Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display element
The use of a specific diamine-based liquid crystal alignment agent with a side chain structure addresses adhesion and reworkability issues, improving the reliability and efficiency of liquid crystal display elements by reducing defects and maintaining display quality.
Patent Information
- Application Number
- JP2021546933
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-19
- Filing Date
- 2020-09-16
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-09-16
AI Technical Summary
Existing liquid crystal alignment films face issues with adhesion and reworkability, leading to deteriorated display quality and increased production costs due to defects requiring removal and substrate recovery.
A liquid crystal alignment agent comprising a specific diamine with a side chain structure and an imide skeleton, formulated with a polymer obtained from a combination of primary and secondary diamines, enhances adhesion and reworkability.
The solution provides a liquid crystal alignment film with improved adhesion and reworkability, reducing defects and maintaining display quality, thus enhancing the reliability and efficiency of liquid crystal display elements.
Smart Images

Figure 0007572661000001 
Figure 0007572661000002 
Figure 0007572661000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a liquid crystal aligning agent, a liquid crystal alignment film, and a liquid crystal display element. [Background technology]
[0002] Conventionally, liquid crystal devices have been widely used as display units for personal computers, mobile phones, television receivers, etc. A liquid crystal device includes, for example, a liquid crystal layer sandwiched between an element substrate and a color filter substrate, pixel electrodes and a common electrode for applying an electric field to the liquid crystal layer, an alignment film for controlling the alignment of liquid crystal molecules in the liquid crystal layer, and thin film transistors (TFTs) for switching electric signals supplied to the pixel electrodes. Known methods for driving liquid crystal molecules include vertical electric field methods such as the TN method and the VA method, and horizontal electric field methods such as the IPS method and the fringe field switching (FFS) method (for example, Patent Document 1).
[0003] In general, the horizontal electric field method, in which electrodes are formed on only one side of the substrate and an electric field is applied parallel to the substrate, is known as a liquid crystal display element that has a wider viewing angle characteristic and is capable of high-quality display compared to the conventional vertical electric field method, in which a voltage is applied to electrodes formed on the top and bottom substrates to drive the liquid crystal. One method for aligning the liquid crystal in a certain direction is to form a polymer film such as polyimide on the substrate and rub the surface with a cloth, a so-called rubbing treatment, which has been widely used industrially.
[0004] A liquid crystal alignment film, which is a component of a liquid crystal display element, is a film for uniformly aligning liquid crystals, but various other characteristics are required in addition to the uniformity of liquid crystal alignment. For example, there is a problem that electric charges accumulate in the liquid crystal alignment film due to the voltage that drives the liquid crystal, and these accumulated electric charges disrupt the alignment of the liquid crystal or affect the display as afterimages or burn-in (hereinafter referred to as residual DC-induced afterimages), significantly reducing the display quality of the liquid crystal display element, so a liquid crystal alignment agent that overcomes these problems has been proposed (Patent Document 2).
[0005] In addition, since the economic efficiency of the production process is very important, it is also required that the element substrate can be easily recycled. That is, after forming a liquid crystal alignment film from a liquid crystal alignment agent, if an inspection of the alignment is performed and a defect is found, it is required that a rework process of removing the liquid crystal alignment film from the substrate and recovering the substrate can be easily performed. However, since a liquid crystal alignment film is required to have adhesion to an undercoat, there is a demand for a liquid crystal alignment agent that can produce a liquid crystal alignment film having the necessary adhesion and that can easily perform a rework process. [Prior art documents] [Patent documents]
[0006] [Patent Document 1] Japanese Patent Application Publication No. 2013-167782 [Patent Document 2] International Publication No. 02 / 33481 Brochure Summary of the Invention [Problem to be solved by the invention]
[0007] In view of the above circumstances, the present invention aims to provide a liquid crystal alignment agent capable of producing a liquid crystal alignment film having necessary properties including adhesion and good reworkability, and a liquid crystal alignment film and a liquid crystal display element produced therefrom. [Means for solving the problem]
[0008] As a result of intensive research, the present inventors have found that by introducing a diamine having a specific side chain structure as a diamine component together with a specific diamine having an imide skeleton, It is possible to manufacture a liquid crystal alignment film that has the necessary properties including adhesion and has good reworkability. This finding led to the completion of the present invention.
[0009] The liquid crystal aligning agent of the present invention for achieving the above object is A liquid crystal aligning agent comprising: a polymer obtained from a diamine component including at least one first diamine represented by the following formula [I] and at least one second diamine having a side chain structure selected from the group represented by the following formulas [S1] to [S3]; and an organic solvent. [ka] (In formula [I], Z 1 is selected from the following formulas [Z-1] to [Z-9]. * represents a bond. [ka] [ka] (In formula [S1], X 1 and X 2 are each independently a single bond, -(CH2) a -(a represents an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 - (a1 is an integer of 1 to 15, A1 represents an oxygen atom or -COO-, and m1 is an integer of 1 to 2. When m1 is 2, a1 and A1 each independently have the above definition). 1 and G 2 each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms or a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with at least one selected from the group consisting of an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 6, preferably 1 to 4. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms; R 1 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom. [ka] (In formula [S2], X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -COO- or -OCO-. 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom. [ka] (In formula [S3], X 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-. 3 represents a structure having a steroid skeleton.) Effect of the Invention
[0010] According to the present invention, It is possible to manufacture a liquid crystal alignment film that has the necessary properties including adhesion and has good reworkability. It is possible to provide a liquid crystal alignment agent, a liquid crystal alignment film, and a liquid crystal display element. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The present invention will now be described in more detail.
[0012] The liquid crystal aligning agent of the present invention contains a polymer obtained from a diamine component including a first diamine having a structure represented by the above formula [I] and a second diamine compound having a side chain structure represented by the above formulas [S1] to [S3], and an organic solvent. First, the diamine will be described.
[0013] <Primary diamine> The primary diamine has a structure represented by the following formula [I]: [ka] (In formula [I], Z 1is as defined in the above formula [I].)
[0014] In the formula [I], the position of the amino group is preferably the para position or meta position as shown in the following formula [I-1] or [I-2]. 1 is selected from the following formulas [Z-1] to [Z-9]. * represents a bond. [ka] [ka]
[0015] The first diamine of the present invention can be obtained by reducing a dinitro compound to convert the nitro group to an amino group. The method for reducing a dinitro compound is not particularly limited, and examples of the method include a method in which reduction is performed using palladium-carbon, platinum oxide, Raney nickel, platinum black, rhodium-alumina, platinum sulfide carbon, or the like as a catalyst, and in a solvent such as ethyl acetate, toluene, tetrahydrofuran, dioxane, or an alcoholic system, with hydrogen gas, hydrazine, or hydrogen chloride. If necessary, the reduction may be performed under pressure using an autoclave, or the like.
[0016] The first diamine compound of the present invention thus obtained can be used as a raw material for polyimide precursors such as polyamic acid and polyamic acid ester, polyimide, polyurea, polyamide, etc. (collectively referred to as "polymer"). For example, this polymer can be dissolved in a specific organic solvent and used as a liquid crystal alignment agent, but is not limited to this application.
[0017] Among the above first diamines, the diamine represented by the following formula [II] is a novel compound. [ka] (In the formula [II], Z 2 is selected from the following formulas [Z-1] to [Z-4], [Z-6] and [Z-7]. * represents a bond. [ka]
[0018] In the formula [II], the position of the amino group is preferably the para position or meta position as in the above formula [I-1] or [I-2]. In this case, in the above formula [I-1] or [I-2], Z 1 is preferably selected from the above formulas [Z-1] to [Z-4], [Z-6] and [Z-7].
[0019] <Secondary diamines having specific side chain structures> The second diamine having a specific side chain structure exhibits vertical alignment properties and has at least one side chain structure selected from the group represented by the following formulas [S1] to [S3]. Hereinafter, examples of the second diamine having such a specific side chain structure, that is, the diamine having the specific side chain structure represented by the formulas [S1] to [S3], will be described in order.
[0020] [A]: A diamine having a specific side chain structure represented by the following formula [S1] [ka] In the above formula [S1], X 1 and X 2 are each independently a single bond, -(CH2) a -(a represents an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 - (a1 is an integer of 1 to 15, A1 represents an oxygen atom or -COO-, and m1 is an integer of 1 to 2. When m1 is 2, a1 and A1 each independently have the above definition).
[0021] Among them, X is the most popular in terms of availability of raw materials and ease of synthesis. 1 and X 2 are each independently a single bond, -(CH2) a-(a is an integer of 1 to 15), -O-, -CH2O- or -COO- is preferred, and a single bond, -(CH2) a -(a represents an integer of 1 to 10), -O-, -CH2O- or -COO- is more preferred.
[0022] In addition, in the above formula [S1], G 1 and G 2 each independently represents a divalent cyclic group selected from the group consisting of a divalent aromatic group having 6 to 12 carbon atoms and a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 6, and preferably 1 to 4.
[0023] In addition, in the above formula [S1], R 1 R represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. 1 Any hydrogen atom forming the group may be substituted with a fluorine atom. Examples of the divalent aromatic group having 6 to 12 carbon atoms include a phenylene group, a biphenyl structure, and a naphthylene group. Examples of the divalent alicyclic group having 3 to 8 carbon atoms include a cyclopropylene group and a cyclohexylene group.
[0024] Therefore, preferred specific examples of the above formula [S1] include the following formulae [S1-x1] to [S1-x7]. [ka]
[0025] In the above formula [S1-x1] to [S1-x7], R 1 is the same as in the above formula [S1]. p is -(CH2) aA1 represents an oxygen atom or -COO-* (the bond marked with "*" is (CH2)). a2 A2 represents an oxygen atom or *-COO- (the bond marked with "*" is (CH2) a2 a3 represents an integer of 0 or 1, and a1 and a2 each independently represent an integer of 2 to 10. Cy represents a 1,4-cyclohexylene group or a 1,4-phenylene group.
[0026] [B]: Diamine having a specific side chain structure represented by the following formula [S2] [ka] In the above formula [S2], X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -COO- or -OCO-. Among them, from the viewpoint of the liquid crystal alignment property of the liquid crystal alignment agent, X 3 is preferably -CONH-, -NHCO-, -O-, -CHO-, -COO- or -OCO-.
[0027] In addition, in the above formula [S2], R 2 R represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms. 2 Any hydrogen atom forming R may be substituted with a fluorine atom. 2 is preferably an alkyl group having 3 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms. Preferred examples of the formula [S2] include X 3 is any one of -O-, -CHO-, -COO-, or -OCO-, and R 2 is preferably an alkyl group having 3 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms, and R 2 is more preferably an alkyl group having 3 to 20 carbon atoms, and R 2Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom.
[0028] [C]: Diamine having a specific side chain structure represented by the following formula [S3] [ka] In the above formula [S3], X 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-. 3 represents a structure having a steroid skeleton. The steroid skeleton here includes a skeleton represented by the following formula (st) in which three six-membered rings and one five-membered ring are bonded. [ka]
[0029] An example of the above formula [S3] is the following formula [S3-x], where Me represents a methyl group. [ka]
[0030] In the formula [S3-x], X represents the formula [X1] or [X2]. Col represents any group selected from the group consisting of the formulas [Col1] to [Col3], and G represents any group selected from the group consisting of the formulas [G1] to [G4]. * represents a site for bonding to another group.
[0031] In the above formula [S3-x], examples of preferred combinations of X, Col, and G include the following combinations: [X1], [Col1], and [G1], [X1], [Col1], and [G2], [X1], [Col2], and [G1], [X1], [Col2], and [G2], [X1], [Col3], and [G2], [X1], [Col3], and [G1], [X2], [Col1], and [G2], [X2], [Col2], and [G2], [X2], [Col2], and [G1], [X2], [Col3], and [G2], [X2], [Col1], and [G1].
[0032] Specific examples of the above formula [S3] include a structure obtained by removing a hydroxyl group (hydroxy group) from the steroid compound described in paragraph
[0024] of JP-A-4-281427, a structure obtained by removing an acid chloride group from the steroid compound described in paragraph
[0030] of the same publication, a structure obtained by removing an amino group from the steroid compound described in paragraph
[0038] of the same publication, a structure obtained by removing a halogen atom from the steroid compound described in paragraph
[0042] of the same publication, and the structures described in paragraphs
[0018] to
[0022] of JP-A-8-146421.
[0033] A representative example of the steroid skeleton is cholesterol (the combination of [Col1] and [G2] in the above formula [S3-x]), but a steroid skeleton that does not contain cholesterol can also be used. That is, an example of a diamine having a steroid skeleton is cholestanyl 3,5-diaminobenzoate, but it is also possible to use a diamine component that does not contain a diamine having a cholesterol skeleton. In addition, as a diamine having a specific side chain structure, one that does not contain an amide bond at the linking position between the diamine and the side chain can also be used. In this embodiment, a liquid crystal alignment agent that can obtain a liquid crystal alignment film or liquid crystal display element that can ensure a high voltage retention rate for a long period of time can be provided, even if a diamine component that does not contain a diamine having a cholesterol skeleton is used.
[0034] The diamine having a side chain structure represented by the above formulae [S1] to [S3] is preferably at least one selected from the diamines represented by the following formulae [1] and [2]. [ka] (In formula [1], Y represents a monovalent group selected from the side chain structures represented by the above formulas [S1] to [S3]. In formula [2], X represents a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -(CH2) m -, -SO2-, -O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m-, -NH-(CH2) m -, -SO2-(CH2) m -, -CONH-(CH2) m -, -CONH-(CH2) m -NHCO-, -COO-(CH2) m -OCO-, -CONH-, -NH-(CH2) m -NH- or -SO2-(CH2) m represents -SO2-; m is an integer of 1 to 8; two Y's each independently represent a monovalent group selected from the side chain structures represented by the above formulas [S1] to [S3].
[0035] Preferred specific examples of the diamine represented by the above formula [1] include diamines represented by the following formulas [1-S1] to [1-S3]. Specific examples of the diamine represented by the formula [2] will be described later in connection with a diamine having a specific two-side chain structure that exhibits vertical alignment. [ka] In the above formula [1-S1], X 1 , X 2 , G 1 , G 2 , R 1 , m and n are the same as those in the above formula [S1]. In the above formula [1-S2], X 3 and R 2 is the same as in the above formula [S2]. In the above formula [1-S3], X 4 and R 3 is the same as in the above formula [S3].
[0036] (Diamine with specific two-side chain structure that exhibits vertical alignment) The diamine having a specific two-side chain structure that exhibits vertical alignment is represented by the above formula [2].
[0037] In the above formula [2], X is a single bond, -O-, -NH-, or -O-(CH2) m It is preferred to designate -O-.
[0038] In addition, in the above formula [2], Y may be in the meta position or the ortho position relative to the position of X, but is preferably in the ortho position. That is, the above formula [2] is preferably the following formula [1']. [ka]
[0039] In the above formula [2], the positions of the two amino groups (-NH2) may be any positions on the benzene ring, but the positions represented by the following formulas [1]-a1 to [1]-a3 are preferred, and the following formula [1]-a1 is more preferred. In the following formulas, X is the same as in the above formula [2]. Note that the following formulas [1]-a1 to [1]-a3 explain the positions of the two amino groups, and the notation of Y represented in the above formula [2] is omitted. [ka]
[0040] Therefore, based on the above formula [1'] and [1]-a1 to [1]-a3, the above formula [2] is preferably any structure selected from the group consisting of the following formulas [1]-a1-1 to [1]-a3-2, and more preferably the structure represented by the following formula [1]-a1-1. In the following formula, X and Y are the same as in the above formula [2]. [ka]
[0041] Examples of the above formulae [S1] to [S3] include the following formulae [S]-1 to [S]-20. Of these, examples of the above formula [S1] are preferably the following formulae [S]-1 to [S]-4, [S]-8 or [S]-10. In the following formulae, * represents the bonding position with the phenyl group in the above formulae [1], [1'] and [1]-a1 to [1]-a3. In [S]-1 to [S]-20, n is an integer from 1 to 20, and m is an integer from 1 to 6. [ka]
[0042] [ka]
[0043] The diamine component contains a two-side chain diamine having a predetermined structure, and thus the liquid crystal alignment film is one in which the ability to vertically align liquid crystals is unlikely to decrease even when exposed to excessive heat. In addition, the diamine component contains the two-side chain diamine, and thus the liquid crystal alignment film is one in which the ability to vertically align liquid crystals is unlikely to decrease even when the film comes into contact with some foreign matter and is damaged. In other words, the diamine component contains the two-side chain diamine, and thus it is possible to provide a liquid crystal alignment agent that can provide a liquid crystal alignment film having the above-mentioned various excellent properties.
[0044] In the present embodiment, when the diamine component contains the first diamine and the second diamine, the content of the first diamine is preferably 10 to 90 mol %, more preferably 20 to 80 mol %, of the total diamine component. The content of the second diamine is preferably 10 to 90 mol %, more preferably 20 to 80 mol %. When other diamines described below are contained, the total content of the first diamine and the second diamine is preferably 95 mol % or less, more preferably 90 mol % or less.
[0045] <Other diamines: diamines having photoreactive side chains> The diamine component of the present embodiment may contain a diamine having a photoreactive side chain as the other diamine. When the diamine component contains a diamine having a photoreactive side chain, the photoreactive side chain can be introduced into the specific polymer or other polymers. Specific examples of diamines having a photoreactive side chain include, but are not limited to, those described in paragraphs
[0124] to
[0132] of Republished Patent Publication No. 2016-140328. More preferred specific examples include the following formulas (a-1) to (a-4). [ka] (X 9 , X 10 each independently represents a bonding group which is a single bond, -O-, -COO-, -NHCO-, or -NH-, and Y represents an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom.
[0046] These diamines having photoreactive side chains can be used alone or in combination of two or more. Whether to use alone or in combination of two or more, and when used in combination of two or more, the ratio, etc., may be appropriately adjusted depending on the liquid crystal alignment property, pretilt angle, voltage retention property, stored charge property, etc., when used as a liquid crystal alignment film, and the response speed of the liquid crystal when used as a liquid crystal display element.
[0047] In the present embodiment, when the diamine component contains a photoreactive side chain diamine, the photoreactive side chain diamine preferably accounts for 10 to 70 mol %, and more preferably 10 to 60 mol %, of the entire diamine component.
[0048] <Other diamines: diamines other than those mentioned above> The other diamines that may be contained in the diamine component for obtaining the specific polymer are not limited to the above-mentioned diamines having a photoreactive side chain. When producing a polyimide precursor and / or a polyimide, other diamines than the above diamines can be used as a diamine component as long as the effects of the present invention are not impaired.Specific examples include diamines described in paragraph
[0135] of republished patent publication WO2016-140328, or 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, diamines represented by the following formulas (z-1) to (z-18), diamines having a radical initiation function such as the following formulas (R1) to (R5), and diamines having a group "-N(D)-" such as the following formulas (5-1) to (5-11) (D represents a protecting group that is detached by heating and replaced with a hydrogen atom, preferably a tert-butoxycarbonyl group). [ka] [ka] [ka] (In the formula, n is an integer of 2 to 10.) [ka]
[0049] Among the diamines described in paragraph
[0135] of the above-mentioned republished patent publication WO2016-140328, preferred specific examples are shown below. p-Phenylenediamine, 2,3,5,6-tetramethyl-p-phenylenediamine, 2,5-dimethyl-p-phenylenediamine, m-phenylenediamine, 2,4-dimethyl-m-phenylenediamine, 2,5-diaminotoluene, 2,6-diaminotoluene, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-dimethoxy-4,4'-diaminobiphenyl, 3,3'-dihydroxy-4,4'-diaminobiphenyl, 3,3'-dicarboxy-4,4'-diaminobiphenyl, 3,3'-difluoro- 4,4'-biphenyl, 3,3'-trifluoromethyl-4,4'-diaminobiphenyl, 3,4'-diaminobiphenyl, 3,3'-diaminobiphenyl, 2,3'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 2,3'-diaminodiphenylmethane, 4,4'-diaminodiphenylether, 3,3'-diaminodiphenylether, 3,4'-diaminodiphenylether, 2,3'-diaminodiphenylether, 4,4'-sulfonyldianiline, 3,3'-Sulfonyldianiline, Bis(4-aminophenyl)silane, Bis(3-aminophenyl)silane, Dimethyl-bis(4-aminophenyl)silane, Dimethyl-bis(3-aminophenyl)silane, 4,4'-thiodianiline, 3,3'-thiodianiline, 4,4'-diaminodiphenylamine, 3,3'-diaminodiphenylamine, 3,4'-diaminodiphenylamine, 2,3'-diaminodiphenylamine, N-methyl(4,4'-diaminodiphenyl)amine, N-methyl(3,3'-diaminodiphenyl)amine, N-methyl(3, 4'-diaminodiphenyl)amine, N-methyl(2,2'-diaminodiphenyl)amine, N-methyl(2,3'-diaminodiphenyl)amine, 4,4'-diaminobenzophenone, 3,3'-diaminobenzophenone, 3,4'-diaminobenzophenone, 1,4-diaminonaphthalene, 2,3'-diaminobenzophenone, 1,5-diaminonaphthalene, 1,2-bis(4-aminophenyl)ethane, 1,2-bis(3-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,3-bis(3-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(3-aminophenyl)butane, bis(3,5-diethyl-4-aminophenyl)methane, 1,3-bis(4-aminophenoxy)propane, 1,3-bis(3-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)butane, 1,4-bis(3-aminophenoxy)butane, 1,5-bis(4-aminophenoxy)pentane, 1,5-bis(3-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,6-bis(3-aminophenoxy)hexane, 1,4-bis(4-aminophenoxy)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-[1,4-phenylenebis(methylene)]dianiline, 4,4'-[1,3-phenylenebis(methylene)]dianiline, 3,4'-[1,4-phenylenebis(methylene)]dianiline, 3,4'-[1,3-phenylenebis(methylene) ]dianiline, 3,3'-[1,4-phenylenebis(methylene)]dianiline, 3,3'-[1,3-phenylenebis(methylene)]dianiline, 1,4-phenylenebis[(4-aminophenyl)methanone], 1,4-phenylenebis[(3-aminophenyl)methanone], 1,3-phenylenebis[(4-aminophenyl)methanone], 1,3-phenylenebis[(3-aminophenyl)methanone], 1,4-phenylenebis(4-aminobenzoate), 1,4-phenylenebis(3-aminobenzoate), 1,3-phenylenebis(4-amino aminobenzoate), 1,3-phenylenebis(3-aminobenzoate), bis(4-aminophenyl)terephthalate, bis(3-aminophenyl)terephthalate, bis(4-aminophenyl)isophthalate, bis(3-aminophenyl)isophthalate, N,N'-(1,4-phenylene)bis(4-aminobenzamide), N,N'-(1,3-phenylene)bis(4-aminobenzamide), N,N'-(1,4-phenylene)bis(3-aminobenzamide), N,N'-(1,3-phenylene)bis(3-aminobenzamide), N,N'-bis(4-aminophenyl)terephthalamide, N,N'-bis(3-aminophenyl)terephthalamide, N,N'-bis(4-aminophenyl)isophthalamide, N,N'-bis(3-aminophenyl)isophthalamide, 9,10-bis(4-aminophenyl)anthracene, 4,4'-bis(4-aminophenoxy)diphenylsulfone, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis[4-(4-aminophenoxy)phenyl]hexafluoropropane, 2,2'-bis(4-aminophenyl)hexafluoropropane, 2,2'-bis(3-aminophenyl) Aromatic diamines such as 2,2'-bis(4-aminophenyl)hexafluoropropane, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(3-aminophenyl)propane, 2,2'-bis(3-amino-4-methylphenyl)propane, 3,5-diaminobenzoic acid, and 2,5-diaminobenzoic acid; alicyclic diamines such as bis(4-aminocyclohexyl)methane and bis(4-amino-3-methylcyclohexyl)methane; and aliphatic diamines such as 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, and 1,6-diaminohexane.
[0050] The above other diamines can be used alone or in combination of two or more depending on the properties, such as liquid crystal alignment property, pretilt angle, voltage holding property, and stored charge, when formed into a liquid crystal alignment film.
[0051] <Polymer> The polymer of the present invention is a polymer obtained by using the above diamine, and preferably includes polyamic acid, polyamic acid ester, polyimide, polyurea, polyamide, etc. obtained by reacting a diamine component with a tetracarboxylic dianhydride. From the viewpoint of use as a liquid crystal aligning agent, it is preferable that the polymer is at least one selected from polyimide precursors such as the above polyamic acid and polyamic acid ester, and polyimides which are imidized products thereof.
[0052] <Tetracarboxylic acid dianhydride> As the tetracarboxylic acid component for obtaining the specific polymer, a tetracarboxylic acid dianhydride represented by the following formula [II'] or a derivative thereof (tetracarboxylic acid, tetracarboxylic acid dihalide, tetracarboxylic acid dialkyl ester, or tetracarboxylic acid dialkyl ester dihalide) (collectively referred to as specific tetracarboxylic acid) can be used.
[0053] [ka] (In formula [II'], Q represents at least one structure selected from the group consisting of the following formulas [II'-a] to [II'-q].) [ka] [ka]
[0054] In formula [II'-a], Q 1 ~Q 4 Each of Q independently represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom, or a benzene ring. 5 and Q 6 each independently represents a hydrogen atom or a methyl group. Among Q in formula [II'], in terms of ease of synthesis and ease of polymerization reactivity in producing a polymer, tetracarboxylic dianhydrides having a structure represented by formula [II'-a], formula [II'-c] to formula [II'-g], formula [II'-k] to formula [II'-m] or formula [II'-p] and tetracarboxylic acid derivatives thereof are preferred. More preferred are those having a structure represented by formula [II'-a], formula [II'-e] to formula [II'-g], formula [II'-l], formula [II'-m] or formula [II'-p]. Particularly preferred are tetracarboxylic dianhydrides having a structure represented by formula [II'-a], formula [II'-e], formula [II'-f], formula [II'-l], formula [II'-m] or formula [II'-p] and tetracarboxylic acid derivatives thereof.
[0055] More specifically, it is preferable to use the following formula [II'-a-1] or formula [II'-a-2]. [ka] The specific tetracarboxylic acid is preferably 50 to 100 mol % in 100 mol % of all the tetracarboxylic acid components, more preferably 70 to 100 mol %, and particularly preferably 80 to 100 mol %.
[0056] The specific tetracarboxylic acid may be used alone or in combination of two or more depending on the properties such as the solubility of the specific polymer in a solvent, the coatability of the liquid crystal alignment agent, the alignment of the liquid crystal when formed into a liquid crystal alignment film, the voltage holding rate, and the stored charge.
[0057] The tetracarboxylic acid component for obtaining the specific polymer may contain a tetracarboxylic acid other than the specific tetracarboxylic acid (hereinafter, also referred to as other tetracarboxylic acid) or a derivative thereof. Examples of the other tetracarboxylic acid include the following tetracarboxylic acid compounds or derivatives thereof (tetracarboxylic acid dianhydride, tetracarboxylic acid dihalide compound, tetracarboxylic acid dialkyl ester compound, or tetracarboxylic acid dialkyl ester dihalide compound).
[0058] That is, other tetracarboxylic acids include 1,2,5,6-naphthalenetetracarboxylic acid, 1,2,5,6-anthracenetetracarboxylic acid, 2,3,3',4-biphenyltetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether, 3,3',4,4'-benzophenonetetracarboxylic acid, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)methane, and 2,2-bis(3,4-dicarboxyphenyl)propane. 1,1,1,3,3,3-hexafluoro-2,2-bis(3,4-dicarboxyphenyl)propane, bis(3,4-dicarboxyphenyl)dimethylsilane, bis(3,4-dicarboxyphenyl)diphenylsilane, 2,3,4,5-pyridinetetracarboxylic acid, 2,6-bis(3,4-dicarboxyphenyl)pyridine, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, and 3,4,9,10-perylenetetracarboxylic acid. Other tetracarboxylic acids can be used alone or in combination depending on the solubility of the specific polymer in a solvent, the coatability of the liquid crystal alignment agent, and properties such as liquid crystal alignment, voltage holding rate, and stored charge when used as a liquid crystal alignment film.
[0059] The polyimide precursor used in the present invention may be a polyamic acid or a polyamic acid ester. All of the constituent units of the polyamic acid ester may have an amic acid ester structure, or may partially contain an amic acid structure.
[0060] <Method of Producing Polymer> The polymer of the present invention is obtained by a method of reacting the above-described diamine component (diamine component consisting of multiple first diamines and multiple second diamines) with a tetracarboxylic acid component. For example, the method includes a method of reacting a diamine component consisting of one or multiple diamines with at least one tetracarboxylic acid component selected from the group consisting of tetracarboxylic dianhydrides and derivatives of the tetracarboxylic acid to obtain a polyamic acid. Specifically, a method of polycondensing a primary or secondary diamine with a tetracarboxylic dianhydride to obtain a polyamic acid is used.
[0061] To obtain a polyamic acid ester, a method of polycondensing a tetracarboxylic acid dialkyl ester in which a carboxylic acid group has been esterified with a primary or secondary diamine, a method of polycondensing a tetracarboxylic acid dihalide in which a carboxylic acid group has been halogenated with a primary or secondary diamine, or a method of converting a carboxy group of a polyamic acid into an ester is used.To obtain a polyimide, a method of ring-closing the above-mentioned polyamic acid or polyamic acid ester to obtain a polyimide is used.
[0062] The reaction between the diamine component and the tetracarboxylic acid component is usually carried out in a solvent. The solvent used at that time is not particularly limited as long as the generated polyimide precursor dissolves in the solvent. Examples of the solvent include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, 1,3-dimethyl-2-imidazolidinone, etc. In addition, when the polyimide precursor has high solvent solubility, methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, or solvents represented by the following formulas [D-1] to [D-3], etc. can be used.
[0063] [ka]
[0064] In formula [D-1], D 1 represents an alkyl group having 1 to 3 carbon atoms. 2 represents an alkyl group having 1 to 3 carbon atoms. 3 represents an alkyl group having 1 to 4 carbon atoms.
[0065] These solvents can be used alone or in combination of two or more. Even if the solvent does not dissolve the polyimide precursor, it may be mixed with the above-mentioned solvent as long as the generated polyimide precursor does not precipitate. In addition, since moisture in the solvent inhibits the polymerization reaction and further causes hydrolysis of the generated polyimide precursor, it is preferable to use a solvent that has been dehydrated and dried.
[0066] When the diamine component and the tetracarboxylic acid component are reacted in a solvent, any of the following methods may be used: a method in which a solution in which the diamine component is dispersed or dissolved in a solvent is stirred, and the tetracarboxylic acid component is added as is or after being dispersed or dissolved in the solvent; a method in which the diamine component is added to a solution in which the tetracarboxylic acid component is dispersed or dissolved in a solvent; a method in which the diamine component and the tetracarboxylic acid component are added alternately; etc. When a plurality of diamine components or tetracarboxylic acid components are used for the reaction, they may be reacted in a premixed state, or may be reacted individually in sequence, or low molecular weight substances that have been reacted individually may be mixed and reacted to form a polymer.
[0067] The temperature at which the diamine component and the tetracarboxylic acid component are polycondensed can be selected from any temperature range of -20 to 150°C, but is preferably in the range of -5 to 100°C. The reaction can be carried out at any concentration, but the concentration of the diamine component and the tetracarboxylic acid component relative to the above solvent is preferably 1 to 50% by mass, more preferably 5 to 30% by mass. The reaction can be carried out at a high concentration in the early stage, and then the solvent can be added.
[0068] In the polymerization reaction of the polyimide precursor, the ratio of the total number of moles of the diamine components to the tetracarboxylic acid components (total number of moles of the diamine components / total number of moles of the tetracarboxylic acid components) is preferably 0.8 to 1.2. As in the case of a normal polycondensation reaction, the closer this molar ratio is to 1.0, the higher the molecular weight of the resulting polyimide precursor will be.
[0069] The polyimide is obtained by ring-closing the polyimide precursor, and the ring-closing rate of the amic acid group (also called the imidization rate) in this polyimide does not necessarily need to be 100%, and can be adjusted as desired depending on the application or purpose. Methods for imidizing the polyimide precursor include thermal imidization, in which a solution of the polyimide precursor is heated as is, and catalytic imidization, in which a catalyst is added to a solution of the polyimide precursor.
[0070] In the liquid crystal aligning agent of the present invention, it is generally believed that the higher the imidization ratio, the more reliable the liquid crystal alignment film can be obtained, but since the polymer of the present invention has an imide ring derived from the first diamine, it is not necessary to increase the imidization ratio, which is advantageous in terms of improving solubility and reworkability.
[0071] The temperature for thermally imidizing the polyimide precursor in a solution is 100 to 400° C., preferably 120 to 250° C., and it is preferable to carry out the imidization while removing water generated by the imidization reaction from the system. Catalytic imidization of the polyimide precursor can be carried out by adding a basic catalyst and an acid anhydride to a solution of the polyimide precursor and stirring the mixture at −20 to 250° C., preferably 0 to 180° C.
[0072] The amount of the basic catalyst is 0.5 to 30 times by mol, preferably 2 to 20 times by mol, the amount of the acid anhydride is 1 to 50 times by mol, preferably 3 to 3 ...
[0073] When recovering the generated polyimide precursor or polyimide from the reaction solution of the polyimide precursor or polyimide, the reaction solution may be poured into a solvent to cause precipitation. Examples of the solvent used for precipitation include methanol, ethanol, isopropyl alcohol, acetone, hexane, butyl cellosolve, heptane, methyl ethyl ketone, methyl isobutyl ketone, toluene, benzene, water, etc. The polymer precipitated by pouring into the solvent can be recovered by filtration, and then dried at normal pressure or reduced pressure, or at room temperature or by heating. In addition, the polymer precipitated and recovered can be redissolved in a solvent and the reprecipitation and recovery operation repeated 2 to 10 times to reduce impurities in the polymer. Examples of the solvent in this case include alcohols, ketones, and hydrocarbons. It is preferable to use three or more solvents selected from these because the efficiency of purification is further improved.
[0074] <Liquid crystal alignment agent> The liquid crystal aligning agent of the present invention contains the above-mentioned polymer (hereinafter also referred to as the specific polymer), but may contain two or more polymers with different structures. In addition to the polymer, it may contain other polymers. Examples of the polymer type include polyamic acid, polyimide, polyamic acid ester, polyester, polyamide, polyurea, polyorganosiloxane, cellulose derivative, polyacetal, polystyrene or its derivative, poly(styrene-phenylmaleimide) derivative, poly(meth)acrylate, etc. When the liquid crystal aligning agent of the present invention contains other polymers, the ratio of the specific polymer to the total polymer components is preferably 5% by mass or more, for example, 5 to 95% by mass.
[0075] The liquid crystal aligning agent generally takes the form of a coating liquid in order to form a uniform thin film. The liquid crystal aligning agent of the present invention is also preferably a coating liquid containing the above-mentioned polymer component and an organic solvent that dissolves the polymer component. In this case, the concentration of the polymer in the liquid crystal aligning agent can be appropriately changed depending on the thickness of the coating film to be formed. In order to form a uniform and defect-free coating film, the concentration is preferably 1% by mass or more, and in order to ensure the storage stability of the solution, the concentration is preferably 10% by mass or less. A particularly preferred concentration of the polymer is 2 to 8% by mass.
[0076] The organic solvent contained in the liquid crystal alignment agent is not particularly limited as long as the polymer component is uniformly dissolved in the organic solvent. Specific examples include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-(n-propyl)-2-pyrrolidone, N-isopropyl-2-pyrrolidone, N-(n-butyl)-2-pyrrolidone, N-(tert-butyl)-2-pyrrolidone, N-(n-pentyl)-2-pyrrolidone, N-methoxypropyl-2-pyrrolidone, and N-ethoxypropyl-2-pyrrolidone. Examples of suitable dimethyl-2-pyrrolidone include diethyl-2-pyrrolidone, N-methoxybutyl-2-pyrrolidone, N-cyclohexyl-2-pyrrolidone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, γ-butyrolactam, dimethylsulfoxide, γ-butyrolactone, γ-valerolactone, 1,3-dimethyl-2-imidazolidinone, methyl ethyl ketone, cyclohexanone, and cyclopentanone. Among these, it is preferable to use N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, or γ-butyrolactone.
[0077] In addition to the above-mentioned solvents, the organic solvent contained in the liquid crystal alignment agent of the present invention may be a solvent that improves the coatability and the surface smoothness of the coating film when the liquid crystal alignment agent is applied. Specific examples of such organic solvents include those described in paragraph
[0177] of republished patent publication WO2016-140328. Preferred specific examples include the following solvents. 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monomethyl ether, butyl lactate, butyl acetate, methyl 3-methoxypropionate, ethyl 3-ethoxypropionate, ethyl 3-methoxypropionate, propyl 3-methoxypropionate, butyl 3-methoxypropionate, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol-n-propyl ether, ethylene glycol-i-propyl ether, ethylene glycol monobutyl ether (butyl cellosolve), ethylene glycol dimethyl ether, ethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monobutyl ... Examples of suitable alkyl ethers include ethylene glycol monobutyl ether, propylene glycol diacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, diisobutyl carbinol (2,6-dimethyl-4-heptanol), diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, and propylene carbonate.
[0078] The liquid crystal alignment agent of the present invention may additionally contain components other than the polymer component and the organic solvent. Examples of such additional components include an adhesion aid for increasing the adhesion between the liquid crystal alignment film and the substrate, or between the liquid crystal alignment film and the sealant, a crosslinking agent for increasing the strength of the liquid crystal alignment film, a dielectric or conductive material for adjusting the dielectric constant or electrical resistance of the liquid crystal alignment film, and an imidization promoter for efficiently proceeding with imidization by heating the polyimide precursor when baking the coating film. Specific examples of these additional components include crosslinkable compounds or known crosslinking agents disclosed in paragraphs
[0104] on page 53 to
[0116] on page 60 of International Publication No. 2015 / 060357. Specific examples of preferred crosslinking agents include compounds represented by the following formulas (CL-1) to (CL-11). The amount of the crosslinking agent is preferably 0.1 to 30 parts by mass, more preferably 1 to 20 parts by mass, relative to 100 parts by mass of the total amount of the polymers contained in the liquid crystal alignment agent. [ka]
[0079] Examples of adhesion aids for improving the adhesion between the liquid crystal alignment film and the substrate include functional silane-containing compounds and epoxy group-containing compounds. Specific examples include those described in paragraph
[0180] of the republished patent publication WO2016-140328.
[0080] <Liquid crystal alignment film> The liquid crystal alignment film of the present invention is obtained from the liquid crystal alignment agent. By using the liquid crystal alignment agent of the present invention, it is possible to provide a liquid crystal alignment film and a liquid crystal display element that are particularly suitable for the VA mode, particularly the PSA mode, in which liquid crystal molecules aligned perpendicular to the substrate are made to respond to an electric field, and that have excellent voltage retention, rapid relaxation of accumulated charges, and excellent afterimage characteristics. As an example of a method for obtaining a liquid crystal alignment film, the liquid crystal alignment agent of the present invention is applied to a substrate, and then dried and baked as necessary to obtain a cured film, which can be used as a liquid crystal alignment film as it is. In addition, this cured film can be rubbed, irradiated with polarized light or light of a specific wavelength, or treated with an ion beam, or irradiated with UV light while applying a voltage to a liquid crystal display element after filling with liquid crystal as an alignment film for PSA. In particular, it is useful to use it as an alignment film for PSA.
[0081] The substrate to which the liquid crystal alignment agent is applied is not particularly limited as long as it is a highly transparent substrate, and in addition to glass substrates and silicon nitride substrates, plastic substrates such as acrylic substrates and polycarbonate substrates can also be used. In this case, it is preferable to use a substrate on which an ITO electrode for driving the liquid crystal is formed in terms of simplifying the process. In addition, in a reflective liquid crystal display element, an opaque material such as a silicon wafer can be used for only one substrate, and in this case, a light-reflecting material such as aluminum can also be used for the electrode.
[0082] The method of applying the liquid crystal alignment agent is not particularly limited, but industrially, screen printing, offset printing, flexographic printing, inkjet printing, etc. are generally used. Other application methods include a dip method, a roll coater method, a slit coater method, a spinner method, a spray method, etc., and these may be used depending on the purpose. After the liquid crystal alignment agent is applied to the substrate, the solvent is evaporated and baked by a heating means such as a hot plate, a heat circulation type oven, an IR (infrared) type oven, etc. The drying and baking process after the liquid crystal alignment agent is applied can be selected at any temperature and time. Although the drying process is not necessarily required, it is preferable to perform a drying process when the time from application to baking is not constant for each substrate, or when baking is not performed immediately after application. This drying is sufficient as long as the solvent is removed to an extent that the coating film shape is not deformed by transportation of the substrate, etc., and the drying means are not particularly limited. For example, a method of drying for 0.5 to 30 minutes, preferably 1 to 5 minutes, on a hot plate at a temperature of 40 to 150 ° C., preferably 60 to 100 ° C., can be mentioned.
[0083] The baking temperature of the coating film formed by applying the liquid crystal alignment agent is not limited, and is, for example, 100 to 350° C., preferably 120 to 300° C., and more preferably 150 to 250° C. The baking time is 5 to 240 minutes, preferably 10 to 90 minutes, and more preferably 20 to 90 minutes. Heating can be performed by a commonly known method, for example, a hot plate, a hot air circulation oven, an infrared oven, or the like.
[0084] The thickness of the liquid crystal alignment film after baking is preferably 5 to 300 nm, more preferably 10 to 200 nm, since if it is too thin, the reliability of the liquid crystal display element may decrease. The liquid crystal alignment film of the present invention is useful as a liquid crystal alignment film for a VA mode, particularly a PSA mode, liquid crystal display element.
[0085] <Liquid crystal display element and its manufacturing method> The liquid crystal display element can be manufactured by forming a liquid crystal alignment film on the substrate by the above method, and then manufacturing a liquid crystal cell by a known method. A specific example of the liquid crystal display element is a vertical alignment type (VA type) liquid crystal display element having a liquid crystal cell having two substrates arranged to face each other, a liquid crystal layer provided between the substrates, and the above liquid crystal alignment film formed by a liquid crystal alignment agent provided between the substrates and the liquid crystal layer. A more preferred example is a vertical alignment type liquid crystal display element (the above PSA mode liquid crystal display element) having a liquid crystal cell manufactured by applying a liquid crystal alignment agent onto two substrates and baking the liquid crystal alignment film to form a liquid crystal alignment film, arranging the two substrates so that the liquid crystal alignment film faces each other, sandwiching a liquid crystal layer made of liquid crystal between the two substrates, i.e., providing the liquid crystal layer in contact with the liquid crystal alignment film, and applying a voltage to the liquid crystal alignment film and the liquid crystal layer while irradiating them with ultraviolet light.
[0086] The substrate of the liquid crystal display element is not particularly limited as long as it is a highly transparent substrate, but is usually a substrate on which a transparent electrode for driving liquid crystal is formed. Specific examples include the same substrates as those described for the liquid crystal alignment film. Although a substrate on which a conventional electrode pattern or protrusion pattern is formed may be used, the liquid crystal display element uses a liquid crystal alignment agent containing the polyimide polymer of the present invention, so that the liquid crystal display element can operate even in a structure in which, for example, a line / slit electrode pattern of 1 μm to 10 μm is formed on one substrate and a slit pattern or protrusion pattern is not formed on the opposing substrate. The liquid crystal display element of this structure can simplify the manufacturing process and obtain a high transmittance.
[0087] Moreover, in highly functional elements such as TFT type elements, elements such as transistors are formed between electrodes for driving liquid crystal and a substrate.
[0088] In the case of a transmissive liquid crystal display element, the above-mentioned substrates are generally used, but in the case of a reflective liquid crystal display element, an opaque substrate such as a silicon wafer can be used for only one of the substrates. In that case, a light-reflecting material such as aluminum can be used for the electrodes formed on the substrate.
[0089] The liquid crystal material constituting the liquid crystal layer of the liquid crystal display element is not particularly limited, and liquid crystal materials used in conventional vertical alignment methods, for example, negative type liquid crystals such as MLC-6608, MLC-6609, and MLC-3023 manufactured by Merck & Co., Inc., can be used. In addition, in a PSA mode liquid crystal display element, a polymerizable compound represented by the following formula, for example, can be used as the liquid crystal component.
[0090] [ka]
[0091] A method of sandwiching a liquid crystal layer between two substrates can include known methods. For example, a method of preparing a pair of substrates on which a liquid crystal alignment film is formed, dispersing spacers such as beads on the liquid crystal alignment film of one substrate, attaching the other substrate so that the surface on which the liquid crystal alignment film is formed faces inward, and injecting liquid crystal under reduced pressure to seal the substrate can be exemplified. A liquid crystal cell can also be produced by a method of preparing a pair of substrates on which a liquid crystal alignment film is formed, dispersing spacers such as beads on the liquid crystal alignment film of one substrate, dripping liquid crystal thereon, and then attaching the other substrate so that the surface on which the liquid crystal alignment film is formed faces inward to seal the substrate. The thickness of the spacer is preferably 1 to 30 μm, more preferably 2 to 10 μm.
[0092] The process of producing a liquid crystal cell by applying ultraviolet light while applying a voltage to the liquid crystal alignment film and the liquid crystal layer can be, for example, a method in which a voltage is applied between electrodes placed on a substrate to apply an electric field to the liquid crystal alignment film and the liquid crystal layer, and ultraviolet light is irradiated while maintaining this electric field. Here, the voltage applied between the electrodes is, for example, 5 to 30 Vp-p, preferably 5 to 20 Vp-p. The irradiation dose of ultraviolet light is, for example, 1 to 60 J / cm. 2 , preferably 40 J / cm 2 A lower amount of ultraviolet irradiation is preferable because it can suppress a decrease in reliability caused by damage to the members constituting the liquid crystal display element, and it can also improve manufacturing efficiency by reducing the ultraviolet irradiation time.
[0093] As described above, when the liquid crystal alignment film and the liquid crystal layer are irradiated with ultraviolet light while applying a voltage, the polymerizable compound reacts to form a polymer, and the polymer memorizes the tilt direction of the liquid crystal molecules, thereby increasing the response speed of the resulting liquid crystal display element. In addition, when the liquid crystal alignment film and the liquid crystal layer are irradiated with ultraviolet light while applying a voltage, the photoreactive side chains of at least one polymer selected from a polyimide precursor having a side chain that vertically aligns liquid crystals, such as a second diamine compound having a side chain structure represented by the above formulas [S1] to [S3] and the above photoreactive side chain, and a polyimide obtained by imidizing the polyimide precursor, react with each other, or the photoreactive side chain of the polymer reacts with the polymerizable compound contained in the liquid crystal layer, thereby increasing the response speed of the resulting liquid crystal display element.
[0094] Next, polarizing plates are provided. Specifically, it is preferable to attach a pair of polarizing plates to the surfaces of the two substrates opposite to the liquid crystal layer.
[0095] In addition, the liquid crystal alignment film and liquid crystal display element of the present invention are not limited to the above configuration and manufacturing method as long as the liquid crystal alignment agent of the present invention is used, and may be manufactured by other known methods. The process from the liquid crystal alignment agent to obtaining a liquid crystal display element is disclosed, for example, in paragraphs
[0074] on page 17 to
[0082] on page 19 of JP2015-135393A. EXAMPLES
[0096] <Example> The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0097] (Diamine compounds) p-PDA: p-phenylenediamine DA-1 to DA-9: primary diamines (also called specific diamines) represented by the following formulas DA-1 to DA-9, respectively. Note that DA-1 to DA-6, DA-7 and DA-8 are novel compounds. SC-1 to SC-4: Side-chain diamines represented by the following formulae SC-1 to SC-4 [ka]
[0098] [ka]
[0099] (Tetracarboxylic acid component) CBDA: 1,2,3,4-cyclobutanetetracarboxylic dianhydride BODA: Bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride TCA: 2,3,5-tricarboxypentyl acetic dianhydride
[0100] (solvent) NMP: N-methyl-2-pyrrolidone BCS: Butyl cellosolve THF: tetrahydrofuran DMF: N,N-dimethylformamide CH2Cl2: Dichloromethane CHCl3: Chloroform
[0101] < 1 H-NMR Measurement Equipment: Fourier transform superconducting nuclear magnetic resonance (FT-NMR) "AVANCE III" (BRUKER) 500MHz Solvent: deuterated chloroform (CDCl3) or deuterated N,N-dimethylsulfoxide ([D6]-DMSO) Standard substance: Tetramethylsilane (TMS)
[0102] <Synthesis of diamine> (Synthesis Example 1) Synthesis of [DA-1]:
[0103] [ka]
[0104] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (39.4 g, 189 mmol) and NMP (394 g) were charged into a 1 L four-neck flask, bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride (23.4 g, 94 mmol) was added in a water bath, and the mixture was stirred at 60 ° C for 6 hours. Then, pyridine (89.2 g, 1128 mmol) and acetic anhydride (60.5 g, 593 mmol) were charged into the reaction solution, and the mixture was stirred at 110 ° C. After the reaction was completed, the reaction system was poured into pure water (2500 g) and the precipitate was filtered off. Then, the obtained crude product was isolated by silica gel column chromatography (eluent: ethyl acetate) to obtain 40.6 g of [DA-1-1].
[0105] [DA-1-1] (33.8 g, 54 mmol) and CH2Cl2 (510 g) were charged into a 1 L four-neck flask, and trifluoroacetic acid (55.0 g, 539 mmol) was added dropwise in a water bath, followed by stirring at room temperature. After the reaction was completed, the precipitate was filtered off and washed with CH2Cl2 (300 g). Pure water (700 g) was added to the obtained crude product, neutralized with triethylamine (50 g), and the precipitate was filtered off. DMF (50 g) and methanol (500 g) were added to the obtained crude product, and repulp washing was performed at room temperature to obtain 11.9 g of [DA-1] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-1]. 1H NMR (500 MHz, [D6]-DMSO):δ7.30-7.33 (m,4H), 6.52-6.58 (m,4H), 5.26 (s,2H), 5.20 (s,2H), 3.33 (s,2H), 3.26-3.28 (m,2H), 2.95-2.98 (m,2H), 2.44-2.48 (m,2H), 1.90-1.94 (m,1H), 1.67-1.73 (m,1H)
[0106] (Synthesis Example 2) Synthesis of [DA-2]:
[0107] [ka]
[0108] tert-Butyl (3-aminophenyl) carbamate (83.4 g, 400 mmol) and NMP (840 g) were charged into a 2 L four-neck flask, bicyclo [3,3,0] octane-2,4,6,8-tetracarboxylic dianhydride (46.6 g, 186 mmol) was added in a water bath, and the mixture was stirred at 60 ° C for 6 hours. Then, pyridine (178.1 g, 2250 mmol) and acetic anhydride (115.5 g, 1120 mmol) were charged into the reaction solution, and the mixture was stirred at 110 ° C. After the reaction was completed, the reaction system was poured into pure water (5000 g), and the precipitate was filtered off. Then, the obtained crude product was isolated by silica gel column chromatography (eluent: ethyl acetate), and 103.5 g of [DA-2-1] was obtained.
[0109] [DA-2-1] (100.5 g, 160 mmol) and CH2Cl2 (1500 g) obtained above were charged into a 2 L four-neck flask, and trifluoroacetic acid (165.7 g, 1620 mmol) was added dropwise in a water bath, followed by stirring at room temperature. After the reaction was completed, the precipitate was filtered off and washed with CH2Cl2 (600 g). Pure water (2000 g) was added to the obtained crude product, neutralized with triethylamine (100 g), and the precipitate was filtered off. DMF (100 g) and methanol (1000 g) were added to the obtained crude product, and repulp washing was performed at room temperature to obtain 32.3 g of [DA-2] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-2]. 1H NMR (500 MHz, [D6]-DMSO):δ7.01-7.08 (m,2H), 6.54-6.58 (m,2H), 6.24-6.31 (m,4H), 5.24 (s,2H), 5.18 (s,2H), 3.37 (s,2H), 3.28-3.30 (m,2H), 2.96-2.97 (d,2H), 2.47-2.53 (m,2H), 1.95-1.99 (m,1H), 1.75-1.80 (m,1H)
[0110] (Synthesis Example 3) Synthesis of [DA-3]:
[0111] [ka]
[0112] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (20.0 g, 96 mmol) and NMP (200 g) were charged into a 1 L four-neck flask, and 1,2,3,4-butanetetracarboxylic dianhydride (8.6 g, 43 mmol) was added in a water bath, followed by stirring at 40 ° C for 6 hours. Next, pyridine (20.5 g, 259 mmol) and acetic anhydride (13.2 g, 130 mmol) were charged into the reaction solution, followed by stirring at 60 ° C. After the reaction was completed, the reaction system was poured into pure water (1000 g) and the precipitate was filtered off. Next, THF (180 g) and methanol (200 g) were added to the obtained crude product, and the mixture was repulped and washed at room temperature, yielding 14.7 g of [DA-3-1].
[0113] [DA-3-1] (14.7 g, 25 mmol) and CH2Cl2 (400 g) obtained above were charged into a 1 L four-neck flask, and trifluoroacetic acid (43.3 g, 380 mmol) was added dropwise in a water bath, followed by stirring at room temperature. After the reaction was completed, hexane (1000 g) was added to the reaction solution, and the precipitate was filtered. Pure water (400 g) was added to the obtained crude product, neutralized with pyridine (40 g), and the precipitate was filtered. DMF (10 g) was added to the obtained crude product, and after repulp washing, ethyl acetate (50 g) was further added to the crude product, and repulp washing was performed at 60 ° C., thereby obtaining 6.6 g of [DA-3] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-3]. 1H NMR (400 MHz, [D6]-DMSO): δ6.84-7.95 (d,4H), 6.56-6.60 (d,4H), 5.31 (s,4H), 3.52-3.55 (t,2H), 2.94-3.01 (q,2H), 2.65-2.67 (d,1H), 2.61-2.62 (d,1H)
[0114] (Synthesis Example 4) Synthesis of [DA-4]:
[0115] [ka]
[0116] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (33.3 g, 160 mmol) and NMP (330 g) were charged into a 1 L four-neck flask, and bicyclo[2.2.2]octane-2,3:5,6-tetracarboxylic dianhydride (20.0 g, 80 mmol) was added in a water bath, followed by stirring at 60° C. for 6 hours. Next, pyridine (38.0 g, 480 mmol) and acetic anhydride (24.5 g, 240 mmol) were charged into the reaction solution, followed by stirring at 110° C. After completion of the reaction, the reaction system was poured into pure water (1500 g) and the precipitate was filtered off. Next, the obtained crude product was isolated by silica gel column chromatography (eluent: ethyl acetate / hexane = 2 / 1 (volume ratio)), and then ethyl acetate (200 g) was added to the crude product and repulp washed at 50 °C to obtain 29.8 g of [DA-4-1].
[0117] In a 1L four-neck flask, the above-obtained [DA-4-1] (29.8 g, 47 mmol) and CHCl3 (440 g) were charged, and trifluoroacetic acid (53.9 g, 473 mmol) was added dropwise in a water bath, followed by stirring at 50°C. After the reaction was completed, the precipitate was filtered off and washed with CHCl3 (300 g). Pure water (300 g) was added to the obtained crude product, neutralized with triethylamine (20 g), and the precipitate was filtered off. DMF (180 g) and methanol (180 g) were added to the obtained crude product, and the product was repulped and washed at room temperature to obtain 16.9 g of [DA-4] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-4]. 1H NMR (500 MHz, [D6]-DMSO):δ6.86-6.88 (d,4H), 6.60-6.62 (d,4H), 5.35 (s,4H), 3.23 (s,4H), 2.50 (s,2H), 1.40 (s,4H)
[0118] (Synthesis Example 5) Synthesis of [DA-5]:
[0119] [ka]
[0120] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (25.0 g, 120 mmol), pyridine (28.5 g, 360 mmol), and NMP (250 g) were charged into a 1 L four-neck flask, and bicyclo[2.2.2]oct-7-ene-2,3,5,6-tetracarboxylic dianhydride (14.9 g, 60 mmol) was added in a water bath, followed by stirring at 80 ° C. After completion of the reaction, the reaction system was poured into pure water (1500 g) and the precipitate was filtered off. Subsequently, methanol (1500 g) was added to the obtained crude product, and the mixture was repulped and washed at room temperature to obtain 30.6 g of [DA-5-1].
[0121] [DA-5-1] (30.6 g, 49 mmol) and CHCl3 (300 g) were charged into a 1 L four-neck flask, and trifluoroacetic acid (55.5 g, 487 mmol) was added dropwise in a water bath, followed by stirring at 50°C. After the reaction was completed, the precipitate was filtered off and washed with CHCl3 (100 g). Methanol (250 g) was added to the obtained crude product, neutralized with triethylamine (20 g), and the precipitate was filtered off. Methanol (100 g) was added to the obtained crude product, and the product was repulped and washed at room temperature to obtain 20.0 g of [DA-5] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-5]. 1H NMR (500 MHz, [D6]-DMSO):δ6.70-6.74 (d,4H), 6.55-6.58 (d,4H), 6.23-6.24 (q,2H), 5.34 (d,4H), 3.45-3.47 (s,2H), 3.30 (s,4H)
[0122] (Synthesis Example 6) Synthesis of [DA-6]:
[0123] [ka]
[0124] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (25.0 g, 120 mmol) and NMP (250 g) were charged into a 1 L four-neck flask, and 1R,2S,4S,5R-cyclohexanetetracarboxylic anhydride (13.5 g, 60 mmol) was added in a water bath, followed by stirring at 50 ° C for 6 hours. Next, pyridine (28.5 g, 360 mmol) and acetic anhydride (18.5 g, 180 mmol) were charged into the reaction solution, followed by stirring at 50 ° C. After completion of the reaction, the reaction system was poured into pure water (1500 g) and the precipitate was filtered off. Next, methanol (150 g) was added to the obtained crude product, and the mixture was repulped and washed at room temperature, yielding 15.4 g of [DA-6-1].
[0125] The above-obtained [DA-6-1] (15.4 g, 26 mmol) and CHCl3 (154 g) were charged into a 1 L four-neck flask, and trifluoroacetic acid (29.1 g, 255 mmol) was added dropwise in a water bath, followed by stirring at 50°C. After the reaction was completed, the precipitate was filtered off and washed with CHCl3 (50 g). Pure water (200 g) was added to the obtained crude product, neutralized with triethylamine (10 g), and the precipitate was filtered off to obtain 9.9 g of [DA-6] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-6]. 1H NMR (500 MHz, [D6]-DMSO):δ6.86-6.88 (d,4H), 6.59-6.62 (d,4H), 5.33 (s,4H), 3.04-3.06 (t,4H), 2.11 (s,4H)
[0126] (Synthesis Example 7) Synthesis of [DA-7]:
[0127] [ka]
[0128] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (33.3 g, 160 mmol) and NMP (300 g) were charged into a 1 L four-neck flask, and tetrahydro-3,3'-dimethyl[3,3'-bifuran]-2,2',5,5'-tetrone (17.2 g, 76 mmol) was added in a water bath, followed by stirring at 40 ° C for 6 hours. Next, pyridine (36.4 g, 460 mmol) and acetic anhydride (23.5 g, 230 mmol) were charged into the reaction solution, followed by stirring at 60 ° C. After completion of the reaction, the reaction system was poured into pure water (1500 g) and the precipitate was filtered off. Next, the obtained crude product was isolated by silica gel column chromatography (eluent: ethyl acetate / hexane = 1 / 1 (volume ratio)), and then methanol (50 g) was added to the obtained crude product and repulped and washed at room temperature to obtain 4.6 g of [DA-7-1].
[0129] In a 1L four-neck flask, the above-obtained [DA-7-1] (4.6 g, 8 mmol) and CHCl3 (50 g) were charged, and trifluoroacetic acid (17.2 g, 152 mmol) was added dropwise in a water bath, followed by stirring at 50°C. After the reaction was completed, hexane (150 g) was added to the reaction solution, and the precipitate was filtered off. Pure water (30 g) was added to the obtained crude product, triethylamine (2 g) was added for neutralization, and the mixture was poured into ethyl acetate (200 g). The organic layer was washed with pure water (300 g) and concentrated. Hexane (30 g) was added to the obtained crude product, and the product was repulped and washed at room temperature to obtain 2.7 g of [DA-7] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-7]. 1H NMR (500 MHz, [D6]-DMSO):δ6.84-6.86 (d,4H), 6.58-6.59 (d,4H), 5.31 (s,4H), 2.98-3.00 (d,2H), 2.67-2.71 (d,2H), 1.45 (s,6H)
[0130] (Synthesis Example 8) Synthesis of [DA-8]:
[0131] [ka]
[0132] A 2L four-neck flask was charged with 4,4'-(ethane-1,2-diylbis(oxy))dianiline (109.5g, 448mmol) and DMF (850g), and di-tert-butyl dicarbonate (32.8g, 151mmol) was added dropwise in a water bath, followed by stirring at room temperature. After completion of the reaction, the reaction solution was concentrated, and the resulting residue was isolated by silica gel column chromatography (eluent: ethyl acetate / hexane = 1 / 1 (volume ratio)), yielding 45.3g of [DA-8-1].
[0133] [DA-8-1] (44.7 g, 130 mmol) and NMP (450 g) were charged into a 1 L four-neck flask, bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride (23.4 g, 94 mmol) was added in a water bath, and the mixture was stirred at 60 ° C for 6 hours. Then, pyridine (58.1 g, 735 mmol) and acetic anhydride (38.2 g, 374 mmol) were charged into the reaction solution and stirred at 110 ° C. After the reaction was completed, the reaction system was poured into pure water (4000 g) and the precipitate was filtered off. Then, DMF (250 g) was added to the obtained crude product, and the mixture was repulped and washed at 70 ° C. to obtain 36.8 g of [DA-8-2].
[0134] [DA-8-2] (36.8 g, 41 mmol) and CHCl3 (750 g) were charged into a 1 L four-neck flask, and trifluoroacetic acid (46.8 g, 410 mmol) was added dropwise in a water bath, followed by stirring at 50°C. After the reaction was completed, the reaction solution was poured into hexane (750 g) and the precipitate was filtered off. Methanol (1200 g) was added to the obtained crude product, and triethylamine (50 g) was added for neutralization, and the precipitate was filtered off. Next, methanol (1200 g) was added to the obtained crude product, and the product was repulped and washed at room temperature to obtain 26.3 g of [DA-8] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-8]. 1H NMR (500 MHz, [D6]-DMSO):δ7.00-7.11 (m,8H), 6.69-6.71 (d,4H), 6.51-6.53 (d,4H), 4.64 (s,4H), 4.27-4.28 (d,4H), 4.16-4.17 (d,4H), 3.40 (s,2H), 3.34 (s,2H), 3.00-3.01 (d,2H), 2.56-2.59 (d,2H), 1.94-1.97 (d,1H), 1.72-1.75 (d,1H)
[0135] (Synthesis Example 9) Synthesis of [DA-9]:
[0136] [ka]
[0137] N-(tert-butoxycarbonyl)-1,4-phenylenediamine (20.0 g, 96 mmol) and NMP (200 g) were charged into a 1 L four-neck flask, and 3-(carboxymethyl)-1,2,4-cyclopentanetricarboxylic acid 1,4:2,3-dianhydride was added in a water bath, and the mixture was stirred at 60 ° C for 6 hours. Then, pyridine (22.8 g, 288 mmol) and acetic anhydride (14.7 g, 144 mmol) were charged into the reaction solution, and the mixture was stirred at 110 ° C. After the reaction was completed, the reaction system was poured into pure water (1000 g) and the precipitate was filtered off. Then, the obtained crude product was isolated by silica gel column chromatography (eluent: ethyl acetate / hexane = 2 / 1 (volume ratio)), and then methanol (300 g) was added to the crude product and repulp washed at room temperature, obtaining 15.6 g of [DA-9-1].
[0138] [DA-9-1] (15.6 g, 26 mmol) and CH2Cl2 (230 g) were charged into a 1 L four-neck flask, and trifluoroacetic acid (29.3 g, 257 mmol) was added dropwise in a water bath, followed by stirring at room temperature. After the reaction was completed, the precipitate was filtered off and washed with CH2Cl2 (200 g). Pure water (100 g) was added to the obtained crude product, neutralized with pyridine (5 g), and the precipitate was filtered off. DMF (30 g) and methanol (300 g) were added to the obtained crude product, and repulp washing was performed at room temperature to obtain 8.3 g of [DA-9] (white solid). The results of 1H-NMR of the target product are shown below. From these results, it was confirmed that the obtained solid was the target [DA-9]. 1H NMR (500 MHz, [D6]-DMSO):δ6.74-6.77 (m,4H), 6.53-6.56 (d,4H), 5.21-5.22 (d,4H), 3.72-3.75 (d,1H), 3.51 (s,1H), 3.03 (s,2H), 2.91-2.99 (m,1H), 2.75-2.81 (m,1H), 2.38-2.41 (d,1H), 2.14-2.17 (m,1H)
[0139] <Preparation of Liquid Crystal Alignment Agent> (Reference example 1) DA-1 (4.30 g, 10.0 mmol) was dissolved in NMP (17.2 g) and stirred at 40° C. for 30 minutes. Then, CBDA (1.82 g, 9.3 mmol) and NMP (7.3 g) were added and reacted at 40° C. for 12 hours to obtain a polyamic acid solution (A). To this polyamic acid solution (A) (15.0 g), NMP (25.0 g) and BCS (10.0 g) were added, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (A1).
[0140] (Reference example 2~Reference example 9) Liquid crystal aligning agents B1 to I1 were prepared in the same manner as in Reference Example 1, except that the first diamine was changed as shown in Table 1.
[0141] (Comparative Reference Example 1) A liquid crystal alignment agent J1 was prepared in the same manner as in Reference Examples 1 to 9, except that the specific diamine was changed to p-PDA.
[0142] [Table 1]
[0143] <Preparation of liquid crystal cell> (Reference example 10) The liquid crystal alignment agent (A1) obtained in Reference Example 1 was spin-coated on the ITO surface of a 3×4 cm ITO-coated glass substrate, baked on a hot plate at 80° C. for 1 minute and 30 seconds, and then baked in an infrared heating furnace at 230° C. for 20 minutes to prepare a polyimide-coated substrate with a thickness of 100 nm. Two polyimide-coated substrates were prepared by the above method, and 4 μm bead spacers were sprayed on the liquid crystal alignment film surface of one substrate, and then a thermosetting sealant (XN-1500T manufactured by Kyoritsu Chemical Co., Ltd.) was printed on top of the bead spacers. Next, the other substrate was attached to the previous substrate with the side on which the liquid crystal alignment film was formed facing inward, and the sealant was cured to prepare an empty cell. PSA polymerizable compound-containing liquid crystal MLC-3023 (Merck product name) was injected into this empty cell by the reduced pressure injection method to prepare a liquid crystal cell. The voltage retention rate of this liquid crystal cell was measured. Next, with a DC voltage of 15 V applied to the liquid crystal cell, UV was irradiated from the outside of the liquid crystal cell at 10 J / cm through a 325 nm cut filter. 2 The UV illuminance was measured using a UV-MO3A manufactured by ORC. Thereafter, in order to inactivate the unreacted polymerizable compound remaining in the liquid crystal cell, the cell was irradiated with UV (UV lamp: FLR40SUV32 / A-1) for 30 minutes without applying voltage using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology Corp. (referred to as secondary PSA treatment). Then, the voltage retention rate was measured.
[0144] <Evaluation of voltage holding ratio> Using the liquid crystal cell prepared above, a voltage of 1V was applied for 60μs in a hot air circulating oven at 60℃, and the voltage was measured 1667msec later, and the voltage retention rate was calculated to determine how long the voltage was retained. A VHR-1 manufactured by Toyo Corporation was used to measure the voltage retention rate.
[0145] (Reference examples 11~15) The VHR was measured in the same manner as in Reference Example 10, except that the liquid crystal alignment agent (A1) was replaced with the liquid crystal alignment agents (B1), (C1), (E1), (F1), and (I1).
[0146] (Comparative Reference Example 2) The VHR was measured in the same manner as in Reference Example 10, except that the liquid crystal aligning agent (J1) was used instead of the liquid crystal aligning agent (A1).
[0147] The VHR measurement results are shown below. [Table 2]
[0148] As shown in Table 2, in Comparative Reference Example 2, the VHR was very low at 20% or less from the beginning, whereas in Reference Examples 10 to 15, the VHR was good at 60% or more even after the second PSA treatment. This result shows that the liquid crystal alignment agent incorporating a specific diamine can ensure higher driving reliability than the liquid crystal alignment agent not incorporating a specific diamine.
[0149] Example 1 DA-1 (2.15 g, 5.0 mmol) and SC-1 (1.90 g, 5.0 mmol) were dissolved in NMP (16.2 g) and stirred at 40° C. for 30 minutes. Then, CBDA (1.82 g, 9.3 mmol) and NMP (7.3 g) were added and reacted at 40° C. for 12 hours to obtain a polyamic acid solution (K). To this polyamic acid solution (K) (15.0 g), NMP (20.0 g) and BCS (15.0 g) were added, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (K1).
[0150] (Examples 2 to 9) Except for changing the specific diamine (first diamine) and the side chain diamine (second diamine) as shown in Table 3, liquid crystal alignment agents L1 to S1 were prepared in the same manner as in Example 1.
[0151] Example 10 DA-1 (3.23 g, 7.5 mmol) and SC-4 (1.90 g, 2.5 mmol) were dissolved in NMP (20.5 g) and stirred at 40°C for 30 minutes. Then, TCA (2.20 g, 9.8 mmol) and NMP (8.8 g) were added and reacted at 60°C for 10 hours to obtain a polyamic acid solution (T). To this polyamic acid solution (T) (15.0 g), NMP (20.0 g) and BCS (15.0 g) were added, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (T1).
[0152] Example 11 DA-5 (2.83 g, 7.0 mmol) and SC-2 (1.30 g, 3.0 mmol) were dissolved in NMP (16.5 g) and stirred at 40° C. for 30 minutes, after which BODA (1.88 g, 7.5 mmol) and NMP (7.5 g) were added and reacted for 5 hours at 60° C. Then, CBDA (0.45 g, 2.3 mmol) and NMP (1.8 g) were added and reacted for 12 hours at 40° C. to obtain a polyamic acid solution (U). To this polyamic acid solution (U) (15.0 g), NMP (20.0 g) and BCS (15.0 g) were added, and the mixture was stirred at room temperature for 5 hours to obtain a liquid crystal aligning agent (U1).
[0153] (Examples 12 and 13) Liquid crystal alignment agents V1 and W1 were prepared in the same manner as in Example 11, except that the specific diamine, side chain diamine, and tetracarboxylic acid components were changed as shown in Table 3.
[0154] [Table 3]
[0155] <Preparation of samples for evaluating seal adhesion> The liquid crystal alignment agent (K1) obtained in Example 1 was filtered through a filter with a pore size of 1.0 μm, spin-coated on a glass substrate with a transparent electrode, dried on a hot plate at 80° C. for 2 minutes, and then baked at 230° C. for 20 minutes to obtain a coating film with a thickness of 100 nm. Two substrates thus obtained were prepared, and 4 μm diameter bead spacers were sprayed on the liquid crystal alignment film surface of one substrate, and then a sealant (XN-1500T manufactured by Kyoritsu Chemical Co., Ltd.) was dropped. Next, the liquid crystal alignment film surface of the other substrate was placed inside, and the substrates were laminated so that the overlap width was 1 cm. At that time, the amount of the sealant dropped was adjusted so that the diameter of the sealant after lamination was about 3 mm. The two laminated substrates were fixed with clips, and then thermally cured at 120° C. for 1 hour to prepare a sample for adhesiveness evaluation.
[0156] <Seal Adhesion Measurement> The prepared sample was fixed at the edges of the top and bottom substrates using a Shimadzu Corporation bench-top precision universal testing machine AGS-X500N, and the pressure (N) was measured when peeling the substrates. The pressure (N) was normalized by the measured diameter of the sealant to evaluate the adhesive strength.
[0157] <Preparation of rework characteristic evaluation sample> (Test Example 1) The liquid crystal alignment agent (K1) obtained in Example 1 was filtered through a filter having a pore size of 1.0 μm, and then spin-coated onto a 3 cm × 4 cm glass substrate with an ITO electrode. The substrate was dried on a hot plate at 80°C for 2 minutes, and then baked at 230°C for 30 minutes to obtain a substrate with a liquid crystal alignment film having a thickness of 100 nm.
[0158] <Evaluation of rework characteristics> The substrate with the liquid crystal alignment film was immersed in a 50 mL beaker containing 15 g of NMP for 30 seconds. At this time, it was confirmed that part of the applied liquid crystal alignment film was immersed in NMP. After 30 seconds, the NMP attached to the substrate was washed away with pure water, and it was visually confirmed whether the liquid crystal alignment film remained in the part immersed in NMP. The case where the liquid crystal alignment film in the part immersed in NMP was completely gone was defined as good reworkability, and the case where the liquid crystal alignment film remained or partially remained was defined as poor reworkability.
[0159] (Test Examples 2 to 13) Except for changing the liquid crystal aligning agent (K1) to the liquid crystal aligning agents of Examples 2 to 13, the same operation as in Test Example 1 was carried out to evaluate the seal adhesion and rework property.
[0160] (Comparative Test Examples 1-10) The same operations as in Example 1 were carried out except that the liquid crystal aligning agent (K1) was changed to the liquid crystal aligning agents of Reference Examples 1 to 9 and Comparative Reference Example 1, and the seal adhesion and rework properties were evaluated.
[0161] (Test example results) The results of the seal adhesion and rework properties are shown below.
[0162] [Table 4]
[0163] In comparison with Comparative Test Examples 1 to 10, which were tested using a liquid crystal alignment agent using only a specific diamine, Test Examples 1 to 13, which were tested using the liquid crystal alignment agents of Examples 1 to 13 in which a side chain diamine was introduced together with the specific diamine, showed excellent rework properties.
Claims
1. A liquid crystal aligning agent comprising at least one first diamine represented by the following formula [I] and at least one second diamine having a side chain structure represented by the following formula [S1], wherein the side chain structure represented by the formula [S1] is at least one selected from the group consisting of the following formulas [S1-x1] to [S1-x7], and a polymer obtained from a diamine component, the side chain structure being at least one selected from the group consisting of the following formulas [S1-x1] to [S1-x7]. [Formula 1] (In formula [I], Z 1 is selected from the following formulas [Z-1] to [Z-9]. * represents a bond. [Case 2] [C3] (In formula [S1], X 1 and X 2 each independently represents a single bond, -(CH 2 ) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -COO-, -OCO- or -((CH 2 ) a1 -A 1 ) m1 - (a1 is an integer from 1 to 15, A 1 represents an oxygen atom or -COO-; m 1 is an integer from 1 to 2. 1 When is 2, a plurality of a1 and A 1 Each of the groups independently has the same definition as above. 1 and G 2 each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms or a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with at least one selected from the group consisting of an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 6. R 1represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms; R 1 Any hydrogen atom forming the formula (I) may be substituted with a fluorine atom. [C4] (In formulas [S1-x1] to [S1-x7], R 1 represents an alkyl group having 1 to 20 carbon atoms. p is -(CH 2 ) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -CH 2 O-, -CH 2 OCO-, -O-(CH 2 ) m represents -O- (where m is an integer of 1 to 6), -COO- or -OCO-. 1 is an oxygen atom or -COO-* (wherein the bond marked with "*" is (CH 2 ) a2 A represents a bond with 2 is an oxygen atom or *-COO- (where the bond marked with "*" is (CH 2 ) a2 a3 is an integer of 0 or 1, and a1 and a2 are each independently an integer of 2 to 10. Cy represents a 1,4-cyclohexylene group or a 1,4-phenylene group.
2. 2. The liquid crystal aligning agent according to claim 1, wherein the polymer is at least one polymer selected from the group consisting of a polyimide precursor which is a polycondensation product of the diamine component and a tetracarboxylic dianhydride, and a polyimide which is an imidization product thereof.
3. The liquid crystal aligning agent according to claim 1 or 2, wherein the diamine component contains at least one diamine selected from the group consisting of diamines represented by the following formulas [1] and [2]: [C5] In formula [1], Y represents a monovalent group selected from the side chain structures represented by formula [S1]. In formula [2], X represents a single bond, —O—, —C(CH 3 ) 2 -, -NH-, -CO-, -(CH 2 ) m -, -SO 2 -, -O-(CH 2 ) m -O-, -OC(CH 3 ) 2 --, --CO-(CH 2 ) m -, -NH-(CH 2 ) m -, -SO 2 - (CH 2 ) m -, -CONH-(CH 2 ) m -, -CONH-(CH 2 ) m -NHCO-, -COO-(CH 2 ) m -OCO-, -CONH-, -NH-(CH 2 ) m -NH- or -SO 2 - (CH 2 ) m -SO 2 -; m is an integer of 1 to 8; and two Y's each independently represent a monovalent group selected from the side chain structure represented by formula [S1].
4. A liquid crystal alignment film obtained from the liquid crystal aligning agent according to any one of claims 1 to 3.
5. A liquid crystal display device comprising the liquid crystal alignment film according to claim 4.
6. A diamine represented by the following formula [II]: [C6] (In formula [II], Z 2 is selected from the following formulas [Z-1], [Z-3], [Z-4], [Z-6] and [Z-7]. * represents a bond. [C7]
7. 7. The diamine of claim 6, represented by the formula: [C8]
Citation Information
Patent Citations
Imide ring-containing diamine and its production
JP1994016629A
Imide group-containing polyamic acid and its production as well as liquid crystal orienting agent
JP1997185064A
Highly transparent poly(amic acid-imide) copolymer and positive-type photosensitive resin composition containing the same, and cured film of the composition
JP2005336243A
Liquid crystal display device
JP2013167782A
Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal element, and manufacturing method of the same
JP2017049576A