Lithium ion conductive composite material comprising at least one polymer and lithium ion conductive particles, and method for producing a lithium ion conductor from said composite material

A lithium ion conductive composite material with spherical particles and controlled polydispersity index addresses the challenge of high particle filling and manufacturing complexity, resulting in enhanced lithium ion conductivity and improved battery performance.

JP7572141B2Active Publication Date: 2024-10-23SCHOTT AG
View PDF 22 Cites 0 Cited by

Patent Information

Application Number
JP2018226845
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2017-12-04
Filing Date
2018-12-03
Publication Date
2024-10-23
Estimated Expiration
2038-12-03

AI Technical Summary

Technical Problem

Existing lithium ion conductive materials face challenges in achieving high particle filling degrees while being economically manufacturable, and the production methods often require complex and costly processes that can lead to materials with low sphericity and poor handling properties.

Method used

A lithium ion conductive composite material comprising spherical particles with a sphericity of at least 0.7 and controlled polydispersity index, allowing for higher volume percentages of particle filling, which can be produced through methods like spray calcination, filamentation of molten salts, or dropletization, and subsequently sintered under elevated temperatures and pressures.

Benefits of technology

The composite material achieves significantly higher particle packing densities, reducing interfacial resistance and enhancing lithium ion conductivity, making it suitable for use in hybrid electrolytes and solid-state batteries with improved safety and performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572141000001
    Figure 0007572141000001
  • Figure 0007572141000002
    Figure 0007572141000002
  • Figure 0007572141000003
    Figure 0007572141000003
Patent Text Reader

Abstract

To provide a lithium ion conductive composite material having practically higher particle filling degree than one conventionally capable of being used, and containing at least one polymer and lithium ion conductive particle.SOLUTION: The problem is solved by a lithium ion conductive composite material containing at least one polymer and lithium ion conducive particle, the particle has spheroidicity Ψ of at least 0.7, the composite material contains at least 20 vol.% of particle when polydispersity index PI of particle diameter distribution is less than 0.7, or the composite material contains at least 30 vol.% of particles when the polydispersity index PI of particle diameter distribution is in a range of 0.7 to less than 1.2, or the composite material contains at least 40 vol.% of particle when the polydispersity index PI of particle diameter distribution is over 1.2.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a lithium ion conducting composite material comprising at least one polymer and lithium ion conducting particles, and to a method for producing a lithium ion conductor from said composite material. [Background technology]

[0002] In recent years, lithium-ion batteries and lithium batteries have become increasingly important, especially for electronic components or in the field of electric vehicles, due in particular to their high energy density, lack of memory effect and very slow voltage drop. Lithium-ion batteries and lithium batteries are generally a family of rechargeable battery types (also called secondary battery types) that are used as storage media for the above-mentioned fields.

[0003] Lithium-ion or lithium batteries essentially consist of three main structural units: an anode (negative electrode), a cathode (positive electrode) and a non-aqueous electrolyte located between the electrodes, which provides for the transfer of lithium ions during operation (charging or discharging). In lithium-ion batteries, the anode is usually based on graphite, into which lithium ions are inserted during charging and from which they are extracted during discharging. In contrast, in lithium batteries, elemental lithium is used as the anode.

[0004] Currently, commercially available lithium-ion batteries mainly use electrolytes in which lithium salts are dissolved in organic solvents, but these batteries have the disadvantage that they can self-destruct and, in extreme cases, catch fire when used incorrectly or overloaded.

[0005] In order to solve these problems, in recent years, so-called lithium solid-state batteries have been investigated in particular, in which the liquid electrolyte matrix based on organic matter is replaced by a solid that also conducts lithium ions. In this case, the solid electrolyte can generally be used in various positions in the battery system, on the one hand, as a separator, the use of a pure solid electrolyte introduced between the electrodes to protect against undesired short circuits and thus ensure the functionality of the entire system is conceivable. For this purpose, the solid electrolyte can be incorporated into the battery either as a layer on one or both electrodes or as a free-standing membrane. On the other hand, it is conceivable to blend it with the electrode active material. In this case, the solid electrolyte provides for the transport of the relevant charge carriers (lithium ions and electrons) to and from the electrode material and the conductive electrode, depending on whether the battery is discharged or charged.

[0006] In principle, the solid electrolyte can be a polymer electrolyte or a polyelectrolyte. In the first case, similar to liquid electrolytes, a lithium-based supporting salt is dissolved in a solid polymer matrix (polyethylene oxide is often used for this). The second one is a polymeric polyfunctional lithium salt. Both electrolytes, polymer electrolytes and polyelectrolytes, similar to liquid-based electrolytes, usually have insufficient chemical and electrochemical stability with respect to elemental lithium and are therefore rather unsuitable for use in lithium batteries. However, alternatively, it is also conceivable to use purely inorganic solid ion conductors as a replacement for the conventionally used organic-based liquid electrolytes. In terms of lithium ion conductivity, oxide-based (e.g. lithium-conducting mixed oxides with garnet-type structure), phosphate-based and sulfide-based lithium ion conducting materials are discussed as being particularly promising. Certain embodiments of them have sufficient chemical and electrochemical stability with respect to elemental lithium. They are therefore suitable for use in lithium batteries. However, this is not the case for other representatives from the class of purely inorganic solid ion conductors. Therefore, in any case, the suitability of the corresponding material as a solid electrolyte in a lithium battery must be verified individually in each individual case. A third embodiment for lithium conductive solids is the so-called hybrid electrolyte, which is a composite material in which particles made of inorganic lithium ion conductive materials are incorporated into a lithium conductive polymer matrix consisting of a polymer electrolyte or polyelectrolyte. Certain hybrid electrolyte embodiments also show sufficient chemical and electrochemical stability with respect to elemental lithium and have the ability to be used in lithium batteries.

[0007] Among the purely inorganic lithium-ion conducting solid electrolytes, the sulfide compositions Li-SP and Li2S-P2S5-P2O5 are sometimes produced by grinding the starting materials under protective gas and subsequent temperature treatment (also usually under protective gas). The production of Li-PS glass ceramics is described in US20050107239 A1, US2009159839 A, and JP2008-120666. Li2S-P2S5-P2O5 can be produced either via a grinding process or via melting, as described in A.Hayashi et al., Journal of Non-Crystalline Solids 355(2009)1919-1923. Glass ceramics in the system Li2S-B2S3-Li4SiO4 can also be produced via the melt route and subsequent quenching, but this process step must be carried out in the absence of air (see US2009011339 A and Y. Seino et al., Solid State Ionics 177 (2006) 2601-2603). The achievable lithium ion conductivity is 2×10 at room temperature. -4 ~6×10 -3 S / cm. It should be noted that in the case of sulfide lithium ion conducting solid electrolytes, production under protective gas and possibly laborious grinding can make their production expensive. Moreover, handling and storage under protective gas or at least in an anhydrous environment in many cases can also be disadvantageous for the production of lithium batteries in certain environments.

[0008] In contrast, solid lithium ion conductors based on oxides are characterized by easier, and thus more convenient, manufacturing and higher chemical stability. Phosphate-based compositions having a crystal layer, which have a crystal structure similar to NASICON (sodium superionic conductor), are mainly known. Generally, this is a glass-ceramic, in which case the starting glass is first melted and then hot-formed (e.g., cast). The starting glass is ceramized in a second step, either directly (“bulk glass-ceramic”) or as a powder (“sintered glass-ceramic”). During ceramization, controlled crystallization can be carried out according to appropriately selected temperature and time, which enables adjustment of the structure of the glass-ceramic optimized for lithium ion conductivity. Thereby, an improvement in conductivity on the order of more than 10 times can be achieved. The document of U.S. Patent Application Publication No. 2003 / 0205467 (US20030205467 A1) describes the production of a glass-ceramic having a main crystal phase Li (1+x) (Al,Ga) x Ti (2-x) (PO4)3(0 < x ≦ 0.8). After crystallization, an ionic conductivity of 0.6 to 1.5×10 -3 S / cm was achieved. The starting glass is very sensitive to crystallization and must be quenched on a metal plate to avoid uncontrolled crystallization. This limits the possibility of forming and the control of the structure in the glass-ceramic.

[0009] In the documents of U.S. Patent No. 6030909 (US6030909) and U.S. Patent No. 6485622 (US6485622), GeO2 and ZrO2 are further introduced into the glass-ceramic. GeO2 broadens the vitrification region and reduces the crystallization tendency. However, in practice, this beneficial effect is limited by the high raw material price of germanium. In contrast, ZrO2 brings about enhanced crystallization. The starting glasses cited in these documents have a tendency for uncontrolled crystallization, and usually, quenching must be carried out to obtain a suitable starting glass.

[0010] Xu et al., in Electrochem. Commun., 6(2004)1233-1237, or in Materials Letters, 58(2004),3428-3431, also reported a 5.7×10 -4 ~6.8×10 -4 describes Li2O-Cr2O3-P2O5 glass ceramics with high conductivity of 1.0 S / cm. However, these starting glasses also have to be quenched due to a strong tendency to crystallize.

[0011] Glass-ceramics containing Fe2O3 have also been described (K. Nagamine et al., Solid State Ionics, 179(2008)508-515). Here, 3×10 -6 Ion conductivity of 1000 S / cm was found. However, the use of iron (or other polyvalent elements) often leads to the appearance of electronic conductivity, which must be avoided in solid electrolytes. Therefore, according to JP2008047412 A, this glass ceramic is preferably used as a cathode material, since electronic conductivity is desired here to facilitate the contact of the cathode.

[0012] US2014 / 0057162 A1 discloses a lithium ion conductive phosphate-based glass ceramic having a conductivity of at least 5×10 -7It describes a glass ceramic having an ionic conductivity of 0.1 S / cm and which can be produced by casting from the melt without the need for quenching, since the starting glass has sufficient crystallization stability. Moreover, both the glass ceramic and the starting glass have sufficient chemical stability in air, so that storage is possible. This is made possible by the fact that the corresponding phosphate-based glass ceramic contains Ta2O5 and / or Nb2O5. Ta2O5 and Nb2O5 can improve the crystallization stability of the glass, since they can likewise be incorporated into the crystalline phase and, by increasing the proportion of the crystalline phase, can positively affect the ionic conductivity.

[0013] Oxide-based inorganic solid ion conductor substances which are of particular importance due to their high lithium ion conductivity are lithium-containing mixed oxides with a garnet-type structure, for example those described in the document DE 102007030604 A1. In this connection, materials containing zirconium and lanthanum have particularly good conductivity, which in their simplest form have the formula Li7La3Zr2O 12 The compound or compounds derived therefrom are often referred to as LLZO for short. The garnet occurs in two modifications, the tetragonal and the cubic modification. The cubic modification of LLZO is particularly important for lithium solid-state batteries, since it has a high lithium ion conductivity. Further investigations of LLZO have shown that the formation of the cubic modification of LLZO can be stabilized, especially by adding further doping metals, for example aluminum. In the scope of this application, non-doped or doped lithium lanthanum zirconium oxide, or compounds derived therefrom, are generally referred to as LLZO. In the past, LLZO has been proven to be chemically and electrochemically stable with respect to elemental lithium, which is used as an anode in lithium batteries, and therefore has great potential for use as an electrolyte in the corresponding systems.

[0014] Many methods are mentioned in the literature for producing LLZO, for example the so-called solid-state method for producing LLZO is known, for example described in US 2010 / 047696 A1 or US 2010 / 0203383 A1. In the method described in the last-mentioned document, the starting material, optionally pre-dried for 12 hours at temperatures up to 900 ° C, is ground in a ball mill and then heated for 12 hours at temperatures between 900 and 1125 ° C, and the product obtained is ground again in a ball mill. The powder obtained is subsequently isostatically pressed and calcined again for 36 hours at a temperature in the range of 1230 ° C. As an alternative to the solid-state method, attempts have been made to produce precursors using sol-gel methods, which can be further processed to the desired crystalline mixed oxides with a garnet-type structure. Such a method is sometimes also referred to as the Pechini method and is described, for example, in Y. Shimonishi et al, Solid State Ionics 183 (2011) 48-53. In this case, lithium, lanthanum and zirconium are used in the form of their nitrates and are heated together in a mixture of water, citric acid and ethylene glycol, during which a black solid is formed, which then has to be heat-treated again at 350 ° C for 5 hours, after which an intermediate product in powder form is obtained, which can then be further processed into the desired final product. DE102013101145 A1 and DE102013224045 A1 describe the preparation of LLZO crystallizing into cubic or tetragonal crystals via a sol-gel process, in some cases starting from alcohol and in some cases from an aqueous sol. A further sol-gel method for producing amorphous LLZO is known from US 2011 / 0053001 A1.

[0015] DE 102014116378 A1 discloses the production of LLZO in the form of a glass ceramic. Glass ceramic is understood to mean a material produced by melting techniques, as described above for phosphate-based solid lithium-ion conductors, and subsequently converted into a glass ceramic. The glass ceramic contains an amorphous fraction of at least 5% by weight. The amorphous fraction has a positive influence on the conductivity. However, the fraction of amorphous phase should not exceed 40% by weight, preferably not exceed 30% by weight, since otherwise the overall conductivity would decrease. A further advantage of the production as a glass ceramic is that its structure can be directly influenced by controlled crystallization, which can further positively influence the conductivity. The glass ceramics described in DE 102014116378 A1 advantageously have a crystallinity of at least 5×10 -5 S / cm, preferably at least 1×10 -4 S / cm. In some cases the ionic conductivity can be significantly higher. [Prior art documents] [Patent documents]

[0016] [Patent Document 1] US Patent Application Publication No. 2005 / 0107239 [Patent Document 2] US Patent Application Publication No. 2009 / 159839 [Patent Document 3] JP 2008-120666 A [Patent Document 4] US Patent Application Publication No. 2009 / 011339 [Patent Document 5] US Patent Application Publication No. 2003 / 0205467 [Patent Document 6] U.S. Patent No. 6,030,909 [Patent Document 7] U.S. Patent No. 6,485,622 [Patent Document 8] JP 2008-047412 A [Patent Document 9] US Patent Application Publication No. 2014 / 0057162 [Patent Document 10] DE 102007030604 [Patent Document 11] US Patent Application Publication No. 2010 / 047696 [Patent Document 12] US Patent Application Publication No. 2010 / 0203383 [Patent Document 13] DE 102013101145 A1 [Patent Document 14] DE 102013224045 A1 [Patent Document 15] US Patent Application Publication No. 2011 / 0053001 [Patent Document 16] DE 102014116378 [Non-patent literature]

[0017] [Non-Patent Document 1] A. Hayashi et al., Journal of Non-Crystalline Solids 355(2009)1919-1923 [Non-Patent Document 2] Y.Seino et al., Solid State Ionics 177(2006)2601-2603 [Non-Patent Document 3] Xu et.al., Electrochem. Commun., 6(2004)1233-1237 [Non-Patent Document 4] Xu et.al., Materials Letters, 58(2004),3428-3431 [Non-Patent Document 5] K. Nagamine et al., Solid State Ionics, 179(2008)508-515 [Non-Patent Document 6] Y.Shimonishi et al, Solid State Ionics 183(2011)48-53 Summary of the Invention [Problem to be solved by the invention]

[0018] The object of the present invention is to provide a lithium ion conducting composite material comprising at least one polymer and lithium ion conducting particles, which should have a substantially higher particle loading than previously achievable. It should be easily and economically manufacturable. Furthermore, the object of the present invention is to find a method for producing a lithium ion conductor from said composite material. [Means for solving the problem]

[0019] The object of the present invention is to provide a lithium ion conductive composite material comprising at least one polymer and lithium ion conductive particles, the particles have a sphericity Ψ of at least 0.7, and the composite material contains at least 20% by volume of the particles with a particle size distribution polydispersity index PI of less than 0.7; or the composite material contains at least 30% by volume of the particles with a particle size distribution polydispersity index PI in the range of 0.7 to less than 1.2; or The composite material contains at least 40% by volume of the particles with a polydispersity index PI of particle size distribution greater than 1.2. The lithium ion conductive composite material solves this problem.

[0020] Here, the sphericity Ψ is a parameter that indicates how spherical a particle is. According to the definition by H. Wadell, the sphericity Ψ of a particle is calculated as the ratio of the surface area of ​​a sphere of equal volume to the surface area of ​​the particle:

number

[0021] Typical sphericity Ψ for different types of particles are: Sphere: 1.0 Droplets, bubbles, round particles: 0.7-1.0 Angular grain: 0.45~0.6 Acicular particles: 0.2~0.45 Platelet: 0.06~0.16 Particles with very rough surfaces: 10 -8 ~10 -4

[0022] In the context of the present invention, high sphericity Ψ is achieved when Ψ has a value of at least 0.7.

[0023] In the context of the present invention, the polydispersity index PI of a particle size distribution is the d 90 Value and d 10 It is understood as the base 10 logarithm of the quotient from the value: PI = log(d 90 / d 10 )

[0024] Generally, higher particle packing can be achieved in composites and composite precursors when the particle size distribution is broader, ie, when the polydispersity index PI has a higher value.

[0025] d value for determining PI, especially d 90 value and d 10 Value definitions The particles of a powder are generally distinguished by their equivalent spherical diameter, which is to be measured, regardless of their sphericity Ψ, and are divided into selected classes according to their size. To describe the particle size distribution, the proportion of each particle class present in the powder is measured.

[0026] Here, different quantity types are used: if particles are counted, the quantity type is number, whereas in the case of metric it is mass, and in the case of uniform density ρ it is volume, as well as from length, projection and surface.

[0027] A distinction is made between: Quantity type: Index: Number 0 Length 1 area 2 Volume (mass) 3

[0028] The conventional quantitative means for describing particle size distribution in powders is the cumulative distribution Q r The index r indicates the type of quantity according to the table above.

[0029] Cumulative distribution function Q r (d) denotes the normalized mass of all particles with an equivalent diameter less than or equal to d. Below we explicitly define the cumulative distributions of the two most conventional mass types: · Number of particles (r=0) N i is the diameter under consideration, d i Let N be the number of all particles examined that have a diameter d such that N is the total number of all particles examined, where

number

number

[0030] In the present invention, i The value is Q3(d i ) is understood to be the equivalent diameter value whose cumulative distribution function takes the following values: d 10 : Q3(d 10) = 10%, i.e., 10% by mass of the particles are d 10 having a diameter of d 50 : Q3(d 50 ) = 50%, i.e., 50% of the particles are d 50 having a diameter of d 90 : Q3(d 90 )=90%, i.e., 90% of the particles are d 90 having a diameter of d 99 : Q3(d 99 ) = 99%, i.e., 99% of the particles are d 99 having a diameter of d 100 : Q3(d 100 ) = 100%, that is, 100% of the particles are d 100 It has the following diameter:

[0031] In the context of this application, the term polydispersity index can be understood synonymously with the term polydispersity index.

[0032] The composite material according to the invention can a) in one embodiment be used directly as a lithium ion conductor or b) in a further embodiment be used as an intermediate product for further processing into a lithium ion conductor.

[0033] Surprisingly, it has been found that a substantially higher particle packing degree can be achieved with particles having a sphericity Ψ of at least 0.7.Thus, a composite material according to the present invention is available which contains at least 20% by volume of said particles when the polydispersity index PI of the particle size distribution has a value less than 0.7, or at least 30% by volume of said particles when the polydispersity index PI of the particle size distribution has a value equal to or greater than 0.7 and less than 1.2, or at least 40% by volume of said particles when the polydispersity index PI of the particle size distribution has a value equal to or greater than 1.2.

[0034] In a particularly preferred embodiment of the invention, the particles have a sphericity Ψ of at least 0.8, particularly preferably at least 0.9.

[0035] In a further embodiment, the composite material preferably contains at least 25 vol.-% of the particles, and particularly preferably at least 30 vol.-% of the particles, when the polydispersity index PI of the particle size distribution has a value of less than 0.7, preferably contains at least 35 vol.-% of the particles, and particularly preferably contains at least 40 vol.-% of the particles, when the polydispersity index PI of the particle size distribution has a value of 0.7 or more and less than 1.2, or preferably contains at least 45 vol.-% of the particles, and particularly preferably contains at least 50 vol.-% of the particles, when the polydispersity index PI of the particle size distribution has a value of 1.2 or more.

[0036] Preferably, the polymer comprises at least one of the following compounds: Polyethylene oxide Polyethylene oxide derivatives Polyvinyl butyral.

[0037] Furthermore, the use of the following polymers is contemplated: polyacrylonitrile, polyesters, polypropylene oxide, ethylene oxide / propylene oxide copolymers, polyethylene oxide crosslinked with trifunctional urethanes, poly(bis(methoxy-ethoxy-ethoxide))phosphazene (MEEP), triol-type polyethylene oxide crosslinked with difunctional urethanes, poly((oligo)oxyethylene)methacrylate-co-alkali metal methacrylates, polymethyl methacrylate (PMMA), polymethylacrylonitrile (PMAN), polysiloxanes and their copolymers and derivatives, polyvinylidene fluoride or polyvinylidene chloride and their copolymers and derivatives, poly(chlorotrifluoroethylene), poly(ethylene-chlorotrifluoroethylene), poly(fluorinated ethylene-propylene), acrylate-based polymers, condensed or crosslinked combinations thereof, and / or physical mixtures thereof.

[0038] The polymer may contain at least one lithium ion conducting compound, in particular lithium bistrifluoromethanesulfonimidate, as lithium ion conducting compound.

[0039] Further usable supporting salts include LiAsF6, LiClO4, LiSbF6, LiPtCl6, LiAlCl4, LiGaCl4, LiSCN, LiAlO4, LiCF3CF2SO3, Li(CF3)SO3(LiTf), LiC(SO2CF3)3, phosphate-based lithium salts, preferably LiPF6, LiPF3(CF3)3(LiFAP) and LiPF4(C2O4)(LiTFOB), borate-based lithium salts, preferably LiBF4, LiB(C2O4)2(LiBOB), LiBF2(C2O4)(LiDFOB), LiB(C2O4)(C3O4)(LiMOB), Li(C2F5BF3)(LiFAB) and Li2B 12 F 12 (LiDFB), and / or lithium salts of sulfonylimides, preferably LiN(FSO2)2 (LiFSI), LiN(SO2CF3)2 (LiTFSI) and / or LiN(SO2C2F5)2 (LiBETI), are considered.

[0040] In addition to the above polymer electrolytes, alternative polyelectrolytes can also be used. + as counter ions, e.g. polystyrene sulfonate (PSS), or polymerized ionic liquids based on imidazolium, pyridinium, phosphonium or guanidinium, which have a discrete number of chemically bound ionic groups and are therefore inherently lithium ion conductive.

[0041] The lithium ion conductive particles are preferably made from at least one lithium ion conductive compound, in particular at least the following lithium ion conductive compounds: Lithium lanthanum zirconate (LLZO) Lithium Aluminum Titanium Phosphate (LATP) Compounds having a garnet-type crystal structure, in particular those having the empirical formula Li 7+x-y M x II M 3-x III M 2-y IV M y V O 12 [In the above formula, M II is a divalent cation, M III is a trivalent cation, M IV is a tetravalent cation, M V is a pentavalent cation, where: Advantageously, 0≦x<3, more preferably 0≦x≦2, 0≦y<2, and particularly preferably 0≦y≦1. or compounds derived therefrom, in particular compounds doped with Al, Nb or Ta, Compounds with the same crystal structure as NaSICon, especially those with the empirical formula Li 1+x-y M 5+ y M 3+ x M 4+ 2-x-y (PO4)3 [In the above formula, x and y are in the range of 0 to 1 and (1+xy)>1; and M is a +3, +4, or +5 cation. or a compound derived therefrom It consists of:

[0042] The particles preferably have an average particle size in the range of 0.02 μm to 100 μm. The two ranges 0.2 μm to 2 μm and 5 μm to 70 μm are also particularly preferred. One of the two ranges 0.2 μm to 2 μm or 5 μm to 70 μm is also particularly preferred.

[0043] In a further preferred embodiment, in the case of the lithium ion conductive composite material, the interfacial resistance for lithium ion conductivity between the polymer and the particles is reduced due to surface modification of the particles, and thus the lithium ion conductivity is higher than in the case of a comparable composite material in which the interfacial resistance between the polymer and the particles is not reduced.

[0044] Preferably, the particles are produced using at least one of the following methods: Spray calcination (especially using pulse reactor technology) Filamentation from molten salts · Dropletization Glass sphere manufacturing.

[0045] Regardless of whether the purely inorganic solid lithium-ion conductor is oxide-, phosphate- or sulfide-based, what is common to all of the production methods described so far in the prior art is that the lithium-ion conductive material obtained in the respective step occurs either in a monolithic structure or at least in an undefined coarse-grained structure and must be brought into the final application form as a powder with a defined particle size and particle size distribution by a further refinement step, usually a milling step. In many cases, the particle size to be achieved is in the μm range or in the sub-μm range. Only then can further processing be made possible. This includes, in particular, on the one hand, the incorporation of the hybrid electrolyte into a polymer, polymer electrolyte or polyelectrolyte for the final production. On the other hand, this includes further processing in a compaction or incorporation into a ceramic slurry and a molding step (e.g. tape casting) to form a ceramic green body which is finally converted into a ceramic component made of the purely inorganic solid ion conductor by sintering.

[0046] By means of a comminution process, such as the milling process described above, it is practically not possible to produce spherical powder particles, but rather fragmentary particles with corners and edges are formed, which therefore have a sphericity significantly below 0.7.

[0047] Non-spherical particles of one and the same material are significantly more difficult to process in many applications than their spherical counterparts, given the same particle size and particle size distribution. This is especially true when incorporated into thermoplastic matrices (for example, when producing hybrid electrolytes) and liquid matrices (for example, relevant when producing ceramic slurries). For the same volumetric filling degree, with comparable particle size or particle size distribution, the viscosity of a particle-filled formulation is significantly higher when non-spherical particles are used than when spherical particles of the same material are used. Conversely, in the case of spherical embodiments, the corresponding formulation can have a significantly higher filling degree than in the case of non-spherical embodiments. This is due to the fact that in formulations filled with non-spherical particles, the particles tend to catch on each other when passing each other in the formulation due to the effect of external shear forces, which increases the internal friction. In contrast, in the case of spherical particles, they can pass each other better.

[0048] When using spherical particles, it is indeed very important that the formulation filled with them achieves a significantly higher volumetric filling degree under comparable prerequisites, for example, a significantly better lithium-ion conductivity can be achieved by increasing the incorporation of inorganic solid electrolytes consisting of spherical particles in hybrid electrolytes, since the lithium-ion conductivity of the inorganic components is usually higher than that of the polymer-based matrix. The ceramic slurry remains pourable even at a relatively high degree of filling when spherical particles are used in the formulation. The green body resulting after drying of the solvent still has a significantly lower porosity, which leads to significantly less shrinkage during the final sintering stage. Artifacts often associated with sintering shrinkage (such as crack formation) can thus be significantly reduced by their action.

[0049] Therefore, in view of the prior art, there is a need for a lithium ion conducting solid electrolyte material in powder form consisting of microscale or sub-microscale particles and having a high sphericity Ψ.

[0050] For example, the following methods can be mentioned: Production of glass spheres: The route for producing particles from lithium-ion conductive materials makes use of the fact that these materials can also be produced, inter alia, via the glass-ceramic route. For this, in conventional melting processes, ideally crystal-free green glass is first melted and then ceramified during a subsequent heating step, converting it into the actual glass-ceramic. In principle, the glass melt used in the first process step can be subjected, upon cooling, to a conventional thermoforming step used for the production of glass spheres. For this, the following method approaches are conceivable: The method disclosed in US Pat. No. 3,499,745 impinges a molten glass jet on a striking wheel, which, if a sufficiently large force is generated, leads to the breakup of the glass jet into partial strands, so-called filaments. This is then first passed through a heated zone, a cooling zone and finally discharged into a collection zone. After the formation of the filaments, the tendency to minimize surface tension comes into play, so that the filaments become rounded. According to EP 1 135 343 B1, sufficient sphericity is then reached once a relaxation time T has elapsed from the time of filament formation, which can be described by the formula T = (d x μ) / σ, where d is the diameter of the sphere formed, μ is the viscosity of the filament, and σ is the surface tension of the filament during the relaxation time. Instead of a striking wheel, a rotor can also be used, as described in US 3 495 961. Other known methods for the production of glass spheres include expanding a combustion gas stream through a molten glass stream to break the glass into individual particles. Such a method is disclosed in US 3 279 905. Alternatively to this, glass particles with a relatively low sphericity can be (partially) remelted and rounded by bringing them into a flame, as described, for example, in DD 282 675 A5.

[0051] Filamentation of molten salt: Analogous to the above-mentioned filament formation and the subsequent formation of spherical droplets from a molten glass jet due to relaxation effects that reduce the surface energy, this can be done correspondingly from a jet of material originating from molten salt. For this, one can proceed in a similar manner technically, with the caveat that the viscosity of the molten glass can differ significantly from that of the molten salt, depending on the temperature selected in each case. The droplet-like material must first be converted into a preceramic intermediate stage, often porous but form-stable except for isotropic shrinkage, by passing it through a hotter zone, and then subsequently converted into the actual solid lithium-ion conductor, either at that stage or in another additional subsequent heating stage. Ideally, dense sintered spheres of solid lithium-ion conductor material are thus obtained.

[0052] Spray calcination (using pulse reactor technology): When using a pulse reactor, as disclosed in DE10111938 A1, DE102006027133 A1, DE102006039462 A1 or EP1927394 A1, a gaseous or liquid mixture in the form of a solution, suspension or dispersion containing all the components for producing a lithium-ion conductive material is brought into a pulsed hot gas stream, in the latter case by fine atomization. In this case, the pulsed hot gas stream is itself generated in the hot gas generator of the reactor by burning natural gas or hydrogen together with the surrounding air. The prevailing temperature there is 500-1500 ° C depending on the choice of the position of the spray introduction point. In the pulsating hot gas stream, intermediate products are formed, which are converted into their final form by further thermal post-treatment in the same or another reactor. In the former case, the reactor can be equipped with an additional fuel supply, which follows the spray introduction point along the pulsating hot gas stream.

[0053] Dropletization method: In the dropletization method, you start with an aqueous or solvent-based salt solution or sol as precursor for the lithium-ion conducting material or with a nanoparticle solution of the lithium-ion conducting material, which is converted into droplets via a suitable nozzle device. After formation, the droplets are optionally dried directly in a suitable process gas stream, for example as described in US4043507 or US5500162, or first stimulated to further agglomerate by bringing them into a suitable liquid medium, as disclosed in US5484559, US6197073, US2004 / 0007789 A1 or WO2015 / 014930 A1, followed by aging, washing and drying. The spherical porous green bodies thus produced are consolidated in a subsequent sintering step into lithium ion conductive ceramic bodies with high sphericity.

[0054] Furthermore, this object is achieved by a method for producing a lithium-ion conductor, in which the composite material according to the invention is sintered, in particular under the action of elevated temperature and / or elevated pressure.

[0055] Both the lithium ion conductive composite material according to the invention and the lithium ion conductor produced from the lithium ion conductive composite material can be used as lithium ion conductive parts or components of such parts depending on the needs and scope of application.

[0056] Furthermore, formulations for producing composite precursors for hybrid electrolytes or ceramic slurries for producing sintered purely inorganic solid lithium-ion conductor components are described in which the viscosity of particle-filled formulations with the same volumetric filling is significantly higher when non-spherical particles are used than when particles with high sphericity Ψ produced according to the invention are used, with the prerequisite that the particle size or particle size distribution in both cases is the same.

[0057] Furthermore, formulations for producing composite precursors for hybrid electrolytes or ceramic slurries for producing sintered purely inorganic solid lithium-ion conductor components are described, in which the corresponding formulations can have a significantly higher degree of filling in the case of spherical embodiments than in the case of non-spherical embodiments, without essentially changing the viscosity, again with the prerequisite that the particle size and particle size distribution do not differ essentially in both cases.

[0058] The lithium ion conductive material produced according to the invention in the form of spherical particles with particle sizes in the μm or subμm range can be incorporated as a filler into polymer electrolytes or polyelectrolytes, whereby the corresponding composites are generally referred to as hybrid electrolytes. For this purpose, it can be optionally pressed into a compact using a suitable tool or incorporated into a ceramic slurry (with or without the addition of a binder) and subjected to a suitable forming process (e.g. tape casting) and in both cases sintered at a temperature that forms a purely inorganic ion-conducting compact. Both application forms of hybrid electrolytes and purely inorganic ceramic solid ion conductors can be used as solid electrolytes in the next generation of rechargeable lithium ion or lithium batteries, for example solid-state lithium batteries (all-solid-state batteries (ASSB)) or lithium-air batteries. On the one hand, it can be used as a separator, i.e. introduced between electrodes, which protects the electrodes from undesired short circuits and thereby ensures the functionality of the entire system. For this purpose, the corresponding composites can be incorporated into the battery as solid electrolytes, either by application as a layer on one or both electrodes or as free-standing films. On the other hand, it is conceivable to mix them with the electrode active materials, either by inclusion of the electrode active materials in the hybrid electrolyte formulation in the case of hybrid electrolytes or by co-sintering with them in the case of purely inorganic ceramic electrolytes. In this case, the solid electrolyte provides for the transport of the relevant charge carriers (lithium ions and electrons) to and from the electrode material and the conductive electrode, depending on whether the battery is being discharged or charged. EXAMPLES

[0059] Example of production of lithium ion conductive particles having a high sphericity Ψ of at least 0.7 from a lithium ion conductive material 1. Preparation of spherical LAGP particles (A) Direct forming from green glass melt The starting glass for the final lithium-ion conducting phosphate-based glass ceramic with the composition 5.7 wt.-% Li2O, 6.1 wt.-% Al2O3, 37.4 wt.-% GeO2 and 50.8 wt.-% P2O5 was melted in an effusion crucible at a temperature of 1650°C.

[0060] The glass melt was held at a temperature of 1600 °C in the selected melting device. It was allowed to flow out through a nozzle with a diameter of 2 mm attached to the bottom of the crucible. The glass jet so produced was dropped onto an 8 mm thick striking wheel with 53 teeth and an outer diameter of 135 mm, rotating around its axis at a speed of 5000 rpm. In this way, the glass stream was filamented into individual partial strands and accelerated at an inclination angle of 20-30 ° measured with respect to the horizontal. It was subsequently passed through a 3 m long tubular furnace, configured in a curved shape that mimicked the trajectory of the filamented glass stream, and heated to 1550 °C with two gas burners. The longitudinally formed filaments were deformed into spheres due to the tendency of the surface energy to be minimized. After leaving the tubular furnace, the glass spheres were further cooled by flying in air until they achieved sufficient morphological stability, and were finally contained in a collection vessel.

[0061] The green glass spheres produced by the above mentioned thermoforming process, cooled and mostly X-ray amorphous, were ceramified during further temperature treatment at a maximum temperature of 850 °C with a holding time of 12 h after nucleation at temperatures ranging from 500 to 600 °C for 2 to 4 h, and thus converted into the final lithium-ion conducting glass-ceramics.

[0062] (B) Forming non-spherical green glass particles by rounding them The starting glass for the final lithium-ion conducting phosphate-based glass-ceramic with the composition 5.7 wt.-% Li2O, 6.1 wt.-% Al2O3, 37.4 wt.-% GeO2 and 50.8 wt.-% P2O5 was melted in a flow crucible at a temperature of 1650°C.

[0063] The glass melt was held in the selected melter at a temperature of 1600° C. It was forced to flow through a 2 mm diameter nozzle attached to the bottom of the crucible into a gap between two counter-rotating water-cooled rollers and quenched to form a green glass ribbon, which was mechanically singulated into small pieces with a hammer.

[0064] The glass fragments are roughly crushed in a ball mill to obtain a particle size d 100 The powder fraction having a particle size of <100 μm was sieved. In a further subsequent step, the sieved green glass powder was dry-milled in an opposed jet mill. 10 = 0.9 μm, d 50 = 5 μm, d 90 = 13 μm and d 99 = 18 μm.

[0065] By bringing the powder into an oxyhydrogen gas flame, the glass particles are remelted and rounded due to the tendency of the surface energy to be minimized. After exiting the flame, the particles are cooled and collected in a collection vessel.

[0066] The green glass spheres produced by the above mentioned thermoforming process, cooled and mostly X-ray amorphous, were ceramified during further temperature treatment at a maximum temperature of 850 °C with a holding time of 12 h after nucleation at temperatures ranging from 500 to 600 °C for 2 to 4 h, and thus converted into the final lithium-ion conducting glass-ceramics.

[0067] 2. Filamentation of molten salt In a first step, a zirconium-containing precursor powder was prepared as follows: 5.0 kg (50.0 mol) of acetylacetone was added dropwise to 23.4 kg (50.0 mol) of zirconium-n-propoxide (70% solution) in a round-bottom flask while stirring. The resulting reaction mixture was stirred for 60 minutes at room temperature. 2.7 kg (150.0) mol of distilled water was then added thereto for hydrolysis. After a reaction time of about 1 hour, the resulting prehydrolyzate was completely dried in a rotary evaporator. A sample of the resulting powder was then heated (900° C. / 5 hours) to measure the oxide content.

[0068] 1.77 kg (5.0 mol) ZrO2 equivalent of the zirconium-containing precursor powder (oxide content: 35% by mass) produced in the preceding step was added together with 2.5 kg (7.5 mol) lanthanum acetate sesquihydrate, 1.95 kg (19.2 mol) lithium acetate dihydrate and 0.15 kg (0.61 mol) aluminium chloride hexahydrate to a ball mill where it was ground for 4 hours in order to produce a powder mixture as homogeneous as possible. As grinding balls for this purpose, Al2O3 spheres with a diameter of 40 mm were used.

[0069] After sieving it, the powder mixture was added to an Al2O3 flow crucible, where it was brought to a temperature of 300 ° C, barely above the melting point of anhydrous lithium acetate, 280-285 ° C. A molten salt was formed, which was then flowed out through a nozzle with a diameter of 2 mm attached to the bottom of the crucible. The jet of molten salt thus formed was dropped onto an 8 mm thick striking wheel with 53 teeth and an outer diameter of 135 mm, rotating around its axis at a speed of 5000 rpm. In this way, the jet of molten salt was filamented into individual partial strands, which were accelerated at an inclination angle of 20-30 ° measured with respect to the horizontal. It was subsequently passed through a 3 m long tubular furnace, configured in a curved shape that imitated the trajectory of the filamentary jet of molten salt. The furnace was electrically heated to maintain a moderate temperature of 300-320 °C in the inlet region, and the molten salt was further maintained, and the initially elongated filaments were transformed into liquid spheres due to the tendency of the surface energy to be minimized. In the subsequent region, the temperature was selected to be significantly higher, reaching a temperature of about 900 °C. Thus, the first step of calcining the liquid spheres was performed here, forming porous preceramic particles as an intermediate stage. After leaving the tubular furnace, it was further cooled by flying in air and finally collected in a collection vessel.

[0070] The porous preceramic particles were consolidated into spheres of the final lithium-ion conducting LLZO material through a further calcination step in a furnace at 1,050 °C with a holding time of 7-8 h.

[0071] 3. Preparation of spherical LLZO particles by spray calcination using a pulse reactor method 2.3 kg (4.7 mol) of zirconium acetylacetone was dissolved in at least 10.0 kg (556 mol) of distilled water in a suitable reaction vessel. 2.4 kg (7 mol) of lanthanum acetate sesquihydrate was dissolved in 10 kg (556 mol) of distilled water in a further reaction vessel. 1.8 kg (18 mol) of lithium acetate dihydrate and 0.14 kg (0.58 mol) of aluminum chloride hexahydrate were dissolved in 5.0 kg (278 mol) of distilled water in a third reaction vessel. After the components were completely dissolved, the solutions were combined and the resulting reaction mixture was stirred at room temperature for 12 hours.

[0072] The solution is conveyed with a peristaltic pump into a pulse reactor with a volume flow of 3 kg / h, where it is finely sprayed through a 1.8 mm titanium nozzle into the reactor interior and heat-treated there, with the temperature of the combustion chamber being kept at 1030° C. and the temperature of the resonance tube at 1136° C. The ratio of the amount of combustion air to the amount of fuel (natural gas) is 10:1 (air:gas).

[0073] The powder is loaded into a square corundum crucible and placed in a box furnace, where the material is brought to a temperature of 1050° C. in an air atmosphere to completely consolidate the spherical fine particles of LLZO.

[0074] 4. Preparation of spherical LLZO particles by the dropletization method Firstly the LLZO material is melted in a so-called skull crucible, as described, for example, in DE 19939782 C1. A water-cooled crucible is used for this, so that during melting a colder protective layer is formed from the material to be melted. The crucible material therefore does not melt during the melting process. The input of energy into the melt is realised by means of high-frequency coupling via an encircling induction coil into the molten material. A condition in this case is a sufficient conductivity of the melt, which in the case of a lithium garnet melt is provided by a high lithium content. During the melting process lithium vapor is produced, which can be easily compensated for by excess lithium. For this, one usually works with a lithium excess of 1.1 to 2 times.

[0075] The raw materials are mixed according to the following composition and charged into an upwardly open skull crucible: 14.65% by weight Li2O, 56.37% by weight La2O3, 21.32% by weight ZrO2 and 7.66% by weight Nb2O5. In order to achieve a certain minimum conductivity, the mixture had to be preheated first. For this purpose, burner heating was used. After reaching the coupling temperature, further heating and homogenization of the melt was achieved by high-frequency coupling via an induction coil. To improve homogenization of the melt, it was stirred with a water-cooled stirrer.

[0076] The materials produced by this route can in principle be converted into glass-ceramic materials with a predominant crystalline phase of the garnet type either by direct solidification from the melt or by quenching followed by a temperature treatment (ceramming). In the examples described here, the direct quenching embodiment was chosen.

[0077] In this case, the material is obtained as a monolithic block and is subjected to various coarse comminution steps, for example by processing with hammers and chisels in a first step, the resulting fragments are comminuted in a jaw crusher in a second step, and the resulting coarse powder is further pre-comminuted in a planetary mill and subsequently sieved in a third step to obtain a particle size d 100 This powder was converted into a powder having a diameter of <100 μm in a further subsequent step by underwater grinding carried out in an attritor. 10 = 0.14 μm, d 50 = 0.42 μm, d 90 = 1.87 μm and d 99 = 2.92 μm. The solids content of LLZO in the milling slurry used was about 30%. To stabilize the particles, a dispersant (Dolapix CE 64 or Dolapix A88, Zschimmer & Schwarz GmbH & Co KG) was added thereto before milling, which proved to be well workable at a rate of 1.0% based on the rate of LLZO in the suspension.

[0078] For further processing, the solids content of the milled slurry was increased to a content of 60% by partially evaporating the water in a rotary evaporator in order to obtain a suitable mix ratio in terms of viscosity.

[0079] Subsequently, ammonium alginate was added as a binder in an amount of 1.0%.

[0080] From the slurry, a shape-stable green body having a size of 0.3 to 2.5 mm was obtained by immersing and reacting in a solution of aluminum lactate or an inorganic acid or an organic acid through a nozzle and / or cannula using a dropletization method.

[0081] Subsequently, sintered spheres were formed from this by a sintering process, which was carried out in an air atmosphere at a temperature of 1150° C. under standard pressure.

[0082] Example for the preparation of a formulation for a lithium ion conductive composite material, filled with at least 20% by volume of lithium ion conductive particles when the polydispersity index PI of the particle size distribution is less than 0.7, or at least 30% by volume of corresponding particles when the polydispersity index PI of the particle size distribution is greater than 0.7 and less than 1.2, or at least 40% by volume of corresponding particles when the polydispersity index PI of the particle size distribution is greater than 1.2: 1. Preparation of a composite material according to the invention (preparation of a hybrid electrolyte membrane based on polyethylene oxide (PEO) / lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) polymer electrolyte filled with LLZO particles) Molar mass 4 x 10 6 1.4 g of polyethylene oxide (PEO, Dow Chemical) with 0.01 g / mol was dried in vacuum for 48 hours at 50° C. The polymer was found to consist of particles with a sphericity of 0.92 and a particle size distribution of d 10 = 1.22 μm, d 50 = 2.77 μm, d 90 = 5.85 μm, d 998.5 g of lithium lanthanum zirconium oxide powder having a value of 0.0001 μm was added. The polydispersity index of the particle size distribution according to the invention is accordingly PI=0.681. The mixture was vigorously ground in a mortar. It was then subjected to a mortar grinding test. The powder had a purity of more than 99%, suitable for battery applications, and was previously heated at 120° C. for 24 hours in a vacuum (10 -7 0.6 g of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI, 3M) dried under 1000 psi (1 bar) was mixed into the mixture. All components were mixed intensively in a mortar until a homogeneous paste was formed. This resulted in a PEO / LiTFSI polymer electrolyte matrix with a lithium ion:ethylene oxide monomer unit ratio (Li:EO) of 1:15, embedded with 50% by volume of inorganic solid lithium ion conductor. The hybrid electrolyte so produced was vacuum packed into a pouch and then heat treated at 100 °C overnight, followed by pressing at 100 °C under a pressure of 50 kN (50–750 kg / cm). 2 The composite membrane was hot pressed (Servitec Polystat 200 T-Presse) with a thickness of about 100 μm.

[0083] The same procedure gave the following particle size distribution: 10 = 0.44 μm, d 50 = 1.24 μm, d 90 = 3.50 μm, d 99 A hybrid electrolyte membrane was produced using LLZO powder consisting of non-spherical particles (Ψ=0.48) with a particle size distribution of 6.94 μm. The polydispersity index of the particle size distribution was PI=0.900 according to the invention in this case. However, in this case, only 4.6 g of LLZO powder could be effectively incorporated into the PEO / LiTFSI polymer electrolyte matrix, i.e., a hybrid electrolyte could only be produced with a volume fraction of up to 29 vol.%.

[0084] 2. Production of the lithium ion conductor according to the invention from the composite material according to the invention (production of a purely inorganic sintered solid electrolyte membrane using the tape casting method based on a casting slurry filled with LATP particles) 11.4 g of polyvinyl butyral (PVB) with a molecular weight of 35000 g / mol (containing, besides vinyl butyral units, 1.7% by weight of vinyl acetate and 18.9% by weight of vinyl alcohol units) were dissolved in 68.4 g of a solvent mixture consisting of ethanol:toluene (4:6). The viscosity of the solution was 200-450 mPa·s. 5.7 g of dioctyl phthalate, acting as a plasticizer, were added to the mixture. Finally, the mixture was dissolved in a dissolver, consisting of particles with a sphericity of 0.94 and a particle size distribution with the following values ​​d 10 = 0.81 μm, d 50 = 2.23 μm, d 90 = 5.17 μm, d 99 200 g of Lithium Aluminum Titanium Phosphate (LATP) glass ceramic powder with a particle size distribution of 8.46 μm was introduced and dispersed. The polydispersity index of the particle size distribution is in this case PI=0.805 according to the invention. The resulting casting material had a viscosity of 4000-5000 mPa·s. The content of glass ceramic powder was about 43% by volume.

[0085] The homogeneous material thus produced was subsequently degassed by vacuum techniques (degassing). This degassed material was fed to a conventional tape casting process in a film stretching apparatus and thus cast into a tape of approximately 0.3 mm thickness (measured after drying). The green tape thus produced was then cut into individual pieces in the desired format.

[0086] The individualized tape pieces were finally sintered at 1000 °C for 4 h to form densified LATP membranes, with a film shrinkage of about 9%.

[0087] The same procedure yielded a particle size distribution with the following values: 10 = 0.68 μm, d 50 = 1.74 μm, d 90 = 3.86 μm, d 99Purely inorganic solid lithium-ion conductor membranes were produced using LATP powder consisting of non-spherical particles (Ψ=0.46) with a diameter of 7.21 μm, where the polydispersity index of the particle size distribution was PI=0.754 according to the invention. However, in this case only 90 g of LATP powder could be effectively incorporated into the binder solution consisting of PVB, dioctyl phthalate and ethanol:toluene, i.e. in this case tape casting slurries could only be produced with a volume content of up to 28% by volume without significantly exceeding the target viscosity of 4000-5000 mPa·s. Due to the significantly reduced solid content, the shrinkage during sintering was about 15%.

Claims

1. A lithium ion conductive composite material comprising at least one polymer and lithium ion conductive particles, the particles have a sphericity Ψ of at least 0.7; and The composite material comprises at least 40% by volume of the particles, the particle size distribution of which has a polydispersity index PI of greater than 1.2, The particles have an average particle size of 0.2 μm to 2 μm, and the polydispersity index PI is PI = log(d 90 / d 10 ) characterized in that it is calculated by The lithium ion conductive composite material.

2. The polymer comprises the compound: polyethylene oxide, Derivatives of polyethylene oxide, Polyvinyl butyral The lithium ion conductive composite material according to claim 1, characterized in that it comprises at least one of the following:

3. 3. A lithium ion conducting composite material according to claim 1, characterized in that the polymer contains at least one lithium ion conducting compound.

4. The particles are made of a lithium ion conducting compound: Lithium lanthanum zirconate (LLZO), Lithium aluminum titanium phosphate (LATP), - Compounds having a garnet-type crystal structure, A compound having the same crystal structure as NaSICon The lithium ion conductive composite material according to any one of claims 1 to 3, characterized in that it comprises at least one of the following:

5. 5. The lithium ion conductive composite material according to claim 1 , characterized in that the interfacial resistance for lithium ion conductivity between the polymer and the particles is reduced due to surface modification of the particles, so that the lithium ion conductivity is higher than in the case of a comparable composite material in which the interfacial resistance between the polymer and the particles is not reduced.

6. 6. A method for producing a lithium ion conducting composite material according to any one of claims 1 to 5, characterized in that the particles are produced using spray calcination, or filamentation from molten salts, or dropwise production, or glass sphere production.

7. 6. A method for producing a lithium ion conductor, characterized in that the composite material according to claim 1 is sintered under the action of elevated temperature and / or elevated pressure.

Citation Information

Patent Citations

  • ion conductor with garnet structure

    DE102007030604A1

  • Lithium-containing solution used in xerogel for producing crystalline composite oxide with garnet-like structure used in lithium-ion battery for electronic device, includes metal ion A e.g. barium and metal ion B e.g. lanthanum and solvent

    DE102013101145A1

  • Method for producing a lithium-ion conductive material with a garnet-like crystal structure, use of the material and method for producing an intermediate product

    DE102013224045A1

  • Process for manufacturing a glass-ceramic ion conductor

    DE102014116378A1

  • Lithium manganese composite oxide and its manufacture

    JP1999016574A