Method for manufacturing solid electrolyte member

The described method addresses the inefficiencies of existing sulfide solid electrolyte production by using a solid-liquid reaction with excess elemental sulfur, facilitating the production of high-ionic conductivity electrolytes suitable for lithium ion batteries without the need for mechanical milling.

JP7571700B2Active Publication Date: 2024-10-23MITSUBISHI MATERIALS CORP
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021157530
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-09-28
Publication Date
2024-10-23
Estimated Expiration
2041-09-28

AI Technical Summary

Technical Problem

Existing methods for producing sulfide solid electrolytes, such as mechanical milling and adding elemental sulfur at low ratios, are energy-intensive, time-consuming, and difficult to scale up, leading to challenges in achieving sufficient ionic conductivity and industrial scalability.

Method used

A method involving the preparation of an aggregate of starting materials with a volume ratio of elemental sulfur to the entire aggregate of 20% or more, heated to 120°C, followed by a solid-liquid reaction at temperatures between 400°C and 1000°C, without mechanical milling, to promote elemental diffusion and chemical reactions, resulting in a solid electrolyte member with sufficient ionic conductivity.

Benefits of technology

This method enables the easy production of sulfide-based solid electrolytes with enhanced ionic conductivity, suitable for lithium ion secondary batteries, by promoting elemental diffusion and crystal growth while avoiding energy-intensive mechanical milling and reducing impurity phases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007571700000002
    Figure 0007571700000002
  • Figure 0007571700000003
    Figure 0007571700000003
  • Figure 0007571700000001
    Figure 0007571700000001
Patent Text Reader

Abstract

To produce a solid electrolyte member having sufficient ionic conductivity with ease.SOLUTION: A production method of a sulfide-based solid electrolyte member includes: a preparation step to prepare an assembly of starting materials which consist of a material for an electrolyte containing at least one element other than sulfur out of elements constituting the solid electrolyte member and elemental sulfur; and a generation step to generate the solid electrolyte member by heating the assembly of starting materials. In the preparation step, a volume ratio of the elemental sulfur to the total assembly when heated to 120°C in the assembly of the starting materials is 20% or more.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a solid electrolyte member. [Background technology]

[0002] In recent years, sulfide-based solid electrolytes, which have high ionic conductivity and are safer than electrolyte solutions, have been attracting attention as electrolytes for lithium-ion secondary batteries. As a method for producing a sulfide solid electrolyte, a process is generally adopted in which a mixture of raw materials is first subjected to mechanical milling to vitrify or amorphize, and then heat-treated to synthesize a sulfide solid electrolyte by a solid-phase reaction. Patent documents 1 and 2, and Examples 5-13 of Patent document 3, describe a method for producing a sulfide solid electrolyte by mechanical milling a mixture of raw materials to vitrify or amorphize, and then heat-treated. Patent Document 4 discloses a method for producing a sulfide solid electrolyte, in which elemental sulfur or a sulfur compound is mixed with a raw material in a ratio of 5 wt% or more of the entire mixture, and the mixture is heat-treated. It is described that this production method can achieve ionic conductivity equivalent to that achieved by passing hydrogen sulfide gas through the heat treatment, even without using hydrogen sulfide gas. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2003-208919 A [Patent Document 2] Patent No. 5527673 [Patent Document 3] Patent No. 5888609 [Patent Document 4] JP 2020-27715 A Summary of the Invention [Problem to be solved by the invention]

[0004] As disclosed in Patent Documents 1-3, when producing a sulfide solid electrolyte, a method of performing mechanical milling on a mixture of raw materials is common. The advantage of mechanical milling is that the elements contained in the raw materials can be mixed at the atomic level to homogenize the chemical composition of the entire raw material mixture. Therefore, it is an essential process when producing sulfide glass and glass ceramics as a sulfide solid electrolyte, and also when producing a crystalline sulfide solid electrolyte, it facilitates the production of a solid electrolyte during subsequent heat treatment. However, mechanical milling requires a large amount of energy and a long time to be performed properly, and it is difficult to scale up to an industrial scale, which is a factor that makes it difficult to realize an easy method for producing a sulfide solid electrolyte. In addition, Patent Document 4 discloses a method for producing a sulfide solid electrolyte by calcining a mixture in which elemental sulfur or a sulfur compound is added to an electrolyte raw material, but the addition ratio of elemental sulfur is significantly different from that of the present invention. In the case of a small addition ratio of elemental sulfur of 5 wt% of the entire raw material mixture as described in claim 2, even if the raw material mixture is heated to a temperature exceeding the melting point of elemental sulfur, most of the electrolyte raw material cannot come into contact with the molten liquid sulfur. Therefore, most of the electrolyte raw material has to go through a solid-phase reaction, not a solid-liquid reaction in which element diffusion is likely to occur and a solid electrolyte is easily produced. Therefore, with regard to Patent Document 4, there is room for improvement in the production process of the sulfide solid electrolyte, and furthermore, in the ionic conductivity of the produced solid electrolyte. For these reasons, there is a need for a method for easily producing a solid electrolyte having sufficient ionic conductivity.

[0005] The present invention has been made in view of the above, and has an object to provide a method for manufacturing a solid electrolyte member that can easily manufacture a solid electrolyte member having sufficient ionic conductivity. [Means for solving the problem]

[0006] In order to solve the above-mentioned problems and achieve the object, the manufacturing method of a solid electrolyte member according to the present disclosure is a manufacturing method of a sulfide-based solid electrolyte member, and includes a preparation step of preparing an assembly of starting materials using elemental sulfur and an electrolyte raw material containing at least an element other than sulfur among the elements constituting the solid electrolyte member as starting materials, and a production step of heating the assembly of starting materials to produce the solid electrolyte member, wherein in the preparation step, when the assembly of starting materials is heated to 120°C, a volume ratio of the elemental sulfur to the entire assembly of starting materials is 20% or more.

[0007] It is preferable that, when the aggregate of starting materials is heated to 120° C., the volume ratio of the elemental sulfur to the entire aggregate of starting materials is 40% or more.

[0008] In the generating step, the aggregate of the starting materials is preferably heated at a heating temperature of 400° C. or more and 1000° C. or less.

[0009] In the preparation step, it is preferable to prepare an assembly of the starting materials by mixing the elemental sulfur and the electrolyte raw material so that, when the prepared assembly of the starting materials is measured by an X-ray diffraction method, a diffraction peak due to a crystalline substance contained in the elemental sulfur and the electrolyte raw material can be detected.

[0010] The solid electrolyte member is LGPS (Li 10 GeP2S 12 When the compound is subjected to X-ray diffraction measurement using CuKα radiation, the following peaks of the formulas (B1) to (B6) are detected as diffraction peaks, and as for the peak of the formula (B7), either no peak is detected or the diffraction intensity of the peak of the formula (B6) is smaller than I A The diffraction intensity of the peak of formula (B7) is I B In this case, I A I B The diffraction intensity I such that the peak intensity ratio of BIt is preferable to produce a solid electrolyte member in which a peak represented by the formula (B7) is detected. 2θ=17.38°±1.0° (B1) 2θ=20.18°±1.0° (B2) 2θ=20.44°±1.0° (B3) 2θ=23.96°±1.0° (B4) 2θ=26.96°±1.0° (B5) 2θ=29.58°±1.0° (B6) 2θ=27.33°±1.0° (B7)

[0011] As the solid electrolyte member, it is preferable to manufacture a solid electrolyte member having an Argyrodite type crystal structure.

[0012] The solid electrolyte member is Li a M b S c It is preferable to produce a solid electrolyte member having a crystal structure of the space group Pnma, and in which, when measured by an X-ray diffraction method using CuKα radiation, peaks of the following formulae (C1) to (C4) are detected as diffraction peaks. 2θ=17.01±0.50 (C1) 2θ=18.50±0.50 (C2) 2θ=25.31±0.50 (C3) 2θ=26.23±0.50 (C4) Here, M is at least one element of Group 13, Group 14, and Group 15, and a, b, and c are numbers greater than 0. Effect of the Invention

[0013] According to the present invention, a solid electrolyte member having sufficient ionic conductivity can be easily produced. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a flowchart showing a method for manufacturing a solid electrolyte member according to the first embodiment. [Diagram 2] FIG. 2 is a schematic diagram of equipment for producing a solid electrolyte member. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The present invention will be described in detail below with reference to the drawings. Note that the present invention is not limited to the following modes for carrying out the invention (hereinafter, referred to as embodiments). Furthermore, the components in the following embodiments include those that a person skilled in the art can easily imagine, those that are substantially the same, and those that are within the so-called equivalent range. Furthermore, the components disclosed in the following embodiments can be appropriately combined.

[0016] (First embodiment) FIG. 1 is a flow chart showing a method for manufacturing a solid electrolyte member according to a first embodiment. The solid electrolyte member according to this embodiment is a sulfide-based solid electrolyte. The solid electrolyte member according to this embodiment is a lithium ion conductor containing Li, P, and S, and is used, for example, in lithium ion secondary batteries. More specifically, the solid electrolyte member according to this embodiment is a so-called LGPS (Li 10 GeP2S 12 ) type crystal structure. Specifically, the solid electrolyte member according to this embodiment has a chemical formula of Li a M b P c S d Here, a, b, c, and d are numbers greater than 0. The element M is at least one element of Groups 13, 14, and 15. In this embodiment, the element M is preferably at least one of Si, Ge, Sn, and Sb. The solid electrolyte member according to this embodiment contains one type of element M, but may contain multiple types of elements M. Thus, the solid electrolyte member according to the present embodiment is a solid electrolyte containing lithium, element M, phosphorus, and sulfur, but is not limited thereto, and may be a sulfide-based solid electrolyte containing a component other than lithium, element M, and phosphorus. In addition, the solid electrolyte member is not limited to one having an LGPS-type crystal structure, and may be a sulfide-based solid electrolyte containing Li a Mb P c S d Other examples of the composition of the solid electrolyte member will be described later.

[0017] As shown in FIG. 1, in the manufacturing method of this embodiment, first, in a preparation step, an assembly of starting material A of the solid electrolyte member is prepared (step S10). The starting materials A are each of the raw materials containing the elements that constitute the solid electrolyte member, and the aggregate of the starting materials A here refers to a mixture (stirring) of the powders of each of the raw materials (each of the starting materials A) without chemical changes to each of the raw materials. Here, it is preferable that each raw material is mixed so as to be uniformly dispersed. In other words, the starting materials A refer to one type of raw material, and the aggregate of the starting materials A refers to an aggregate of each of the starting materials A mixed together. In addition, the aggregate of the starting materials A refers to an aggregate of the raw materials in a state before the process of producing the solid electrolyte member is started, rather than an intermediate product produced during the process of producing the solid electrolyte member. Furthermore, the aggregate of the starting materials A here refers to an aggregate of the raw materials in a state before being stored in the furnace 10 described below. In this production method, the starting material A is made up of the electrolyte raw material and elemental sulfur.

[0018] (Raw material for electrolyte) The electrolyte raw material is a material containing at least an element other than sulfur among the elements constituting the solid electrolyte member. That is, the electrolyte raw material may be a non-sulfide that does not contain sulfur (including one containing sulfur as an inevitable impurity) or a sulfide that contains sulfur, but is not elemental sulfur. More specifically, the electrolyte raw material is preferably at least one of an element other than sulfur that constitutes the solid electrolyte member, a compound of elements other than sulfur that constitute the solid electrolyte member, and a sulfide of an element other than sulfur that constitutes the solid electrolyte member. In this embodiment, it is preferable that the solid electrolyte member does not contain elements other than the elements constituting the solid electrolyte member, except for inevitable impurities.

[0019] The amount of the electrolyte raw material to be mixed can be calculated from the composition of the solid electrolyte member to be manufactured and the mass of the solid electrolyte member to be manufactured. That is, the electrolyte raw material is selected so that the solid electrolyte member to be manufactured has a desired composition (here, Li a M b P c S d ) and are weighed out and mixed in a mass ratio to obtain the desired mass.

[0020] In this embodiment, the solid electrolyte member is Li a M b P c S d Therefore, the electrolyte raw material is preferably at least one of element lithium, element M, element phosphorus, a compound consisting of at least two of lithium, element M, and phosphorus, and a sulfide of at least one of lithium, element M, and phosphorus. When there are multiple types of element M, each element M may be prepared as an element, or a compound of elements M together or a solid solution of elements M together (e.g., Si-Ge solid solution, Si-Sn solid solution, Ge-Sn solid solution, etc.) may be prepared, or a sulfide of a solid solution of elements M together (i.e., SiGeS 4、 As a compound consisting of at least two of lithium, element M, and phosphorus, a compound consisting of lithium and element M (e.g., Li 22 Si5, Li 17 Ge4, Li 17 Sn4, etc.), compounds of lithium and phosphorus (e.g. Li3P), compounds of element M and phosphorus (e.g. SiP, GeP, Sn3P4, etc.), and compounds of lithium, element M, and phosphorus (e.g. Li5SiP3, Li5GeP3, Li5SnP3, etc.).

[0021] More specifically, in this embodiment, the electrolyte raw material includes a Li raw material containing lithium, an M raw material containing the element M, and a P raw material containing phosphorus.

[0022] (Li raw material) When the Li raw material is a non-sulfide, it is at least one of elemental lithium, a compound of lithium and element M, a compound of lithium and phosphorus, and a compound of lithium, element M, and phosphorus. When the Li raw material is a sulfide, it is at least one of a compound of lithium and sulfur (lithium sulfide), a compound of lithium, element M, and sulfur (e.g., Li4SiS4, Li4GeS4, Li4SnS4, etc.), a compound of lithium, phosphorus, and sulfur (e.g., Li3PS4), and a compound of lithium, element M, phosphorus, and sulfur. When the Li raw material is a compound of lithium and another element, the Li raw material also serves as a raw material of the other element. For example, when the Li raw material is a compound of lithium and phosphorus, the compound of lithium and phosphorus can be said to be a Li raw material and a P raw material.

[0023] (M raw material) When the M raw material is a non-sulfide, it is at least one of a simple substance of element M, a compound of lithium and element M, a compound of element M and phosphorus, and a compound of lithium, element M and phosphorus. When the M raw material is a sulfide, it is at least one of a compound of element M and sulfur (e.g., SiS, SiS2, GeS, GeS2, SnS, SnS2, etc. Also, when there are multiple types of element M, it is at least one of a compound of lithium, element M and sulfur (e.g., Li4SiS4, Li4GeS4, Li4SnS4, etc.), a compound of element M, phosphorus and sulfur, and a compound of lithium, element M, phosphorus and sulfur.

[0024] (P raw material) When the P raw material is a non-sulfide, it is at least one of a phosphorus element, a compound of lithium and phosphorus, a compound of element M and phosphorus, and a compound of lithium, element M and phosphorus. When the P raw material is a sulfide, it is at least one of a compound of phosphorus and sulfur (phosphorus sulfide), a compound of lithium, phosphorus and sulfur (e.g., Li3PS4), a compound of element M, phosphorus and sulfur, and a compound of lithium, element M, phosphorus and sulfur.

[0025] In the present production method, a plurality of types of electrolyte raw materials having different chemical compositions may be prepared, or a single type of electrolyte raw material may be prepared. The electrolyte material is preferably in a particulate (powder) form.

[0026] (elemental sulfur) Elemental sulfur refers to sulfur that does not contain elements other than sulfur, except for inevitable impurities. In other descriptions of this embodiment, each raw material may contain inevitable impurities unless otherwise specified. In addition, the elemental sulfur to be added may be any of α sulfur (orthorhombic sulfur), β sulfur (monoclinic sulfur), γ sulfur (monoclinic sulfur), and other sulfur allotropes.

[0027] In the preparation step, the amount of elemental sulfur added as the starting material A is adjusted to a value corresponding to the amount of the solid electrolyte material (Li a M b P c S d), that is, the amount of elemental sulfur in the stoichiometric ratio is made larger than the amount of elemental sulfur necessary and sufficient to produce the starting material A. Specifically, the volume ratio of elemental sulfur in the assembly of starting material A when the assembly of starting material A is heated to 120°C is the volume ratio of elemental sulfur. That is, the volume ratio of elemental sulfur added refers to the ratio of the total volume of elemental sulfur contained in the assembly of starting material A in an environment of 120°C to the total volume of the assembly of starting material A in an environment of 120°C where elemental sulfur melts. In this case, in the present manufacturing method, elemental sulfur is added to the electrolyte raw material to prepare the assembly so that the volume ratio of elemental sulfur is 20% or more. In addition, in the present manufacturing method, the volume ratio of elemental sulfur added is preferably 40% or more, and more preferably 55% or more. By setting the volume ratio of elemental sulfur added in this range, the molten liquid sulfur can permeate the entire electrolyte raw material in a solid powder form and make sufficient contact with it. As a result, the element diffusion and chemical reaction of the electrolyte raw material are promoted by the solid-liquid reaction, and a solid electrolyte member having sufficient ionic conductivity can be easily manufactured. Furthermore, when manufacturing a solid electrolyte member having an LGPS crystal structure, by setting the volume ratio of the additive within the above range, the generation and crystal growth of the solid electrolyte member are promoted, and the generation of sulfur deficiency and by-products (heterogeneous phases or impurity phases) is suppressed, so that the decrease in the ionic conductivity of the solid electrolyte member can be appropriately suppressed.

[0028] In the preparation step, the volume ratio of the added sulfur is preferably 80% or less, more preferably 70% or less, and even more preferably 60% or less. By setting the volume ratio of the added sulfur in this range, the risk of clogging of the device piping due to gasified sulfur is suppressed, and the solid electrolyte member can be appropriately manufactured.

[0029] The volume ratio of addition can be calculated from the mass and density of the electrolyte raw material blended as the starting raw material A and the mass and density of the elemental sulfur added as the starting raw material A. That is, the volume of the electrolyte raw material at 120 ° C. at which elemental sulfur melts is calculated from the mass and density of the electrolyte raw material to be blended, the volume of elemental sulfur at 120 ° C. is calculated from the mass and density of the elemental sulfur to be added, and the calculated volume of elemental sulfur is divided by the sum of the volume of the electrolyte raw material and the volume of elemental sulfur to be added, and the value expressed as a percentage is the volume ratio of addition. In other words, the amount of elemental sulfur to be added can be calculated as follows. First, the required mass of the electrolyte raw material is calculated from the mass of the solid electrolyte member to be manufactured, and the volume of the electrolyte raw material at 120 ° C. is calculated from the required mass of the electrolyte raw material and the density of the electrolyte raw material. Then, the required volume of elemental sulfur at 120 ° C. is calculated from the volume of the electrolyte raw material at 120 ° C. and the target volume ratio of addition. Then, the amount of elemental sulfur to be added (mass of elemental sulfur to be added) is calculated from the required volume of elemental sulfur at 120° C. and the density of elemental sulfur.

[0030] (Mixing method) Next, a method for mixing each raw material will be described. In the preparation step, the raw materials for the electrolyte are weighed to have the above-mentioned mass ratio, and the elemental sulfur is weighed to have the above-mentioned volume ratio of addition. Then, the raw materials for the electrolyte and the elemental sulfur are used as starting raw material A, and the raw materials of starting raw material A are mixed to form an aggregate of starting raw material A. There are no particular limitations on the equipment or tools used for mixing, and mixing can be done with a general mixer, blender, ball mill, bead mill, mortar, or the like. In this embodiment, the electrolyte raw material and elemental sulfur are weighed and mixed in a glove box in an argon atmosphere with a low dew point temperature and oxygen concentration, but the present invention is not limited thereto, and they may be mixed in an inert gas atmosphere such as nitrogen. In this embodiment, the mixed electrolyte raw material and elemental sulfur are heat-treated in particulate (powder) form, but they may be molded into pellets or other shapes.

[0031] In the preparation step, the raw materials (electrolyte raw materials and elemental sulfur) weighed as starting raw material A are mixed to form an aggregate of starting raw material A. When mixing the raw materials, mechanical milling may be performed to make the entire raw materials amorphous or vitrified, and the chemical composition of the entire raw materials may be homogenized at the atomic level. When mechanical milling is performed and the X-ray diffraction pattern of the aggregate of starting raw material A is measured, diffraction peaks due to crystalline substances not contained in the electrolyte raw materials and elemental sulfur that constitute starting raw material A may be detected. However, in the present manufacturing method, since the solid-liquid reaction can promote the element diffusion and chemical reaction of the electrolyte raw materials, a solid electrolyte having sufficient ionic conductivity can be manufactured without necessarily performing mechanical milling. Therefore, it is economically preferable to limit the mixing to the extent that each raw material is uniformly dispersed without mechanical or chemical changes, without performing mechanical milling, which requires a large amount of energy and a long time. In this case, when the X-ray diffraction pattern of the aggregate of starting raw material A is measured, diffraction peaks due to crystalline substances contained in the electrolyte raw materials and elemental sulfur constituting starting raw material A are detected, and diffraction peaks due to other crystals are not detected, so that such an X-ray diffraction pattern can be said to be preferable as the measurement result of the X-ray diffraction of the aggregate of starting raw material A.

[0032] In the preparation step, the mixing conditions for each raw material are set, for example, to a mixing time of 10 minutes or less and an upper limit of the load per unit area applied in the shear direction of 0.1 N / mm 2 If the ratio is set to the range below, energy consumption in the mixing step can be suppressed, which is economically and rationally preferable. In this case, for example, when Li2S, metallic Ge (simple Ge), and simple P are used as the electrolyte raw materials, when an aggregate of starting raw material A, which is a mixture of electrolyte raw materials and simple sulfur, is measured by X-ray diffraction using CuKα radiation, at least the peaks of the following formulas (A1) to (A6) are detected as diffraction peaks. Note that the diffraction peak here refers to a peak whose intensity is equal to or greater than a threshold value, and the threshold value here is, for example, a relative intensity of 5 when the maximum peak intensity of the measurement result is taken as 100.

[0033] 2θ=23.06±0.50 (A1) 2θ=27.00±0.50 (A2) 2θ=27.28±0.50 (A3) 2θ=27.71±0.50 (A4) 2θ=44.81±0.50 (A5) 2θ=45.31±0.50 (A6)

[0034] As shown in Fig. 1, after preparing an assembly of starting material A in the preparation step, the assembly of starting material A is heated to perform a production step of producing a solid electrolyte member (step S12). That is, before the production step, the electrolyte raw material and elemental sulfur contained in starting material A are not bonded to each other by chemical reaction, but in the production step, they are bonded to each other by chemical reaction and have a chemical formula of Li a M b P c S d A solid electrolyte member represented by the formula (1) is generated. Since elemental sulfur has a melting point lower than that of the electrolyte raw material, when the elemental sulfur is heated to the melting point of elemental sulfur or higher in the generation step, the elemental sulfur melts, and the molten liquid sulfur and the solid electrolyte raw material coexist. Here, the elemental sulfur is added at a mixing ratio such that the volume ratio of the added elemental sulfur to the entire mixture is 20% or more, so that the amount of liquid sulfur that can come into contact with the solid electrolyte raw material is large. Therefore, the liquid sulfur permeates the entire electrolyte raw material, which is a solid powder (in other words, the entire electrolyte raw material, which is a solid, is immersed in liquid sulfur), and all of the electrolyte raw material can come into contact with the liquid sulfur, so that the elemental diffusion and chemical reaction of the electrolyte raw material are promoted by the solid-liquid reaction, and the solid electrolyte member can be appropriately generated. In addition, in this manufacturing method, excess elemental sulfur exceeding the stoichiometric ratio is added, but the excess elemental sulfur after the solid electrolyte is produced evaporates when heated to a temperature close to the boiling point of sulfur (e.g., 400°C or higher) and is automatically removed from the solid electrolyte to the outside of the system. Therefore, there is no risk of elemental sulfur remaining and inhibiting the ionic conduction of the solid electrolyte, and a solid electrolyte member with sufficient ionic conductivity can be easily manufactured.

[0035] (Heating conditions in the generation step) Specifically, in the production step, the aggregate of the starting material A is heated to a temperature T1 and is maintained at the temperature T1 for a predetermined period of time to produce the solid electrolyte member. The temperature T1 is preferably 400°C or more and 1000°C or less, more preferably 450°C or more and 650°C or less, and even more preferably 500°C or more and 600°C or less. By setting the temperature T1 in this range, the assembly of the starting material A and the generated solid electrolyte member can be given the following appropriate thermal history. Before reaching the temperature T1, the assembly of the starting material A is given a thermal history of more than the melting point and less than the boiling point of elemental sulfur (for example, more than 120°C and less than 400°C), so that contact between the high-temperature liquid sulfur and the electrolyte raw material is induced, and the generation of the solid electrolyte member is promoted. In addition, the generated solid electrolyte member is given a thermal history of a temperature close to the boiling point of elemental sulfur (at least 400°C or more), so that the excess elemental sulfur is removed from the solid electrolyte by evaporation. As a result, a solid electrolyte member having sufficient ionic conductivity can be easily generated. The holding time at temperature T1 is preferably 30 minutes to 72 hours, more preferably 1 hour to 24 hours, and even more preferably 1 hour to 12 hours. By setting the holding time within this range, the raw materials are appropriately reacted, and even when temperature T1 is lower than 444.6° C., which is the boiling point of sulfur, excess elemental sulfur exceeding the stoichiometric ratio of the solid electrolyte member can be slowly evaporated and removed, and a solid electrolyte member having sufficient ionic conductivity can be appropriately produced. The heating rate to temperature T1 is preferably 0.5° C. / min to 20° C. / min, more preferably 3° C. / min to 15° C., and even more preferably 5° C. / min to 10° C. By setting the heating rate within this range, the electrolyte raw material can be quickly heated to temperature T1 while preventing the elemental sulfur from rapidly evaporating, and therefore, at temperature T1, the time for the high-temperature liquid sulfur to come into contact with the solid electrolyte raw material is sufficiently secured. This can promote the reaction for producing the solid electrolyte, and a solid electrolyte member having sufficient ionic conductivity can be easily produced.

[0036] FIG. 2 is a schematic diagram of an equipment for producing a solid electrolyte member. As shown in FIG. 2, a furnace 10 is a furnace for heating a starting material A to produce a solid electrolyte member. There is no particular restriction on the furnace material of the furnace 10, but from an economical point of view, it is preferable to use a material that does not corrode even when it comes into contact with vapor of elemental sulfur (for example, ceramics or a metal with a hot-dip aluminum plating treatment on the surface) as the furnace material. The furnace 10 is provided with a heating section 12. The heating section 12 is a heat source for heating the inside of the furnace 10. Note that the structure of FIG. 2 is an example, and the equipment for producing a solid electrolyte member is not limited to the structure of FIG. 2, and may be a tubular furnace as well as a muffle furnace or a retort furnace. Alternatively, an electric furnace in which the heat source is not covered with a furnace material may be used, and the solid electrolyte member may be produced by directly putting the aggregate of the starting material A into a rotary kiln without putting it in a firing vessel.

[0037] In the generation step, starting material A is placed in a calcination container in furnace 10 in a specified gas atmosphere, and is heated in heating section 12 while supplying a specified gas until it reaches temperature T1, and is maintained at temperature T1 for a specified retention time. There is no particular restriction on the material of the container for containing the aggregate of starting material A. However, from an economical standpoint, it is preferable to use a material whose surface is not corroded even when it comes into contact with vapor of elemental sulfur or molten liquid sulfur (for example, a ceramic sintering container (for example, a sagger, crucible, etc.) such as alumina, zirconia, carbon, silicon carbide, etc.). The container for containing the aggregate of starting material A may be either a container with a lid or without a lid, but a container with a lid that can gently suppress the evaporation of elemental sulfur is preferable. In addition, in order to evaporate and remove the excess elemental sulfur after the production of the solid electrolyte from the system, a container with an open lid that can release the gas inside the container is preferable. The gas supplied to the furnace 10 may be an inert gas (rare gas) such as argon, or may be hydrogen sulfide. For example, heating may be performed while flowing argon at 100 mL / min. The elemental sulfur in the starting material A melts before the temperature reaches T1, and a solid electrolyte member is produced by a solid-liquid reaction between the molten liquid sulfur and the other raw materials.

[0038] In this manner, in this manufacturing method, once the assembly of starting material A is stored in the furnace 10, a solid electrolyte member is produced without removing the starting material A from the furnace 10. In other words, in this manufacturing method, the sulfides (intermediate products) of Li, element M, and P produced from the starting material A are not taken out of the furnace 10, but are kept in the furnace 10 to produce a solid electrolyte member. That is, the sulfides (intermediate products) of Li, element M, and P produced from the starting material A react to become a solid electrolyte member while kept in the furnace 10 in a predetermined gas atmosphere and without being exposed to the air.

[0039] In the present embodiment, only one heating step at temperature T1 is performed in the generating step, but multiple heating steps may be performed. In this case, for example, before heating at temperature T1, a step of heating at temperature T2 for a predetermined time to melt elemental sulfur may be performed. By providing a step of heating at temperature T2, it is possible to perform firing at temperature T1 in a state in which the molten liquid sulfur has permeated the entire electrolyte raw material, and the solid electrolyte member can be appropriately generated. Here, temperature T2 is a temperature higher than the melting point of elemental sulfur and lower than temperature T1, for example, 120°C or higher and 400°C or lower.

[0040] Moreover, the solid electrolyte member produced by the above method preferably has a crystal structure belonging to the space group P42 / nmc, and when measured by X-ray diffraction using CuKα radiation, the diffraction peaks of the following formulas (B1) to (B6) are detected. Moreover, when the solid electrolyte member according to this embodiment is measured by X-ray diffraction using CuKα radiation, the peak of formula (B7) is not detected as a diffraction peak, or even if it is detected, the diffraction intensity of the peak of formula (B6) is less than I A The diffraction intensity of the peak of formula (B7) is I B In this case, I B / I A (I A I BThe peak intensity ratio of Li to Li2O3 is preferably less than 50%, more preferably 10% or less, and particularly preferably 1% or less. That is, the solid electrolyte member according to the present embodiment has a so-called LGPS type crystal structure. a M b P c S d (More preferably Li 10.35 Ge1.35P 1.65 S 12 The diffraction intensity refers to the peak height of the waveform measured by X-ray diffraction.

[0041] 2θ=17.38°±1.0° (B1) 2θ=20.18°±1.0° (B2) 2θ=20.44°±1.0° (B3) 2θ=23.96°±1.0° (B4) 2θ=26.96°±1.0° (B5) 2θ=29.58°±1.0° (B6) 2θ=27.33°±1.0° (B7)

[0042] (effect) As described above, the method for producing a solid electrolyte member according to the present embodiment is a method for producing a sulfide-based solid electrolyte member, and includes a preparation step and a production step. In the preparation step, an assembly of starting raw material A is prepared using an electrolyte raw material containing at least elements other than sulfur among the elements constituting the solid electrolyte member, and elemental sulfur. In the production step, the assembly of starting raw material A is heated to produce the solid electrolyte member. In the preparation step, the assembly of starting raw material A has a volume ratio (addition volume ratio) of elemental sulfur to the entire assembly of starting raw material A of 20% or more in an environment of 120°C at which elemental sulfur melts.

[0043] Usually, when manufacturing a solid electrolyte member, raw materials are mixed by mechanical milling in order to obtain sufficient ionic conductivity. This mixes the contained elements at the atomic level, and the chemical composition of the entire raw material mixture is made uniform, which facilitates the reaction of generating a solid electrolyte during the subsequent heat treatment. However, in order to properly perform mechanical milling, a large amount of energy and time are required, and it is difficult to enlarge it to an industrial scale. In contrast, in the manufacturing method according to the present embodiment, elemental sulfur is added so that the added volume ratio at 120°C is 20% or more. In this way, by adding excess elemental sulfur exceeding the stoichiometric ratio and increasing the volume ratio of elemental sulfur, the molten liquid sulfur permeates the entire solid electrolyte raw material, and it becomes possible to contact all of the electrolyte raw material with the liquid sulfur. As a result, the element diffusion and chemical reaction of the electrolyte raw material are promoted by the solid-liquid reaction, which promotes the generation and crystal growth of the solid electrolyte member, and reduces sulfur deficiency and by-products (heterogeneous phases or impurity phases) generated during the synthesis of a sulfide solid electrolyte, making it possible to manufacture a solid electrolyte member having sufficient ionic conductivity. Since this method utilizes a solid-liquid reaction that is more reactive than a solid-phase reaction between solid electrolyte raw materials or a gas-solid reaction between hydrogen sulfide gas and an electrolyte raw material, this method is particularly effective when using raw materials that are not highly reactive with sulfur (e.g., elemental Si, elemental Ge, etc.). In addition, since mechanical milling is not required, it becomes possible to easily manufacture solid electrolyte members with sufficient ionic conductivity by a process suitable for mass production.

[0044] In addition, the volume ratio of elemental sulfur added to the aggregate of starting material A is preferably 40% or more. By setting the volume ratio of added elemental sulfur within this range, the solid-liquid reaction between the molten liquid sulfur and the solid electrolyte raw material is further promoted, making it possible to easily produce a solid electrolyte member with sufficient ionic conductivity.

[0045] In the generating step, the starting material A is preferably heated at a heating temperature of 400° C. or more and 1000° C. or less. By heating the starting material A within this temperature range, the solid electrolyte member can be appropriately produced.

[0046] In the preparation step, it is preferable to prepare an assembly of starting raw material A by mixing the raw material for electrolyte and elemental sulfur so that a diffraction peak due to a crystalline substance contained in the raw material for electrolyte and elemental sulfur constituting starting raw material A can be detected when the prepared assembly of starting raw material A is measured by an X-ray diffraction method. According to this production method, since the solid electrolyte member is produced by a solid-liquid reaction, the solid electrolyte member can be appropriately produced even if the raw materials are mixed to the extent that crystalline substance remains in the raw materials. Therefore, according to this production method, it is possible to simplify the mixing process and produce many solid electrolyte members in a short time.

[0047] In addition, in this embodiment, it is preferable to manufacture a solid electrolyte member having an LGPS type crystal structure. Since the LGPS type has high ionic conductivity, it can be suitably used in lithium ion secondary batteries and the like. In addition, when manufacturing a LGPS type solid electrolyte member, by setting the addition volume ratio within the above range, it is possible to promote the generation and crystal growth of the solid electrolyte member, and to suppress the generation of sulfur deficiency and by-products (heterogeneous phases or impurity phases), thereby suppressing the decrease in the ionic conductivity of the solid electrolyte member.

[0048] (Other examples) In the above explanation, the chemical formula is Li a M b P c S d However, the composition of the solid electrolyte member to be manufactured is not limited to this. Other embodiments of the solid electrolyte member will be described below.

[0049] Second embodiment As described in the second embodiment, the solid electrolyte member has the chemical formula Li a M b P c S d Ha e Here, a, b, c, d, and e are numbers greater than 0. The element Ha is a halogen element, and more preferably at least one element selected from the group consisting of F, Cl, Br, and I.

[0050] When the solid electrolyte member of the second embodiment is measured by an X-ray diffraction method using CuKα radiation, it is preferable that a peak be detected at the position of the following formula (B6).

[0051] 2θ=29.58°±1.0° (B6)

[0052] Furthermore, when the solid electrolyte member of the second embodiment is measured by an X-ray diffraction method using CuKα radiation, a peak may or may not be detected at the position of the following formula (B7). That is, in the second embodiment, a solid electrolyte member in which a peak is detected at the position of formula (B7) may be manufactured, or a solid electrolyte member in which a peak is not detected at the position of formula (B7) may be manufactured.

[0053] 2θ=27.33°±1.0° (B7)

[0054] Here, the diffraction intensity of the peak at the position of formula (B6) in the X-ray diffraction measurement using CuKα radiation of the solid electrolyte member of the second embodiment is I A The diffraction intensity at the position of formula (B7) in the X-ray diffraction measurement using CuKα radiation is I B When I B / I A (I A I B The peak intensity ratio of the first peak to the second peak is preferably less than 50%, more preferably 10% or less, and particularly preferably 1% or less.

[0055] Third embodiment As described in the third embodiment, the solid electrolyte member has the chemical formula Li a M b P c X d S e Ha f Here, a, b, c, d, e, and f are numbers greater than 0. The element Ha is a halogen element, and more preferably at least one of F, Cl, Br, and I. The element X is a Group 16 element other than S, and more preferably at least one element selected from the group consisting of O, Se and Te.

[0056] In the solid electrolyte member of the third embodiment, a peak is preferably detected at the position of formula (B6) in the same manner as in the solid electrolyte member of the second embodiment. In addition, in the solid electrolyte member produced in the third embodiment, a peak may or may not be detected at the position of formula (B7) in the same manner as in the solid electrolyte member of the second embodiment. In the solid electrolyte member of the third embodiment, a peak is preferably detected at the position of formula (B6) in the same manner as in the solid electrolyte member of the second embodiment. B / I A (I A I B The peak intensity ratio of the first peak to the second peak is preferably less than 50%, more preferably 10% or less, and particularly preferably 1% or less.

[0057] In the third embodiment, the element Ha and the element X are introduced into the solid electrolyte member of the present embodiment, but the element X may be introduced without the element Ha being introduced. a M b P c X d S e In this case, a, b, c, d, and e are numbers greater than 0.

[0058] (Fourth embodiment) The solid electrolyte member of the fourth embodiment has an Argyrodite-type crystal structure. a P b S c Ha d Here, a, b, c, and d are numbers greater than 0. The Argyrodite-type crystal structure is, for example, a crystal structure possessed by a group of compounds derived from a mineral represented by the chemical formula Ag8GeS6. The element Ha is a halogen element, and more preferably at least one of F, Cl, Br, and I.

[0059] Fifth embodiment The solid electrolyte member of the fifth embodiment has an Argyrodite-type crystal structure. a P b X c S d Ha e Here, a, b, c, d, and e are numbers greater than 0. The element Ha is a halogen element, and more preferably at least one of F, Cl, Br, and I. The element X is a Group 16 element other than S, and more preferably at least one element selected from the group consisting of O, Se and Te.

[0060] Sixth embodiment The solid electrolyte member of the sixth embodiment has the chemical formula Li a M b S c where a, b, and c are numbers greater than 0. Here, the element M is preferably at least one element of groups 13, 14, and 15, and more preferably at least one of Si, Ge, As, Sn, and Sb. A part of the element M may be substituted with P or W. When the solid electrolyte member of the sixth embodiment is measured by an X-ray diffraction method using CuKα radiation, it is preferable that peaks are detected at positions of the following formulas (C1) to (C4).

[0061] 2θ=17.01±0.50 (C1) 2θ=18.50±0.50 (C2) 2θ=25.31±0.50 (C3) 2θ=26.23±0.50 (C4)

[0062] In the sixth embodiment, P is excluded from the solid electrolyte member of the present embodiment, but the element X may be introduced therein. That is, the solid electrolyte member may be Li a M b X c S dIt may also be represented by the following. In this case, a, b, c, and d are numbers greater than 0, the element X is an element of Group 16 other than S, and more preferably, at least one element of O, Se, and Te.

Examples

[0063] Hereinafter, the present invention will be described in detail while showing Examples and Comparative Examples. In both the Examples and Comparative Examples, the solid electrolyte member was synthesized by changing the type of starting material A in each example. The synthesized solid electrolyte member was taken out in a glove box under an argon atmosphere, pulverized in an agate mortar, and then the crystal structure was confirmed by X-ray diffraction measurement (XRD measurement) using CuKα rays. Thereafter, the ionic conductivity was measured as the performance of the solid electrolyte member. The results are shown in Table 1.

[0064] <XRD Measurement> For the XRD measurement, θ-2θ measurement was performed using an XRD apparatus “D8 ADVANCE” manufactured by Bruker in the range of 10° ≤ 2θ ≤ 55° under the conditions of a step width of 0.01° and an integration time of 1.2 seconds / step. The measurement sample was prepared in a glove box under an argon atmosphere, and the solid electrolyte member pulverized in an agate mortar was sealed in a sealable measurement cell, and powder X-ray diffraction measurement was performed while maintaining a state of not being exposed to the atmosphere.

[0065] <Example 1> In Example 1, lithium sulfide (Li2S) was used as the Li raw material, germanium sulfide (GeS2) was used as the M raw material, and diphosphorus pentasulfide (P2S5) was used as the P raw material. In a glove box with an argon atmosphere, a dew point of -70°C or less, and an oxygen concentration of 10 ppm or less, lithium sulfide, germanium sulfide, and diphosphorus pentasulfide, which are raw materials for the electrolyte, were weighed out to obtain a desired composition, and elemental sulfur was weighed out so that the volume ratio of the added material at 120°C was 20%, and each raw material for the electrolyte and elemental sulfur were mixed in an agate mortar for 5 minutes until the color was uniform, to generate an aggregate of starting raw materials. Here, 3.93 g of lithium sulfide, 3.05 g of germanium sulfide, 3.03 g of diphosphorus pentasulfide, and 2.18 g of elemental sulfur were mixed. The assembly of the starting materials was then placed in a furnace, and the inside of the furnace was heated to 550°C at 5°C / min in an argon atmosphere, and held at 550°C for 6 hours. Thereafter, the furnace was cooled to room temperature at 2°C / min to obtain a solid electrolyte member. The solid electrolyte member of Example 1 showed diffraction peaks of formulas (B1) to (B6) in an XRD measurement using CuKα radiation, and was therefore confirmed to have an LGPS-type crystal structure, and I B / I A (I A I B The peak intensity ratio of the two peaks was 0.50%.

[0066] <Example 2> In Example 2, the volume ratio of elemental sulfur added was changed to 30%, and 3.74 g of elemental sulfur was mixed as the starting material. A solid electrolyte member was obtained in the same manner as in Example 1. The solid electrolyte member of Example 2 showed diffraction peaks of formulas (B1) to (B6) in XRD measurement using CuKα radiation, and was therefore confirmed to have an LGPS-type crystal structure. B / I A (I A I B The peak intensity ratio of the two peaks was 0.41%.

[0067] <Comparative Examples 1 to 3> In Comparative Example 1, the volume ratio of elemental sulfur added was changed to 0%, i.e., elemental sulfur was not added. Except for this, a solid electrolyte member was obtained in the same manner as in Example 1. In Comparative Examples 2 and 3, the volume ratio of elemental sulfur added was changed to 6% and 10%, respectively. The solid electrolyte members of Comparative Examples 1 to 3 showed diffraction peaks of formulas (B1) to (B6) in XRD measurement using CuKα radiation, and therefore were all confirmed to have an LGPS-type crystal structure. B / I A (I A I B The peak intensity ratios of the peaks (peak intensity ratios of the peaks) were 4.7% in Comparative Example 1, 1.9% in Comparative Example 2, and 1.1% in Comparative Example 3, respectively.

[0068] <Examples 3 to 5> In Examples 3, 4, and 5, the types and amounts of the electrolyte raw materials were changed as shown in Table 1, and the volume ratios of elemental sulfur added were 20%, 40%, and 55%, respectively. Except for this, solid electrolyte members were obtained in the same manner as in Example 1. The solid electrolyte members of Examples 3 to 5 showed diffraction peaks of formulas (B1) to (B6) in XRD measurement using CuKα radiation, and therefore were confirmed to all have an LGPS-type crystal structure. B / I A (I A I B The peak intensity ratios of the peaks (peak intensity ratios of the peaks) were 39% in Example 3, 0.37% in Example 4, and 0.11% in Example 5, respectively.

[0069] <Comparative Example 4> In Comparative Example 4, a solid electrolyte member was obtained in the same manner as in Example 3, except that the volume ratio of elemental sulfur added was 10%. The solid electrolyte member of Comparative Example 4 showed diffraction peaks of formulas (B1) to (B6) in XRD measurement using CuKα radiation, and was therefore confirmed to have an LGPS-type crystal structure. B / I A (I A I B The peak intensity ratio of the two peaks was 150%.

[0070] <Example 6> In Example 6, a solid electrolyte member was obtained in the same manner as in Example 1, except that the types and amounts of the electrolyte raw materials were changed as shown in Table 1. The solid electrolyte member of Example 6 showed diffraction peaks of formulas (B1) to (B6) in an XRD measurement using CuKα radiation, and was therefore confirmed to have an LGPS-type crystal structure. B / I A (I A I B The peak intensity ratio of the two peaks was 0.45%.

[0071] <Comparative Example 5> In Comparative Example 5, a solid electrolyte member was obtained in the same manner as in Example 6, except that the volume ratio of elemental sulfur added was 10%. The solid electrolyte member of Comparative Example 5 showed diffraction peaks of formulas (B1) to (B6) in XRD measurement using CuKα radiation, and was therefore confirmed to have an LGPS-type crystal structure. B / I A (I A I B The peak intensity ratio of the two peaks was 1.6%.

[0072] <Example 7> In Example 7, a solid electrolyte member was obtained in the same manner as in Example 1, except that the types and amounts of the electrolyte raw materials were changed as shown in Table 1. The solid electrolyte member of Example 7 was confirmed to have an Argyrodite-type crystal structure by XRD measurement using CuKα radiation.

[0073] <Comparative Examples 6 and 7> In Comparative Examples 6 and 7, solid electrolyte members were obtained in the same manner as in Example 7, except that the volume ratios of elemental sulfur added were 6% and 10%, respectively. The solid electrolyte members of Comparative Examples 6 and 7 were confirmed to have an Argyrodite-type crystal structure by XRD measurement using CuKα radiation.

[0074] <Examples 8 and 9> In Examples 8 and 9, the types and amounts of the electrolyte raw materials were changed as shown in Table 1, and the volume ratios of elemental sulfur added were set to 20% and 40%, respectively, and other than that, solid electrolyte members were obtained in the same manner as in Example 1. The solid electrolyte members of Examples 8 and 9 were confirmed to have an Argyrodite-type crystal structure by XRD measurement using CuKα radiation.

[0075] <Comparative Example 8> In Comparative Example 8, a solid electrolyte member was obtained in the same manner as in Example 8, except that the volume ratio of elemental sulfur added was 10%. It was confirmed that the solid electrolyte member of Comparative Example 8 had an Argyrodite-type crystal structure by XRD measurement using CuKα radiation.

[0076] <Example 10> In Example 10, a solid electrolyte member was obtained in the same manner as in Example 1, except that the types and amounts of the electrolyte raw materials were changed as shown in Table 1. It was confirmed that the solid electrolyte member of Example 10 had a crystal structure in which diffraction peaks were detected at the positions of formulas (C1) to (C4) by XRD measurement using CuKα radiation.

[0077] <Comparative Example 9> In Comparative Example 9, a solid electrolyte member was obtained in the same manner as in Example 10, except that the volume ratio of elemental sulfur added was 10%. It was confirmed that the solid electrolyte member of Comparative Example 9 had a crystal structure in which diffraction peaks were detected at the positions of formulas (C1) to (C4) by XRD measurement using CuKα radiation.

[0078] <Ionic conductivity measurement> Each of the solid electrolyte members obtained as described above was taken out of a glove box in an argon atmosphere, crushed in an agate mortar, and 0.3 g was weighed out and filled into a stainless steel ion conductivity measurement cell (cylindrical type with an inner diameter of 17 mm). Then, the ion conductivity (mS / cm) was measured by an AC impedance method using a Biologic Corporation measurement device "Potentio / Galvanostat SP-300" under the conditions of a measurement temperature of 25°C, a measurement frequency of 1Hz to 1MHz, and an applied pressure of 360MPa to the measurement cell. The measurement results are shown in Table 1.

[0079] [Table 1]

[0080] In Table 1, when the ionic conductivity of the same type of solid electrolyte material is compared, such as in Comparative Examples 1-3 for Examples 1-2, Comparative Example 4 for Examples 3-5, Comparative Example 5 for Example 6, Comparative Examples 6-7 for Example 7, Comparative Example 8 for Examples 8-9, and Comparative Example 9 for Example 10, the ionic conductivity of the Examples is higher than that of the Comparative Examples in all cases. Furthermore, in many cases, the ionic conductivity of the Examples is more than twice that of the Comparative Examples, and the difference in ionic conductivity between the Examples and the Comparative Examples is large for the exceptions of Example 1 and Comparative Example 3 (the ionic conductivity of Example 1 is about 1.98 times that of Comparative Example 3) and Example 7 and Comparative Example 7 (the ionic conductivity of Example 7 is about 1.88 times that of Comparative Example 7). This shows that the present manufacturing method in which elemental sulfur is excessively added at a volume ratio of 20% or more as in Examples 1-10 is effective in improving the ionic conductivity of the sulfide-based solid electrolyte, compared to, for example, the manufacturing method in which the volume ratio of elemental sulfur is lower than 20% as in Comparative Examples 1-9. In particular, the ionic conductivity of Examples 1 to 2, 4 to 7, and 9 was 8 mS / cm or more, making it clear that a solid electrolyte having sufficient ionic conductivity could be produced. Furthermore, when comparing Example 3 with Examples 4 and 5, or Example 8 with Example 9, it can be seen that by adding 40% or more by volume of elemental sulfur, the ionic conductivity of the sulfide-based solid electrolyte can be improved more than when 20% by volume of elemental sulfur is added. As described above, as exemplified in Examples 1 to 10, by adding an excess of elemental sulfur of 20% or more by volume ratio, mechanical milling becomes unnecessary, and it becomes possible to easily manufacture a solid electrolyte having sufficient ionic conductivity. In this manufacturing method, an excess of elemental sulfur exceeding the stoichiometric ratio is added, but the elemental sulfur that is surplus after the solid electrolyte is generated evaporates at the stage of heating to a temperature close to the boiling point of sulfur (for example, 400°C or higher) and is automatically removed from the solid electrolyte to the outside of the system. Therefore, the added elemental sulfur does not remain after the heat treatment, and there is no risk of inhibiting the ionic conduction of the solid electrolyte. Since the ionic conductivity is improved by about two times by such a simple and convenient method of adding elemental sulfur, and a solid electrolyte having a sufficient ionic conductivity of 8 mS / cm or more can be easily obtained, this manufacturing method has a great manufacturing advantage compared to the existing manufacturing method using mechanical milling.

[0081] Although the embodiment of the present invention has been described above, the embodiment is not limited to the contents of this embodiment. The above-mentioned components include those that a person skilled in the art can easily imagine, those that are substantially the same, and those that are within the so-called equivalent range. Furthermore, the above-mentioned components can be appropriately combined. Furthermore, various omissions, substitutions, or modifications of the components can be made without departing from the gist of the above-mentioned embodiment. [Explanation of symbols]

[0082] A. Starting material

Claims

1. A method for producing a sulfide-based solid electrolyte member, comprising the steps of: a preparation step of mixing an electrolyte raw material including at least an element other than sulfur among elements constituting the solid electrolyte member with elemental sulfur to prepare a starting raw material, and preparing an assembly of the starting raw material; heating the collection of starting materials in an inert gas atmosphere to produce the solid electrolyte member; Including, In the preparation step, when the assembly of the starting materials is heated to 120° C., the volume ratio of the elemental sulfur to the entire assembly of the starting materials is 40% or more. A method for producing a solid electrolyte member.

2. The method for producing a solid electrolyte member according to claim 1 , wherein in the generating step, the assembly of the starting materials is heated at a heating temperature of 400° C. or more and 1000° C. or less.

3. In the preparation step, When the aggregate of the starting materials prepared was measured by an X-ray diffraction method, 3. The method for producing a solid electrolyte member according to claim 1, wherein the elemental sulfur and the raw material for the electrolyte are mixed together to prepare an assembly of the starting raw materials so that a diffraction peak due to a crystalline substance contained in the elemental sulfur and the raw material for the electrolyte can be detected.

4. A method for producing a sulfide-based solid electrolyte member, comprising the steps of: a preparation step of preparing an assembly of starting materials using an electrolyte raw material including at least an element other than sulfur among elements constituting the solid electrolyte member and elemental sulfur as starting materials; heating the collection of starting materials to produce the solid electrolyte member; Including, In the preparation step, when the assembly of starting materials is heated to 120° C., a volume ratio of the elemental sulfur to the entire assembly of the starting materials is 20% or more; The solid electrolyte member is a member having a space group P4 2 / nmc-affiliated LGPS (Li 10 GeP 2 S 12 ) type crystal structure, and when measured by X-ray diffraction using CuKα radiation, As diffraction peaks, peaks of the following formulas (B1) to (B6) were detected, As for the peak of formula (B7), the peak is not detected, or the diffraction intensity of the peak of formula (B6) is I A The diffraction intensity of the peak of formula (B7) is I B In this case, I A I against B The diffraction intensity I B The method for producing a solid electrolyte member, comprising the steps of: producing a solid electrolyte member in which a peak represented by formula (B7) is detected. 2θ=17.38°±1.0°...(B1) 2θ=20.18°±1.0°...(B2) 2θ=20.44°±1.0°...(B3) 2θ=23.96°±1.0°...(B4) 2θ=26.96°±1.0°...(B5) 2θ=29.58°±1.0°...(B6) 2θ=27.33°±1.0°...(B7)

5. The method for producing a solid electrolyte member according to claim 1 , wherein the solid electrolyte member produced has an Argyrodite-type crystal structure.

6. A method for producing a sulfide-based solid electrolyte member, comprising the steps of: a preparation step of preparing an assembly of starting materials using an electrolyte raw material including at least an element other than sulfur among elements constituting the solid electrolyte member and elemental sulfur as starting materials; heating the collection of starting materials to produce the solid electrolyte member; Including, In the preparation step, when the assembly of starting materials is heated to 120° C., a volume ratio of the elemental sulfur to the entire assembly of the starting materials is 20% or more; The solid electrolyte member is Li a M b S c and a crystal structure of space group Pnma, and when measured by an X-ray diffraction method using CuKα radiation, peaks of the following formulas (C1) to (C4) are detected as diffraction peaks. 2θ=17.01±0.50...(C1) 2θ=18.50±0.50...(C2) 2θ=25.31±0.50...(C3) 2θ=26.23±0.50...(C4) Here, M is at least one element of Group 13, Group 14, and Group 15, and a, b, and c are numbers greater than 0.

Citation Information

Patent Citations

  • Piezoelectric ceramics

    JP1980027673A

  • Method and device for size measurement

    JP1983088609A

  • Manufacturing method of lithium ion conductive sulfide glass and glass ceramics as well as all solid-type battery using same glass ceramics

    JP2003208919A

  • Sulfide solid electrolyte, electrode mixture material, and lithium ion battery

    JP2017199631A

  • Manufacturing method of crystalline sulfide-based solid electrolyte

    JP2020027715A