Antiviral agent consisting of metallic copper particles
Coating metallic copper fine particles with fatty acids and esters addresses aggregation and oxidation issues, ensuring high and sustained antiviral efficacy against diverse viruses.
Patent Information
- Application Number
- JP2020066385
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-04-03
- Filing Date
- 2020-04-02
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-04-02
AI Technical Summary
Existing antiviral agents using monovalent copper compounds face issues with aggregation, reduced particle surface area, decreased contact with viruses, and impaired transparency due to large particle sizes, leading to diminished antiviral properties and oxidation of cuprous oxide to copper(II) oxide.
Coating metallic copper fine particles with a fatty acid and/or ester compound to a specific ratio of 0.1 to 10% by mass, maintaining a 10% or more metallic copper ratio at the surface, and controlling the particle size between 100 nm to 500 μm to prevent aggregation and oxidation, enhancing antiviral activity.
The coated metallic copper particles exhibit long-lasting antiviral properties against viruses with and without an envelope structure, maintaining high antiviral activity and preventing oxidation, even after storage for extended periods.
Smart Images

Figure 0007572156000003 
Figure 0007572156000004 
Figure 0007572156000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an antiviral agent, and more specifically, to an antiviral agent containing metallic copper as an active ingredient. [Background technology]
[0002] Conventionally, silver ions or copper (II) ions have been used as active ingredients in materials having antibacterial or antiviral properties, and various antiviral materials have been proposed in which these metal ions are supported on substances such as zeolite or silica gel or dispersed in a solvent. However, although the above metal ions can exhibit antiviral activity against viruses having an envelope structure, such as influenza viruses, they are unable to exhibit antiviral activity against viruses that do not have an envelope structure, such as noroviruses.
[0003] Monovalent copper compounds are also known as metal compounds capable of exhibiting antiviral properties, regardless of the presence or absence of an envelope structure. For example, the following Patent Document 1 describes an antiviral composition that contains fine particles of a monovalent copper compound, a reducing agent, and a dispersion medium, and has a pH of 6 or less. The following Patent Document 2 describes an antiviral composition having a BET specific surface area of 5 to 100 m2. 2 The patent document 3 below describes an antibacterial and antiviral composition that contains cuprous oxide particles of 100000000 / g, a saccharide having an aldehyde group, and a photocatalytic substance. The patent document 3 below describes an antiviral coating film that contains a copper-supported oxide having an average secondary particle diameter of 80 nm to 600 nm, in which at least one of copper particles and copper compound particles is supported on an oxide particle, barium sulfate having an average secondary particle diameter of 1 μm to 15 μm, and a water-repellent resin binder. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Patent No. 5194185 [Patent Document 2] JP 2013-82654 A [Patent Document 3] JP 2015-205998 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, fine particles of a monovalent copper compound tend to aggregate, making it difficult to uniformly disperse the monovalent copper compound. Thus, when the dispersion liquid is used as an antiviral composition or when it is mixed with a paint and used as a coated antiviral molded body, it has been difficult to efficiently express the antiviral properties of the fine particles of the monovalent copper compound. In addition, when a monovalent copper compound having a large particle size as described in the above patent document is used, the particle surface area is reduced, and the antiviral properties are reduced due to a decrease in the chance of contact with the virus. In addition, an antiviral molded body coated with a monovalent copper compound having a large particle size has a problem that the haze and light transmittance are deteriorated, resulting in a loss of transparency. Furthermore, fine particles of monovalent copper compounds can be obtained by pulverization, but since there is no coating agent or stabilizer, they tend to aggregate, and there are problems with this method, such as the tendency for cuprous oxide to oxidize to copper(II) oxide.
[0006] In order to solve these problems, the present inventors have conducted intensive research into microparticles that can efficiently exhibit high antiviral properties, and as a result, have found that metallic copper can exhibit higher antiviral properties than monovalent copper compounds, and that by coating the surface of metallic copper microparticles with a fatty acid and an ester compound of the fatty acid, the microparticles can be uniformly dispersed without aggregation even when contained in a low-boiling point solvent at a high concentration. However, although the above-mentioned metallic copper microparticles can be made into a uniform dispersion without aggregation in the state of a dispersion, the metallic copper microparticles alone without a medium are prone to aggregation, making it difficult to efficiently exhibit antiviral properties. In addition, the amount of organic matter (fatty acid and ester compound) coated per secondary particle of the metallic copper microparticles increases due to aggregation, and there is a problem that it is not possible to obtain an antiviral agent consisting of a fine particle powder having high antiviral properties as obtained in a dispersion. Therefore, an object of the present invention is to provide an antiviral agent that can efficiently exhibit antiviral activity, has excellent oxidation resistance of metallic copper as an active ingredient, and can exhibit excellent antiviral activity for a long period of time. [Means for solving the problem]
[0007] According to the present invention, the present invention provides a coating material comprising metallic copper fine particles coated with a fatty acid and / or an ester compound, the amount of the fatty acid and / or ester compound coated on the metallic copper fine particles is 0.1 to 10% by mass, The antiviral agent is characterized in that, when the surface of the metallic copper microparticle aggregate is measured by X-ray photoelectron spectroscopy, the ratio of metallic copper to all copper components at the depth where the metallic copper components are first measured is maintained at 10% or more.
[0008] In the antiviral agent of the present invention, 1. The amount of the fatty acid and / or ester compound coated on the metallic copper fine particles is 0.1 to 20% by mass; 2. The average secondary particle size of the metallic copper fine particles is 100 nm to 500 μm; 3. The metallic copper fine particles are dispersed in a solvent. 4. A resin composition in which the metallic copper fine particles are dispersed in a resin. 5. The antiviral activity value of an antiviral agent containing the metallic copper fine particles in an amount of 0.01 to 2.0% by mass is 3.0 or more. is preferred. Effect of the Invention
[0009] In the antiviral agent of the present invention, the metallic copper microparticles, which are an antiviral active ingredient, are coated with a fatty acid and / or an ester compound, thereby effectively preventing oxidation and aggregation of the metallic copper microparticles, and enabling excellent antiviral properties to be exhibited for a long period of time. That is, in the present invention, it was found that when the surface of a metallic copper microparticle aggregate is measured by X-ray photoelectron spectroscopy, if the ratio of metallic copper to the total copper components at the depth where the metallic copper components are first measured is maintained at 10% or more, the antiviral properties can be sufficiently exhibited, and a necessary and sufficient amount of fatty acid and ester compound coating for suppressing the oxidation and aggregation of metallic copper described above without inhibiting the antiviral properties was found.
[0010] The above-mentioned effect of the antiviral agent of the present invention is also clear from the results of the examples described below. That is, the antiviral agents made of the metallic copper microparticle powder prepared in Examples 1 to 7 have a surface composition of 100% metallic copper, and the antiviral evaluations performed on Examples 1 and 6 are also high. On the other hand, as in Comparative Example 1, it is found that in metallic copper microparticles in which fatty acid copper is thermally decomposed and not coated with fatty acid and / or ester compound, metallic copper is easily oxidized (Comparative Example 1). In addition, the antiviral agent made of the metallic copper microparticle powder prepared in Example 9 has a surface composition of 46% metallic copper, but has antiviral properties equivalent to those of Example 6, which has 100% metallic copper. In addition, as is clear from FIG. 2, in the antiviral agent of the present invention, even when stored in the air for 8 months, 46% metallic copper remains without being oxidized, and it is clear that the antiviral agent of the present invention can exhibit excellent antiviral properties for a long period of time.
[0011] The antiviral agent of the present invention can exhibit antiviral activity regardless of the presence or absence of an envelope structure, and can also exhibit antiviral activity against viruses that do not have an envelope structure, such as norovirus. [Brief description of the drawings]
[0012] [Figure 1] FIG. 1 is a diagram showing an X-ray photoelectron spectroscopy chart of the antiviral agent obtained in Example 1. [Diagram 2] FIG. 1 shows an X-ray photoelectron spectroscopy chart of the antiviral agent obtained in Example 9. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] (Antiviral Agents) The antiviral agent of the present invention is composed of metallic copper microparticles coated with fatty acids and / or ester compounds, and metallic copper, which is an active ingredient exhibiting antiviral properties, can adsorb viruses and inactivate them, and can exhibit excellent antiviral properties regardless of the presence or absence of an envelope structure. That is, the excellent antiviral properties of the antiviral agent of the present invention are believed to be due to the oxidizing power of active oxygen generated from metallic copper, which denatures the proteins of viruses composed of microproteins, and metallic copper reacts with the thiol groups of the proteins of the viruses to denature the proteins, thereby inactivating the viruses. The mechanism by which metallic copper microparticles coated with fatty acids and / or ester compounds exhibit antiviral properties is not clear, but it is believed that viruses attached to the coating present on the surface of the metallic copper microparticles are replaced by the coating and come into contact with metallic copper.
[0014] The metallic copper microparticles constituting the antiviral agent of the present invention are configured so that fatty acids or ester compounds are coordinated around the metallic copper microparticles, while the ester compounds have an affinity for fatty acids and are therefore thought to be coordinated around the fatty acids or mixed with the fatty acids. The metallic copper microparticles constituting the antiviral agent of the present invention have their surfaces coated with a fatty acid and / or an ester compound, which prevents oxidation of the microparticle surface caused by increased surface activity of the metallic copper microparticles and inhibits aggregation of the microparticles, allowing the agent to exhibit excellent antiviral properties over a long period of time. In the present invention, when the surface of the metallic copper microparticle aggregate is measured by X-ray photoelectron spectroscopy, the ratio of metallic copper to the total copper components at the depth where the metallic copper components are first measured is maintained at 10% or more, which is an important feature. That is, the oxidation and aggregation of the metallic copper microparticles are suppressed by covering the surface of the metallic copper microparticles with a fatty acid and / or an ester compound, and the amount of metallic copper at the interface between this coating and the metallic copper microparticles is important for efficiently expressing antiviral properties. Therefore, in the present invention, the amount of metallic copper components at the depth where the metallic copper components are first measured (corresponding to the thickness of the coating) is measured, and it has been found that excellent antiviral properties can be obtained if this metallic copper component is maintained at 10% or more, preferably 20% or more, and particularly preferably 40% or more of the total copper components. Note that the above value is a result obtained by measuring the entire surface of the metallic copper microparticle aggregate by X-ray photoelectron spectroscopy and averaging the results, and therefore can approximate the individual state of the metallic copper microparticles present on the surface of the aggregate.
[0015] In addition, in the antiviral agent of the present invention, as described below, in the production of the metallic copper microparticle powder constituting the antiviral agent, excess fatty acid, ester compound, or unreacted fatty acid copper, etc. are efficiently removed, so that filtration and washing are easy, and the powder state of the metallic copper microparticles with a small average secondary particle size and a large surface area can be maintained, and as a result, excellent antiviral properties are obtained. Also, as described above, the amount of fatty acid and ester compound coating on the metallic copper microparticles is 0.1 to 10 mass%, which is smaller than that of metallic copper microparticles recovered by removing the solvent from a conventional metallic copper microparticle-containing dispersion liquid, and the properties of the metallic copper microparticles, such as antiviral properties, can be efficiently expressed.
[0016] Examples of fatty acids that may be used to coat the surface of the metallic copper microparticles include myristic acid, stearic acid, oleic acid, palmitic acid, n-decanoic acid, para-toic acid, succinic acid, malonic acid, tartaric acid, malic acid, glutaric acid, adipic acid, acetic acid, etc., and although combinations of multiple types of these may be used, higher fatty acids having 10 to 22 carbon atoms, and of these, stearic acid, are particularly preferred. The ester compound coating the surface of the metallic copper microparticles is preferably an ester compound derived from the fatty acids and polyols that are the raw materials in the method for producing metallic copper microparticle powder of the present invention described below, but it is also possible to blend ester compounds other than those derived from the raw materials, and these may be different ester compounds, but it is preferable that they are of the same type as the ester compounds derived from the raw materials. Suitable ester compounds for coating the surface of metallic copper microparticles include ester compounds of the above-mentioned fatty acids and the polyols described below, such as, but not limited to, diethylene glycol distearate, ethylene glycol distearate, propylene glycol distearate, polyethylene glycol distearate, and polypropylene glycol distearate.
[0017] In the present invention, the average primary particle size of the metallic copper fine particles is preferably in the range of 10 to 500 nm, particularly 10 to 200 nm. When the average primary particle size of the metallic copper fine particles is in the above range, it is possible to efficiently exhibit excellent antiviral performance. That is, metallic copper fine particles having such a small average primary particle size can efficiently generate active oxygen because the contact rate of the metallic copper fine particles with oxygen is high, and it is possible to exhibit excellent antiviral performance. In addition, the average primary particle size referred to in this specification is the average of metallic copper fine particles with no gaps between them, and the measurement method will be described later. In addition, the aggregate of metallic copper fine particles of the present invention is a state in which a powder consisting of secondary particles formed by agglomeration of the primary particles of the metallic copper fine particles is compressed and molded so that no gaps are formed between the secondary particles. The metallic copper microparticle powder constituting the antiviral agent of the present invention is composed of primary particles having the above-mentioned average primary particle size, and preferably has an average secondary particle size in the range of 100 nm to 500 μm, particularly 100 nm to 100 μm, which allows the agent to exhibit excellent antiviral properties in a powder state and also provides remarkably excellent handling properties, such as coatability.
[0018] (First Manufacturing Method) The metallic copper fine particle powder coated with a fatty acid and / or an ester compound which constitutes the antiviral agent of the present invention can be prepared by the following production method. (1) First step A polyol dispersion liquid is prepared by adding fatty acid copper to a polyol and heating the mixture, in which metallic copper fine particles having a surface coated with a fatty acid and / or an ester compound of the fatty acid and a polyol are dispersed. The heating temperature is a temperature below the decomposition start temperature of the fatty acid copper used, and specifically, is preferably in the range of 160 to 230°C. The heating and mixing time is preferably 60 to 360 minutes. If the heating temperature is equal to or higher than the decomposition start temperature of the fatty acid copper, the fatty acid and / or the ester compound will not coat the metallic copper fine particles, and the metallic copper fine particles may be oxidized immediately.
[0019] The amount of fatty acid copper is preferably in the range of 0.1 to 5% by mass per polyol. If the amount of fatty acid copper is less than the above range, there is a risk that sufficient antiviral properties cannot be imparted to the dispersion liquid compared to when it is in the above range. On the other hand, if the amount of fatty acid copper is more than the above range, there is a risk that the economic efficiency is inferior and the coatability and moldability are impaired compared to when it is in the above range. Examples of the polyol include ethylene glycol, diethylene glycol, triethylene glycol, polyethylene glycol, polypropylene glycol, and glycerin, and are appropriately selected in combination with the low-boiling point solvent described below.
[0020] (2)Second process Next, the polyol dispersion in which the metallic copper particles coated with a fatty acid and / or an ester compound of the fatty acid and a polyol are dispersed is mixed with a low boiling point solvent to prepare a mixed liquid. The low boiling point solvent is preferably added in an amount of 10 to 200% by mass based on the polyol. Examples of low-boiling point solvents include esters such as methyl acetate, ethyl acetate, and butyl acetate, hydrocarbons such as hexane, heptane, toluene, xylene, and cyclohexane, and ketones such as methyl isobutyl ketone, methyl ethyl ketone, and cyclohexanone, but ester solvents are preferred, and among them, butyl acetate, ethyl acetate, and methyl isobutyl ketone can be preferably used. It is important that the low-boiling point solvent is not miscible with the polyol, and it is preferable to combine the polyol and the low-boiling point solvent so that the difference in solubility parameter (Sp value) between them is 3 or more. Preferably, when diethylene glycol (Sp value: 12.6) is used as the polyol, butyl acetate (Sp value: 8.4) is used as the low boiling point solvent.
[0021] In the method for producing the metallic copper microparticle powder constituting the antiviral agent of the present invention, it is important that no dispersant is mixed into the low-boiling solvent. As a result, the metallic copper microparticles coated with fatty acids and / or ester compounds do not migrate to the low-boiling solvent but remain precipitated in the polyol. On the other hand, impurities, in addition to excess fatty acid copper or free fatty acids or ester compounds present in the polyol, migrate to the low-boiling solvent. As a result, metallic copper microparticles coated with fatty acids and / or ester compounds are present in the polyol with reduced impurities. Since the metallic copper particles are sufficiently coated with the ester compound of fatty acid and polyol in the first step described above, it is not necessary to specifically add an ester compound to the low-boiling point solvent, but it may be possible to add one depending on the amount of coating in the first step.
[0022] (3) Third step The mixed liquid is allowed to stand for 30 to 120 minutes at a temperature of 0 to 40° C. to cause phase separation of the polyol and the low-boiling solvent. When the mixed liquid is phase-separated, excess fatty acid copper, free fatty acid or fatty acid ester compound, or impurities present in the mixed liquid are extracted into the low-boiling solvent side, and metallic copper fine particles coated with fatty acid and / or ester compound of the fatty acid and polyol remain in a precipitated state in the polyol. Next, the low-boiling point solvent is removed from the phase-separated mixture to obtain a dispersion in which metallic copper particles coated with a fatty acid and / or an ester compound of the fatty acid and a polyol have precipitated in the polyol. The low boiling point solvent can be removed by a conventionally known separation method such as simple distillation, reduced pressure distillation, precision distillation, thin film distillation, extraction, or the like. The copper metal fine particle powder can be recovered from the polyol by a conventionally known separation method such as membrane separation, centrifugation, evaporation, decantation, etc., but is not limited thereto, and is preferably recovered by membrane separation. The separated metallic copper microparticles are thoroughly washed with water or a low-boiling point solvent such as butyl acetate or hexane, and then heated and dried at 40 to 50°C for 60 to 360 minutes to thoroughly remove moisture, thereby obtaining a dry metallic copper microparticle powder with a coating amount of fatty acid and ester compound of 0.1 to 20 mass%.
[0023] (Second Manufacturing Method) In addition to the above-mentioned production method, fine metallic copper particles coated with a fatty acid and / or an ester compound of a fatty acid in a low boiling point solvent can also be prepared by the following method. That is, by carrying out the same process as in the first manufacturing method described above, except that in the first step, a combination of a fatty acid and a copper compound is added instead of fatty acid copper, a dispersion liquid containing dispersed metallic copper microparticles coated with a fatty acid and / or an ester compound of the fatty acid can be prepared, and then by carrying out the second and third steps described above, a dry metallic copper microparticle powder can be obtained in the same manner.
[0024] (Other manufacturing methods) According to the above-mentioned first and second production methods, the metallic copper microparticle powder constituting the antiviral agent of the present invention can be efficiently produced as metallic copper microparticles coated with a fatty acid and / or an ester compound of the fatty acid and a polyol in a coating amount of 0.1 to 20 mass %, but the metallic copper microparticle powder coated with a fatty acid and / or an ester compound can also be produced by the following method. That is, the polyol dispersion liquid in which the metallic copper fine particles coated with the fatty acid and / or the ester compound of the fatty acid and the polyol obtained in the first step of the first manufacturing method described above are dispersed may be used as it is, and the metallic copper fine particles recovered from this dispersion liquid may be used. In this case, the viscosity of the polyol dispersion liquid is high due to the excess fatty acid copper, or free fatty acid or ester compound, as well as impurities, and it is difficult to remove the low boiling point solvent as it is, so the viscosity is reduced by diluting with ethanol or the like, and then the solvent is removed. In addition, the fatty acid copper is heated under an inert atmosphere to reduce it, and then the ester compound described above is added and the mixture is pulverized and mixed to produce metallic copper fine particle powder coated with at least the ester compound.
[0025] (Use of antiviral agents) As described above, the antiviral agent of the present invention has excellent antiviral properties, and therefore, by being fixed to the surface of a molded body or being contained in a molded body, the metallic copper compound fine particle powder reacts with oxygen to generate active oxygen, thereby enabling the agent to exhibit excellent antiviral performance. For example, the antiviral agent can be prepared as a dispersion liquid by dispersing it in water such as purified water or ion-exchanged water; lower alcohols such as methanol, ethanol, propanol, isopropanol, or butanol; or general denatured alcohols such as methanol-modified, benzol-modified, triol-modified, methyl ethyl ketone-modified, denatonium benzoate-modified, or fragrance-modified; or the like, or the antiviral agent can be redispersed in a low-boiling point solvent such as the above-mentioned butyl acetate to prepare a dispersion liquid. When preparing the dispersion, it is preferable to add a dispersant to improve the dispersibility of the metallic copper fine particle powder constituting the antiviral agent in the dispersion medium. The amount of the dispersant to be added varies depending on the amount of metallic copper fine particles coated with fatty acid and / or ester compound of the fatty acid in the dispersion, but is preferably 0.01 to 2 mass% per dispersion medium. As the dispersant, a polymer dispersant having at least one of the following as an adsorption group: a primary, secondary or tertiary amine or an amine salt with a neutralized counter ion thereof, a carboxylic acid or a carboxylate, or a hydroxyl group, and having a fatty acid, polyether, polyester, polyurethane, or polyarylate in the main chain and side chain can be used. These dispersants have adsorption groups that adsorb to the surface of the copper compound microparticles, improve compatibility with non-aqueous solvents through the main chain or side chains, and generate repulsive forces due to steric hindrance of the polymer chains, suppressing aggregation of the copper compound microparticles, allowing them to be uniformly dispersed in the non-aqueous solvent, and eliminating aggregation over time. As the polymer dispersant, a type consisting of only a main chain, a type having a comb structure with side chains, or a type having a star structure can be used.
[0026] A dispersion containing such an antiviral agent is suitably used as a diluting solvent for a coating composition or a resin composition, and this makes it possible to impart antiviral performance to a coating film made of such a coating composition or a resin molded product made of a resin composition without impairing the transparency of the coating composition or resin composition. Examples of such coating compositions include those having a thermosetting resin such as a phenolic resin, an epoxy resin, a urethane resin, a melamine resin, a urea resin, an alkyd resin, an unsaturated polyester resin, or a silicone resin, or a photocurable acrylic resin as a base resin. In addition to the above-mentioned thermosetting resins, examples of the resin composition include olefin resins such as low-, medium-, and high-density polyethylene, linear low-density polyethylene, linear very low-density polyethylene, isotactic polypropylene, syndiotactic polypropylene, propylene-ethylene copolymer, polybutene-1, ethylene-butene-1 copolymer, propylene-butene-1 copolymer, and ethylene-propylene-butene-1 copolymer; polyester resins such as polyethylene terephthalate, polybutylene terephthalate, and polyethylene naphthalate; polyamide resins such as nylon 6, nylon 6,6, and nylon 6,10; and thermoplastic resins such as polycarbonate resins.
[0027] More specific examples of uses include molded articles obtained by using a nonwoven fabric, a resin film, a textile product, or the like as a substrate and applying a paint composition containing the antiviral composition to the surface of the substrate to form a coating film; and molded articles obtained by directly molding a resin composition containing the antiviral composition into a molded article such as a film, a sheet, a nonwoven fabric, or a fiber. EXAMPLES
[0028] Example 1 2.5% by mass of copper stearate was added to diethylene glycol and heated with stirring. After reaching 190°C, the mixture was heated for 2 hours and then cooled to 120°C or less, butyl acetate was added, and the mixture was stirred for about 1 minute. After the mixture was left to stand and the diethylene glycol layer and butyl acetate layer were separated, the butyl acetate layer was removed to obtain a diethylene glycol dispersion containing metallic copper particles. This diethylene glycol dispersion was suction filtered through a membrane filter having a pore size of 10 μm, washed with water, and then dried at 50° C. for 2 hours to obtain a fine metallic copper powder.
[0029] Example 2 A metallic copper fine particle powder was prepared in the same manner as in Example 1, except that the heating temperature was changed to 210°C.
[0030] Example 3 A metallic copper fine particle powder was prepared in the same manner as in Example 1, except that copper stearate was changed to copper laurate.
[0031] Example 4 A metallic copper fine particle powder was prepared in the same manner as in Example 1, except that copper stearate was changed to stearic acid and copper acetate.
[0032] Example 5 A metallic copper fine particle powder was prepared in the same manner as in Example 1, except that diethylene glycol was changed to ethylene glycol.
[0033] Example 6 A metallic copper fine particle powder was prepared in the same manner as in Example 1, except that diethylene glycol was changed to glycerin.
[0034] Example 7 2.5% by mass of copper stearate was added to the glycerin and heated with stirring. After heating for 2 hours from the point where the temperature reached 190°C, the glycerin dispersion was cooled to room temperature. The same amount of ethanol as the glycerin was added and stirred, and the mixture was suction filtered using a membrane filter with a pore size of 10 μm. The mixture was washed with hexane and butyl acetate to obtain a metallic copper fine particle powder.
[0035] Example 8 The fine copper metal powder of Example 7 was stored in the air for two months.
[0036] Example 9 The fine copper metal powder of Example 8 was stored in the air for 6 months.
[0037] [Preparation of metallic copper particle dispersion] Example 10 <In the case of aqueous dispersion> 0.5% by mass of a dispersant, DISPERBYK-2060 (manufactured by BYK-Chemie), was added to distilled water and stirred. Next, the copper metal fine particle powder obtained in Example 1 was added so that the copper metal content was 0.5% by mass, and stirred. Ultrasonic treatment was performed for 10 minutes to obtain a copper metal fine particle dispersion.
[0038] <Butyl acetate dispersion> 0.5% by mass of a dispersant, DISPERBYK-2090 (manufactured by BYK-Chemie), was added to butyl acetate and stirred. Next, the copper metal fine particle powder obtained in Example 1 was added so that the copper metal content was 0.5% by mass, and stirred. Ultrasonic treatment was performed for 10 minutes to obtain a copper metal fine particle dispersion.
[0039] Comparative Example 1 The preparation was carried out in the same manner as in Example 1, except that the heating temperature was changed to 250°C.
[0040] Comparative Example 2 A fine metallic copper powder was prepared in the same manner as in Example 7, except that the washing was carried out with ethanol.
[0041] Comparative Example 3 0.05% by mass of metallic copper microparticle reagent (Sigma-Aldrich) and 1.0% by mass of DISPERBYK-2090 were added to butyl acetate, and the mixture was stirred with an ultrasonic vibration device to obtain a dispersion.
[0042] (Evaluation of the surface composition of metallic copper particles) Approximately 0.1 g of metallic copper fine particle powder was molded into a circular shape with a diameter of approximately 5 mm using a KBr tablet molder. The molded product was measured using an X-ray photoelectron spectrometer K-Alpha (manufactured by Thermo Fisher Scientific Co., Ltd.) under the following conditions: measurement diameter: 0.4 mmφ, X-ray source: Al monochromator, measurement elements: Cu2p, O1s, C1s, step size: 0.1 eV. The component ratios were calculated from the areas of the metallic copper-derived peak (approximately 933 eV) and the copper oxide and other-derived peaks (approximately 935 eV) in the obtained chart.
[0043] (Antiviral evaluation) <In the case of aqueous dispersion> A coating liquid was prepared by mixing 90% by mass of a dispersion liquid adjusted so that the metal component concentration in the binder resin was 0.05% by mass with 9.95% by mass of an acrylic resin as the binder resin. An unprocessed nonwoven fabric was immersed in the coating liquid, taken out, and the excess liquid was removed with a roller-type wringer, and then dried in a dryer at 80°C for 5 minutes. It was then dried in a dryer at 150°C for 2 minutes to obtain a nonwoven fabric with metallic copper particles fixed thereon.
[0044] <In the case of solvent-based dispersion> A coating liquid was prepared by mixing 90% by mass of a dispersion liquid adjusted so that the metal component concentration in the binder resin was 0.05% by mass, 9.9% by mass of a photocurable acrylic resin as a binder resin, and 0.1% by mass of a photopolymerization initiator. An unprocessed nonwoven fabric was immersed in the coating liquid, taken out, and the excess liquid was removed with a roller-type wringer, and then dried in a dryer at 90°C for 2 minutes. After that, UV irradiation was performed for 10 minutes to obtain a nonwoven fabric with metallic copper particles fixed thereto.
[0045] (Method for evaluating antiviral properties of nonwoven fabric) 1. Host cells are infected with the virus, cultured, and then the cell debris is removed by centrifugation to obtain a virus suspension. 2. Dilute the virus suspension from step 1 above 10-fold with sterile distilled water to prepare the test virus suspension. 3. Inoculate 0.2 mL of the test virus suspension onto a 0.4 g test piece of nonwoven fabric. 4. After leaving the specimen at 25°C for 2 hours, add 20 mL of SCDLP medium and mix with a vortex mixer to wash out the virus from the specimen. 5. Measure the viral infectivity using the plaque assay method and calculate the antiviral activity value. 6. If the antiviral activity value is 3.0 or higher, it can be determined that the product has sufficient antiviral properties against that virus.
[0046] (Method for measuring the amount of organic coating) Using a thermogravimetric and differential thermogravimetric analyzer (TG / DTA7220, Hitachi High-Tech Science Corp.), approximately 10 mg of powder sample was heated in a nitrogen atmosphere to 600° C. at 10° C. / min. The weight loss from the obtained chart was taken as the amount of organic coating containing fatty acid and / or ester compound.
[0047] (Method for measuring the average primary particle size and average secondary particle size of metallic copper particles) Measurement method of average primary particle size: A powder sample was observed with a scanning electron microscope (S-4800, Hitachi High-Tech Science Co., Ltd.) and images were obtained. The average primary particle size was calculated using image analysis type particle size distribution measurement software Mac-View. Measurement method for average secondary particle size of powdered metallic copper fine particles: The average secondary particle size was measured by a wet method using a laser diffraction particle size distribution measuring device (SALD-3100, manufactured by Shimadzu Corporation).
[0048] The feasibility of producing metallic copper particles and the results of measuring the surface composition of the metallic copper particle aggregates by X-ray photoelectron spectroscopy are shown in Table 1. The antiviral properties of the nonwoven fabric against influenza virus and feline calicivirus are shown in Table 2. An X-ray photoelectron spectroscopy chart of the metallic copper particle aggregate of Example 1 is shown in FIG. 1, and an X-ray photoelectron spectroscopy chart of the metallic copper particle aggregate of Example 9 is shown in FIG.
[0049] [Table 1]
[0050] [Table 2] [Industrial Applicability]
[0051] The antiviral agent of the present invention, in the form of a dispersion, is contained as a diluent in a resin composition that constitutes a textile product or the like, or is directly applied to or impregnated into a textile product or the like, making it possible to impart antiviral properties to textile products such as paper products, masks, wet tissues, air conditioner filters, air purifier filters, clothing, work clothes, curtains, carpets, automotive parts, packaging parts, freshness-preserving materials, sheets, towels, bath mats, diaper covers, stuffed animals, slippers, shoe insoles, and cleaning supplies such as wipers. Furthermore, by using a low-boiling point solvent as the dispersion medium of the dispersion, it can also be used as a diluent for a paint composition or a resin composition, thereby making it possible to impart antiviral properties to the coating film or resin molded product. Furthermore, the material can be used for medical equipment, packaging films for medical equipment, waste containers, garbage bags, wall materials and floor materials in nursing homes or public facilities such as hospitals and schools, wax coating materials, and vomit disposal equipment. Furthermore, in addition to sanitary products, the composition can be used for a variety of applications, including conductive films, films, metal plates, glass plates, marine paints, heat exchanger fins, ceramic products such as tableware, rubber products, metal products such as faucets, additives for humidifiers, liquid detergents, ion adsorbents, and deodorants.
Claims
1. An antiviral agent comprising metallic copper microparticles coated with a fatty acid and / or an ester compound, wherein the amount of the fatty acid and / or ester compound coated on the metallic copper microparticles is 0.1 to 10 mass %, and when the surface of the metallic copper microparticle aggregate is measured by X-ray photoelectron spectroscopy, the ratio of metallic copper to all copper components at the depth where the metallic copper components are initially measured is maintained at 10% or more.
2. 2. The antiviral agent according to claim 1, wherein the average secondary particle size of the metallic copper particles is 100 nm to 500 μm.
3. 3. The antiviral agent according to claim 1, wherein the metallic copper fine particles are dispersed in a solvent.
4. 3. The antiviral agent according to claim 1, which is a resin composition in which the metallic copper fine particles are dispersed in a resin.
5. The antiviral agent according to any one of claims 1 to 4, wherein the antiviral agent contains the metallic copper fine particles in an amount of 0.01 to 2.0% by mass, and has an antiviral activity value of 3.0 or more.
Citation Information
Patent Citations
Kachoshikikuranpu
JP1976094185A
Method of manufacturing dispersion of metallic ultrafine particle modified by fatty acid
JP2009226400A
Ultrafine composite metal particles and method for manufacturing the same
JP2011052326A
Antimicrobial and antiviral composition and method of producing the same
JP2013082654A
Antiviral coating film
JP2015205998A