Magnesium peroxide-containing composition, oxygen supply agent and method for producing said composition
A stabilized magnesium peroxide composition is produced by controlling impurities and water content, and incorporating carbonation, addressing the challenges of conventional methods to achieve high oxygen concentration and stability for use as an oxygen supply agent.
Patent Information
- Application Number
- JP2020059769
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-03-30
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-03-30
AI Technical Summary
Conventional magnesium peroxide production methods face challenges in achieving high effective oxygen concentration and stability, with issues such as poor filterability, difficulty in granulation, and higher manufacturing costs, while maintaining a stable product.
A composition containing magnesium peroxide with controlled impurities, water content, and carbonate levels, produced through a method involving the reaction of magnesium hydroxide or oxide with hydrogen peroxide and subsequent carbonation, utilizing a chelating agent to stabilize the reaction.
The method results in a magnesium peroxide composition with high effective oxygen concentration and stability, suitable for use as an oxygen supply agent, enhancing its performance and efficiency.
Smart Images

Figure 0007572790000027 
Figure 0007572790000028 
Figure 0007572790000029
Abstract
Description
[Technical field]
[0001] The present invention relates to a composition containing magnesium peroxide, an oxygen supplying agent, and a method for producing the composition. [Background technology]
[0002] Magnesium peroxide (MgO 2 ) has the property of releasing oxygen by reacting with water and hydrolyzing, and therefore has been applied and developed as an oxygen supplying agent in a wide range of fields, such as agricultural applications, soil purification, and water quality improvement (Patent Documents 1 to 4, etc.). MgO 2 In agricultural applications, calcium peroxide (CaO 2 ) is known to be superior.
[0003] Magnesium peroxide (MgO 2 ) is magnesium oxide (MgO) or magnesium hydroxide (Mg(OH) 2 ) and hydrogen peroxide (H 2 O 2 ) in a large amount of water. To date, there have been several production methods, such as a method of stabilizing the reaction by reacting with carbon dioxide, carbonic acid or a water-soluble salt thereof in the reaction (Patent Document 6), and a method of reducing the impurity CaO, such as Mg(OH) 2 A manufacturing method using raw materials (Patent Document 7), MgO 2 There are known production methods, such as a granulation method in which the water content in the granules is adjusted to improve efficiency (Patent Document 8).
[0004] However, conventional MgO 2 The manufacturing method of this product produces high-purity MgO that exhibits a high effective oxygen concentration, which is important for oxygen supply performance. 2 and obtaining MgO 2 It has been difficult to obtain a highly stable product that suppresses the decomposition of calcium peroxide. In addition, there are many problems in the synthesis of calcium peroxide, such as poor filterability, difficulty in granulation, and higher production costs than calcium peroxide. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] Special Publication No. 2017-516465 [Patent Document 2] JP 2017-222566 A [Patent Document 3] JP 2018-955 A [Patent Document 4] JP 2012-229352 A [Patent Document 5] Japanese Patent Application Laid-Open No. 61-166304 [Patent Document 6] Japanese Patent Application Publication No. 61-286206 [Patent Document 7] JP 2004-107127 A [Patent Document 8] JP 2016-16995 A Summary of the Invention [Problem to be solved by the invention]
[0006] An object of the present invention is to provide a magnesium peroxide-containing composition having a high effective oxygen concentration and stability, an oxygen supplying agent, and a method for producing the composition. [Means for solving the problem]
[0007] The present invention was achieved through studies aimed at solving the above problems, and has the following gist.
[0008] 1. A composition containing magnesium peroxide represented by the following general formula (1): In the composition The concentration of impurities containing a complex formed of a chelating agent and a metal is 5% by mass or less, The moisture content is 3 to 12% by mass, A composition having a carbonate concentration of 2 to 20 mass %.
[0009] [ka]
[0010] [In formula (1), X p represents a complex consisting of a chelating agent and a metal, Z represents a carbonate, a represents a value between 0.1 and 1, b represents a value between 0 and 0.1, and c represents a value between 0 and 0.9.
[0011] 2. X in the general formula (1) p but, A composition which is a complex consisting of an organophosphorus compound and a metal.
[0012] 3. A composition wherein the organophosphorus compound is etidronic acid, pyrophosphate or orthophosphate.
[0013] 4. X in the general formula (1) p but, A composition which is a complex containing Ca, Mn, Fe, Cu or Al.
[0014] 5. An oxygen supply containing the above composition.
[0015] 6. A method for producing magnesium peroxide granules containing the composition.
[0016] 7. A method for producing a composition containing magnesium peroxide represented by the following general formula (2), comprising carrying out steps 1 and 2:
[0017] [ka]
[0018] [In formula (2), X p represents a complex consisting of a chelating agent and a metal, Z represents a carbonate, a represents a value between 0.1 and 1, b represents a value between 0 and 0.1, and c represents a value between 0 and 0.9.
[0019] Step 1: A hydroxide or oxide of magnesium; A composition comprising a chelating agent; React with hydrogen peroxide to obtain peroxide.
[0020] Step 2: The peroxide obtained in step 1 is treated with To contain carbon dioxide or carbonate.
[0021] 8. A manufacturing method characterized by carrying out step 1 or step 2 continuously. Effect of the Invention
[0022] The magnesium peroxide-containing composition of the present invention is useful as an oxygen supplying agent because it has a high effective oxygen concentration and is highly stable. Furthermore, the production method of the present invention makes it possible to efficiently or continuously produce a magnesium peroxide-containing composition that has a high effective oxygen concentration and is highly stable. [Brief description of the drawings]
[0023] [Figure 1] 1A to 1C are diagrams illustrating an example of a process of a manufacturing method according to the present invention. [Diagram 2] FIG. 4 is a graph showing the relationship between reaction time and residual hydrogen peroxide concentration in Examples 4 to 7 of the present invention. [Diagram 3] FIG. 2 is a graph showing the relationship between reaction time and available oxygen of a composition containing magnesium peroxide in Examples 4 to 7 of the present invention. [Figure 4] FIG. 2 is a graph showing the results of a stability test at 40° C. of the magnesium peroxide-containing compositions of Examples 8 to 11 of the present invention and Comparative Examples 5 and 6. [Diagram 5] FIG. 2 is a graph showing the relationship between the reaction temperature and the available oxygen of the magnesium peroxide-containing composition in Examples 12 to 15 of the present invention. [Figure 6] FIG. 1 is a graph showing the relationship between the concentration of hydrogen peroxide added and the available oxygen of the magnesium peroxide-containing composition in Examples 16 to 18 of the present invention. [Figure 7]FIG. 2 is a graph showing the relationship between the addition (dropping) time of an aqueous hydrogen peroxide solution and the available oxygen of a magnesium peroxide-containing composition in Examples 16, 19, and 20 of the present invention. [Figure 8] FIG. 13 is a graph showing the relationship between the amount of hydrogen peroxide added and the available oxygen of the magnesium peroxide-containing composition in Example 21 of the present invention. [Figure 9] FIG. 1 is a graph showing the relationship between the change in hydrogen peroxide concentration during the reaction in Example 21 of the present invention and the change in available oxygen of the magnesium peroxide-containing composition. [Figure 10] FIG. 31 is a diagram showing an example of a continuous production system according to Example 31 of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0024] DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described in detail below with reference to the preferred embodiments. Note that the present invention is not limited to the following embodiments, and can be embodied in various forms within the scope of the present invention.
[0025] The "composition containing magnesium peroxide" of the present invention is made of magnesium peroxide (MgO 2 ) into the product (product, product), MgO 2 (hereinafter referred to as "MgO 2 (These are sometimes abbreviated as "MgO-containing composition"). 2 is a magnesium peroxide, and is mainly converted into magnesium hydroxide (Mg(OH) 2 ) and hydrogen peroxide (H 2 O 2 ) is reacted with MgO 2 is hydrolyzed to MgO 2 One oxygen atom can be released per mole. Therefore, MgO 2 The theoretical available oxygen (concentration (mass%)) per unit mass is 16.0 / 56.3=28.4 mass% based on the molecular weight ratio.
[0026] [ka]
[0027] The "composition containing magnesium peroxide" of the present invention is a composition containing the magnesium peroxide, "an impurity containing a complex of a chelating agent and a metal", water, a carbonate, and other components. Therefore, the "composition containing magnesium peroxide" of the present invention is represented by the following general formula (1).
[0028] [ka]
[0029] [In formula (1), X p represents a complex consisting of a chelating agent and a metal, Z represents a carbonate, a represents a value between 0.1 and 1, b represents a value between 0 and 0.1, and c represents a value between 0 and 0.9.
[0030] The magnesium peroxide (MgO 2 The composition containing MgO is characterized in that magnesium (Mg) or other metal atoms contained in the composition are incorporated as impurities in the form of a complex consisting of a chelating agent and a metal atom, as described above. 2 The present invention is characterized in that the carbon dioxide gas contains a carbonate salt therein, and thus it is possible to obtain a high effective oxygen concentration and high stability.
[0031] The "chelating agent" in the "complex of a chelating agent and a metal" of the present invention refers to a compound (ligand) capable of forming a complex (chelate complex) by coordinate bonding with a metal ion at multiple coordination sites. Specifically, 1-Hydroxyethylidene-1,1-diphosphonic acid (etidronic acid, HEDP), Pyrophosphate (diphosphate), orthophosphate, Nitrilotri(methylphosphonic acid) (NTMP), 2-Phosphonobutane-1,2,4-tricarboxylic acid (PBTC), Ethylenediaminetetramethylenephosphonic acid (EDTMP), 1,1-Bis(diphenylphosphino)methane (DPPM), 1,2-Bis(diphenylphosphino)ethane (DPPE), 1,3-Bis(diphenylphosphino)propane (DPPP), 1,1'-Bis(diphenylphosphino)ferrocene (DPPF), 2,2'-Bis(diphenylphosphino)-1,1'-binaphthyl (BINAP), 4,5'-Bis(diphenylphosphino)-9,9'-dimethylxanthene (Xantphos), other diphosphines, 1,1,1-tris(diphenylphosphinomethyl)ethane, triphosphines such as bis(2-diphenylphosphinoethyl)phenylphosphine; Organophosphorus compounds such as; Glycine, ethylenediaminetetraacetic acid (EDTA), trans-1,2-cyclohexanediaminetetraacetic acid (CyDTA), Nitrilotriacetic acid (NTA), Diethylenetriaminepentaacetic acid (DTPA), N-(2-hydroxyethyl)ethylenediaminetriacetic acid (HEDTA), Triethylenetetramine-N,N,N',N'',N''',N'''-hexaacetic acid (TTHA), 1,3-propanediamine-N,N,N',N'-tetraacetic acid (PDTA), 1,3-Diamino-2-hydroxypropane-N,N,N',N'-tetraacetic acid (DPTA-OH), N-(2-hydroxyethyl)iminodiacetic acid (HIDA), N,N-di(2-hydroxyethyl)glycine (DHEG), Glycol ether diamine tetraacetic acid (GEDTA), N,N-dicarboxymethylglutamic acid tetrasodium salt (GLDA), Aminocarboxylic acids such as ethylenediamine-N,N'-disuccinic acid (EDDS); Alkylene diamines such as ethylene diamine, 2-methyl-1,3-propane diamine, etc.; Trishydroxymethylaminomethane; Bipyridine, phenanthroline; Oxalic acid, citric acid, gluconic acid; porphyrins, crown ethers and other cyclic compounds; and the like.
[0032] The chelating agent is magnesium peroxide (MgO 2 In the process of preparing a composition containing MgO, it can form complexes with various metal ions, including magnesium. 2 The metals other than Mg contained in the raw material are not included in the target MgO 2 Therefore, magnesium peroxide (MgO 2 In the composition containing the chelating agent, the amount of metals other than Mg is preferably small, and the concentration of impurities containing complexes of the chelating agent and metals other than Mg is preferably low, specifically, 5 mass % or less.
[0033] The "impurities" in the "impurities containing a complex of a chelating agent and a metal" in the composition of the present invention include "complexes of a chelating agent and a metal" (X p ), impurities containing metal atoms or metal ions that do not form chelate complexes, and also atoms, ions, and molecules other than metals (excluding water). These impurities are 2 Other impurities are contained in water, chelating agents, carbonates, or these raw materials.
[0034] The raw material for magnesium peroxide is magnesium hydroxide (Mg(OH) 2 ) or magnesium oxide (MgO), and as shown in the above formula (3), magnesium hydroxide is preferred. A specific example of an impurity in the "impurity containing a complex consisting of a chelating agent and a metal" of the present invention is an impurity in a raw material containing magnesium hydroxide. In the present invention, the raw material for magnesium hydroxide is not particularly limited, and may be seawater (brine) or minerals containing Mg, such as hydrotalcite and magnesite, and commercially available magnesium hydroxide can be used. These Mg(OH) 2Examples of metal impurities contained in include transition metals, alkali metals, alkaline earth metals, other metals, such as iron (Fe), manganese (Mn), chromium (Cr), calcium (Ca), aluminum (Al), lithium (Li), sodium (Na), potassium (K), nickel (Ni), and silicon (Si), as well as ions, oxides, and other compounds containing these metals.
[0035] As impurities other than metals in the "impurities containing a complex of a chelating agent and a metal" of the present invention, metal oxides or SiO 2 These include oxygen, chloride ions, sulfate ions, other water-soluble or water-insoluble components, other organic compounds, and organometallic compounds.
[0036] The "composition containing magnesium peroxide" of the present invention contains water, and the water content is expressed as the mass ratio of water to the entire composition, i.e., the water content (mass%). The water indicated by the "water content" in the composition containing magnesium peroxide of the present invention may be water that forms a suspension (slurry) by suspending the raw material magnesium hydroxide, etc., and may be water that is contained in the "H 2 MgO 2 It refers to the moisture that may be contained in the composition obtained after the drying step after production. In the present invention, the moisture content in the "composition containing magnesium peroxide" is 3 to 12 mass %.
[0037] The "composition containing magnesium peroxide" of the present invention is a composition in which magnesium peroxide is dissolved in carbon dioxide (CO 2 ), Carbonic acid (H 2 CO 3 ) or its salts to form a partially carbonated 3 By subjecting the composition to the treatment of magnesium peroxide (zinc peroxide), deterioration in quality, such as deterioration over time, can be prevented. Thus, the "composition containing magnesium peroxide" may contain a carbonate (Z) in addition to the main component magnesium peroxide for stabilization.
[0038] The "carbonate" in the "composition containing magnesium peroxide" of the present invention, or the "carbonate" represented by "Z" in the general formula (1), is MgCO 3 may be the main component, MgCO 3 , Mg(OH) 2 , water, magnesium bicarbonate (Mg), magnesium oxide (MgO), or a carbonate with a metal (Cu, Fe, Mn, Na, etc.) contained in the magnesium peroxide raw material, specifically MnCO 3 , FeCO 3 The composition may be a mixture of other components. In addition, the agent (stabilizer) added during the carbonation process may be sodium bicarbonate (NaHCO 3 ), ammonium bicarbonate (NH 4 NaHCO 3 ), ammonium carbonate ((NH 4 ) 2 CO 3 ), magnesium peroxide (Mg(CO 3 )) carbonates or other Li, Na, K, H, NH 4 The concentration of these carbonates contained in the "composition containing magnesium peroxide" is 3 - This corresponds to 2 to 20% by mass.
[0039] As described above, the "magnesium peroxide" or "composition containing magnesium peroxide" of the present invention is represented by the above general formula (1), in which MgO 2 , X p The composition ratios of Mg or MgO in the raw material are represented by a, b, and c, each of which is independently 0 to 1. a is preferably 0.1 to 1, more preferably 0.65 to 1, and even more preferably 0.80 to 1. b is preferably 0 to 0.1, and more preferably 0 to 0.01. c is preferably 0 to 0.9, more preferably 0 to 0.7, and even more preferably 0 to 0.5. The preferred values of a, b, and c depend on the Mg or MgO content in the raw material. 2It is based on the maximum value when impurities other than the components corresponding to a are not purified and removed during the manufacturing process. Therefore, a is preferably larger than the above-mentioned preferable range of a, and b is preferably smaller than the above-mentioned preferable range of b. Note that water is not included in the above-mentioned general formula (1). When a=1, b is preferably 0 to 0.003, and c is preferably 0 to 0.3.
[0040] The "complex of a chelating agent and a metal" in the general formula (1) (X p ) is preferably an "organophosphorus compound and a metal complex." In addition, the "organophosphorus compound" in the "organophosphorus compound and a metal complex" is preferably etidronic acid, pyrophosphoric acid, or orthophosphoric acid.
[0041] The "complex of a chelating agent and a metal" in the general formula (1) (X p ) is preferably a complex containing Ca, Mn, Fe, Cu or Al.
[0042] A method for producing a "composition containing magnesium peroxide" represented by the following general formula (2) will be specifically described below. The production method of the present invention is a method for producing a composition containing magnesium peroxide, which includes carrying out the following steps 1 and 2. Each symbol in the following general formula (2) has the same meaning as in the above general formula (1).
[0043] [ka]
[0044] [In formula (2), X p represents a complex consisting of a chelating agent and a metal, Z represents a carbonate, a represents a value between 0.1 and 1, b represents a value between 0 and 0.1, and c represents a value between 0 and 0.9.
[0045] Step 1: A hydroxide or oxide of magnesium; A composition comprising a chelating agent; React with hydrogen peroxide to obtain peroxide.
[0046] Step 2: The peroxide obtained in step 1 is treated with To contain carbon dioxide or carbonate.
[0047] The method for producing a composition containing magnesium peroxide of the present invention is a method that is composed of the above-mentioned composition and steps, and is a method that can efficiently produce magnesium peroxide that has a high effective oxygen concentration and high stability.
[0048] First, the details of step 1 will be described. In step 1, the "hydroxide or oxide of magnesium" is specifically magnesium hydroxide (Mg(OH) 2 It refers to a raw material containing magnesium peroxide (MgO) or magnesium oxide (MgO) as a main component. In particular, the raw material magnesium hydroxide is not particularly limited, and may be seawater (brine) or minerals containing Mg, such as hydrotalcite or magnesite, as shown in the "composition containing magnesium peroxide" represented by the general formula (1), and commercially available magnesium hydroxide may be used. More specifically, one having a magnesium oxide content of 60 mass% or more (actual measured value or standard value) may be used, but is not particularly limited.
[0049] In step 1, the Mg(OH) 2 As components other than the "hydroxide or oxide of magnesium" such as those described above in the "composition containing magnesium peroxide", metals such as Ca, Fe, Al, Si, etc. or their metal oxides may be contained. As components other than metals, metal oxides or SiO 2 These include oxygen, chloride ions, sulfate ions, other water-soluble or water-insoluble components, other organic compounds, and organometallic compounds. On the other hand, magnesium oxide can be hydrated with water by a known method to produce Mg(OH). 2 can be obtained and can be used as a similar raw material. 2Before carrying out step 1, the raw material containing Mg(OH) is mixed with an appropriate amount of water, stirred, filtered or dehydrated, and then extracted with Mg(OH) 2 A washing step may be carried out to remove water-soluble impurities other than magnesium and foreign matter containing other metals. By removing metals other than magnesium by such washing, the decomposition of hydrogen peroxide is suppressed, and the effect of increasing the available oxygen in the composition containing magnesium peroxide can be obtained.
[0050] The particle size of the powder of "magnesium hydroxide or oxide" in step 1 may be 80 μm or less, and may be 30 μm or less, or may be 10 μm or less, as long as the median of the particle size distribution is 80 μm or less. The bulk density of the powder is not particularly limited, and may be, for example, 0.5 to 0.9 g / mL. The specific surface area of the powder is not particularly limited, and may be 40 to 60 μm.
[0051] The "chelating agent" in the "composition containing a chelating agent" in step 1 may be the same as those exemplified in the general formula (1). The chelating agent is preferably an organic phosphorus compound, and the organic phosphorus compound is more preferably etidronic acid, pyrophosphoric acid, or orthophosphoric acid. The "chelating agent" of the present invention may be diluted with a solvent such as water, or may represent a solution containing a solvent such as water for dilution. The "composition containing a chelating agent" is preferably an aqueous solution containing a chelating agent. When the chelating agent is diluted, it may be at any concentration, and may be diluted at a concentration of 20 to 80% by mass.
[0052] The water used in the manufacturing method of the "composition containing magnesium peroxide" of the present invention is not particularly limited, and may be ordinary water, such as tap water, industrial water, deionized water (ion-exchanged water), distilled water, etc. As long as it does not interfere with the advantageous effects of the present invention, water with a low metal ion concentration is preferred from the viewpoint of washing the composition after production with water.
[0053] Known devices can be used as the device for producing the composition containing magnesium peroxide of the present invention. The container is not limited as long as it can uniformly mix and stir raw materials such as magnesium hydroxide or oxide (powder or slurry), composition or aqueous solution containing a chelating agent, hydrogen peroxide or aqueous hydrogen peroxide solution, or water. The material of the reaction container can be any of glass containers, metal containers such as stainless steel, and resin containers, but it is preferable to use one that is acid-resistant and base-resistant, and is preferably heat-resistant for heating and drying. The size of the container is preferably 1.5 to 3 times the total volume of all samples such as liquids and powders for sufficient stirring.
[0054] In the following, magnesium-containing raw materials are referred to as magnesium hydroxide (Mg(OH) 2 A specific example of step 1 using Mg(OH) will be described. In step 1, first, Mg(OH) 2 It is preferable to prepare a mixture or suspension (slurry) by mixing magnesium with water. The concentration of magnesium in the slurry is Mg(OH) 2 In this case, the content may be 30% by mass or more, specifically, 35 to 50% by mass. Alternatively, a commercially available product already prepared as a slurry may be used and appropriately diluted. Next, Mg(OH) 2 A composition containing a chelating agent, for example, an aqueous solution of a chelating agent, is added to the container containing the Mg(OH) / water mixture and mixed. 2 In order to mix uniformly with water, it is preferable to dissolve the chelating agent in advance in the form of an aqueous solution. A commercially available aqueous solution or other solution can be used as the chelating agent.
[0055] The mixing ratio of the "hydroxide or oxide of magnesium" and the "composition containing a chelating agent" in step 1 is, for example, Mg(OH) 2 The amount of the chelating agent is preferably 0.05 to 1.2 mass%, more preferably 0.1 to 1.0 mass%, and even more preferably 0.1 to 0.5 mass% relative to the total amount of Mg(OH) 2, H 2 O 2 In this case, it is preferably 1 mass % or less of the total charged amount, more preferably 0.5 mass % or less, and further preferably 0.2 mass % or less.
[0056] In step 1, for example as described above, Mg(OH) 2 After the chelating agent and water are mixed in the appropriate ratio, the reaction vessel is stirred and heated or cooled to an appropriate temperature, preferably to keep the temperature constant, taking into consideration changes in room temperature and heat generated by the reaction. Next, hydrogen peroxide (H 2 O 2 ) and react to obtain peroxide. 2 O 2 is preferably an aqueous solution mixed with water at an appropriate concentration. 2 O 2 The concentration may be 10 to 65% by mass, and more preferably 20 to 50% by mass. In step 1, the mixing ratio of "hydroxide or oxide of magnesium" and "hydrogen peroxide" is preferably approximately the same molar ratio as represented by the reaction formula (3) above, or the molar ratio of hydrogen peroxide is equal to or greater than the molar ratio of "hydroxide or oxide of magnesium", and is at most approximately twice as high.
[0057] In step 1, the hydrogen peroxide (H 2 O 2 It is preferable to add H over a certain period of time rather than adding the entire amount in a short period of time. 2 O 2 The larger the amount, the longer the addition time is, or it is preferable to appropriately select a time between 15 minutes and 2 hours, and more preferably between 20 and 60 minutes. Furthermore, in order to avoid a sudden increase in temperature due to the reaction during the addition, it is preferable to adjust the addition speed and minimize the temperature change. A heating device or a cooling device may be used to adjust the temperature. The temperature during the reaction is preferably 30 to 70°C, more preferably 35 to 55°C. Furthermore, H 2 O2 After the entire amount is added, it is preferable to continue stirring for a certain period of time in order to progress the reaction or to mix uniformly. The temperature during stirring may be kept constant or may be gradually cooled. The stirring time may be set to any desired time such as 30 minutes, 1 hour, 2 hours or more. However, H 2 O 2 After the addition, the reaction is complete and magnesium peroxide (MgO 2 Even if the amount of the MgO-containing composition reaches its maximum, if it is left in the aqueous solution after the reaction or if it is filtered and left in a wet state, the MgO 2 The available oxygen concentration of the composition may decrease. Therefore, the reaction may be 2 O 2 While checking the concentration, 2 O 2 After the consumption of the magnesium peroxide, it is preferable to move to the following step 2 after suitable stirring. It is preferable to carry out the operation from step 1 to step 2 continuously without interruption. A peroxide can be obtained by the above step 1, and as a specific example, a mixed liquid containing "a magnesium peroxide-containing composition" as a peroxide and water can be obtained in the reaction liquid.
[0058] In step 2, after the reaction in step 1, the peroxide obtained in step 1 is reacted with carbon dioxide or a carbonate (carbonation) to incorporate the peroxide. Specifically, carbon dioxide (CO 2 ) or a carbonate is added. The carbonate in step 2 is the same as the carbonate represented by (Z) in the general formula (1). 2 A specific example of carbonation by the addition of the following will be described.
[0059] Carbon dioxide (CO 2 The amount of MgO in the obtained magnesium peroxide is 2 Any suitable amount may be added as long as it increases the stabilization of the magnesium peroxide. Specifically, the concentration of carbonate in the target "composition containing magnesium peroxide" is preferably 2% by mass or more, and more preferably 2 to 20% by mass. 2It is more preferable to add
[0060] Carbon dioxide (CO 2 ) or methods for adding carbonate include CO 2 In the case of step 1, CO 2 Alternatively, a gas supply pipe (gas introduction pipe) may be used to send CO to react with the peroxide. 2 The purity of the gas may be any suitable level, for example, 99% or more, or 99.5% or more. The gas supply rate may also be appropriately selected.
[0061] In the above step 2, after a reaction in which carbon dioxide or a carbonate is contained in the peroxide (inside the peroxide), magnesium peroxide (MgO 2 When the MgO-containing composition contains moisture, it can be filtered (or dehydrated) using a known filtering device (pressure type, suction type, etc.) or a device such as a centrifuge. The moisture content after filtration can be adjusted appropriately. Furthermore, after filtration, the wet composition may be spread in a batt-shaped container and air-dried at room temperature, or it can be dried using a warm air dryer such as a shelf dryer. The drying temperature and drying time are not limited as long as they are the temperature and time that can remove moisture, but an appropriate drying time can be selected at a temperature in the range of 40 to 100°C, for example, between 1 and 12 hours. MgO after drying 2 The moisture content of the magnesium-containing composition is preferably 15% by mass or less, and less is preferable for storage, more preferably 12% by mass or less, further preferably 10% by mass or less, and particularly preferably 5% by mass or less. The magnesium-containing composition thus dried may be further pulverized using a known pulverizer, or a sieve or classifier may be used to make the particle size uniform.
[0062] The magnesium peroxide-containing composition of the present invention (MgO 2 An example of a method for producing the compound-containing composition is shown in FIG. 1 as a specific process diagram.
[0063] A method for measuring the amount equivalent to the purity of "magnesium peroxide" in the "composition containing magnesium peroxide" of the present invention is to measure the available oxygen concentration (mass%) (or simply available oxygen (%)), which represents the proportion of the mass of oxygen that the composition can release per unit mass. If the measurement sample is entirely magnesium peroxide, the theoretical available oxygen (%) is 28.4 mass%. A specific example of a method for analyzing the available oxygen in a composition is oxidation-reduction titration (potassium permanganate titration).
[0064] Methods for measuring the moisture content of the composition containing magnesium peroxide of the present invention include infrared or near-infrared absorption methods; the Karl Fischer (KF) method using coulometric titration or volumetric titration; thermal analysis using a thermogravimetry-differential thermal analysis (TG-DTA) device; heat drying methods using a heat drying type moisture meter or the like; gas chromatography (GC) method; nuclear magnetic resonance absorption methods; electrical resistance methods; dielectric constant methods; and distillation methods.
[0065] The composition containing magnesium peroxide of the present invention (MgO 2 The method for producing the composition (containing composition) is as follows: In step 1, by continuously supplying raw materials such as "hydroxide or oxide of magnesium," "composition containing a chelating agent," or "hydrogen peroxide," it is possible to obtain "peroxide" continuously. Specifically, a method is to connect a supply device such as a pipe or a liquid delivery device for continuously supplying these raw materials to a container (reaction tank) in which the raw materials are reacted, and perform step 1 of the reaction continuously. The material of the device and container for this continuous supply is not particularly limited, and known materials can be used. The rate and amount of raw materials supplied and the reaction temperature can be appropriately adjusted. In addition, the container that receives the "peroxide" may be replaced every time a certain amount of the reaction is performed, or this container may be connected to another container, reaction device, storage container, etc.
[0066] In addition, in step 2, by continuously supplying "the peroxide obtained in step 1" and "carbon dioxide or carbonate", the reaction for "adding carbon dioxide or carbonate to the peroxide obtained in step 1" in step 2 can be continuously carried out. Specifically, a device for continuously obtaining "peroxide" in step 1, a gas supply device for carbon dioxide or the like (cylinder and its piping), a stirring device, a liquid delivery device (roller pump, liquid delivery pump, etc.), a heating or cooling device, various containers, etc. can be used. Others used in step 1 can be used in the same way. In addition, "continuously carrying out step 1 or step 2" in the present invention includes carrying out "step 1" and "step 2" separately, alternately, or simultaneously in succession, and specifically, a continuous production system for the purpose of mass synthesis of a product of a composition containing magnesium peroxide can be constructed.
[0067] The composition containing magnesium peroxide of the present invention (MgO 2 As an example of application, the MgO-containing composition of the present invention can be used as an oxygen supplying agent or the like in a wide range of applications such as the above-mentioned agriculture and soil purification. Other components, such as carriers such as solid carriers and liquid carriers, surfactants, and other auxiliary agents, may be appropriately selected and mixed with the composition within a range that does not affect the effect of the intended agent, and the composition can be granulated or the surface can be coated. These components for mixing can be appropriately added during or after the process of the manufacturing method of the present invention. In addition, the MgO of the present invention can be used in a wide range of applications such as agriculture and soil purification such as the above-mentioned agriculture and soil purification. In addition, the MgO of the present invention can be used in a wide range of applications ... in the range that does not affect the effect of the intended agent, other components, such as carriers such as solid carriers and liquid carriers, surfactants, and other auxiliary agents may be appropriately selected and mixed with the composition, and the composition can be granulated or the surface can be coated. These ingredients for mixing can be appropriately added during or after the process of the manufacturing method of the present invention. 2 The composition containing the magnesium peroxide can be granulated to an appropriate particle size using known materials and granulating equipment to produce magnesium peroxide granules. Furthermore, the surface of the particles of the composition can be coated with an appropriate substance. The concentrations of the components of these materials, or the manufacturing conditions such as the temperature during mixing and granulation, can be appropriately adjusted taking into account safety and effectiveness.
[0068] Examples of solid carriers include carbonates such as magnesium carbonate and calcium carbonate; sulfates; peroxides such as calcium peroxide; and natural or synthetic mineral fine powders or granules such as bentonite, kaolin clay, silica clay, pyrophyllite clay, acid clay, talc, diatomaceous earth, zeolite (zeolite), silicon oxide, silicates, and various other salts. These can be used alone or in combination of two or more. The solid carrier may be previously pulverized.
[0069] Examples of liquid carriers include water; hydrocarbons such as aliphatic hydrocarbons, aromatic hydrocarbons, kerosene, and machine oil; alcohols; ketones such as cyclohexanone; esters such as fatty acid methyl esters; vegetable oils such as coconut oil, soybean oil, and rapeseed oil; and organic solvents such as dimethyl sulfoxide and acetonitrile. These can be used alone or in combination of two or more. Considering the impact on the environment, water is preferred as the liquid carrier. The liquid carrier may also be used by mixing it with the above solid carriers.
[0070] Examples of surfactants include anionic surfactants such as dialkyl sulfosuccinate salts, alkylaryl sulfonate salts, and polyoxyethylene alkyl ether phosphate salts; nonionic surfactants such as alkyl glucosides, polyoxyethylene alkyl ethers, polyoxyethylene alkyl phenyl ethers, and sorbitan fatty acid esters; and cationic surfactants such as polyoxyethylene alkyl methyl ammonium salts and alkyl amidoamine salts. These can be used alone or in combination of two or more.
[0071] Other auxiliary agents include, for example, grinding aids, powdering aids, binding aids, lubricants, emulsifiers, thickeners, pH adjusters, coating agent auxiliary agents, defoamers, dissolving aids, or suspension dispersion aids, and specifically, sugars, lignin sulfonates, alginates, and other salts, carboxylates (formates, acetates, glycolates, lactates, butyrates, succinates, malates, tartrates, citrates, and propionates), polyvinyl alcohol, carboxymethylcellulose, stearic acid, gum arabic, organic bentonite, phenylxylylethane, polyethylene glycol, vinyl acetate, petrolatum, and biodegradable plastics (biodegradable polylactic acid, polycaprolactone, polyhydroxyalkanoates, polyglycolic acid, modified polyvinyl alcohol, casein, polyurethane, polyurea, and the like). These can be used alone or in combination of two or more. EXAMPLES
[0072] Hereinafter, the present invention will be described in detail with reference to examples. However, the present invention is not limited to the following examples.
[0073] [Examples 1 and 2] <Analysis of impurities in magnesium hydroxide raw materials> The following two types of magnesium hydroxide (Mg(OH) 2 ) Raw materials were prepared: Example 1 Mg(OH) 2 (Manufactured by Naikai Salt Co., Ltd.) Example 2 Mg(OH) 2 (Kamishima Chemical Co., Ltd., model number: #200) First, these Mg(OH) 2 In order to analyze the impurities contained in the raw materials, ICP emission spectrometry was performed on the product. The results of measuring the powder of the product as is were compared with the results of measuring the metal concentration in the filtrate washed with ion-exchanged water using the following method. In a 500 mL glass flask, 165 g of ion-exchanged water and the above Mg(OH) 2 100 g of Mg(OH) was added, stirred for 10 minutes, washed, and then suction filtered. 2The metal concentration in the filtrate after washing the raw material was measured by ICP atomic emission spectrometry (Agilent Technologies, Inc., device name: Multi-type ICP atomic emission spectrometer (ICP-OES), model: 720-ES). The results are shown in Table 1.
[0074] [Table 1]
[0075] From Table 1, Mg(OH) 2 In the raw material and in the filtrate after washing the raw material, iron (Fe) and manganese (Mn) were detected as metals that decompose hydrogen peroxide. 2 It was confirmed that the impurity concentration in the raw materials differs depending on the product, and further, the amount of metals such as Fe and Mn dissolved in the liquid also differs. In the present invention, these metal impurities are sequestered using a chelating agent to produce a composition containing magnesium peroxide that exhibits a high effective oxygen concentration and is highly stable. With this method, although pretreatment of washing the raw materials with a large amount of water may be performed, this is no longer an essential step, and production costs can be reduced.
[0076] [Example 3] At room temperature (20 to 25°C), 163 g of ion-exchanged water and 0.24 g of a chelating agent (manufactured by Chelesto Corporation, product name: Chelesto PH-210 (60 mass% etidronic acid (HEDP) / solution), molecular weight 206.028 g / mol) were placed in a 500 mL glass reaction vessel with a lid and stirred. The chelating agent (Chelest PH-210) is hereinafter also referred to as the "stabilizing agent". The magnesium hydroxide (Mg(OH) 2 100 g (1.71 mol) of 45% by mass hydrogen peroxide (manufactured by Hodogaya Chemical Co., Ltd.) was added to the suspension and stirred. 2 O 2207 g (2.74 mol) of ethanol (adjusted concentration) was added over 30 minutes and allowed to react (reaction time: 30 minutes). The temperature during the reaction was maintained at 40°C. After the reaction, the mixture was cooled to 20°C while stirring. The stirring conditions were set to be appropriate for uniformly mixing the solution. The amounts of each component charged as above were taken as the total amounts, and are shown in Table 2.
[0077] Mg(OH) 2 If the molar ratio of (a) is 1 and the molar ratio of etidronic acid is (b), then the MgO 2 If the composition contains all of these Mg and etidronic acid components, then from the values in Table 2, b = 0.0007 / 1.71 = approximately 0.0004. In the actual reaction, some of the Mg is converted to X p Since the compound is included in a "complex of a chelating agent and a metal" represented by (a) or a "carbonate" represented by (z), the ratio of a:b changes to a larger value than the above ratio.
[0078] [Table 2]
[0079] Next, carbon dioxide (CO 2 ) (Tohoku Air & Water Co., Ltd., liquefied carbon dioxide gas (purity 99.95% or more) 30 kg cylinder) 10 g (0.23 mol, 5.09 L / standard condition STP) (Mg(OH) 2 Equivalent to 10% by mass of Mg(OH) 2 CO 2 is 0.23 / 1.71 = approx. 0.13, and CO 2 If all is used for Mg-only carbonation, MgO 2 The molar ratio a:c of CO:Mg carbonate can be 0.87:0.13. 2 Since a part of the sulphuric acid is consumed as carbonation or loss of other metal impurities, the ratio of c may be low.) was blown into the suspension after the reaction through a hose for 10 minutes (in the following Examples and Comparative Examples, a part of the sulphuric acid was blown into the suspension through a hose for 10 minutes). 2 (The description of the injection is omitted.) 2After the blowing, the mixture was suction filtered, and a wet solid (wet) with a mass of 218 g was collected by filtration, and 220 g of filtrate was obtained. The filtered solid was dried at 100° C. for 2 hours in a dryer (manufactured by Fuji Scientific Instruments Co., Ltd., product name: BOX furnace standard machine, model: TYPE-G) to obtain magnesium peroxide (MgO 2 ) containing composition (yield 95 g, dry, dried MgO 2 ) was obtained.
[0080] The above MgO 2 The moisture content of the composition after drying was measured using a moisture meter (Kett Electric Laboratory, device name: infrared moisture meter, model: FD-800) and was found to be 1.0% by mass. The available oxygen concentration in the composition (hereinafter simply referred to as available oxygen (mass%)) was measured using the potassium permanganate titration method described below and was found to be 12.45% by mass. Furthermore, the hydrogen peroxide (H 2 O 2 ) concentration (mass %) was similarly analyzed by potassium permanganate titration and found to be 11.7 mass %.
[0081] <Analysis method for magnesium peroxide (potassium permanganate titration method)> Prepare the following reagents: Sulfuric acid solution (1+9): Put 900 mL of pure water into a 1 L container, add 100 mL of sulfuric acid (special grade, 96%) while stirring, and cool. 1N potassium permanganate standard solution (e.g., manufactured by Wako Pure Chemical Industries, Ltd.) 15% by volume nitric acid solution: Put 750 mL of pure water into a 1 L container, add 250 mL of nitric acid (60% by mass) while stirring, and cool. Next, weigh out approximately 0.5 to 1 g of the sample accurately (sample amount: S(g)), and dissolve it by sequentially adding approximately 50 mL of pure water, 10 mL of nitric acid, and 10 mL of sulfuric acid solution. This sample solution is titrated with 1N potassium permanganate standard solution. The end point is when the titrant turns a light pink color for 30 seconds. The available oxygen (%) is calculated using the following formula. Available oxygen (%) = [(8 / 1000) × f 1 ×A] / S(g)×100(%) f 1 : Factor of 1N potassium permanganate standard solution A: Titration constant of 1N potassium permanganate standard solution (mL) S: Sample collection amount (g)
[0082] [Comparative Example 1] In Example 3, instead of the chelating agent (Chilest PH-210) as a stabilizer, poly-α-hydroxyacrylic acid sodium (manufactured by Hodogaya Chemical Co., Ltd., Pale Black 1200 (PHAS 30% by mass solution, average molecular weight 10,000 to 15,000), which is a stabilizer for hydrogen peroxide, was used, and the amount of PHAS added was set to 0.24 g (Mg(OH) 2 The other production conditions were the same as in Example 3. 2 The results are summarized in Table 3.
[0083] [Comparative Example 2] In Example 3, instead of the chelating agent (Chilest PH-210) as a stabilizer, No. 3 sodium silicate (manufactured by Komune Chemical Co., Ltd.), which is a stabilizer for hydrogen peroxide, was used, and the amount added was 0.24 g (Mg(OH) 2 The other manufacturing conditions were the same as in Example 3. 2 The results are summarized in Table 3.
[0084] [Comparative Example 3] In Example 3, the amount of the chelating agent (Chelest PH-210) added as a stabilizer was changed from 0.24 g to 2.35 g (Mg(OH) 2 2.35% by mass, molar ratio a:b=Mg(OH) 2 : etidronic acid = 1.72:0.007 = 1:0.004, 0.5% by mass of the total amount charged, and the other production conditions were the same as in Example 3. 2 The results are summarized in Table 3.
[0085] [Comparative Example 4] Instead of the method of Example 3, a composition containing magnesium peroxide was produced by the following method. 210 g of ion-exchanged water, Mg(OH) 2 140 g (2.4 mol, 1.4 times the molar equivalent of Example 3) of Naikai Salt Co., Ltd. was placed in a 1 L container and stirred without adding a chelating agent. 2 O 2 Aqueous solution 187g (3.84mol←Mg(OH) 2 The reaction was carried out for 30 minutes. The temperature during the reaction was kept at 40°C. After the reaction, the mixture was cooled to 20°C and filtered by suction. The wet filtrate (MgO 2 The residue (composition) was dried at 100° C. for 1 hour in a tray dryer, and 148.2 g of the wet composition was added with CO in the same manner as in Example 3. 2 CO was blown into the tank. 2 After injection, CO 2 Contains MgO 2 The weight of the composition was increased to 158.2 g, and the mixture was further dried at 100° C. for 1.5 hours with stirring to obtain 143.1 g of MgO. 2 After drying, a composition containing MgO was obtained. 2 The moisture content (mass%) and available oxygen (%) of the composition, and H in the filtrate 2 O 2 The concentration was measured in the same manner as in Example 3. The results are summarized in Table 3.
[0086] [Table 3]
[0087] As shown in Table 3, the MgO obtained in the examples 2The available oxygen content of the composition was superior to that of the composition containing other stabilizers. In addition, in each reaction, the container had to be heated to maintain the liquid temperature at 40°C during the reaction in Example 3 and Comparative Example 3, but cooling was required in Comparative Examples 1, 2, and 4. From this, the heat generated during the reaction in the Examples is less than that in the Comparative Examples, and therefore safer. In addition, a comparison between Example 3 and Comparative Example 3 revealed that when a large amount of chelating agent (stabilizer) was added, the synthesis of magnesium peroxide hardly progressed.
[0088] From the results in Table 3, it can be seen that the H present in the charged liquid before the reaction 2 O 2 The amount of available oxygen in the aqueous solution was taken as 100%, and the MgO obtained in Example 3 was 2 The percentage of available oxygen (reaction amount) in the composition was calculated to be 27.0%. Similarly, the amount of H remaining in the filtrate and wet composition was calculated to be 27.0%. 2 O 2 The ratio of available oxygen in the aqueous solution (residual amount) was 43.1%, and the amount of available oxygen that was ineffective in the reaction (ineffective decomposition amount) was 29.9%. The results of calculating the reaction amount, residual amount, and ineffective decomposition amount for Comparative Examples 1 to 4 are summarized in Table 4.
[0089] [Table 4]
[0090] From Table 4, in comparison with Example 3, H 2 O 2 Although the residual amount is large and the amount of ineffective decomposition is small, MgO 2 The reason for the small reaction amount of H is presumably due to the excessive amount of chelating agent used as a stabilizer. On the other hand, in Comparative Example 4, in which no stabilizer was added, 2 O 2 The residual amount of MgO is small, and the amount of ineffective decomposition is large. 2 This is necessary to improve the available oxygen of the composition in which it is contained.
[0091] [Example 4] <Reaction time and MgO 2 Relationship of available oxygen in the composition> In the same manner as in Example 3, 163 g of ion-exchanged water, 0.24 g (0.05% by mass based on the total amount of the charged chelating agent (Chelest PH-210), and Mg(OH) 2 (Mg(OH) manufactured by Naikai Salt Co., Ltd., the same as used in Example 1) 2 Corresponding to the raw material. Used without cleaning.) 100g (1.72mol) was added and stirred (molar ratio Mg(OH) 2 : etidronic acid = 1:0.0004). 2 O 2 207 g (2.74 mol) of the aqueous solution was added (total amount: 470 g) to start the reaction. The other production conditions were the same as in Example 3. 2 O 2 The addition start time was set to 0 minutes, and H 2 O 2 The addition was carried out over a period of 0 to 10 minutes. 2 O 2 After the addition was completed (10 min), samples of the reaction mixture (approximately 0.5 to 1 g) were taken at 15-min intervals, filtered, and the remaining H in the filtrate was measured by potassium permanganate titration. 2 O 2 The concentration (mass%) was analyzed. The residue was washed with ion-exchanged water, dried at 100°C for 10 minutes, and the available oxygen (%) was analyzed. 2 O 2 The reaction was completed 130 minutes after the start of the addition. After the reaction was completed, carbonation was carried out between 130 and 140 minutes, and the magnesium peroxide-containing composition (Dry MgO 2 ) was obtained, and the dried MgO 2 The available oxygen (%) of the contained composition was measured, and the results are shown in Table 5.
[0092] [Examples 5 and 6] <Reaction time and MgO 2 Relationship of available oxygen in the composition> In Example 4, the amount of the chelating agent (Chelest PH-210) added was 0.1% by mass (molar ratio a:b=Mg(OH) 2 : etidronic acid = 1:0.0008) and 0.2 mass% (molar ratio a:b = Mg(OH)2 The same experiment as in Example 4 was carried out except that the ratio of ethanol to ethanol was 1:0.0016. 2 O 2 Concentration (mass%) and MgO 2 The relationship between the content of the composition and the available oxygen (%) was analyzed, and the results are shown in Table 5.
[0093] [Example 7] <Reaction time and MgO 2 Relationship of available oxygen in the composition> In Example 5, Mg(OH) 2 (manufactured by Naikai Salt Industry Co., Ltd.) was used as the same Mg(OH) 2 The amount of chelating agent added (0.1% by mass) to the total amount of the mixture was the same as in Example 5 (molar ratio a:b = Mg(OH) 2 : etidronic acid = 1:0.0008), and other experiments were performed under the same conditions. The reaction time and residual H 2 O 2 Concentration (mass%) and MgO 2 The relationship between the content of the composition and the available oxygen (%) was analyzed, and the results are summarized in Table 5.
[0094] [Table 5]
[0095] Regarding the results in Table 5, the reaction time and residual H 2 O 2 Concentration and MgO 2 The available oxygen concentration in the composition is shown in graphs in Figures 2 and 3. From the tables and figures, it can be seen that the MgO used in Example 1 2 When using raw materials (manufactured by Naikai Salt Co., Ltd.), when the amount of chelating agent added is 0.1 mass% of the total charge, MgO 2 The available oxygen of the composition containing the fluorine was the highest. From Figure 2, the remaining H 2 O 2The concentration was about 15% by mass, suggesting that the reaction can be made more efficient by extending the reaction time. Also, from FIG. 3, even if the reaction time was extended to 30 minutes or more as in Example 3, the available oxygen remained almost constant and did not decrease. In Comparative Example 3, it is known that the amount of chelating agent added to the reaction liquid of 0.5% by mass relative to the total charged amount is excessive and the reaction does not proceed. From FIG. 3 Example 6, with an addition amount of 0.2% by mass, the rise in available oxygen is slow, the start of the reaction is delayed, and the amount added is slightly excessive. The Mg(OH) used in Examples 1 and 2 2 The final dried MgO obtained due to the difference in raw materials 2 It was found that the available oxygen of the containing compositions was different.
[0096] [Examples 8 to 11] <Long-term stability test of magnesium peroxide-containing composition> Four types of MgO produced in Examples 4 to 7 2 10 g of the composition (each manufactured on a different date) was placed in a polystyrene rod bottle and left to stand in a 40°C thermostatic chamber (Kusumoto Chemicals Co., Ltd., equipment: high temperature thermostatic chamber, model: ETAC HT220) for approximately 2 months (62 days). During this period, 0.5 to 1 g was taken from each sample tube on days 0, 13, 28, and 62, and the available oxygen was measured. As an index of stability, the ratio of the available oxygen on day 62 to the available oxygen on day 0 was calculated using the MgO 2 The results were expressed as the stability (%) of the composition. The results are shown in Table 6 and FIG.
[0097] [Comparative Example 5] MgO produced in Comparative Example 4 2 Containing composition (Mg(OH) of Example 1) 2 The raw material (manufactured by Naikai Salt Co., Ltd.) was used, and the stability was measured after standing at 40°C for 0, 13, 28, and 62 days using the same experimental method as in Examples 8 to 11. The results are shown in Table 6 and Figure 4.
[0098] [Comparative Example 6] Mg(OH) of Example 2 2Using the raw material (manufactured by Konoshima Chemical Co., Ltd., model number: #200), MgO was synthesized in the same manner as in Comparative Example 4. 2 The resulting compositions containing the compound were allowed to stand at 40° C. in the same manner as in Examples 8 to 11, and the available oxygen and stability were measured on days 0, 13, 28, and 62. The results are shown in Table 6 and FIG.
[0099] [Table 6]
[0100] From Table 6 and FIG. 4, the available oxygen value on day 0 varies from 10 to 16% by mass, but after 62 days, all samples maintain a stability of 94% or more. In the measurements of Examples 8 to 11, Comparative Examples 5 and 6, the change in moisture content is not taken into consideration, so the stability may exceed 100% as in the result of Comparative Example 6. Magnesium peroxide is highly hygroscopic, and the moisture content is higher on day 0 than on day 62. Therefore, if the amount of sample taken for measurement from the sample tube is the same each time, it becomes drier as the days pass, and the available oxygen appears to be a high value, and it is presumed that the stability may exceed 100%.
[0101] [Examples 12 to 15] <Reaction temperature considerations> In Example 3, 100 g of Mg(OH) 2 The amount of ion-exchanged water and chelating agent used was changed as shown in Table 7. The chelating agent (Chelest PH-210) was dissolved in ion-exchanged water in advance and placed in a reaction vessel. Magnesium hydroxide (Mg(OH) 2 ) (manufactured by Naikai Salt Industry Co., Ltd.) was added to this suspension, and 100 g of 35% by mass of hydrogen peroxide (H 2 O 2 The aqueous solution of 1,2-dichlorophenyl ether was added dropwise over 60 minutes. The temperature during the reaction was controlled to 40°C, 45°C, 50°C, or 60°C by controlling the temperature of the vessel. 2 O 2The start of the dropwise addition (addition) was defined as the start of the reaction (0 min), and 10 mL of the suspension was sampled every 20 min. Each 10 mL sample was filtered, the filtered residue was washed with ion-exchanged water, and dried at 100°C for 10 min using the moisture meter (used in Example 3). The moisture content was analyzed, and the MgO produced in the dried product was analyzed. 2 The available oxygen in the composition was analyzed by the potassium permanganate titration method. The analysis was performed up to 120 minutes of reaction time. The reaction temperature (°C) and the MgO content at the reaction time from the start of addition were 2 The results of measuring the relationship with the available oxygen (%) of the magnesium-containing composition are shown in Table 8 and Figure 5. The available oxygen value in Table 8 is calculated as the available oxygen of the magnesium-containing portion excluding moisture, taking into account the reduction in moisture (in the following examples, unless otherwise specified, the available oxygen taking moisture into account is shown).
[0102] [Table 7]
[0103] [Table 8]
[0104] From Table 8 and Figure 5, 35 mass% H 2 O 2 Using the concentration, MgO 2 In the production of the composition containing the benzoyl peroxide, the reaction time was 100 to 120 minutes, and the reaction temperature was 40°C or 45°C, and the available oxygen was higher than that of the reaction temperature of 50°C or 60°C. The available oxygen tended to decrease as the reaction temperature increased.
[0105] [Examples 16 to 18] <Study on the concentration of added hydrogen peroxide> In Examples 12 and 13, MgO was added at 40° C. and 45° C. 2 Since the available oxygen of the composition is high, the reaction temperature was set at 42°C. Other experimental conditions were as shown in Table 9. 2 O 2The concentration was set to 35 mass %, 45 mass % or 60 mass %, and the reaction time was examined up to 120 minutes in the same manner as in Examples 12 to 15. The results are shown in Table 10 and FIG.
[0106] [Table 9]
[0107] [Table 10]
[0108] From Table 9 and Figure 6, 35 mass% H 2 O 2 The one with the aqueous solution added has the highest available oxygen. 2 O 2 There was a tendency for the amount of available oxygen to decrease as the concentration increased.
[0109] [Examples 19 and 20] <Examination of hydrogen peroxide solution addition time> H in Example 16 2 O 2 The same procedure as in Example 16 was used to add 35% by mass H, except that the dropwise addition time was changed from 60 minutes to 20 minutes or 40 minutes. 2 O 2 MgO using aqueous solution at 42°C and reaction time up to 120 minutes 2 The compositions containing the composition were analyzed for available oxygen, and the results are shown in Table 11 and FIG.
[0110] [Table 11]
[0111] From Table 11 and Figure 7, H 2 O 2 There was no significant change in the available oxygen by changing the instillation time between 20 and 60 minutes.
[0112] [Example 21] <Consideration of the amount of hydrogen peroxide to be added> Mg(OH) as raw material for Example 16 2 35% by mass H for 13.6 mol 2 O 2 In a test conducted by reacting 1.7 mol of aqueous solution, Mg(OH) 2 and H 2 O 2 35% by mass H so that the molar amount of 2 O 2 The amount of the aqueous solution added (dropped) was increased, and the experiment was carried out in the same manner as in Example 16 at a reaction temperature of 42°C. MgO was added every 10 minutes of reaction time. 2 Analysis of the available oxygen in the composition and H in the filtrate 2 O 2 A concentration analysis was performed. 2 O 2 Molar amount of Mg(OH) 2 The reaction was carried out in the same manner with the molar amount increased to 1.25 times and 1.5 times that of H. The results are shown in Figure 8. 2 O 2 There was a tendency for the amount of available oxygen to increase as the amount added increased.
[0113] 1.5 times the molar amount of H obtained in Example 21 2 O 2 In the reaction using 2 O 2 Changes in concentration and MgO 2 The change in the available oxygen of the composition containing H is compared with that of the composition containing H. 2 O 2 The reaction started when the concentration reached 18% by mass, and the reaction time was about 70 minutes. 2 O 2 It was found that the reaction was terminated at a concentration of 2% by mass or less, more specifically, 1% by mass or less.
[0114] [Examples 22 to 24] <Consideration of mass production> The amount of the preparation conditions carried out in Example 20, H 2 O 2 Concentration of aqueous solution, reaction temperature, H 2 O 2Under the same test conditions for the drop (addition) time, the scale of 40 times the mass shown in Table 12 (Mg(OH) 2 The test in Example 22 was carried out using 4 kg of magnesium peroxide. In place of the magnesium peroxide used in Example 20 (manufactured by Naikai Salt Industry Co., Ltd., raw material in Example 1), in Examples 23 and 24, magnesium peroxide (manufactured by Konoshima Chemical Co., Ltd., model number: #200, raw material in Example 2) was used to obtain Mg(OH) 2 Tests were performed under similar test conditions with 100g or 4kg. 2 The results of the analysis of the contained compositions are shown in Table 12.
[0115] [Table 12]
[0116] As shown in Table 12, Mg(OH) 2 In the raw material, the maximum value of available oxygen decreased when the scale was increased from 100g to 20kg. On the other hand, the Mg(OH) 2 For the raw material, the maximum available oxygen values were higher than those in Example 1 for both 100g and 20kg.
[0117] [Example 25] <Consideration of drying conditions> 4kg-Mg(OH) obtained in Example 24 2 MgO produced using raw materials 2 The drying of the composition containing MgO was carried out as follows. 2 The composition containing MgO was dehydrated until most of the moisture was removed. The filtered material was divided into 3 kg, 2 kg, and 1 kg portions for each portion, and dried in the shelf dryer by spreading them evenly on the shelf (480 mm x 750 mm). The thicknesses of the spread compositions were 5 mm, 10 mm, and 15 mm, respectively. The temperature inside the dryer was set to 90°C. The drying time and the MgO content were measured for drying times of 60 minutes, 120 minutes, and 180 minutes. 2 The relationship between the available oxygen of the composition was measured, and the results are shown in Table 13.
[0118] [Table 13]
[0119] Drying was terminated when the moisture content was 5% or less in Table 13. Table 13 shows that the shorter the drying time, the higher the available oxygen.
[0120] [Example 26] 4kg-Mg(OH) prepared in the same manner as in Example 25 2 MgO produced using raw materials 2 In the case of the composition containing the sucrose-containing compound, a test was conducted in which 2 kg of the composition before drying was dried at a temperature of 90°C, but this was changed to 80°C or 100°C. In either case, the composition was dried to a moisture content of 5% by mass or less in 120 to 180 minutes. The available oxygen content after drying was 13 to 16%.
[0121] [Examples 27 to 29] The Mg(OH) of Example 2 was prepared in the same manner as in Example 23. 2 Using the raw material (manufactured by Konoshima Chemical Co., Ltd., model number: #200), MgO was added in the amounts shown in Table 14. 2 The composition was prepared by adding ion-exchanged water, etidronic acid solution, Mg(OH) 2 After the raw materials are added, 2 O 2 The addition of the aqueous solution (dropwise) was started. 2 O 2 After the addition of the aqueous solution, the temperature of the reaction solution rose, so the temperature was allowed to drop and the addition was resumed. After the addition was completed, the mixture was stirred for 60 minutes, and the H 2 O 2 The reaction was terminated when the concentration reached 2% by mass or less. 2 After blowing, dehydration, and wetting the MgO 2 A composition containing MgO was obtained. The drying was performed using the shelf dryer (used in Example 3) and a vibration dryer (manufactured by Chuo Kakoki Co., Ltd., model: VU-95). The drying temperature was 90°C, and the drying was completed when the moisture content was 10% or less. 2The MgO-containing composition was crushed using a commercially available crusher, and then packed in bags of 20.05 kg each and sealed. The manufacturing conditions not described above were the same as those in the other examples. 2 The moisture content and available oxygen of the contained compositions are summarized in Table 14.
[0122] [Table 14]
[0123] [Example 30] <Magnesium peroxide granulation test> The manufacturing method (granulation method) of granules (magnesium peroxide granules) using the composition containing magnesium peroxide of the present invention will be described in the following examples. 2 Water was added to the composition containing MgO to prepare a composition with a moisture content of 24 to 35% by mass, which was used as a pre-granulation sample. The composition after the moisture content adjustment was granulated using a commercially available pug mixer (hole diameter 1 mm) and dried in the same manner as described above. In addition, a MgO sample with a moisture content of 35% by mass was used to adjust the moisture content. 2 The composition contains magnesium carbonate (MgCO 3 The moisture content was adjusted and granulation was carried out. The results are shown in Table 15.
[0124] [Table 15]
[0125] As shown in Table 15, granulation is possible by adjusting the moisture content to 26 to 28% by mass. It was found that the available oxygen decreases when a powder other than magnesium peroxide is used for adjusting the moisture content. 2 When bentonite and Parwell G (calcium peroxide) were used in the composition to adjust the moisture content, heat was generated during mixing, which was thought to be due to ineffective decomposition, and granulation was halted. When mixing these powders to manufacture magnesium peroxide granules, cooling during mixing is required.
[0126] [Example 31] <Consideration of continuous manufacturing> MgO 2 A method for producing a composition containing MgO by continuously reacting the composition (sometimes abbreviated as a continuous production method) was investigated. FIG. 10 shows an example of a system for constructing the continuous production method of the present invention. With reference to FIG. 10, 2 The continuous production method of the composition is explained below. The equipment such as heating / cooling equipment, pumps, and agitators, or materials made of glass, metal, or resin were appropriately selected and used. (1) A reaction vessel (31-1) is charged with 30% by mass of Mg(OH). 2 200 g of the mixture (slurry) is taken and heated to a constant temperature using the heating and cooling device attached to the reactor. The reactor is stirred using the stirring device (31-4). *30 mass%Mg(OH) 2 / water mixture (slurry) preparation method: Mg(OH) 2 Mix 300 g of (Konoshima Chemical Co., Ltd., model number: #200), 691 g of ion-exchanged water, and 9 g of 10% by mass chelating agent (a 10-fold dilution of Chelest PH-210) (total 1000 g). (2) When the temperature becomes constant, Mg(OH) 2 (Mainly Mg(OH) 2 Mg(OH) from the slurry reservoir (31-2) 2 The slurry is added to the reaction tank (31-1), and at the same time, 60% by mass H 2 O 2 The aqueous solution begins to be added to the reaction vessel (31-1). (3) When the liquid in the reaction tank (31-1) reaches a certain amount, the liquid flows out of the pipe attached to the reaction tank (overflow). When the overflow starts, the cooling of the overflow receiver (31-6) at the outlet of the pipe is started, and at the same time, the CO 2 The overflow receiver is agitated with a stirring device (such as a stirrer), and is equipped with a heating / cooling device (including ice water cooling), and a gas supply device such as a carbon dioxide cylinder and its piping. (4) After overflow begins, replace the overflow receiver (container part 31-6) at regular intervals. (5) Measure the mass of the liquid flowing into the overflow receiver and filter it using a suction filter or similar device. (6) H in the filtrate 2 O 2 The concentration was analyzed. At the same time, the filtered material (wet MgO 2 Dry the composition (shelf dryer, drying temperature: 90°C, drying time: 3 to 4 hours). (7) MgO after drying 2 The contained composition is analyzed for moisture content and available oxygen.
[0127] Using the above continuous production method, the reaction temperature was changed from 50 to 70 ° C. (Examples 31-1 to 3). Under the reaction conditions in Table 16, Mg (OH) 2 Slurry and H 2 O 2 Tests in which the reaction time was changed from 12 to 31 minutes by changing the addition rate of the aqueous solution (Examples 31-4 to 31-6), and Mg(OH) 2 Slurry and H 2 O 2 Hydrogen peroxide / Mg(OH) reaction by varying the rate of addition of the aqueous solution 2 The results are shown in Table 16.
[0128] [Table 16]
[0129] From Table 16, as the reaction temperature increases, the H 2 O 2 and the resulting MgO 2 Both decompose, so MgO 2 The available oxygen of the composition containing the fluorine-containing compound was reduced. In addition, the longer the reaction time, the lower the available oxygen. 2 O 2 Mg(OH) 2 At lower molar ratios, the available oxygen was lower.
[0130] [Example 32] <Stability test> MgO 2 In order to investigate the stability of the composition containing various MgO, the following tests were carried out. 2 Several tens of grams of the composition were placed in a 100 mL polystyrene rod bottle (manufactured by Sanshin Kogyo Co., Ltd.) and left to stand in a 40°C thermostatic chamber (manufactured by Kato Co., Ltd.) for one month (30 days) (this can be considered a one-year storage test in an environment of normal temperature and humidity). Every 10 days, 0.5 to 1 g of the composition was sampled and the available oxygen was analyzed by potassium permanganate titration to check the stability. The following three types of samples were used: (1) Magnesium peroxide-containing composition (prepared as in Example 29) (2) Magnesium peroxide hydrate (MgO 2 : Surfactant (Toho Chemical Industry Co., Ltd., Sorpol 5060) = Mixed at 95:5 (mass ratio) (3) Magnesium peroxide with 2% PVA (Polynyl alcohol (PVA) (Wako Pure Chemical Industries, Ltd., special grade reagent) was used. PVA and MgO were mixed so that the total amount was 2 mass%. 2 The above was mixed using a kneader (Model KDHJ-20, manufactured by Fuji Paudal Co., Ltd. (currently Dalton Co., Ltd.).) The stability index is expressed as the percentage of available oxygen at each elapsed day, with the available oxygen at the start of the test (day 0) taken as the standard (100%). The results are shown in Table 17.
[0131] [Table 17]
[0132] Magnesium peroxide (MgO 2 ) decreases with the passage of time, which means that MgO 2 This means that oxygen is being generated by the decomposition of MgO. 2The amount of oxygen generated by the decomposition of can be calculated from the decomposition reaction formula (4) below. 0.5 mol of oxygen is released by the decomposition of 1 mol of magnesium peroxide. Using the stability test results in Table 17, the amount of oxygen generated by decomposition (volume (L)) per 1 kg of the magnesium peroxide-containing composition was calculated as follows. The results are shown in Table 18. From these results, the performance (stability, etc.) of the magnesium peroxide-containing composition of the present invention as an oxygen supplying agent can be obtained.
[0133] [ka]
[0134] [Table 18]
[0135] From these examples, it was found that the composition containing magnesium peroxide of the present invention is a composition containing magnesium peroxide that has a high effective oxygen concentration and is highly stable. [Industrial Applicability]
[0136] The magnesium peroxide-containing composition obtained by the production method of the present invention can provide a magnesium peroxide-containing composition having a high effective oxygen concentration and stability. The composition obtained by the present invention can be used as an oxygen supply agent and can be utilized in agricultural applications, soil purification, water quality improvement, and the like. [Explanation of symbols]
[0137] 31 Continuous manufacturing system for compositions containing magnesium peroxide 31-1 Reactor 31-2 Mg(OH) 2 Slurry Storage Tank 31-3 Hydrogen peroxide storage tank 31-4 Mixing device 31-5 Liquid delivery pump 31-6 Overflow receiver (heating, cooling, stirring, CO 2 (Including the supply system.)
Claims
1. A composition containing magnesium peroxide represented by the following general formula (1), The concentration of impurities containing a complex of etidronic acid and a metal is 5% by mass or less; The moisture content is 3 to 12% by mass, The carbonate concentration is CO 3 2- The composition is characterized in that the content is 2 to 20 mass% in terms of the mass of the composition. 【Chemistry 1】 [In formula (1), X p represents a complex of etidronic acid and a metal, Z represents a carbonate, a represents 0.1 to 1, b represents more than 0 to 0.1, and c represents more than 0 to 0.
9.
2. X in the general formula (1) p but, 2. The composition of claim 1 which is a complex containing Ca, Mn, Fe, Cu or Al.
3. 3. An oxygen supply comprising the composition according to claim 1 or 2.
4. A step of adding water and / or a carbonate to the composition according to claim 1 or 2 to obtain a pre-granulation sample; Next, a step of granulating the obtained pre-granulation sample; and A method for producing magnesium peroxide granules, comprising the step of drying the granulated sample.
5. A method for producing a composition containing magnesium peroxide represented by the following general formula (2), A manufacturing method comprising carrying out steps 1 and 2. 【Chemistry 2】 [In formula (2), X p represents a complex of etidronic acid and a metal, Z represents a carbonate, a represents 0.1 to 1, b represents more than 0 to 0.1, and c represents more than 0 to 0.
9. Step 1: A hydroxide or oxide of magnesium, A composition containing etidronic acid as a chelating agent; React with hydrogen peroxide to obtain peroxide. Step 2: The peroxide obtained in step 1 is treated with To contain carbon dioxide or carbonate.
6. The method according to claim 5 , wherein the step 1 or the step 2 is carried out continuously.
Citation Information
Patent Citations
Promotion of germination of paddy seed
JP1986166304A
Stabilizing method for divalent metallic peroxide
JP1986286206A
Method for stabilizing peroxide of divalent metal
JP1987017006A
Oxygen supplier
JP1992089302A
Process for producing magnesium peroxide
JP2004107127A