Method of dismantling the object and method of recycling the parts

By applying a high voltage pulse to a conductive material to generate a shock wave, the method addresses the inefficiencies of existing disassembly methods, enabling selective and local dismantling with reduced energy and time, suitable for objects with or without conductive members.

JP7572667B2Active Publication Date: 2024-10-24WASEDA UNIV +1
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020081408
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-01
Publication Date
2024-10-24
Estimated Expiration
2040-05-01

AI Technical Summary

Technical Problem

Existing methods for dismantling objects, such as communication terminals and home appliances, face challenges in selectively and locally disassembling specific parts without conductive members, require excessive energy, and are inefficient in terms of time and energy consumption.

Method used

A method involving a conductive material, such as a thin wire, is brought into contact with the object's surface, and a high voltage pulse is applied to generate a shock wave, allowing for selective and local disassembly by separating object members.

Benefits of technology

The method enables efficient, selective, and local dismantling of specific parts with reduced energy use and time, preserving the functionality of non-contacted members for easy recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572667000001
    Figure 0007572667000001
  • Figure 0007572667000002
    Figure 0007572667000002
  • Figure 0007572667000003
    Figure 0007572667000003
Patent Text Reader

Abstract

To provide an object dismantling method which enables a specific site of an object to be selectively and locally dismantled without reference to whether or not the object is a conductive member, which requires only a small amount of energy for dismantlement and which enables the dismantlement to be executed in a short period of time, and a member regeneration method.SOLUTION: In an object dismantling method, a conductive member is brought into contact with one part of a surface of an object in which at least two members are joined together; shock waves are generated by applying a high voltage pulse to the conductive member in the atmosphere; and the members of the object are separated from each other by making the shock waves act on a junction of the object.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for dismantling an object and a method for recycling components. [Background technology]

[0002] Communication terminal devices and home appliances that are no longer in use due to breakdowns or changes in their product life cycles are collected by businesses and then disassembled and recycled or reused. Traditionally, this type of work has often involved disassembly by hand, followed by physical disassembly using a crusher. However, this type of work requires a lot of manpower, and there have been problems with recycling and reusing the disassembled parts.

[0003] Under these circumstances, various methods for decomposing an object by generating a pulsed power discharge in a liquid have been proposed in recent years (for example, Patent Documents 1 to 5). In particular, claim 12 and examples of Patent Document 5 disclose a method for recovering materials from a liquid crystal panel having electrodes (transparent electrodes) on the inner surfaces of a pair of substrates, in which a current is passed through the electrodes (transparent electrodes) while the liquid crystal panel is immersed in a liquid, thereby separating the pair of substrates into individual substrates. Furthermore, Patent Document 6 discloses a method for dismantling a plasma display device having a metal plate-attached panel in which a metal plate is adhered to the non-display surface of the plasma display panel via an adhesive, in which the plasma display panel and the metal plate are separated by inductively heating the metal plate-attached panel. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Special Publication No. 2012-517892 [Patent Document 2] Japanese Patent Application Publication No. 9-75769 [Patent Document 3] Special Publication No. 2018-506429 [Patent Document 4] JP 2017-104796 A [Patent Document 5] JP 2002-254059 A [Patent Document 6] JP 2004-111092 A Summary of the Invention [Problem to be solved by the invention]

[0005] However, the inventions described in the above Patent Documents 1 to 4 all involve dismantling in a liquid medium such as water, and do not involve dismantling in the atmosphere. Therefore, all of them involve high randomness in the discharge path, making it difficult to selectively and locally dismantle a specific portion of an object having a certain size.

[0006] Furthermore, if the number of high-voltage pulses is increased in order to dismantle the desired parts of the object, the entire object may be dismantled or may be crushed into smaller pieces than necessary. This causes the problem of a large amount of energy required for dismantling as unnecessary parts are dismantled into smaller pieces.

[0007] The method disclosed in claim 12 and the examples of Patent Document 5 is able to separate the two glass substrates of the liquid crystal panel, which is the object to be disassembled, because the two glass substrates have transparent electrodes on their inner surfaces, but it cannot be applied to objects that do not have conductive members (electrodes) on their inner surfaces.

[0008] The invention described in Patent Document 6 requires induction heating of a panel with a metal plate, and cannot be applied to an object that does not have a conductive member (metal plate).

[0009] In light of the above-mentioned circumstances, the present invention aims to provide a method for dismantling objects, which is capable of selectively and locally dismantling specific parts of an object regardless of whether the object has conductive components, which requires a small amount of energy for dismantling, and which can complete the dismantling in a short time, and a method for recycling components. [Means for solving the problem]

[0010] The present invention includes the following aspects.

[0011] [1] A conductive material is brought into contact with a portion of the surface of an object having at least two members joined together; A method for dismantling an object, comprising applying a high-voltage pulse to the conductive material in the atmosphere to generate shock waves, and applying the shock waves to joints of the object to peel apart components of the object. [2] The method for dismantling an object described in [1] above, wherein the conductive material is a thin wire. [3] The method for dismantling an object according to [2] above, wherein the fine wire has a diameter of 0.01 to 4 mm. [4] The method for dismantling the object described in [2] or [3] above, wherein the thin wire contains copper. [5] The method for dismantling an object described in any one of [1] to [4], wherein when a high-voltage pulse is applied to the conductive material, the capacitance is 10 to 10,000 μF, the applied voltage is 2 to 100 kV, and the number of applications is 1 to 10 or less. [6] A method for regenerating components, comprising recovering and reusing peeled components using the method for dismantling an object according to any one of [1] to [5] above. Effect of the Invention

[0012] According to the present invention, it is possible to provide a method for dismantling an object, which is capable of selectively and locally dismantling specific parts of an object regardless of whether the object has conductive components, which requires a small amount of energy for dismantling, and which can complete the dismantling in a short time, and a method for recycling components. [Brief description of the drawings]

[0013] [Figure 1] 1 is a schematic diagram showing a method for dismantling an object according to a first embodiment of the present invention, in which (a1), (a2) and (a4) are cross-sectional views, and (a3) ​​is a top view. [Diagram 2] 11 is a schematic cross-sectional view showing a state in which a conductive material 3 is brought into contact with a surface of component 1A, of surfaces of object 2 having components 1A to 1D, in a method for dismantling an object according to a second embodiment of the present invention. FIG. [Diagram 3] This is a photograph showing the appearance of a glass door panel 16 removed from a small refrigerator with a thin copper wire 17 in contact with the front glass plate. [Figure 4] This is an external photograph showing how the glass door panel 16 shown in FIG. 3 is dismantled by shock waves as a result of the wire explosion. [Diagram 5] This is a photograph showing the appearance of a glass door panel removed from a small refrigerator, with a thin aluminum wire placed at the boundary between the glass plate and the plastic casing at one end of the glass door panel and in contact with the surface of the glass door panel. [Figure 6] This is an external photograph showing how a portion of the glass door panel shown in Figure 5 near the wire was disintegrated by the shock waves as a result of the wire explosion. [Figure 7] This is a photograph showing the appearance of a glass door panel, part of which was dismantled by shock waves as shown in Figure 6, with thin aluminum wires placed at the boundary between the glass plate and the plastic casing on the other end opposite the arrangement of thin wires in Figure 5, with the thin wires in contact with the surface of the glass door panel. [Figure 8] This is an external photograph showing how, as a result of the wire explosion, the plastic casing of the glass door panel shown in Figure 7 was broken by the shock wave, causing separation between the glass plate and the plastic casing, resulting in the dismantling of the glass door panel as the target object. [Figure 9] This is a photograph showing the appearance of a ceramic-coated sample object being disintegrated by shock waves as a result of a wire explosion. [Figure 10] This is an external photograph showing how the ceramic-coated sample object was disintegrated by the shock waves as a result of the second wire explosion. [Figure 11]This is a photograph showing the appearance of a ceramic-coated sample object being disintegrated by shock waves as a result of a wire explosion. [Figure 12] 1 is a front view photograph of the exterior of the object of Reference Example 1 before dismantling. [Figure 13] 1 is a photograph showing the object of Reference Example 1 after dismantling. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] <<How to dismantle the object>> The method of dismantling an object of the present invention involves bringing a conductive material into contact with a portion of the surface of an object formed by joining at least two components, applying a high-voltage pulse to the conductive material in the atmosphere to generate shock waves, and applying the shock waves to the joined portion of the object to peel the components of the object apart.

[0015] A conductive material is brought into contact with a portion of the surface of an object, and a high-voltage pulse is applied to the conductive material in the atmosphere, causing the conductive material to turn into plasma and generate shock waves. The shock waves propagate through the components and act on the joints of the object, peeling the components of the object apart and dismantling the object. The method for dismantling an object of the present invention involves contacting a conductive material with a portion of the surface of the object and applying a high-voltage pulse to the conductive material in the atmosphere to generate shock waves, making it possible to selectively and locally dismantle specific portions of the object. Since the conductive material serves as the source of the shock waves, the amount of energy required for dismantling is small, and dismantling can be completed in a short time.

[0016] A detailed description will be given below of an embodiment of a method for dismantling an object to which the present invention is applied. Note that the drawings used in the following description may show characteristic parts in an enlarged scale for the sake of convenience in order to make the characteristics easier to understand, and the dimensional ratios of each component may not necessarily be the same as in reality. The present invention is not limited to the embodiment shown below.

[0017] [First embodiment] Fig. 1 is a schematic diagram showing a method for dismantling an object according to a first embodiment of the present invention, in which (a1), (a2) and (a4) are cross-sectional views, and (a3) ​​is a top view.

[0018] (Object) In this embodiment, the object 2 is a ceramic coating sample. The member 1A is a ceramic film as an insulator, and the member 1B is an iron plate. The object 2 is an iron plate with a ceramic film bonded to the entire surface of the iron plate ((a1) in FIG. 1).

[0019] The combination of the member 1A and the member 1B is not limited to the combination of the ceramic film and the iron plate, but may be a combination of an insulator and an insulator, a combination of an insulator and a conductive member, or a combination of a conductive member and a conductive member. It is preferable that the object has at least one insulating member.

[0020] The insulating member 1A is preferably in the form of a plate, membrane or film. Examples of the insulating member 1A include a ceramic membrane, a plastic plate, a glass plate, and the like.

[0021] The thickness of the member 1A is preferably 50,000 μm or less, more preferably 10,000 μm or less, and even more preferably 5,000 μm or less, since it is close to the joining point of the objects to be peeled off. The thickness of the member 1A is preferably 2 μm or more, may be 10 μm or more, or may be 50 μm or more. The thickness of the member 1A is preferably 2 to 50,000 μm, more preferably 10 to 10,000 μm, and even more preferably 50 to 5,000 μm.

[0022] (Conductive materials) In this embodiment, the conductive material 3 is a thin wire made of metal. The metal type of the thin wire as the conductive material 3 is not limited as long as it can generate a shock wave by the explosion of the thin wire. Examples of the metal type of the thin wire include copper, aluminum, silver, and tungsten. The thin wire preferably contains copper or aluminum, and more preferably contains copper. The thin wire preferably has a small electrical resistance (easy to flow a large current), a low melting point and boiling point, a small specific heat, and a small specific gravity (easy to generate Joule heat). The conductive material 3 is not limited to a thin metal wire, as long as it can generate a shock wave capable of peeling apart the components of an object by applying a high voltage pulse. In addition to a thin metal wire, examples of the conductive material 3 include a conductive paste and a metal foil. Examples of the conductive paste include a silver paste and a carbon paste, and examples of the metal foil include an aluminum foil and a copper foil.

[0023] (Step of contacting conductive material) In FIG. 1, first, a thin metallic wire is brought into contact with the center along the longitudinal direction of the surface on the ceramic film side of the ceramic coating sample ((a1)⇒(a2) in FIG. 1). In this embodiment, the thin wire is brought into contact so as to traverse from one side of the surface of the ceramic film to the opposite side ((a2) in FIG. 1). The position at which the thin wire is brought into contact may be selected according to the positions of the target components to be peeled off, but a position that includes at least the insulator portion of the target is preferred. In this embodiment, it is preferable to bring a conductive material into contact with the surface on the insulator member 1A side. In a method for dismantling an object including one insulating member and another insulating member, since the shock wave attenuates as the travel distance increases, it is preferable to contact the conductive material at a position close to the joint of the object to be peeled off, and it is more preferable to contact the conductive material with a portion of the surface of the thinner insulating member of the one insulating member and the other insulating member.

[0024] The length of the thin wire may be longer or shorter than the longitudinal length of the member with which the thin wire comes into contact. When the target object includes an insulating member and a conductive member, the length of the thin wire is preferably shorter than the longitudinal length of the insulating member with which the thin wire comes into contact. This reduces the risk of the thin wire passing electricity through the conductive member and damaging the conductive member that is to remain functional after the target object is disassembled.

[0025] When the conductive material is brought into contact with the surface of the object, the length of the conductive material in the longitudinal direction is preferably 0.4 times or more, more preferably 0.5 times or more, and even more preferably 0.6 times or more, relative to the length of the member on the side where the conductive material is brought into contact, from the viewpoint of efficiency. The length of the conductive material in the longitudinal direction is preferably 1.0 times or less, more preferably 0.9 times or less, and even more preferably 0.8 times or less, relative to the length of the member on the side where the conductive material is brought into contact. The length of the conductive material in the longitudinal direction is preferably 0.4 to 1.0 times, more preferably 0.5 to 0.9 times, and even more preferably 0.6 to 0.8 times, relative to the length of the member on the side where the conductive material is brought into contact.

[0026] The length over which the conductive material is in contact with the surface of the object may be 10 to 2000 mm, 20 to 1000 mm, or 40 to 500 mm.

[0027] When the conductive material is a thin wire, the diameter of the thin wire may be 0.01 to 4 mm, 0.2 to 2 mm, or 0.4 to 1 mm. There is no limitation on the number of thin wires to be brought into contact with at least a part of the surface of the object, and the number may be 1, 1 to 2, or 1 to 3, and may be increased or decreased as appropriate according to the material and size of the object to be disassembled.

[0028] In this embodiment, electrodes 9, 10 connected to the high-voltage pulse application device 6 via electric wires 7, 8 are then abutted against both ends of the thin wire (FIG. 1 (a3)). The thin wire is longer than the distance from one side of the surface near the center of the ceramic film to the opposite side. The electrodes 9, 10 are alligator clips. The alligator clips are clamped to the portions of both ends of the thin wire that protrude from the ceramic film. The method of connection to the high-voltage pulse application device 6 is not limited to this.

[0029] The high-voltage pulse application device 6 can instantly discharge the electric charge stored in a large-capacity capacitor. The high-voltage pulse application device can be appropriately selected from known devices. The suitable output conditions of the high-voltage pulse application device 6 can be appropriately selected depending on the thickness of the member on the side that contacts the conductive material, the area of ​​the bonded portion of the object to be peeled off, the bond strength, etc.

[0030] For example, the capacitance of the high-voltage pulse application device 6 is preferably 10 μF or more, more preferably 20 μF or more, and even more preferably 30 μF or more. The capacitance of the high-voltage pulse application device 6 is preferably 10,000 μF or less, more preferably 1,000 μF or less, and even more preferably 100 μF or less. The capacitance of the high-voltage pulse application device 6 is preferably 10 to 10,000 μF, more preferably 20 to 1,000 μF, and even more preferably 30 to 100 μF.

[0031] (Removal process of bonded objects) Next, a high voltage pulse is applied to the thin metal wire, which is the conductive material 3, to turn the metal into plasma and generate shock waves, which are then applied to the joint between the members 1A and 1B of the object ((a4) in FIG. 1), thereby peeling the members 1A and 1B of the object apart. The thin metal wire, which is the conductive material 3, is turned into plasma and explodes, and the shock waves propagate through the member 1A. The shock waves are transmitted to the joint between the members 1A and 1B of the object, and the acoustic impedance (density x speed of sound) of the two materials, 1A and 1B, is different, so stress is generated at the interface between the members 1A and 1B, and the members are peeled apart. At this time, the thin metal wire, which is the conductive material 3, is turned into plasma and changes into fine particles, and the member 1A on the side that contacts the conductive material may also be fragmented or broken into fine particles. By adjusting the output of the high-voltage pulse application device 6 so that the iron plate of the component 1B on the side that does not come into contact with the conductive material can maintain the functionality of the component 1B, it is possible to prevent the component 1B on the side that does not come into contact with the conductive material from being destroyed.

[0032] It is preferable that the materials to be peeled have a large difference in acoustic impedance (density x speed of sound), which is affected by many physical properties such as the material composition, microstructure, particle or fiber orientation, porosity, and temperature.

[0033] It is more efficient if the propagation direction of the shock wave is the same as the desired peeling direction. In (a2) of Fig. 1, the joint surface of the parts 1A and 1B to be peeled is approximately parallel to the surface of the object with the conductive material in contact. In (a4) of Fig. 1, the propagation direction of the shock wave is from the conductive material 3 to the part 1A to the part 1B, which is the same as the peeling direction between the parts 1A and 1B (the up-down direction in (a4) of Fig. 1).

[0034] The voltage applied from the high-voltage pulse application device 6 is not limited as long as it is a condition that can sufficiently perform peeling between the members of the object, but is preferably 2 kV or more, more preferably 5 kV or more, and even more preferably 10 kV or more. The voltage applied from the high-voltage pulse application device 6 is preferably 100 kV or less, more preferably 50 kV or less, and even more preferably 20 kV or less. The voltage applied from the high-voltage pulse application device 6 is preferably 2 to 100 kV, more preferably 5 to 50 kV, and even more preferably 10 to 20 kV.

[0035] In the object dismantling method of this embodiment, the number of applications by high-voltage pulse application device 6 is preferably 1 or more and 10 or less, more preferably 5 or less, and even more preferably 3 or less.

[0036] The method for dismantling an object of this embodiment involves contacting a portion of the surface of the object with a conductive material and applying a high-voltage pulse to the conductive material in the atmosphere to generate shock waves. This makes it possible to selectively and locally dismantle specific portions of an object regardless of whether the object has a conductive member or not, reduces the number of times the application of voltage is applied, reduces the amount of energy required for dismantling, and enables dismantling to be completed in a short time.

[0037] In addition, the member on the side not in contact with the conductive material can be left with its shape substantially intact.

[0038] In the method for dismantling an object according to the present embodiment, the object can be dismantled into a shape or material that is easy to recycle by selecting conditions such as the position where the conductive material is brought into contact, the capacitance when applying a high voltage pulse to the conductive material, the applied voltage, the number of times of application, etc. An example of a shape or material that is easy to recycle is a powder with a diameter of several mm, or separation into a specific ceramic and a specific metal.

[0039] [Second embodiment] FIG. 2 is a schematic cross-sectional view showing a state in which a conductive material 3 is brought into contact with the surface of component 1A, among the surfaces of object 2 having components 1A to 1D, in a method for dismantling an object according to a second embodiment of the present invention.

[0040] In this embodiment, the target object 2 is a glass door panel of a refrigerator. Member 1A is a glass plate acting as an insulator, member 1B is silver decorative paper, member 1C is urethane resin, and member 1D is a resin housing. Member 1A is joined to member 1B, and member 1B is joined to member 1D. Members 1B and 1C are not joined to each other. In this embodiment, the conductive material 3 is a thin copper wire.

[0041] In the second embodiment, the method for dismantling an object involves bringing a thin wire of conductive material 3 into contact with the surface of the center portion along the longitudinal direction of the glass plate of member 1A, applying a high voltage pulse to the thin wire of conductive material 3 to turn the copper wire into plasma and generate shock waves, and peeling off the silver decorative paper of member 1B and the plastic casing of member 1D of object 2. In the second embodiment, the copper thin wire of conductive material 3 is turned into plasma and turns into fine particles, and the glass plate of member 1A and the silver decorative paper of member 1B turn into fragments. The polyurethane resin of member 1C and the plastic casing of member 1D can be left in almost their original form.

[0042] In the second embodiment of the method for dismantling an object, as in the first embodiment, a conductive material is brought into contact with a portion of the surface of the object and a high-voltage pulse is applied to the conductive material in the atmosphere to generate shock waves, making it possible to selectively and locally dismantle specific parts of the object, reducing the number of times the pulse is applied, reducing the amount of energy required for dismantling, and completing the dismantling in a short time.

[0043] In the method for dismantling an object according to the present embodiment, the object can be dismantled into a shape or material that is easy to recycle by selecting conditions such as the position where the conductive material is brought into contact, the capacitance when applying a high voltage pulse to the conductive material, the applied voltage, the number of times of application, etc. An example of a shape or material that is easy to recycle is a powder with a diameter of several mm, or separation into a specific glass and a specific resin.

[0044] [Other embodiments] In the method for dismantling an object of the present invention, the surface of the object with which the conductive material is brought into contact can be appropriately selected depending on the joint portion of the object to be peeled off. In FIG. 1, a conductive material 3 may be in contact with a side surface of the member 1A and a side surface of the member 1B so as to traverse the members 1A and 1B. In FIG. 1, the conductive material 3 may be disposed at the boundary between the member 1A and the member 1B so that the conductive material 3 contacts the side surface of the member 1A and the side surface of the member 1B. In FIG. 2, the conductive material 3 may be in contact with the side surface of the member 1A, the side surface of the member 1B, and the side surface of the member 1D so as to traverse the members 1A, 1B, and 1D. In FIG. 2, the conductive material 3 may be disposed at the boundary between the member 1A and the member 1B so that the conductive material 3 contacts the side surface of the member 1A and the side surface of the member 1B.

[0045] <<How to recycle materials>> The method for recycling components of the present invention involves recovering and reusing peeled components using the method for dismantling an object described above. The method for dismantling an object of the present invention is capable of selectively and locally dismantling a specific portion of an object and dismantling the object into a shape or material that is easy to recycle, so that the peeled members can be recovered and reused using the method for dismantling an object. The recovered members can be used as they are or can be reused after being processed. EXAMPLES

[0046] The present invention will be described in more detail below with reference to specific examples, although the present invention is not limited to the following examples.

[0047] [Example 1] In recent years, high-end refrigerators have adopted glass door panels 16. Figure 3 is a photograph showing the appearance of the glass door panel 16 removed from a commercially available small refrigerator, with a thin copper wire 17 in contact with the front glass plate. The thin copper wire 17 is in contact with the surface of the central portion along the longitudinal direction of the glass plate. In the glass door panel 16 (i.e., the object 2), similarly to the embodiment shown in FIG. 2, thin wires 17 corresponding to the conductive material 3 are in contact with the surface of the central portion along the longitudinal direction of the glass plate of the member 1A. In FIG. 2, the member 1B is a silver decorative paper, the member 1C is a urethane resin, and the member 1D is a resin housing. The glass plate of the member 1A is joined to the silver decorative paper of the member 1B, and the silver decorative paper of the member 1B is joined to the resin housing of the member 1D. The inside of the resin housing of the member 1D is filled with urethane resin 1C as a heat insulating material. In addition, the mating surfaces of the silver decorative paper of the member 1B and the resin housing 1D are firmly joined by an adhesive sheet, ensuring high heat insulating performance.

[0048] The dimensions of the glass door panel 16 are 250 mm x 170 mm x 85 mm. The copper wire is 260 mm long and 0.9 mm in diameter. Dismantling the glass door panel 16, which is firmly joined in this way, is difficult using the conventional dismantling technique of laser cutting, and the dismantling method has not yet been determined.

[0049] A high-voltage pulse was applied to the electrodes attached to both ends of the wire, with a capacitor capacity of 40 μF and an applied voltage of 15 kV, causing the wire to explode.

[0050] Fig. 4 is an external photograph showing the state in which the glass door panel 16 shown in Fig. 3 was dismantled by shock waves as a result of the wire explosion. The shock waves generated by the wire explosion near the arrangement of the wires caused the glass plate and silver decorative paper to peel off from the resin housing, enabling dismantling. In Example 1, the glass door panel was selectively and locally dismantled with one application, leaving behind the urethane resin and the resin housing.

[0051] [Example 2] 5 is a photograph showing the appearance of a glass door panel removed from a commercially available small refrigerator, with a thin aluminum wire placed at the boundary between the glass plate and the resin casing at one end of the glass door panel and in contact with the surface of the glass door panel, in the method for dismantling an object according to Example 2. The dimensions of glass door panel 16 of this small refrigerator are 240 mm×150 mm×85 mm, and the internal structure is similar to that of glass door panel 16 of Example 1. The thin aluminum wire is 260 mm long and has a wire diameter of 0.9 mm.

[0052] A high-voltage pulse was applied to the electrodes attached to both ends of the wire, with a capacitor capacity of 40 μF and an applied voltage of 15 kV, causing the wire to explode.

[0053] Figure 6 is a photograph showing the appearance of a portion of the glass door panel shown in Figure 5 near the wire, which was disintegrated by the shock waves as a result of the wire explosion.

[0054] Figure 7 is a photograph showing the appearance of a glass door panel, part of which was dismantled by shock waves as shown in Figure 6, with a thin aluminum wire placed at the boundary between the glass plate and the resin housing on the other end opposite the arrangement of the thin wires in Figure 5, and the thin wire brought into contact with the surface of the glass door panel. The thin aluminum wire is 260 mm long and has a wire diameter of 0.9 mm.

[0055] A high-voltage pulse was applied to the electrodes attached to both ends of the wire, with a capacitor capacity of 40 μF and an applied voltage of 15 kV, causing the wire to explode.

[0056] Fig. 8 is an external photograph showing how the resin casing of the glass door panel shown in Fig. 7 is broken by the shock wave as a result of the wire explosion, the glass plate and the resin casing are peeled off, and the glass door panel as the target is dismantled. In Example 2, the glass door panel was selectively and locally dismantled with most of the urethane resin remaining after two applications of the voltage.

[0057] [Example 3] An attempt was made to dismantle a sample object, an iron plate with one side ceramic-coated. The dimensions of the iron plate were 100 mm x 100 mm x 5 mm, and the ceramic coating was 100 μm thick. A thin copper wire, 120 mm long and 0.9 mm in diameter, was brought into contact with the center of the ceramic-coated side of the sample object. A high-voltage pulse was applied from electrodes abutting both ends of the wire, with a capacitor capacity of 40 μF and an applied voltage of 15 kV. This resulted in an explosion of the wire.

[0058] Figure 9 is a photograph showing the appearance of the ceramic-coated sample object being dismantled by the shock waves as a result of the wire explosion. The ceramic coating in a 20 mm wide area, including the wire placement area, peeled off from the iron plate, and the iron plate side was left intact, allowing for selective and localized dismantling.

[0059] [Example 4] A copper thin wire having a length of 120 mm and a wire diameter of 0.9 mm was contacted with the ceramic-coated sample object similar to that of Example 3 except that the thickness of the ceramic coating film in Example 3 was changed to 500 μm. A high-voltage pulse was applied from electrodes in contact with both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a thin wire explosion occurred. However, peeling of the ceramic coating film was not confirmed. Furthermore, a copper thin wire having a length of 70 mm and a wire diameter of 0.9 mm was contacted with the ceramic-coated sample object near the center of the ceramic coating side. A high-voltage pulse was applied from electrodes in contact with both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a second thin wire explosion occurred.

[0060] Figure 10 is a photograph showing the appearance of the ceramic-coated sample object being dismantled by the shock waves as a result of the second wire explosion. The length of the wire was shortened. As a result, about half of the ceramic coating film peeled off from the iron plate, and the iron plate side was left intact, allowing for selective and localized dismantling.

[0061] [Example 5] A copper thin wire having a length of 70 mm and a wire diameter of 0.9 mm was brought into contact with the center of the ceramic coating side of the sample object, which was the same as in Example 4 and had a ceramic coating film thickness of 500 μm. A high-voltage pulse was applied from electrodes abutting both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a thin wire explosion occurred. However, peeling of the ceramic coating film was not confirmed. Furthermore, a copper thin wire having a length of 70 mm and a wire diameter of 0.9 mm was brought into contact with the center of the ceramic coating side of the sample object. A high-voltage pulse was applied from electrodes abutting both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a second thin wire explosion occurred.

[0062] As a result of the second wire explosion, similar to Example 4, about half of the ceramic coating film peeled off from the iron plate, and the iron plate side was left intact, allowing for selective and localized dismantling.

[0063] [Example 6] A copper thin wire having a length of 70 mm and a wire diameter of 0.9 mm was contacted with the ceramic-coated sample object similar to that of Example 3 except that the thickness of the ceramic coating film was changed to 300 μm. A high-voltage pulse was applied from electrodes in contact with both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a thin wire explosion occurred. However, peeling of the ceramic coating film was not confirmed. Furthermore, a copper thin wire having a length of 70 mm and a wire diameter of 0.9 mm was contacted with the ceramic-coated sample object similar to that of Example 3. A high-voltage pulse was applied from electrodes in contact with both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a second thin wire explosion occurred.

[0064] As a result of the second wire explosion, a 30 mm wide section of the ceramic coating, including the wire placement, peeled off from the steel plate, allowing the steel plate side to be left intact and dismantled selectively and locally.

[0065] [Example 7] For the same sample object with a ceramic coating film thickness of 100 μm as in Example 3, a copper thin wire with a length of 70 mm and a wire diameter of 0.9 mm was brought into contact with the vicinity of the center of the ceramic coating side of the sample object. A high voltage pulse was applied from electrodes abutting both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a thin wire explosion occurred. However, peeling of the ceramic coating film was not confirmed. Furthermore, a copper thin wire with a length of 70 mm and a wire diameter of 0.9 mm was brought into contact with the vicinity of the center of the ceramic coating side of the sample object. A high voltage pulse was applied from electrodes abutting both ends of the thin wire under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, a second thin wire explosion occurred.

[0066] As a result of the second wire explosion, a 30 mm-wide area of ​​the ceramic coating film, including the wire placement, peeled off from the steel plate, allowing the steel plate side to be left intact and dismantled selectively and locally.

[0067] [Example 8] For the same sample object with a ceramic coating film thickness of 500 μm as in Example 4, two copper thin wires, each 70 mm long and 0.9 mm in diameter, were arranged in a cross shape near the center of the ceramic coating side of the sample object and brought into contact with each other. A high voltage pulse was applied from electrodes abutting both ends of one of these thin wires under the conditions of a capacitor capacity of 40 μF and an applied voltage of 15 kV. As a result, the first thin wire explosion occurred.

[0068] Figure 11 is a photograph showing the appearance of the ceramic-coated sample object being dismantled by the shock waves as a result of the first wire explosion. In the first wire explosion, about 94% of the ceramic coating film surface area was peeled off from the iron plate, and the iron plate side was left intact, allowing for selective and localized dismantling.

[0069] [Reference example 1] 12 is a front view photograph of the exterior of glass door panel 16 (subject) removed from a commercially available small refrigerator, showing the subject of Reference Example 1 before dismantling. The dimensions of the glass door panel of this small refrigerator are 250 mm × 170 mm × 85 mm, and the internal structure is similar to that of glass door panel 16 of Example 1.

[0070] A pair of electrodes was placed 70 mm apart on the surface of the glass plate of the glass door panel 16, and a high voltage pulse was applied from the pair of electrodes under the conditions of a capacitor capacity of 0.8 μF and an applied voltage of 45 kV. As a result, the glass plate was broken at a local portion including the portion where the pair of electrodes were in contact, and peeled off from the resin housing together with the silver decorative paper. In addition, a pair of electrodes was placed 70 mm apart on another portion of the surface of the glass plate of the glass door panel 16, and a high voltage pulse was applied from the pair of electrodes under the same conditions. As a result, the glass plate broke a second time. Furthermore, a high voltage pulse was applied 13 times in the same manner, causing a 15th breakage.

[0071] FIG. 13 is a photograph showing the state of the glass door panel 16 shown in FIG. 12 after the 15th breaking attempt.

[0072] In Examples 1 to 8, the object could be dismantled by applying the high voltage pulse 1 to 3 times, whereas in Reference Example 1, the object could be dismantled only after applying the high voltage pulse 15 times. [Industrial Applicability]

[0073] The method for dismantling an object of the present invention can be used to dismantle objects such as home appliances and mobile communication terminals that are no longer in use due to a breakdown or a change in the product life cycle. Furthermore, the peeled members can be recovered and reused by using the method for dismantling an object of the present invention. [Explanation of symbols]

[0074] 1A...Component A 1B...Part B 1C...Part C 1D...Component D 2. Object 3. Conductive materials 6 High voltage pulse application device 7,8...Electric wire 9,10...electrode 16. Glass door panel 17...Thin line

Claims

1. An object is formed by joining at least two members, and includes one insulating member and another insulating member. The object includes one insulating member and another insulating member, and a conductive material is brought into contact with a part of a surface of the thinner insulating member of the first insulating member and the other insulating member, or a conductive material is brought into contact with a part of a surface of the ceramic-coated side of a ceramic-coated iron plate; a method for dismantling an object, comprising applying a high voltage pulse to the conductive material in the atmosphere to generate shock waves, and applying the shock waves to joints of the object to separate components of the object, A method for dismantling an object, in which when a high-voltage pulse is applied to the conductive material, the capacitance is 10 to 10,000 μF, the applied voltage is 2 to 100 kV, and the number of applications is 1 to 10 times or less (however, this does not include a method for dismantling a solar panel, which is characterized by abutting a plurality of electrodes at spaced positions on a conductor on a cell sheet that constitutes a solar panel, applying a voltage between the plurality of electrodes, and selectively extracting useful substances from the cell sheet by an electric pulse).

2. The method for dismantling an object according to claim 1 , wherein the conductive material is a thin wire.

3. The method for dismantling an object according to claim 2, wherein the fine wire has a diameter of 0.01 to 4 mm.

4. The method for dismantling an object according to claim 2 or 3, wherein the thin wire contains copper.

5. A method for regenerating components, comprising recovering and reusing peeled components using the method for dismantling an object according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Method for fragmenting and pulverizing solid coagulated fromnonmetallic component or partially from metal component

    JP1997075769A

  • Method and apparatus for separation of junction body

    JP2000037622A

  • Material recovery method from liquid crystal display panel

    JP2002254059A

  • Method for disassembling plasma display device

    JP2004111092A

  • Method and system for reusing materials and / or products using pulsed power.

    JP2012517892A