Catalyst containing materials

The ceramic matrix catalyst composite addresses the issue of catalyst pooling and migration in thrusters by embedding catalytic particles within a refractory matrix, ensuring sustained catalytic activity through self-replacement of exposed particles.

JP7572432B2Active Publication Date: 2024-10-23AEROJET ROCKETDYNE INC
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022530162
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2019-11-25
Publication Date
2024-10-23
Estimated Expiration
2039-11-25

AI Technical Summary

Technical Problem

Supported catalysts in high-temperature applications, such as thrusters, suffer from catalyst pooling and migration, leading to reduced durability and effectiveness over time.

Method used

A ceramic matrix catalyst composite is developed, where catalytic metal elements or oxides are dispersed and embedded within a refractory matrix, preventing migration and enabling self-replacement of exposed particles to maintain catalytic activity.

Benefits of technology

The ceramic matrix catalyst composite enhances durability and maintains catalytic effectiveness by preventing pooling and migration, ensuring consistent performance over time.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572432000001
    Figure 0007572432000001
  • Figure 0007572432000002
    Figure 0007572432000002
  • Figure 0007572432000003
    Figure 0007572432000003
Patent Text Reader

Abstract

The catalyst-containing material comprises a refractory matrix and particles of one or more catalytic metal elements or catalytic oxides that are dispersed and embedded throughout the refractory matrix.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to catalyst structures and compositions that are useful in a variety of applications, such as in thrusters. [Background technology]

[0002] Catalysts are known and used in a variety of structures and compositions to facilitate many different chemical reactions. For example, platinum group metals are often used as catalysts in supported catalyst structures. Example structures include catalyst powders attached to the outer surface of a core support particle, and catalysts impregnated into a porous high surface area support. Summary of the Invention [Means for solving the problem]

[0003] A catalyst-containing material according to one example of the present disclosure includes a refractory matrix and particles of one or more catalytic metal elements or catalytic oxides that are dispersed and embedded throughout the refractory matrix.

[0004] In further embodiments of any of the preceding embodiments, the particles include one or more catalytic metal elements selected from Ir, Pt, Pd, Rh, Os, Ru, Re, and combinations thereof.

[0005] In a further embodiment of any of the preceding embodiments, the one or more catalytic metal elements is Ir.

[0006] In a further embodiment of any of the preceding embodiments, the particles are comprised in a catalytic oxide and are selected from V2O5, MnO2, and combinations thereof.

[0007] In a further embodiment of any of the preceding embodiments, the refractory matrix is ​​an oxide selected from CeO2, HfO2, ZrO2, Y2O3, Ln2O3, and combinations thereof, where Ln is a lanthanide element.

[0008] In a further embodiment of any of the preceding embodiments, the refractory matrix is ​​an oxide selected from CeO2, HfO2, and combinations thereof.

[0009] In a further embodiment of any of the preceding embodiments, the refractory matrix is ​​selected from refractory metals and ceramic refractories.

[0010] Further embodiments of any of the preceding embodiments include between 5% and 50% by weight of particles of one or more catalytic metal elements or catalytic oxides and between 95% and 50% by weight of a ceramic oxide matrix.

[0011] Further embodiments of any of the preceding embodiments include 30% to 40% by weight of particles of one or more catalytic metal elements or catalytic oxides and 70% to 60% by weight of a refractory matrix.

[0012] In a further embodiment of any of the preceding embodiments, the refractory matrix is ​​a binary composition of two different oxides selected from CeO2, HfO2, ZrO2, Y2O3, Ln2O3, where Ln is a lanthanide element.

[0013] In a further embodiment of any of the preceding embodiments, the refractory matrix is ​​a binary composition of CeO2 and HfO2.

[0014] In further embodiments of any of the preceding embodiments, the particles include one or more catalytic metal elements selected from Ir, Pt, Pd, Rh, Os, Ru, Re, and combinations thereof, and the refractory matrix is ​​an oxide selected from CeO2, HfO2, ZrO2, YO3, La2O3, and combinations thereof, and the particles include 5% to 50% by weight of the one or more catalytic metal elements or catalytic oxide particles and 95% to 50% by weight of the refractory matrix.

[0015] In a further embodiment of any of the preceding embodiments, the particles include one or more catalytic metal elements and are Ir, and the refractory matrix is ​​an oxide selected from CeO2, HfO2, and combinations thereof, comprising 30% to 40% by weight of the particles of one or more catalytic metal elements or catalytic oxides and 70% to 60% by weight of the refractory matrix.

[0016] In a further embodiment of any of the preceding embodiments, the material comprises particles including one or more catalytic metal elements that are Ir, and a refractory matrix that is an oxide selected from CeO2, HfO2, and combinations thereof, comprising 30% to 40% by weight of the particles of the one or more catalytic metal elements and 70% to 60% by weight of the refractory matrix.

[0017] In a further embodiment of any of the preceding embodiments, a thruster includes a combustion chamber, an injector for supplying propellant to the combustion chamber, and the catalyst-containing material of any of the preceding embodiments disposed in the combustion chamber to catalyze a reaction of the propellant.

[0018] A method of making a catalyst-containing material according to one example of the present disclosure includes providing a mixture of matrix particles and particles of one or more catalytic metal elements or catalytic oxides, combining the mixture with at least a binder to produce one or more green state bodies, and heat treating the one or more green state bodies, which causes sintering of the matrix particles to produce a refractory matrix having dispersed and embedded therein the particles of one or more catalytic metal elements or catalytic oxides.

[0019] A further embodiment of any of the preceding embodiments includes granulating one or more of the green bodies.

[0020] In further embodiments of any of the preceding embodiments, the particles include one or more catalytic metal elements selected from Ir, Pt, Pd, Rh, Os, Ru, Re, and combinations thereof.

[0021] In further embodiments of any of the preceding embodiments, the particles are ceramic oxide particles selected from CeO2, HfO2, ZrO2, Y2O3, Ln2O3, and combinations thereof, where Ln is a lanthanide element.

[0022] A thruster according to one example of the present disclosure includes a combustion chamber, an injector for supplying propellant to the combustion chamber, an outlet for discharging decomposition products from the combustion chamber, and a catalyst-containing material within the combustion chamber for catalyzing a reaction of the propellant. The ceramic matrix catalyst composite includes a refractory matrix and particles of one or more catalytic metal elements or catalytic oxides dispersed and embedded throughout the refractory matrix.

[0023] In further embodiments of any of the preceding embodiments, the particles include one or more catalytic metal elements selected from Ir, Pt, Pd, Rh, Os, Ru, Re, and combinations thereof, and the refractory matrix is ​​an oxide selected from CeO2, HfO2, ZrO2, YO3, Ln2O3, and combinations thereof, where Ln is a lanthanide element, and the particles include 5% to 50% by weight of the one or more catalytic metal elements or ceramic oxide particles and 95% to 50% by weight of the refractory matrix.

[0024] In a further embodiment of any of the preceding embodiments, the particles include one or more catalytic metal elements and are Ir, and the refractory matrix is ​​an oxide selected from CeO2, HfO2, and combinations thereof, comprising 30% to 40% by weight of the particles of one or more catalytic metal elements or catalytic oxides and 70% to 60% by weight of the refractory matrix.

[0025] The various features and advantages of the present disclosure will become apparent to those skilled in the art from the following detailed description. The drawings that accompany the detailed description are briefly described as follows. [Brief description of the drawings]

[0026] [Figure 1] FIG. 2 is a cross-sectional view of a catalyst-containing material. [Diagram 2] 1 is a cross-sectional view of a catalyst-containing material after a period of use. [Diagram 3] FIG. 1 illustrates a method for producing a catalyst-containing material. [Figure 4] FIG. 1 illustrates an example thruster having a catalyst-containing material. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0027] In some high temperature applications, such as thrusters, and even in some low temperature applications, catalysts in supported catalysts may pool or migrate into agglomerates that reduce catalytic effectiveness. Thus, these supported catalysts exhibit relatively poor durability in terms of maintaining catalytic effectiveness. The prevailing thinking regarding catalyst structure may, at least in part, hinder the solution of this problem. For example, in typical supported catalyst structures, the paradigm is that all catalysts are exposed to maximize contact with one or more reactants. Thus, over the same period of time, all catalysts may be subject to continuous pooling or migration. In this regard, disclosed herein are ceramic matrix catalyst composites for promoting improved durability.

[0028] FIG. 1 illustrates a cross-sectional view of an example catalyst-containing material 20 (hereinafter, "material 20"). As shown, material 20 is in the form of granules. Such granules may be provided, for example, to a catalyst bed for contact with one or more reactants. However, it should be understood that material 20 is not limited to granules, and material 20 may be provided in other forms dictated by the end use, such as, but not limited to, a cylinder, a rod, or other engineered shape.

[0029] Material 20 includes refractory matrix 22 and particles 24 (only some of which are numbered in the figure). Particles 24 are comprised of one or more catalytic metal elements or oxides (generally designated 24a), and particles 24 are dispersed and embedded throughout refractory matrix 22. For example, particles 24 are comprised solely of catalytic metal elements or oxides 24a. The term "dispersed" refers to particles 24 that are relatively uniformly spatially distributed throughout the extent of refractory matrix 22. The term "embedded" refers to particles 24 that are firmly embedded in refractory matrix 22, such as by being substantially or completely surrounded by and in intimate contact with refractory matrix 22. Such embedding causes metal particles 24 to be "anchored" in refractory matrix 22, as opposed to supported catalysts, where the catalyst is simply deposited into existing pores of the support.

[0030] The refractory matrix 22 is composed of one or more refractories. As used herein, "refractory" or "refractories" refers to one or more high temperature materials selected from among two material classifications including those known as refractory materials and refractory metals. Refractory materials are understood to be non-metallic materials with chemical and physical properties suitable for use in environments above 1,000°F (538°C), such as many ceramics. Refractory metals are understood to be niobium, molybdenum, tantalum, tungsten, rhenium, titanium, vanadium, chromium, zirconium, hafnium, ruthenium, rhodium, osmium, and iridium.

[0031] In one example, the refractory matrix 22 is monolithic and therefore composed of only one of the refractories listed above, such as a single metal element or a single refractory compound. In another example, the refractory matrix 22 is composite and therefore composed of two or more of the refractories listed above. In a further example, the refractory matrix 22 also has one or more refractories provided as reinforcement and distributed throughout the refractory matrix 22 (but different from the catalytic metal element 24a dispersed in the refractory matrix 22). In one example, the reinforcement refractory includes a fiber or fiber network formed from a refractory or refractories that is chemically different from the refractory or refractories of the refractory matrix 22. For example, in one non-limiting example, the refractory reinforcement is zirconium fiber and the refractory matrix 22 is selected from the refractories listed above, but does not include zirconium.

[0032] Ceramic refractories include, but are not limited to, refractory borides, nitrides, carbides, and oxides. "Ceramic" generally refers to an inorganic non-metallic solid compound having one or more metal or semi-metal elements combined with boron, nitrogen, carbon, oxygen, or combinations thereof, and may be crystalline, partially crystalline, or amorphous. Examples include, but are not limited to, TiB2, NbB2, Si3N4, and SiC. Examples of ceramic oxides are selected from CeO2, HfO2, ZrO2, Y2O3, and Ln2O3, where Ln is a lanthanide element selected from La, Nd, Eu, Tb, Er, and Yb.

[0033] The one or more catalytic metal elements 24a of the exemplary particles 24 are selected from Ir, Pt, Pd, Rh, Os, Ru, Re, and combinations thereof. In one particular example, the refractory matrix 22 is selected from CeO2, HfO2, or combinations thereof, and the catalytic metal is Ir. In further examples, the refractory matrix 22 may also include other ceramic oxides, and the catalytic metal may also include other metals. However, in further examples, the refractory matrix 22 consists only of CeO2, HfO2, or combinations thereof, and the catalytic metal consists only of Ir, such that the material 20 is composed only of Ir and CeO2, HfO2, or combinations thereof. In further examples, the metallic elements of the above examples are substituted for catalytic oxides such as V2O5 or MnO2.

[0034] The relative amounts of refractory matrix 22 and particles 24 can be varied for catalytic effect. Most typically, the amounts are 5% to 50% particles 24 and 95% to 50% refractory matrix 22 by weight, based on the combined weight of matrix 22 and particles 24. In a further example, the amounts are 30% to 40% particles 24 and 70% to 60% refractory matrix 22 by weight. In the above example amounts, it is assumed that material 20 is comprised only of ceramic oxide matrix 22 and particles 24. If material 20 has other components, the same amounts as above can be used, based on the combined weight of matrix 22 and particles 24 only (i.e., excluding the weight of the other components).

[0035] The structure of material 20 having particles 24 dispersed and embedded throughout refractory matrix 22 facilitates mitigation of pooling or migration. For example, as shown in Figure 1, some of the particles 24 are initially located near the outer surface of material 20 (e.g., the outer surface of the granules in this case), with at least a portion of those particles 24 exposed at the outer surface of refractory matrix 22. Other particles 24 are located below the outer surface and are not exposed.

[0036] The exposed particles 24 can contact the reactant(s) and thus participate in a catalytic reaction with the reactant(s). The refractory matrix 22 prevents or substantially prevents the particles 24 below the outer surface from contacting the reactant(s). Thus, the particles 24 below the outer surface are dormant and do not participate, or do not substantially participate, in a catalytic reaction.

[0037] With use over time, the exposed particles 24 may pool or migrate. However, in material 20, the movement of the initially exposed particles 24 due to pooling or migration indicates that additional particles 24 underneath are now exposed. Figure 2 shows particles 24 after some of the original particles 24 originally at the surface have migrated, resulting in newly exposed particles 24 underneath. The newly exposed particles 24 can then come into direct open contact with the reactant(s) and thus contribute to the catalytic reaction.

[0038] With further use over time, the particles 24 exposed by the movement of the particles above them will themselves pool or migrate to a new location, thereby exposing the next particle 24 below them, and so on. In that way, the material 20 essentially "self-replaces" particles 24 lost through pooling or migration, thereby compensating for the lost catalytic effect of the pooled / moved particles 24 with the catalytic effect of the newly exposed particles 24.

[0039] 3 illustrates an exemplary method 40 of manufacturing material 20. Method 40 includes steps 42, 44, and 46. Although each step is shown in a separate block, it should be understood that each step represents acts or functions that may be combined, further divided into substeps, or used with other method steps.

[0040] In step 42, a mixture of matrix particles and particles 24 is provided. The mixture can be provided as a pre-prepared mixture or can be prepared from starting materials. In the latter case, the starting matrix particles are mixed with the starting particles 24. If the matrix particles include multiple particle compositions, this can also include mixing the multiple compositions of the matrix particles together. Similarly, if the particles 24 include multiple compositions, the multiple compositions are mixed together. The order of mixing is not particularly noteworthy, and the starting materials can be mixed at once or in two or more sub-mixtures, which are then combined into the final mixture.

[0041] The starting matrix particles and starting particles 24 are most typically dry powders. For example, for ease of processing, the starting matrix particles are provided as a powder of the refractory that forms the refractory matrix 22 so that no chemical conversion of the starting matrix particles is required. Furthermore, the use of a powder of the refractory eliminates the need for chemical conversion. The characteristics of the dry powders are not particularly noteworthy, but generally, the matrix powder particles and particles 24 have a size, on average, of less than 100 micrometers, with one further example being 5-30 micrometers. The powders are mixed in a weight percentage ratio that corresponds to the desired percentages in the material 20. In this regard, the powders are mixed according to the percentages described above for the refractory matrix 22 and particles 24 in the material 20. Known techniques for mixing can be used. One example technique involves combining the dry powders and then mixing using a vibrating shaker (also known as a "paint shaker").

[0042] At step 44, the mixture is combined with at least a binder to produce a green state body. Most commonly, the binder is a polymer or resin, although other types of binders may be used instead, depending on the desired form of the green state body and additional processing steps. One example of a useful binder is a polyvinyl butyral resin, one such example being Butvar® B-79.

[0043] A solvent can be added to soften the binder and make the green body more moldable. For example, the solvent is one or more organic solvents, such as, but not limited to, isopropanol, methanol, or ethanol. In one example, an amount of solvent is added so that the green body becomes a thick paste. For example, the paste is easily moldable, but is self-supporting to retain the molded shape. In most cases, the green body is formed into one or more shapes that are desired or related to the end use. For example, forming can include, but is not limited to, extruding, molding, pressing, stamping, cutting, and splitting. In one particular example, the green body is extruded and then granulated by cutting or splitting into granules (i.e., a plurality of granular green body).

[0044] In step 46, the green body (or bodies, if applicable) is heat treated. The heat treatment sinters the matrix particles to produce the refractory matrix 22. The binder and residual solvent are also burned. The particles 24 mixed with the matrix particles thereby become embedded in the refractory matrix 22. Sintering is a solid-state thermal process in which the matrix particles fuse into a solid without melting. The temperature, environment, and pressure of sintering can vary depending on the composition of the refractory. Most typically, sintering is performed at a temperature substantially below the melting temperature of the refractory, in a cover gas that is inert with respect to reaction with the ceramic oxide, or alternatively in a reactive gas to promote chemical transformation. The sintering temperature varies, but is typically 40%-70% of the melting temperature. Additionally, sintering can be performed to control the heating rate, cooling rate, hold time, and / or temperature cycle according to a heating profile. An air or oxygen environment can be used to mitigate ceramic oxide loss.

[0045] During sintering, the matrix particles fuse together, trapping the particles 24 in the refractory matrix 22. Because sintering is primarily a solid mass transport phenomenon, chemical reactions during the process are expected to be minimal. Thus, if the dry starting powder composition is the composition selected for the refractory matrix 22 and particles 24, the composition of the refractory matrix 22 and particles 24 is expected to be equal to the composition of the dry starting powder. However, it is also possible that components of the dry starting powder react to produce a new, different composition or phase in the refractory matrix 22.

[0046] After sintering, the resulting consolidated material 20 is ready for use or may be subjected to additional processing steps depending on the end application. Comparative methods for depositing catalysts on the surface of a support typically involve the use of metal salts that require a step to reduce the metal (e.g., Ir salt to Ir metal). Method 40 avoids the use of such salts, thereby reducing the required steps and processing times. The following examples further demonstrate method 40.

[0047] Example 1 Ceramic oxide catalyst composite: HfO2 / CeO2 nominally 9 wt% Ir.

[0048] Dry powders of 0.5 grams Ir, 4.59 grams HfO2, 0.41 grams CeO2, and 0.21 grams B-79 were combined and mixed on a vibratory shaker for 15 minutes. A volume of 1.05 milliliters of isopropanol was then added and mixing continued for an additional 30 minutes. The resulting mixture had the consistency of a thick paste. The paste was then extruded into "noodles" and allowed to dry overnight. The dried noodles were then pressed through a size 20 mesh sieve to produce a granular green body. The granular green body was sintered in an air environment at a heating rate of 150°C / hr to 1700°C, held at that temperature for 10 hours, and then cooled to below 100°C at a rate of -150°C / hr. The resulting granules contained HfO2 / CeO2 alloy and Ir metal as shown by X-ray diffraction analysis.

[0049] Example 2 Ceramic oxide catalyst composite: HfO2 / CeO2 nominally 20 wt% Ir.

[0050] Dry powders of 1.0 gram Ir, 3.68 grams HfO2, 0.33 grams CeO2, and 0.16 grams B-79 were combined and mixed on a vibratory shaker for 15 minutes. A volume of 1.68 milliliters of isopropanol was then added and mixing continued for another 15 minutes. The mixture was fluid. Nitrogen gas was blown through the mixture to remove the isopropanol until a paste was obtained. The paste was then extruded into "noodles", dried, and then pressed through a size 20 mesh sieve to produce a granular green body. The granular green body was sintered in an air environment to 1700°C at a heating rate of 150°C / hr, held at that temperature for 10 hours, and then cooled to below 100°C at a rate of -150°C / hr.

[0051] Example 3 Ceramic oxide catalyst composite: HfO2 / CeO2 nominally 30 wt% Ir.

[0052] Dry powders of 1.5 grams Ir, 3.2 grams HfO2, 0.3 grams CeO2, and 0.14 grams B-79 were combined and mixed on a vibrating shaker for 15 minutes. A volume of 0.74 milliliters of isopropanol was then added and mixing continued for another 15 minutes, at which point the mixture was still powdery. An additional volume of 0.07 milliliters was added and mixing continued for another 5 minutes. This was repeated until the mixture was the consistency of a thick paste. The paste was then extruded into "noodles", dried, and then pressed through a size 20 mesh sieve to produce a granular green body. The granular green body was sintered in an air environment to 1700°C at a heating rate of 150°C / hour, held at that temperature for 10 hours, and then cooled to below 100°C at a rate of -150°C / hour.

[0053] Example 4 Ceramic oxide catalyst composite: HfO2 / CeO2 nominally 40 wt% Ir.

[0054] Dry powders of 65.47 grams of Ir (pre-sieved to -325 mesh), 89.94 grams of HfO2, 8.18 grams of CeO2, and 3.92 grams of B-79 were combined and mixed on a vibratory shaker for 15 minutes. A volume of 20.60 milliliters of isopropanol was then added and mixing continued for 15 minutes. The mixture appeared slightly dry, so an additional 3 milliliters of isopropanol was added and mixing continued for another 30 minutes. The resulting mixture had the consistency of a thick paste. The paste was then extruded into "noodles," dried, and then pressed through a size 20 mesh sieve to produce a granular green body. The granular green body was sintered in an air environment to 1700°C at a heating rate of 150°C / hr, held at that temperature for 10 hours, and then cooled to below 100°C at a rate of -150°C / hr. A further reduction step was used to reduce potential surface oxides on the accessible iridium metal.

[0055] FIG. 4 shows an example of the material 20. In this example, the material 20 is in a thruster 60. The thruster 60 includes a combustion chamber 62, an injector 64 for supplying a propellant P to the combustion chamber 62, and an outlet 66 for discharging decomposition gas C from the combustion chamber 62. In this example, the outlet 66 is a nozzle, but may alternatively be an orifice or other type of outlet. The material 20 is disposed in the combustion chamber 62 as a catalyst bed 68. The propellant P is introduced into the combustion chamber 62 via the injector 64. The catalyst bed 68 serves to promote ignition and decomposition of the propellant. The propellants are typically liquids and include, but are not limited to, ionic liquid monopropellants, hydrazine-based propellant blends, triazole-based propellant blends, peroxide-based propellants, and carbohydrazide-based propellant blends. The decomposition products are discharged through the outlet 66 to generate thrust.

[0056] Although combinations of features are shown in the illustrated examples, not all of them need to be combined to realize the advantages of various embodiments of the present disclosure. In other words, a system designed in accordance with an embodiment of the present disclosure does not necessarily include all of the features shown in any one of the drawings, or all of the portions shown diagrammatically in the drawings. Furthermore, selected features of one exemplary embodiment can be combined with selected features of other exemplary embodiments.

[0057] The foregoing description is exemplary rather than restrictive in nature. Variations and modifications to the disclosed examples may become apparent to those skilled in the art that do not necessarily depart from the present disclosure. The scope of legal protection given to this disclosure can only be determined by studying the following claims.

Claims

1. a fire-resistant matrix; particles comprised of a catalytic oxide dispersed and embedded throughout said refractory matrix; Equipped with The refractory matrix is ​​CeO 2 and HfO 2 is a two-component composition of A catalyst-containing material, wherein said particles are selected from V2O5, MnO2, and combinations thereof.

2. 2. The catalyst-containing material of claim 1, comprising: 5% to 50% by weight of particles composed of said catalytic oxide; and 95% to 50% by weight of said refractory matrix.

3. 3. The catalyst-containing material of claim 2, comprising 30% to 40% by weight of particles composed of said catalytic oxide and 70% to 60% by weight of said refractory matrix.

4. 13. A thruster comprising: a combustion chamber; an injector for supplying a propellant to said combustion chamber; and a catalyst-containing material as recited in claim 1 disposed in said combustion chamber to catalyze a reaction of said propellant.

5. Providing a mixture of matrix particles and particles composed of one or more catalytic metal elements or composed of catalytic oxides; combining the mixture with at least a binder to form one or more green bodies; heat treating the one or more green state bodies; Prepare for this.

4. A method for producing a catalyst-containing material, characterized in that the heat treatment causes sintering of the matrix particles, thereby producing a refractory matrix having dispersed and embedded therein particles composed of the one or more catalytic metal elements or the catalytic oxide.

6. The method of claim 5 further comprising granulating the one or more green bodies.

7. 6. The method of claim 5, wherein the particles are comprised of the one or more catalytic metal elements and are selected from Ir, Pt, Pd, Rh, Os, Ru, Re, and combinations thereof.

8. The particles are CeO 2 , HfO 2 , ZrO 2 , Y 2 O 3 , Ln 2 O 3 6. The method of claim 5, wherein the ceramic oxide particles are selected from the group consisting of: Ln, Ln+Ln, and combinations thereof, wherein Ln is a lanthanide element.

9. A combustion chamber; an injector for supplying a propellant to the combustion chamber; an outlet for discharging decomposition products from the combustion chamber; a catalyst-containing material disposed within the combustion chamber to catalyze a reaction of the propellant; Equipped with The catalyst-containing material is a fire-resistant matrix; particles comprised of a catalytic oxide dispersed and embedded throughout said refractory matrix; Equipped with the refractory matrix is ​​a binary composition of CeO 2 and HfO 2 ; A thruster, wherein said particles are selected from V2O5, MnO2, and combinations thereof.

Citation Information

Patent Citations

  • Porous catalyst, and method of producing the same

    JP2011224428A

  • Catalysts, gas generators, and thrusters with improved heating capacity and corrosion resistance.

    JP2014519408A

  • Catalyst

    JP2016175008A

  • Honeycomb structure and method for producing the same

    JP2017000936A

  • Corrosion resistant catalysts for decomposition of liquid monopropellants

    US20120297779A1