Hydrogen storage alloy for alkaline batteries
A hydrogen storage alloy with a controlled crystal structure and elemental composition addresses durability and discharge capacity issues, enhancing alkaline storage battery performance for diverse applications.
Patent Information
- Application Number
- JP2021142486
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2020-09-23
- Filing Date
- 2021-09-01
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2041-09-01
AI Technical Summary
Existing hydrogen storage alloys for alkaline storage batteries face issues with durability, discharge capacity, and cycle life, particularly due to cracking and corrosion, which hinder their application in high-performance batteries.
A hydrogen storage alloy with a specific crystal structure and composition, characterized by a ratio of diffraction intensities and controlled elemental ratios, including rare earth elements, magnesium, nickel, and additional elements, is developed to enhance durability and discharge capacity.
The alloy achieves high discharge capacity, improved cycle life, and reduced internal resistance, making it suitable for various applications including consumer, industrial, and automotive uses.
Smart Images

Figure 0007572056000004 
Figure 0007572056000005 
Figure 0007572056000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a hydrogen storage alloy for use in an alkaline storage battery. [Background technology]
[0002] Nickel-metal hydride secondary batteries, a typical example of alkaline storage batteries, are characterized by their high capacity compared to nickel-cadmium batteries and the fact that they do not contain any environmentally hazardous substances. For this reason, in recent years, they have come to be widely used in a variety of applications, from mobile phones and personal computers, to power tools, and consumer applications as replacements for alkaline primary batteries, to storage batteries for hybrid electric vehicles (HEVs).
[0003] Conventionally, hydrogen storage alloys with an AB5 crystal structure have been used for the negative electrodes of alkaline storage batteries, but this alloy has limitations in terms of reducing the size and weight of batteries, and there has been a demand for the development of new hydrogen storage alloys that can achieve a small size and high capacity. As a solution to this problem, Patent Documents 1 and 2 propose rare earth-Mg transition metal hydrogen storage alloys that contain Mg.
[0004] In addition, one possible method for reducing the size and weight of the battery is to reduce the amount of hydrogen storage alloy used in the negative electrode, but reducing the amount of hydrogen storage alloy causes a new problem of reduced output due to a decrease in nickel active sites. To solve this problem, Patent Document 3 proposes a method for increasing the operating voltage by using a hydrogen storage alloy with a high hydrogen equilibrium pressure.
[0005] In addition, some rare earth-Mg-Ni based alloys have been proposed as hydrogen storage alloys. For example, in Patent Document 4, a rare earth-Mg-Ni based alloy having the general formula: (La a Ce b Pr c Nd d A e ) 1-x Mg x (Ni 1-y T y ) z(In the formula, A represents at least one element selected from the group consisting of Pm and the like, T represents at least one element selected from the group consisting of V and the like, and a, b, c, d, and e are in the ranges represented by 0 ≦ a ≦ 0.25, 0 ≦ b ≦ 0.2, 0 ≦ c, 0 ≦ d, 0 ≦ e and satisfy the relationship represented by a + b + c + d + e = 1, and x, y, and z are in the ranges represented by 0 < x < 1, 0 ≦ y ≦ 0.5, 2.5 ≦ z ≦ 4.5 respectively) A hydrogen storage alloy having a composition represented by is disclosed.
[0006] Further, Patent Document 5 discloses, as a hydrogen storage alloy that suppresses an increase in the internal pressure of a battery during charging after over-discharge and contributes to an improvement in the cycle life of the battery, a general formula: (La a Pr b Nd c Z d ) 1-w Mg w Ni z-x-y Al x T y (In the formula, the symbol Z represents an element selected from the group consisting of Ce and the like, the symbol T represents an element selected from the group consisting of V and the like, and the subscripts a, b, c, and d are in the ranges represented by 0 ≦ a ≦ 0.25, 0 < b, 0 < c, 0 ≦ d ≦ 0.20 and satisfy a + b + c + d = 1 and the relationship represented by 0.20 ≦ b / c ≦ 0.35, and the subscripts x, y, z, and w are in the ranges represented by 0.15 ≦ x ≦ 0.30, 0 ≦ y ≦ 0.5, 3.3 ≦ z ≦ 3.8, 0.05 ≦ w ≦ 0.15 respectively) A hydrogen storage alloy having a composition represented by is disclosed.
[0007] Patent Document 6 discloses, as a rare earth-Mg-Ni-based hydrogen storage alloy excellent in alkali resistance and inexpensive, a general formula: (Ce a Pr b Nd c Y d A e ) 1-w Mg w Ni x Al y T z(In the formula, A represents at least one element selected from the group consisting of Pm, Sm, etc., T represents at least one element selected from the group consisting of V, Nb, etc., a, b, c, d, e satisfy the relationships a > 0, b ≥ 0, c ≥ 0, d ≥ 0, e ≥ 0, a + b + c + d + e = 1, and w, x, y, z are respectively in the ranges represented by 0.08 ≤ w ≤ 0.13, 3.2 ≤ x + y + z ≤ 4.2, 0.15 ≤ y ≤ 0.25, 0 ≤ z ≤ 0.1), a hydrogen storage alloy having the composition represented thereby is disclosed.
[0008] Furthermore, Patent Document 7 discloses a general formula: Ln 1-x Mg x Ni y A z (In the formula, Ln is at least one element selected from rare earth elements including Y, Ca, Zr, and Ti, A is at least one element selected from Co, Mn, V, Cr, Nb, Al, Ga, Zn, Sn, Cu, Si, P, and B, and the subscripts x, y, and z satisfy the conditions 0.05 ≤ x < 0.25, 0 < z ≤ 1.5, 2.8 ≤ y + z ≤ 4.0). In the hydrogen storage alloy represented thereby, a hydrogen storage alloy is disclosed in which Sm is contained in the above Ln in an amount of 20 mol% or more.
[0009] Furthermore, Patent Document 8 discloses, as a hydrogen storage alloy excellent in alkali resistance, a general formula: (La a Sm b A c ) 1-w Mg w Ni x Al y T z (In the formula, A and T each represent at least one element selected from the group consisting of the group consisting of Pr, Nd, etc. and the group consisting of V, Nb, etc., and the subscripts a, b, c respectively satisfy the relationships a > 0, b > 0, 0.1 > c ≥ 0, a + b + c = 1, and the subscripts w, x, y, z are respectively in the ranges represented by 0.1 < w ≤ 1, 0.05 ≤ y ≤ 0.35, 0 ≤ z ≤ 0.5, 3.2 ≤ x + y + z ≤ 3.8). A hydrogen storage alloy having the composition represented thereby is disclosed.
[0010] In addition, Patent Document 9 describes a hydrogen storage alloy negative electrode for an alkaline storage battery, which is composed of a rare earth metal such as La, and has the general formula (La x Ln y ) 1一z Mg z Ni t-u T u (T: selected from Al, Co, Mn, Zn, Ln: at least one selected from rare earth elements other than La and Y, x>y, 0.09≦z≦0.14, 3.65≦t≦3.80, 0.05≦u≦0.25), and A5B of hexagonal system (2H) 19 A5B type structure and trigonal (3R) system 19 A5B type structure and A2B7 type structure, 2H type 19 The powder X-ray diffraction intensity peak of the Cu-Kα type structure is the A5B of the 3R system. 19 It is disclosed that the present invention uses a larger A2B7 type structure and a larger A2B7 type structure.
[0011] On the other hand, Non-Patent Document 1 describes a hydrogen storage alloy in which La is replaced with Ce, La 0.8-x Ce x Mg 0.2 Ni 3.5 (x=0~0.20) has been reported. The evaluation results of this alloy concluded that x=0.1 is the optimal composition after considering the electrochemical properties comprehensively.
[0012] In addition, Non-Patent Document 2 includes a chapter on the effect of Ce on RE-Mg-Ni hydrogen storage alloys (RE: rare earth elements). (La 0.5 Nd 0.5 ) 0.85 Mg 0.15 Ni 3.3 Al 0.2 (La 0.45 Nd 0.45 Ce 0.1 ) 0.85 Mg 0.15 Ni 3.3 Al 0.2 (La 0.4 Nd 0.4 Ce 0.2 )0.85 Mg 0.15 Ni 3.3 Al 0.2 (La 0.3 Nd 0.3 Ce 0.4 ) 0.85 Mg 0.15 Ni 3.3 Al 0.2 The alloy is disclosed and the results of its evaluation are reported.
[0013] In addition, Non-Patent Document 3 reports the characteristics of La-Sm-Mg-Ni based hydrogen storage alloys. 0.6 Sm 0.15 Mg 0.25 Ni 3.4 The phase constitution and electrochemical properties of the alloys are presented. [Prior art documents] [Patent documents]
[0014] [Patent Document 1] Japanese Patent Application Publication No. 11-323469 [Patent Document 2] WO 01 / 48841 [Patent Document 3] JP 2005-32573 A [Patent Document 4] JP 2005-290473 A [Patent Document 5] JP 2007-169724 A [Patent Document 6] JP 2008-84668 A [Patent Document 7] JP 2009-74164 A [Patent Document 8] JP 2009-108379 A [Patent Document 9] JP 2014-229593 A [Non-patent literature]
[0015] [Non-Patent Document 1] S. Xiangqian et al., Intern. J. Hydrogen Energy, 34, 395(2009) [Non-Patent Document 2] Shigekazu Yasuoka, PhD thesis: Practical application of rare earth-Mg-Ni (superlattice) hydrogen storage alloys and development of high-performance commercial nickel-metal hydride batteries using them (2017, Kyoto University) [Non-Patent Document 3] L. Zhang et al., Intern. J. Hydrogen Energy 41 1791(2016) Summary of the Invention [Problem to be solved by the invention]
[0016] However, in the techniques disclosed in Patent Documents 1 and 2, the alloys were not optimized and the techniques have not been put to practical use in various applications.
[0017] Furthermore, in the technique disclosed in Patent Document 3, when a hydrogen storage alloy with a high hydrogen equilibrium pressure is used, a new problem occurs in that the charge / discharge cycle life is shortened.
[0018] Furthermore, in the technology disclosed in Patent Document 4, the content of La, which is a relatively inexpensive material, is kept low, and as a result, the alloy contains large amounts of expensive Pr, Nd, and Ti, and therefore, it is not possible to provide an inexpensive hydrogen storage alloy that is excellent in durability.
[0019] Furthermore, the technology disclosed in Patent Document 5, like Patent Document 4, requires Pr and Nd as the alloy and contains a small amount of La, so that it is not possible to provide an inexpensive hydrogen storage alloy that is excellent in durability.
[0020] In addition, the technology disclosed in Patent Document 6 does not include La, and although it contains Ce, the alloy contains relatively large amounts of Pr and Nd, so it is not possible to provide an inexpensive hydrogen storage alloy that is excellent in durability.
[0021] Furthermore, the technology disclosed in Patent Document 8 uses an alloy containing a relatively large amount of Sm, which is a cheaper element than Pr and Nd, but does not provide a hydrogen storage alloy that is cheap and has excellent durability.
[0022] In addition, the technology disclosed in Patent Document 8 uses an alloy containing relatively large amounts of La and Sm, which are cheaper elements than Pr and Nd, but does not provide a hydrogen storage alloy that is cheap and has excellent durability. In particular, Zr is essential in the examples, and only a B / A ratio of 3.6 is disclosed. In addition, although it is said that the hydrogen equilibrium pressure, which is reduced by increasing the La content, can be raised to a level that can be used in batteries, setting an inexpensive La-rich composition is often insufficient.
[0023] Furthermore, the technology disclosed in Patent Document 9 is A5B 19 This is an alkaline storage battery that uses a hydrogen storage alloy with a crystal structure as the main phase in the negative electrode, but there are issues regarding the need for further durability, and it is insufficient for the purpose of achieving a highly reliable battery.
[0024] On the other hand, Non-Patent Document 1 shows a rare earth-Mg-Ni alloy in which part of the La is substituted with Ce. In a prototype evaluation of this alloy, it is concluded that an alloy with a Ce substitution amount of x=0.1 is the optimal composition after considering the overall electrochemical properties, but this alloy has not yet been put to practical use.
[0025] Furthermore, Non-Patent Document 2 concludes that it has become clear that rare earth-Mg-Ni alloys containing Ce have a low hydrogen absorption / release capacity and are prone to pulverization when hydrogen absorption / release is repeated, resulting in significant degradation in batteries.
[0026] Furthermore, Non-Patent Document 3 concludes that La 0.60 Sm 0.15 Mg 0.25 Ni 3.4 The electrochemical properties of the alloy are reported, but the cycling characteristics are not satisfactory, decreasing to 80% of the initial capacity after 140 charge / discharge cycles.
[0027] In other words, in rare earth-Mg-Ni hydrogen storage alloys, repeated hydrogen absorption and release causes cracks in the alloy, accelerating pulverization and creating new surfaces. If the alloy has low corrosion resistance, the alloy surface will react to produce rare earth hydroxides, depleting the electrolyte, and ultimately increasing the internal resistance of the battery and decreasing the discharge capacity, shortening the battery life.
[0028] The present invention has been made in consideration of these problems in the prior art, and has an object to provide a hydrogen storage alloy that contributes to the realization of highly durable alkaline storage batteries. [Means for solving the problem]
[0029] In order to achieve the above-mentioned object, the present inventors conducted extensive research into a hydrogen storage alloy for use in the negative electrode of an alkaline storage battery that combines durability, a high battery discharge capacity, low cost, etc. As a result, the present inventors discovered that an alloy containing at least rare earth elements, magnesium, nickel, aluminum, etc. can achieve durability by controlling the diffraction intensity based on a specific crystal structure, and thus developed the present invention.
[0030] That is, the hydrogen storage alloy for alkaline storage batteries according to the present invention is a hydrogen storage alloy whose main phase has an A2B7 type crystal structure, and contains rare earth elements, magnesium, nickel, and at least one selected from aluminum, zinc, tin, and silicon. In an X-ray diffraction measurement using Cu-Kα radiation as an X-ray source, the diffraction line intensity Ia of the (107) plane of the A2B72H structure appearing at 2θ=32.5 to 33.5° is smaller than that of the A5B 19 The ratio Ib / Ia of the diffraction line intensities Ib of the (109) plane of the 2H structure is characterized by being 0.05 or more and 1.0 or less.
[0031] In addition, the hydrogen storage alloy for an alkaline storage battery according to the present invention is preferably represented by the following general formula (1). (La 1-a-b Ce a Sm b )1-c Mg c Ni d M e T f (1) Here, M, T and the subscripts a, b, c, d, e and f in the above formula (1) are M: at least one selected from Al, Zn, Sn, and Si; T: At least one selected from Cr, Mo, and V; 0 <a≦0.10、 0≦b≦0.15, 0 <a+b≦0.16 0.225≦c≦0.32, 0.03≦e≦0.16, 0≦f≦0.03, 3.25≦d+e+f<3.50 Meet the conditions. Effect of the Invention
[0032] The hydrogen storage alloy for alkaline storage batteries of the present invention is excellent in durability and discharge capacity, and a nickel-hydrogen secondary battery using the alloy has a high power density and an excellent charge / discharge cycle life, and therefore has excellent discharge capacity characteristics and can be used in a variety of applications, such as consumer applications, industrial applications, and vehicle applications. [Brief description of the drawings]
[0033] [Figure 1] 1 is a partially cutaway perspective view illustrating an alkaline storage battery using a hydrogen storage alloy according to the present invention. [Diagram 2] 1 is a graph showing an example of the results of X-ray diffraction measurement of a hydrogen storage alloy according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0034] An alkaline storage battery using the hydrogen storage alloy of the present invention will be described with reference to Fig. 1, which is a partially cutaway perspective view showing one example of the battery. The alkaline storage battery 10 is a storage battery in which a group of electrodes consisting of a nickel positive electrode 1 using nickel hydroxide (Ni(OH)2) as the main positive electrode active material, a hydrogen storage alloy negative electrode 2 using the hydrogen storage alloy (MH) of the present invention as the negative electrode active material, and a separator 3 is provided in a housing 4 together with an electrolyte layer (not shown) filled with an alkaline electrolyte.
[0035] This battery 10 corresponds to a so-called nickel-metal hydride battery (Ni-MH battery), and the following reaction occurs.
[0036] Positive electrode: NiOOH+H2O+e - =Ni(OH)2+OH - Negative electrode: MH+OH - =M+H2O+e -
[0037] [Hydrogen storage alloy] The hydrogen storage alloy according to the present invention for use in the negative electrode of an alkaline storage battery will now be described.
[0038] The hydrogen storage alloy of the present invention is a hydrogen storage alloy whose main phase has an A2B7 type crystal structure, and contains rare earth elements, magnesium, nickel, and at least one selected from aluminum, zinc, tin, and silicon. In an X-ray diffraction (XRD) measurement using Cu-Kα radiation as an X-ray source, the diffraction line intensity (Ia) of the (107) plane of the A2B7 type crystal structure (2H type) appearing at 2θ=32.5 to 33.5° is higher than the diffraction line intensity (Ia) of the A5B 19 The ratio (Ib / Ia) of the diffraction intensity (Ib) of the (109) plane of the A2B7 type crystal structure (2H type) to the diffraction intensity (Ia) of the (107) plane of the A5B type crystal structure (2H type) with a hexagonal (2H) crystal structure must be in the range of 0.05 to 1.0. 19If the ratio (Ib / Ia) of the diffraction line intensity (Ib) of the (109) plane of the type crystal structure is less than 0.05 or exceeds 1.0, cracking (pulverization) due to hydrogen absorption and release is promoted, and durability becomes insufficient. Preferably, Ib / Ia is in the range of 0.08 to 0.95.
[0039] The hydrogen storage alloy of the present invention preferably has a component composition represented by the following general formula (1). Note (La 1-a-b Ce a Sm b ) 1-c Mg c Ni d M e T f (1) Here, M, T and the subscripts a, b, c, d, e and f in the above formula (1) are M: at least one selected from Al, Zn, Sn, and Si; T: At least one selected from Cr, Mo, and V; 0 <a≦0.10、 0≦b≦0.15, 0 <a+b≦0.16 0.225≦c≦0.32, 0.03≦e≦0.16, 0≦f≦0.03, 3.25≦d+e+f<3.50 Meet the conditions.
[0040] A2B7 type phase (2H) and A5B 19 When a hydrogen storage alloy having the above-mentioned intensity ratio in X-ray diffraction of the phase (2H) and preferably satisfying the component composition represented by the above general formula (1) is used as the negative electrode of an alkaline storage battery, it imparts high discharge capacity and cycle life characteristics to the battery, thereby contributing to the achievement of smaller, lighter, and more durable alkaline storage batteries.
[0041] The reasons for limiting the composition of the hydrogen storage alloy of the present invention will be explained below. Rare earth element: La 1-a-b Ce a Sm b(However, 0 < a ≤ 0.10, 0 ≤ b ≤ 0.15, 0 < a + b ≤ 0.16) The hydrogen storage alloy of the present invention contains rare earth elements as elements of component A in the main phase of A2B7 type structure, sub-phases of A5B 19 type structure, AB3 type structure, AB2 type structure, and AB5 type structure. As rare earth elements, in principle, two elements, La and Ce, are essential as basic components that provide hydrogen storage capacity. Also, since La and Ce have different atomic radii, the hydrogen equilibrium pressure can be controlled by this component ratio, and the hydrogen equilibrium pressure required for the battery can be arbitrarily set. The atomic ratio a value of Ce in the rare earth elements needs to be in the range exceeding 0 and not exceeding 0.10. When the a value exceeds 0.10, cracking accompanying hydrogen absorption and desorption is promoted, leading to a decrease in cycle life. On the other hand, when the a value is 0, that is, when Ce is not included, it becomes difficult to control the hydrogen equilibrium pressure sufficiently, which has an adverse effect on battery characteristics. Within this range, it is easy to set the hydrogen equilibrium pressure suitable for the battery. Preferably, the atomic ratio a value of Ce is in the range of 0.005 or more and 0.09 or less.
[0042] Sm can be optionally contained as a rare earth element other than La and Ce. Sm, like La and Ce, occupies a rare earth site as an element of component A in the main phase of A2B7 type structure, sub-phases of A5B 19 type structure, AB3 type structure, AB2 type structure, and AB5 type structure, and is a component that provides hydrogen storage capacity similar to these elements. Although Sm has a lower effect of raising the equilibrium pressure compared to Ce, the durability is improved by substituting La together with Ce. The upper limit of the b value representing the atomic ratio of Sm in the rare earth elements is 0.15, and exceeding it will deteriorate the cycle life characteristics in balance with the amount of Ce. Preferably, b ≤ 0.14. Also, the substitution amount of Ce and Sm for La is in the range of 0 < a + b ≤ 0.16. When a + b exceeds 0.16, the suppression of cracking becomes insufficient. Preferably, 0.005 ≤ a + b ≤ 0.15.
[0043] A composition with a high La content has a high discharge capacity, and when combined with other elements, the discharge capacity characteristics are further improved. In addition, the rare earth elements Pr and Nd are not actively used, but they may be included at the unavoidable impurity level.
[0044] Mg:Mg c (where 0.225≦c≦0.32) Mg has an A2B7 structure for the main phase and an A5B structure for the subphase. 19 In the present invention, it is an essential element as the A component element of the AB type structure, AB3 type structure, AB2 type structure, and AB5 type structure, and contributes to improving the discharge capacity and cycle life characteristics. The c value, which represents the atomic ratio of Mg in the A component, is in the range of 0.225 to 0.32. When the c value is less than 0.225, the A2B7 phase and the A5B 19 The X-ray diffraction intensity ratio of the phases cannot be controlled, and as a result, sufficient cycle life characteristics cannot be obtained, and the hydrogen release ability gradually decreases, resulting in a decrease in discharge capacity. On the other hand, if the c value exceeds 0.32, cracking due to hydrogen absorption and release is promoted, and cycle life characteristics, i.e., durability, decrease. The c value is preferably in the range of 0.225 to 0.30.
[0045] Ni:Ni d Ni has an A2B7 structure for the main phase and an A5B structure for the subphase. 19 It is the main element of the B component in the AB structure, AB3 structure, AB2 structure, and AB5 structure. Its atomic ratio d value will be described later.
[0046] M:M e (where 0.03≦e≦0.16) M is at least one selected from Al, Sn, Zn, and Si. The main phase has an A2B7 type structure, and the subphase has an A5B 19It is an element contained as an element of the B component of the AB type structure, AB3 type structure, AB2 type structure, and AB5 type structure. It is effective in adjusting the hydrogen equilibrium pressure related to the battery voltage, and can improve corrosion resistance, and is effective in improving the durability of the fine hydrogen storage alloy, that is, the cycle life characteristics. In order to reliably express the above effect, the e value representing the atomic ratio of M to the A component is set to a range of 0.03 to 0.16. If the e value is less than 0.03, the corrosion resistance becomes insufficient, resulting in an increase in saturation magnetization and an insufficient cycle life. On the other hand, if the e value exceeds 0.16, the discharge capacity decreases. The preferred e value is in the range of 0.035 to 0.15. In addition, it is preferable that Al is present among the M elements, and the atomic ratio of Al is preferably 0.03 or more within the range of e.
[0047] T:T f (where 0≦f≦0.03) T is at least one selected from Cr, Mo, and V, and like M, it has an A2B7 type structure for the main phase and an A5B type structure for the subphase. 19 It is an element contained as an element of the B component of the AB3 type structure, AB2 type structure, and AB5 type structure. It is effective in adjusting the hydrogen equilibrium pressure related to the battery voltage, and the synergistic effect with the M element increases corrosion resistance and improves durability. In particular, it is effective in improving the durability of fine hydrogen storage alloys, that is, cycle life characteristics. In order to reliably exhibit the above effect, the f value, which represents the atomic ratio of T to the A component, is 0.03 or less. If the f value exceeds 0.03, excessive T induces cracks due to the absorption and release of hydrogen, resulting in a decrease in durability and insufficient cycle life. The preferred f value is in the range of 0.025 or less, and it is preferable that the T element, especially Cr, exists within the scope of the invention in which the amount of the M element is particularly small. In addition, a combination of Cr and Mo or V is preferred.
[0048] Ratio of A component to B component: 3.25≦d+e+f<3.50 A2B7 type structure of main phase, A5B type structure of subphase 19The stoichiometric ratio, which is the molar ratio of the B component (Ni, M and T) to the A component having the AB type structure, AB3 type structure, AB2 type structure, or AB5 type structure, i.e., the value of d+e+f represented by the general formula, is preferably in the range of 3.25 to less than 3.50. If it is less than 3.25, the subphase, i.e., the AB2 phase, gradually increases, and in particular the discharge capacity decreases, and the A5B 19 On the other hand, when the temperature is 3.50 or higher, the AB5 phase or A5B phase is not formed, and the cycle life is reduced. 19 If the number of phases increases too much, cracking due to hydrogen absorption and release will be promoted, resulting in a decrease in durability, that is, cycle life.The preferable range is 3.30 or more and 3.49 or less.
[0049] [Method of manufacturing hydrogen storage alloy] Next, a method for producing the hydrogen storage alloy of the present invention will be described. The hydrogen storage alloy of the present invention is prepared by weighing out rare earth elements (Ce, Sm, La, etc.), magnesium (Mg), nickel (Ni), and other elements such as aluminum (Al) and chromium (Cr) to substitute for Ni at a predetermined molar ratio, and then putting these raw materials into an alumina crucible placed in a high-frequency induction furnace and melting them under an inert gas atmosphere such as argon gas, and casting the melt into a mold to prepare an ingot of the hydrogen storage alloy. Alternatively, a flake-shaped sample having a thickness of about 200 to 500 μm may be directly prepared by using a strip casting method.
[0050] In addition, since the hydrogen storage alloy of the present invention contains Mg, which has a low melting point and a high vapor pressure, as a main component, if all the raw materials of the alloy components are melted at once, Mg evaporates, and it may be difficult to obtain an alloy with a target chemical composition. Therefore, when producing the hydrogen storage alloy of the present invention by a melting method, it is preferable to first melt the other alloy components except Mg, and then add Mg raw materials such as metallic Mg and Mg alloys into the molten metal. In addition, this melting process is preferably performed under an inert gas atmosphere such as argon or helium, and specifically, it is preferable to perform the melting process under a reduced pressure or pressurized atmosphere in which an inert gas containing 80 vol% or more of argon gas is adjusted to 0.05 to 0.2 MPa.
[0051] The alloy melted under the above conditions is then preferably cast into a water-cooled mold and solidified to form an ingot of a hydrogen storage alloy. The melting point (T m The hydrogen storage alloy of the present invention is characterized in that the ingot after casting is heated to a temperature above 700° C. in an atmosphere of an inert gas such as argon or helium, or nitrogen gas, or a mixture of these gases, and the melting point (T m ) or less for 3 to 50 hours. This heat treatment produces the A2B7 phase as the main phase and the A5B 19 The hydrogen storage alloy can have at least one or more crystal phases selected from the group consisting of the A2B7 phase, AB3 phase, AB2 phase, and AB5 phase. If the ratio of the A2B7 phase in the hydrogen storage alloy is the largest among the constituent phases, it is the main phase, and it is sufficient if it is at least 40 mass% or more. As is clear from the results of X-ray diffraction measurement (Figure 2), the A2B7 phase is a hexagonal (2H) Ce2Ni7 type, but it may also contain some rhombohedral (3R) Gd2Co7 type. The A5B phase, which is a subphase, 19 GdCo type structure (hexagonal 19 PrCo phase or rhombohedral 19 phase) and AB3 type structure (hexagonal CeNi3 phase or rhombohedral PuNi3 phase), and a small amount of AB2 phase (MgZn2 phase) and AB5 phase (CaCu5 phase) may be present, but since the AB2 phase reduces the discharge capacity and the AB5 phase reduces the cycle life, it is preferable to keep them as small as possible. The crystal structure of the main phase of the obtained hydrogen storage alloy is an A2B7 type structure, which can be confirmed by X-ray diffraction measurement using Cu-Kα radiation and metal structure observation by SEM. It can also be determined from the X-ray diffraction results by Rietveld analysis.
[0052] If the heat treatment temperature is less than 700° C., the diffusion of the elements is insufficient, and subphases remain, which may lead to a decrease in the discharge capacity of the battery and a deterioration in the cycle life characteristics. m -20℃ or higher (T m If the heat treatment temperature is higher than -20°C, the crystal grains of the main phase will become coarse and the Mg component will evaporate, which may result in pulverization and a change in the chemical composition, resulting in a decrease in the amount of hydrogen storage. Therefore, the heat treatment temperature is preferably 750°C to (T m -30°C). More preferably, the range is 770°C to (T m -50℃).
[0053] In addition, if the heat treatment is held for 3 hours or less, the ratio of the main phase may not be stably increased to 40 mass% or more. In addition, the homogenization of the chemical components of the main phase may be insufficient, so that the expansion and contraction during hydrogen absorption and release may become non-uniform, and the amount of distortion and defects may increase, which may adversely affect the cycle life characteristics. The heat treatment is preferably held for 4 hours or more, and from the viewpoint of homogenization of the main phase and improvement of crystallinity, it is more preferable to hold for 5 hours or more. However, if the holding time exceeds 50 hours, the amount of evaporation of Mg increases, which may change the chemical composition, resulting in the formation of an AB5 type subphase. In addition, this is not preferable because it may increase the manufacturing cost and cause a dust explosion due to evaporated Mg fine powder.
[0054] The heat-treated alloy is pulverized by a dry or wet method. When pulverizing by a dry method, for example, a hammer mill or ACM pulverizer is used to pulverize the alloy, which can produce a powder with an average particle size of 20 to 100 μm. On the other hand, when pulverizing by a wet method, a bead mill or an attritor is used to pulverize the alloy. In particular, when obtaining a fine powder with an average particle size of 20 μm or less, wet pulverization is preferable because it can be produced safely. The particle size may be set to an appropriate range depending on the application, for example, D50 = 8 to 100 μm. Here, the average particle size D50 of the alloy particles is a value measured using a laser diffraction / scattering type particle size distribution measuring device, and an example of the measuring device that can be used is the MT3300EXII model manufactured by Microtrack Bell.
[0055] The finely pulverized alloy particles may then be subjected to a surface treatment, such as an alkali treatment using an alkaline aqueous solution of KOH or NaOH, or an acid treatment using an aqueous solution of nitric acid, sulfuric acid, or hydrochloric acid. By performing these surface treatments, a layer made of Ni (alkali-treated layer or acid-treated layer) is formed on at least a part of the surface of the alloy particles, and the progress of alloy corrosion can be suppressed and durability can be increased, thereby improving the cycle life characteristics of the battery and the discharge characteristics over a wide temperature range. In particular, in the case of acid treatment, it is preferable to use hydrochloric acid, since it is possible to precipitate Ni while minimizing damage to the alloy surface. In addition, when the alloy is pulverized by a wet method, the surface treatment can be performed at the same time. EXAMPLES
[0056] The present invention will be described below with reference to examples. Evaluation cells using hydrogen storage alloys No. 1 to 50 having the composition shown in Tables 1-1 to 1-3 below as negative electrode active materials were fabricated as described below, and experiments were conducted to evaluate the characteristics of the evaluation cells. Note that alloys No. 1 to 21 and 34 to 50 shown in Tables 1-1 to 1-3 are alloy examples (invention examples) that meet the conditions of the present invention, and No. 22 to 33 are alloy examples (comparative examples) that do not meet the conditions of the present invention. Furthermore, alloy No. 22 of the comparative example was used as a reference alloy for evaluating the characteristics of the cells.
[0057] (Preparation of negative electrode active material) The raw materials of alloys No. 1 to 50 shown in Tables 1-1 to 1-3 (Sm, La, Ce, Mg, Ni, Al, Cr, Zn, Sn, Si, V and Mo each have a purity of 99% or more) were melted in an argon atmosphere (Ar: 100 vol%, 0.1 MPa) using a high-frequency induction heating furnace and cast into ingots. Next, these alloy ingots were heated to 3000° C. in an argon atmosphere (Ar: 90 vol%, 0.1 MPa) until the melting point T m After heat treatment at -50°C (940 to 1130°C) for 10 hours, the mixture was coarsely crushed and then finely crushed with a hammer mill to a mass-based D50 of 25 μm to prepare a sample (negative electrode active material) for cell evaluation.
[0058] X-ray diffraction (XRD) measurements were performed on these alloys using Cu-Kα radiation as an X-ray source, and the diffraction intensity of the (107) plane of the A2B72H structure was compared with that of the A5B 19 The ratio Ib / Ia of the diffraction line intensity Ib of the (109) plane of the 2H structure was determined and listed in Tables 1-1 to 1-3. The XRD measurement conditions were a scan speed of 0.5° / min, a tube voltage of 40 kV, a tube current of 40 mA, and a scan step of 0.02°. An example of the XRD measurement results is shown in Figure 2. In Figure 2, A is the 2θ diffraction line of the (107) plane of the A2B7 phase (2H type), and B is the A5B 19 The diffraction lines are from the (109) plane of the CaCu5 phase (2H type). Note that No. 22 has a CaCu5 type crystal structure, and these cannot be evaluated.
[0059] (Preparation of evaluation cells) <Negative electrode> The negative electrode active material prepared above, Ni powder as a conductive additive, and two types of binders (styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC)) were mixed in a weight ratio of negative electrode active material:Ni powder:SBR:CMC=95.5:3.0:1.0:0.5, and kneaded to form a paste-like composition. This paste-like composition was applied to a punching metal, dried at 80℃, and then roll-pressed with a load of 15kN to obtain a negative electrode.
[0060] <Positive electrode> Nickel hydroxide (Ni(OH)2), metallic cobalt (Co) as a conductive additive, and two types of binders (styrene-butadiene rubber (SBR) and carboxymethyl cellulose (CMC)) were mixed in a mass ratio of Ni(OH)2:Co:SBR:CMC=95.5:2.0:2.0:0.5 and kneaded to form a paste-like composition. This paste-like composition was applied to porous nickel, dried at 80℃, and then roll-pressed with a load of 15kN to obtain a positive electrode.
[0061] <Electrolyte> The electrolyte used was an alkaline aqueous solution prepared by mixing pure water with potassium hydroxide (KOH) to give a concentration of 6 mol / L.
[0062] <Evaluation cell> The positive electrode was placed as a counter electrode and the negative electrode was placed as a working electrode in an acrylic case, and the electrolyte was poured into the cell to prepare a cell using a Hg / HgO electrode as a reference electrode, which was then used for an evaluation test. The capacity ratio of the working electrode to the counter electrode was adjusted to working electrode:counter electrode=1:3. A polyethylene nonwoven fabric was placed between the positive electrode and the negative electrode as a separator.
[0063] (Cell Characterization) The evaluation tests of the evaluation cells for the alloys Nos. 1 to 50 obtained as described above were carried out as follows.
[0064] (1) Discharge capacity of the electrode The discharge capacity of the working electrode was confirmed using the following procedure. After constant current charging at a current value of 80 mA / g per active material of the working electrode for 10 hours, constant current discharging was performed at a current value of 40 mA / g per active material of the working electrode. The discharge termination condition was a working electrode potential of -0.5 V. The above charge / discharge was repeated 10 times, and the maximum discharge capacity was taken as the discharge capacity of the working electrode. It was confirmed that the discharge capacity of the working electrode was saturated and stabilized after 10 charge / discharge cycles. The evaluation temperature was 25°C. The measured discharge capacity was calculated by the following formula (2) using the discharge capacity of alloy No. 22 shown in Table 1-2 as the reference capacity, and the ratio to this was calculated. Those with a ratio of more than 1.15 were evaluated as having a larger discharge capacity than alloy No. 22 and being superior. The evaluation temperature was 25°C. Discharge capacity = (discharge capacity of evaluated alloy) / (discharge capacity of alloy No. 22) (2)
[0065] (2) Cycle life characteristics Using the cells in which the discharge capacity of the working electrode was confirmed in the above (1) Discharge capacity of the electrode, the cycle life characteristics of the working electrode were determined by the following procedure. The evaluation temperature was 45°C. When the current value required to complete charging or discharging the discharge capacity of the working electrode confirmed in (1) Discharge capacity of electrode in 1 hour was defined as 1C, constant current charging and constant current discharging were performed at a current value of C / 2 within a range of 30-70% charge rate of the working electrode, and this cycle was repeated 300 times. The discharge capacity after 300 cycles was measured, and the capacity retention rate was calculated by the following formula (3). Capacity retention rate = (discharge capacity at 300th cycle) / (discharge capacity at 1st cycle) (3) In the evaluation of the cycle life characteristics, the capacity retention rate after 300 cycles of Alloy No. 22 shown in Table 1-2 was set as the reference capacity retention rate, and the ratio to this was calculated using the following formula (4). Alloys with a ratio of more than 1.20 were evaluated as having greater cycle life characteristics than Alloy No. 22 and being superior. Cycle life characteristic = (Capacity retention rate of test alloy after 300 cycles) / (Capacity retention rate of alloy No. 22 after 300 cycles) (4)
[0066] (3) Cost The alloy cost was calculated from the unit price per mass of each raw material and the mass ratio of the alloys with the composition shown in Tables 1-1 to 1-3. It was then evaluated relative to the standard alloy No. 22. In the cost evaluation shown in Tables 1-1 to 1-3, 1 or less (cheaper than the standard alloy) was ◯, the same to less than 1.2 times was △, and 1.2 times or more was ×.
[0067] As is clear from Tables 1-1 to 1-3, the alloys No. 1 to 21 and 34 to 50 of the invention examples have better characteristics of various parameters than the alloy No. 22, and as a result, the evaluation values of the discharge capacity and cycle life characteristics are improved in a well-balanced manner in the battery evaluation. Specifically, the discharge capacity is 1.15 times or more than the reference alloy (No. 22), and the cycle life characteristics are 1.20 times or more. In contrast, it is found that the evaluation values of any of the electrode characteristics of the alloys No. 23 to 33 of the comparative examples do not satisfy the above criteria. In terms of cost, the alloys of the present invention are also kept low.
[0068] [Table 1-1]
[0069] [Table 1-2]
[0070] [Table 1-3] [Industrial Applicability]
[0071] The hydrogen storage alloy of the present invention is superior to the conventionally used AB5-type hydrogen storage alloys in both discharge capacity and cycle life characteristics, and is therefore suitable as an alloy for the negative electrodes of a wide range of alkaline storage batteries, from consumer applications as a replacement for alkaline primary batteries to various industrial and automotive applications. [Explanation of symbols]
[0072] 1: Positive electrode 2: Negative electrode 3: Separator 4: Housing (battery case) 10: Alkaline storage battery
Claims
[Claim 1] A 2 B 7 Phase and A 5 B 19 phase and, optionally, AB 3 Phase, AB 2 Phase and AB 5 and at least one selected from the group consisting of, by mass, A 2 B 7 A hydrogen storage alloy having a crystal structure in which the Fe phase accounts for the largest proportion of the constituent phases, The hydrogen storage alloy is represented by the following general formula (1): In X-ray diffraction measurement using Cu-Kα radiation as an X-ray source, A 2 B 7 A appearing at 2θ = 31.5 to 32.5° for the diffraction line intensity Ia of the (107) plane of the 2H structure 5 B 19 A hydrogen storage alloy for alkaline storage batteries, characterized in that the ratio Ib / Ia of the diffraction line intensities Ib of the (109) plane of the 2H structure is 0.05 or more and 1.0 or less. (La 1-a-b Ce a Sm b ) 1-c Mg c Ni d M e T f ... (1) Here, M, T and the subscripts a, b, c, d, e and f in the above formula (1) are M: Al, or Al and at least one selected from Zn, Sn, and Si; T: at least one selected from Cr, Mo, and V; 0<a≦0.10, 0≦b≦0.15, 0<a+b≦0.16 0.225≦c≦0.32, 0.03≦e≦0.16, 0≦f≦0.03, 3.25≦d+e+f<3.50 Meet the conditions.
Citation Information
Patent Citations
Hydrogen storage alloy and secondary battery
JP1999323469A
Hydrogen storage alloy powder for sealed alkaline storage battery and sealed alkaline storage battery using it
JP2005032573A
Hydrogen occlusion alloy, hydrogen occlusion alloy particle and secondary battery
JP2005290473A
Hydrogen occlusion alloy and alkaline secondary battery using the hydrogen occlusion alloy
JP2007169724A
Hydrogen storage alloy and sealed alkaline storage battery using the same
JP2008084668A