Unit cell and battery cell including the same
Adhesive compositions with controlled shear strengths and viscosities are used to bond electrodes and separation membranes, addressing displacement and damage issues in conventional lamination methods, improving battery cell manufacturing.
Patent Information
- Application Number
- JP2023512034
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2022-04-19
- Filing Date
- 2022-04-27
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2042-04-27
AI Technical Summary
Conventional lamination methods using heat and pressure for bonding electrodes and separation membranes in pouch-type batteries can cause displacement, damage, and uneven adhesive strength, leading to manufacturing issues.
The use of an adhesive composition to bond electrodes and separation membranes, with specific shear strengths and viscosities for the first and second adhesive parts, ensuring uniform adhesion and preventing displacement and damage.
Prevents movement and deformation of electrodes and separation membranes, enhancing manufacturing efficiency and reducing defects in battery cells.
Smart Images

Figure 0007572114000003 
Figure 0007572114000004 
Figure 0007572114000005
Abstract
Description
[Technical field]
[0001] Cross-reference to related application(s) This application claims the benefit of priority based on Korean Patent Application No. 10-2021-0066461 filed on May 24, 2021, and Korean Patent Application No. 10-2022-0048387 filed on April 19, 2022, and all contents disclosed in the documents of said Korean patent applications are incorporated herein by reference.
[0002] The present invention relates to a unit cell and a battery cell including the same, and more particularly to a unit cell in which electrodes and separators are bonded to each other using an adhesive composition instead of conventional lamination using heat and pressure, and a battery cell including the same. [Background technology]
[0003] With technological development and increasing demand for mobile devices, the demand for secondary batteries as an energy source is rapidly increasing. In particular, secondary batteries are attracting great attention as an energy source for power devices such as electric bicycles, electric cars, and hybrid electric cars as well as for mobile devices such as mobile phones, digital cameras, laptops, and wearable devices.
[0004] Such secondary batteries are classified into cylindrical batteries and prismatic batteries in which the electrode assembly is housed in a cylindrical or prismatic metal can, and pouch batteries in which the electrode assembly is housed in a pouch case made of an aluminum laminate sheet, according to the shape of the battery case. Here, the electrode assembly housed in the battery case is a power generating element capable of charging and discharging, which is composed of a positive electrode, a negative electrode, and a separator structure interposed between the positive electrode and the negative electrode, and is classified into a jelly roll type in which a separator is interposed between a long sheet-like positive electrode and a negative electrode coated with an active material, and which is wound up, and a stack type in which a number of positive electrodes and negative electrodes are stacked in sequence with a separator interposed therebetween.
[0005] Among these, the use of pouch-type batteries, which have a structure in which a stack-type or stack / folding-type electrode assembly is built into a pouch-type battery case made of an aluminum laminate sheet, is gradually increasing due to low manufacturing costs, small weight, easy modification, etc.
[0006] Here, in the case of a stack-type electrode assembly, a method is generally used in which a unit cell is manufactured in advance and then a plurality of the unit cells are stacked to manufacture the electrode assembly. More specifically, the unit cells are stacked alternately in the order of separator-anode-separator-cathode, and heat and pressure are applied to the unit cells through a laminating device, thereby fixing each component to each other.
[0007] However, after the separator-anode-separator-cathode are alternately stacked in this order, before entering the laminating device or during lamination, a part of the separator or electrode may be pushed out from the correct position, which may cause damage or a difference in adhesive strength.
[0008] For this reason, it is necessary to develop a unit cell in which movement between the electrodes and the separator is prevented and deformation and damage of the electrodes and the separator can be prevented. Summary of the Invention [Problem to be solved by the invention]
[0009] The object of the present invention is to provide a unit cell in which an electrode and a separator and a separator are bonded to each other using an adhesive composition instead of the conventional lamination using heat and pressure, and a battery cell including the unit cell.
[0010] The problems to be solved by the present invention are not limited to the problems described above, and problems not mentioned will be clearly understood by a person having ordinary skill in the art to which the present invention pertains from this specification and the accompanying drawings. [Means for solving the problem]
[0011] According to one embodiment of the present invention, a unit cell includes a predetermined number of alternately stacked separators and electrodes; a first adhesive portion between the separator and the electrode and made of a first adhesive composition; and a second adhesive portion between the separator and another separator and made of a second adhesive composition, wherein the shear strength of the first adhesive portion is equal to or less than the shear strength of the second adhesive portion.
[0012] The first adhesive portion may have a shear strength of 0.15 MPa or more and 0.5 MPa or less, and the second adhesive portion may have a shear strength of 0.15 MPa or more and 3.5 MPa or less.
[0013] The second adhesive portion may have a shear strength of 1.5 MPa or more and 3.5 MPa or less.
[0014] The viscosity of the first adhesive portion may be the same as or less than the viscosity of the second adhesive portion.
[0015] The viscosity of the first adhesive portion may be 50 cP (at 150° C.) to 120 cP (at 150° C.), and the viscosity of the second adhesive portion may be 50 cP (at 150° C.) to 12,000 cP (at 150° C.).
[0016] The viscosity of the second adhesive portion may be 800 cP (at 150° C.) to 12,000 cP (at 150° C.).
[0017] The first adhesive portion may have a thickness smaller than a thickness of the electrode, and the second adhesive portion may have a thickness equal to or smaller than a thickness of the electrode.
[0018] The thickness of the first adhesive portion may be 0.01% to 10% of the thickness of the electrode, and the thickness of the second adhesive portion may be 90% to 100% of the thickness of the electrode.
[0019] The adhesive strength of the first adhesive portion may be the same as or greater than the adhesive strength of the second adhesive portion.
[0020] The adhesive strength of the first adhesive portion is 50 gf / mm 2 More than ~100gf / mm 2 The adhesive strength of the second adhesive portion is 20 gf / mm 2 More than ~100gf / mm 2 It can be the following:
[0021] The second adhesive portion may be located between an end of the separator and an end of the electrode.
[0022] The width of the second adhesive portion may be smaller than a distance between an edge of the separator and an edge of the electrode.
[0023] The first adhesive portion and the second adhesive portion may each be formed in a pattern including a plurality of dots spaced apart from one another.
[0024] The dots included in the second adhesive portion may have a diameter smaller than a distance between an edge of the electrode and an edge of the separator.
[0025] The first adhesive composition may be made of at least one of an EVA (Ethylene vinyl acetate)-based material, an acrylic-based material, and an epoxy-based material, and the second adhesive composition may be made of at least one of an EVA (Ethylene vinyl acetate)-based material, an acrylic-based material, an epoxy-based material, a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
[0026] The second adhesive composition may be made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
[0027] According to another embodiment of the present invention, an electrode assembly is formed by alternately stacking the unit cells, and the first adhesive portion includes an adhesive pattern disposed at the same position between each of the electrodes and the separator.
[0028] According to another embodiment of the present invention, the electrode assembly is formed by alternately stacking the unit cells, and the first adhesive portion includes adhesive patterns disposed in a staggered manner between the electrodes and the separators.
[0029] A battery cell according to another embodiment of the present invention includes an electrode assembly in which the unit cells are alternately stacked, and an electrolyte.
[0030] The first adhesive portion may have a property of being dissolved in an electrolyte solution.
[0031] The battery cell may have a zigzag shape due to the separator being folded.
[0032] According to another embodiment of the present invention, a method for manufacturing a unit cell includes the steps of: applying a first adhesive to at least one of a first surface of an electrode or a bonding area of a first separator; applying the first adhesive to at least one of a second surface of the electrode or a bonding area of a second separator, the second surface of the electrode being located on an opposite side of the electrode from the first surface of the electrode; applying a second adhesive to at least one of a peripheral area of the first separator or a peripheral area of the second separator; and stacking the electrode between the first separator and the second separator such that the first surface of the electrode contacts the bonding area of the first separator and the second surface of the electrode contacts the bonding area of the second separator to form at least a portion of a stack, the stack being formed such that the peripheral areas of the first and second separators extend outward beyond the periphery of the electrodes, the peripheral areas of the first and second separators face each other without an electrode therebetween, and a shear strength of the first adhesive is equal to or less than a shear strength of the second adhesive.
[0033] The method of manufacturing the unit cell may further include compressing the stack along a direction perpendicular to the first surface of the electrode and the second surface of the electrode.
[0034] The method for manufacturing the unit cell may further include disposing the stack and an electrolyte in a battery case.
[0035] The peripheral regions of each of the first and second separators may extend around the periphery of each of the first and second separators, such that each of the peripheral regions surrounds a joining region of each of the first and second separators.
[0036] The first adhesive may have a shear strength of 0.15 MPa or more and 0.5 MPa or less, and the second adhesive may have a shear strength of 0.15 MPa or more and 3.5 MPa or less.
[0037] The second adhesive may have a shear strength of 1.5 MPa or more and 3.5 MPa or less.
[0038] The viscosity of the first adhesive may be less than or equal to the viscosity of the second adhesive.
[0039] The viscosity of the first adhesive may be 50 cP (at 150° C.) to 120 cP (at 150° C.), and the viscosity of the second adhesive may be 50 cP (at 150° C.) to 12,000 cP (at 150° C.).
[0040] The viscosity of the second adhesive may be 800 cP (at 150° C.) to 12,000 cP (at 150° C.).
[0041] The thickness of the first adhesive may be less than the thickness of the electrode, and the thickness of the second adhesive may be the same as or less than the thickness of the electrode.
[0042] The thickness of the first adhesive may be 0.01% to 10% of the thickness of the electrode, and the thickness of the second adhesive may be 90% to 100% of the thickness of the electrode.
[0043] The adhesive strength of the first adhesive may be greater than or equal to the adhesive strength of the second adhesive.
[0044] The adhesive strength of the first adhesive is 50gf / mm 2 More than 100gf / mm 2 The adhesive strength of the second adhesive is 20 gf / mm 2 More than 100gf / mm 2 It can be the following:
[0045] The width of the second adhesive applied to the peripheral regions of the first and second separators may be smaller than the width of the peripheral regions to which the second adhesive is applied.
[0046] The first adhesive and the second adhesive may each be applied in a respective dot pattern that is spaced apart from one another.
[0047] Each dot in the dot pattern of the second adhesive may have a diameter smaller than a width of a peripheral region of each of the first and second separators.
[0048] In the first adhesive dot pattern, the dots may be arranged in a grid of rows and columns.
[0049] The first adhesive may be made of at least one of an ethylene-vinyl acetate (EVA)-based material, an acrylic-based material, and an epoxy-based material, and the second adhesive may be made of at least one of an ethylene-vinyl acetate (EVA)-based material, an acrylic-based material, an epoxy-based material, a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
[0050] The second adhesive may be made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material. Effect of the Invention
[0051] According to an embodiment, the unit cell of the present invention and a battery cell including the same can prevent movement between the electrodes and the separator and between the separators by adhering the electrodes and the separators using an adhesive composition instead of the conventional lamination using heat and pressure, thereby preventing deformation and damage of the electrodes and the separator.
[0052] The effects of the present invention are not limited to the effects described above, and effects not mentioned will be clearly understood by those having ordinary skill in the art to which the present invention pertains from this specification and the accompanying drawings. [Brief description of the drawings]
[0053] [Figure 1] FIG. 2 is an exploded perspective view of a unit cell according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a perspective view showing a unit cell in which the components of FIG. 1 are combined. [Diagram 3] FIG. 3 is a cross-sectional view taken along axis AA in FIG. 2. [Figure 4] 3A to 3C are cross-sectional views showing a process in which the unit cell of FIG. 2 is pressurized. [Diagram 5] 3 is a view showing a process in which a first adhesive portion and a second adhesive portion included in the unit cell of FIG. 2 are applied; [Figure 6] FIG. 4 is a top view of a battery cell according to another embodiment of the present invention. [Figure 7] 3 is a graph showing Linear Sweep Voltammetry (LSV) of an adhesive composition included in the unit cell of FIG. 2. [Figure 8] 4 is a cross-sectional view showing an electrode assembly according to another embodiment of the present invention. [Figure 9] 4 is a cross-sectional view showing an electrode assembly according to still another embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0054] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention may, however, be embodied in various different forms and should not be construed as being limited to the embodiments set forth herein.
[0055] In order to clearly explain the present invention, parts unnecessary for the explanation are omitted, and the same reference numerals are used throughout the specification to refer to the same or similar components.
[0056] In addition, the size and thickness of each component shown in the drawings are arbitrarily shown for convenience of explanation, and the present invention is not necessarily limited to those shown in the drawings. In the drawings, thicknesses are enlarged to clearly show multiple layers and regions. In the drawings, thicknesses of some layers and regions are exaggerated for convenience of explanation.
[0057] Furthermore, throughout the specification, when a part is said to "comprise" a certain element, this does not mean that it excludes other elements and may further include other elements, unless specifically stated to the contrary.
[0058] Also, throughout the specification, a reference to "in a plane" means when the subject part is viewed from above, and a reference to "in cross section" means when the subject part is cut vertically and viewed from the side.
[0059] Hereinafter, a unit cell according to an embodiment of the present invention will be described.
[0060] Fig. 1 is an exploded perspective view of a unit cell according to an embodiment of the present invention, Fig. 2 is a perspective view showing a unit cell in which the components of Fig. 1 are combined, Fig. 3 is a cross-sectional view taken along the AA axis of Fig. 2.
[0061] 1 and 2, a unit cell according to an embodiment of the present invention includes a predetermined number of alternately stacked separators 210, 250 and electrodes 110, 150; a first adhesive portion 310 located between the separators 210, 250 and the electrodes 110, 150 and made of a first adhesive composition; and a second adhesive portion 350 located between the separators 210, 250 and other separators 210, 250 and made of a second adhesive composition.
[0062] More specifically, the separators 210, 250 include a lower separator 210 and an upper separator 250, and the electrodes 110, 150 include a first electrode 110 and a second electrode 150, and may be stacked in the order of the lower separator 210, the first electrode 110, the upper separator 250, and the second electrode 150.
[0063] Here, the first electrode 110 may include a first electrode tab 115 protruding in one direction, and the second electrode 150 may include a second electrode tab 155 protruding in one direction. As an example, as shown in Figs. 1 and 2, the first electrode 110 and the second electrode 150 are stacked such that the upper separator 250 is located between them, and the first electrode tab 115 of the first electrode 110 and the second electrode tab 155 of the second electrode 150 may be stacked such that they are located in opposite directions. However, the present embodiment is not limited thereto, and a structure in which the first electrode tab 115 and the second electrode tab 155 are stacked such that they are located in the same direction may also be included in the present embodiment.
[0064] Here, the first electrode 110 and the second electrode 150 may each include an electrode current collector and an active material layer located on the electrode current collector. Here, the active material layer may be made of an electrode composition including an electrode active material. More specifically, the first electrode 110 and the second electrode 150 may be a positive electrode or a negative electrode. Here, the positive electrode may include a positive electrode current collector and an active material layer including a positive electrode active material, and the negative electrode may include a negative electrode current collector and an active material layer including a negative electrode active material. As an example, the first electrode 110 may be a negative electrode, and the second electrode 150 may be a positive electrode. However, the present embodiment is not limited to this, and the opposite case may also be included in the present embodiment.
[0065] The negative electrode active material may be a common negative electrode active material for lithium secondary batteries in the art, and examples thereof include lithium metal, lithium alloy, petroleum coke, activated carbon, graphite, silicon, tin, metal oxides, and other carbons.
[0066] In addition, the positive electrode active material may be, for example, selected from the group consisting of lithium-cobalt oxide, lithium-manganese oxide, lithium-nickel-manganese oxide, lithium-manganese-cobalt oxide, lithium-nickel-manganese-cobalt oxide, and lithium iron phosphate, or may be a combination thereof or a composite oxide thereof.
[0067] The negative electrode current collector or the positive electrode current collector is not particularly limited as long as it does not induce a chemical change in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel surface-treated with carbon, nickel, titanium, silver, etc. may be used.
[0068] The separators 210 and 250 may separate the first electrode 110 and the second electrode 150 and provide a path for lithium ions to move. In addition, the separators 210 and 250 include a lower separator 210 and an upper separator 250, and the lower separator 210 and the upper separator 250 may be made of different or the same material.
[0069] For example, the separators 210 and 250 may be any separator that is generally used in lithium secondary batteries, and are preferably one that has low resistance to ion migration of the electrolyte and excellent electrolyte humidification capability. Specifically, a porous polymer film, for example, a porous polymer film made of a polyolefin polymer such as an ethylene homopolymer, a propylene homopolymer, an ethylene / butene copolymer, an ethylene / hexene copolymer, or an ethylene / methacrylate copolymer, or a laminate structure of two or more layers thereof, may be used.
[0070] Hereinafter, the first adhesive part 310 and the second adhesive part 350 included in the unit cell according to this embodiment will be mainly described.
[0071] Referring to Figures 1 and 3, the first adhesive portion 310 may be located at least one of between the first electrode 110 and the lower separator 210, between the first electrode 110 and the upper separator 250, and between the second electrode 150 and the upper separator 250.
[0072] The first adhesive portion 310 may be made of a first adhesive composition, and the second adhesive portion 350 may be made of a second adhesive composition. As an example, the first adhesive composition may be made of at least one of an EVA (Ethylene vinyl acetate)-based material, an acrylic material, and an epoxy-based material, and the second adhesive composition may be made of at least one of an EVA (Ethylene vinyl acetate)-based material, an acrylic material, an epoxy-based material, a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material. More preferably, the second adhesive composition may be made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material among the above-mentioned materials.
[0073] As a result, the first adhesive part 310 can fix the first electrode 110 and the second electrode 150 to the lower separation film 210 and / or the upper separation film 250, respectively. In other words, unlike the conventional lamination process, the first adhesive part 310 can prevent movement between the electrodes 110, 150 and the separation films 210, 250, and can prevent deformation and damage of the electrodes 110, 150 and the separation films 210, 250.
[0074] 1 and 3, the first adhesive portion 310 and the second adhesive portion 350 are formed at different positions, and therefore may have different physical properties or physical conditions.
[0075] The shear strength of the first adhesive part 310 may be the same as or smaller than the shear strength of the second adhesive part 350. Here, the shear strength of the first adhesive part 310 may be 0.15 MPa or more and 0.5 MPa or less, and the shear strength of the second adhesive part 350 may be 0.15 MPa or more and 3.5 MPa or less.
[0076] For example, the shear strength of the first adhesive portion 310 and the shear strength of the second adhesive portion 350 may be 0.15 MPa or more and 0.5 MPa or less. More specifically, the shear strength of the first adhesive portion 310 and the shear strength of the second adhesive portion 350 may be 0.2 MPa or more and 0.5 MPa or less.
[0077] As a result, since the first adhesive portion 310 and the second adhesive portion 350 have shear strength within the aforementioned range, the first adhesive portion 310 and the second adhesive portion 350 can be easily pressed by the pressing rolls 510, 520 (FIG. 4), respectively.
[0078] On the other hand, if the shear strength of the first adhesive part 310 and the second adhesive part 350 is less than 0.15 MPa, it may be disadvantageous to the adhesion and fixation between the electrodes 210, 250 and the separators 210, 250. Also, if the shear strength of the first adhesive part 310 and the second adhesive part 350 exceeds 0.5 MPa, the first adhesive part 310 may not be easily compressed by the compression rolls 510, 520 (FIG. 4), and the first thickness d1 of the first adhesive part 310 may be excessively large or uneven.
[0079] As another example, the shear strength of the first adhesive portion 310 may be 0.15 MPa or more and 0.5 MPa or less, and the shear strength of the second adhesive portion 350 may be 1.5 MPa or more and 3.5 MPa or less. More specifically, the shear strength of the first adhesive portion 310 may be 0.2 MPa or more and 0.5 MPa or less, and the shear strength of the second adhesive portion 350 may be 2.0 MPa or more and 3.5 MPa or less.
[0080] As a result, the second adhesive part 350 of the first adhesive part 310 has a shear strength within the above-mentioned range, so that the second adhesive part 350 can be easily compressed by the compression rolls 510, 520 (FIG. 4), respectively. In addition, since the shear strength of the second adhesive part 350 is greater than the shear strength of the first adhesive part 310, it is possible to prevent a phenomenon in which a part of the second adhesive part 350 comes into contact with the electrodes 110, 150 or escapes from the ends of the separators 210, 250 and leaks to the outside.
[0081] On the other hand, if the shear strength of the second adhesive part 350 is less than 1.5 MPa, the second adhesive part 350 may spread out to both sides during some processes, causing problems such as a portion of the second adhesive part 350 contacting the electrodes 110, 150 or leaking out of the ends of the separators 210, 250. Also, if the shear strength of the second adhesive part 350 exceeds 3.5 MPa, the second adhesive part 350 may not be easily compressed by the compression rolls 510, 520 (FIG. 4), and the second thickness d2 of the second adhesive part 350 may be excessively large or uneven.
[0082] Also, the first thickness d1 of the first adhesive portion 310 may be smaller than the second thickness d2 of the second adhesive portion 350. More specifically, the first thickness d1 of the first adhesive portion 310 may be smaller than the thickness D1 of the electrodes 110 and 150, and the second thickness d2 of the second adhesive portion 350 may be equal to or smaller than the thickness D1 of the electrodes 110 and 150. For example, as shown in FIG. 3, the first thickness d1 of the first adhesive portion 310 may be smaller than the thickness d2 of the first electrode 110, and the second thickness d2 of the second adhesive portion 350 may be equal to or smaller than the thickness D1 of the first electrode 110.
[0083] As a result, the first adhesive part 310 has a relatively small thickness, thereby reducing gaps that may occur between the electrodes 110, 150 and the separators 210, 250, and improving the spatial efficiency of the unit cell 100. In addition, the second adhesive part 350 has a similar thickness to the first electrode 110, thereby allowing the lower separator 210 and the upper separator 250 to be easily adhered and fixed, while the thickness of the unit cell 100 may be relatively uniform.
[0084] In addition, the first thickness d1 of the first adhesive portion 310 may be 0.01% to 10% of the thickness D1 of the electrodes 110 and 150. More specifically, the first thickness d1 of the first adhesive portion 310 may be 0.05% to 8% of the thickness D1 of the electrodes 110 and 150. As an example, the first thickness d1 of the first adhesive portion 310 may be 1% to 5.0% of the thickness D1 of the electrodes 110 and 150.
[0085] As a result, the first thickness d1 of the first adhesive portion 310 has a ratio within the above-mentioned range to the thickness D1 of the electrodes 110, 150, so that the electrodes 110, 150 and the separators 210, 250 can be easily adhered and fixed to each other while the thickness of the unit cell 100 can be relatively uniform.
[0086] On the other hand, if the first thickness d1 of the first adhesive part 310 is less than 0.01% of the thickness D1 of the electrodes 110, 150, the fixing force between the electrodes 110, 150 and the separators 210, 250 is insufficient, which may cause the electrodes 110, 150 and the separators 210, 250 to separate from each other in a subsequent process. Also, if the first thickness d1 of the first adhesive part 310 is more than 10% of the thickness D1 of the electrodes 110, 150, the gap between the electrodes 110, 150 and the separators 210, 250 is too large, which may cause a problem of reduced space efficiency and battery capacity of the unit cell 100.
[0087] FIG. 4 is a cross-sectional view showing a process in which the unit cell of FIG. 2 is pressurized.
[0088] 3 and 4, the first thickness d1 of the first adhesive portion 310 and the second thickness d2 of the second adhesive portion 350 may be thicknesses after the unit cell 100 is compressed in the up, down and both sides by the compression rolls 510 and 520. Here, the compression rolls 510 and 520 may be rolls such as nip rolls, and may compress the unit cell 100 in the up, down and both sides of the unit cell 100.
[0089] Here, in the unit cell 100 before being compressed by the compression rolls 510, 520, the third thickness d3 of the first adhesive portion 310 may be greater than the first thickness d1 of the first adhesive portion 310. More specifically, the third thickness d3 of the first adhesive portion 310 may be 40% to 60% of the thickness D1 of the electrodes 110, 150. As an example, the third thickness d3 of the first adhesive portion 310 may be 45% to 55% of the thickness D1 of the electrodes 110, 150.
[0090] In addition, the fourth thickness d4 of the second adhesive portion 350 may be greater than the second thickness d2. More specifically, the fourth thickness d4 of the second adhesive portion 350 may be 90% or more and 105% or less of the thickness D1 of the electrodes 110, 150. As an example, the fourth thickness d4 of the second adhesive portion 350 may be 95% or more and 105% or less of the thickness D1 of the electrodes 110, 150.
[0091] As a result, the thicknesses of the first adhesive part 310 and the second adhesive part 350 before being compressed by the compression rolls 510 and 520 may have a thickness ratio in the above-mentioned range. Therefore, even after the unit cell 100 is compressed by the compression rolls 510 and 520, the separators 210 and 250 or the electrodes 210 and 250 and the separators 210 and 250 may be easily bonded and fixed, and the thickness of the unit cell 100 may be relatively uniform.
[0092] In addition, the adhesive strength of the first adhesive portion 310 may be the same as or greater than the adhesive strength of the second adhesive portion 350. Here, the adhesive strength of the first adhesive portion 310 and the second adhesive portion 350 may be measured by applying 15 dots of the first adhesive composition and the second adhesive composition at intervals of 3 mm between a pair of tension jigs prepared in advance, and then peeling them off vertically.
[0093] At this time, the adhesive strength of the first adhesive portion 310 is 50 gf / mm 2 More than ~100gf / mm 2 The adhesive strength of the second adhesive portion 350 is 20 gf / mm 2 More than ~100gf / mm 2 More specifically, the adhesive strength of the first adhesive portion 310 may be 55 gf / mm 2 More than ~95gf / mm 2 The adhesive strength of the second adhesive portion 350 is 25 gf / mm 2 More than ~95gf / mm 2 As an example, the adhesive strength of the first adhesive portion 310 may be 60 gf / mm 2 Over 90gf / mm 2 The adhesive strength of the second adhesive portion 350 is 25 gf / mm 2 Over 90gf / mm 2 It can be the following:
[0094] As a result, since the first adhesive portion 310 and the second adhesive portion 350 have adhesive strength within the aforementioned range, the first adhesive portion 310 and the second adhesive portion 350 can easily adhere and fix the separation membranes 210, 250 between the electrodes 210, 250 and the separation membranes 210, 250, respectively.
[0095] In contrast, the adhesive strength of the first adhesive portion 310 is 50 gf / mm 2 Less than 100gf / mm 2 If it exceeds this value, there is a problem that the electrodes 210, 250 and the separators 210, 250 may separate from each other in the post-process, making the manufacturing process difficult. 2 Less than 100gf / mm 2 If it is excessive, there is a problem that the upper separator 250 and the lower separator 210 are separated from each other in the post-process, making the manufacturing process difficult.
[0096] FIG. 5 is a view showing a process in which the first adhesive portion and the second adhesive portion included in the unit cell of FIG. 2 are applied.
[0097] Also, the viscosity of the first adhesive part 310 may be the same as or lower than the viscosity of the second adhesive part 350. More specifically, referring to FIG. 3 and FIG. 5, the first adhesive part 310 and the second adhesive part 350 may be applied to the electrodes 110, 150 and / or the separators 210, 250 by the applicator 600. As an example, the applicator 600 may be an apparatus such as an inkjet ejection apparatus, and the applicator 600 may include a housing 610 that changes the volume of an internal pressure chamber, a wall surface 620 that reduces the volume of the pressure chamber, and an outlet 610a from which the adhesive composition is discharged. In other words, the viscosity of the first adhesive part 310 and the second adhesive part 350 may be the discharged viscosity discharged from the outlet 610a of the applicator 600.
[0098] More specifically, the viscosity of the first adhesive portion 310 and the second adhesive portion 350 may be the viscosity (cP (at 150° C.)) discharged from the discharge port 610a of the coating device 600 at 150 degrees Celsius. Here, the viscosity of the first adhesive portion 310 may be 50 cP (at 150° C.) to 120 cP (at 150° C.), and the viscosity of the second adhesive portion 350 may be 50 cP (at 150° C.) to 12,000 cP (at 150° C.).
[0099] As an example, the viscosity of the first adhesive section 310 and the viscosity of the second adhesive section 350 may each be 60 cP (at 150° C.) to 110 cP (at 150° C.). More specifically, the viscosity of the first adhesive section 310 and the viscosity of the second adhesive section 350 may each be 70 cP (at 150° C.) to 100 cP (at 150° C.).
[0100] As a result, since the first adhesive portion 310 and the second adhesive portion 350 have a viscosity within the aforementioned range, the first adhesive portion 310 and the second adhesive portion 350 have an adhesive strength that can easily bond and fix the separation membranes 210, 250 between the electrodes 210, 250 and the separation membranes 210, 250, respectively, while improving the discharge stability of the coating device 600.
[0101] On the other hand, if the viscosity of the first adhesive part 310 and the second adhesive part 350 is less than 60 cP (at 150° C.), it may be disadvantageous to the adhesion and fixation between the electrodes 110, 150 and the separators 210, 250. Also, if the viscosity of the first adhesive part 310 and the second adhesive part 350 is more than 120 cP (at 150° C.), the first adhesive part 310 may not be easily compressed by the compression rolls 510, 520 (FIG. 4), and the first thickness d1 of the first adhesive part 310 may be excessively large or uneven.
[0102] As another example, the viscosity of the first adhesive portion 310 may be 60 cP (at 150° C.) to 110 cP (at 150° C.), and the viscosity of the second adhesive portion 350 may be 800 cP (at 150° C.) to 12,000 cP (at 150° C.). More specifically, the viscosity of the first adhesive portion 310 may be 70 cP (at 150° C.) to 100 cP (at 150° C.), and the viscosity of the second adhesive portion 350 may be 850 cP (at 150° C.) to 11,000 cP (at 150° C.).
[0103] As a result, since the first adhesive part 310 and the second adhesive part 350 have a viscosity in the above-mentioned range, the first adhesive part 310 and the second adhesive part 350 have an adhesive force that can easily bond and fix the separation membranes 210, 250 or the electrodes 110, 150 and the separation membranes 210, 250, respectively, while improving the discharge stability of the coating device 600. In addition, since the viscosity of the second adhesive part 350 is higher than that of the first adhesive part 310, it is possible to prevent a phenomenon in which a part of the second adhesive part 350 comes into contact with the electrodes 110, 150 or escapes from the ends of the separation membranes 210, 250 and leaks to the outside.
[0104] On the other hand, if the viscosity of the second adhesive part 350 is less than 800 cP (at 150° C.), there is a problem that the second adhesive part 350 spreads to both sides during some processes, and a part of the second adhesive part 350 comes into contact with the electrodes 110, 150, or escapes from the ends of the separation membranes 210, 250 and leaks to the outside. In addition, if the viscosity of the second adhesive part 350 exceeds 12000 cP (at 150° C.), there is a problem that the discharge stability of the coating device 600 decreases.
[0105] Here, the first width r1 of the second adhesive portion 350 may be smaller than the distance D2 between the ends of the separators 210, 250 and the ends of the electrodes 110, 150. More specifically, the first width r1 of the second adhesive portion 350 may be a width after the unit cell 100 is compressed in the up, down and both sides by the compression rolls 510, 520. That is, the first width r1 of the second adhesive portion 350 may be larger than the second width r2 of the second adhesive portion 350 before being compressed by the compression rolls 510, 520.
[0106] As a result, since the first width r1 of the second adhesive portion 350 is smaller than the distance D2 between the end of the separation membrane 210, 250 and the end of the electrode 110, 150, even after the second adhesive portion 350 is compressed by the compression rolls 510, 520, it is possible to prevent a portion of the second adhesive portion 350 from contacting the electrode 110, 150 or from escaping from the end of the separation membrane 210, 250 and leaking to the outside.
[0107] Also, the first adhesive portion 310 and the second adhesive portion 350 may be formed in a pattern including a plurality of dots spaced apart from each other, as shown in Figures 1 and 3. Here, the intervals between the dots may be adjusted to be the same or different as necessary.
[0108] As a result, since the first adhesive portion 310 and the second adhesive portion 350 can be formed in the above-mentioned pattern, when an electrolyte is injected into the electrode assembly 1100 (FIG. 4) including the plurality of unit cells 100, the electrode assembly 1100 (FIG. 4) can be rapidly impregnated. More specifically, since the plurality of dots are spaced apart from each other in the first adhesive portion 310 and the second adhesive portion 350, the electrolyte can flow between the plurality of dots. In other words, the manufacturing time of the battery cell 100 (FIG. 4) can be relatively shortened, and the yield can also be improved.
[0109] The first adhesive portion 310 may obstruct the passage of lithium ions between the electrodes 110, 150 and the separators 210, 250. To prevent this, the first adhesive portion 310 is preferably made of a material that is highly soluble in the electrolyte.
[0110] According to an embodiment of the present invention, the first adhesive portion 310 and the second adhesive portion 350 may include materials having different compositions. For example, the first adhesive composition forming the first adhesive portion 310 may be made of at least one of an Ethylene vinyl acetate (EVA)-based material, an acrylic-based material, and an epoxy-based material, and the second adhesive composition forming the second adhesive portion 350 may be made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material. For example, when the first adhesive composition is made of an acrylic-based material, it can be considered that the acrylic-based material has a certain degree of solubility in the electrolyte because it contains an ester group.
[0111] Thus, compared to the second adhesive composition contained in the second adhesive portion 350, the first adhesive composition contained in the first adhesive portion 310 may be dissolved between the electrodes 110, 150 and the separators 210, 250 when an electrolyte is injected into an electrode assembly 1100 (FIG. 6) including a plurality of unit cells 100. That is, in this case, the first adhesive portion 310 located between the electrodes 110, 150 and the separators 210, 250 may not be dissolved in the electrolyte and may not obstruct the lithium ion passage between the electrodes 110, 150 and the separators 210, 250.
[0112] Here, the dots included in the second adhesive portion 350 may have a diameter smaller than the distance D2 between the ends of the electrodes 110, 150 and the ends of the separators 210, 250. Here, the diameter of the second adhesive portion 350 may be described as the same as the widths r1, r2 of the second adhesive portion 350 described above.
[0113] Referring to FIG. 7, unlike the first adhesive composition included in the first adhesive portion 310 corresponding to position 1, the second adhesive composition included in the second adhesive portion 350 corresponding to position 2 is confirmed to have an oxidation reaction at about 4.0V as a result of Linear Sweep Voltammetry (LSV). This may cause a side reaction in the battery cell, which may shorten the capacity and life. Therefore, it is not preferable to use the second adhesive composition in the first adhesive portion 310. One of the reasons for forming the second adhesive portion 350 is to prevent the separator from breaking during the electrolyte injection process. The result as shown in FIG. 7 may be obtained when at least one of an ethylene-vinyl acetate-based material, an acrylic-based material, and an epoxy-based material is used as the first adhesive composition, and at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material is used as the second adhesive composition.
[0114] The separator according to the embodiment described herein may be a CCS (Ceramic Coated Separator). In general, a separator has a substrate film and a coating layer formed on at least one surface of the substrate film, and the coating layer may include alumina powder and a binder that binds them together. A safety reinforced separator (SRS) has a large amount of binder coated on the surface of the coating layer, but a CCS may not have a binder coated on the surface of the coating layer or may have a much lower binder content distributed on the surface compared to an SRS. For example, in the case of a CCS separator according to the present embodiment, the binder content coated on the surface of the coating layer of the separator may be about 3 wt% or less.
[0115] When the separator is CCS, the internal electrodes included in the electrode assembly are transported in an unfixed state, and therefore the alignment may be disturbed during transport. Of course, when the separator is CCS, it can be fixed by heat and pressure, but the alignment of the internal electrodes may be disturbed during the process of transporting the laminate of the electrodes and separator to a fixing device using heat and pressure after the laminate is formed. In addition, there is a disadvantage that an expensive separator with a high binder content must be used to attach the electrodes and separator using heat and pressure. In contrast, according to the present embodiment, the alignment of the internal electrodes can be prevented from being disturbed during transport while increasing the fixing force.
[0116] FIG. 6 is a top view of a battery cell according to another embodiment of the present invention.
[0117] 2 and 6, a battery cell 1000 according to another embodiment of the present invention includes an electrolyte together with an electrode assembly 1100 in which the unit cells 100 described above are alternately stacked. Here, first electrode tabs 1150 in which the first electrode tabs 115 of the unit cells 100 are stacked and second electrode tabs 1550 in which the second electrode tabs 155 of the unit cells 100 are stacked may be electrically connected to electrode leads 3000, respectively. A lead film 4000 may be located on the upper and / or lower part of the electrode lead 3000.
[0118] Also, the electrode assembly 1100 is installed inside the battery case 120, and the electrode assembly 1100 may be positioned in a recessed receiving portion 2100 together with the electrolyte. Also, the sealing portion 2500 may be formed by sealing the outer circumferential surfaces of the battery case 2000 by heat fusing them together.
[0119] For example, the electrolyte may be at least one of an organic liquid electrolyte, an inorganic liquid electrolyte, a solid polymer electrolyte, a gel polymer electrolyte, a solid inorganic electrolyte, and a molten inorganic electrolyte, but is not limited thereto and may include any commonly used electrolyte.
[0120] The present invention will be described below with reference to more specific examples. However, the following examples are provided to illustrate the present invention and are not intended to limit the scope of the present invention.
[0121] <Experimental Example 1 - Measurement of shear strength, viscosity, and adhesive strength> The adhesive compositions were tested for shear strength, viscosity, and adhesive strength, respectively, for ethylene vinyl acetate (EVA)-based materials, acrylic-based materials, epoxy-based materials, polyolefin-based materials, rubber-based materials, polyamide-based materials, and polyurethane-based materials.
[0122] Here, the acrylic material is BASF's acResin 204UV, the EVA material is Henkel's Technomelt 4046, the epoxy material is Henkel's Lotite EA608, the polyolefin material is Henkel's Supra 502, the rubber material is Henkel's 2802 dispomelt, the polyamide material is Henkel's HPX 002, and the polyurethane material is Fuller's EH9702.
[0123] The shear strength was measured using a universal testing machine (UTM) according to the ASTM D3163 standard, and the results are shown in Table 1.
[0124] The viscosity can be measured at 10 rpm by replacing the spindle part of the Brookfield DV2T LV TJ10 model with a cone and plate and applying a CPA-40Z cone. The results are shown in Table 1.
[0125] The adhesive strength can be measured by applying 15 dots of one of the above adhesive compositions at 3 mm intervals between a pair of tension jigs prepared in advance, and then peeling them vertically. The results are shown in Table 1.
[0126] [Table 1]
[0127] <Example 1> LiNi as the positive electrode active material 0.6 Mn 0.2 Co 0.2 O2, carbon black as a conductive agent, and polyvinylidene fluoride (PVdF) as a binder were used, and the weight ratio of the positive electrode active material:conductive agent:binder was set to 96:2:2, and NMP as a solvent was added to the mixture to prepare a positive electrode active material slurry. The positive electrode active material slurry was applied to an aluminum current collector, which was then dried and rolled to prepare a positive electrode. The thickness of the positive electrode was 200 um.
[0128] Artificial graphite was used as the negative active material, carbon black as the conductive agent, and an SBR emulsion aqueous solution as the binder. The weight ratio of the negative active material:conductive agent:binder was 94:1:5, and water was added to the mixture to prepare a negative active material slurry. The negative active material slurry was applied to a copper current collector, which was then dried and rolled to prepare a negative electrode. The thickness of the negative electrode was 200 um.
[0129] A slurry of Al2O3 and PVDF mixed in a weight ratio of 94:6 was applied to both sides of a polyethylene / polypropylene base sheet (thickness: 10 μm) (thickness: 3 μm each) and dried at 60°C to manufacture a separator. The separator is named upper separator and lower separator according to its position.
[0130] The manufactured lower separator, anode, upper separator, and cathode were alternately stacked in this order, with a first adhesive portion made of acResin 204UV located between the separator and the anode and between the separator and the cathode, and a second adhesive portion made of acResin 204UV located between the upper separator and the lower separator to manufacture a unit cell.
[0131] <Example 2> A unit cell was manufactured in the same manner as in Example 1 except that the second adhesive part was made of a composition consisting of Supra 502.
[0132] <Example 3> In Example 1, the first adhesive part was made of a composition made of Lotite EA608, and the second adhesive part was made of a composition made of Supra 502. Except for this, a unit cell was manufactured in the same manner as in Example 1.
[0133] <Example 4> In Example 1, the first adhesive part was made of a composition made of Technomelt 4046, and the second adhesive part was made of a composition made of Supra 502. Except for this, a unit cell was manufactured in the same manner as in Example 1.
[0134] <Comparative Example 1> In Example 1, the first adhesive part was made of a composition containing Supra 502. Except for this, a unit cell was manufactured in the same manner as in Example 1.
[0135] <Comparative Example 2> A unit cell was manufactured in the same manner as in Example 1, except that the second adhesive portion was not formed between the upper and lower separators.
[0136] <Comparative Example 3> In Example 1, the first adhesive was made of a composition made of 2802 dispomelt, and the second adhesive was not formed between the upper and lower separators. Except for this, a unit cell was manufactured in the same manner as in Example 1.
[0137] <Comparative Example 4> In Example 1, the second adhesive was a composition made of Supra502, and the first adhesive was not formed between the separator and the negative electrode and between the separator and the positive electrode. Except for this, a unit cell was manufactured in the same manner as in Example 1.
[0138] <Comparative Example 5> In Example 1, the second adhesive was made of a composition made of 2802 dispomelt, and the first adhesive was not formed between the separator and the negative electrode and between the separator and the positive electrode. Except for this, a unit cell was manufactured in the same manner as in Example 1.
[0139] <Experimental Example 2 - Measurement of electrode misalignment and adhesive thickness> For each of the unit cells manufactured in Examples 1 to 4 and Comparative Examples 1 to 5, the electrode misalignment was measured at a resolution of 33 um / pixel under conditions of 170 kV, 200 umA, and 34 W using a CT scanner from GE. The results are shown in Table 2.
[0140] In addition, for each of the unit cells manufactured in Examples 1 to 4 and Comparative Examples 1 to 5, the thickness of the first adhesive portion and / or the second adhesive portion was measured after the unit cells were compressed in the up, down and both sides by a compression roll. The results are shown in Table 2.
[0141] [Table 2]
[0142] <Analysis of Experimental Results> Referring to Tables 1 and 2, it can be seen that when a composition consisting of acResin 204UV, Lotite EA608, and Technomelt 4046 is used in the first adhesive portion as in Examples 1 to 4, the problem of electrode slippage does not occur, the thickness of the first adhesive portion is 5% or less of the thickness of the electrode (200 um), and the thickness of the second adhesive portion is approximately equal to or smaller than the thickness of the electrode (200 um). In particular, in the case of Example 1, unlike Examples 2 to 4, it can be seen that a composition consisting of acResin 204UV is used in the second adhesive portion, and both the first adhesive portion and the second adhesive portion have excellent adhesive strength.
[0143] In contrast, when a composition consisting of Supra502 is used in the first adhesive portion as in Comparative Example 1, unlike Examples 1 and 2, the thickness of the first adhesive portion is 25% to 30% of the electrode thickness (200 um), respectively, and it can be confirmed that the thickness of the first adhesive portion appears excessively large.
[0144] This is because Supra502 used in Comparative Example 1 has a higher shear strength and viscosity than acResin 204UV, Lotite EA608, and Technomelt 4046 used in Examples 1 to 4, and therefore the thickness of the first adhesive portion appears to be greater than in Examples 1 to 4. The same can be interpreted for 2802dispomelt, HPX 002, and EH9702, which have higher shear strength than Supra502.
[0145] Therefore, when the first adhesive portion is made of at least one of acrylic, EVA, and epoxy-based materials such as acResin 204UV, Lotite EA608, and Technomelt 4046, the thickness of the first adhesive portion can be very small compared to the electrode thickness (200 um) while eliminating the problem of electrode misalignment.
[0146] In addition, in the case of the second adhesive part, whether it is made of acResin 204UV or Supra502 as in Examples 1 to 4 and Comparative Example 1, it was confirmed that the problem of electrode slippage does not occur, and the thickness of the second adhesive part is approximately equal to or smaller than the thickness of the electrode (200 um). In other words, it was confirmed that the thickness of the second adhesive part after compression is measured almost similarly regardless of the shear strength and viscosity of the composition.
[0147] Thus, the second adhesive portion may be made of at least one of acrylic, EVA, epoxy, polyolefin, rubber, polyamide, and polyurethane-based materials, such as acResin 204UV, Lotite EA608, Technomelt 4046, Supra502, 2802dispomelt, HPX 002, and EH9702.
[0148] However, if the shear strength or viscosity of the second adhesive part is low, when the second adhesive part is left for a long time during the process, a phenomenon may occur in which a part of the second adhesive part comes into contact with the electrode or escapes from the edge of the separator and leaks to the outside.
[0149] Therefore, as in Examples 2 to 4, it is more preferable that the second adhesive portion is made of at least one of polyolefin-based, rubber-based, polyamide-based, and polyurethane-based materials, such as Supra502, 2802dispomelt, HPX 002, and EH9702.
[0150] In addition, in the case of Comparative Examples 2 and 3, where only the first adhesive part is located within the unit cell, it can be seen that, unlike Comparative Example 3, the thickness of the first adhesive part in Comparative Example 2 is similar to that in Examples 1 and 2. However, in both Comparative Examples 2 and 3, an adhesive layer is not formed between the upper and lower separators, which may cause problems such as the separator breaking during additional processes, thereby increasing the defective rate of the electrode.
[0151] In addition, in the case of Comparative Example 4 and Comparative Example 5, when only the second adhesive part is located inside the unit cell, it can be seen that the thickness of the second adhesive part is similar to that of Examples 1 to 4. However, since no adhesive layer is formed between the separator and the positive electrode and between the separator and the negative electrode, there may be a problem of the electrodes being misaligned, which may increase the defective rate of the electrodes.
[0152] As a result, unlike Comparative Examples 2 to 5, in Examples 1 to 4, the first adhesive portion and the second adhesive portion are all contained within the unit cell, so that the first adhesive portion and the second adhesive portion can prevent movement between the electrode and the separation membrane and between the separation membranes, and unlike conventional lamination processes, deformation and damage of the electrode and the separation membrane can be prevented.
[0153] FIG. 8 is a cross-sectional view showing an electrode assembly according to another embodiment of the present invention.
[0154] 8, the electrode assembly 3 according to this embodiment may include an electrode stack 40 manufactured by repeatedly forming the radical units 30 a plurality of times. Here, the radical units 30 may be units in which the separator 322 is folded to have a zigzag pattern to cover the electrode 31, and the electrode 31 and the separator 322 are stacked. That is, the radical units 30 may be units in which the electrode 31 and the separator 322 are stacked in sequence, with one side and the other side of the separator 322 being folded in sequence to cover the electrode 31.
[0155] The electrode assembly 3 may have a fixing tape attached thereto, but instead of the fixing tape, one end of the separator 322 may surround a portion of the outer surface of the electrode stack 40. The basic unit 30 of this embodiment may have the electrodes 3112, 3122 and the separator 322 adhered to each other with an adhesive 34. As a result, the electrodes 3112, 3122 and the separator 322 can maintain their alignment due to the adhesive force of the adhesive 34.
[0156] In the electrode stack 40 of the present embodiment, the separator 322 covers the upper, lower and one side of the electrodes 3112 and 3122, and the stacked alignment state of the radical units 30 can be maintained without the fixing tape. In addition, when the fixing tape is attached to the outside of the electrode stack 40 of the present embodiment or when one end of the separator 322 is surrounded, the stacked alignment state of the radical units 30 can be more stably maintained.
[0157] In addition, in the electrode assembly 3 manufactured in this embodiment, the adhesive 34 may be disposed at the same position between each of the electrodes 3112, 3122 and the separator 322. For example, as shown in Fig. 8, in the electrode assembly 3 of this embodiment, the adhesive 34 disposed between the lower part of the first electrode 3112 and the separator 322 and the adhesive 34 disposed between the upper part of the first electrode 3112 and the separator 322 may be disposed on the same vertical line based on the bottom surface of the first electrode 3112 or the separator 322, respectively, and the intervals at which the adhesives 34 are disposed may be the same. This can be similarly explained in the case of the adhesive 34 disposed between the second electrode 3122 and the separator 322.
[0158] As a result, in the electrode assembly 3 manufactured in this embodiment, the adhesive 34 is disposed at the same position between each of the electrodes 3112, 3122 and the separator 322, which is advantageous in that process time and efficiency can be increased.
[0159] FIG. 9 is a cross-sectional view showing an electrode assembly according to still another embodiment of the present invention.
[0160] 9, in the electrode assembly 4 according to the present embodiment, the adhesive 34 may be disposed between the electrodes 3112, 3122 and the separator 322, and the adhesives 34 disposed in adjacent layers may be disposed in a staggered cross shape. As an example, as shown in FIG. 9, in the electrode assembly 4 according to the present embodiment, the first adhesive 34-1 disposed between the lower part of the first electrode 3112 and the separator 322 and the second adhesive 34-2 disposed between the upper part of the first electrode 3112 and the separator 322 may be disposed in a staggered manner. In this case, the first adhesive 34-1 and the second adhesive 34-2 are merely disposed in a staggered manner, and the intervals at which they are applied may be the same. This can be similarly explained in the case of the adhesive 14 disposed between the second electrode 3122 and the separator 322.
[0161] However, the present invention is not limited thereto, and the structure in which the first adhesive 34-1 and the second adhesive 34-2 are arranged to be offset from each other may be manufactured by applying the adhesive in various ways.
[0162] As a result, in the electrode assembly 4 of the present embodiment, the adhesives 34 are disposed between the electrodes 3112, 3122 and the separator 322, and the adhesives 34 disposed in adjacent layers are staggered, thereby minimizing an increase in the thickness of the electrode assembly 4 due to the adhesives 34. At the same time, since the adhesives 34 disposed in adjacent layers are staggered, the adhesives 34 may be more easily dissolved in the electrolyte contained in the battery cell described above.
[0163] The adhesive 34 used in the electrode assemblies 3 and 4 shown in FIGS. 8 and 9 may use the first adhesive composition contained in the first adhesive portion 310 described above.
[0164] Although the preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto, and various modifications and improvements made by those skilled in the art using the basic concept of the present invention defined in the claims also fall within the scope of the present invention. [Explanation of symbols]
[0165] 100: unit cell 110: 1st electrode 150: 2nd electrode 210: Lower separation membrane 250: Upper separation membrane 310: 1st adhesive part 350:Second adhesive part 510, 520: Pressure roll 600: Coating equipment 1000: Battery cells 1100: Electrode assembly 2000: Battery case 3000: Electrode lead 4000: Lead film
Claims
1. A predetermined number of alternately stacked separators and electrodes; a first adhesive portion located between the separator and the electrode and made of a first adhesive composition; and A second adhesive portion is located between the separation membrane and another separation membrane and is made of a second adhesive composition; The shear strength of the first bonded portion is less than the shear strength of the second bonded portion of the unit cell.
2. A separator and an electrode stacked alternately in a predetermined number; a first adhesive portion located between the separator and the electrode and made of a first adhesive composition; and A second adhesive portion is located between the separation membrane and another separation membrane and is made of a second adhesive composition; the shear strength of the first adhesive portion is equal to or less than the shear strength of the second adhesive portion; The viscosity of the first adhesive portion is equal to or less than the viscosity of the second adhesive portion; The viscosity of the first adhesive portion is 50 cP (at 150° C.) to 120 cP (at 150° C.), The viscosity of the second adhesive portion is 800 cP (at 150° C.) to 12,000 cP (at 150° C.).
3. A separator and an electrode stacked alternately in a predetermined number; a first adhesive portion located between the separator and the electrode and made of a first adhesive composition; and A second adhesive portion is located between the separation membrane and another separation membrane and is made of a second adhesive composition; the shear strength of the first adhesive portion is equal to or less than the shear strength of the second adhesive portion; the thickness of the first adhesive portion is smaller than the thickness of the electrode; the thickness of the second adhesive portion is equal to or smaller than the thickness of the electrode; the thickness of the first adhesive portion is 0.01% or more and 10% or less of the thickness of the electrode, A unit cell, wherein the thickness of the second adhesive portion is 90% or more and 100% or less of the thickness of the electrode.
4. A separator and an electrode stacked alternately in a predetermined number; a first adhesive portion located between the separator and the electrode and made of a first adhesive composition; and A second adhesive portion is located between the separation membrane and another separation membrane and is made of a second adhesive composition; the shear strength of the first adhesive portion is equal to or less than the shear strength of the second adhesive portion; The first adhesive composition is made of at least one of an ethylene vinyl acetate (EVA)-based material, an acrylic-based material, and an epoxy-based material; The second adhesive composition has a unit cell made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
5. A separator and an electrode stacked alternately in a predetermined number; a first adhesive portion located between the separator and the electrode and made of a first adhesive composition; and A second adhesive portion is located between the separation membrane and another separation membrane and is made of a second adhesive composition; the shear strength of the first adhesive portion is equal to or less than the shear strength of the second adhesive portion; The first adhesive portion is a unit cell having a property of being dissolved in an electrolyte.
6. The shear strength of the first adhesive portion is 0.15 MPa or more and 0.5 MPa or less, The unit cell according to claim 2 , wherein the second adhesive portion has a shear strength of 0.15 MPa or more and 3.5 MPa or less.
7. The unit cell according to claim 1 , wherein the second adhesive portion has a shear strength of 1.5 MPa or more and 3.5 MPa or less.
8. 6. The unit cell of claim 1, 3 or 5, wherein the viscosity of the first adhesive is the same as or less than the viscosity of the second adhesive.
9. The viscosity of the first adhesive portion is 50 cP (at 150° C.) to 120 cP (at 150° C.), The unit cell according to claim 8 , wherein the viscosity of the second adhesive portion is 50 cP (at 150° C.) to 12,000 cP (at 150° C.).
10. The unit cell according to claim 9 , wherein the viscosity of the second adhesive portion is 800 cP (at 150° C.) to 12,000 cP (at 150° C.).
11. the thickness of the first adhesive portion is smaller than the thickness of the electrode; The unit cell of claim 1 , 2 , 4 , or 5 , wherein a thickness of the second adhesive portion is equal to or smaller than a thickness of the electrode.
12. the thickness of the first adhesive portion is 0.01% or more and 10% or less of the thickness of the electrode, The unit cell according to claim 11 , wherein the thickness of the second adhesive portion is 90% or more and 100% or less of the thickness of the electrode.
13. The unit cell of claim 1 , wherein an adhesive strength of the first adhesive portion is equal to or greater than an adhesive strength of the second adhesive portion.
14. The adhesive strength of the first adhesive portion is 50 gf / mm 2 More than 100gf / mm 2 is as follows: The adhesive strength of the second adhesive portion is 20 gf / mm 2 More than 100gf / mm 2 14. The unit cell of claim 13, wherein:
15. The unit cell according to claim 1 , wherein the second adhesive portion is located between an end of the separator and an end of the electrode.
16. The unit cell of claim 15 , wherein a width of the second adhesive portion is smaller than a distance between an edge of the separator and an edge of the electrode.
17. The unit cell of claim 15 , wherein the first adhesive portion and the second adhesive portion are each formed in a pattern including a plurality of dots spaced apart from one another.
18. The unit cell of claim 17 , wherein the dots included in the second adhesive portion have a diameter smaller than a distance between an end of the electrode and an end of the separator.
19. The first adhesive composition is made of at least one of an ethylene vinyl acetate (EVA)-based material, an acrylic-based material, and an epoxy-based material; 6. The unit cell of claim 1, wherein the second adhesive composition is made of at least one of an ethylene vinyl acetate (EVA)-based material, an acrylic-based material, an epoxy-based material, a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
20. 20. The unit cell of claim 19, wherein the second adhesive composition comprises at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
21. 6. An electrode assembly formed by alternately stacking the unit cells according to claim 1, The first adhesive portion includes an adhesive pattern disposed at the same position between the electrode and the separator.
22. 6. An electrode assembly formed by alternately stacking the unit cells according to claim 1, The first adhesive portion includes adhesive patterns disposed between the electrodes and the separator in a staggered manner.
23. A battery cell comprising an electrode assembly in which the unit cells according to any one of claims 1 to 4 are alternately stacked, and an electrolyte.
24. The unit cell according to claim 1 , wherein the first adhesive portion has a property of being dissolved in an electrolyte solution.
25. 24. The battery cell of claim 23, wherein the separator is folded to have a zigzag shape.
26. A separator and an electrode stacked alternately in a predetermined number; a first adhesive portion located between the separator and the electrode and made of a first adhesive composition; and A second adhesive portion is located between the separation membrane and another separation membrane and is made of a second adhesive composition; The first adhesive portion has a shear strength equal to or smaller than that of the second adhesive portion, and the electrode assembly includes unit cells alternately stacked together with an electrolyte. The separator is folded to have a zigzag shape.
27. applying a first adhesive to at least one of a first surface of the electrode or a bonding area of a first separator; applying the first adhesive to at least one of a second surface of the electrode or a bonding area of a second separator, the second surface of the electrode being on an opposite side of the electrode from the first surface; applying a second adhesive to at least one of a peripheral region of the first separator or a peripheral region of the second separator; and forming at least a portion of a stack by stacking the electrode between the first separator and the second separator such that a first surface of the electrode contacts a bonding area of the first separator and a second surface of the electrode contacts a bonding area of the second separator; the stack is formed such that peripheral regions of the first and second separators extend outward beyond a periphery of the electrode; The first and second separators face each other in their peripheral regions without an electrode therebetween, The method for manufacturing a unit cell, wherein the first adhesive has a shear strength less than the shear strength of the second adhesive.
28. The method of claim 27, further comprising: applying a first adhesive to at least one of a first surface of the electrode or a bonding area of a first separator; applying the first adhesive to at least one of a second surface of the electrode or a bonding area of a second separator, the second surface of the electrode being on an opposite side of the electrode from the first surface; applying a second adhesive to at least one of a peripheral region of the first separator or a peripheral region of the second separator; and forming at least a portion of a stack by stacking the electrode between the first separator and the second separator such that a first surface of the electrode contacts a bonding area of the first separator and a second surface of the electrode contacts a bonding area of the second separator; the stack is formed such that peripheral regions of the first and second separators extend outward beyond a periphery of the electrode; The first and second separators face each other in their peripheral regions without an electrode therebetween, the shear strength of the first adhesive is equal to or less than the shear strength of the second adhesive; The viscosity of the first adhesive is equal to or less than the viscosity of the second adhesive; The viscosity of the first adhesive is 50 cP (at 150° C.) to 120 cP (at 150° C.), The second adhesive has a viscosity of 800 cP (at 150° C.) to 12,000 cP (at 150° C.).
29. The method of claim 29, further comprising: applying a first adhesive to at least one of a first surface of the electrode or a bonding area of a first separator; applying the first adhesive to at least one of a second surface of the electrode or a bonding area of a second separator, the second surface of the electrode being on an opposite side of the electrode from the first surface; applying a second adhesive to at least one of a peripheral region of the first separator or a peripheral region of the second separator; and forming at least a portion of a stack by stacking the electrode between the first separator and the second separator such that a first surface of the electrode contacts a bonding area of the first separator and a second surface of the electrode contacts a bonding area of the second separator; the stack is formed such that peripheral regions of the first and second separators extend outward beyond a periphery of the electrode; The first and second separators face each other in their peripheral regions without an electrode therebetween, the shear strength of the first adhesive is equal to or less than the shear strength of the second adhesive; the thickness of the first adhesive is less than the thickness of the electrode; the thickness of the second adhesive is equal to or less than the thickness of the electrode; the thickness of the first adhesive is 0.01% to 10% of the thickness of the electrode; A method for manufacturing a unit cell, wherein the thickness of the second adhesive is 90% or more and 100% or less of the thickness of the electrode.
30. The method of claim 30, further comprising: applying a first adhesive to at least one of a first surface of the electrode or a bonding area of a first separator; applying the first adhesive to at least one of a second surface of the electrode or a bonding area of a second separator, the second surface of the electrode being on an opposite side of the electrode from the first surface; applying a second adhesive to at least one of a peripheral region of the first separator or a peripheral region of the second separator; and forming at least a portion of a stack by stacking the electrode between the first separator and the second separator such that a first surface of the electrode contacts a bonding area of the first separator and a second surface of the electrode contacts a bonding area of the second separator; the stack is formed such that peripheral regions of the first and second separators extend outward beyond a periphery of the electrode; The first and second separators face each other in their peripheral regions without an electrode therebetween, the shear strength of the first adhesive is equal to or less than the shear strength of the second adhesive; The first adhesive is made of at least one of an ethylene-vinyl acetate (EVA)-based material, an acrylic-based material, and an epoxy-based material; The second adhesive is made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
31. The method of claim 30, further comprising: applying a first adhesive to at least one of a first surface of the electrode or a bonding area of a first separator; applying the first adhesive to at least one of a second surface of the electrode or a bonding area of a second separator, the second surface of the electrode being on an opposite side of the electrode from the first surface; applying a second adhesive to at least one of a peripheral region of the first separator or a peripheral region of the second separator; and forming at least a portion of a stack by stacking the electrode between the first separator and the second separator such that a first surface of the electrode contacts a bonding area of the first separator and a second surface of the electrode contacts a bonding area of the second separator; the stack is formed such that peripheral regions of the first and second separators extend outward beyond a periphery of the electrode; The first and second separators face each other in their peripheral regions without an electrode therebetween, the shear strength of the first adhesive is equal to or less than the shear strength of the second adhesive; The first adhesive has a property of being dissolved in an electrolyte.
32. 32. The method of claim 27, further comprising compressing the stack along a direction perpendicular to the first surface of the electrode and the second surface of the electrode.
33. 32. The method for producing a unit cell according to any one of claims 27 to 31, further comprising the step of disposing the stack and an electrolyte in a battery case.
34. 32. The method for manufacturing a unit cell according to claim 27, wherein the peripheral regions of the first and second isolation membranes extend around the periphery of the first and second isolation membranes, respectively, such that each of the peripheral regions surrounds a bonding region of each of the first and second isolation membranes.
35. 32. The method for manufacturing a unit cell according to claim 28, wherein the first adhesive has a shear strength of 0.15 MPa or more and 0.5 MPa or less, and the second adhesive has a shear strength of 0.15 MPa or more and 3.5 MPa or less.
36. The method for manufacturing a unit cell according to claim 28 , wherein the second adhesive has a shear strength of 1.5 MPa or more and 3.5 MPa or less.
37. The method for manufacturing a unit cell according to any one of claims 27 and 29 to 31, wherein the viscosity of the first adhesive is equal to or lower than the viscosity of the second adhesive.
38. The viscosity of the first adhesive is 50 cP (at 150° C.) to 120 cP (at 150° C.), The method for manufacturing a unit cell according to claim 37, wherein the viscosity of the second adhesive is 50 cP (at 150° C.) to 12,000 cP (at 150° C.).
39. The method for manufacturing a unit cell according to claim 38, wherein the viscosity of the second adhesive is 800 cP (at 150° C.) to 12,000 cP (at 150° C.).
40. the thickness of the first adhesive is less than the thickness of the electrode; 32. The method for manufacturing a unit cell according to claim 27, 28, 30, or 31, wherein the thickness of the second adhesive is equal to or smaller than the thickness of the electrode.
41. the thickness of the first adhesive is 0.01% to 10% of the thickness of the electrode; The method for manufacturing a unit cell according to claim 40, wherein a thickness of the second adhesive is 90% or more and 100% or less of a thickness of the electrode.
42. 32. The method for manufacturing a unit cell according to claim 27, wherein an adhesive strength of the first adhesive is equal to or greater than an adhesive strength of the second adhesive.
43. The adhesive strength of the first adhesive is 50 gf / mm 2 More than 100gf / mm 2 is as follows: The adhesive strength of the second adhesive is 20 gf / mm 2 More than 100gf / mm 2 43. The method of claim 42, wherein:
44. 32. The method of claim 27, wherein a width of the second adhesive applied to the peripheral regions of the first and second separators is smaller than a width of the peripheral regions to which the second adhesive is applied.
45. 32. The method of claim 27, wherein the first adhesive and the second adhesive are applied in respective dot patterns spaced apart from one another.
46. 46. The method of claim 45, wherein each dot in the dot pattern of the second adhesive has a diameter smaller than a width of a peripheral region of each of the first and second separators.
47. 46. The method of claim 45, wherein the dot pattern of the first adhesive is arranged in a grid of rows and columns.
48. 32. The method of claim 27, wherein the first adhesive is made of at least one of an EVA-based material, an acrylic-based material, and an epoxy-based material, and the second adhesive is made of at least one of an EVA-based material, an acrylic-based material, an epoxy-based material, a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
49. 49. The method of claim 48, wherein the second adhesive is made of at least one of a polyolefin-based material, a rubber-based material, a polyamide-based material, and a polyurethane-based material.
Citation Information
Patent Citations
Packaged positive electrode plate, laminated electrode body, electric storage element, and method of manufacturing packaged positive electrode plate
JP2018152226A
Laminated electrode body and power storage element
JP2019053862A
Electrode body and power storage element
JP2019091581A