How to adjust an electron microscope

By embedding thin plates like Ni, Cu, and Zn in electron microscopes and adjusting brightness and contrast peaks, the method addresses inconsistencies in electron microscope observations, enabling clearer and more accurate material structure analysis.

JP7572286B2Active Publication Date: 2024-10-23TDK CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2021058812
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-30
Publication Date
2024-10-23
Estimated Expiration
2041-03-30

AI Technical Summary

Technical Problem

Existing methods for observing material structures in electron microscopes often result in inconsistent brightness and contrast, leading to errors in classification and identification of material structures due to variations in electron microscope types and operators.

Method used

A method involving embedding multiple types of thin plates within the electron microscope's field of view, adjusting the brightness and contrast peaks to predetermined positions and sizes, using thin plates like Ni, Cu, and Zn, to standardize the brightness and contrast of backscattered electron images.

Benefits of technology

This approach allows for clearer observation and accurate classification of material structures by standardizing brightness and contrast, independent of electron microscope type or operator, enhancing the clarity and reliability of material structure analysis.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572286000001
    Figure 0007572286000001
  • Figure 0007572286000002
    Figure 0007572286000002
  • Figure 0007572286000003
    Figure 0007572286000003
Patent Text Reader

Abstract

To provide an adjusting method for an electron microscope capable of more clearly observing the microstructures of various materials.SOLUTION: An adjusting method for an electron microscope includes the steps of embedding two or more image preparation thin plates in a board and including them in the same field of view of the electron microscope, creating a first luminance histogram before adjustment, and adjusting the location of a luminance peak derived from each thin plate in the first luminance histogram before adjustment to a predetermined location and adjusting the difference between the luminance peak locations derived from each thin plate to a predetermined size.SELECTED DRAWING: Figure 5
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for adjusting an electron microscope. [Background technology]

[0002] Patent Document 1 describes an invention related to a method for evaluating the metal structure of a rare earth-containing alloy. Specifically, it describes a method of drawing a straight line in a specific direction in a microscopic image of a cross section of a rare earth-containing alloy, and distinguishing the main phase from the R-rich phase based on the brightness of the main phase and the brightness of the R-rich phase that intersect with the straight line. In the evaluation method of Patent Document 1, the R-rich phase interval is calculated by dividing the number of times the brightness of the main phase changes to the brightness of the R-rich phase by the length of the straight line. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2008-058323 A Summary of the Invention [Problem to be solved by the invention]

[0004] An object of the present invention is to provide a method for adjusting an electron microscope so as to enable clearer observation of the structure of various materials. [Means for solving the problem]

[0005] In order to achieve the above object, a method for adjusting an electron microscope according to the present invention comprises the steps of: embedding two or more image preparation plates in a substrate to contain them within the same field of view of an electron microscope; creating a first unadjusted luminance histogram for the field of view; The method includes a step of adjusting the positions of the luminance peaks originating from each thin plate in the first luminance histogram before the adjustment to a predetermined position, and adjusting the difference between the positions of the luminance peaks originating from each thin plate to a predetermined magnitude.

[0006] The two or more image preparation sheets may be a Ni sheet, a Cu sheet and a Zn sheet.

[0007] The two or more types of thin plates for image preparation may be two types of thin plates selected from a Ni thin plate, a Cu thin plate, and a Zn thin plate.

[0008] The two or more image preparation sheets may be a Cu sheet and a Zn sheet.

[0009] The second brightness histogram after adjustment has the minimum brightness set to 0 and the maximum brightness set to (B n -1) B n It may be created in gradations, The second brightness histogram after adjustment shows that the difference in the brightness peak positions of adjacent thin plates is all (B n ×40 / 256) or more (B n × 60 / 256).

[0010] The above-mentioned method for adjusting an electron microscope may be used for observing an RTB-based permanent magnet alloy, and R may be a rare earth element, T may be a transition metal element, and B may be boron. [Brief description of the drawings]

[0011] [Figure 1] This is a backscattered electron image of an RTB-based permanent magnet alloy taken with an electron microscope before adjustment. [Diagram 2] 2 is a luminance histogram of the RTB permanent magnet alloy in FIG. 1. [Diagram 3] This is a backscattered electron image of the standard sample taken by an electron microscope before adjustment. [Figure 4] This is the first luminance histogram before adjustment. [Diagram 5] This is a backscattered electron image of the standard sample taken by an electron microscope after adjustment. [Figure 6] The second luminance histogram after adjustment. [Figure 7] This is a backscattered electron image of the RTB permanent magnet alloy taken with an electron microscope after adjustment. [Figure 8] 8 is a luminance histogram of the RTB permanent magnet alloy of FIG. 7. [Figure 9] This is a backscattered electron image of an RTB-based permanent magnet alloy taken with an electron microscope before adjustment. [Figure 10] FIG. 10 is a luminance histogram of the RTB permanent magnet alloy of FIG. [Figure 11] This is a backscattered electron image of the standard sample taken by an electron microscope before adjustment. [Figure 12] This is the first luminance histogram before adjustment. [Figure 13] This is a backscattered electron image of the standard sample taken by an electron microscope after adjustment. [Figure 14] The second luminance histogram after adjustment. [Figure 15] This is a backscattered electron image of the RTB permanent magnet alloy taken with an electron microscope after adjustment. [Figure 16] 16 is a luminance histogram of the RTB permanent magnet alloy of FIG. 15. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0012] Hereinafter, the present invention will be described based on an embodiment.

[0013] The method for adjusting an electron microscope according to this embodiment includes the steps of: embedding two or more image preparation plates in a substrate to contain them within the same field of view of an electron microscope; creating a first unadjusted luminance histogram for the field of view; The method includes a step of adjusting the positions of the luminance peaks originating from each thin plate in the first luminance histogram before the adjustment to a predetermined position, and adjusting the difference between the positions of the luminance peaks originating from each thin plate to a predetermined magnitude.

[0014] According to the method for adjusting an electron microscope according to the present embodiment, it is possible to observe the structure of various materials more clearly. Furthermore, even if the type of electron microscope is changed, it is possible to adjust the brightness and contrast of the backscattered electron image to the same degree, so that the structure of various materials can be observed.

[0015] There is no particular limit to the types of materials observed after adjustment. Various alloys may be used. The method for adjusting an electron microscope according to this embodiment is particularly suitable for observing the structure of an alloy for an RTB permanent magnet.

[0016] There is no particular restriction on the type of thin plate used for image adjustment. However, the thin plate must be homogeneous in order to be used for image adjustment. Specifically, when creating a brightness histogram from a backscattered electron image, the position of the brightness peak originating from the thin plate must be clearly identifiable.

[0017] There are no particular limitations on how to select two or more types of thin plates for image adjustment. Generally, the greater the average atomic number of a backscattered electron image, the brighter it becomes. If a thin plate made of a single element with an atomic number close to the average atomic number of the main phase (the phase that occupies the majority of the material) in the material whose structure is actually being observed is used, the structure of the material can be observed appropriately without further changing the brightness after adjusting the electron microscope. However, the thin plate for image adjustment should not be selected based only on the atomic number, but other factors should also be considered as appropriate.

[0018] If the above material is an RTB-based permanent magnet alloy, where R is a rare earth element, T is a transition metal element, and B is boron, the main phase (R 14 The average atomic number of the GaAs (crystal phase B) is about 34. If only the atomic number is taken into consideration, it is effective to use a thin plate made of a single element selected from Ga (atomic number 31), Ge (atomic number 32), As (atomic number 33), Se (atomic number 34), Br (atomic number 35), Kr (atomic number 36) and Rb (atomic number 37) as a thin plate for image adjustment. However, among these, only Ge forms a stable solid at room temperature by itself. Furthermore, Ge is difficult to process and is expensive, making it difficult to use as a thin plate for image adjustment.

[0019] In addition, as the thin plate for image adjustment, an elemental substance of an element having an atomic number smaller than the average atomic number of the main phase is more preferably used than an elemental substance of an element having an atomic number larger than the average atomic number of the main phase.

[0020] As the conditions for the elemental substance preferably used as the thin plate for image adjustment, there may be mentioned that the elemental substance is easy to handle, the elemental substance is inexpensive, the elemental substance is a transition metal elemental substance, and the elemental substance has an atomic number close to the average atomic number of the main phase.

[0021] Among the elemental substances of elements having an atomic number smaller than the average atomic number of the main phase, there are elemental substances that relatively preferably satisfy these conditions. Therefore, an elemental substance of an element having an atomic number smaller than the average atomic number of the main phase is preferably used as the thin plate for image adjustment.

[0022] Therefore, when observing an R-T-B-based permanent magnet alloy, it is normal to select elemental substances such as Ni, Cu, Zn, etc. as two or more types of thin plates for image adjustment, considering the atomic number, workability, price, etc. Also, the types of elements selected as two or more types of thin plates for image adjustment may be selected so that the difference in atomic numbers between adjacent elements is 1 when the selected elements are arranged in ascending order of atomic number.

[0023] Hereinafter, the adjustment method of an electron microscope for observing an R-T-B-based permanent magnet alloy will be described by taking the case where two or more types of thin plates for image adjustment are Ni thin plate, Cu thin plate, and Zn thin plate, and the case where they are Cu thin plate and Zn thin plate as examples. However, the adjustment method of the electron microscope is not limited to the case where two or more types of thin plates for image adjustment are Ni thin plate, Cu thin plate, and Zn thin plate, and the case where they are Cu thin plate and Zn thin plate. Regarding the types of two or more types of thin plates for image adjustment, for example, two or more types of thin plates for image adjustment may be two types of thin plates selected from Ni thin plate, Cu thin plate, and Zn thin plate.

[0024] <When using Ni thin plate, Cu thin plate and Zn thin plate>

[0025] A Ni thin plate, a Cu thin plate, and a Zn thin plate are prepared as thin plates for image adjustment. At least the Ni thin plate, the Cu thin plate, and the Zn thin plate are embedded in a substrate to prepare a standard sample. The substrate may be an embedding resin for electron microscope observation. There is no particular limit to the thickness of each thin plate. For example, it may be 0.05 to 0.20 mm.

[0026] Next, the cross section of the standard sample is mirror-polished and gold is evaporated. By mirror-polishing the cross section and evaporation of gold, the brightness and contrast can be suitably adjusted.

[0027] Next, the standard sample is set in the electron microscope. The imaging mode is backscattered electron imaging. There is no particular limit to the number of pixels, which varies depending on the material being observed. For example, 1280 x 960 pixels. There is no particular limit to the magnification, but the magnification should be such that the Ni thin plate, Cu thin plate, and Zn thin plate are in the same field of view. For example, it may be 100 to 500 times.

[0028] Next, the field of view is shifted so that the Ni thin plate, the Cu thin plate, and the Zn thin plate are in the same field of view. There is no particular restriction on the order of the thin plates.

[0029] Next, set the minimum brightness to 0 and the maximum brightness to B. n Set B to -1 n Create the first luminance histogram before gradation adjustment. B n The value may be between 16 and 65536. In addition, since the brightness histogram is created by a computer program, B n is often a power of 2.

[0030] Then, the positions of the luminance peaks originating from each thin plate are adjusted to a predetermined position, and the difference between the luminance peak positions originating from each thin plate is adjusted to a predetermined size. The above-mentioned predetermined positions and predetermined sizes in the adjusted second luminance histogram vary depending on the material to be actually observed after the electron microscope adjustment. n ×35 / 256) or more (B n × 65 / 256).

[0031] In this case, the position of the brightness peak due to the Cu thin plate is (B n ×150 / 256) ((B n ×145 / 256)~(B n The brightness may be adjusted so that the difference between the positions of the brightness peaks derived from the Ni thin plate and the Cu thin plate is (B n ×55 / 256) degree ((B n ×45 / 256)~(B n × 65 / 256), the difference between the position of the brightness peak derived from the Cu thin plate and the position of the brightness peak derived from the Zn thin plate is (B n ×45 / 256) ((B n ×35 / 256)~(B n By adjusting the contrast, it is possible to adjust the difference in the positions of the brightness peaks. The higher the contrast, the larger the difference in the positions of the brightness peaks. Furthermore, the standard deviation of the brightness peaks becomes larger. The difference between the positions of the brightness peaks derived from the Ni thin plate and the Cu thin plate is defined as (B n × 55 / 256), the difference between the position of the brightness peak derived from the Cu thin plate and the position of the brightness peak derived from the Zn thin plate will automatically be (B n When adjusting the contrast, the position of the brightness peak due to the Cu thin plate is adjusted to about (B n The brightness is adjusted as necessary to maintain the brightness at approximately the same level (approximately 150 / 256 × 150). As a result, the second luminance histogram after adjustment is obtained.

[0032] Once the brightness and contrast adjustments have been completed, the material may be observed immediately. However, depending on the type of material, further brightness adjustments may be performed. When observing an alloy for an RTB permanent magnet, for example, a brightness histogram is created by placing the alloy for an RTB permanent magnet in the field of view while maintaining the contrast, increasing the magnification so that only the main phase, which will be described later, is in the field of view, and the position of the peak is (B n ×110 / 256) ((Bn ×105 / 256) to (B n The brightness may be adjusted so as to be (×115 / 256). There is no limit to the magnification when increasing the magnification, but it may be 10,000 times or less.

[0033] Furthermore, in order to easily perform this brightness adjustment, the alloy plate for R-T-B permanent magnet may be embedded in a standard sample together with Ni thin plate, Cu thin plate and Zn thin plate. In this case, the alloy for R-T-B permanent magnet can be put into the visual field by changing the observation range of the standard sample. Furthermore, heat treatment may be performed on the alloy plate for R-T-B permanent magnet before embedding it in the standard sample. By performing heat treatment, the process of making only the main phase enter the visual field of the electron microscope in order to adjust the brightness becomes easy. There are no particular restrictions on the heat treatment time and temperature when performing heat treatment. For example, heat treatment is performed at 800 to 1000 °C for 30 to 120 minutes.

[0034] When embedding the alloy plate for R-T-B permanent magnet in a standard sample together with Ni thin plate, Cu thin plate and Zn thin plate, the alloy plate for R-T-B permanent magnet may be arranged on both sides of the portion including Ni thin plate, Cu thin plate and Zn thin plate. By arranging the alloy plates for R-T-B permanent magnets on both sides, the stability of mirror polishing is improved.

[0035] <When using Cu thin plate and Zn thin plate>

[0036] Prepare Cu thin plate and Zn thin plate as thin plates for image adjustment. Then, at least the Cu thin plate and the Zn thin plate are embedded in a base material to prepare a standard sample. The base material may be an embedding resin for electron microscope observation. There are no particular restrictions on the thickness of each thin plate. For example, it may be 0.05 to 0.20 mm.

[0037] Next, the cross-section of the standard sample is mirror-polished and gold evaporation is performed. By mirror-polishing the cross-section and performing gold evaporation, the brightness and contrast can be suitably adjusted.

[0038] Next, the standard sample is set in the electron microscope. The imaging mode is backscattered electron imaging. There is no particular limit to the number of pixels, which varies depending on the material being observed. For example, 1280 x 960 pixels. There is no particular limit to the magnification, but the magnification should be such that the Cu thin plate and the Zn thin plate are in the same field of view. For example, it may be 100 to 500 times.

[0039] Next, the field of view is shifted so that the Cu thin plate and the Zn thin plate are in the same field of view.

[0040] Next, set the minimum brightness to 0 and the maximum brightness to B. n Set B to -1 n Create the first luminance histogram before gradation adjustment. B n The value may be between 16 and 65536. In addition, since the brightness histogram is created by a computer program, B n is often a power of 2.

[0041] Then, the positions of the luminance peaks originating from each thin plate are adjusted to a predetermined position, and the difference between the luminance peak positions originating from each thin plate is adjusted to a predetermined size. The above-mentioned predetermined positions and predetermined sizes in the adjusted second luminance histogram vary depending on the material to be actually observed after the electron microscope adjustment. n ×35 / 256) or more (B n × 65 / 256).

[0042] In this case, the position of the brightness peak due to the Cu thin plate is (B n ×110 / 256) ((B n ×105 / 256~B n By adjusting the brightness, the position of each brightness peak can be adjusted. Furthermore, the difference between the position of the brightness peak derived from the Cu thin plate and the position of the brightness peak derived from the Zn thin plate is adjusted so that (B n ×55 / 256) degree ((B n ×45 / 256~B nBy adjusting the contrast, it is possible to adjust the difference in the positions of the brightness peaks. The higher the contrast, the larger the difference in the positions of the brightness peaks. Furthermore, the standard deviation of the brightness peaks becomes larger. When adjusting the contrast, it is possible to adjust the position of the brightness peak derived from the Cu thin plate to (B n The brightness is adjusted as necessary to maintain the brightness at approximately the same level (approximately 110 × 110 / 256). As a result, the second adjusted luminance histogram is obtained.

[0043] Once the brightness and contrast adjustments have been completed, the material may be observed immediately. However, depending on the type of material, further brightness adjustments may be performed. When observing an alloy for an RTB permanent magnet, for example, a brightness histogram is created by placing the alloy for an RTB permanent magnet in the field of view while maintaining the contrast, increasing the magnification so that only the main phase, which will be described later, is in the field of view, and the position of the peak is (B n ×110 / 256) degree (B n ×105 / 256~B n The brightness may be adjusted so that the magnification is 10,000 times or less. There is no limit to the magnification when increasing the magnification, but it may be set to 10,000 times or less.

[0044] Furthermore, in order to easily adjust the brightness, the RTB permanent magnet alloy plate may be embedded in a standard sample together with a Cu thin plate and a Zn thin plate. In this case, the RTB permanent magnet alloy can be brought into view by changing the observation range of the standard sample. Furthermore, the RTB permanent magnet alloy plate may be heat-treated before being embedded in the standard sample. By carrying out the heat treatment, the process of bringing only the main phase into the field of view of the electron microscope in order to adjust the brightness can be facilitated. There is no particular limit to the heat treatment time and temperature when carrying out the heat treatment. For example, the heat treatment is carried out at 800 to 1000°C for 30 to 120 minutes.

[0045] When embedding an alloy plate for an R-T-B series permanent magnet together with Cu thin plates and Zn thin plates in a standard sample, the alloy plates for the R-T-B series permanent magnet may be arranged on both sides of the portion including the Cu thin plates and the Zn thin plates. By arranging the alloy plates for the R-T-B series permanent magnet on both sides, the stability of mirror polishing is improved.

[0046] <Microstructure of the alloy for the R-T-B series permanent magnet> The method for adjusting the electron microscope according to the present embodiment is particularly preferably used when obtaining a backscattered electron image of the alloy for the R-T-B series permanent magnet. Hereinafter, the microstructure of the alloy for the R-T-B series permanent magnet will be described. The alloy for the R-T-B series permanent magnet contains R, T, and B, where R is a rare earth element, T is a transition metal element, and B is boron.

[0047] Generally, the alloy for the R-T-B series permanent magnet contains a columnar crystal main phase having an R2T 14 B-type crystal structure and an R-rich phase having a higher R content than the main phase.

[0048] In the cross-section of the alloy for the R-T-B series permanent magnet, a clear difference can be confirmed between the main phase (phase with low brightness) and the R-rich phase (phase with high brightness), and a structure (hereinafter referred to as the normal structure) in which most of the shapes of the R-rich phases are linear occupies most of the area. Most of the main phases included in the normal structure are columnar crystals. In the normal structure, the average interval between the R-rich phases having a linear shape (hereinafter referred to as linear R-rich phases) is 2 μm or more. Further, the normal structure is a structure in which primary dendrites extend in the direction of solidification of the alloy, in other words, in the thickness direction of the alloy.

[0049] In addition to the normal structure, the alloy for the R-T-B series permanent magnet includes a structure containing a main phase that is not a columnar crystal. The main phase that is not a columnar crystal is called a non-columnar crystal, and the structure containing the non-columnar crystal is called a non-columnar crystal structure. Further, the non-columnar crystal structure is not necessarily a structure in which primary dendrites extend in the direction of solidification of the alloy. Furthermore, the non-columnar crystal structure can be classified into multiple types of non-columnar crystal structures.

[0050] Here, the observation of RTB permanent magnet alloys, particularly the classification of normal structures and non-columnar structures, can be performed by visually inspecting the backscattered electron images. However, unless the brightness and contrast of the backscattered electron images themselves are adjusted to the same degree for everyone, differences in brightness and contrast of the backscattered electron images themselves will cause errors in the classification results.

[0051] Furthermore, it has been considered to identify the structure of an alloy for an RTB permanent magnet from the brightness information of a backscattered electron image. In particular, it has been considered to classify the structure from the peak position and standard deviation of the brightness histogram when the alloy for an RTB permanent magnet is divided into many sections and a brightness histogram is created from the brightness information of each section. However, if the brightness and contrast of the backscattered electron image itself are not adjusted to the same extent regardless of the type of electron microscope and the operator, an error will occur in the classification result due to the difference in brightness and contrast of the backscattered electron image itself. If the brightness and contrast, especially the contrast, are not adjusted to the same extent regardless of the type of electron microscope and the operator, it becomes difficult to distinguish between a normal structure and a non-columnar structure from the peak position and standard deviation of the brightness histogram.

[0052] It is difficult to adjust the brightness and contrast to the same level regardless of the type of electron microscope or the observer by using only RTB-based permanent magnet alloys. In particular, it is difficult to adjust the contrast to the same level regardless of the type of electron microscope or the observer.

[0053] By using the electron microscope adjustment method according to the present embodiment, the brightness and contrast of the backscattered electron image itself can be adjusted suitably and to the same degree, regardless of the type of electron microscope and the operator. As a result, the structure of the material can be clearly observed from the backscattered electron image, regardless of the type of electron microscope and the operator. Furthermore, the structure of the material can be clearly identified from the brightness information of the backscattered electron image, regardless of the type of electron microscope and the operator. EXAMPLES

[0054] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.

[0055] (Example 1: When Ni thin plate, Cu thin plate and Zn thin plate are used) First, an alloy for RTB permanent magnets was prepared by strip casting as the material to be observed, with the composition being 25.3 mass% Nd, 6.2 mass% Pr, 0.90 mass% B, 0.3 mass% Al, 0.9 mass% Co, 0.2 mass% Cu, 0.5 mass% Zr, 0.6 mass% Ga, and the balance Fe.

[0056] Figure 1 is an example of a backscattered electron image of an RTB permanent magnet alloy taken by an electron microscope before adjustment. Figure 2 is a brightness histogram of the RTB permanent magnet alloy in Figure 1. Backscattered electron images obtained using an electron microscope before adjustment vary greatly depending on the type of electron microscope and the type of material measured immediately before. However, as shown in Figure 2, the peak position of the brightness histogram is often on the lower brightness side than the desired position, and the standard deviation of the brightness histogram is often smaller than the desired size. The magnification was 350 times and the number of pixels was 1280 x 960 pixels.

[0057] In order to observe the cross section of the obtained RTB permanent magnet alloy with an electron microscope (manufactured by JEOL Ltd.), the brightness and contrast of the electron microscope were adjusted by the following method.

[0058] First, the obtained RTB permanent magnet alloy was heat-treated at 1000°C for 120 minutes to obtain two heat-treated plates for incorporation into standard samples.

[0059] Next, a 0.1 mm thick Ni thin plate, a 0.1 mm thick Cu thin plate, and a 0.1 mm thick Zn thin plate were prepared. Next, the heat-treated plate, Ni thin plate, Cu thin plate, and Zn thin plate were embedded in an embedding resin for electron microscope observation. At this time, the heat-treated plate, Ni thin plate, Cu thin plate, Zn thin plate, and heat-treated plate were arranged in this order so that the cross sections of each plate were parallel to the thickness direction, to prepare a standard sample.

[0060] Next, the cross section of the standard sample was mirror-polished and gold was evaporated onto it.

[0061] Next, the standard sample was set in an electron microscope. The imaging mode was set to a backscattered electron image, with a magnification of 150 and a pixel count of 1280 × 960 pixels.

[0062] Next, the field of view was adjusted so that the Ni thin plate, the Cu thin plate, and the Zn thin plate were in that order within the same field of view.

[0063] Next, 256 gradations (B n = 256) to create a first luminance histogram before adjustment, and then the brightness was adjusted so that the position of the luminance peak derived from the Cu thin plate was about 150 (145 to 155). Furthermore, the contrast was adjusted so that the difference between the position of the luminance peak derived from the Ni thin plate and the position of the luminance peak derived from the Cu thin plate was about 55 (45 to 65), and the difference between the position of the luminance peak derived from the Cu thin plate and the position of the luminance peak derived from the Zn thin plate was about 45 (35 to 55). When adjusting the contrast, the brightness was additionally adjusted as necessary to maintain the position of the luminance peak derived from the Cu thin plate at about 150. The luminance histogram obtained by the adjustment is the second luminance histogram after adjustment.

[0064] Figure 3 shows a backscattered electron image of the standard sample taken by an electron microscope before adjustment. From the left, a Ni thin plate, a Cu thin plate, and a Zn thin plate are lined up in the same field of view in that order. Figure 4 shows the first brightness histogram before adjustment.

[0065] Figure 5 is a backscattered electron image of the standard sample taken by an electron microscope after adjustment. From the left, a Ni thin plate, a Cu thin plate, and a Zn thin plate are lined up in the same field of view, in that order. Figure 6 is the second brightness histogram after adjustment. By adjusting the brightness and contrast of the backscattered electron image shown in Figure 3 using the method described above, the position of the brightness peak moves to the low brightness side, and the difference in the positions of the brightness peaks originating from adjacent thin plates becomes larger. In Figure 6, the position of the brightness peak originating from the Ni thin plate is approximately 91, the position of the brightness peak originating from the Cu thin plate is approximately 147, and the position of the brightness peak originating from the Zn thin plate is approximately 193.

[0066] Comparing Figures 4 and 6, the positions of the brightness peaks originating from each thin plate in Figure 6 have shifted to the lower brightness side compared to Figure 4, and the difference in the positions of the brightness peaks has become larger. However, the heights of the brightness peaks originating from each thin plate hardly change. In other words, even if the brightness and contrast of the electron microscope are adjusted, the heights of the brightness peaks hardly change at all.

[0067] Next, while maintaining the contrast, the field of view was moved to the position where the heat-treated sample was placed. Then, the magnification was increased so that the white phase (R-rich phase) was not included in the field of view and only the main phase was included. The maximum magnification was about 10,000 times. Furthermore, the brightness was adjusted so that the peak position of the brightness histogram was about 110 (105 to 115). Finally, the standard sample was removed from the electron microscope.

[0068] The backscattered electron image obtained by observing the RTB permanent magnet alloy using the electron microscope after adjustment at the same magnification and the same number of pixels as before adjustment is shown in Figure 7. Figure 8 is a brightness histogram of the RTB permanent magnet alloy in Figure 7.

[0069] Figure 7 has stronger contrast than Figure 1. Also, Figure 8 has a larger standard deviation of the brightness histogram than Figure 2. From the above, the alloy structure of the RTB permanent magnet alloy can be observed more clearly in Figure 7. In other words, the main phase and the R-rich phase can be more clearly distinguished.

[0070] (Example 2: When using Cu thin plate and Zn thin plate) First, an alloy for RTB permanent magnets was prepared by strip casting as the material to be observed, with the composition being 24.1% by mass of Nd, 6.4% by mass of Pr, 0.4% by mass of Tb, 0.84% ​​by mass of B, 0.2% by mass of Al, 0.9% by mass of Co, 0.2% by mass of Cu, 0.5% by mass of Zr, 0.6% by mass of Ga, and the balance being Fe.

[0071] Figure 9 is an example of a backscattered electron image of an RTB permanent magnet alloy taken by an electron microscope before adjustment. Figure 10 is a brightness histogram of the RTB permanent magnet alloy in Figure 9. Backscattered electron images obtained using an electron microscope before adjustment vary greatly depending on the type of electron microscope and the type of material measured immediately before. However, the peak position of the brightness histogram shown in Figure 10 is often on the lower brightness side than the desired position, and the standard deviation of the brightness histogram shown in Figure 10 is often smaller than the desired size. The magnification was 350 times and the number of pixels was 1280 x 960 pixels.

[0072] In order to observe the cross section of the obtained RTB permanent magnet alloy with an electron microscope (manufactured by JEOL Ltd.), the brightness and contrast of the electron microscope were adjusted by the following method.

[0073] First, the obtained RTB permanent magnet alloy was heat-treated at 1000°C for 120 minutes to obtain two heat-treated plates for incorporation into standard samples.

[0074] Next, a 0.1 mm thick Cu thin plate and a 0.1 mm thick Zn thin plate were prepared. The heat-treated plate, Cu thin plate, and Zn thin plate were then embedded in an embedding resin for electron microscope observation. At this time, the heat-treated plate, Cu thin plate, Zn thin plate, and heat-treated product were arranged in this order so that the cross sections of each plate were parallel to the thickness direction, to prepare a standard sample.

[0075] Next, the cross section of the standard sample was mirror-polished and gold was evaporated onto it.

[0076] Next, the standard sample was set in an electron microscope. The imaging mode was set to a backscattered electron image, with a magnification of 350 and a pixel count of 1280 × 960 pixels.

[0077] Next, the field of view was adjusted so that the Cu thin plate and the Zn thin plate were in that order within the same field of view.

[0078] Next, 256 gradations (B n = 256) to create a first luminance histogram before adjustment, and then the brightness was adjusted so that the position of the luminance peak derived from the Cu thin plate was approximately 110 (105 to 115). Furthermore, the contrast was adjusted so that the difference between the position of the luminance peak derived from the Cu thin plate and the position of the luminance peak derived from the Zn thin plate was approximately 55 (45 to 65). When adjusting the contrast, the brightness was additionally adjusted as necessary to maintain the position of the luminance peak derived from the Cu thin plate at approximately 110. The luminance histogram obtained by the adjustment is the second luminance histogram after adjustment.

[0079] Figure 13 is a backscattered electron image of the standard sample taken by an electron microscope after adjustment. From the left, a Cu thin plate and a Zn thin plate are lined up in that order in the same field of view. Figure 14 is the second brightness histogram after adjustment. By adjusting the brightness and contrast of the backscattered electron image shown in Figure 11 using the method described above, the position of the brightness peak moves to the low brightness side and the difference in the positions of the brightness peaks originating from adjacent thin plates becomes larger. In Figure 14, the position of the brightness peak originating from the Cu thin plate is approximately 109, and the position of the brightness peak originating from the Zn thin plate is approximately 162.

[0080] Comparing Figures 12 and 14, the brightness peaks originating from the Zn thin plates in Figure 14 have shifted to the higher brightness side compared to Figure 12, and the difference in the positions of the brightness peaks has become larger. However, the heights of the brightness peaks originating from each thin plate remain almost unchanged. In other words, even if the brightness and contrast of the electron microscope are adjusted, the heights of the brightness peaks remain almost unchanged.

[0081] Next, while maintaining the contrast, the field of view was moved to the position where the heat-treated sample was placed. Then, the magnification was increased so that the white phase (R-rich phase) was not included in the field of view and only the main phase was included. The maximum magnification was about 10,000 times. Furthermore, the brightness was adjusted so that the peak position of the brightness histogram was about 110 (105 to 115). Finally, the standard sample was removed from the electron microscope.

[0082] The backscattered electron image obtained by observing the RTB permanent magnet alloy using the electron microscope after adjustment at the same magnification and the same number of pixels as before adjustment is shown in Figure 15. Figure 16 is a brightness histogram of the RTB permanent magnet alloy in Figure 15.

[0083] Figure 15 has stronger contrast than Figure 9. Also, Figure 16 has a larger standard deviation of the brightness histogram than Figure 10. From the above, the alloy structure of the RTB permanent magnet alloy can be observed more clearly in Figure 15. In other words, the main phase and the R-rich phase can be more clearly distinguished.

Claims

1. embedding two or more image preparation plates in a substrate to contain them within the same field of view of an electron microscope; creating a first unadjusted luminance histogram for the field of view; a step of adjusting the positions of the luminance peaks originating from each thin plate in the first luminance histogram before the adjustment to a predetermined position, and adjusting a difference in the positions of the luminance peaks originating from each thin plate to a predetermined magnitude.

2. 2. The method for observing an RTB system alloy for a permanent magnet according to claim 1, wherein the two or more types of thin plates for image preparation are a Ni thin plate, a Cu thin plate and a Zn thin plate.

3. 2. The method for observing an RTB system alloy for a permanent magnet according to claim 1, wherein the two or more types of thin plates for image preparation are two types of thin plates selected from a Ni thin plate, a Cu thin plate and a Zn thin plate.

4. 2. The method for observing an RTB system alloy for a permanent magnet according to claim 1, wherein the two or more types of thin plates for image preparation are a Cu thin plate and a Zn thin plate.

5. The second luminance histogram after adjustment has the minimum luminance at 0 and the maximum luminance at (B n -1) B n Created in gradations, The second luminance histogram after the adjustment shows that the difference between the luminance peak positions of adjacent thin plates is all (B n ×40 / 256) or more (B n 5. The method for observing an RTB system alloy for permanent magnets according to claim 2, wherein the refractive index is 0.01×60 / 256) or less.

Citation Information

Patent Citations

  • Automatic brightness / contrast adjusting system of electron microscope

    JP1992328234A

  • Electron microscope

    JP1999233058A

  • Method of evaluating metal structure of r-t-b magnet alloy

    JP2008058323A

  • Rare earth-transition metal-boron-based rare earth sintered magnet, and manufacturing method thereof

    JP2014132628A

  • Thin r-t-b alloy, r-t-b based sintered magnet, and production method for same

    WO2013054845A1