Composite material containing silicon and graphite and method for producing same
A silicon/graphite composite with a carbon matrix and graphene coating addresses expansion and conductivity issues, offering improved performance and scalability for lithium ion batteries.
Patent Information
- Application Number
- JP2021577961
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-06-26
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-06-26
AI Technical Summary
Existing silicon/graphite composites for lithium ion batteries face challenges such as high expansion, insufficient cycle life, and irreversible capacity loss due to unstable solid electrolyte interface (SEI) formation and poor electronic conductivity, with current methods being costly, difficult to scale, or providing inadequate performance.
A composite material comprising silicon nanoparticles coated with graphite particles, few-layer graphene, and a carbon matrix, optionally with an amorphous carbon outer layer and additional oxides, is produced through a process involving size reduction, mixing, spray drying, and heat treatment to enhance stability and conductivity.
The composite material exhibits improved capacity, reduced expansion, and extended cycle life, with enhanced electrical conductivity and stability, making it suitable for commercial applications.
Smart Images

Figure 0007572064000003 
Figure 0007572064000004 
Figure 0007572064000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a composite material comprising silicon and graphite. More particularly, the composite material of the present invention is intended for use as an anode material in lithium-ion batteries.
[0002] In one highly preferred form, the present invention further relates to an anode composite comprising a composite material comprising silicon and graphite.
[0003] The present invention further relates to a method for producing a composite material comprising silicon and graphite. [Background technology]
[0004] It is now understood that silicon / graphite composites have some potential as lithium ion anode materials. However, many drawbacks associated with silicon / graphite composites are well known and understood. These drawbacks include high levels of expansion, up to 400%, and poor cycle life. Commercial applications of silicon / graphite composites must address at least these challenges.
[0005] The irreversible capacity loss of silicon-containing anodes as currently known and understood is currently being addressed by using nanostructured silicon particles as the electroactive material. Silicon nanoparticles and nanostructured silicon have been reported to be more resistant to volume changes during charging and discharging when compared to microscale particles (Non-Patent Document 1). However, nanoscale particles are known to be difficult to prepare and handle, and therefore are considered unsuitable for commercial-scale applications. In addition to challenges related to the size of silicon particles, the nature of the silicon surface also plays an important role in the formation of the solid electrode interface (SEI) and electronic conductivity. Since the SEI on the surface of silicon is not stable and will continually consume lithium, it is necessary to modify the surface to avoid or at least reduce the exposure of silicon to the electrolyte. Furthermore, silicon is not considered a particularly good conductive material.
[0006] Core-shell structured graphite / silicon@pyrolytic carbon (Gr / Si@C) composites have been fabricated using mechanical grinding, spray drying, and pitch (Non-Patent Document 2). This prior art process shows what is believed to be a relatively scalable and cost-effective method. Due to the presence of silicon and carbon coating of graphite, the cycling performance is much improved compared to many prior art techniques. However, the low first cycle efficiency of 77.9% with a capacity of 637.7mAh / g is far from the level required by the battery industry.
[0007] US Patent No. 5,399,363 first describes the production of silicon nanoparticles by ball milling of silicon particulates in a solvent. A pyrolytic "amorphous" carbon precursor containing at least one oxygen or nitrogen atom is added to the silicon nanoparticles and solvent, the solvent is removed, and the remaining silicon nanoparticles are coated with a thick layer of pyrolytic carbon precursor. These coated silicon nanoparticles are then pyrolyzed to form composite particles containing multiple silicon nanoparticles dispersed in a conductive pyrolytic carbon matrix. Since this prior art process uses a large amount of amorphous carbon, significant first cycle loss (FCL) and expansion remain a major issue. The amorphous carbon is believed to contribute to a large portion of the unacceptable FCL and expansion experienced. Furthermore, as the Si@C expands, the amorphous carbon is not elastic, weakening the silicon-carbon bond.
[0008] By electroless plating of a thick layer of nickel onto micron-sized silicon, graphene-caged silicon structures were formed, and excellent battery performance such as high capacity, low expansion, long cycle life, and low FCL was achieved (Non-Patent Document 3).
[0009] Silicon nanoparticles coated with few-layer graphene have also been described as being formed by chemical vapor deposition (CVD) (Non-Patent Document 4). Again, these coated silicon nanoparticles are said to provide superior battery performance, such as high capacity, low expansion, long cycle life, and low FCL. However, the process of forming these graphene-coated materials is known to be expensive and not scalable, especially to the levels required for commercial applications.
[0010] A more cost-effective method of coating few-layer graphene on silicon is described in US Pat. No. 5,399,633, which involves coating silicon with graphene by bead milling of a mixture of graphite and silicon. However, the use of this method does not produce a product with the required performance, e.g., there is a significant capacity loss (>45%) in the first 200 cycles.
[0011] US Patent No. 5,399,633 describes the manufacture of a carbon-silicon composite by preparing a silicon-carbon-polymer matrix, followed by heat treatment to carbonize the matrix. The carbonized matrix is ground and mixed with a carbon feedstock, followed by carbonization to produce the carbon-silicon composite of the invention. The carbon-silicon composite is used as an anode slurry to provide an anode for a secondary battery.
[0012] US Patent No. 5,399,633 describes the preparation of a negative active material comprising forming silicon-carbon primary particles having an apparent density of about 2 grams per cubic centimeter or greater, and heat treating a plurality of the primary particles, a second carbonaceous material, and a foaming agent to form porous silicon-carbon secondary particles, which may or may not be provided with an additional coating layer.
[0013] The composite materials and methods of the present invention have as one object to substantially overcome one or more of the above-mentioned problems associated with prior art processes, or at least to provide a useful alternative thereto.
[0014] The foregoing discussion of the background art is intended only to facilitate an understanding of the present invention. This discussion is not an admission or acknowledgement that any material referred to is or was part of the common general knowledge at the priority date of this application.
[0015] Throughout this specification, unless the context clearly indicates otherwise, the term "comprise" or variations such as "comprises" or "comprising" are understood to mean the inclusion of a specified integer or group of integers and not the exclusion of other integers or groups of integers.
[0016] Throughout this specification and claims, unless the context indicates otherwise, the term "ball mill" is understood to include the term "bead mill" and the term "bead mill" is understood to include the term "ball mill." Similarly, unless the context indicates otherwise, the term "ball mill" and / or the term "bead mill" is understood to include the term "grinding" and the term "grinding" is understood to include the term "bead mill" and / or the term "ball mill," depending on the context.
[0017] Throughout this specification and claims, unless the context indicates otherwise, the term "mechanofusion" is taken to mean mixing by inducing a mechanochemical reaction between multiple particles to produce new particles with new properties. Similarly, the term "mixing" is understood to include the term mechanofusion. Summary of the Invention
[0018] According to the present invention, Coated with graphite particles A plurality of silicon nanoparticles; Few-layer graphene particles, graphite nanoparticles, Carbon matrix, and Amorphous Carbon an outer shell; Coated with graphite particles Silicon nanoparticles and the few-layer graphene particles; The graphite Nano Particles and each A composite material is provided that includes silicon and graphite held within the carbon matrix.
[0019] Preferably, the carbon matrix is provided in the form of an amorphous carbon matrix, a crystalline carbon matrix, or a combination of both an amorphous carbon matrix and a crystalline carbon matrix.
[0020] G The graphite particles are preferably in the form of graphene-like nanosheets. 。
[0021] In one form, a further outer layer of amorphous carbon is provided around the plurality of silicon nanoparticles, graphite particles, and carbon matrix, but within the shell.
[0022] The amorphous carbon outer layer may further comprise one or more oxides, preferably present in the form of Al2O3, TiO2, ZrO2, BaTiO3, MgO, CuO, ZnO, Fe2O3, GeO2, Li2O, MnO, NiO, or zeolites, or any combination thereof.
[0023] Preferably, the oxide has a particle size of about 20 nm to 1 micron.
[0024] Preferably, the composite material has a level of elasticity imparted by the presence of one or more of graphite particles, graphene, few layer graphene, and graphite nanoparticles, which may be disposed within an amorphous carbon matrix.
[0025] The present invention further provides an anode composite comprising the composite material described above.
[0026] According to the present invention there is further provided a method for the production of a composite material, said method comprising the steps of: (i) Silicon particles in a solvent , optionally subjecting the graphite particles to a size reduction step in the presence of a polymer; With graphite particles Coated Silicon Nanoparticles , few-layer graphene particles, and graphite nanoparticles and producing (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii), Multiple graphite particle coated Silicon nanoparticles, Few-layer graphene particles, graphite nanoparticles and a carbon matrix, Each of the particles and forming a composite material in which the carbon matrix is supported by the carbon nanotube. (iv) the compound of step (iii) material coating the binder; (v) the compound of step (iv) material and heat treating the resulting mixture to produce a shell comprising amorphous carbon.
[0027] Preferably, the shell further comprises one or more oxides, more preferably provided in the form of Al2O3, TiO2, ZrO2, BaTiO3, MgO, CuO, ZnO, Fe2O3, GeO2, Li2O, MnO, NiO, or a zeolite, or any combination thereof.
[0028] In one form of the invention, the method further comprises an initial step in which the silicon material is subjected to a size reduction process in a solvent to produce silicon nanoparticles in step (i).
[0029] Preferably, the first step silicon material is provided in the form of micron-scale silicon particles.
[0030] In one aspect of the invention, the size reduction step of step (i) provides silicon nanoparticles having a size of about 20-200 nm.
[0031] More preferably, the initial step and the size reduction step of step (i) are each milling steps.More preferably, the milling steps are carried out in one or more bead mills.
[0032] In one aspect of the invention, the solvent is provided in the form of a non-aqueous solvent, preferably in the form of isopropyl alcohol.
[0033] In one form of the invention, the polymer is selected from the group of polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), and poly(methyl methacrylate) (PMMA).
[0034] The treatment of step (ii) may in one aspect of the invention be provided in the form of spray drying, preferably in the presence of a binder.
[0035] The treatment of step (ii) may in a further aspect of the invention be provided in the form of a mixing step, which preferably includes a hybridization process, whereby the secondary particles or products produced are spheroidized.
[0036] Preferably, the heat treatment of steps (iii) and (v) is provided in the form of pyrolysis.
[0037] More preferably, the heat treatments of steps (iii) and (v) convert any binder present to amorphous carbon.
[0038] The temperature of the heat treatment in step (iii) is preferably lower than the temperature in step (v).
[0039] After the heat treatment of step (iii), the surface area (BET) of the composite material is preferably about 70 to 120 m 2 After the heat treatment in step (v), the BET of the material is preferably about 10 to 30 m 2 / g.
[0040] Preferably, the graphite particles for milling step (i) are provided in the form of pre-exfoliated graphite particles.
[0041] In one form of the invention, the milling process of step (i) produces graphene attached to the silicon nanoparticles.
[0042] The heat treatment in step (iii) is preferably carried out at a temperature of about 500°C to 700°C.
[0043] More preferably, the heat treatment in step (v) is carried out at a temperature of about 750°C to 1100°C.
[0044] More preferably, the heat treatment in step (v) is carried out at a temperature of about 850°C to 1000°C.
[0045] According to the present invention there is further provided a method for the production of a composite material, said method comprising the steps of: (i) subjecting silicon particles to a size reduction process together with graphite particles in a solvent and / or in the presence of a polymer to produce coated silicon nanoparticles; (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii) to produce a composite material comprising a plurality of coated silicon nanoparticles, graphite particles, and a carbon matrix, the graphite particles being held within the carbon matrix; (iv) coating the composite of step (iii) with a binder; (v) heat treating the composite of step (iv) to convert the binder and produce a shell comprising amorphous carbon.
[0046] Preferably, the treating in step (ii) is carried out by spray drying or mechanofusion.
[0047] According to the present invention there is further provided a method for the manufacture of an anode composite, said method comprising the steps of: (i) subjecting silicon particles to a size reduction process together with graphite particles in a solvent and / or in the presence of a polymer to produce coated silicon nanoparticles; (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii) to produce an anode composite comprising a plurality of coated silicon nanoparticles, graphite particles, and a carbon matrix, the graphite particles being held within the carbon matrix; (iv) coating the composite of step (iii) with a binder; (v) heat treating the composite of step (iv) to convert the binder and produce a shell comprising amorphous carbon.
[0048] In one form of the invention, the method further comprises an initial step in which the silicon material is subjected to a size reduction process in a solvent to produce the silicon particles of step (i).
[0049] Preferably, the first step silicon material is provided in the form of micron-scale silicon particles.
[0050] More preferably, the initial step and the size reduction step of step (i) are each milling steps.More preferably, the milling steps are carried out in one or more bead mills.
[0051] In one aspect of the invention, the solvent is provided in the form of a non-aqueous solvent, preferably in the form of isopropyl alcohol.
[0052] In one form of the invention, the polymer is selected from the group of polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), and poly(methyl methacrylate) (PMMA).
[0053] The treatment of step (ii) may in one aspect of the invention be provided in the form of spray drying, preferably in the presence of a binder.
[0054] The treatment of step (ii) may in a further aspect of the invention be provided in the form of a mechanofusion or mixing step, which preferably comprises a hybridization process, whereby the secondary particles or products produced are spheronized.
[0055] Preferably, the heat treatment in step (iii) is provided in the form of pyrolysis.
[0056] More preferably, the heat treatment in step (iii) converts any binder present to amorphous carbon.
[0057] Preferably, the graphite particles for milling step (i) are provided in the form of pre-exfoliated graphite particles.
[0058] In one form of the invention, the milling process of step (i) produces graphene attached to the silicon nanoparticles.
[0059] The heat treatment in step (iii) is preferably carried out at a temperature of about 500°C to 700°C.
[0060] More preferably, the heat treatment in step (v) is carried out at a temperature of about 750°C to 1100°C.
[0061] More preferably, the heat treatment in step (v) is carried out at a temperature of about 850°C to 1000°C. The invention will now be described, by way of example only, with reference to two embodiments thereof and the accompanying drawings, in which: [Brief description of the drawings]
[0062] [Figure 1] FIG. 1 is a schematic diagram of a process for the manufacture of a composite material according to the present invention. [Diagram 2] FIG. 2 is a scanning electron micrograph (SEM) of Applicant's graphite material, showing flake graphite mixed with few-layer graphene (FLG). [Diagram 3] FIG. 3 is a scanning electron micrograph (SEM) of Applicant's bead milled exfoliated graphite (10% exfoliated graphite in IPA with 168 minutes of bead milling). [Figure 4] FIG. 4 shows some scanning electron microscope (SEM) images of the composite materials of the invention, where * indicates thin flakes of graphite and ** indicates few layer graphene. [Diagram 5] FIG. 5 shows the results of half-cell testing of the composite of the present invention, where different amounts of the composite are cycled under the following conditions - lithiation: 1st cycle: 0.1C~5mV, then hold at 5mV until 0.01C, other cycles: 0.2C~5mV, then hold at 5mV until 0.25C; delithiation: 1st cycle: 0.1C~1.0V, other cycles: 0.2C~1.0V, the silicon content of the composite is 30~50%Wt. [Figure 6] Figure 6 shows the results of the calendering effect test of the Si@C and Gr@Si@C1@C2 anode composites, respectively. [Figure 7]FIG. 7 shows the results of full cell testing of the composite material of the present invention. [Figure 8a] FIG. 8a shows the cycling and capacity retention results of the full cell test of the composite material, with 97% capacity retention after 140 cycles at 0.5C. [Figure 8b] FIG. 8b shows the cycling and capacity retention results of the full cell test of the composite material, with 97% capacity retention after 140 cycles at 0.5C.
[0063] Best Mode for Carrying Out the Invention The present invention provides a composite material comprising silicon and graphite, comprising a plurality of silicon nanoparticles, graphite particles, a carbon matrix, and an outer shell, the silicon nanoparticles and the graphite particles being held within the carbon matrix, the carbon matrix being provided in the form of an amorphous carbon matrix, a crystalline carbon matrix, or a combination of both the amorphous and crystalline carbon matrices.
[0064] The silicon nanoparticles can be coated with graphite particles. The graphite particles can be provided in the form of graphene-like nanosheets. The composite can further include a plurality of few-layer graphene particles. The composite can further include graphite particles larger than the nanoparticle scale. The composite has a level of elasticity imparted by the presence of one or more of graphite particles, graphene, few-layer graphene, and graphite nanoparticles (GNPs) disposed within an amorphous carbon matrix.
[0065] In one form, a further outer layer of amorphous carbon is provided around the plurality of silicon nanoparticles, graphite particles, and carbon matrix, but within the shell.
[0066] The amorphous carbon outer layer may further comprise one or more oxides, preferably in the form of Al2O3, TiO2, ZrO2, BaTiO3, MgO, CuO, ZnO, Fe2O3, GeO2, Li2O, MnO, NiO, or zeolites, or any combination thereof. The oxides have a particle size of about 20 nm to 1 micron.
[0067] The present invention further provides an anode composite comprising a composite material in one of the forms described above and / or below.
[0068] The present invention further provides a method for the production of a composite material, said method comprising the steps of: (i) subjecting silicon particles to a size reduction process together with graphite particles in a solvent and / or in the presence of a polymer to produce coated silicon nanoparticles; (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii) to produce a composite material comprising a plurality of coated silicon nanoparticles, graphite particles, and a carbon matrix, the graphite particles being held within the carbon matrix; (iv) coating the composite of step (iii) with a binder; (v) heat treating the composite of step (iv) to produce a shell comprising amorphous carbon.
[0069] The shell further comprises one or more oxides, for example, provided in the form of Al2O3, TiO2, ZrO2, BaTiO3, MgO, CuO, ZnO, Fe2O3, GeO2, Li2O, MnO, NiO, or a zeolite, or any combination thereof.
[0070] In one form of the invention, the method further comprises an initial step in which the silicon material is subjected to a size reduction process in a solvent to produce silicon nanoparticles in step (i).
[0071] The silicon material of the first step is provided in the form of micron-scale silicon particles. The first step and the size reduction step of step (i) are each milling steps. More preferably, the milling steps are carried out in one or more bead mills.
[0072] The solvent is provided in the form of a non-aqueous solvent. One suitable non-aqueous solvent is isopropyl alcohol (IPA).
[0073] When a polymer is present, it is for example selected from the group of polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), and poly(methyl methacrylate) (PMMA). The polymer is present at 1-40% wt / wt and the silicon particles are present at 1-80% wt / wt. In one preferred form of the invention, the polymer is present at 5% wt / wt and the silicon particles are present at 10% wt / wt.
[0074] The treatment of step (ii) can be provided in the form of a spray drying, preferably in the presence of a binder, or in the form of a mixing or mechanofusion step. The mixing step includes a hybridization process, which results in spheronization of the secondary particles or products produced.
[0075] The heat treatment of step (iii) is provided in the form of pyrolysis, which converts the binder present into amorphous carbon.
[0076] The graphite particles for the size reduction step (i) are provided in the form of pre-exfoliated graphite particles, and the size reduction step produces graphene that is attached to the silicon nanoparticles.
[0077] The heat treatment in step (iii) is preferably carried out at a temperature of about 500° C. to 700° C. The heat treatment in step (v) is carried out at a temperature of about 750° C. to 1100° C., or in one preferred embodiment at a temperature of about 850° C. to 1000° C.
[0078] The present invention further provides a method for the production of a composite material, said method comprising the steps of: (i) subjecting silicon particles to a size reduction process together with graphite particles in a solvent and / or in the presence of a polymer to produce coated silicon nanoparticles; (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii) to produce a composite material comprising a plurality of coated silicon nanoparticles, graphite particles, and a carbon matrix, the graphite particles being held within the carbon matrix; (iv) coating the composite of step (iii) with a binder; (v) heat treating the composite of step (iv) to convert the binder and produce a shell comprising amorphous carbon.
[0079] The present invention further provides a method for the manufacture of an anode composite, the method comprising the steps of: (i) subjecting silicon particles to a size reduction process together with graphite particles in a solvent and / or in the presence of a polymer to produce coated silicon nanoparticles; (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii) to produce an anode composite comprising a plurality of coated silicon nanoparticles, graphite particles, and a carbon matrix, the graphite particles being held within the carbon matrix; (iv) coating the composite of step (iii) with a binder; (v) heat treating the composite of step (iv) to convert the binder and produce a shell comprising amorphous carbon.
[0080] In one form of the invention, the method further comprises an initial step in which a silicon material is subjected to a size reduction process in a solvent to produce silicon nanoparticles of step (i), the silicon material of the initial step being provided in the form of micron-scale silicon particles.
[0081] The initial step and the size reduction step of step (i) are each milling steps, which are carried out in one or more bead mills.
[0082] In one aspect of the invention, the solvent is provided in the form of a non-aqueous solvent. The solvent may be provided in the form of isopropyl alcohol.
[0083] When present, the polymer is for example selected from the group of polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), and poly(methyl methacrylate) (PMMA). The polymer is present at 1-40% wt / wt and the silicon particles are present at 1-80% wt / wt. In one preferred form of the invention, the polymer is present at 5% wt / wt and the silicon particles are present at 10% wt / wt.
[0084] The treatment of step (ii) can be provided in the form of spray drying, preferably in the presence of a binder. Alternatively, the treatment of step (ii) can be provided in the form of mixing. The mixing step includes a hybridization process, which results in spheronization of the product.
[0085] The heat treatment of step (iii) is provided in the form of pyrolysis, which converts the binder present into amorphous carbon.
[0086] The graphite particles for milling step (i) are provided in the form of pre-exfoliated graphite particles.
[0087] In one form of the invention, the milling process of step (i) produces graphene attached to the silicon nanoparticles.
[0088] The heat treatment in step (iii) is preferably carried out at a temperature of about 500° C. to 700° C. The heat treatment in step (v) is carried out at a temperature of about 750° C. to 1100° C., or in one preferred embodiment at a temperature of about 850° C. to 1000° C.
[0089] FIG. 1 shows a process 10 according to a first embodiment of the present invention, which is aimed at producing a final composite material 42. The process 10 includes an initial silicon material size reduction step, e.g., milling step 14, which produces silicon nanoparticles 16, and another size reduction step, e.g., milling step 18, in which the silicon nanoparticles are milled in a solvent with graphite particles 20 to produce graphite nanoparticles 22, few-layer graphene 24, and graphene-coated silicon nanoparticles 26, respectively. The solvent is a non-aqueous solvent, e.g., isopropyl alcohol. The milling steps 14 and 18 can be conveniently carried out in one or more ceramic bead mills, utilizing beads of 500 micron size.
[0090] The silicon nanoparticles may be provided, for example, at about 80 nm to 150 nm. The graphite particles 20 may be provided at a size of less than about 30 microns. In one form of the invention, the graphite particles are provided in the form of pre-exfoliated graphite.
[0091] The process 10 further includes a processing step 28, such as a spray drying or mechanofusion step, in which the product of the milling step 18 is spray dried or mechanofused with the addition of a binder 30 to produce secondary particles or composites 32. The binder 30 can be provided in the form of a pitch. Alternatively, another organic carbon source can constitute the binder 30. The composites 32 produced by the processing step 28 are, for example, 1 to 40 microns in size.
[0092] The process 10 further includes a heat treatment step, such as pyrolysis 34, of the composite 32, which converts the binder 30 to amorphous carbon to form the first intermediate composite material 12. Pyrolysis 34 is performed at a temperature of about 500°C to 700°C.
[0093] A further coating is applied to the first intermediate composite material 12 using a binder 36, e.g., an organic source, to form a second intermediate composite material 38. In one form, the binder 36 is provided in the form of a pitch. The binder 36, in some forms, can include one or a mixture of oxide materials. The oxide material can be, for example, Al2O3, TiO2, ZrO2, BaTiO3, MgO, CuO, ZnO, Fe2O3, GeO2, Li2O, MnO, NiO, or a zeolite, or any combination thereof.
[0094] The process 10 further includes a further heat treatment step, e.g., a pyrolysis step 40, in which the second intermediate composite 38 is pyrolyzed and the binder 36 is converted to amorphous carbon to form a composite material 42. The pyrolysis step 40 is carried out at a temperature between 750°C and 1100°C, e.g., between 800°C and 1000°C.
[0095] Due to the presence of graphene, FLGs, and GNPs, Applicants realize that the composite has elastic properties that help incorporate the micron-sized anode composite during expansion (lithiation) and prevent or at least reduce direct exposure of the silicon surface to the electrolyte.
[0096] Applicants believe that advantages of the composites of the present invention include one or more of the use of low-cost bead milling to produce nanoscale silicon particles of 20 nm to 200 nm, low-cost bead milling to form graphene-coated silicon particles, and the production of FLGs and GNPs during bead milling. The use of FLGs and GNPs in the composites and anode composites of the present invention to increase the elasticity of the composites is a further advantage that can be realized by the present invention.
[0097] According to another embodiment of the invention, the "separate" size reduction step comprises mixing the graphite particles with silicon nanoparticles in the presence of a polymer while being subjected to mixing / size reduction. The polymer is selected from the group of polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), and poly(methyl methacrylate) (PMMA). The polymer is present at 1-40% wt / wt and the silicon particles are present at 1-80% wt / wt. In one preferred form of the invention, the polymer is present at 5% wt / wt and the silicon particles are present at 10% wt / wt.
[0098] The resulting mixture is sent to a treatment step (ii). The treatment step is provided in the form of a mixing step including a hybridization process, which results in spheronization of the product. This hybridization or spheronization process provides "potato" shaped particles. The mixed or spheronized product is then sent to a heat treatment step as described above according to the first embodiment of the invention. However, in this second embodiment, the polymer becomes a carbon matrix, which holds / locates the graphite particles inside said carbon matrix as they surround the silicon nanoparticles, without the need for an additional binder as utilized in the first embodiment of the invention.
[0099] The process of the present invention may be better understood with reference to the following non-limiting examples. EXAMPLES
[0100] Talga Graphite FIG. 2 shows a typical natural graphite obtained from Applicant's proprietary source. The graphite is seen to be in flake form mixed with FLGs. In the case of spherical materials, the contact is usually found to be head to head. Whereas, in the case of flaky materials, the contact may be face to face. Thus, in a silicon and graphite mixture, the flake graphite is better suited to maintain physical contact during expansion and extraction of silicon. It is further understood by Applicant that the FLGs in the mixture also play an important role in maintaining good contact due to their high flexibility.
[0101] Talga Exfoliated Graphite The applicants have developed a unique exfoliated graphite for multiple applications, which the applicants refer to as Talga HSA, as described in detail in International Patent Application PCT / GB2018 / 052095 (WO 2019 / 020999), the entire contents of which are incorporated herein by reference.
[0102] Applicant's HSA widens the gaps between the graphene layers of graphite. Thus, compared to typical or "regular" graphite, the graphene layers are more easily exfoliated from the HSA to form FLGs during bead milling. As shown in FIG. 3, after about 168 minutes of bead milling of 10% HSA in IPA, the material is dominated by FLGs and thin flakes.
[0103] SEM of silicon / graphite composite To prepare the silicon / graphite composites (Gr@Si@C1@C2) according to the present invention, micron-sized silicon particles were first bead-milled into nanoscale particles (d50, 50-200 nm) in a non-aqueous solvent (e.g., IPA). HSA was then added to the milled silicon / IPA mixture and further milled, whereby the HSA produced FLGs, graphene, GNPs (graphite nanoparticles), and thin flakes. Spray drying was used to convert the nanomixture into micron-sized secondary particles. As an organic binder was used during spray drying or bead milling, a heat treatment was performed to convert them into amorphous carbon. Figure 4 shows an SEM image of the silicon / graphite secondary particles after heat treatment. It can be seen that the nanomaterials were converted into manageable micron-sized particles, including GNPs and FLGs.
[0104] Electrochemical characterization in half cells Half-cell tests were performed on Gr@Si@C1@C2 and the graphite control sample. Figure 5 shows the delithiation capability of Gr@Si@C1@C2 at various loadings. The details of the composites are given in Table 1 below.
[0105] As can be easily seen, each of the silicon / graphite composites according to the present invention exhibits higher capacity compared to the pristine graphite material, and the capacity increases with the loading of Gr@Si@C1@C2.
[0106] The details of the half-cell test of Si / graphite composites (results shown in FIG. 5) include: Coatings A-D: Active material (graphite+Gr@Si@C1@C2): CMC:SBR: Cmix=94:2:2:2 (by weight); Coatings E: Active material (Gr@Si@C1@C2): CMC:SBR: Cmix=80:8:8:4; Lithiation: 1st cycle: C / 10~5mV, then hold at 5mV until C / 100, other cycles: C / 5~5mV, then hold at 5mV until C / 40; Delithiation: 1st cycle: C / 10~1.0V, other cycles: C / 5~1.0V; A: graphite sample; B-E, 8%, 16.1%, 32.2%, and 80% Gr@Si@C1@C2, respectively. Details of A-E are shown in Table 1 below.
[0107] In the above details and in Table 1 below, CMC refers to carboxymethyl cellulose and SBR refers to styrene butadiene rubber. Table 1 -Details of the complexes A to E shown in Figure 5 [Table 1]
[0108] Comparison of Si@C and Gr@Si@C1@C2 During bead milling, 1,5-dihydroxynaphthane was used to completely replace EG. After spray drying and pyrolysis, the product is referred to as Si@C. Table 2 below shows some comparisons. It can be seen that the example with 2.5% Si in Gr@Si@C1@C2 has a higher capacity than the example with 3.4% Si in Si@C. When the Si content is similar, for example 10%, the Gr@Si@C1@C2 material has about 12% higher capacity compared to Si@C. The capacity data for 5% and 10% Si@C shows that the capacity of 5% Si content is about 460mAh / g, which is also about 10% lower than the capacity of Gr@Si@C1@C2 with similar silicon content. It is also shown that if Gr@Si@C1@C2 has a similar capacity to Si@C, a better cycling life can be reasonably expected. Table 2Comparison of -Si@C and Gr@Si@C1@C2 [Table 2]
[0109] Next, Figure 6 shows the effect of calendaring on half-cell capacity retention using anode composites Si@C and Gr@Si@C1@C2, respectively. Details of the calendaring effect test (results are shown in Figure 6) include: coating of Si@C: active material (graphite + Si@C): CMC: SBR: Cmix = (84.6: 9.4:): 2: 2: 2 (by weight); coating of Gr@Si@C1@C2: active material (Gr@Si@C1@C2): CMC: SBR: Cmix = (78.8: 15.2): 2: 2: 2; Si@CC and Gr@Si@CC (Gr@Si@C1@C2) are the same as above, but after coating, they were pressed with 2 tonnes; Lithiation: 1st cycle: C / 10 to 5 mV, then held at 5 mV until C / 100, other cycles: C / 5 to 5 mV, then held at 5 mV until C / 40. Delithiation: 1st cycle: C / 10~1.0V, other cycles: C / 5~1.0V.
[0110] For the tests conducted on the calendaring effect, two coatings with similar capacity (~490mAh / g) were used. For comparison, a 2-ton press was applied after coating. As shown in FIG. 6, for Si@C, the capacity retention decreased by about 5% from 96.4% to 91.5% after 50 cycles. However, for the composites containing Gr@Si@C1@C2, only a decrease of about 0.5% was observed. This indicates that the structure of the composites containing Gr@Si@C1@C2 is much more stable than that containing Si@C. The applicant understands that the contents of FLG, graphene, and GNP in Gr@Si@C1@C2 played an important role in maintaining the structure due to their relatively high flexibility.
[0111] Comparison between Si@C, Gr@Si@C, and Gr@Si@C1@C2 To form Gr@Si@C1@C2, the binder 30 is converted into carbon with high surface area using a relatively low temperature, e.g., 500-700°C, to form Gr@Si@C, which is then further coated with a binder 36, such as pitch or dihydroxynaphthalene, by conventional mixing in a solvent. The solvent is then evaporated and further heat treatment is performed at a relatively high temperature, e.g., 800-1000°C, to form the final product, Gr@Si@C1@C2. The binder 36 may contain either a content or a mixture of Al2O3, TiO2, and / or other ceramic materials.
[0112] Figure 7 shows the full cell data of commercial graphite, Si@C, Gr@Si@C, and Gr@Si@C1@C2 anode materials. Anode coating:active material:CMC:SBR:Cmix=94:2:2:2 (by weight), active materials are selected from graphite, Si@C, Gr@Si@C, and Gr@Si@C1@C2, respectively. Except for the graphite control sample, the silicon content in the active material is about 4%. After coating, all anode coatings have a capacity of about 1.3 g / cm 3 The cathode is of NMC111. The N / P capacity ratio is about 1.05. Charge: 1st cycle, C / 10 to 4.2V, then hold at 4.2V until C / 100; other cycles: C / 2 to 4.2V, then hold at 4.2V until C / 10; Discharge: 1st cycle, C / 10 to 3.0V; other cycles: C / 2 to 3.0V.
[0113] Figures 8a and 8b show the full cell data of the composite of the present invention. The Gr@Si@C1@C2 additive in the graphite anode (meaning about 3% Si in the final anode) results in ~97% capacity retention after 140 cycles at 0.5C. The cell is cycled with the following protocol: Charge: 1st and 2nd cycles: C / 10 to 4.2V, then hold at 4.2V until C / 100; other cycles: C / 2 to 4.2V, then hold at 4.2V until C / 10. Discharge: 1st and 2nd cycles: C / 10 to 3.0V; other cycles: C / 2 to 3.0V. N / P~1.05.
[0114] It is envisioned that the spray dryer described above may be advantageously replaced, for example, by a spouted fluidized bed system without departing from the scope of the present invention.
[0115] It is further envisaged that the size reduction step (i) provides graphite particles having a high or large "aspect ratio", which may include all or a portion of the expected graphite nanoparticles as well as few layer graphene (FLG) being produced.
[0116] As can be seen by reference to the above, the composite material and method of making the same of the present invention provides one or more advantages when compared to conventional techniques, such as low cost ball or bead milling to produce nanoscale silicon particles, low cost ball or bead milling to form graphene coated silicon particles, production of few layer graphene and graphite nanoparticles by the same low cost ball or bead milling, and the ability to provide composite materials with relatively high levels of elasticity. It is believed that one aspect of the present invention, the second embodiment, does not require the presence of graphene, graphite particles being sufficient.
[0117] The composites and anode materials of the present invention provide improved capacity and better cycle life, at least in part as a result of the multiple layers of graphene-like material that cover the silicon nanoparticles after milling, and provide improved resistance to expansion and improved electrical conductivity, which may be due to, for example, a "graphene sliding" effect. Furthermore, it is understood that the FLGs and GNPs created during bead milling maintain the electrical conductivity of the secondary particles during lithiation / delithiation (expansion / extraction) due to their high flexibility.
[0118] Additionally, the coating step (iv) and further heat treatment step (v) are believed to provide further protection to the Gr@Si@C or intermediate composites, including silicon graphene, graphite, and carbon matrix composites. This further layer or shell helps to provide a stable SEI, reduce contact between silicon and the electrolyte, and reduce outward expansion during lithiation.
[0119] Modifications and variations that are obvious to one skilled in the art are deemed to be within the scope of the present invention. [Prior art documents] [Patent documents]
[0120] [Patent Document 1] International Patent Application PCT / GB2018 / 051689 (International Publication No. 2018 / 229515) [Patent Document 2] International Publication No. 2015 / 073674 A1 [Patent Document 3] US2016 / 064731 (Jung Sung-Ho et al.) [Patent Document 4] US2018 / 097229 (Jo Sungnim et al.) [Non-patent literature]
[0121] [Non-Patent Document 1] XH Liu et al., “Size-Dependent Fracture of Silicon Nanoparticles During Lithiation”, ACS Nano, 2012, 6 (2), 1522-1531 [Non-Patent Document 2] Li et al, “Scalable synthesis of a novel structured graphite / silicon / pyrolysed carbon composite as anode material for high-performance lithium-ion batteries”, Journal of Alloys and Compounds 688 (2016) 1072-1079 [Non-Patent Document 3] Li et al., “Growth of conformal graphene cages on micrometre-sized silicon particles as stable battery anodes”, Nature Energy, Vol. 1., Article No. 15029 (2016) [Non-Patent Document 4] Son et al., “Silicon carbide-free graphene growth on silicon for lithium-ion battery with high volumetric energy density”, Nature Communications, Vol. 6., Article No. 7393 (2015)
Claims
1. A composite material comprising silicon and graphite, comprising a plurality of silicon nanoparticles coated with graphene particles, few-layer graphene particles, graphite nanoparticles, a carbon matrix, and an amorphous carbon outer shell, wherein the silicon nanoparticles coated with graphene particles, the few-layer graphene particles, and the graphite nanoparticles are each held within the carbon matrix.
2. The carbon matrix is (i) an amorphous carbon matrix; (ii) a crystalline carbon matrix; or (iii) The composite material of claim 1 provided in the form of a combination of both an amorphous carbon matrix and a crystalline carbon matrix.
3. 3. The composite material of claim 1, wherein the graphene particles are in the form of graphene nanosheets.
4. The amorphous carbon outer shell is (i) one or more oxides; or (ii) Al 2 O 3 , TiO 2 , ZrO 2 , BaTiO 3 , MgO, CuO, ZnO, Fe 2 O 3 , GeO 2 , Li 2 4. The composite material of claim 1, further comprising one or more oxides present in the form of O, MnO, NiO, or zeolites, or any combination thereof.
5. The composite material of claim 4, wherein the oxide has a particle size of from 20 nm to 1 micron.
6. An anode composite comprising a composite material according to any one of claims 1 to 5.
7. 1. A method for the production of a composite material, comprising: (i) subjecting silicon particles to a size reduction process together with graphite particles in a solvent, optionally in the presence of a polymer, to produce silicon nanoparticles coated with graphene particles, few layer graphene particles, and graphite nanoparticles; (ii) processing the product of step (i) with or without a binder to produce a composite; (iii) heat treating the composite of step (ii) to produce a composite material comprising a plurality of silicon nanoparticles coated with graphene particles, few layer graphene particles, graphite nanoparticles, and a carbon matrix, each of the plurality of silicon nanoparticles coated with graphene particles, few layer graphene particles, and graphite nanoparticles being held within the carbon matrix; (iv) coating the composite material of step (iii) with a binder; (v) heat treating the composite material of step (iv) to produce a shell comprising amorphous carbon.
8. The shell is (i) one or more oxides; or (ii) Al 2 O 3 , TiO 2 , ZrO 2 , BaTiO 3 , MgO, CuO, ZnO, Fe 2 O 3 , GeO 2 , Li 2 8. The method of claim 7, further comprising one or more oxides present in the form of O, MnO, NiO, or a zeolite, or any combination thereof.
9. 9. A method according to any of claims 7 to 8, further comprising an initial step in which a silicon material is subjected to a size reduction step in a solvent to produce said silicon nanoparticles of step (i).
10. The method of claim 9 , wherein the silicon material of the first step is provided in the form of micron-scale silicon particles.
11. A method according to any of claims 7 to 10, wherein the size reduction step of step (i) provides silicon nanoparticles having a size between 20 and 200 nm.
12. 11. The method of any of claims 9 to 10, wherein the initial step and the size reduction step of step (i) are each grinding steps.
13. 13. The method of claim 12, wherein the grinding step is carried out in one or more bead mills.
14. The solvent is (i) a non-aqueous solvent; or 14. The method of claim 7, wherein (ii) is provided in the form of isopropyl alcohol.
15. 15. The method of any of claims 7 to 14, wherein the polymer is selected from the group of polyethylene oxide (PEO), polyvinyl alcohol (PVA), polyvinylidene fluoride (PVDF), poly(vinylidene fluoride-co-hexafluoropropylene) (PVDF-HFP), and poly(methyl methacrylate) (PMMA).
16. The treatment of step (ii) (i) spray drying in the presence of a binder; (ii) a mixing step; or 16. The method according to any of claims 7 to 15, wherein (iii) the secondary particles or products produced are provided in the form of a mixing step including a hybridization process, in which they are spheronized.
17. 17. The method according to any of claims 7 to 16, wherein the heat treatment of steps (iii) and (v) is provided in the form of pyrolysis.
18. 18. The method of any of claims 7 to 17, wherein the heat treatment of steps (iii) and (v) converts any binder present into amorphous carbon.
19. 19. The method of any of claims 7 to 18, wherein the temperature of the heat treatment in step (iii) is lower than the temperature of the heat treatment in step (v).
20. After the heat treatment of step (iii), the surface area (BET) of the composite material is between 70 and 120 m 2 The method according to any one of claims 7 to 19, wherein the molecular weight is 1 / g.
21. After the heat treatment of step (v), the surface area (BET) of the composite material is between 10 and 30 m 2 The method according to any one of claims 7 to 20, wherein the molecular weight is 1 / g.
22. 22. The method of any of claims 7 to 21, wherein the graphite particles of milling step (i) are provided in the form of pre-exfoliated graphite particles.
23. 23. The method of any of claims 7 to 22, wherein the milling process of step (i) produces graphene attached to the silicon nanoparticles.
24. The method according to any of claims 7 to 23, wherein the heat treatment in step (iii) is carried out at a temperature between 500°C and 700°C.
25. The heat treatment of step (v) (i) 750°C to 1100°C; or (ii) A method according to any one of claims 7 to 24, carried out at a temperature of from 850°C to 1000°C.
26. 8. The method according to claim 7, wherein the treating in step (ii) is carried out by spray drying or mechanofusion.
Citation Information
Patent Citations
Graphene-silicon-based composite negative electrode material for lithium ion battery and preparation method thereof
CN109873152A
Carbon-silicon complex and method for producing the same
JP2016054145A
Carbon-silicon composite and manufacturing method thereof
US20160064731A1
Negative active material, lithium secondary battery including the material, and method of manufacturing the material