is provided below the thermal head 1. A thermal transfer sheet 5 and an image receiving sheet 7 are sandwiched between the thermal head 1 and the platen roll 2. The thermal head 1 heats the thermal transfer sheet 5, and prints an image by sublimation-transferring Y, M, and C to the image receiving sheet 7, and transfers a protective layer onto the image.
[0015] The thermal transfer sheet 5 is fed from a supply roll 3 , passes through a thermal head 1 , and is collected by a collection roll 4 .
[0016] The thermal transfer printing device comprises a control device 20 that controls the driving of each component, a storage unit 30 that stores image data of the image to be printed, and an input unit 32 that accepts input of the copy-permitted area. The control device 20 comprises a copy-permitted area setting unit 21 and a print control unit 22. The copy-permitted area setting unit 21 and the print control unit 22 may be configured as hardware or software. If configured as software, a program that realizes at least some of the functions may be stored on a recording medium such as a CD-ROM and read and executed by a computer.
[0017] The thermal transfer printing device according to this embodiment produces a print including a copyable portion and a non-copyable portion when copied by a color copier. The input unit 32 accepts input of the area permitted to be copied from the user. The input unit 32 is, for example, a touch panel, a mouse, a keyboard, or the like.
[0018] The copy-permitted-area setting unit 21 sets, as a copy-permitted area, an area of the image to be printed that is input via the input unit 32. The copy-permitted-area setting unit 21 also sets, as a copy-prohibited area, an area of the image to be printed other than the copy-permitted area.
[0019] An input of a copy-prohibited area may be received from a user, and an area other than the copy-prohibited area may be set as a copy-permitted area.
[0020] As will be described later, the print control unit 22 controls the thermal head 1 so as to transfer the protective layer to the copying permitted area and not to transfer the protective layer to the copying prohibited area.
[0021] The thermal transfer sheet 5 has a Y layer 51, an M layer 52, a C layer 53, and a protective layer 54, which are provided in face order on a substrate. Conventionally known materials can be used for the Y layer 51, the M layer 52, the C layer 53, and the substrate. A release layer containing a filler is provided between the protective layer 54 and the substrate.
[0022] The release layer adjusts the adhesion between the substrate and the protective layer 54 and facilitates peeling of the protective layer 54. Such a release layer includes, for example, various waxes such as silicone wax, various resins such as silicone resin, fluororesin, acrylic resin, water-soluble resin, cellulose derivative resin, polyurethane, acetate-based polyvinyl, acrylic vinyl ether resin, and maleic anhydride resin, and mixtures thereof.
[0023] The filler contained in the release layer may be an organic filler, an inorganic filler, or an organic-inorganic hybrid filler. The filler may be in the form of a powder or a sol.
[0024] When the release layer contains a filler, the interface between the release layer and the protective layer 54 becomes uneven due to the filler. When the protective layer 54 is peeled off from the release layer and transferred to a recipient, unevenness is formed on the surface of the protective layer 54 on the recipient.
[0025] The volume average particle diameter of the filler contained in the release layer is preferably 1 μm or more and 10 μm or less, and more preferably 2 μm or more and 5 μm or less. By making the volume average particle diameter of the filler 1 μm or more, it is possible to form a desired unevenness on the surface of the protective layer 54. By making the volume average particle diameter of the filler 10 μm or less, it is possible to maintain ink stability (dispersibility).
[0026] The volume average particle size can be determined by a measuring device using a laser dynamic light scattering method, a method using a TEM, or the BET method (a method in which molecules with a known adsorption area are adsorbed on the surface of powder particles at the temperature of liquid nitrogen, and the specific surface area of the sample is determined from the amount of adsorption). For example, it can be measured in accordance with JIS-Z-8819-2 (issued in 2001) using a particle size distribution / particle size distribution measuring device (e.g., Nanotrac particle size distribution measuring device, manufactured by Nikkiso Co., Ltd.) or a specific surface area / pore size distribution measuring device (e.g., manufactured by Shimadzu Corporation).
[0027] The filler is contained in an amount of preferably 5% by mass or more and 50% by mass or less, and more preferably 10% by mass or more and 30% by mass or less, based on the total solid content of the release layer.
[0028] The thickness of the release layer is preferably from 0.1 μm to 4 μm, more preferably from 0.5 μm to 2 μm. By making the thickness of the release layer within the above preferred range, a transfer product having a deeper matte finish can be produced.
[0029] The protective layer 54 contains a binder resin. There are no particular limitations on the binder resin, so long as it has suitable releasability from the release layer of the thermal transfer sheet and has the desired physical properties as a surface protective layer after transfer. Examples of the binder resin include thermoplastic resins such as cellulose derivatives, such as ethyl cellulose, nitrocellulose, and cellulose acetate, acrylic resins, such as polymethyl methacrylate, polyethyl methacrylate, and polybutyl acrylate, vinyl polymers, such as polyvinyl chloride, vinyl chloride-vinyl acetate copolymer, and polyvinyl butyral, and thermosetting resins, such as unsaturated polyester resins, polyurethane resins, and aminoalkyd resins.
[0030] The thickness of the protective layer is preferably 1 μm or more and 20 μm or less.
[0031] Next, the configuration of the image-receiving sheet 7 will be described. As shown in Fig. 3, the image-receiving sheet 7 includes a substrate 71, and a metal-containing layer 72 and a receiving layer 73 laminated in this order on one surface of the substrate 71. As shown in Fig. 4, an intermediate layer 74 may be provided between the metal-containing layer 72 and the receiving layer 73. Also, a porous layer (not shown) may be provided between the substrate 71 and the metal-containing layer 72. Another layer may be further provided between the layers.
[0032] The 45-degree specular gloss of the receiving layer 73 side of the image-receiving sheet 7 is preferably 800 or more, and more preferably 1000 or more. This allows a print having a high gloss to be produced. The 45-degree specular gloss of the image-receiving sheet is measured in the receiving layer using a glossmeter (VG7000, manufactured by Nippon Denshoku Industries Co., Ltd.) in accordance with the 45-degree specular gloss measurement method described in JIS Z8741.
[0033] Next, each layer of the image-receiving sheet will be described.
[0034] (base material) Examples of the substrate include polyesters such as polyethylene terephthalate (PET), polybutylene terephthalate (PBT), polyethylene naphthalate (PEN), 1,4-polycyclohexylene dimethylene terephthalate, and terephthalic acid-cyclohexanedimethanol-ethylene glycol copolymers; polyamides such as nylon 6 and nylon 6,6; polyolefins such as polyethylene (PE), polypropylene (PP), and polymethylpentene; polyvinyl chloride, polyvinyl alcohol (PVA), polyvinyl acetate, vinyl chloride-vinyl acetate copolymers, and polyvinyl butyrate. Examples of the resin film include films (hereinafter simply referred to as "resin films") made of vinyl resins such as polyvinylpyrrolidone (PVP), (meth)acrylic resins such as polyacrylate, polymethacrylate, and polymethyl methacrylate, imide resins such as polyimide and polyetherimide, cellulose resins such as cellophane, cellulose acetate, nitrocellulose, cellulose acetate propionate (CAP), and cellulose acetate butyrate (CAB), styrene resins such as polystyrene (PS), polycarbonate, and ionomer resins.
[0035] In addition, as the substrate, a paper substrate such as condenser paper, glassine paper, parchment paper, synthetic paper, fine paper, art paper, coated paper, uncoated paper, cast coated paper, wallpaper, cellulose fiber paper, synthetic resin-impregnated paper, backing paper, and impregnated paper (synthetic resin-impregnated paper, emulsion-impregnated paper, synthetic rubber latex-impregnated paper) may be used.
[0036] From the viewpoint of mechanical strength, the thickness of the substrate is preferably 50 μm or more and 300 μm or less.
[0037] (metal-containing layer) The metal-containing layer is a vapor-deposited film or a metal ink layer.
[0038] The type of the deposited film is not particularly limited, and the film can be formed using metals such as aluminum, zinc, silicon, magnesium, calcium, potassium, tin, sodium, titanium, lead, and zirconium, as well as oxides of these metals.
[0039] The thickness of the evaporated film is not particularly limited, and can be, for example, 1 nm or more and 150 nm or less.
[0040] The deposition film can be formed on the surface of a substrate or the like by using a conventionally known method, and examples of such methods include physical vapor deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, as well as chemical vapor deposition methods (CVD methods) such as plasma chemical vapor deposition, thermal chemical vapor deposition, and photochemical vapor deposition.
[0041] The metallic ink layer 7 contains metallic powder and a solvent-based resin.
[0042] The solvent-based resin means a resin that dissolves in a solvent-based solvent. Examples of the solvent-based resin include vinyl chloride resin, vinylidene chloride resin, vinyl acetate resin, acrylic resin, olefin resin, polyester resin, polyurethane resin, and copolymers thereof.
[0043] Examples of the metal powder include gold, silver, copper, aluminum, magnesium, and alloys thereof. The metal powder particles are preferably flake-like or foil-like, and preferably have a thickness of 0.001 μm to 3 μm and an average diameter of 0.1 μm to 100 μm.
[0044] There is no particular limitation on the method for forming the metallic ink layer, but for example, the above-described solvent-based resin can be dissolved in an appropriate solvent-based solvent, to which metal powder and various other components as required are added to prepare a coating liquid for the metallic ink layer, which can be applied to the substrate 71 by a known method such as gravure printing, screen printing, or reverse roll coating using a gravure plate, and then dried to form the metallic ink layer. There is no particular limitation on the thickness of the metallic ink layer, but it is preferably in the range of 0.1 μm to 3 μm.
[0045] (Receptive layer) The receiving layer is a layer that receives the sublimation dye transferred from the dye layer of the thermal transfer sheet and maintains the formed image.
[0046] The receiving layer includes a resin material, and the resin material has transparency and has the above-mentioned 45 degree specular gloss. As long as the above can be achieved, the resin may be, for example, an olefin resin, a vinyl resin, Acrylic resin, cellulose resin, ester resin, amide resin, carbonate resin, Examples of the resin material for the receiving layer include ethylene resin, urethane resin, and ionomer resin. It may contain two or more ingredients.
[0047] The thickness of the receiving layer is preferably from 0.5 μm to 20 μm, more preferably from 1.0 μm to 10 μm, which can improve the density of the image formed on the receiving layer and the prevention of concave curl of the image-receiving sheet.
[0048] (Middle class) The intermediate layer is provided between the metal-containing layer and the receiving layer to improve adhesion between the layers.
[0049] The intermediate layer contains a resin material, and the resin material is not limited as long as it is transparent and can achieve the above-mentioned 45 degree specular gloss, and examples of the resin material include polyester, polyurethane, polycarbonate, (meth)acrylic resin, styrene resin, vinyl resin, and cellulose resin.
[0050] The thickness of the intermediate layer is not particularly limited, and can be, for example, 0.1 μm or more and 3.0 μm or less.
[0051] The intermediate layer can be formed by dispersing or dissolving the above-mentioned materials in water or a suitable solvent to prepare a coating liquid, and then applying this onto the metal-containing layer by a known means such as roll coating, reverse roll coating, gravure coating, reverse gravure coating, bar coating, or rod coating, and drying.
[0052] (Porous layer) The porous layer is composed of a porous film having fine voids therein. Examples of resin materials constituting the porous film include polyolefins such as PE and PP, vinyl resins such as polyvinyl acetate, vinyl chloride-vinyl acetate copolymer and ethylene-vinyl acetate copolymer, polyesters such as PET and PBT, styrene resins, and polyamides.
[0053] (Printed matter) The thermal head 1 of the thermal transfer printing device heats the Y layer 51, M layer 52, and C layer 53 of the thermal transfer sheet 5 based on image data stored in the memory unit 30, and transfers the dye to the receiving layer 73 of the image receiving sheet 7 to form an image.
[0054] Next, the thermal head 1 heats the protective layer 54 of the thermal transfer sheet 5, and transfers the protective layer 54 onto the receiving layer 73 of the image receiving sheet 7, producing the print 10. At this time, as shown in Figures 5 and 6, the protective layer 54 is transferred to the copy permitted area R1, but not to the copy prohibited area R2. Therefore, the surface of the receiving layer 73 is exposed in the copy prohibited area R2. In the example shown in Figure 6, the area of the face image and name is set as the copy prohibited area R2.
[0055] In the copy-permitted area R1, the protective layer 54 with an uneven surface is transferred onto the receiving layer 73. Because the surface of the protective layer 54 is uneven, the 45-degree specular gloss is lower in the copy-permitted area R1 than in the copy-prohibited area R2. For example, the 45-degree specular gloss of the copy-permitted area R1 is approximately 0.1% to 50% of the 45-degree specular gloss of the copy-prohibited area R2.
[0056] Consider the case where this print 10 is reproduced by a color copier. In general, a color copier irradiates light from a light source at an angle of 45° to the normal to the document surface, receives the light reflected and scattered by the document surface at an angle of 0° to the normal to the document surface with a light receiving section such as a CCD, and reads the intensity of the received light.
[0057] Light irradiated from the light source of a color copier onto the copy-permitted area R1 is diffusely reflected by the unevenness of the protective layer surface, and the reflected light reaches the light-receiving section to reproduce the image. On the other hand, light irradiated from the light source onto the copy-prohibited area R2 at 45° is specularly reflected in the -45° direction, and almost none of the reflected light reaches the light-receiving section at 0°. Therefore, as shown in Figure 7, in the copy F, the copy-prohibited area R2 is reproduced as black (or dark gray).
[0058] Since the copy-prohibited area R2 turns black, it is easy to determine whether the print is genuine or a color-copied copy. In addition, since a protective layer with an uneven surface is transferred to the copy-permitted area R1, the design of the image to be printed is not affected.
[0059] 8, the release layer does not contain a filler, and the protective layer 55 having a flat interface with the release layer is transferred onto the receiving layer 73, and the energy applied by the thermal head 1 during transfer is controlled to perform a matte treatment to form an uneven pattern on the surface of the protective layer 55 in the copy-permitted area R1. The energy applied when transferring the protective layer 55 to the copy-permitted area R1 is made higher than the energy applied when transferring the protective layer 55 to the copy-prohibited area R2. In the copy-permitted area R1, the surface of the protective layer 55 has a matte finish with low gloss, and in the copy-prohibited area R2, the surface of the protective layer 55 has a gloss finish with high gloss.
[0060] The uneven pattern that gives the surface of protective layer 55 a matte finish has, for example, an arithmetic mean height Sa of 1.8 μm or more and 2.5 μm or less and a maximum height Sz of 20 μm or more and 50 μm or less, when surface analysis is performed using a laser microscope (manufactured by Keyence Corporation).
[0061] When the print shown in FIG. 8 is color-copied, the copy-prohibited areas will turn black in the copy.
[0062] The thermal transfer sheet 5 may include a protective layer 54 provided on a release layer containing a filler, and a protective layer 55 provided on a release layer not containing a filler. In this case, as shown in Fig. 9, the protective layer 54 having an uneven surface is transferred onto the receiving layer 73 in the copy permitted area R1, and the protective layer 55 is transferred (with a glossy finish) onto the receiving layer 73 in the copy prohibited area R2.
[0063] As shown in Fig. 10, a metal-containing layer 72 may be formed on a substrate 71 only in the copy-prohibited region R2. After an image is formed on the receiving layer 73, a protective layer 55 provided on a release layer that does not contain a filler is transferred in a glossy tone onto the receiving layer 73. Since the copy-permitted region R1 does not have the metal-containing layer 72, the 45-degree specular gloss is low, and when a color copy is made, the image is reproduced in the copy. On the other hand, since the copy-prohibited region R2 has the metal-containing layer 72, the 45-degree specular gloss is high, and when a color copy is made, the copy turns black.
[0064] In the above embodiment, an example was described in which protective layer 54 is provided on a release layer containing a filler, and unevenness is formed on the surface of protective layer 54 transferred onto receiving layer 73, but filler may be contained in the protective layer itself, not in the release layer. As shown in Fig. 11, protective layer 56 containing filler is transferred to duplication permitted area R1.
[0065] The volume average particle diameter of the filler contained in the protective layer 56 is preferably 0.01 μm or more and 10 μm or less. By making the volume average particle diameter of the filler 10 μm or less, the transparency of the protective layer can be maintained. By making the volume average particle diameter of the filler 0.01 μm or more, the dispersibility can be maintained, and the stability of the protective layer coating liquid is improved.
[0066] The filler is contained in an amount of preferably 5% by mass or more and 60% by mass or less, and more preferably 10% by mass or more and 50% by mass or less, based on the total solid content of the protective layer. EXAMPLES
[0067] The present disclosure will now be described in more detail with reference to examples, but the present disclosure is not limited to these examples.
[0068] Example 1 A 25 μm thick PET film (Toyobo Co., Ltd., E5100) was prepared, and a coating liquid for a metal ink layer having the following composition was applied and dried to form a metal ink layer having a thickness of 1.0 μm. Next, a 150 μm thick wood-free paper was prepared, and a coating liquid for an adhesive layer having the following composition was applied and dried to form a 3.0 μm thick adhesive layer, and the adhesive layer was laminated to the metal ink coated surface of the PET film having the metal ink layer. A coating liquid for an intermediate layer having the following composition was applied on this PET surface and dried to form a (transparent) intermediate layer having a thickness of 1.0 μm. A coating liquid for a receiving layer having the following composition was applied on the intermediate layer and dried to form a receiving layer having a thickness of 4.0 μm, and an image receiving sheet of Example 1 was obtained.
[0069] <Coating fluid for metal ink layer> Binder (polyurethane) 20 parts by weight (Nipporun (registered trademark) 5253 Tosoh Corporation) Aluminum pigment (acrylic coating) 10 parts by weight Methyl ethyl ketone (MEK) 150 parts by weight
[0070] <Coating liquid for adhesive layer> Polyol resin 30 parts by weight (Mitsui Chemicals, Takelac (registered trademark) A-969V) Isocyanate compound 10 parts by weight (Takenate (registered trademark) A-5, manufactured by Mitsui Chemicals, Inc.) Ethyl acetate 60 parts by weight
[0071] <Coating fluid for intermediate layer> Urethane resin 30 parts by weight (Manufactured by Tosoh Corporation, Niporun (registered trademark)) Isocyanate 0.5 parts by weight (Tosoh Corporation, Coronate (registered trademark) HX) ·MEK 30 parts by mass
[0072] <Coating solution for receiving layer> Vinyl chloride-vinyl acetate copolymer 60 parts by weight (Nissin Chemical Industry Co., Ltd., Solvine (registered trademark) C) Epoxy modified silicone resin 1.2 parts by weight (Shin-Etsu Chemical Co., Ltd., X-22-3000T) Methylstyrene-modified silicone resin 0.6 parts by weight (Shin-Etsu Chemical Co., Ltd., X-24-510) ·MEK 150 parts by mass Toluene 150 parts by weight
[0073] Example 2 The adhesive layer coating liquid having the above composition was applied to one side of a 150 μm thick piece of wood-free paper and dried to form an adhesive layer having a thickness of 3 μm, and a 25 μm thick aluminum-deposited PET film (Toyobo Co., Ltd., Metalite KY-27-CR, vapor deposition film thickness: 45 nm) was laminated through the adhesive layer so that the aluminum-deposited surface became the adhesive surface. The intermediate layer coating liquid having the above composition was applied to the PET surface of this aluminum-deposited PET film and dried to form an intermediate layer having a thickness of 1 μm. The receiving layer coating liquid having the above composition was applied to the intermediate layer and dried to form a receiving layer having a thickness of 4 μm, and an image-receiving sheet of Example 2 was obtained.
[0074] Example 3 The adhesive layer coating liquid having the above composition was applied to one side of a 150 μm thick wood-free paper and dried to form an adhesive layer having a thickness of 3 μm, and a 35 μm thick porous PP film (Mitsui Chemicals Tohcello Co., Ltd., SP-U) was laminated as a porous layer through the adhesive layer. The metal ink layer coating liquid having the above composition was applied to the porous PP film and dried to form a metal ink layer having a thickness of 1 μm. The receiving layer coating liquid having the above composition was applied to this metal ink layer and dried to form a receiving layer having a thickness of 4 μm, and an image receiving sheet of Example 3 was obtained.
[0075] Comparative Example 1 An image-receiving sheet of Comparative Example 1 was obtained in the same manner as in Example 3, except that instead of the metallic ink layer, a white intermediate layer coating liquid having the following composition was applied to a porous PP film and dried to form a white intermediate layer having a thickness of 1 μm.
[0076] <White intermediate layer coating fluid> Urethane resin 30 parts by weight (Manufactured by Tosoh Corporation, Niporun (registered trademark)) Isocyanate 0.5 parts by weight (Tosoh Corporation, Coronate (registered trademark) HX) Titanium oxide (TCA888, manufactured by Tochem Products Co., Ltd.) 15 parts by weight ·MEK 100 parts by mass
[0077] <<Mirror gloss evaluation>> The image receiving sheet produced in the above examples and comparative examples, a dye-sublimation thermal transfer printer (DS620, manufactured by Dai Nippon Printing Co., Ltd.), and a genuine ribbon for the printer equipped with a dye layer containing a sublimation dye and a protective layer were prepared. In an environment of 20°C and 30% RH, the sublimation dye was sublimated and transferred from the genuine ribbon onto the receiving layer of the image receiving sheet, and the protective layer was also transferred. An 11-step color chart image (a 7-color, 11-step image of Ye, Mg, Cy, BK, R, G, and B) was formed in gloss mode, and a print was obtained. The obtained prints were visually observed and evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1. (Evaluation Criteria) A: It was confirmed that the printed matter had an extremely high mirror gloss. B: It was confirmed that the printed matter had a high mirror gloss. C: The gloss of the printed matter was insufficient.
[0078] <<Surface smoothness evaluation>> The prints produced in the above specular gloss evaluation were visually observed and evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1. (Evaluation Criteria) A: It was confirmed that the printed matter had an extremely high level of surface smoothness. B: It was confirmed that the printed matter had a high level of surface smoothness. C: The surface smoothness of the printed matter was insufficient.
[0079] <<Anti-counterfeiting evaluation>> The prints produced in the above specular gloss evaluation were copied using a color scanner (GT-X830, manufactured by Seiko Epson Corporation) in standard mode, and the copies were evaluated based on the following evaluation criteria. The evaluation results are summarized in Table 1.
[0080] (Evaluation Criteria) A: The image turned black, and it was easy to tell at a glance that it was a copy. B: The image became slightly darker, and it was possible to tell that it was a copy. C: The image was almost completely reproduced, and it was impossible to tell at first glance that it was a copy.
[0081] [Table 1]
[0082] Although the present disclosure has been described in detail with reference to specific embodiments, it will be apparent to those skilled in the art that various modifications can be made without departing from the spirit and scope of the present disclosure. [Explanation of symbols]
[0083] 1 Thermal head 2 Platen Roll 5 Thermal transfer sheet 54, 55, 56 protective layer 7 Receiving sheet 71 Base material 72 Metal-containing layer 73 Receptor
Claims
1. Receiving input of a copy permission area of an image; forming the image on a receiving layer of an image receiving sheet having a substrate, a metal-containing layer provided on the substrate, and a receiving layer provided on the metal-containing layer; a step of transferring a protective layer from a thermal transfer sheet to an area of the receiving layer on which the image is formed, the area corresponding to the copying permitted area, so that an uneven surface is provided; A method for manufacturing a printed matter comprising the steps of:
2. The method for producing a printed matter according to claim 1 , wherein the protective layer is not transferred to an area on the receiving layer that corresponds to a copying prohibited area other than the copying permitted area.
3. Receiving input of a copy permission area of an image; forming the image on a receiving layer of an image receiving sheet having a substrate, a metal-containing layer provided on the substrate, and a receiving layer provided on the metal-containing layer; transferring a protective layer from a thermal transfer sheet onto the receiving layer on which the image is formed; Equipped with A method for manufacturing a printed matter, in which the energy applied to the thermal transfer sheet during protective layer transfer is higher in an area corresponding to the copying-permitted area than in an area corresponding to a copying-prohibited area other than the copying-permitted area, thereby forming a concave-convex pattern on the surface of the protective layer.
4. an input unit for receiving an input of a copy permission area of an image; a supply unit that supplies a thermal transfer sheet having a color material layer including a color material and a protective layer; a thermal head for heating the color material layer of the thermal transfer sheet, forming the image on the receiving layer of an image receiving sheet having a substrate, a metal-containing layer provided on the substrate, and a receiving layer provided on the metal-containing layer, heating the protective layer, and transferring the protective layer so that an uneven surface is provided in an area corresponding to the duplication permitted area on the receiving layer on which the image has been formed; A thermal transfer printing device comprising:
5. A substrate; a metal-containing layer provided on the substrate; a receiving layer provided on the metal-containing layer and having an image formed thereon; a protective layer containing a filler and provided in an area corresponding to an image duplication permitted area on the receiving layer; A printed matter that has the above features.
Citation Information
Patent Citations
Printed matter
JP1998000850A
Duplication preventing medium and manufacture thereof
JP1998081058A
Ink ribbon, printer, and image printing method
JP2007001129A
Thermal transfer image receiving sheet and production method of printed matter
JP2020138411A