Photocurable resin composition and method for producing photo-modeled object using same
A photocurable resin composition combining triacrylate, diacrylate, and monoacrylamide compounds addresses the stability and strength challenges in stereolithography, achieving high heat resistance and mechanical strength with stable low-temperature performance.
Patent Information
- Application Number
- JP2020179162
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-10-26
- Publication Date
- 2024-10-23
- Estimated Expiration
- 2040-10-26
AI Technical Summary
Existing photocurable resin compositions used in stereolithography face challenges in achieving both high heat resistance and mechanical strength while maintaining stability during low-temperature storage, as triacrylate compounds with an isocyanuric ring and three (meth)acryloyl groups tend to crystallize and solidify, affecting workability and the curing reaction.
A photocurable resin composition comprising a triacrylate compound with an isocyanuric ring and three (meth)acryloyl groups, combined with a diacrylate and monoacrylamide compound, in specific mass proportions, to enhance heat resistance and mechanical strength while preventing solidification during low-temperature storage.
The composition provides stereolithographic objects with excellent heat resistance, mechanical strength, and stability during low-temperature storage, ensuring high workability and effective curing without solidification issues.
Smart Images

Figure 0007572207000008 
Figure 0007572207000001 
Figure 0007572207000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a photocurable resin composition and a method for producing a stereolithographic object using the same. [Background technology]
[0002] With the development of three-dimensional photo-fabrication technology such as 3D printers, there is an increasing demand for improved heat resistance and mechanical strength of photo-fabricated objects. For example, Patent Document 1 proposes a curable composition for a sheet used in three-dimensional molding, which contains a compound such as 2-hydroxyethyl acrylate, 2-hydroxyethyl methacrylate, a bifunctional or higher (meth)acrylate compound, and a photoradical polymerization initiator, does not contain a urethane (meth)acrylate compound, or the content of the urethane (meth)acrylate compound is more than 0 mass% and less than 4 mass% with respect to the total mass of the curable composition, and the molecular weight between crosslinking points of the obtained cured product is 50 g / mol or more and 2,000 g / mol or less. It also teaches that a bifunctional or higher (meth)acrylate compound having an isocyanuric ring structure can be used as the bifunctional or higher (meth)acrylate compound. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-19276 A Summary of the Invention [Problem to be solved by the invention]
[0004] The present inventors have found that a photocurable resin composition that gives a photo-modeled object with significantly improved heat resistance and mechanical strength can be obtained by using a triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups. However, a triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups has a high crystallinity at room temperature, and therefore there is a problem that a part or all of the photocurable resin composition solidifies during low-temperature storage. [Means for solving the problem]
[0005] One aspect of the present invention relates to a photocurable resin composition comprising a polymerizable compound and a photopolymerization initiator, the polymerizable compound comprising a first compound and a second compound each containing nitrogen, the first compound being a triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups, the second compound being at least one selected from the group consisting of a diacrylate compound having an isocyanuric ring and two (meth)acryloyl groups, and a monoacrylamide compound having one (meth)acryloyl group, and the proportion of the first compound in the total mass of the first compound and the second compound is 50 mass% or more and 90 mass% or less.
[0006] Another aspect of the present invention relates to a method for producing a photo-molded object, comprising the steps of: forming a liquid film of the photo-curable resin composition and photo-curing the liquid film to form a pattern; forming another liquid film in contact with the pattern; and photo-curing the other liquid film on the pattern to laminate the other pattern. Effect of the Invention
[0007] The present invention provides a photocurable resin composition which has excellent stability during low-temperature storage and which can give a stereolithographic object having excellent heat resistance and mechanical strength. [Brief description of the drawings]
[0008] [Figure 1] FIG. 2 is a schematic diagram for explaining a process of forming a stereolithography object using a photocurable resin composition according to one embodiment of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The photocurable resin composition according to the embodiment of the present invention will be specifically described, but the present invention is not limited to the following embodiment, and various changes and modifications are possible.
[0010] In addition, the (meth)acryloyl group means an acryloyl group, a methacryloyl group, or both of these. Similarly, the (meth)acrylate means an acrylate, a methacrylate, or both of these. Similarly, the term "(meth)acrylic" means "acrylic" or "methacrylic", or both of these.
[0011] A photo-modeled object needs heat resistance and mechanical strength necessary to express the function of the photo-modeled object. On the other hand, a photo-curable resin composition that gives such a photo-modeled object by curing is required to have not only photo-curability but also excellent workability, reactivity, etc. A triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups contributes greatly to improving the heat resistance and mechanical strength of a photo-modeled object, but may crystallize during low-temperature storage and solidify at least a part of the photo-curable resin composition. When a photo-curable resin composition solidifies, not only does its workability decrease, but the curing reaction of the solidified part is restricted, and the expected physical properties of the photo-modeled object may not be obtained. There is often a trade-off between the heat resistance and mechanical strength of the photo-modeled object and the stability of the photo-curable resin composition during low-temperature storage, and it is difficult to achieve both. Furthermore, a photo-modeled object is required to have low shrinkage during curing and shape accuracy, etc. A photo-curable resin composition is required to have low viscosity and a fast curing speed, etc.
[0012] The photocurable resin composition according to an embodiment of the present invention (hereinafter also referred to as "photocurable resin composition A") and a stereolithographic object formed using the same can satisfy the various requirements described above with a high degree of satisfaction.
[0013] [Photocurable resin composition A] The photocurable resin composition A includes a polymerizable compound and a photopolymerization initiator. The polymerizable compound includes a first compound and a second compound, each of which contains nitrogen.
[0014] The first compound is a triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups, which significantly contributes to improving the heat resistance and mechanical strength of the stereolithography object. Meanwhile, the second compound is at least one selected from the group consisting of a diacrylate compound having an isocyanuric ring and two (meth)acryloyl groups and a monoacrylamide compound having one (meth)acryloyl group, which contributes to improving the heat resistance and mechanical strength of the stereolithography object and also suppresses the solidification of the photocurable resin composition A during low-temperature storage caused by the first compound.
[0015] Here, the ratio of the first compound to the total mass of the first compound and the second compound is 50 mass% or more and 90 mass% or less. Although the photocurable resin composition A having this composition contains a fairly large amount of the first compound, it is difficult to solidify when stored at low temperatures and has excellent storage stability.
[0016] If the ratio of the first compound to the total mass of the first compound and the second compound is less than 50% by mass, it is difficult to achieve both the heat resistance and mechanical strength of the photo-modeled object with sufficient satisfaction. Also, if the ratio of the first compound to the total mass of the first compound and the second compound exceeds 90% by mass, it is difficult to ensure the stability of the photocurable resin composition A during low-temperature storage. In order to achieve both the heat resistance and mechanical strength of the photo-modeled object and the stability of the photocurable resin composition A during low-temperature storage with a higher degree of satisfaction, it is desirable to set the ratio of the first compound to the total mass of the first compound and the second compound to 60% by mass or more and 87% by mass or less.
[0017] [Polymerizable compound] The polymerizable compound is not particularly limited, but refers to a compound that undergoes chain polymerization, and chain polymerization includes addition polymerization, ring-opening polymerization, etc. Load polymerization includes radical polymerization, cationic polymerization, anionic polymerization, coordination polymerization, etc. The polymerization reaction may be photosensitized polymerization. The polymerizable compound includes polymerizable monomers, polymerizable oligomers, etc.
[0018] The term "polymerizable" in polymerizable monomers and polymerizable oligomers means that the monomer or oligomer has a polymerizable group that participates in a curing reaction using a photopolymerization initiator. A polymerizable oligomer is one that contains at least a repeating portion of a structural unit (the number of repeats is 2 or more), and is distinguished from a polymerizable monomer.
[0019] The viscosity of the photocurable resin composition A is, for example, 10 mPa·s or more and 3000 mPa·s or less at 25° C. In order to easily ensure high photo-modeling properties, the viscosity at 25° C. is preferably 2000 mPa·s or less, and more preferably 1000 mPa·s or less. The viscosity of the photocurable resin composition A can be measured, for example, using a cone-plate type E-type viscometer at a rotation speed of 20 rpm.
[0020] The polymerizable compound can be separated from the photocurable resin composition A by using a known separation method such as, for example, centrifugation, extraction, crystallization, column chromatography, recrystallization, etc. The polymerizable compound can be identified by, for example, analyzing the photocurable resin composition A by gas chromatography, liquid chromatography, mass spectrometry, etc.
[0021] [First compound] The first compound is a triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups (hereinafter, also referred to as "triacrylate compound A"). Triacrylate compound A is classified as a polymerizable monomer. A cured product containing triacrylate compound A as a main component has a Tg of, for example, 230°C or higher. Here, the main component means that 50% by mass or more (for example, 70% by mass or more) of the cured product is derived from the first compound. The first compound is a component that greatly contributes to improving the heat resistance and mechanical strength of the stereolithography object.
[0022] On the other hand, the first compound alone is solid at room temperature and has high crystallinity, which greatly affects the storage stability of the photocurable resin composition. In order to sufficiently improve the heat resistance and mechanical strength of the stereolithography object while ensuring the stability of the photocurable resin composition during low-temperature storage, it is necessary to use the first compound in combination with at least the second compound.
[0023] The triacrylate compound A has three substituents bonded to the three nitrogen atoms of the isocyanuric ring, respectively. Each of the three substituents has a (meth)acryloyl group. The triacrylate compound A is, for example, a compound represented by the formula (1):
[0024] [ka]
[0025] Here, R1, R2 and R3 are each an independent organic group. The organic group is preferably a linear or branched aliphatic group, and at least one of the hydrogen atoms of the aliphatic group may be substituted. Among them, a linear alkylene group is preferable in that it has a small steric hindrance and is easy to ensure a high Tg. That is, the triacrylate compound A may contain a tris(acryloyloxyalkyl)isocyanurate having three acryloyloxyalkyl groups as three substituents. Here, the number of carbon atoms in the alkylene chain of the three acryloyloxyalkyl groups is preferably 1 to 4, and may be 2 to 3, each independently, in that it has a smaller steric hindrance and is easy to ensure a higher Tg. For example, the acryloyloxyalkyl group may be an acryloyloxyethyl group. Specifically, the triacrylate compound A is represented by the formula (2):
[0026] [ka]
[0027] The triacrylate compound A may be a tris(2-acryloyloxyethyl)isocyanurate (or a tris(2-hydroxyethyl)isocyanurate triacrylate) represented by the formula: The triacrylate compound A may be used alone or in combination of two or more kinds, and 70% by mass or more, further 90% by mass or more, or 100% of the triacrylate compound A may be tris(acryloyloxyalkyl)isocyanurate or tris(2-acryloyloxyethyl)isocyanurate.
[0028] [Second compound] The second compound is at least one selected from the group consisting of a diacrylate compound having an isocyanuric ring and two (meth)acryloyl groups (hereinafter also referred to as "diacrylate compound A") and a monoacrylamide compound having one (meth)acryloyl group (hereinafter also simply referred to as "monoacrylamide compound A"). The second compound containing nitrogen has a high affinity with the first compound containing nitrogen and is difficult to solidify, so that when it coexists with the first compound which is easy to solidify, it has the effect of highly suppressing the solidification of the first compound.
[0029] (Diacrylate Compound A) The diacrylate compound A has a structure in which one of the three substituents of the triacrylate compound A is replaced with a substituent or atom (e.g., hydrogen, fluorine, etc.) that does not have a (meth)acryloyl group. A cured product containing the diacrylate compound A as a main component has high heat resistance and mechanical strength. Here, the main component means that 50 mass % or more (e.g., 70 mass % or more) of the cured product is derived from the diacrylate compound A.
[0030] The substituents that do not have a (meth)acryloyl group include a hydroxyalkyl group, an allyl group (CH 2 =CH-CH 2-) and the like. The number of carbon atoms in the alkylene chain of the hydroxyalkyl group is preferably 1 to 4, and may be 2 to 3, in terms of less steric hindrance and easiness in securing a higher Tg. For example, the hydroxyalkyl group may be a 2-hydroxyethyl group. The diacrylate compound A may be used alone or in combination of two or more kinds, and 70% by mass or more, further 90% by mass or more, or 100% of the diacrylate compound A may be trishydroxyalkylisocyanurate diacrylate or tris2-hydroxyethylisocyanurate diacrylate.
[0031] The second compound may be 50% by mass or more of the diacrylate compound A, or 70% by mass or more or 90% by mass or more of the diacrylate compound A. In this way, when the main component of the second compound is the diacrylate compound A, the total ratio of the first compound and the second compound to the mass of the polymerizable compound may be 30% by mass or more, 35% by mass or more, or 40% by mass or more. In addition, the total ratio of the first compound and the second compound to the mass of the polymerizable compound may be 60% by mass or less, 55% by mass or less, 50% by mass or less, or 45% by mass or less. When limiting the range, these upper and lower limits can be arbitrarily combined. For example, the total ratio of the first compound and the second compound to the mass of the polymerizable compound may be 30% by mass or more and 60% by mass or less, 30% by mass or more and 50% by mass or less, or 35% by mass or more and 55% by mass or less.
[0032] (Monoacrylamide compound A) The monoacrylamide compound A can be in a low-viscosity liquid state at room temperature (25° C.). In addition, a cured product containing the monoacrylamide compound A as a main component can have a Tg of, for example, 130° C. or higher, and therefore a shaped product having high mechanical strength can be easily obtained. Here, the main component means that 50% by mass or more (for example, 70% by mass or more) of the cured product is derived from the monoacrylamide compound A.
[0033] The monoacrylamide compound A can be obtained, for example, as an acid amide of a nitrogen-containing compound and (meth)acrylic acid. Examples of the nitrogen-containing compound constituting the (meth)acrylic acid and acid amide include aliphatic amines (triethylamine, ethanolamine, etc.), alicyclic amines (cyclohexylamine, etc.), aromatic amines (aniline, etc.), and nitrogen-containing cyclic compounds. The nitrogen-containing cyclic compounds have a heterocycle containing a nitrogen atom, and the heterocycle is preferably a 5-membered to 8-membered ring, and may be a 5-membered or 6-membered ring. The heterocycle may be a heterocycle containing ether oxygen or the like. Specific examples of the nitrogen-containing cyclic compounds include pyrrole, pyrrolidine, piperidine, pyrimidine, morpholine, and thiazine. The heterocycle may have aromaticity, but is preferably an alicyclic ring.
[0034] Among them, heterocyclic (meth)acrylamides having a heterocycle containing a nitrogen atom have a lower viscosity, a smaller steric hindrance, and are easy to secure a high Tg. Acryloylmorpholine may be used as the monoacrylamide compound A. 70% by mass or more, further 90% by mass or more, or 100% of the monoacrylamide compound A may be heterocyclic (meth)acrylamide or acryloylmorpholine.
[0035] As the monoacrylamide compound A other than acryloylmorpholine, for example, N-alkyl(meth)acrylamide, N,N-dialkyl(meth)acrylamide, etc. may be used. Here, the hydrogen atom of the alkyl group may be substituted with a hydroxy group, an amino group, etc. The number of carbon atoms of the alkyl group may be, for example, 1 to 6. More specifically, dimethylacrylamide, isopropylacrylamide, diethylacrylamide, hydroxyethylacrylamide, etc. may be used.
[0036] The second polymerizable compound may be 50% by mass or more of the monoacrylamide compound A, or may be 70% by mass or more or 90% by mass or more of the monoacrylamide compound A. In this way, when the main component of the second compound is the monoacrylamide compound A, the total ratio of the first compound and the second compound to the mass of the polymerizable compound may be 50% by mass or more, 55% by mass or more, or 60% by mass or more. In addition, the total ratio of the first compound and the second compound to the mass of the polymerizable compound may be 80% by mass or less, 75% by mass or less, or 70% by mass or less. When limiting the range, these upper and lower limits can be arbitrarily combined. For example, the total ratio of the first compound and the second compound to the mass of the polymerizable compound may be 50% by mass or more and 80% by mass or less, 55% by mass or more and 75% by mass or less, or 60% by mass or more and 75% by mass or less.
[0037] [Third compound] The polymerizable compound contained in the photocurable resin composition A may further include a third compound different from the first compound and the second compound. Polymerizable compounds other than the first compound and the second compound are classified as third compounds. The content of the third compound in the photocurable resin composition is determined by the total content of the first compound and the second compound. The third compound will be described below.
[0038] (Polymerizable monomer) The polymerizable monomer that can be used as the third compound may be monofunctional or polyfunctional. The polymerizable group of the polymerizable monomer may be, for example, a group having a polymerizable carbon-carbon unsaturated bond such as a vinyl group, an allyl group, an acryloyl group, or a methacryloyl group, and the (meth)acryloyl group is preferred. In this case, a high curing speed is obtained, and it is suitable for modeling applications such as photo-modeling.
[0039] Examples of the monofunctional polymerizable monomer (hereinafter also referred to as the first monomer) include vinyl monomers, allyl monomers, and acrylic monomers. Examples of the vinyl monomers include monomers having a vinyl group, such as vinyl ethers of monohydric alcohols, aromatic vinyl monomers (styrene, etc.), alicyclic vinyl monomers, and heterocyclic compounds having a vinyl group (N-vinylpyrrolidone, etc.). Examples of the allyl monomers include monomers having an allyl group, such as allyl ethers of monohydric alcohols. Examples of the acrylic monomers include monomers having a (meth)acryloyl group, such as (meth)acrylic acid esters of monohydric alcohols, and (meth)acrylic acid. The first monomer may be used alone or in combination of two or more.
[0040] The monohydric alcohol may be any of aliphatic alcohols, alicyclic alcohols, and aromatic alcohols. The aliphatic alcohols may have an aromatic ring, an aliphatic ring, or a heterocyclic ring. The aliphatic ring may be a bridged ring. Examples of the aliphatic alcohol include alkyl alcohols (C 111, 112, 113, 114, 115, 116, 117, 118, 119, 120, 121, 122, 123, 124, 125, 126, 127, 128, 129, 130, 131, 132, 133, 134, 135, 136, 137, 138, 139, 140, 141, 142, 143, 144, 145, 146, 147, 148, 149, 150, 151, 152, 153, 154, 155, 156, 157, 158, 159, 160, 161, 162, 163, 164, 165, 166, 167, 168, 169, 170, 171, 172, 173, 174, 175, 176, 177, 178, 179 ... 1-20 Examples of the alicyclic alcohol include alicyclic C cyclohexanol, menthol, borneol, isoborneol, dicyclopentanyl alcohol, etc. 5-20 Alcohol (alicyclic C 5-10 Aromatic alcohols include aromatic C alcohols such as phenol and naphthol. 6-10 Examples of heterocyclic alcohols include aliphatic alcohols (C1-4 Examples of heterocyclic alcohols include furfuryl alcohol and tetrahydrofurfuryl alcohol.
[0041] The polymerizable monomer preferably has an aliphatic ring. In this case, the curing reaction proceeds efficiently, a high-strength molded object is easily obtained, and distortion during curing is reduced. Specifically, it is preferable to use an ester of an alicyclic alcohol and (meth)acrylic acid as the polymerizable monomer.
[0042] When a polyfunctional polymerizable monomer (hereinafter also referred to as a second monomer) is used, a crosslinked structure is formed by curing, which makes it easier to further increase the strength of the cured product. As the second monomer, one having two or more polymerizable groups can be used. The number of polymerizable groups is, for example, 2 to 4, and may be 2 or 3. The second monomer may be used alone or in combination of two or more types. When multiple types of second monomers are used, the types of polymerizable groups in each second monomer may all be the same, some may be the same, or all may be different.
[0043] The second monomer may be, for example, a compound in which at least two hydroxyl groups of a polyol are replaced with at least one selected from the group consisting of a vinyl ether group, an allyl ether group, an acryloyloxy group, and a methacryloyloxy group. The polyol may be any of an aliphatic polyol, an alicyclic polyol, and an aromatic polyol. The alkylene glycol may be, for example, a C 10 polyol such as ethylene glycol, trimethylene glycol, 1,4-butanediol, or hexanediol. 2-10Examples of the aliphatic polyol include alkylene glycol. Aliphatic polyols include those having an aromatic ring, an aliphatic ring, or a heterocyclic ring. Examples of such aliphatic polyols include cyclohexane dimethanol, benzene dimethanol, and dioxane glycol. It is preferable that the second monomer (specifically, the polyol forming the second monomer) has an aliphatic ring or a heterocyclic ring. In this case, the curing reaction is likely to proceed efficiently. In addition, a molded object having high strength is likely to be obtained, and distortion during curing is small. More specifically, it is preferable to use a heterocyclic compound having a vinyl group, an ester of an alicyclic alcohol and (meth)acrylic acid, an ester of a heterocyclic alcohol and (meth)acrylic acid (e.g., dioxane glycol diacrylate), or the like as the second monomer.
[0044] Specific examples of preferable third compounds will be described in further detail below. (Polycyclic Aliphatic Di(meth)acrylates) A cured product mainly composed of a polycyclic aliphatic di(meth)acrylate can have a Tg of, for example, 170°C or higher, so that a shaped product having high mechanical strength is easily obtained, and distortion during curing is small. In addition, a polycyclic aliphatic di(meth)acrylate has a low viscosity and a fast curing speed. A polycyclic aliphatic refers to an aliphatic compound having two or more carbon rings among alicyclic compounds. Examples of a polycyclic aliphatic include bicycloundecane, decahydronaphthalene, and tricyclodecane dimethanol. A polycyclic aliphatic di(meth)acrylate has a structure in which at least two hydroxyl groups of a polycyclic aliphatic polyol are replaced with (meth)acryloyloxy groups, for example. A specific example of a typical polycyclic aliphatic di(meth)acrylate with a high Tg of a cured product is tricyclodecane dimethanol diacrylate. The structure of tricyclodecane dimethanol diacrylate is shown below.
[0045] [ka]
[0046] (Poly(meth)acrylate having four or more (meth)acryloyl groups) A cured product mainly composed of a poly(meth)acrylate having four or more (meth)acryloyl groups can have a Tg of, for example, 230° C. or higher, and therefore can easily produce a shaped product having high mechanical strength. In consideration of the shrinkage rate during curing, the number of (meth)acryloyl groups in the poly(meth)acrylate having four or more (meth)acryloyl groups is preferably 6 or less, and more preferably 5 or less.
[0047] A poly(meth)acrylate having four or more (meth)acryloyl groups has a structure in which at least four hydroxyl groups of an aliphatic polyol having four or more hydroxyl groups are replaced with (meth)acryloyloxy groups. Examples of aliphatic polyols having four or more hydroxyl groups include ditrimethylolpropane, pentaerythritol, dipentaerythritol, and sugar alcohols. Specific examples of poly(meth)acrylates having four or more (meth)acryloyl groups include ditrimethylolpropane tetraacrylate, pentaerythritol tetraacrylate, and dipentaerythritol hexaacrylate. Among them, ditrimethylolpropane tetraacrylate is preferred in that the cured product has a high Tg, high low-temperature stability, low viscosity, and a relatively small shrinkage rate during curing. The structure of ditrimethylolpropane tetraacrylate is shown below.
[0048] [ka]
[0049] The total proportion of the polycyclic aliphatic di(meth)acrylate and the poly(meth)acrylate having four or more (meth)acryloyl groups in the third compound is desirably 90 mass % or more.
[0050] (Third compound having an isocyanuric ring) The third compound may include, for example, a monoacrylate compound having an isocyanuric ring and one (meth)acryloyl group (hereinafter also referred to as "monoacrylate compound A"). The monoacrylate compound A has a structure in which two of the three substituents of the triacrylate compound A are replaced with a substituent or atom (e.g., hydrogen, fluorine, etc.) that does not have a (meth)acryloyl group. The substituent that does not have a (meth)acryloyl group is the same as that of the diacrylate compound A. Specific examples of the monoacrylate compound A include trishydroxyalkylisocyanurate monoacrylate and tris2-hydroxyethylisocyanurate monoacrylate.
[0051] The third compound may contain triallyl isocyanurate. Triallyl isocyanurate has an isocyanuric ring and three allyl groups, so that it is expected to have improved heat resistance and mechanical strength similar to those of the first and second compounds.
[0052] Preferred embodiments of the present invention are listed below. (First embodiment) A polymerizable compound and a photopolymerization initiator are included, the polymerizable compound includes a first compound and a second compound each containing nitrogen; the first compound is a triacrylate compound A having an isocyanuric ring and three (meth)acryloyl groups; the second compound is at least one selected from the group consisting of a diacrylate compound A having an isocyanuric ring and two (meth)acryloyl groups and a monoacrylamide compound A having one (meth)acryloyl group; a ratio of the first compound to a total mass of the first compound and the second compound is 50 mass% or more and 90 mass% or less, a total mass ratio of the first compound and the second compound in the polymerizable compound is 20 mass % or more and 80 mass % or less.
[0053] Second embodiment In the first embodiment, 50% by weight or more, further 70% by weight or more, and further 90% by weight or more of the second compound is the diacrylate compound A; a total ratio of the first compound and the second compound to the mass of the polymerizable compound is 35 mass% or more and 60 mass% or less, or 35 mass% or more and 55 mass% or less, or 40 mass% or more and 50 mass% or less.
[0054] Third embodiment In the first embodiment, 50% by mass or more, further 70% by mass or more, further 90% by mass or more of the second polymerizable compound is the monoacrylamide compound A, a total ratio of the first compound and the second compound to the mass of the polymerizable compound is 50 mass% or more and 80 mass% or less, or 55 mass% or more and 75 mass% or less, or 60 mass% or more and 70 mass% or less.
[0055] (Fourth embodiment) In a first embodiment, the photocurable resin composition further includes a polycyclic aliphatic di(meth)acrylate, and a proportion of the polycyclic aliphatic di(meth)acrylate in the mass of the polymerizable compound is 15 mass% or more and 60 mass% or less.
[0056] Fifth embodiment In a second embodiment, the photocurable resin composition further includes a polycyclic aliphatic di(meth)acrylate, and a proportion of the polycyclic aliphatic di(meth)acrylate in the mass of the polymerizable compound is 30 mass% or more and 60 mass% or less, or 35 mass% or more and 55 mass% or less.
[0057] Sixth embodiment In a third embodiment, the photocurable resin composition further includes a polycyclic aliphatic di(meth)acrylate, and a proportion of the polycyclic aliphatic di(meth)acrylate in the mass of the polymerizable compound is 15 mass% or more and 40 mass% or less, or 20 mass% or more and 35 mass% or less.
[0058] Seventh embodiment In a fourth embodiment, the photocurable resin composition further comprises a poly(meth)acrylate having four or more (meth)acryloyl groups, and the proportion of the poly(meth)acrylate having four or more (meth)acryloyl groups in the mass of the polymerizable compound is 5 mass% or more and 20 mass% or less.
[0059] Eighth embodiment In a fifth or sixth embodiment, the photocurable resin composition further comprises a poly(meth)acrylate having four or more (meth)acryloyl groups, and the proportion of the poly(meth)acrylate having four or more (meth)acryloyl groups in the mass of the polymerizable compound is 5 mass% or more and 15 mass% or less.
[0060] [Photopolymerization initiator] The photopolymerization initiator contained in the photocurable resin composition A is activated by the action of light to initiate polymerization of the polymerizable compound. Examples of the photopolymerization initiator include radical polymerization initiators that generate radicals by the action of light, as well as those that generate acids (or cations) by the action of light (specifically, cation generators). The photopolymerization initiator may be used alone or in combination of two or more. The photopolymerization initiator is selected depending on the type of the polymerizable compound, for example, whether it is radically polymerizable or cationic polymerizable. Examples of the radical polymerization initiator (radical photopolymerization initiator) include alkylphenone-based photopolymerization initiators and acylphosphine oxide-based photopolymerization initiators. Examples of the photopolymerization initiator are shown below, but are not limited to these.
[0061] Examples of alkylphenone photopolymerization initiators include 2,2-dimethoxy-1,2-diphenylethan-1-one, 1-hydroxy-cyclohexyl-phenyl-ketone, 2-hydroxy-2-methyl-1-phenyl-propan-1-one, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methyl-propionyl)-benzyl]phenyl}-2-methyl-propan-1-one, 2-methyl-1-(4-methylthiophenyl)-2-morpholinopropan-1-one, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and the like.
[0062] Examples of the acylphosphine oxide photopolymerization initiator include 2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide, bis(2,4,6-trimethylbenzoyl)-phenyl-phosphine oxide, and the like. (others) The photocurable resin composition A may further contain other known additives, such as a thiol compound, an amine compound, a colorant, a UV absorber, an antioxidant, a polymerization inhibitor, a defoamer, a filler, and a stabilizer.
[0063] (Storage stability) Photocurable resin composition A desirably satisfies at least condition 1 of the following <Conditions 1 to 3>, more desirably satisfies conditions 1 and 2, and most desirably satisfies all of conditions 1 to 3.
[0064] <Condition 1> When the photocurable resin composition A is cooled at -30°C for 72 hours, heated to 23°C, and then allowed to stand at 23°C for 48 hours, the entire photocurable resin composition A becomes liquid. After cooling at -30°C for 72 hours, the photocurable resin composition A may be in a solidified state.
[0065] <Condition 2> When the photocurable resin composition A, which is entirely liquid, is allowed to stand at 5° C. for one month, the photocurable resin composition A remains entirely liquid thereafter.
[0066] <Condition 3> When 0.1 mass % of crystals of tris(2-acryloyloxyethyl)isocyanurate (triacrylate compound A) are added to photocurable resin composition A, which is liquid as a whole, and the composition is allowed to stand at 5°C for 72 hours, the entire photocurable resin composition A (excluding the added crystals) remains liquid even after the addition.
[0067] Photocurable resin composition A that satisfies condition 1 can be stored, for example, in a frozen state, because even if at least a portion of photocurable resin composition A solidifies at an extremely low temperature, it will return to a stable liquid state when it is subsequently returned to room temperature (23°C).
[0068] Photocurable resin composition A that satisfies condition 2 always maintains a stable liquid state throughout, even when stored for a long period of time at low temperature (5°C), and therefore photocurable resin composition A can be used safely even in winter or in cold regions.
[0069] Photocurable resin composition A that satisfies condition 3 can be said to have extremely high stability, even if seed crystals are added, because the seed crystals do not induce solidification and the composition can maintain a liquid state.
[0070] The photocurable resin composition A is suitable for forming a three-dimensional photo-modeled object (also called a "photo-modeled object" or a "cured object") by curing it by irradiation with light. The present invention also includes a photo-modeled object of the photocurable resin composition A. The photo-modeled object has, for example, a layered structure in which a layered cured pattern formed by photocuring is laminated in multiple layers. Such a photo-modeled object can be manufactured by a 3D printer. That is, the photocurable resin composition A is suitable as a three-dimensional photo-modeling material for a 3D printer.
[0071] [Stereolithography] Stereolithography is used in a variety of applications that require high heat resistance and mechanical strength, such as electronic devices, electrical devices, medical devices, electrical appliances, robot-related products, and vehicle-related products.
[0072] The stereolithography can be produced by a production method including, for example, a step (i) of forming a liquid film of a photocurable resin composition and curing the liquid film to form a pattern, a step (ii) of forming another liquid film so as to be in contact with the pattern, and a step (iii) of curing the other liquid film on the pattern to laminate another pattern. Usually, the steps (ii) and (iii) are subsequently repeated several times.
[0073] (Heavy Deflection Temperature (HDT)) The deflection temperature under load (HDT) of the cured product of the photocurable resin composition A is measured by an edgewise method at a load of 0.45 MPa in accordance with ASTM D648. The HDT is, for example, 200°C or higher, and depending on the composition of the photocurable resin composition A, an HDT of 240°C or higher or 280°C or higher can be achieved. Such a cured product can be said to have extremely high heat resistance.
[0074] The deflection temperature under load (HDT) is measured using a test piece formed from a cured product of the photocurable resin composition A or a photo-fabricated product. The test piece used is 12.7 mm in height, 6.4 mm in width, and 127 mm in length. The deflection temperatures under load (HDT) of multiple (e.g., five) test pieces are measured and averaged to obtain an average value. HDT is the temperature at which the deflection amount becomes 2.6 mm.
[0075] (Tensile strength) The tensile strength of the cured product of the photocurable resin composition A is measured in accordance with ASTM D638. The tensile strength is, for example, 50 MPa or more, and can reach 60 MPa or more or 70 MPa or more depending on the composition of the photocurable resin composition A. Such a cured product can be said to have extremely high mechanical strength.
[0076] The tensile strength is measured using a test piece formed from a cured product of the photocurable resin composition A or a photo-fabricated product. The test piece is usually 4 mm thick, 6 mm wide at the parallel part, 115 mm long, and 33 mm long at the parallel part (Type IV). The measurement is performed under the conditions of 23°C, 65 mm distance between chucks, and 5 mm / min tensile speed. A commercially available tensile tester is used for the measurement. The tensile strength is the maximum stress measured until the test piece breaks. The tensile strength is measured for multiple (e.g., five) test pieces, and the average value is calculated by averaging.
[0077] The test pieces for HDT and tensile strength are produced, for example, by a method for producing a stereolithography object by repeating steps (i) to (iii) described below. The thickness of the liquid film or two-dimensional pattern per layer is 25 μm to 100 μm.
[0078] [Method of manufacturing optically modeled objects] The method for producing a stereolithography product includes a step of forming a stereolithography product using a photocurable resin composition A. The step of forming a stereolithography product includes a step (i) of forming a liquid film of the photocurable resin composition A and photocuring the liquid film to form a pattern, a step (ii) of forming another liquid film so as to be in contact with the pattern, and a step (iii) of photocuring the other liquid film on the pattern to laminate another pattern.
[0079] The procedure for bat-type stereolithography is illustrated below. Fig. 1 shows an example of forming a three-dimensional object using a photo-fabrication apparatus (patterning apparatus) equipped with a resin tank (vat). In the illustrated example, a suspension-type modeling is shown, but there is no particular limitation as long as it is a method capable of performing three-dimensional photofabrication using a photocurable resin composition. There is also no particular limitation on the type of light irradiation (exposure), and it may be point exposure or surface exposure.
[0080] The patterning apparatus 1 includes a platform 2 having a pattern forming surface 2a, a resin tank 3 containing a photocurable resin composition 5, and a projector 4 as a light source for a surface exposure system.
[0081] (i) A step of forming a liquid film and curing it to form a pattern In step (i), as shown in (a), first, the pattern-forming surface 2a of the platform 2 is immersed in the photocurable resin composition 5 contained in the resin tank 3 while facing the projector 4 (i.e., the bottom surface of the resin tank 3). At this time, the height of the pattern-forming surface 2a (or the platform 2) is adjusted so that a liquid film 7a (liquid film a) is formed between the pattern-forming surface 2a and the projector 4 (or the bottom surface of the resin tank 3). Next, as shown in (b), light L is irradiated (surface exposure) from the projector 4 toward the liquid film 7a, thereby photocuring the liquid film 7a and forming a pattern 8a (pattern a).
[0082] In the patterning apparatus 1, the resin tank 3 serves as a supply unit for the photocurable resin composition 5. It is desirable that at least a portion of the resin tank between the liquid film and the projector 4 (the bottom surface in the illustrated example) is transparent to the exposure wavelength so that the liquid film is irradiated with light from the light source. The shape, material, size, etc. of the platform 2 are not particularly limited.
[0083] After the liquid film a is formed, the liquid film a is photocured by irradiating light from a light source toward the liquid film a. The light irradiation can be performed by a known method. The exposure method is not particularly limited, and may be point exposure or surface exposure. As the light source, a known light source used for photocuring can be used. In the case of the point exposure method, for example, a plotter type, a galvano laser (or galvano scanner) type, an SLA (stereolithography) type, etc. can be mentioned. In the case of the surface exposure method, it is convenient to use a projector as the light source. As the projector, an LCD (transmissive liquid crystal) type, an LCoS (reflective liquid crystal) type, and a DLP (registered trademark, Digital Light Processing) type can be exemplified. The exposure wavelength can be appropriately selected according to the components of the photocurable resin composition (particularly, the type of initiator).
[0084] (ii) forming a liquid film between the pattern a and the light source In step (ii), a photocurable resin composition is supplied between the pattern a obtained in step (i) and a light source to form a liquid film (liquid film b). That is, the liquid film b is formed on the pattern a formed on the pattern formation surface. For the supply of the photocurable resin composition, the explanation for step (i) can be referred to.
[0085] 1(c), after the two-dimensional pattern 8a (two-dimensional pattern a) is formed, the pattern forming surface 2a may be raised together with the platform 2. Then, a photocurable resin composition 5 is supplied between the two-dimensional pattern 8a and the bottom surface of the resin tank 3, whereby a liquid film 7b (liquid film b) can be formed.
[0086] (iii) A process of laminating another pattern b on the pattern a In step (iii), the liquid film b formed in step (ii) is exposed to light from a light source to photocure the liquid film b, and another pattern (pattern b obtained by photocure of the liquid film b) is laminated on the pattern a. By laminating the patterns in this way in the thickness direction, a three-dimensional modeling pattern can be formed.
[0087] For example, as shown in (d) of FIG. 1, the liquid film 7b (liquid film b) formed between the pattern 8a (pattern a) and the bottom surface of the resin tank 3 is exposed to light from the projector 4 to photo-cure the liquid film 7b. This photo-cure converts the liquid film 7b into the pattern 8b (pattern b). In this way, the pattern 8b can be laminated on the pattern 8a. For the light source, exposure wavelength, etc., see the description of step (i).
[0088] (iv) Repeating steps (ii) and (iii) The first step may include a step (iv) of repeating the steps (ii) and (iii) multiple times. This step (iv) results in multiple patterns b being stacked in the thickness direction, resulting in a more three-dimensional shaping pattern. The number of repetitions may be appropriately determined depending on the shape and size of the desired three-dimensional object (three-dimensional shaping pattern).
[0089] For example, as shown in FIG. 1(e), the platform 2 is raised with the pattern 8a (pattern a) and the pattern 8b (pattern b) laminated on the pattern forming surface 2a. At this time, a liquid film 7b (liquid film b) is formed between the pattern 8b and the bottom surface of the resin tank 3. Then, as shown in FIG. 1(f), the projector 4 exposes the liquid film 7b to light, and the liquid film 7b is photocured. As a result, another pattern 8b (pattern b) is formed on the pattern 8b. Then, by alternately repeating (e) and (f), a plurality of patterns 8b (two-dimensional patterns b) can be laminated.
[0090] When uncured photocurable resin composition remains on the three-dimensionally shaped pattern obtained in step (iii) or (iv), the pattern may be subjected to a cleaning treatment using a solvent.
[0091] The three-dimensional pattern obtained in step (iii) or step (iv) may be post-cured as necessary. The post-curing may be performed by irradiating the pattern with light. The light irradiation conditions may be appropriately adjusted depending on the type of photocurable resin composition and the degree of curing of the obtained pattern. The post-curing may be performed on a part of the pattern or on the entire pattern.
[0092] [Example] The present invention will be specifically described below based on examples and comparative examples, but the present invention is not limited to the following examples.
[0093] (1) Preparation of photocurable resin composition The components shown in Table 1 were mixed in the mass ratios shown in Tables 2 and 3, and heated in an oven at 80°C for 3 hours or more while stirring to dissolve the solid components, thereby preparing a homogeneous liquid photocurable resin composition A.
[0094] (2) Evaluation The photocurable resin composition obtained in (1) above was evaluated as follows.
[0095] (a) Viscosity The viscosity of the photocurable resin composition was measured at 25° C. and a rotation speed of 20 rpm using an E-type viscometer (TVE-20H, Toki Sangyo Co., Ltd.).
[0096] (b) HDT Using a 3D printer (Sonic mini manufactured by Phrozen), the above-mentioned test pieces were produced under the conditions of an irradiation time of 5 seconds per layer and a pitch of 50 μm in the z-axis (height direction). Using this test piece, the HDT (℃) was measured under the above-mentioned conditions in accordance with ASTM D648.
[0097] (c) Tensile strength Using a 3D printer (Sonic mini manufactured by Phrozen), the above-mentioned test pieces were produced under the conditions of an irradiation time of 5 seconds per layer and a pitch of 50 μm in the z-axis (height direction). Using this test piece, the tensile strength (MPa) was measured under the above-mentioned conditions in accordance with ASTM D638.
[0098] The test pieces for HDT and tensile strength were post-cured by irradiating each side with light for 10 minutes (total of 20 minutes) using EeezCure180 manufactured by XYZ PRINTING Co., Ltd. The test pieces were then annealed in an oven at 230°C for 30 minutes.
[0099] (d) Low temperature stability Check whether the above conditions 1 to 3 are met, If all conditions 1 to 3 are met, ◎ If condition 1 and condition 2 are met, mark them with a circle. If only condition 1 is satisfied, it is marked as △. A case where all of conditions 1 to 3 were not satisfied was evaluated as ×.
[0100] The evaluation results of the Examples and Comparative Examples are shown in Tables 2 and 3. Entry Nos. 1 to 5 are Examples and 6 to 14 are Comparative Examples. When the test piece cracked during annealing and the measurement was stopped, this is indicated with an * in Tables 2 and 3. When no measurement was performed, this is indicated with a -.
[0101] [Table 1]
[0102] The ingredients in Table 1 are as follows: "ACMO": acryloylmorpholine (second compound) "SR833NS": Tricyclodecane dimethanol diacrylate (polycyclic aliphatic diacrylate) "M370": Tris 2-hydroxyethyl isocyanurate triacrylate (triacrylate compound A (first compound)) "M-313": A mixture of the following triacrylate compound A (first compound) and diacrylate compound A (second compound) Tris 2-hydroxyethyl isocyanurate triacrylate 65% by mass (first compound) Tris 2-hydroxyethyl isocyanurate diacrylate 35% by mass (second compound) "M-923": A mixture of the following triacrylate compound A (first compound), diacrylate compound A (second compound), and monoacrylate compound A (third compound) Tris 2-hydroxyethyl isocyanurate triacrylate 40% by mass Tris 2-hydroxyethyl isocyanurate diacrylate 50% by mass Tris 2-hydroxyethyl isocyanurate monoacrylate 10% by mass "AD-TMP": Ditrimethylolpropane tetraacrylate (polyacrylate with four acryloyl groups) "Omnirad TPO-H": Diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (photopolymerization initiator) "Omnirad 819": Phenylbis(2,4,6-trimethylbenzoyl)phosphine oxide (photopolymerization initiator)
[0103] [Table 2]
[0104] [Table 3]
[0105] Although the present invention has been described with respect to the presently preferred embodiments, such disclosure should not be interpreted as limiting. Various variations and modifications will no doubt become apparent to those skilled in the art to which the present invention pertains upon reading the above disclosure. Accordingly, the appended claims should be interpreted to cover all variations and modifications without departing from the true spirit and scope of the present invention. [Industrial Applicability]
[0106] The photocurable resin composition according to the present invention is suitable as a material for forming a three-dimensional stereolithographic object in stereolithography applications. [Explanation of symbols]
[0107] 1: photolithography device, 2: platform, 2a: pattern forming surface, 3: resin tank, 4: projector, 5: photocurable resin composition, 6: release agent layer, 7a: liquid film a, 7b: liquid film b, 8a: two-dimensional pattern a, 8b: two-dimensional pattern b, L: light
Claims
1. The composition includes a polymerizable compound (excluding a silicon-containing α,β-unsaturated double bond group-containing compound) and a photopolymerization initiator, the polymerizable compound includes a first compound and a second compound each containing nitrogen, the first compound is a triacrylate compound having an isocyanuric ring and three (meth)acryloyl groups; the second compound is at least one selected from the group consisting of a diacrylate compound having an isocyanuric ring and two (meth)acryloyl groups and a monoacrylamide compound having one (meth)acryloyl group; a ratio of the first compound to a total mass of the first compound and the second compound is 50 mass% or more and 90 mass% or less, a total mass ratio of the first compound and the second compound in the polymerizable compound is 20 mass% or more and 80 mass% or less, the polymerizable compound further comprises a poly(meth)acrylate having four or more (meth)acryloyl groups; A photocurable resin composition used for forming a three-dimensional photo-modeled object having a layered structure in which layered cured patterns formed by photocuring are stacked in multiple layers, wherein the proportion of the poly(meth)acrylate having four or more (meth)acryloyl groups in the mass of the polymerizable compound is 5 mass% or more and 25 mass% or less.
2. 50% by mass or more of the second compound is the diacrylate compound, 2. The photocurable resin composition according to claim 1, wherein a total ratio of the first compound and the second compound to a mass of the polymerizable compound is 30 mass% or more and 60 mass% or less.
3. 50% by mass or more of the second compound is the monoacrylamide compound, 2 . The photocurable resin composition according to claim 1 , wherein a total ratio of the first compound and the second compound to a mass of the polymerizable compound is 50 mass % or more and 80 mass % or less.
4. The photocurable resin composition according to any one of claims 1 to 3, wherein the triacrylate compound comprises tris(acryloyloxyalkyl)isocyanurate.
5. The photocurable resin composition according to any one of claims 1 to 4, wherein the monoacrylamide compound comprises a heterocyclic acrylamide having a heterocycle containing a nitrogen atom.
6. The photocurable resin composition according to any one of claims 1 to 5, wherein the polymerizable compound further comprises a polycyclic aliphatic di(meth)acrylate.
7. The photocurable resin composition according to claim 6 , wherein a proportion of the polycyclic aliphatic di(meth)acrylate in the mass of the polymerizable compound is 15 mass % or more and 70 mass % or less.
8. The photocurable resin composition according to any one of claims 1 to 7, wherein the photocurable resin composition is cooled at -30°C for 72 hours, heated to 23°C, and then allowed to stand at 23°C for 48 hours, and the entire composition is liquid.
9. The photocurable resin composition according to any one of claims 1 to 8, wherein when the photocurable resin composition is allowed to stand at 5°C for one month, the photocurable resin composition remains liquid as a whole.
10. The photocurable resin composition according to any one of claims 1 to 9, wherein a deflection temperature under load of the cured product of the photocurable resin composition is 280°C or higher, as measured by an edgewise method at a load of 0.45 MPa in accordance with ASTM D648.
11. The photocurable resin composition according to any one of claims 1 to 10, which is for a 3D printer.
12. A process for forming a stereolithography object using the photocurable resin composition according to claim 1, The step of forming a stereolithography object includes: (i) forming a liquid film of the photocurable resin composition and photocuring the liquid film to form a pattern; (ii) forming another liquid film in contact with the pattern; and (iii) photocuring the other liquid film on the pattern to laminate another pattern.
Citation Information
Patent Citations
Coating composition curable with active energy ray
JP2003213159A
Active energy ray-curable resin composition for casting, and optical component
JP2011256307A
Ultraviolet ray curable resin composition and slid member and manufacturing method of slide member
JP2016135871A
Active energy ray-polymerizable resin composition for optical three-dimensional molding, and three-dimensional molded object
JP2016160372A
Curable composition for sheet used for three-dimensional molding, laminate sheet for three-dimensional molding and manufacturing method therefor, and three-dimensional structure and manufacturing method therefor