Dispersions and moldings
A dispersion of thermoplastic tetrafluoroethylene polymer with metal and silicon oxide fillers addresses the limitations of existing technologies by achieving high thermal conductivity, electrical properties, and scratch resistance in formed layers.
Patent Information
- Application Number
- JP2021520784
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-25
- Filing Date
- 2020-05-18
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-05-18
AI Technical Summary
Existing dispersions containing tetrafluoroethylene polymers and metal oxide fillers face challenges in forming layers with excellent thermal conductivity, adhesiveness, and scratch resistance due to restricted filler content or reduced dispersibility, affecting the physical properties of the formed layer.
A dispersion comprising a thermoplastic tetrafluoroethylene polymer with specific properties, combined with metal and silicon oxide fillers, in a polar liquid medium, ensures high dispersibility and uniform distribution of fillers, enhancing thermal conductivity, electrical properties, and scratch resistance.
The dispersion forms layers with improved thermal conductivity, electrical properties, and scratch resistance, resulting in molded products with enhanced adhesiveness and uniform filler distribution.
Smart Images

Figure 0007571723000001 
Figure 0007571723000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a dispersion containing a tetrafluoroethylene-based polymer, a metal oxide filler, and a silicon oxide filler, and a molded article thereof. [Background technology]
[0002] Tetrafluoroethylene polymers such as polytetrafluoroethylene (PTFE) have excellent physical properties such as chemical resistance, water and oil repellency, heat resistance, and electrical properties, and dispersions containing powders of these polymers are useful as materials for coating substrate surfaces with a layer of tetrafluoroethylene polymer.
[0003] Such a dispersion liquid must have excellent physical properties of the liquid itself and the layer formed therefrom. Furthermore, in recent years, in applications for coating the surface of metal substrates and the like, there has been a demand for further improvement in the latter physical properties, such as adhesion, thermal conductivity (heat dissipation), scratch resistance, and electrical properties of the layer. As a dispersion liquid suitable for such applications, a dispersion liquid containing a tetrafluoroethylene-based polymer powder and a metal oxide filler has been proposed (see Patent Documents 1 to 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent Publication No. 2017-110220 [Patent Document 2] Patent Publication No. 2018-059032 [Patent Document 3] International Publication No. 2018 / 110644 Summary of the Invention [Problem to be solved by the invention]
[0005] However, it is difficult to prepare a dispersion liquid containing a tetrafluoroethylene polymer powder that can easily form a layer having excellent physical properties while retaining the physical properties of the liquid itself. In the dispersions of Patent Documents 1 and 2, the content of the metal oxide filler is restricted or its dispersibility is reduced depending on the state of the dispersion medium and the particle size of the metal oxide filler (see, for example, Table 1 in paragraph number
[0050] and Table 5 in paragraph number
[0054] in Patent Document 1). As a result, there is a problem that the form of the dispersion is limited, and it is difficult to form a layer having excellent thermal conductivity, adhesiveness and adhesion, particularly a layer having excellent thermal conductivity (heat dissipation). The dispersion of Patent Document 3 contains a large amount of a polymer other than a tetrafluoroethylene-based polymer (such as a water-soluble acrylic polymer containing a sulfonic acid group) as an adhesive component, and therefore has the problem that the physical properties (durability, weather resistance, etc.) of the tetrafluoroethylene-based polymer are difficult to fully exhibit in the layer formed. As a result of extensive investigations, the present inventors have found that by combining a specific tetrafluoroethylene-based polymer with a specific filler, a dispersion can be obtained that can easily form a layer that highly exhibits the physical properties of both the fillers and the physical properties of the tetrafluoroethylene-based polymer. [Means for solving the problem]
[0006] The present invention has the following aspects. [1] A dispersion comprising a powder of a thermoplastic tetrafluoroethylene-based polymer having a melting temperature of 200 to 320°C, a metal oxide filler containing more than 50% by mass of a metal oxide, a silicon oxide filler containing more than 50% by mass of silicon oxide, and a polar liquid dispersion medium, wherein the content of the metal oxide filler is 5% by mass or more. [2] The dispersion of [1], wherein the tetrafluoroethylene-based polymer is at least one polymer selected from the group consisting of polymers containing units based on tetrafluoroethylene and units based on a monomer having an oxygen-containing polar group, polymers containing 2 mol % or more of units based on tetrafluoroethylene and units based on perfluoro(propyl vinyl ether), and polymers containing units based on tetrafluoroethylene and units based on perfluoro(methyl vinyl ether). [3] The dispersion liquid according to [1] or [2], wherein the metal oxide is at least one metal oxide selected from the group consisting of aluminum oxide, lead oxide, iron oxide, tin oxide, magnesium oxide, titanium oxide, zinc oxide, antimony pentoxide, zirconium oxide, lanthanum oxide, neodymium oxide, cerium oxide, and niobium oxide. [4] The dispersion according to any one of [1] to [3], wherein the metal oxide filler further contains silicon oxide. [5] The dispersion liquid according to any one of [1] to [4], wherein the metal oxide filler is a particulate filler having an average particle size equal to or greater than the average particle size of the powder, or is fibrous and has an average fiber length equal to or greater than the average particle size of the powder. [6] The dispersion liquid according to any one of [1] to [5], wherein the silicon oxide filler has a spherical or scaly shape. [7] The dispersion liquid according to any one of [1] to [6], wherein the silicon oxide filler has a hollow structure. [8] The dispersion liquid according to any one of [1] to [7], wherein the mass ratio of the content of the silicon oxide filler to the content of the metal oxide filler is less than 1. [9] Any of the dispersions [1] to [8], having a viscosity of 10,000 mPa s or less at 25°C.
[10] A dispersion of any of [1] to [9], having a thixotropic ratio at 25°C of 1.0 to 2.5.
[11] A method for producing a laminate, comprising applying a dispersion liquid according to any one of [1] to
[10] to a base layer, heating the base layer to volatilize the liquid dispersion medium, and further heating the base layer to bake the tetrafluoroethylene-based polymer, thereby obtaining a laminate having the base layer and a polymer layer containing the tetrafluoroethylene-based polymer, the metal oxide filler, and the silicon oxide filler.
[12] A molded article comprising a thermoplastic tetrafluoroethylene polymer having a melting temperature of 200 to 320°C, a metal oxide filler containing more than 50% by mass of a metal oxide, and a silicon oxide filler containing more than 50% by mass of silicon oxide, wherein the content of the tetrafluoroethylene polymer is 50% by mass or more and the sum of the content of the metal oxide filler and the content of the silicon oxide filler is 10% by mass or more.
[13] The molding of
[12] , having a thickness of 1 to 1000 μm.
[14] A molded article of
[12] or
[13] having a thermal conductivity of 1 W / mK or more.
[15] Any of the moldings
[12] to
[14] , having a dielectric tangent of 0.005 or less. Effect of the Invention
[0007] According to the present invention, there is obtained a dispersion liquid which has good physical properties (dispersibility, coatability) of the liquid itself and which can easily form a polymer layer which is excellent in thermal conductivity, scratch resistance, electrical properties, etc., as well as a laminate and a molded product having such a polymer layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The following terms have the following meanings. The "melt viscosity of polymer" is a value measured in accordance with ASTM D1238 using a flow tester and a 2Φ-8L die, with a polymer sample (2 g) that had been heated at the measurement temperature in advance for 5 minutes being held at the measurement temperature under a load of 0.7 MPa. The "melting temperature (melting point) of a polymer" is the temperature corresponding to the maximum value of the melting peak of the polymer as measured by differential scanning calorimetry (DSC). "Average particle size of powder (D50)" is the cumulative 50% diameter on a volume basis of powder determined by laser diffraction / scattering method. In other words, the particle size distribution of powder is measured by laser diffraction / scattering method, and a cumulative curve is calculated with the total volume of the group of powder particles as 100%, and the particle size is the point on the cumulative curve where the cumulative volume is 50%. "D90 of powder" is the volume-based cumulative 90% diameter of the powder measured in a similar manner. The D50 and D90 of a powder are determined by dispersing the powder in water and analyzing it by the laser diffraction / scattering method using a laser diffraction / scattering type particle size distribution measuring device (LA-920 measuring device, manufactured by Horiba, Ltd.). The "viscosity of the dispersion liquid" is a value measured using a Brookfield viscometer at room temperature (25°C) and a rotation speed of 30 rpm. The measurement is repeated three times, and the average value of the three measured values is used. The "thixotropy ratio of the dispersion" is a value calculated by dividing the viscosity η1 measured at a rotation speed of 30 rpm by the viscosity η2 measured at a rotation speed of 60 rpm. Each viscosity measurement is repeated three times, and the average value of the three measured values is used. "Ten-point average roughness (Rzjis)" is a value specified in Appendix JA of JIS B 0601:2013. "Peel strength" is the maximum load (N / cm) applied when a laminate cut into a rectangle (length 100 mm, width 10 mm) is fixed at a position 50 mm from one end in the longitudinal direction, and the polymer layer is peeled off from the substrate (aluminum foil) at an angle of 90° to the laminate at a pulling speed of 50 mm / min. "Thermal conductivity of the molded product" is a value measured in accordance with ASTM D5470. The "unit" in a polymer may be an atomic group formed directly from a monomer by a polymerization reaction, or may be an atomic group in which a part of the structure is converted by treating a polymer obtained by a polymerization reaction with a predetermined method. A unit based on monomer A contained in a polymer is also simply referred to as a "monomer A unit". "(Meth)acrylate" is a general term for acrylate and methacrylate.
[0009] The dispersion of the present invention contains a powder (hereinafter also referred to as "F powder") of a tetrafluoroethylene-based polymer (hereinafter also referred to as "F polymer") having a melting temperature of 200 to 300°C and thermoplasticity, a metal oxide filler (hereinafter also referred to as "MO filler") containing more than 50 mass% of a metal oxide, a silicon oxide filler (hereinafter also referred to as "SO filler") containing more than 50 mass% of silicon oxide, and a polar liquid dispersion medium. The content of the MO filler contained in the dispersion of the present invention is 5 mass% or more. The dispersion of the present invention is a dispersion in which the F powder, the MO filler, and the SO filler are each dispersed.
[0010] The dispersion of the present invention has excellent dispersibility, and can easily form a dense F polymer molded product (including coatings, films, and other aspects such as a polymer layer formed on the surface of a substrate; the same applies below) in which the MO filler and SO filler are highly dispersed. The reason for this is not necessarily clear, but it is believed that the F polymer has predetermined physical properties, which results in excellent dispersibility of the F powder, and the F powder flows highly during layer formation, promoting homogeneous distribution of the filler in the layer. In addition, it is believed that the silicon oxide contained in the SO filler not only improves the layer properties (reduced linear expansion, improved electrical properties, etc.), but also improves the homogeneous distribution and orientation of the MO filler. As a result, it is presumed that even in the molded product, the MO filler and the SO filler are uniformly and firmly held in the matrix formed from the F polymer, and the respective physical properties are imparted to the molded product satisfactorily. The above-mentioned effects are more pronounced in the preferred embodiments of the present invention described below.
[0011] The D50 of the F powder in the present invention is preferably 40 μm or less, more preferably 20 μm or less, and particularly preferably 8 μm or less. The D50 of the F powder is preferably 0.01 μm or more, more preferably 0.1 μm or more, and particularly preferably 1 μm or more. The D90 of the F powder is preferably 80 μm or less, and more preferably 50 μm or less. In this range of D50 and D90, the flowability and dispersibility of the F powder are good, and the molded product is most likely to exhibit excellent electrical properties (low dielectric constant, low transmission loss, etc.), heat resistance, and scratch resistance. The loose packing bulk density of the F powder is more preferably 0.08 to 0.5 g / mL. The dense packing bulk density of the F powder is more preferably 0.1 to 0.8 g / mL. When the loose packing bulk density or dense packing bulk density is within the above range, the handleability of the F powder is excellent.
[0012] The F powder in the present invention may contain a resin other than the F polymer, but preferably contains the F polymer as the main component. The content of the F polymer in the powder is preferably 80% by mass or more, more preferably 100% by mass. Examples of the resin include heat-resistant polymers such as aromatic polyesters, polyamideimides, thermoplastic polyimides, polyphenylene ethers, and polyphenylene oxides.
[0013] The F polymer in the present invention is a thermoplastic polymer containing units based on tetrafluoroethylene (TFE) (hereinafter also referred to as "TFE units"). The melting temperature of the F polymer is 200 to 320° C., and preferably 260 to 320° C. In this case, the filler is easily dispersed to a high degree in the formation of the molded product, and the adhesiveness and surface flatness of the molded product are easily improved. The melt viscosity of F polymer at 380℃ is 1×10 2 ~1×10 6 Pa s is preferred, 1×10 3 ~1×10 6 Pa·s is more preferred.
[0014] A suitable embodiment of the F polymer is a polymer containing a unit based on a monomer having a TFE unit and an oxygen-containing polar group (hereinafter also referred to as "F polymer 1"). Since the F polymer 1 has high dispersibility in a polar liquid dispersion medium and high affinity with each of the MO filler and the SO filler, it highly interacts with the F polymer 1 and the liquid dispersion medium, and the sedimentation of the F powder and both fillers in the dispersion liquid is easily effectively suppressed. In addition, it is easy to include a fine spherulite structure on its surface. As a result, even in a molded article formed from such a dispersion liquid, both fillers are uniformly and firmly held in the matrix formed from the F polymer 1, and the physical properties based on the metal oxide and silicon oxide are easily imparted to the molded article.
[0015] The oxygen-containing polar group of the F polymer 1 may be contained in the polymer main chain terminal portion. It may also be contained in the polymer by surface treatment (radiation treatment, electron beam treatment, corona treatment, plasma treatment, etc.). The oxygen-containing polar group of the F polymer 1 may also be a group prepared by modifying a polymer having a group capable of forming an oxygen-containing polar group. The oxygen-containing polar group contained in the polymer terminal group can be obtained by adjusting the components (polymerization initiator, chain transfer agent, etc.) used in the polymerization of the polymer. The oxygen-containing polar group is a polar atomic group containing an oxygen atom. However, the oxygen-containing polar group in the present invention does not include an ester bond itself or an ether bond itself, but includes an atomic group containing these bonds as a characteristic group.
[0016] The oxygen-containing polar group is preferably at least one group selected from the group consisting of a hydroxyl group, a carbonyl group-containing group, an acetal group, and an oxycycloalkane group, more preferably -CF2CH2OH, -C(CF3)2OH, a 1,2-glycol group (-CH(OH)CH2OH), an acetal group, >C(O), -CF2C(O)OH, >CFC(O)OH, a carboxamide group (-C(O)NH2, etc.), an acid anhydride residue (-C(O)OC(O)-), an imide residue (-C(O)NHC(O)-, etc.), a dicarboxylic acid residue (-CH(C(O)OH)CH2C(O)OH, etc.), a carbonate group (-OC(O)O-), an epoxy group, and an oxetanyl group, and even more preferably an acid anhydride residue. Furthermore, from the viewpoint of not impairing the adhesiveness of the F powder, the oxygen-containing polar group is particularly preferably a polar group which is a cyclic group or a ring-opening group thereof, such as a cyclic acid anhydride residue, a cyclic imide residue, a cyclic carbonate group, a cyclic acetal group, a 1,2-dicarboxylic acid residue, or a 1,2-glycol group, with a cyclic acid anhydride residue being most preferred.
[0017] More preferably, F polymer 1 is a polymer having TFE units, units based on hexafluoropropylene, perfluoro(alkyl vinyl ether) (PAVE) or fluoroalkylethylene (FAE) (hereinafter also referred to as "PAE units"), and units based on a monomer having an oxygen-containing polar group. Of all the units constituting the F polymer 1, the proportion of TFE units, the proportion of PAE units and the proportion of units based on the above-mentioned monomers are preferably 50 to 99 mol %, 0 to 10 mol % and 0.01 to 3 mol %, respectively.
[0018] Examples of PAVE include CF2=CFOCF3 (PMVE), CF2=CFOCF2CF3, CF2=CFOCF2CF2CF3 (PPVE), CF2=CFOCF2CF2CF2CF3, and CF2=CFO(CF2)8F, with PMVE or PPVE being preferred. FAEs include CH2=CH(CF2)2F, CH2=CH(CF2)3F, CH2=CH(CF2)4F(PFBE), CH2=CF(CF2)3H, and CH2=CF(CF2)4H. The PAE unit is preferably a PAVE-based unit.
[0019] The unit based on a monomer having an oxygen-containing polar group is preferably a unit based on a monomer having an acid anhydride residue, more preferably itaconic anhydride, citraconic anhydride, 5-norbornene-2,3-dicarboxylic anhydride (hereinafter also referred to as "NAH") or maleic anhydride, and further preferably NAH. The polar unit may be one type or two or more types.
[0020] Furthermore, the F polymer 1 may further contain other units. The other units may be of one type or of two or more types. Examples of monomers forming other units include ethylene, propylene, vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and chlorotrifluoroethylene.
[0021] A preferred embodiment of the F polymer is a polymer (hereinafter also referred to as "F polymer 2") containing 2 mol% or more of TFE units and units based on perfluoropropyl vinyl ether (hereinafter also referred to as "PPVE units"). F polymer 2 containing 2 mol% or more of PPVE units is likely to generate microcrystals and is likely to incorporate a filler to a high degree to form a dense molded product. F polymer 2 is composed of TFE units and PPVE units, and preferably contains 96 to 98 mol% of TFE units and 2 to 4 mol% of PPVE units.
[0022] A preferred embodiment of the F polymer is a polymer (hereinafter also referred to as "F polymer 3") containing TFE units and units based on perfluoromethylvinyl ether (hereinafter also referred to as "PMVE units"). Since F polymer 3 contains PMVE units with short side chains, it is easy to generate microcrystals and easily incorporates a filler to a high degree to form a dense molded product. F polymer 3 preferably contains 10 to 20 mol % of PMVE units. F polymer 3 is composed of TFE units and PMVE units, and preferably contains 80 to 90 mol % of TFE units and 10 to 20 mol % of PMVE units.
[0023] The MO filler in the present invention is a filler containing more than 50 mass % of a metal oxide. The metal oxide contained in the MO filler may be one type or two or more types. The content of the metal oxide in the MO filler is preferably 90% by mass or more, more preferably 95% by mass or more, and is preferably 100% by mass or less.
[0024] From the viewpoint of improving the thermal conductivity and scratch resistance of the molded product, the metal oxide is preferably at least one selected from the group consisting of aluminum oxide, lead oxide, iron oxide, tin oxide, calcium oxide, magnesium oxide, titanium oxide, zinc oxide, antimony pentoxide, zirconium oxide, lanthanum oxide, neodymium oxide, cerium oxide, and niobium oxide, and from the viewpoint of thermal conductivity, it is more preferably aluminum oxide or magnesium oxide, and from the viewpoint of low dielectric tangent, it is even more preferably magnesium oxide.
[0025] Examples of magnesium oxide include hard-burned magnesium oxide such as electrofused magnesia and magnesia clinker, and specific examples thereof include Magnesia RF-10C and Magnesia RF-50 (manufactured by Ube Material Industries, Ltd.).
[0026] The MO filler preferably further contains silicon oxide (silica). In this case, the interaction between the components in the dispersion is enhanced, and dispersibility is likely to be improved. The content of silicon oxide contained in the MO filler is preferably 0% by mass or more and 50% by mass or less, and more preferably 0% by mass or more and 20% by mass or less. The silicon oxide contained in the MO filler is preferably contained on the surface of the filler, and is preferably contained so as to cover the surface of the filler. In this case, not only the dispersibility of the dispersion is improved, but also the balance of physical properties derived from the metal oxide in the molded product formed therefrom is improved. In addition, the water resistance of the molded product is likely to be improved.
[0027] The silicon oxide contained in the MO filler is preferably derived from a silicon oxide filler or a cured product of a silane coupling agent, reactive silicone or siloxane. The silane coupling agent is preferably 3-aminopropyltriethoxysilane, vinyltrimethoxysilane, 3-mercaptopropyltrimethoxysilane, 3-glycidoxypropylmethyldiethoxysilane, 3-methacryloxypropyltriethoxysilane or 3-isocyanatopropyltriethoxysilane. The siloxane is preferably a polysiloxane or an oligomeric siloxane, more preferably an oligomeric siloxane. The oligomeric siloxane is preferably an oligomeric siloxane having a reactive group in the side chain. Examples of the reactive group include a vinyl group, an amino group, an epoxy group, a methacryloxy group, an acryloxy group, and a mercapto group. The average degree of polymerization of the oligomeric siloxane is preferably 2 to 20.
[0028] The oligomeric siloxane is preferably a homopolymer of a silane coupling agent having a reactive group, or a copolymer of a silane coupling agent having a reactive group and a silane coupling agent having no reactive group, and more preferably a homopolymer of vinylmethoxysilane, or a copolymer of trimethoxysilane having an amino group and trimethoxysilane having an alkyl group. Specific examples of oligomeric siloxanes include those described in JP-A-5-194544 and JP-A-2000-178449, and more specific examples include Dynasylan 6490 and Dynasylan 1146 (manufactured by Evonik Degussa Japan Ltd.). A specific example of the MO filler containing silicon oxide is a filler containing magnesium oxide, calcium oxide, and silicon oxide in the amounts of 94.0 to 99.7 mass%, 0.1 to 1.5 mass%, and 0.1 to 3.0 mass%, respectively. Such an MO filler is preferably obtained by mixing and firing the respective components.
[0029] The MO filler may be particulate or fibrous. If a particulate filler is used, a part of the filler particles is exposed on the surface of the molded article, and the wear resistance and scratch resistance of the surface of the molded article are more likely to be improved. On the other hand, if a fibrous filler is used, the surface flatness of the molded article is improved and the sliding property of the surface is improved, so that the scratch resistance is also more likely to be improved.
[0030] The particulate filler preferably has an average particle size (D50) of 0.02 to 200 μm. The fibrous filler preferably has an average fiber length of 0.05 to 300 μm. The fibrous filler preferably has an average fiber diameter of 0.01 to 15 μm. The average particle size of the particulate filler is preferably equal to or greater than the average particle size of the powder, and the average fiber length of the fibrous filler is preferably equal to or greater than the average particle size of the powder. In this case, not only is the sedimentation of the filler in the dispersion suppressed, but the physical properties (heat conductivity, scratch resistance, electrical properties, etc.) of the molded product are more likely to be improved.
[0031] A preferred embodiment of the MO filler is aluminum oxide or magnesium oxide particles, or aluminum oxide or magnesium oxide fibers. The use of such particles tends to further increase the abrasion resistance and scratch resistance of the surface of the molded article. On the other hand, the use of such fibers tends to further increase the scratch resistance of the surface of the molded article. In addition, preferred embodiments of the MO filler include magnesium oxide particles surface-treated with an oligomeric siloxane having a reactive group, and magnesium oxide particles containing silicon oxide and calcium oxide. Such fillers are likely to improve the low dielectric tangent and low transmission loss of molded articles.
[0032] The MO filler may further contain a nitride (boron nitride, silicon nitride, aluminum nitride, etc.). In such a preferred embodiment, the content of the nitride is preferably 5 to 75 mass%. In addition, an embodiment of the MO filler containing a nitride may have a core-shell structure with a metal oxide as the core and a nitride as the shell. When forming such a core-shell type MO filler, a sintering aid may be further used.
[0033] The SO filler in the present invention is a filler containing silicon oxide, which is different from the MO filler. The content of silicon oxide in the SO filler is more than 50 mass %, and preferably 90 mass % or more. The content of silicon oxide is preferably 100 mass % or less. The SO filler is preferably a silica filler, a talc filler, or a steatite filler. In this case, the interaction between the components in the dispersion is enhanced, and dispersibility is easily improved. In addition, the balance of physical properties derived from silicon oxide in the molded product is easily improved, and in particular, electrical properties (low dielectric tangent, etc.) are easily improved.
[0034] At least a part of the surface of the SO filler is preferably surface-treated. The shape of the SO filler may be any of granular, needle-like (fibrous) and plate-like. Specific shapes of the SO filler include spherical, scale-like, layered, leaf-like, apricot kernel-like, columnar, cockscomb-like, equiaxed, leaf-like, micaceous, block-like, flat, wedge-like, rosette-like, net-like and prismatic shapes. The SO filler preferably has a spherical or scaly shape, which enhances the interaction between the components in the dispersion and improves dispersibility, thereby improving the balance of physical properties derived from the components in the molded product formed therefrom.
[0035] The average particle size of the SO filler is preferably 0.1 to 10 μm. A specific example of the filler containing spherical silicon oxide is a filler containing substantially spherical silicon oxide. Note that the substantially spherical filler refers to an inorganic filler in which 95% or more of the particles are spherical and have a ratio of the minor axis to the major axis of 0.7 or more when observed with a scanning electron microscope (SEM).
[0036] The spherical silicon oxide-containing filler may have a single-layer structure or a multi-layer structure, and the spherical SO filler may be a sintered ceramic. A specific example of the scaly SO filler is a filler having an average major axis (average value of diameter in the longitudinal direction) of 1 μm or more and 10 μm or less, and an average minor axis of 0.01 μm or more and 1 μm or less. The scaly SO filler may have a single-layer structure or a multi-layer structure, and may be a sintered ceramic.
[0037] The SO filler preferably has a hollow structure, in which case the molded product obtained from it is likely to have a well-balanced linear expansion property and electrical properties (particularly low dielectric constant and low dielectric loss tangent). The hollow ratio of the hollow SO filler (average volume ratio of voids per filler particle) is preferably 50 to 80%, and the pressure resistance of the hollow SO filler is preferably 20 MPa or more.
[0038] Specific examples of SO fillers include spherical silica fillers (such as the "Admafine" series manufactured by Admatechs and the "SFP" series manufactured by Denka), hollow silica fillers (such as the "E-SPHERES" series manufactured by Taiheiyo Cement Corporation, the "Silinax" series manufactured by Nippon Steel Mining Co., Ltd., and the "Ecocospher" series manufactured by Emerson & Cumming Co., Ltd.), talc fillers (such as the "SG" series manufactured by Nippon Talc Co., Ltd.), and steatite fillers (such as the "BST" series manufactured by Nippon Talc Co., Ltd.). The SO filler may be used alone or in combination with two or more kinds. The SO filler may be used in combination with a hollow filler and a non-hollow filler. In such a case, the dispersion tends to have excellent dispersion stability, and the molded product tends to have excellent low linear expansion and low dielectric tangent.
[0039] The polar liquid dispersion medium in the present invention is a liquid component that disperses the F powder, the MO filler, and the SO filler, and is a compound that is liquid at 25°C. The liquid dispersion medium may be protic or aprotic. The liquid dispersion medium may be an aqueous solvent or a non-aqueous solvent. The liquid dispersion medium may be used alone or in combination of two or more kinds. The liquid dispersion medium is preferably water, an amide, an alcohol, a sulfoxide, an ester, a ketone or a glycol ether, more preferably water, a ketone or an amide, and even more preferably a ketone or an amide.
[0040] Specific examples of liquid dispersion media include water, methanol, ethanol, isopropanol, N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, dimethyl sulfoxide, diethyl ether, dioxane, ethyl lactate, ethyl acetate, butyl acetate, methyl ethyl ketone, methyl isopropyl ketone, cyclopentanone, cyclohexanone, ethylene glycol monoisopropyl ether, and cellosolve (methyl cellosolve, ethyl cellosolve, etc.). Particularly preferred liquid dispersion media are water, methyl ethyl ketone, cyclohexanone or N-methyl-2-pyrrolidone.
[0041] From the viewpoint of further improving the dispersibility of the F powder, the MO filler, and the SO filler, the dispersion of the present invention preferably further contains a nonionic surfactant (dispersant). In addition, the nonionic surfactant acts to increase the viscosity of the dispersion, and is also considered to function as an anti-settling agent that prevents the F powder and both fillers from settling in the dispersion. Examples of such nonionic surfactants include non-polymeric compounds containing a hydroxyl group and a polyoxyalkylene group (1), compounds containing a hydrolyzable silyl group (2), non-polymeric compounds having a fluorine-containing group and a hydroxyl group (3), polyhydroxy compounds (4), polymers containing an acetal group or a hemiacetal group (5), and polymers containing a hydroxyl group or a polyoxyalkylene group (6).
[0042] Specific examples of the compound (1) include oxyalkylene glycols and oxyalkylene glycol monoethers, and more specifically, compounds represented by the general formula: R 1 O(CH2CH2O) m1 A compound represented by the formula: 1 represents a hydrogen atom or an alkyl group having 10 to 15 carbon atoms, and m1 represents the average number of moles added and is an integer of 1 to 15. Specific examples of the compound (2) include compounds represented by the general formula: (R 21 ) m21 -Si-(OR 22 ) 4-m21 A silicon compound represented by the formula: 21 is an alkyl group having 1 to 12 carbon atoms, R 22 is an alkyl group having 1 to 4 carbon atoms, and m21 is an integer of 1 to 3. Specific examples of the compound (3) include compounds represented by the general formula: R 33 -O-(CH2CH2O) m31 (CH2CH(CH3)O) m32 A compound represented by the formula: 31 is a polyfluoroalkyl group having 1 to 12 carbon atoms, m31 is an integer of 1 to 12, b is an integer of 1 to 20, and m32 is an integer of 0 to 12.
[0043] Specific examples of the polyhydroxy compound (4) include polyvinyl alcohol, polyethylene glycol, polyethylene oxide, hydroxyethyl cellulose, hydroxypropyl methyl cellulose, carboxymethyl cellulose, starch, agarose, and lactose. A specific example of the polymer (5) is a terpolymer containing a unit based on vinyl butyral, a unit based on vinyl acetate, and a unit based on vinyl alcohol. The ratio of each unit is not particularly limited, but is set in consideration of the ease of interaction with the F polymer, metal oxide, and solvent. Specific examples of the polymer (6) include fluorine-based surfactants, silicone-based surfactants, and acetylene-based surfactants.
[0044] As the nonionic surfactant, a polymeric nonionic surfactant having an alcoholic hydroxyl group or a polyoxyalkylene group, and a perfluoroalkyl group, a perfluoroalkyl group having an etheric oxygen atom, or a perfluoroalkenyl group on the side chain (hereinafter also referred to as "polymer dispersant F") is preferred. In this case, the affinity of the nonionic surfactant for each component is well balanced, and in addition to the dispersibility of the powder and filler in the dispersion, the film-forming property is likely to be further improved.
[0045] The polymer dispersant F more preferably has a fluorine content of 10 to 50 mass % and a hydroxyl value of 10 to 35 mgKOH / g. The polymer dispersant F may be a polymer containing a unit based on fluoro(meth)acrylate and a unit based on oxyalkylene glycol mono(meth)acrylate. This polymer is a polymer other than the F polymer. Specific examples of the former (meth)acrylate include CH2=C(CH3)C(O)OCH2CH2(CF2)6F, CH2=CHC(O)OCH2CH2(CF2)6F, CH2=C(CH3)C(O)OCH2CH2(CF2)4F, CH2=CClC(O)OCH2CH2(CF2)4F, CH2=C(CH3)C(O)OCH2CH2CH2CH2OCF(CF3)C(=C(CF3)2)(CF(CF3)2), and CH2=CH3C(O)OCH2CH2CH2CH2OCF(CF3)C(=C(CF3)2)(CF(CF3)2).
[0046] Specific examples of the latter (meth)acrylate include CH2=C(CH3)C(O)(OCH2CH2)4OH, CH2=C(CH3)C(O)(OCH2CH2)9OH, and CH2=C(CH3)C(O)(OCH2CH2). 23 OH, CH2=C(CH3)C(O)(OCH2CH2) 66 OH, CH2=C(CH3)C(O)(OCH2CH2) 90 OH, CH2=C(CH3)C(O)(OCH2CH2) 120 OH, CH2=CHC(O)(OCH2CH2)4OH, CH2=CHC(O)(OCH2CH2)8OH, CH2=C(CH3)C(O)(OCH2CH(CH3))4OH, CH2= C(CH3)C(O)(OCH2CH(CH3))8OH, CH2=C(CH3)C(O)(OCH2CH(CH3))9OH, CH2=C(CH3)C(O)(OCH2CH(CH3)) 13 OH, CH2=C(CH3)C(O)(OCH2CH2)4·(OCH2CH(CH3))3OH, CH2=C(CH3)C(O)(OCH2CH2) 10 (OCH2CH2CH2CH2)5OH.
[0047] The dispersion of the present invention preferably further contains a binder from the viewpoints of improving the coatability of the dispersion (such as suppressing the falling off of the F powder when a polymer layer is formed from the dispersion) and the smoothness of the molded product. As the binder, maleimide resin, polyimide resin, polyamic acid resin, polyamideimide resin, (meth)acrylic resin, urethane resin, glyoxal resin or phenol resin is preferable, and maleimide resin, polyimide resin or polyamic acid resin is more preferable. These resins are preferably thermoplastic resins, and particularly preferably thermoplastic resins whose glass transition temperature is equal to or lower than the melting temperature of the F polymer. Furthermore, these resins are preferably binder resins that dissolve in a liquid dispersion medium.
[0048] The content of the F polymer in the dispersion of the present invention is preferably 5% by mass or more, more preferably 10 to 60% by mass, and more preferably 20 to 40% by mass, which makes it easy to form a molded product having excellent physical properties (particularly electrical properties). The content of the MO filler in the dispersion of the present invention is 5% by mass or more, preferably 8% by mass or more, and more preferably 10% by mass or more, and the upper limit is usually preferably 50% by mass, and more preferably 40% by mass. The content of the SO filler in the dispersion of the present invention is preferably 1% by mass or more, more preferably 3% by mass or more, and even more preferably 5% by mass or more, with the upper limit being preferably 40% by mass, and more preferably 30% by mass. The ratio of the content of the SO filler to the content of the MO filler in the dispersion of the present invention is less than 1, and preferably 0.8 or less, and more preferably 0.2 or more, and more preferably 0.5 or more.
[0049] The content of the liquid dispersion medium in the dispersion of the present invention is preferably 15 to 55% by mass, more preferably 25 to 50% by mass, in which case the dispersion has excellent coatability and is likely to have improved film-forming properties. Furthermore, when the dispersion of the present invention contains a nonionic surfactant, the content thereof is preferably 0.1 to 10 mass %, more preferably 0.5 to 5 mass %, which further enhances the dispersibility of the powder and filler in the dispersion, and tends to further improve the physical properties (thermal conductivity, scratch resistance, etc.) of the molded product. When the dispersion of the present invention contains a binder, the content thereof is preferably 0.1 to 30% by mass, more preferably 1 to 10% by mass. The ratio of the content of the binder resin to the content of the F polymer is preferably 1.0 or less, more preferably 0.01 to 0.5.
[0050] The sum of the F polymer content, the MO filler content and the SO filler content contained in the dispersion of the present invention is preferably 20% by mass or more, more preferably 30% by mass or more, and even more preferably 40% by mass or more. As described above, since the F polymer and both fillers highly interact with each other in the dispersion, even if the above sum is high, the dispersion of the present invention has excellent dispersibility and coatability. The above sum is preferably 80% by mass or less. The mass ratio of the content of the MO filler to the content of the F polymer is preferably 0.1 or more, more preferably 0.3 or more. This mass ratio is preferably 2 or less, more preferably 1 or less. The mass ratio of the content of the SO filler to the content of the F polymer is preferably 0.1 or more, more preferably 0.2 or more. This mass ratio is preferably 2 or less, more preferably 1 or less. As described above, since the F polymer, the MO filler and the SO filler interact highly in the dispersion, even when the mass ratio is high, the dispersion of the present invention has excellent dispersibility and coatability. As a result, a molded product containing both fillers uniformly and at high concentrations can be easily formed from the dispersion of the present invention. The mass ratio is preferably 2 or less, more preferably 1 or less.
[0051] The dispersion of the present invention may further contain other resins. Examples of such other resins include epoxy resins, liquid crystalline polyester resins, polyolefin resins, cyanate ester resins, vinyl ester resins, urea resins, diallyl phthalate resins, melamine resins, guanamine resins, melamine-urea co-condensation resins, styrene resins, polycarbonate resins, polyarylate resins, polysulfones, polyarylsulfones, aromatic polyamide resins, aromatic polyether amides, polyphenylene sulfide, polyaryl ether ketones, and polyphenylene ethers. These other resins may or may not be soluble in the dispersion, may be thermosetting or thermoplastic, and may be modified. The dispersion of the present invention may further contain a thixotropic agent, an antifoaming agent, a silane coupling agent, a dehydrating agent, a plasticizer, a weathering agent, an antioxidant, a heat stabilizer, a lubricant, an antistatic agent, a brightening agent, a colorant, a conductive agent, a release agent, a surface treatment agent, a viscosity adjusting agent, or a flame retardant.
[0052] The viscosity of the dispersion of the present invention at 25° C. is preferably 10,000 mPa·s or less, more preferably 50 to 5,000 mPa·s, and even more preferably 100 to 1,000 mPa·s, in which case the dispersion is excellent not only in dispersibility but also in handleability. The thixotropy ratio of the dispersion of the present invention is preferably from 1.0 to 2.5, more preferably from 1.2 to 2.0, in which case not only is the dispersion excellent in dispersibility, but the homogeneity of the molded product is also likely to be improved.
[0053] The dispersion of the present invention contains a large amount of F powder, MO filler, and silicic acid filler, and has excellent dispersion stability. In addition, the molded product obtained from the dispersion can have the physical properties of the F polymer and the filler to a high degree. By using the dispersion of the present invention, a thick molded product having a thermal conductivity of 1 W / mK or more and a molded product having a dielectric loss tangent of 0.005 or less can be easily obtained.
[0054] The method for producing the laminate of the present invention is a method in which the dispersion of the present invention is applied to a substrate layer, heated to volatilize the polar liquid dispersion medium, and further heated to bake the F polymer, thereby obtaining a laminate having a substrate layer and a polymer layer containing an F polymer, an MO filler, and an SO filler (hereinafter also referred to as "the laminate").
[0055] Examples of the base layer in the present invention include metal substrates (metal foils of copper, nickel, aluminum, titanium, alloys thereof, etc.), resin films (films of polyimide, polyarylate, polysulfone, polyarylsulfone, polyamide, polyetheramide, polyphenylene sulfide, polyaryletherketone, polyamideimide, liquid crystalline polyester, liquid crystalline polyesteramide, etc.), and prepregs (precursors of fiber-reinforced resin substrates). As the base layer, a metal substrate and a resin film are preferred.
[0056] The metal substrate is preferably a copper foil, more preferably a rolled copper foil with no front and back distinction or an electrolytic copper foil with front and back distinction, and even more preferably a rolled copper foil. Since the rolled copper foil has a small surface roughness, the transmission loss can be reduced even when the laminate is processed into a printed wiring board. The surface of the metal substrate may be provided with an anticorrosive layer (such as an oxide film of chromate or the like), a heat-resistant layer, a roughening treatment layer, or a silane coupling agent treatment layer. The resin film is preferably a polyimide film. The thickness of the substrate layer is preferably 0.1 to 150 μm. Specifically, if the substrate layer is a metal foil, the thickness of the substrate layer is preferably 1 to 30 μm. If the substrate layer is a resin film, the thickness of the substrate layer is preferably 1 to 150 μm, and more preferably 10 to 50 μm.
[0057] The dispersion liquid may be applied to only one surface of the substrate layer, or may be applied to both surfaces of the substrate layer. In the former case, a laminate having a substrate layer and a polymer layer on one surface of the substrate layer is obtained, and in the latter case, a laminate having a substrate layer and a polymer layer on both surfaces of the substrate layer is obtained. The latter laminate is less likely to warp, and therefore has excellent handling properties during processing. The dispersion can be applied by a method such as spraying, roll coating, spin coating, gravure coating, microgravure coating, gravure offset, knife coating, kiss coating, bar coating, die coating, fountain-meyer bar, or slot die coating. The heating is preferably carried out within a temperature range in which the F polymer is baked. The heating may be carried out at a constant temperature or at different temperatures. Examples of the heating method include a method using an oven, a method using a ventilated drying furnace, and a method using heat rays such as infrared rays. The heating may be carried out either under normal pressure or under reduced pressure.
[0058] The laminate may have a polymer layer in contact with at least one surface of the substrate layer. Examples of the layer structure include substrate layer / polymer layer, substrate layer / polymer layer / substrate layer, polymer layer / substrate layer / polymer layer, and substrate layer / polymer layer / other substrate layer / polymer layer / substrate layer. The term "substrate layer / polymer layer" refers to a substrate layer and a polymer layer laminated in this order, and the same applies to other layer structures. The definitions of the other base layers, including the ranges and preferred embodiments, are the same as those of the base layer described above.
[0059] In the present laminate, the thickness of the polymer layer is preferably from 1 to 100 μm, more preferably from 5 to 75 μm, and even more preferably from 10 to 50 μm. The present laminate also has a high peel strength between the polymer layer and the substrate layer, which is preferably 10 N / cm or more. The thermal conductivity of the polymer layer is preferably 1 W / m·K or more, more preferably 2 W / m·K or more, and even more preferably 3 W / m·K or more. The upper limit of the thermal conductivity of the polymer layer is 100 W / m·K.
[0060] Since this laminate comprises a polymer layer containing F powder, MO filler, and SO filler, it has excellent physical properties such as heat resistance, electrical properties, thermal conductivity (heat dissipation), and scratch resistance, and is useful as an electronic substrate material such as a flexible printed wiring board or a rigid printed wiring board, or as a heat dissipation substrate, particularly for automobiles. For example, if the base layer of the laminate is a metal foil, a printed wiring board can be manufactured by etching the metal foil to form a metal conductor wiring (transmission circuit) of a predetermined pattern. Such a printed wiring board has a metal conductor wiring and a polymer layer in this order. Examples of the configuration include a metal conductor wiring / polymer layer and a metal conductor wiring / polymer layer / metal conductor wiring. In addition, a plurality of printed wiring boards having the above configuration may be multi-layered. The dispersion of the present invention may also be used to form a bonding sheet, an interlayer insulating film, a solder resist, or a coverlay film for a printed wiring board.
[0061] A preferred embodiment of the printed wiring board formed from the present laminate includes an embodiment having, in this order, a metal foil or a transmission circuit formed by processing the metal foil, a polymer layer, and an aluminum substrate. Examples of configurations of the above-mentioned aspects include metal foil / polymer layer / aluminum substrate, transmission circuit formed by processing metal foil / polymer layer / aluminum substrate, metal foil / polymer layer / aluminum substrate / polymer layer / metal foil, the above-mentioned transmission circuit / polymer layer / aluminum substrate / polymer layer / the above-mentioned transmission circuit, and the above-mentioned transmission circuit / polymer layer / aluminum substrate / polymer layer / metal foil.
[0062] A suitable embodiment of the printed wiring board formed from the present laminate includes an embodiment having, in this order, a metal foil or a transmission circuit formed by processing the metal foil, a polymer layer, and a resin film layer. Examples of the configuration of the above embodiment include metal foil / polymer layer / resin film layer, transmission circuit / polymer layer / resin film layer formed by processing metal foil, metal foil / polymer layer / resin film layer / polymer layer / metal foil, the above-mentioned transmission circuit / polymer layer / resin film layer / polymer layer / the above-mentioned transmission circuit, and the above-mentioned transmission circuit / polymer layer / resin film layer / polymer layer / metal foil.
[0063] The polymer layer in the present invention is highly uniform and contains an F polymer with excellent adhesiveness and heat resistance, an SO filler with excellent electrical properties, and a large amount of MO filler, so that it is easy to firmly adhere to any substrate (metal foil or transmission circuit and aluminum substrate). The laminate or printed wiring board of this embodiment can be said to be an aluminum-based laminate or aluminum-based printed wiring board with excellent heat resistance and thermal conductivity, and can be suitably used in applications such as power modules (for LED lighting, etc.) that are used in high-temperature atmospheres and require high heat dissipation.
[0064] The polymer layer in these embodiments may be surface-treated to further improve adhesion. Examples of the surface treatment include corona treatment, plasma treatment, and electron beam treatment. In addition, an adhesive layer (such as a layer formed by a silane coupling agent) may be formed on the surface of the polymer layer to further improve adhesion. The thickness of the polymer layer is preferably from 1 to 200 μm, more preferably from 3 to 20 μm. Examples of the material for the aluminum substrate include aluminum and aluminum alloys. From the viewpoint of annealing resistance, the aluminum alloy is preferably an alloy of aluminum with manganese, magnesium or chromium. The surface of the aluminum substrate may be subjected to a roughening treatment or a coating treatment. The thickness of the aluminum substrate is preferably 0.5 to 3 mm. If the thicknesses of the polymer layer and the aluminum substrate are within the above ranges, a circuit board with higher heat dissipation properties can be easily formed.
[0065] The molded article of the present invention contains an F polymer, an MO filler, and an SO filler. The content of the polymer in the molded article is 50% by mass or more, and the total content of the MO filler and the SO filler in the molded article is 10% by mass or more. The definitions of the F polymer, MO filler and SO filler in the molded product of the present invention, including their preferred embodiments and scope, are the same as those explained in the manufacturing method of the dispersion and laminate of the present invention. The molded article of the present invention is preferably a monolayer film consisting of a polymer layer.
[0066] In the molded product of the present invention, the MO filler and the SO filler are uniformly and firmly held in the F polymer matrix, and it is believed that the physical properties based on the metal oxide and silicon oxide (thermal conductivity, scratch resistance, electrical properties, etc.) are well exhibited. In addition, since the F polymer has an oxygen-containing polar group, the molded product exhibits high adhesiveness on its surface. Therefore, when the molded product of the present invention is adhered to a circuit board on which a semiconductor chip is mounted so as to cover the semiconductor chip, it can be used as a heat dissipation film, a protective film, etc. In addition, the molded product of the present invention can be suitably used as an adhesive layer between a heat-generating electronic component and a heat sink.
[0067] The content of the F polymer in the molded product of the present invention is preferably 50% by mass or more, more preferably 60 to 80% by mass, which makes it easier to form a polymer layer having excellent physical properties (particularly electrical properties). The sum of the contents of the MO filler and the SO filler contained in the molded product of the present invention is 10% by mass or more, and preferably 20% by mass or more. The upper limit of the sum of the contents of the MO filler and the SO filler contained in the molded product of the present invention is 50% by mass. A polymer layer containing a large amount of metal oxide filler can more suitably exhibit physical properties based on metal oxide (thermal conductivity, scratch resistance, etc.). In addition, a polymer layer containing a large amount of SO filler can more suitably exhibit physical properties based on silicon oxide (electrical properties, low linear expansion, etc.).
[0068] The content of the MO filler in the molded product of the present invention is preferably 5% by mass or more, more preferably 20% by mass or more, with the upper limit usually being 45% by mass. The content of the SO filler in the molded product is preferably 5% by mass or more, more preferably 20% by mass or more, and the upper limit is usually 45% by mass.
[0069] The thickness of the molded product of the present invention is preferably 1 to 1000 μm, more preferably 5 to 100 μm, and even more preferably 10 to 50 μm. A molded product of such a thickness can exhibit high flexibility (pliability) while ensuring sufficient mechanical strength. Therefore, it is useful as a heat dissipation film, a protective film, etc.
[0070] The thermal conductivity of the molded product of the present invention is preferably 1 W / mK or more, more preferably 2 W / m K or more, and even more preferably 3 W / m K or more. The upper limit of the thermal conductivity of the molded product is 100 W / m K. Since the molded product has excellent thermal conductivity, it is useful as a heat dissipation film. The dielectric loss tangent of the molded product is preferably 0.005 or less, more preferably 0.003 or less. The lower limit of the dielectric loss tangent of the molded product is 0. The molded product of the present invention has excellent low dielectric loss tangent and is therefore useful as a material for electronic device substrates such as printed circuit boards.
[0071] Furthermore, for the purpose of increasing electrical insulation and mechanical strength, a fiber base material may be embedded in the molded product. The fiber substrate is preferably a heat-resistant woven fabric that can withstand heat, more preferably a glass fiber woven fabric, a carbon fiber woven fabric, an aramid fiber woven fabric or a metal fiber woven fabric, and even more preferably a glass fiber woven fabric or a carbon fiber woven fabric. In particular, from the viewpoint of improving electrical insulation, it is preferable to use, as the fiber substrate, a plain-woven glass fiber fabric composed of an electrically insulating E-glass yarn as specified in JIS R 3410: 2006. In this case, if the fiber substrate is treated with a silane coupling agent, the adhesion with the F polymer is further improved.
[0072] The molded product of the present invention may be obtained by applying the dispersion of the present invention to the surface of a substrate layer, heating the dispersion to form a polymer layer containing an F polymer, an MO filler, and an SO filler, and then removing the substrate layer. In other words, the molded product of the present invention can be obtained by removing the substrate from the laminate of the present invention. Here, the molded product in which the fiber substrate is embedded can be produced by impregnating the fiber substrate with the dispersion of the present invention, and then heating the fiber substrate to bake the F powder.
[0073] In the production of the present molded article, the substrate layer can be removed by either wet etching or dry etching. When the substrate layer is a metal foil, the metal foil is preferably removed by wet etching. In this case, the wet etching is preferably performed using an acid solution. If the F polymer has an oxygen-containing polar group, it is activated by an acid solution, and the adhesion of the surface (contact surface) of the molded product after the metal foil is removed is more likely to be increased. Here, an example of the activation of the oxygen-containing polar group is the conversion of an acid anhydride group to a 1,2-dicarboxylic acid group. The acid solution can be an aqueous solution of an inorganic acid such as hydrochloric acid, dilute nitric acid, or hydrofluoric acid. In addition, when a roughened metal foil is used, minute irregularities are transferred to the surface (contact surface) of the film, which improves adhesion to other substrates when the substrate is bonded to the surface of the molded product.
[0074] As described above, by using wet etching to remove the metal foil, it is possible to reliably remove the metal foil while preventing damage to the minute irregularities transferred to the surface of the molded article. The molded article of the present invention is heat-pressed to a base layer to obtain a laminate having the base layer and the molded article. The definition of the base layer, including its preferred embodiment and scope, is the same as that of the laminate of the present invention.
[0075] Although the dispersion, the method for producing a laminate, and the molded product of the present invention have been described above, the present invention is not limited to the configurations of the above-mentioned embodiments. For example, the dispersion and the molded product of the present invention may each additionally have any other constituent in the constitution of the above embodiment, or may be substituted with any constituent that produces a similar effect. Furthermore, the method for producing a laminate of the present invention may further include any other step in the configuration of each of the above-described embodiments, or may be substituted with any other step that produces a similar effect. EXAMPLES
[0076] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. 1. Preparation of each ingredient [powder] Powder 1: Powder (D50: 1.8 μm, D90: 5.2 μm) made of a copolymer (melting temperature: 300° C.) containing 98.0 mol%, 0.1 mol%, and 1.9 mol% of TFE units, NAH units, and PPVE units, in that order, and having an oxygen-containing polar group. Powder 2: Powder consisting of a copolymer (melting temperature 305°C) containing 97.5 mol% TFE units and 2.5 mol% PPVE units, in that order, and having no oxygen-containing polar group (D50: 18.8 μm, D90: 52.3 μm) Powder 3: Powder consisting of a copolymer (melting temperature 305°C) containing 98.7 mol% TFE units and 1.3 mol% PPVE units, in that order, and having no oxygen-containing polar group (D50: 0.3 μm, D90: 0.9 μm) Powder 4: Powder made of non-melting PTFE (D50: 3.2 μm)
[0077] [Filler] MO1: Granular magnesium oxide filler (D50: 10 μm. Ube Material Industries, Ltd., "Magnesia RF-10C." Magnesium oxide content: over 50% by mass.) MO2: Aluminum oxide filler (D50: 3 μm. Sumitomo Chemical Co., Ltd., "AA-3". Aluminum oxide content: over 50% by mass.) SO1: Spherical and hollow silica filler (D50: 4μm. Taiheiyo Cement Corporation, "E-SPHERES". Silicon oxide content: over 50% by mass.) SO2: Scaly steatite filler (D50: 4.8μm, average major axis: 5.7μm, average minor axis: 0.3μm, aspect ratio: 20, Nippon Talc Co., Ltd. "BST". Silicon oxide content: over 50% by mass.) [Binding agent] Varnish 1: Varnish in which thermoplastic aromatic polyimide (PI1) is dissolved in NMP [Nonionic surfactants] Surfactant 1: CH2=C(CH3)C(O)OCH2CH2(CF2)6F and CH2=C(CH3)C(O)(OCH2CH2) 23 Copolymer with OH [Liquid dispersion medium] NMP: N-methyl-2-pyrrolidone
[0078] 2. Preparation of Dispersion (Example 1) First, powder 1, varnish 1, surfactant 1, and NMP were added to a pot, and zirconia balls were added. The pot was then rolled at 150 rpm for 1 hour to prepare a composition. Filler MO1, filler SO1, surfactant 1, and NMP were added to another pot, and zirconia balls were added. The pot was then rolled at 150 rpm for 1 hour to prepare a composition. In addition, both compositions were put into another pot, and zirconia balls were put in. The pot was then rolled at 150 rpm for 1 hour to obtain Dispersion 1 containing Powder 1 (20 parts by mass), Filler MO1 (10 parts by mass), Filler SO1 (5 parts by mass), PI1 (1 part by mass), Surfactant 1 (4 parts by mass), and NMP (60 parts by mass).
[0079] (Examples 2 to 8) Dispersions 2 to 8 were obtained in the same manner as in Example 1, except that the types and amounts of the powder, filler, varnish, surfactant, and liquid dispersion medium were changed as shown in Table 1 below.
[0080] [Table 1]
[0081] 3. Evaluation 3-1. Evaluation of dispersion liquid 3-1-1. Evaluation of dispersion stability After each dispersion was stored in a container at 25° C., its dispersibility was visually confirmed and the dispersion stability was evaluated according to the following criteria. [Evaluation Criteria] ◯: No aggregates visible. △: Aggregates are visible at the bottom of the container. They are uniformly redispersed when stirred with shear. ×: Aggregates are visible at the bottom of the container. Redispersion is difficult even with stirring under shear. 3-1-2. Viscosity measurement The viscosity of each dispersion was measured using a Brookfield viscometer at room temperature (25° C.) and a rotation speed of 30 rpm. Each viscosity measurement was repeated three times, and the average value of the three measured values was recorded as the viscosity. 3-1-3. Evaluation of thixotropy The viscosity of each dispersion was measured using a B-type viscometer at room temperature (25°C) and a rotation speed of 30 rpm, and was defined as viscosity η1. Similarly, the viscosity was measured at a rotation speed of 60 rpm, and was defined as viscosity η2. The thixotropy ratio was calculated by dividing η1 by η2. Each viscosity measurement was repeated three times, and the average of the three measured values was used.
[0082] 3-2. Evaluation of laminate 3-2-1. Evaluation of adhesion First, the dispersion liquid 1 was applied to the surface of a copper foil having a thickness of 18 μm by a roll-to-roll gravure reverse method to form a liquid coating. Next, the copper foil on which the liquid coating was formed was passed through a drying oven at 120° C. for 5 minutes and dried by heating. After that, the dried coating was heated at 340° C. for 3 minutes in a far-infrared oven under a nitrogen atmosphere. This produced a laminate 1 in which a polymer layer (thickness 10 μm) was formed on the surface of the copper foil.
[0083] Laminates 2 to 8 were obtained in the same manner as Laminate 1, except that Dispersion 1 was changed as shown in Dispersions 2 to 8. In this case, the dried coating formed from Dispersion 8 was more prone to powdering than the liquid coating formed from Dispersion 1. Rectangular test pieces (100 mm long, 10 mm wide) were cut out from the obtained laminates 1 to 3 and 5 to 8. The test pieces were fixed at a position 50 mm from one end in the longitudinal direction, and the copper foil and the polymer layer were peeled off at an angle of 90° to the test piece from one end in the longitudinal direction at a pulling speed of 50 mm / min. The maximum load applied at this time was measured as the peel strength (N / cm) and evaluated according to the following criteria: Laminate 4 was not evaluated because it did not have a uniform polymer layer. [Evaluation Criteria] ○:10N / cm or more △: 5N / cm or more and less than 10N / cm ×: Less than 5N / cm
[0084] 3-2-2.Evaluation of transmission loss A transmission line was formed in each of the laminates 1 to 3 and 5 to 8 to prepare a printed circuit board. A microstrip line was used to form the transmission line. A 28 GHz signal in the printed circuit board was processed using a vector network analyzer (manufactured by Keysight Technologies, Inc., "E8361A"), and the S21 parameter representing the transmission loss was measured using a Universal Test Fixture as a probe. At that time, the characteristic impedance of the line was set to 50Ω, and the length of the transmission line of the printed circuit board was set to 50 mm, and the transmission loss was measured.
[0085] The transmission loss was measured using the "S21-parameter," a circuit network parameter used to express the characteristics of high-frequency electronic circuits and components. The closer this value is to 0, the smaller the transmission loss. [Evaluation Criteria] ○: -1.0dB or more and less than 0dB △: -1.2dB or more - less than 1.0dB ×: Less than -1.2 dB
[0086] 3-3. Film evaluation 3-3-1.Evaluation of thermal conductivity The copper foil of the laminate 1 was removed by etching with an aqueous solution of ferric chloride to obtain a film 1. Films 2, 3 and 5 to 8 were obtained in the same manner as Film 1, except that Laminate 1 was changed to Laminates 2, 3 and 5 to 8. Film 8 was more brittle than Film 1.
[0087] Next, a 10 mm × 10 mm square test piece was cut from the center of each film, and the thermal conductivity (W / m K) in the in-plane direction was measured and evaluated according to the following criteria. [Evaluation Criteria] ○:3W / m·K or more △: 1 W / m K or more and less than 3 W / m K ×: Less than 1 W / m K
[0088] 3-3-2.Evaluation of dielectric tangent Test pieces measuring 5 cm×10 cm were cut out from the center of each of Films 1 to 3 and 5 to 8, and the dielectric loss tangents of the films (measurement frequency: 10 GHz) were measured by the SPDR (split post dielectric resonance) method. [Evaluation Criteria] ○: Less than 0.0010 △: 0.0010 or more and 0.0025 or less ×: More than 0.0025
[0089] The above results are summarized in Table 2.
[0090] [Table 2]
[0091] Incidentally, alumina particles were partially exposed on the surface of film 7. It was also confirmed that the adhesiveness of film 3 was improved when the surface of film 3 was corona-treated in a nitrogen gas atmosphere containing vinyl acetate.
[0092] 4. Fabrication of Aluminum-Based Circuit Boards Dispersion 7 was applied to the surface of a copper foil having a thickness of 12 μm by a roll-to-roll gravure reverse method to form a liquid coating. Next, the copper foil on which the liquid coating was formed was passed through a drying oven at 120° C. for 5 minutes and dried by heating. After that, the dried coating was heated at 340° C. for 3 minutes in a far-infrared oven under a nitrogen atmosphere. This produced a laminate in which a polymer layer (thickness: 5 μm) was formed on the surface of the copper foil. Next, the polymer layer of this laminate was placed opposite an aluminum substrate and thermocompression bonded at 300°C to obtain a laminate in which copper foil, polymer layer, and aluminum substrate were laminated in that order. Furthermore, the copper foil of the laminate was etched to form a transmission circuit, obtaining an aluminum-based circuit board. The thermal conductivity of this circuit board was 10 W / m K or higher, and it had excellent heat dissipation properties.
[0093] 5. Preparation of films by spray coating Dispersion 7 was used to coat the surface of an aluminum foil having a thickness of 18 μm by spray coating to form a liquid coating. The aluminum foil on which the liquid coating was formed was then passed through a drying oven at 120° C. for 5 minutes and dried by heating. The process of coating again by spray coating and drying was then repeated four times. The dried coating was then heated at 340° C. for 3 minutes in a far-infrared oven under a nitrogen atmosphere. This resulted in a laminate 9 in which a polymer layer (thickness: 200 μm) was formed on the surface of the aluminum foil. The aluminum foil of laminate 9 was removed by etching to obtain film 9. The thermal conductivity of film 9 was measured in the same manner as in the above-mentioned "3-3-1", and the thermal conductivity of film 9 was evaluated as "good". [Industrial Applicability]
[0094] The dispersion and molded product of the present invention are useful as materials for forming coating layers in antenna parts, printed wiring boards, aircraft parts, automobile parts, power semiconductor parts, heat exchangers, sports equipment, food industry products, saws, packings, gaskets, sliding bearings, etc. The coating layers formed from the dispersion and molded product of the present invention are excellent in chemical resistance, water and oil repellency, heat resistance, electrical properties, etc., and are particularly excellent in adhesion, thermal conductivity (heat dissipation), electrical properties and scratch resistance. The dispersion and molded product of the present invention are particularly suitable as materials for printed wiring boards used in electronic device substrates such as radars, network routers, backplanes, and wireless infrastructures, substrates for various sensors in automobiles, and substrates for engine management sensors, which require heat dissipation and high frequency characteristics. The dispersion and molded product of the present invention are also suitable as materials for forming outer surface coating layers of heat exchangers (fins, heat transfer tubes, etc.) for cold and hot equipment, which require heat dissipation and antifouling properties. In addition, the entire contents of the specifications, claims, drawings and abstracts of Japanese Patent Application No. 2019-095078 filed on May 21, 2019, Japanese Patent Application No. 2019-144674 filed on August 6, 2019, and Japanese Patent Application No. 2019-212480 filed on November 25, 2019 are hereby incorporated by reference as the disclosure of the specification of the present invention.
Claims
1. The powder comprises a tetrafluoroethylene-based polymer having a melting temperature of 200 to 320°C and a thermoplasticity, the average particle size (D50) of which is 1 μm or more and 20 μm or less, a metal oxide filler which is an aluminum oxide or magnesium oxide particle having an average particle size (D50) of 0.02 to 200 μm, a spherical silicon oxide filler which is a silica filler, a talc filler or a steatite filler having an average particle size (D50) of 0.1 to 10 μm, and a polar liquid dispersion medium; The content of the metal oxide filler is 5% by mass or more, the sum of the content of the tetrafluoroethylene-based polymer, the content of the metal oxide filler, and the content of the silicon oxide filler is 20% by mass or more and 80% by mass or less, a mass ratio of the content of the metal oxide filler to the content of the tetrafluoroethylene-based polymer, and a mass ratio of the content of the silicon oxide filler to the content of the tetrafluoroethylene-based polymer, each of which is 0.1 or more and 2 or less.
2. 2. The dispersion according to claim 1, wherein the tetrafluoroethylene-based polymer is at least one polymer selected from the group consisting of a polymer containing units based on tetrafluoroethylene and units based on a monomer having an oxygen-containing polar group, a polymer containing 2 mol % or more of units based on tetrafluoroethylene and units based on perfluoro(propyl vinyl ether), and a polymer containing units based on tetrafluoroethylene and units based on perfluoro(methyl vinyl ether).
3. 3. The dispersion of claim 1 or 2, wherein the metal oxide filler further comprises silicon oxide.
4. The dispersion according to any one of claims 1 to 3, wherein the silicon oxide filler has a hollow structure.
5. 5. The dispersion according to claim 1, wherein the mass ratio of the content of the silicon oxide filler to the content of the metal oxide filler is less than 1.
6. The dispersion according to any one of claims 1 to 5, having a viscosity at 25°C of 10,000 mPa·s or less.
7. The dispersion according to any one of claims 1 to 6, having a thixotropy ratio at 25°C of 1.0 to 2.
5.
8. A method for producing a laminate, comprising applying the dispersion liquid according to any one of claims 1 to 7 to a base layer, heating the base layer to volatilize the liquid dispersion medium, and further heating the base layer to bake the tetrafluoroethylene-based polymer, thereby obtaining a laminate having the base layer and a polymer layer containing the tetrafluoroethylene-based polymer, the metal oxide filler, and the silicon oxide filler.
9. The filler comprises a tetrafluoroethylene-based polymer having a melting temperature of 200 to 320° C. and thermoplasticity, a metal oxide filler which is an aluminum oxide or magnesium oxide particle having an average particle diameter (D50) of 0.02 to 200 μm, and a silicon oxide filler which is a spherical silica filler, a talc filler, or a steatite filler having an average particle diameter (D50) of 0.1 to 10 μm, The content of the tetrafluoroethylene-based polymer is 50% by mass or more, a mass ratio of the content of the metal oxide filler to the content of the tetrafluoroethylene-based polymer, and a mass ratio of the content of the silicon oxide filler to the content of the tetrafluoroethylene-based polymer are each 0.1 or more and 2 or less, and the sum of the content of the metal oxide filler and the content of the silicon oxide filler is 10 mass% or more.
10. The molded article according to claim 9, having a thickness of 1 to 1000 μm.
11. The molded article according to claim 9 or 10, having a thermal conductivity of 1 W / mK or more.
12. The molded article according to any one of claims 9 to 11, having a dielectric loss tangent of 0.005 or less.
Citation Information
Patent Citations
Corrosion-resistant anti-fatigue cable sheath material
CN104098897A
Composition for sliding member
JP1986266451A
Composite dielectric and circuit board
JP1993128912A
Fluorine-based resin-aluminum oxide mixed dispersion and method for producing the same
JP2017110220A
Solid molding of fluorine resin and metal oxide, and method for producing the solid
JP2018059032A