Manufacturing method of submerged arc welded joint

The dual flux dispersion port system stabilizes flux distribution in multi-electrode submerged arc welding, addressing gas blow-up and improving weld metal quality by controlling oxygen and nitrogen levels, resulting in enhanced mechanical properties and appearance of submerged arc welded joints.

JP7571694B2Active Publication Date: 2024-10-23JFE STEEL CORP
View PDF 14 Cites 0 Cited by

Patent Information

Application Number
JP2021149351
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-14
Publication Date
2024-10-23
Estimated Expiration
2041-09-14

AI Technical Summary

Technical Problem

Existing multi-electrode submerged arc welding methods face challenges in maintaining sufficient flux dispersion height, particularly around rear electrodes, leading to gas blow-up, increased oxygen and nitrogen content in weld metal, and poor bead appearance due to high arc pressure and gas scattering, especially when using low-density flux with coarse particles.

Method used

Implementing a flux dispersion method with a first and second flux dispersion port, where the second port is positioned horizontally apart from the welding line to stabilize flux distribution across multiple electrodes, ensuring adequate shielding and reducing gas blow-up, thereby controlling oxygen and nitrogen levels in the weld metal.

Benefits of technology

This approach suppresses gas blow-up, maintains stable bead width, reduces oxygen and nitrogen content in the weld metal to desired ranges, and enhances the mechanical properties and appearance of submerged arc welded joints.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571694000008
    Figure 0007571694000008
  • Figure 0007571694000009
    Figure 0007571694000009
  • Figure 0007571694000010
    Figure 0007571694000010
Patent Text Reader

Abstract

To provide a manufacturing method of a multi-electrode submerged arc weld joint.SOLUTION: Steel plates 1 are brought into abutment together, and a submerged arc weld joint is manufactured by multi-electrode submerged arc welding of two or more electrodes. In spraying of a flux 4, the flux 4 is sprayed on a welding line in front of a first electrode in the welding direction from a first flux spraying port 13. Also, at least on one side at a predetermined distance apart horizontally from the weld line from a second flux spraying port 23a, the flux 4 is sprayed in a range from a position in front of a wire tip of the first electrode in the welding direction to a position behind the wire tip of a tail end electrode in the welding direction, and thereby the multi-electrode submerged arc welding is given. As a result, the occurrence of gas blow-up is suppressed to reduce variation of a bead width, and thereby undercut is suppressed. Further, the amount of oxygen and the amount of nitrogen are reduced to predetermined ranges, and thereby the weld joint having a beautiful bead exterior appearance and weld metal with high toughness is obtained.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a submerged arc welded joint formed by butt-jointing thick steel plates and welding them by a multi-electrode submerged arc welding method, and to a method for manufacturing the same. In particular, the present invention relates to a technology for improving the bead appearance of a welded joint, suppressing increases in the oxygen and nitrogen contents of the weld metal, and simultaneously improving the toughness of the weld metal. [Background technology]

[0002] The submerged arc welding method used for welding thick steel plates is characterized by its high efficiency by using a large current, and by using multiple electrodes to increase the deposition rate and further increase the welding speed. For example, in welding large diameter steel pipes, multi-electrode submerged arc welding using four or five electrodes is used (for example, see Patent Document 1).

[0003] In the submerged arc welding method, granular flux is spread on the weld line of steel plates, a welding wire is inserted into the flux, and an arc is generated within the flux to melt the steel plate base material, welding wire, and flux and weld the joint. The molten flux helps to shape the bead surface and isolates the molten metal from the atmosphere, improving the mechanical properties of the weld metal.

[0004] Normally, in multi-electrode submerged arc welding, flux is sprayed from a flux spray port located in front of the first electrode in the welding direction. However, to improve the bead appearance and weld metal properties, it is necessary to ensure a sufficient flux spray height around the electrodes.

[0005] To address such problems, for example, Patent Document 2 describes a submerged arc welding device in which a torch is provided with multiple welding wire supply units spaced apart in the traveling direction (welding direction), and flux supply units are provided at least at the front and rear of the torch in the traveling direction (welding direction).

[0006] Patent Document 3 describes a method of spreading flux in submerged arc welding, in which flux is spread by changing the thickness of the flux so that the rear part of the electrode torch is thicker than the front part, using flux spreader pipes arranged before and after the electrode torch in the welding direction. This method makes it possible to perform submerged arc welding on ascending inclined joints with an inclination angle of 6° or more, and is said to be able to obtain good beads with no molten metal flow.

[0007] Patent Document 4 describes a method of spreading flux in submerged arc welding, in which the flux surface temperature is detected during welding, and the rotation speed of a screw conveyor for spreading flux is controlled based on the result to control the amount of flux spread. This method is said to be capable of controlling the amount of flux spread regardless of the welding conditions.

[0008] Patent Document 5 describes a multi-electrode submerged arc welding method using three or more electrodes, which is characterized by replacing the atmospheric components between the flux particles before dispersion with a gas that does not contain nitrogen gas and covering the area from the leading edge of the flux dispersion position to the rear of the molten pool with a shield cover. This method is said to be able to suppress an increase in the nitrogen content of the weld metal in high-efficiency submerged arc welding.

[0009] Patent Document 6 also describes an apparatus for supplying flux to a submerged welding arc. The apparatus for supplying flux described in Patent Document 6 includes a tank for collecting flux, a divider to which the flux is supplied from the tank by gravity via a passage, and two passages for supplying flux from the divider by gravity to the front and rear of a suspended movable electrode, respectively. In the apparatus described in Patent Document 6, the tank is attached at a predetermined height above the welding arc, and a vacuum device is disposed to collect excess flux behind the movable electrode and guide it to the tank. [Prior art documents] [Patent documents]

[0010] [Patent Document 1] Japanese Patent Application Publication No. 53-119240 [Patent Document 2] Japanese Utility Model Application Publication No. 59-120072 [Patent Document 3] Japanese Patent Application Publication No. 56-009076 [Patent Document 4] Japanese Patent Application Publication No. 03-013274 [Patent Document 5] JP 2010-029931 A [Patent Document 6] Japanese Unexamined Patent Publication No. 55-117594 Summary of the Invention [Problem to be solved by the invention]

[0011] However, the techniques described in Patent Documents 2 to 6 had a problem in that the flux spray height around each electrode in multi-electrode submerged arc welding, particularly the flux spray height around the rear electrode, could not be stably maintained at a sufficient height.

[0012] Usually, in multi-electrode submerged arc welding, the flux is dispersed from a flux dispersion port arranged in front of the first electrode in the welding direction. However, the flux is melted or dispersed by the arc of each electrode, and the flux is pushed away on both sides of the weld line by the forward movement of the electrode, so the flux dispersion height around the electrode becomes lower as the electrode is closer to the rear. Moreover, since a large current is used in submerged arc welding, the arc pressure is high, and the rear electrode with a lower flux dispersion height has a stronger gas blow-up, making it difficult to obtain the effect of isolating the molten metal from the atmosphere. Therefore, the amount of oxygen and nitrogen in the weld metal increases, which reduces the mechanical properties of the weld metal, and the gas blow-up makes it difficult to obtain a beautiful bead appearance. In particular, the more electrodes there are, the stronger this tendency becomes. In particular, when a flux with a low bulk density and a coarse grain size is used, the arc pressure cannot be suppressed by the flux, making it difficult to suppress the occurrence of gas blow-up.

[0013] An object of the present invention is to solve the above-mentioned problems of the conventional technology, and to provide a method for manufacturing a submerged arc welded joint having excellent mechanical properties, which can prevent the occurrence of gas blowing, produce a submerged arc welded joint having a beautiful bead appearance and a weld metal with low amounts of oxygen and nitrogen. [Means for solving the problem]

[0014] In order to achieve the above object, the inventors butted thick steel plates together and produced welded joints using a multi-electrode submerged arc welding method with variously modified flux spraying methods. During welding, the state of gas blowing up was observed, and the bead appearance of the obtained welded joints was observed, and the amounts of oxygen and nitrogen in the weld metal were measured.

[0015] As a result, they came up with the idea of ​​distributing flux from a first flux dispersion port on the weld line forward in the welding direction of the leading electrode (first electrode), and further disposing a second flux dispersion port to spray flux at least on one side at a predetermined distance horizontally from the weld line, and in the range of the electrodes along the welding direction. As a result, they found that it is possible to stably secure the desired flux dispersion thickness from the periphery of the leading electrode to the periphery of the rearmost electrode, prevent gas blowing up during welding, and obtain a submerged arc welded joint with an excellent bead appearance and weld metal with reduced oxygen and nitrogen contents within appropriate ranges.

[0016] The present invention was completed based on these findings and through further investigation, and the gist of the present invention is as follows. [1] A submerged arc welded joint, characterized in that the weld metal of the welded joint contains, by mass%, oxygen: 250 to 350 ppm, nitrogen: 30 to 60 ppm, and the difference between the maximum and minimum bead widths of the weld metal is 3.0 mm or less. [2] A method for manufacturing a submerged arc welded joint, characterized in that when thick steel plates are butted together and a submerged arc welded joint is produced by multi-electrode submerged arc welding, a flux spraying device having first and second flux spraying ports is used, and flux is sprayed from the first flux spraying port onto the weld line forward in the welding direction of a first electrode of the multiple electrodes, and flux is sprayed from the second flux spraying port on at least one side horizontally a predetermined distance from the weld line, in a range from a position forward in the welding direction of the wire tip of the first electrode to a position rearward in the welding direction of the wire tip of the rearmost electrode of the multiple electrodes, and the multi-electrode submerged arc welding is performed. [3] A method for manufacturing a submerged arc welded joint as described in [2], characterized in that the predetermined horizontal distance from the weld line is 20 to 100 mm from the weld line to the end of the second flux spray port. [4] The flux spraying device includes a flux storage tank for storing flux, a first flux delivery pipe connected to the flux storage tank for delivering the flux, a first flux delivery port connected to the first flux delivery pipe for spraying the flux, a second flux delivery pipe connected to the flux storage tank for delivering the flux, and a second flux delivery port connected to the second flux delivery pipe for spraying the flux, and the first flux delivery port is configured to spray the flux onto a weld line ahead of the welding direction of the first electrode. the second flux spray port is a spray port that sprays the flux on at least one side that is a predetermined distance horizontally away from the weld line, and the second flux spray port is arranged so that a front end of the second flux spray port in the welding direction is located forward in the welding direction of the wire tip of the first electrode, and a rear end of the second flux spray port in the welding direction is located rearward in the welding direction of the wire tip of the rearmost electrode. [5] The cross-sectional area of ​​the first flux supply pipe and the second flux supply pipe is 600 mm 2The method for manufacturing a submerged arc welded joint according to [4], characterized in that: [6] A method for manufacturing a submerged arc welded joint described in [4] or [5], characterized in that the inclination angle of the central axis of the first flux feed pipe and the second flux feed pipe with respect to a horizontal plane is 30° or more over their entire length. [7] A method for manufacturing a submerged arc welded joint according to any one of [2] to [6], characterized in that the thick steel plate has a plate thickness of 20 mm or more and a tensile strength of 415 MPa or more. Effect of the Invention

[0017] According to the present invention, it is possible to suppress the occurrence of gas blowing around the electrodes and fluctuations in bead width, and further to reduce the amounts of oxygen and nitrogen to a predetermined range, and it is possible to obtain a multi-electrode submerged arc welded joint having a highly tough weld metal, which is of outstanding industrial value. In addition, according to the present invention, it is possible to suppress undercut by suppressing fluctuations in bead width. [Brief description of the drawings]

[0018] [Figure 1] FIG. 2 is an explanatory diagram showing a schematic example of a flux spraying device that can be used in the present invention. [Diagram 2] FIG. 2 is an explanatory diagram illustrating an example of the arrangement of first and second flux spraying ports. [Diagram 3] FIG. 2 is an explanatory diagram illustrating a groove shape used in the examples. [Figure 4] FIG. 2 is an explanatory diagram showing how to take a Charpy impact test piece. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0019] The present invention is a method for manufacturing a submerged arc welded joint in which thick steel plates are butt-jointed together and a submerged arc welded joint is obtained by multi-electrode submerged arc welding with two or more electrodes.

[0020] The resulting submerged arc welded joint will be a single-layer or multi-layer welded joint depending on the thickness of the steel plate used, the desired welding conditions, and the like.

[0021] In the present invention, the thick steel plate used is preferably a steel plate having a plate thickness of 20 mm or more and a tensile strength of 415 MPa or more.

[0022] Next, the prepared thick steel plates are butted together, a groove having a predetermined shape is formed on the butted surfaces, and multi-electrode submerged arc welding with two or more electrodes is performed using a welding wire and flux to obtain a submerged arc welded joint.

[0023] The welding wire used is preferably selected from solid wires (commercially available) for submerged arc welding that are suitable for the above-mentioned thick steel plate that is the material to be welded and that are specified in JIS Z 3351, but flux cored wires can also be used. From the viewpoint of welding stability, it is preferable that the welding wire used is 2.4 mmΦ or more.

[0024] The flux used is preferably selected from commercially available submerged arc welding fluxes that are suitable for the above-mentioned thick steel plate and are specified in JIS Z 3352. The flux used may be any of molten type, sintered type, and sintered type.

[0025] In the present invention, the welding conditions for multi-electrode submerged arc welding need not be particularly limited as long as the desired welded joint can be formed, and any welding conditions such as the number of electrodes, groove shape, current, voltage, and current density used in a conventional multi-electrode submerged arc welding method can be applied. For example, the distance between adjacent electrodes is preferably 8 to 30 mm, measured at the wire tip positions on the steel sheet surface. If the distance between the electrodes is less than 8 mm, the distance is too narrow and the contact tips for power supply may come into contact with each other, while if the distance exceeds 30 mm, slag inclusion or the like occurs, degrading the quality of the welded portion.

[0026] As for the inclination angle of each electrode, it is preferable that the inclination angle of the first electrode is -20 to 0° with respect to the welding direction, and the inclination angle of the second and subsequent electrodes is in the range of 5 to 25° with respect to the immediately preceding electrode, with a line perpendicular to the steel sheet being taken as 0°. Note that, with regard to the inclination angle, the + side means the forward angle side, and the - side means the reverse angle side.

[0027] The welding speed of the multi-electrode submerged arc welding is not particularly limited and can be appropriately determined as required, but is preferably about 500 to 5000 mm / min from the viewpoint of welding workability.

[0028] In the present invention, flux is preferably sprayed using a flux spraying device 100, an example of which is shown in Fig. 1. The flux spraying device 100 used in the present invention is preferably a device having a first flux spraying port 13 and second flux spraying ports 23a and / or 23b arranged to surround a plurality of electrodes (five electrodes 31 to 35 in Fig. 2), as an example of the arrangement of the flux spraying device 100 is shown in Fig. 2.

[0029] The first flux spray port 13 is disposed at a predetermined position on the weld line ahead of the first electrode 31 of the multiple electrodes in the welding direction so that the flux can be sprayed on the weld line with an appropriate width. The outlet shape of the first flux spray port 13 is not particularly limited, but is preferably circular, square, rectangular, or elliptical. The first flux spray port used does not need to have a constant cross-sectional area, but should have a minimum cross-sectional area of ​​600 mm2 so that the flux does not get clogged in the flux feed pipe. 2 It is preferable that the amount is equal to or more than that.

[0030] Also, the second flux spraying ports 23a, 23b are arranged at least on one side at a horizontal distance B from the weld line so that an appropriate flux spray height can be maintained around the multiple electrodes from the first electrode 31 arranged along the weld line to the rearmost electrode (the fifth electrode 35 in FIG. 2), as shown in FIG. 2(b). It is preferable to arrange the second flux spraying ports on both sides of the weld line as shown in FIG. 2(a), from the viewpoint that the flux can be uniformly sprayed in a direction perpendicular to the weld line and a symmetrical excess weld can be formed with respect to the weld line. The "predetermined distance B" here is the distance B from the weld line to the end of the second flux spraying ports 23a, 23b, and is preferably 20 to 100 mm. If the distance B from the weld line to the end of the flux spray nozzle is less than 20 mm, there is a high risk of interference between the welding torch and the flux spray nozzle. On the other hand, if it exceeds 100 mm, the thickness of the flux sprayed directly above the weld line becomes thin.

[0031] Furthermore, the second flux spray ports 23a, 23b are disposed so that the front end of the second flux spray port in the welding direction is located forward of the tip of the welding wire of the first electrode, and the rear end of the second flux spray port in the welding direction is located rear of the tip of the welding wire of the rearmost electrode, respectively. This makes it possible to maintain a uniform and appropriate flux spray height around the multiple electrodes from the first electrode to the rearmost electrode.

[0032] The shape of the outlet side of the second flux spraying ports 23a and 23b is not particularly limited, but is preferably rectangular. The second flux spraying port used does not need to have a constant cross-sectional area, but should have a minimum cross-sectional area of ​​600 mm2 so that the flux does not clog the flux feed pipe. 2 It is preferable that the amount is equal to or more than that.

[0033] In the flux spraying device 100 used in the present invention, one end of a flux feed pipe is connected to each of the inlets of the flux spraying ports described above, and the other end of the flux feed pipe is connected to a flux storage tank so that the stored flux can be fed to the flux spraying port.

[0034] One end of a first flux supply pipe 12 is connected to the first flux spray port 13, and the other end of the first flux supply pipe 12 is connected to a flux storage tank 11, so that flux can be supplied to the flux spray port. Similarly, one ends of second flux supply pipes 22a and 22b are connected to the second flux spray ports 23a and 23b, respectively, and the other ends of the second flux supply pipes 22a and 22b are connected to a flux storage tank 21(11).

[0035] In the present invention, the connection of the flux spray port, the flux feed pipe, and the flux storage tank is not limited to the above-mentioned connection method. A flux feed pipe may be connected to the flux storage tank, the connected flux feed pipe may be a flux feed pipe that branches off in the middle, and two flux spray ports may be connected to each end of the branch. For example, the flux spraying device used in the present invention may be a device having a flux storage tank that stores flux, a flux feed pipe that is connected to the flux storage tank and feeds the flux, the flux feed pipe that branches off in the middle, a first flux spray port that is connected to one end of the branched flux feed pipe and sprays the flux, and a second flux spray port that is connected to the other end of the branched flux feed pipe and sprays the flux.

[0036] The cross-sectional shape of the flux feed pipe is not particularly limited, but is preferably circular. Furthermore, in order to prevent clogging of the flux feed pipe with the flux, the minimum cross-sectional area of ​​the flux feed pipe is 600 mm 2 More preferably, it is 1200 mm or more. 2The flux feed pipe is preferably made of a material that can be bent relatively freely, such as polyvinyl chloride or silicone rubber, from the viewpoint of workability.

[0037] In addition, it is preferable to arrange the flux supply pipes 12, 22 so that the angle α (°) with respect to the horizontal plane measured along the center line of the pipe is kept at α: 30° or more over the entire length from the flux storage tank 11 (21) to the flux spray port 13, 23. If the inclination of the flux supply pipe with respect to the horizontal plane becomes small, such as α: less than 30°, the flux will be retained inside the pipe, the flux spray height around the electrode will be small, and gas will be easily blown up.

[0038] The flux storage tank 11 (21) is a storage container for storing the flux 4, and is not particularly limited in size, etc., as long as it can store the amount of flux required for submerged arc welding. The flux storage tanks may be provided separately for the first flux spray port 13 and the second flux spray port 23, but there is no problem if they are shared due to the installation location.

[0039] 1 shows only the flux spraying device 100, a plurality of electrodes (contact tips) 3, and the welding wire 2, and does not show the welding wire supply means connected to each electrode, the welding power source, etc., but any common welding device (welding power source, control device, welding machine, etc.) can be used. The flux is preferably sprayed along the welding line before welding, or sprayed forward in the welding direction from the welding point in conjunction with the welding machine.

[0040] In multi-electrode submerged arc welding, the appropriate flux scattering height is preferably a height sufficient to cover the contact tips of each electrode with flux, that is, approximately 30 to 40 mm from the surface of the material to be welded (steel plate).

[0041] In the present invention, when performing multi-electrode submerged arc welding using a flux spraying device for multi-electrode submerged arc welding as shown in Fig. 1, it is preferable to adjust the lower surface height of the flux spraying ports 13, 23a, 23b to the above-mentioned height from the surface of the material to be welded (steel plate). This makes it possible to cover the arcs of the multiple electrodes with flux, prevents gas blowing up during welding, and provides excellent stability in the bead width, resulting in the production of weld metal of excellent quality.

[0042] The submerged arc welded joint obtained by butting the above-mentioned thick steel plates together and subjecting them to multi-electrode submerged arc welding under the above-mentioned welding conditions has a weld metal with a composition containing, by mass%, oxygen: 250 to 350 ppm and nitrogen: 30 to 60 ppm, and with the difference between the maximum and minimum bead widths being 3.0 mm or less.

[0043] When the oxygen content of the weld metal exceeds 350 ppm by mass or the nitrogen content exceeds 60 ppm by mass, grain boundary ferrite is formed, and the toughness of the weld metal decreases. On the other hand, when the oxygen content of the weld metal is less than 250 ppm by mass or the nitrogen content is less than 30 ppm by mass, bainite is formed instead of intragranular acicular ferrite, and the toughness of the weld metal decreases. In order to obtain such oxygen and nitrogen contents in the weld metal, it is necessary to perform stable welding without gas blowing, and for this purpose, it is necessary to adopt a flux spraying method such as that of the present invention, which can ensure a sufficient height for the flux spraying height around the electrode.

[0044] Furthermore, if the difference between the maximum and minimum bead widths of the weld metal exceeds 3.0 mm, an undercut with a depth of 0.5 mm or more will occur, degrading the bead appearance.

[0045] The present invention will now be further described with reference to examples. EXAMPLES

[0046] A thick steel plate (thickness: 38 mm, tensile strength: 590 MPa) having the chemical composition shown in Table 1 was prepared. Two (a pair) test plates (length: 1200 mm) 1, 1' were taken from the prepared thick steel plate, and a one-sided Y groove with an angle of 70° and a groove depth of 15 mm as shown in Figure 3 was prepared as the groove, and the test specimens were butted together. Next, using these test specimens, submerged arc welded joints (length of weld in normal state: 1000 mm) were produced by the multi-electrode submerged arc welding method.

[0047] The multi-electrode submerged arc welding was performed by five-electrode submerged arc welding with the electrode arrangement shown in Table 4, and the flux was sprayed using a flux spraying device for multi-electrode submerged arc welding having first and second flux spray ports, an example of which is shown in Figure 1. The flux used was a commercially available sintered flux (bulk density: 1.2 g / ml, average particle size: 800 μm) with the composition shown in Table 2, as specified in JIS Z 3351, which is compatible with the above-mentioned thick steel plate, and the welding wire used was a commercially available welding wire (diameter: 4.0 mmΦ) with the composition shown in Table 3, as specified in JIS Z 3352, which is compatible with the above-mentioned thick steel plate.

[0048] [Table 1]

[0049] [Table 2]

[0050] [Table 3]

[0051] [Table 4]

[0052] In performing multi-electrode submerged arc welding, the conditions of flux spraying were changed by varying the minimum cross-sectional area and minimum inclination angle of the flux feed pipe in the flux spraying device, as well as the arrangement of the flux spraying port, as shown in Table 5. The arrangements of the flux spraying port used were as shown in Figures 2(a) to (f).

[0053] 2(a) shows a case where the first flux spray port 13 is arranged on the weld line, and the second flux spray ports 23a and 23b are arranged on both sides of the weld line at a predetermined distance B in the horizontal direction, and FIG. 2(b) shows a case where the first flux spray port 13 is arranged on the weld line, and the second flux spray port 23a is arranged on one side at a predetermined distance B in the horizontal direction from the weld line. In both FIG. 2(a) and FIG. 2(b), the second flux spray port 23 is arranged so that its front end in the welding direction is located forward of the welding wire of the first electrode 31 in the welding direction, and its rear end in the welding direction is located rear of the welding wire of the rearmost electrode 35 in the welding direction.

[0054] FIG. 2(c) is a comparative example in which only the first flux spray port 13 is arranged on the weld line, FIG. 2(d) is a comparative example in which only the second flux spray ports 23a and 23b are arranged on both sides of the weld line, separated horizontally by a predetermined distance B, and FIG. 2(e) and FIG. 2(f) are comparative examples in which the first flux spray port 13 is arranged on the weld line, and the second flux spray ports 23a and 23b are arranged on both sides of the weld line, separated horizontally by a predetermined distance B. In FIG. 2(e), the rear ends of the second flux spray ports 23a, 23b in the welding direction are positioned forward of the welding wire of the rearmost electrode 35, and in FIG. 2(f), the front ends of the second flux spray ports 23a, 23b in the welding direction are positioned rearward of the welding wire of the first electrode.

[0055] The first flux spray port 13 has a circular cross section, and the cross section on the spray port outlet side has a cross section area equal to or larger than the minimum cross section of the flux feed pipe. The second flux spray port 23a has a cross section on the spray port outlet side has a cross section area equal to or larger than the minimum cross section of the flux feed pipe.

[0056] In order to allow gravity feeding of the flux, the cross-sectional area of ​​the flux feed pipes 12 and 22 was set within the appropriate range shown in Table 5, and the minimum inclination angle α of the flux feed pipes with respect to the horizontal plane throughout the entire path was adjusted to the angle shown in Table 5. The flux feed pipes were made of silicone rubber.

[0057] Then, multi-electrode submerged arc welding was performed. The welding conditions were as shown in Table 6. The welding speed was 1000 mm / min, and the welding heat input was 9.83 kJ / mm. In addition, for welded joint No. 13, Ar gas was blown into the flux storage tank before welding to perform gas purging to expel air present between the flux grains.

[0058] [Table 5]

[0059] [Table 6]

[0060] During welding, the time during which gas blowing occurred was measured. From the obtained time during which gas blowing occurred, the gas blowing property was evaluated as follows: no gas blowing occurred, ◯, when gas blowing occurred for less than 3 consecutive seconds, ×, when gas blowing occurred for 3 consecutive seconds or more.

[0061] In addition, the bead was observed for the steady portion of the obtained welded joint, and if undercut was found, a sample was taken from the portion and the cross-sectional macro shape was observed to measure the depth of the undercut. The occurrence of the undercut was evaluated as follows: no undercut: ⊚, undercut with a depth of less than 0.5 mm: ◯, undercut with a depth of 0.5 mm or more: ×.

[0062] Furthermore, for the steady part of the obtained welded joint, the bead width was measured from the surface with a vernier caliper at 10 mm intervals along the weld bead, the maximum and minimum values ​​were obtained, and the difference between them was calculated. The bead width stability was then evaluated as follows: if the difference between the maximum and minimum values ​​of the obtained bead width was less than 2.0 mm, it was marked as ◎, if it was 2.0 mm or more and 3.0 mm or less, it was marked as ◯, and if it exceeded 3.0 mm, it was marked as ×.

[0063] Furthermore, analytical samples were taken from the weld metal portion of the obtained welded joint at 100 mm intervals along the welding direction, and the oxygen and nitrogen contents of the weld metal were analyzed using infrared absorption analysis to determine the maximum and minimum values ​​of the oxygen and nitrogen contents in the welded joint.

[0064] In addition, Charpy impact test specimens (V notch) were taken from the weld metal of the obtained welded joint at 100 mm intervals along the welding direction, from a position 2 mm below the surface of the steel plate, so that the notch position was at the center of the weld metal. Then, a Charpy impact test was performed at a test temperature of -30°C, and the absorbed energy vE -30 The impact properties were evaluated by measuring the Charpy impact strength (J). The positions of the Charpy impact test pieces (V notch) are shown in Figure 4.

[0065] The results obtained are shown in Table 7.

[0066] [Table 7]

[0067] In all of the examples of the present invention, no gas blowing occurred for more than 3 consecutive seconds during welding (ratings: ◎ and ◯), making it possible to prevent gas blowing.In addition, the difference between the maximum and minimum bead widths of the weld metal was 3.0 mm or less (ratings: ◎ and ◯), indicating excellent bead width stability.Furthermore, the oxygen content in the weld metal was 250 ppm by mass or more and 350 ppm by mass or less, and the nitrogen content was 30 ppm by mass or more and 60 ppm by mass or less, reducing the oxygen and nitrogen contents in the weld metal to within the appropriate range, thereby improving the toughness of the weld metal.

[0068] Furthermore, in the present invention, the cross-sectional area of ​​each of the flux feed pipes 12 and 22 is 600 mm 2 As described above, in the case of welded joints No. 6 to No. 8, which satisfy the following conditions: the minimum inclination angle of the flux supply pipes 12, 22 with respect to the horizontal plane is 30° or more, the second flux spray port 23 is provided on both sides of the weld line, and the specified horizontal distance B from the weld line is within the range of 20 to 100 mm, there is no occurrence of gas blowing up (◎), the difference between the maximum and minimum values ​​of the bead width is less than 2.0 mm (◎), the bead width stability is particularly excellent, there is no occurrence of undercut, and the oxygen and nitrogen amounts in the weld metal are kept low within appropriate ranges, thereby improving the toughness of the weld metal.

[0069] On the other hand, in the comparative example in which the flux was sprayed outside the range of the present invention, gas blowing occurred violently during welding, the bead width became unstable, and deep undercut occurred. In addition, the oxygen content in the weld metal exceeded 350 mass ppm, the nitrogen content exceeded 60 mass ppm, and the Charpy impact test absorption energy vE -30 In welded joint No. 13, the oxygen content of the weld metal was less than 250 mass ppm and the nitrogen content was less than 30 mass ppm due to gas purging, and the vE -30 The weld metal toughness was reduced to less than 100 J. [Explanation of symbols]

[0070] 1 thick steel plate 2. Welding wire 3 Contact tip (electrode) 4. Flux 7 Welding metal 8 Charpy impact test specimen 11 Flux storage tank (flux hopper) 12 First flux delivery tube 13 First flux spray nozzle 21 Flux storage tank (flux hopper) 22, 22a, 22b Second flux delivery tube 23, 23a, 23b Second flux spray port 31 1st electrode 35 Last electrode (5th electrode) 100 Flux spraying device for multi-electrode submerged arc welding (Flux spraying device)

Claims

1. 1. A method for manufacturing a submerged arc welded joint, comprising the steps of: butting thick steel plates together and producing a submerged arc welded joint by multi-electrode submerged arc welding; using a flux spraying device having first and second flux spraying ports, spraying flux from the first flux spraying port onto a weld line forward in the welding direction of a first electrode of the multiple electrodes; and spraying flux from the second flux spraying port on at least one side horizontally a predetermined distance from the weld line, in a range from a position forward in the welding direction of the wire tip of the first electrode to a position rearward in the welding direction of the wire tip of the rearmost electrode of the multiple electrodes, thereby performing the multi-electrode submerged arc welding.

2. 2. The method for manufacturing a submerged arc welded joint according to claim 1, wherein the predetermined horizontal distance from the weld line is a distance from the weld line to an end of the second flux spray port, the distance being 20 to 100 mm.

3. The flux spraying device includes a flux storage tank for storing flux, a first flux delivery pipe connected to the flux storage tank for delivering the flux, a first flux delivery port connected to the first flux delivery pipe for delivering the flux, a second flux delivery pipe connected to the flux storage tank for delivering the flux, and a second flux delivery port connected to the second flux delivery pipe for delivering the flux, and the first flux delivery port delivers the flux onto a weld line ahead of the welding direction of the first electrode.

3. The method for manufacturing a submerged arc welded joint according to claim 1, wherein the first flux spray port is a flux spray port that sprays the flux on at least one side horizontally a predetermined distance away from the weld line, and the second flux spray port is arranged so that a front end of the second flux spray port in the welding direction is located forward in the welding direction of the position of the wire tip of the first electrode, and a rear end of the second flux spray port in the welding direction is located rearward in the welding direction of the position of the wire tip of the rearmost electrode.

4. The cross-sectional area of ​​the first flux delivery pipe and the second flux delivery pipe is 600 mm 2 The method for manufacturing a submerged arc welded joint according to claim 3,

5. 5. The method for manufacturing a submerged arc welded joint according to claim 3, wherein the inclination angle of the central axis of the first flux feed pipe and the central axis of the second flux feed pipe with respect to a horizontal plane is 30° or more over the entire length.

6. The method for manufacturing a submerged arc welded joint according to any one of claims 1 to 5, characterized in that the thick steel plate has a plate thickness of 20 mm or more and a tensile strength of 419 MPa or more.

Citation Information

Patent Citations

  • Automatic arc welding method for high efficiency multielectrodes of low temperature high toughness steel

    JP1978119240A

  • Device for feeding flux to submerged welding arc

    JP1980117594A

  • Flux spraying method of submerged arc welding

    JP1981009076A

  • Submerged arc welding device and oil - -

    JP1984120072U

  • Flux spreader

    JP1985046971U