Compound, composition, film, laminate and display device
A compound in the 370-470 nm range, combined with smectic liquid crystal compounds, addresses the low dichroic ratio issue in existing polarizing films, achieving high-performance polarizing films with enhanced alignment and X-ray diffraction peaks.
Patent Information
- Application Number
- JP2020183803
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-02
- Publication Date
- 2024-10-24
- Estimated Expiration
- 2040-11-02
AI Technical Summary
Existing polarizing films with bisazo dyes having a 1,4-naphthylene structure exhibit low dichroic ratios when combined with higher order smectic liquid crystal compounds, leading to poor polarizing performance.
A compound represented by formula (1) with a maximum absorption wavelength between 370 nm and 470 nm, combined with a smectic liquid crystal compound, forms a polarizing film with a high dichroic ratio, using a composition that includes a polymerizable liquid crystal compound and a liquid crystal polymer compound.
The composition achieves a polarizing film with a high dichroic ratio, enhancing the polarizing performance by aligning the liquid crystal compounds in a smectic phase, resulting in a film with excellent orientational order and Bragg peaks in X-ray diffraction.
Smart Images

Figure 0007572838000001 
Figure 0007572838000002 
Figure 0007572838000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a compound, a composition, a film, a laminate, and a display device. [Background technology]
[0002] There is a continuous demand for thinner displays such as image display panels, and further thinner polarizing plates, polarizers, and other components thereof are also being demanded. In response to such demands, for example, a thin host-guest type polarizer has been proposed that includes a polarizing film containing a polymerizable liquid crystal compound and a dye compound exhibiting dichroism (see, for example, Patent Documents 1 and 2). Patent Document 3 describes a bisazo dye having a 1,4-naphthylene structure as a yellow to orange dichroic dye having an absorption maximum in the wavelength range of 370 nm to 470 nm. [Prior art documents] [Patent documents]
[0003] [Patent Document 1] Special Publication No. 2007-510946 [Patent Document 2] JP 2013-37353 A [Patent Document 3] Japanese Patent Application Publication No. 56-104984 Summary of the Invention [Problem to be solved by the invention]
[0004] However, when the bisazo dye having a 1,4-naphthylene structure described in Patent Document 3 is combined with a higher-order smectic liquid crystal compound, the dichroic ratio is low when the dye is dispersed among dense molecular chains formed by the higher-order smectic liquid crystal compound, and a polarizing film with poor polarization performance may be obtained.
[0005] An object of the present invention is to provide a compound capable of forming a polarizing film having a maximum absorption wavelength in the wavelength range of 370 nm or more and 470 nm or less and having a high dichroic ratio, and a composition comprising said compound and a liquid crystalline compound and capable of forming a polarizing film having a high dichroic ratio. [Means for solving the problem]
[0006] The present invention provides the following [1] to
[10] . [1] A composition comprising a compound represented by the following formula (1) and having a maximum absorption wavelength in the wavelength range of 370 nm or more and 470 nm or less, and a liquid crystalline compound including at least one of a polymerizable liquid crystalline compound and a liquid crystalline polymer compound: [ka] In formula (1), x represents 1 or 2. R 1 and R 2 each independently represents an alkyl group, an alkoxy group, an alkoxycarbonyl group, or an alkanoyloxy group, and at least one of the hydrogen atoms of these groups may be substituted with a polymerizable group. Ar 1 , Ar 2 and Ar 3 each independently represents a divalent aromatic group selected from the group consisting of a thiazoldiyl group, a benzothiazoldiyl group, a thieno[2,3-d]thiazol-2,5-diyl group, and a 1,4-phenylene group; Ar 1 , Ar 2 and Ar 3 At least one of the aromatic groups is a thiazoldiyl group, a benzothiazoldiyl group, or a thieno[2,3-d]thiazole-2,5-diyl group, and these aromatic groups may be substituted with at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group. If x is 2, then two Ar 3 may be the same or different.] [2] The composition according to [1], wherein the liquid crystal compound is a smectic liquid crystal compound. [3] In the formula (1), Ar 1 , Ar 2 and Ar 3 At least one of R is a benzothiazolediyl group; 1 and R 2 each independently represents an alkyl group, an alkoxy group, or an alkoxycarbonyl group. [4] In the formula (1), at least Ar 1 The composition according to any one of [1] to [3], wherein is a benzothiazolediyl group. [5] A compound represented by the following formula (1a) having a maximum absorption wavelength in the wavelength range of 370 nm or more and 470 nm or less. [ka] In formula (1a), y represents 1 or 2. R 11 and R 12 each independently represents an alkyl group, an alkoxy group, an alkoxycarbonyl group, or an alkanoyloxy group, and at least one of the hydrogen atoms of these groups may be substituted with a polymerizable group. Ar 11 , Ar 12 and Ar 13 each independently represents a divalent aromatic group selected from the group consisting of a thiazoldiyl group, a benzothiazoldiyl group, and a 1,4-phenylene group; Ar 11 , Ar 12 and Ar 13 At least one of the aromatic groups is a thiazoldiyl group or a benzothiazoldiyl group, and these aromatic groups may be substituted with at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group. If y is 2, then 2 Ar 13 may be the same or different.] [6] In the formula (1a), Ar 11 , Ar 12 and Ar 13 At least one of the groups is a benzothiazolediyl group. [7] In the formula (1a), at least Ar 11 is a benzothiazolediyl group. [8] A film formed from the composition according to any one of [1] to [4]. [9] A laminate comprising the film according to [8].
[10] A display device comprising the laminate described in [9]. Effect of the Invention
[0007] According to the present invention, it is possible to provide a compound that has an absorption maximum in the wavelength range of 370 nm or more and 470 nm or less and is capable of forming a polarizing film with a high dichroic ratio, and a composition that contains the compound and a liquid crystalline compound and is capable of forming a polarizing film with a high dichroic ratio. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] In this specification, the term "step" includes not only an independent step, but also a step that cannot be clearly distinguished from other steps, as long as the intended purpose of the step is achieved. In addition, the content of each component in the composition means the total amount of the multiple substances present in the composition when multiple substances corresponding to each component are present in the composition, unless otherwise specified. Hereinafter, the embodiment of the present invention will be described in detail. Note that the scope of the present invention is not limited to the embodiment described here, and various modifications can be made within the scope of the present invention.
[0009] <Composition> The composition according to the present embodiment contains a compound represented by the following formula (1) and having a maximum absorption wavelength in the wavelength range of 370 nm to 470 nm, and a liquid crystalline compound containing at least one of a polymerizable liquid crystal compound and a liquid crystalline polymer compound. The composition is used, for example, as a material for forming a polarizing film. That is, the composition may be a composition for forming a polarizing film. A polarizing plate having a polarizing film obtained by using the composition as a material for forming the polarizing film can exhibit an excellent dichroic ratio.
[0010] A compound represented by formula (1) The composition contains at least one compound represented by the following formula (1) (hereinafter also referred to as compound (1)). Compound (1) has a maximum absorption wavelength (λmax) in the range of 370 nm to 470 nm, and is used, for example, as a dye compound (e.g., a dichroic dye compound) in the composition. Compound (1) contained in the composition may be a compound represented by formula (1a) described later.
[0011] [ka]
[0012] x represents 1 or 2, preferably 1. 1 and R 2 R each independently represents an alkyl group, an alkoxy group, an alkoxycarbonyl group, or an alkanoyloxy group. 1 and R 2 are each independently preferably an alkyl group, an alkoxy group, or an alkoxycarbonyl group, and more preferably an alkyl group or an alkoxy group. 1 or R 2 The hydrogen atoms of the alkyl groups in R 1 or R 2 At least one hydrogen atom of the alkyl group moiety of the group represented by the formula (I) may be substituted with a polymerizable group. The polymerizable group is preferably a radically polymerizable group, and examples thereof include a (meth)acrylate group ((meth)acryloyloxy group) and a styryl group (vinylphenyl group), and among these, a (meth)acrylate group is preferred. 1 or R 2 When the group represented by the formula (I) has a polymerizable group, the number of the polymerizable group is, for example, 1 or 2, and preferably 1.
[0013] R 1 and R 2The number of carbon atoms in the alkyl group in the above, and the alkyl group moiety in the alkoxy group, alkoxycarbonyl group, and alkanoyloxy group may be, for example, 1 to 16, and preferably 1 to 10. The alkyl group or alkyl group moiety may be linear or branched. Specific examples of the alkyl group or alkyl group moiety include a 1-methylethyl group, a 2-methylpropyl group, a butyl group, a 2-methylbutyl group, a 3-methylbutyl group, a hexyl group, and a 3,7-dimethyloctyl group.
[0014] Ar 1 , Ar 2 and Ar 3 each independently represents a divalent aromatic group selected from the group consisting of a thiazoldiyl group, a benzothiazoldiyl group, a thieno[2,3-d]thiazol-2,5-diyl group, and a 1,4-phenylene group. 1 , Ar 2 and Ar 3 At least one of Ar is a thiazoldiyl group, a benzothiazoldiyl group, or a thieno[2,3-d]thiazol-2,5-diyl group, and is preferably a benzothiazoldiyl group. 1 , Ar 2 or Ar 3 The aromatic group represented by the formula (I) may be substituted with at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group. 1 , Ar 2 or Ar 3 When the aromatic group represented by the following formula (I) has a substituent, the number of the substituents is, for example, 1 or 2, and preferably 1.
[0015] Ar 1 , Ar 2 or Ar 3 The thiazolediyl group represented by the formula (2) may be a thiazole-2,4-diyl group or a thiazole-2,5-diyl group, and may be represented by the following formula (2): 1 , Ar 2 or Ar 3The benzothiazolediyl group represented by the formula (3) may be a benzothiazole-2,5-diyl group or a benzothiazole-2,6-diyl group, and may be represented by the following formula (3): 1 , Ar 2 or Ar 3 The thieno[2,3-d]thiazole-2,5-diyl group represented by the formula (4) may be represented by, for example, the following formula (4): 1 , Ar 2 or Ar 3 The 1,4-phenylene group represented by the following formula (5) may be represented, for example:
[0016] [ka]
[0017] X in formulas (2), (3) and (5) 1 Each of X in formula (4) independently represents at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group. 2 represents a hydrogen atom, a halogen atom, a methyl group, a hydroxyl group or a methoxy group. m2 represents 0 or 1. m3 represents an integer from 0 to 3. m5 represents an integer from 0 to 4.
[0018] Specific examples of compound (1) include compounds represented by the following formulas (1-1) to (1-41), but the present invention is not limited thereto.
[0019] [ka]
[0020] [ka]
[0021] [ka]
[0022] From the viewpoint of the dichroic ratio, compound (1) is preferably at least one selected from the group consisting of compounds represented by any one of formulas (1-1) to (1-33), and more preferably at least one selected from the group consisting of compounds represented by any one of formulas (1-1) to (1-23).
[0023] Compound (1) may have a maximum absorption wavelength (λmax) in the wavelength range of 370 nm to 470 nm. The wavelength range of the maximum absorption wavelength of compound (1) may be preferably 400 nm to 470 nm, more preferably 420 nm to 460 nm. The upper and lower limits in the above ranges may be arbitrarily combined. The maximum absorption wavelength is measured at room temperature (e.g., 25°C) for an acetonitrile solution of compound (1).
[0024] The maximum absorption wavelength of the compound (1) is, for example, Ar 1 , Ar 2 and Ar 3 The framework structure of Ar 1 , Ar 2 and Ar 3 Substituents x and R in 1 , R 2 By appropriately selecting the above, it is possible to adjust the wavelength to a desired wavelength.
[0025] The content of compound (1) in the composition is, for example, preferably 50 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, and even more preferably 0.1 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the solid content of the composition. Within the above range, compound (1) can be sufficiently dispersed. This allows efficient production of a film made of compound (1) and in which the occurrence of defects is sufficiently suppressed. In this specification, the solid content refers to the total amount of components excluding volatile components such as solvents from the composition. The composition may contain only one type of compound (1), or may contain a combination of two or more types with different structures. When the composition contains two or more types of compound (1), they may have different maximum absorption wavelengths.
[0026] A polarizing plate having a polarizing film containing a composition containing compound (1) as a dye component as a forming material can achieve an excellent dichroic ratio (DR). The dichroic ratio (DR) of a polarizing plate having a polarizing film containing the composition as a forming material may be, for example, 20 or more, preferably 25 or more, more preferably 30 or more, even more preferably 35 or more, 40 or more, 45 or more, or 50 or more. The dichroic ratio of the polarizing plate is measured by the method described below. In addition, a film containing a composition containing compound (1) as a forming material includes a film containing compound (1) as an independent molecule, and a film containing a partial structure derived from compound (1) that is generated by the reaction of compound (1) with another compound.
[0027] The composition contains the compound (1) having a specific structure, and thus can form a polarizing film that can achieve an excellent dichroic ratio in the wavelength range of, for example, 390 nm to 510 nm. This can be considered, for example, as follows. In the compound (1), Ar 1 , Ar 2 and Ar 3 At least one of the R 1 and R 2 This is believed to enable the formation of a polarizing film having a maximum absorption wavelength in a wavelength range of, for example, 390 nm or more and 510 nm or less (e.g., orange color), preferably in a wavelength range of 420 nm or more and 500 nm or less, and more preferably in a wavelength range of 440 nm or more and 490 nm or less.
[0028] Method for producing compound (1) Compound (1) can be produced by appropriately applying a conventionally known synthesis method. Specifically, the azo structure (-N=N-) in compound (1) can be constructed by converting an aromatic amine compound having a primary amino group into a diazonium salt with sodium nitrite or the like, and diazo-coupling it with an aromatic compound, for example, with reference to the description of the production example in paragraphs
[0220] to
[0268] of International Publication WO2016 / 136561. In addition, an azo structure containing a thiazole structure can be constructed, for example, with reference to the description in J. Mol. Struct., 2011, 987,158.
[0029] R 1 or R 2 Compound (1) in which is an alkoxy group can be prepared by, for example, reacting a precursor having a hydroxy group with S N By applying a disubstitution reaction, the compound (1) having the desired alkoxy group can be produced. N The displace-ment reaction may be carried out under conventionally known reaction conditions as appropriate, or the description in, for example, J. Am. Chem. Soc., 2008, 130, 13079 may be referred to.
[0030] The reaction time in the production method of compound (1) can also be determined by appropriately sampling the reaction mixture during the reaction and confirming the degree of disappearance of the raw material compounds, the degree of production of compound (1), and the like by a known analytical means such as liquid chromatography or gas chromatography.
[0031] After the reaction, compound (1) can be isolated from the reaction mixture by known methods such as recrystallization, reprecipitation, extraction and various types of chromatography, or by an appropriate combination of these procedures.
[0032] The composition may further contain other dye compounds other than compound (1), for example, at least one kind of dichroic dye. Examples of other dye compounds include azo dyes such as monoazo dyes, bisazo dyes, trisazo dyes, tetrakisazo dyes, and stilbene azo dyes, and at least one kind selected from the group consisting of these is preferable. The composition may contain one kind of other dye compound alone, or may contain two or more kinds in combination. For example, when used as a coating type polarizing plate material, it is preferable that the other dye compounds contained in the composition have a maximum absorption wavelength in a wavelength range different from that of compound (1). For example, when used as a coating type polarizing plate material, the composition preferably contains three or more kinds of dichroic dyes in combination, including compound (1), and more preferably contains three or more kinds of azo dyes in combination. When the composition contains three or more kinds of dye compounds in combination with different maximum absorption wavelengths, for example, absorption can be obtained in the entire visible light range by a film formed from the composition.
[0033] When the composition contains other dye compounds, the content thereof is preferably 50 parts by mass or less, more preferably 0.1 parts by mass or more and 10 parts by mass or less, and even more preferably 0.1 parts by mass or more and 5 parts by mass or less, relative to 100 parts by mass of the solid content of the composition. If it is within the above range, the other dye compounds can be sufficiently dispersed.
[0034] liquid crystal compound The composition contains a liquid crystal compound including at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound in addition to compound (1). The composition may contain both a polymerizable liquid crystal compound and a liquid crystal polymer compound, and the polymerizable liquid crystal compound and the liquid crystal polymer compound contained in the composition may each be two or more kinds. By containing at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, a composition can be formed in which compound (1) is dispersed in the polymerizable liquid crystal compound and the liquid crystal polymer compound.
[0035] The liquid crystalline polymer compound may be a thermotropic liquid crystal polymer or a lyotropic liquid crystal polymer. The liquid crystalline polymer compound is preferably a thermotropic liquid crystal polymer, since it allows precise control of the film thickness.
[0036] Liquid crystals are classified into smectic liquid crystals, nematic liquid crystals, and cholesteric liquid crystals according to the molecular arrangement structure in the liquid crystal state. Among them, smectic liquid crystals are preferably used for polarizing film applications. Therefore, the polymerizable liquid crystal compound is preferably a polymerizable smectic liquid crystal compound, and the liquid crystalline polymer compound is preferably a smectic liquid crystalline polymer compound.
[0037] By using a polymerizable liquid crystal compound exhibiting smectic liquid crystallinity and a polymer compound exhibiting smectic liquid crystallinity, a polarizing film with a high degree of orientation order can be formed. The liquid crystal state exhibited by the polymerizable liquid crystal compound and the liquid crystal polymer compound is preferably a smectic phase (smectic liquid crystal state), and more preferably a high-order smectic phase (high-order smectic liquid crystal state) from the viewpoint of realizing a higher degree of orientation order. Here, the high-order smectic phase means a smectic B phase, a smectic D phase, a smectic E phase, a smectic F phase, a smectic G phase, a smectic H phase, a smectic I phase, a smectic J phase, a smectic K phase, and a smectic L phase, and among these, the smectic B phase, the smectic F phase, and the smectic I phase are more preferable. A polarizing film with a high degree of orientation order can obtain a Bragg peak derived from a high-order structure such as a hexatic phase or a crystal phase in an X-ray diffraction measurement. The Bragg peak means a peak derived from the planar periodic structure of molecular orientation. The periodic interval (order period) of the polarizing film obtained from the composition is preferably 0.3 nm or more and 0.6 nm or less. The polymerizable liquid crystal compound or liquid crystal polymer compound may be a polymerizable smectic liquid crystal compound or a smectic liquid crystal polymer compound that shows a Bragg peak derived from a higher order structure in X-ray diffraction measurement.
[0038] Compound (1) can exhibit high dichroism even when dispersed among dense molecular chains formed from at least one of a smectic liquid crystal polymerizable liquid crystal compound and a smectic liquid crystal polymer compound. Therefore, a composition containing at least one of a polymerizable liquid crystal compound and a liquid crystal polymer compound, particularly at least one of a smectic liquid crystal polymerizable liquid crystal compound and a smectic liquid crystal polymer compound, and compound (1) can provide a polarizing film with a high dichroic ratio.
[0039] Polymerizable liquid crystal compound The polymerizable liquid crystal compound is a compound that has at least one polymerizable group in the molecule and can show a liquid crystal phase by being aligned. The polymerizable liquid crystal compound is preferably a compound that can show a liquid crystal phase by being aligned alone. The polymerizable group means a functional group that can be involved in a polymerization reaction, and is preferably a radical polymerizable group.
[0040] The polymerizable liquid crystal compound is not particularly limited as long as it has at least one polymerizable group and preferably exhibits smectic liquid crystal properties, and any known polymerizable liquid crystal compound can be used. Specific examples of the polymerizable liquid crystal compound include a compound represented by the following formula (A) (hereinafter, also referred to as "polymerizable liquid crystal compound (A)"). U 1 -V 1 -W 1 -(X 1 -Y 1 ) m -X 2 -Y 2 -X 3 -W 2 -V 2 -U 2 (A)
[0041] In formula (A), m is an integer from 1 to 3. 1 , X 2 and X 3 each independently represents a divalent aromatic group or a divalent alicyclic hydrocarbon group. When m is 2 or 3, X 1may be the same or different. X 1 , X 2 and X 3 At least three selected from the group consisting of Y represent a divalent 6-membered hydrocarbon ring group. 1 , Y 2 , W 1 and W 2 each independently represents a single bond or a divalent linking group. When m is 2 or 3, Y 1 may be the same or different. 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent. At least one of -CH2- constituting the alkanediyl group may be substituted with -O-, -CO-, -S- or -NH-. 1 and U 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them represents a polymerizable group.
[0042] X 1 , X 2 and X 3 In the above, examples of the divalent aromatic group include a 1,4-phenylene group and a 1,4-naphthylene group. Examples of the divalent alicyclic hydrocarbon group include a cyclohexane-1,4-diyl group. 1 , X 2 and X 3 At least one of the divalent aromatic group and the divalent alicyclic hydrocarbon group in the formula (I) may have a substituent. Examples of the substituent include an alkyl group having 1 to 4 carbon atoms, such as a methyl group, an ethyl group, or an n-butyl group, a cyano group, or a halogen atom. At least one of the -CH2- groups constituting the divalent alicyclic hydrocarbon group may be substituted with -O-, -S-, or -NR-. Here, R represents an alkyl group having 1 to 6 carbon atoms or a phenyl group.
[0043] X 1 , X 2 and X 3Examples of the divalent 6-membered hydrocarbon ring group in include an optionally substituted 1,4-phenylene group and an optionally substituted cyclohexane-1,4-diyl group.
[0044] X 1 , X 2 and X 3 The divalent aromatic group in is preferably a 1,4-phenylene group which may have a substituent, more preferably an unsubstituted 1,4-phenylene group, and the divalent alicyclic hydrocarbon group is preferably a cyclohexane-1,4-diyl group which may have a substituent, more preferably a trans-cyclohexane-1,4-diyl group which may have a substituent, and even more preferably an unsubstituted trans-cyclohexane-1,4-diyl group.
[0045] Y 1 and Y 2 each independently represents a single bond or a divalent linking group. Examples of the divalent linking group include -CH2CH2-, -CHO-, -(C=O)O-, -O(C=O)O-, -N=N-, -CR a =CR b -, -C≡C- and -CR a ═N-, where R a and R b Each of Y independently represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms. 1 is preferably -CH2CH2-, -(C=O)O- or a single bond. 2 is preferably -CH2CH2- or -CH2O-.
[0046] W 1 and W 2 Each of W independently represents a single bond or a divalent linking group. The divalent linking group is, for example, at least one selected from the group consisting of -O-, -S-, -(C=O)O-, and -O(C=O)O-. 1 and W 2 are each independently preferably a single bond or -O-.
[0047] V 1 and V 2 each independently represents an alkanediyl group having 1 to 20 carbon atoms which may have a substituent. At least one of -CH2- constituting the alkanediyl group may be replaced by -O-, -CO-, -S- or -NH-.
[0048] V 1 and V 2 Examples of the alkanediyl group represented by the formula (I) include a methylene group, an ethylene group, a propane-1,3-diyl group, a butane-1,3-diyl group, a butane-1,4-diyl group, a pentane-1,5-diyl group, a hexane-1,6-diyl group, a heptane-1,7-diyl group, an octane-1,8-diyl group, a decane-1,10-diyl group, a tetradecane-1,1-diyl group, and an icosane-1,20-diyl group. 1 and V 2 is preferably an alkanediyl group having 2 to 12 carbon atoms, and more preferably an alkanediyl group having 6 to 12 carbon atoms.
[0049] Examples of the substituent that the optionally substituted alkanediyl group having 1 to 20 carbon atoms may have include a cyano group and a halogen atom. The alkanediyl group is preferably an alkanediyl group having no substituent, and more preferably an alkanediyl group having no substituent and being linear.
[0050] U 1 and U 2 each independently represents a polymerizable group or a hydrogen atom, and at least one of them represents a polymerizable group. 1 and U 2 is preferably a polymerizable group. 1 and U 2 Preferably, both of U are polymerizable groups, and preferably both are radically polymerizable groups. 1 and a polymerizable group represented by U 2 The polymerizable groups represented by U may be different from each other, but are preferably the same type of group. 1 and U 2Examples of the polymerizable group in the polymerizable liquid crystal compound include the same polymerizable groups as those exemplified above. 1 and U 2 The polymerizable group represented by the formula (I) is preferably at least one selected from the group consisting of a vinyloxy group, an acryloyloxy group, a methacryloyloxy group, an oxiranyl group, and an oxetanyl group, and more preferably an acryloyloxy group.
[0051] Specific examples of the polymerizable liquid crystal compound (A) include compounds represented by the following formulae (A-1) to (A-17). When the polymerizable liquid crystal compound (A) has a cyclohexane-1,4-diyl group, the cyclohexane-1,4-diyl group is preferably a trans type.
[0052] [ka]
[0053] [ka]
[0054] [ka]
[0055] Among them, the polymerizable liquid crystal compound (A) is preferably at least one selected from the group consisting of compounds represented by any of formulas (A-2), (A-3), (A-4), (A-5), (A-6), (A-7), (A-8), (A-13), (A-14), (A-15), (A-16) and (A-17). The polymerizable liquid crystal compound (A) may be used alone or in combination of two or more.
[0056] The polymerizable liquid crystal compound (A) can be produced by the method described in the known documents such as Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996) and Japanese Patent No. 4719156.
[0057] Liquid crystal polymer The liquid crystalline polymer compound may be a compound obtained by polymerizing the polymerizable liquid crystal compound (hereinafter, also referred to as a polymer of the polymerizable liquid crystal compound), or may be another liquid crystalline polymer compound, and is preferably a polymer of the polymerizable liquid crystal compound.
[0058] The polymer of the polymerizable liquid crystal compound may use two or more of the polymerizable liquid crystal compounds as raw material monomers. The polymer of the polymerizable liquid crystal compound may also contain a monomer other than the polymerizable liquid crystal compound as a raw material monomer.
[0059] The content of the polymerizable liquid crystal compound in the polymer of the polymerizable liquid crystal compound is usually 1 mol % or more and 100 mol % or less, based on the total amount of structural units derived from the polymerizable liquid crystal compound that constitute the polymer of the polymerizable liquid crystal compound. From the viewpoint of increasing the orientation of the polymer of the polymerizable liquid crystal compound, the content is preferably 30 mol % or more and 100 mol % or less, more preferably 50 mol % or more and 100 mol %, and even more preferably 80 mol % or more and 100 mol % or less.
[0060] The other liquid crystal polymer compounds include polymer compounds having liquid crystal groups.For example, the polymer compounds that become the backbone include polyolefins such as polyethylene and polypropylene; cyclic olefin resins such as norbornene polymers; polyalkylene ethers, polyvinyl alcohols; polymethacrylic acid esters; polyacrylic acid esters; and the like, and these polymer compounds have liquid crystal groups.Among them, polymethacrylic acid esters and polyacrylic acid esters having liquid crystal groups are preferred.
[0061] The other liquid crystal polymer compound may contain two or more kinds of liquid crystal groups. The liquid crystal group may be contained in the main chain of the polymer compound which is the mother skeleton, may be contained in the side chain of the polymer compound which is the mother skeleton, or may be contained in both the main chain and the side chain of the polymer compound which is the mother skeleton. The liquid crystal group may be a group formed by removing one hydrogen atom from a compound having at least two 6-membered hydrocarbon ring structures, or a group formed by removing two hydrogen atoms from the compound.
[0062] The content of the liquid crystalline group in the other liquid crystalline polymer compound is usually 1 mol % or more and 100 mol % or less, based on the total amount of the structural units constituting the polymer compound that is the parent skeleton of the other liquid crystalline polymer compound. From the viewpoint of increasing the orientation of the other liquid crystalline polymer compound, the content is preferably 30 mol % or more and 100 mol % or less, more preferably 50 mol % or more and 100 mol % or less, and even more preferably 80 mol % or more and 100 mol % or less.
[0063] In the case where two or more kinds of polymerizable liquid crystal compounds are combined in the composition, it is preferable that at least one of them is a polymerizable liquid crystal compound (A), and more preferable that two or more of them are polymerizable liquid crystal compounds (A). By combining two or more kinds of polymerizable liquid crystal compounds, the liquid crystal phase may be temporarily maintained even at a temperature below the liquid crystal-crystal phase transition temperature. The content of the polymerizable liquid crystal compound (A) contained in the composition is preferably 40 mass% or more, more preferably 60 mass% or more, in total, based on the total mass of all the polymerizable liquid crystal compounds in the composition, and all the polymerizable liquid crystal compounds may be polymerizable liquid crystal compounds (A). When the content of the polymerizable liquid crystal compound (A) is within the above range, the polymerizable liquid crystal compounds are easily aligned with a high degree of orientation order, and the compound represented by formula (1) is aligned along the alignment, so that a polarizing film having excellent polarization performance can be obtained.
[0064] From the viewpoint of increasing the orientation of the polymerizable liquid crystal compound and the liquid crystal polymer compound, the total content of the polymerizable liquid crystal compound and the liquid crystal polymer compound in the composition is, for example, 50 parts by mass or more, preferably 70 parts by mass or more and 99.9 parts by mass or less, more preferably 70 parts by mass or more and 99.5 parts by mass or less, even more preferably 80 parts by mass or more and 99 parts by mass or less, particularly preferably 80 parts by mass or more and 94 parts by mass or less, and even more preferably 80 parts by mass or more and 90 parts by mass or less, relative to 100 parts by mass of the solid content of the composition.
[0065] The content of compound (1) in the composition is usually 0.1 to 50 parts by mass, preferably 0.1 to 20 parts by mass, more preferably 0.1 to 10 parts by mass, and even more preferably 0.1 to 5 parts by mass, relative to 100 parts by mass of the total amount of the polymerizable liquid crystal compound and the liquid crystal polymer compound. When the content of compound (1) is 50 parts by mass or less relative to the total amount of the polymerizable liquid crystal compound and the liquid crystal polymer compound, there is a tendency that the orientation disorder of the polymerizable liquid crystal compound, the liquid crystal polymer compound, and compound (1) is small, and a polarizing film having a high degree of orientation order can be obtained.
[0066] polymer compound The composition may further contain a polymer compound in addition to the compound (1), the polymerizable liquid crystal compound, and the liquid crystal polymer compound. When the composition contains a polymer compound, the compound (1) may be easily dispersed in the composition. The polymer compound that the composition may contain is not particularly limited as long as it can disperse the compound (1). In terms of easiness in uniformly dispersing the compound (1), an acrylic polymer such as polymethyl methacrylate (PMMA) is preferable. The polymer compound may also be a polymer compound obtained by polymerizing the above-mentioned polymerizable liquid crystal compound. The weight average molecular weight of the polymer compound in terms of polystyrene is, for example, 10,000 to 200,000, preferably 20,000 to 150,000.
[0067] When the composition contains a polymer compound, the content thereof can be appropriately selected depending on the purpose, etc. The content of the polymer compound is preferably 10 parts by mass or less, more preferably 5.0 parts by mass or less, and even more preferably 3.0 parts by mass or less, relative to 100 parts by mass of the solid content of the composition.
[0068] The composition preferably further contains a liquid medium such as a solvent and a polymerization initiator, and may further contain a photosensitizer, a polymerization inhibitor, a leveling agent, etc., as necessary.
[0069] solvent The solvent is preferably a solvent capable of completely dissolving the compound (1), the polymerizable liquid crystal compound, the liquid crystalline polymer compound, and the polymer compound, and is preferably a solvent inactive to the polymerization reaction of the polymerizable liquid crystal compound.
[0070] Examples of the solvent include alcohol solvents, ester solvents, ketone solvents, aliphatic hydrocarbon solvents, aromatic hydrocarbon solvents, nitrile solvents, ether solvents, chlorine-containing solvents, etc. These solvents may be used alone or in combination of two or more.
[0071] When the composition contains a solvent, the content of the solvent is preferably 50% by mass or more and 98% by mass or less with respect to the total amount of the composition. In other words, the content of the solid content in the composition is preferably 2% by mass or more and 50% by mass or less. When the solid content is 50% by mass or less, the viscosity of the composition is low, and the thickness of the film obtained from the composition, for example, the film, tends to be approximately uniform, and the film tends to be less likely to have unevenness. The content of the solid content can be determined in consideration of the thickness of the film to be produced.
[0072] Polymerization initiator The polymerization initiator is a compound capable of initiating the polymerization reaction of the polymerizable liquid crystal compound. The polymerization initiator is preferably a photopolymerization initiator, since it can initiate the polymerization reaction under lower temperature conditions. Specifically, a photopolymerization initiator capable of generating active radicals or acids by the action of light is exemplified, and among them, a photopolymerization initiator capable of generating radicals by the action of light is preferred.
[0073] Examples of the polymerization initiator include benzoin compounds, benzophenone compounds, alkylphenone compounds, acylphosphine oxide compounds, triazine compounds, iodonium salts, and sulfonium salts. The polymerization initiator can be appropriately selected from known polymerization initiators according to the purpose. The polymerization initiator can be used alone or in combination of two or more.
[0074] When the composition contains a polymerization initiator, the content of the polymerization initiator may be appropriately determined according to the type and amount of the polymerizable liquid crystal compound contained in the composition. The content of the polymerization initiator is, for example, 0.001 parts by mass or more, 0.01 parts by mass or more, 0.1 parts by mass or more, or 0.5 parts by mass or more, and is, for example, 30% by mass or less, 10% by mass or less, or 8% by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound. The content of the polymerization initiator is preferably 0.001 parts by mass or more and 30 parts by mass or less, more preferably 0.01 parts by mass or more and 10 parts by mass or less, and even more preferably 0.1 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound. When the content of the polymerization initiator is within the above range, the polymerizable liquid crystal compound can be polymerized without disturbing the orientation.
[0075] Photosensitizers When the composition contains a photopolymerization initiator, the composition may preferably contain at least one type of photosensitizer. The composition contains a photopolymerization initiator and a photosensitizer, which tends to promote the polymerization reaction of the polymerizable liquid crystal compound. Examples of the photosensitizer include xanthone compounds such as xanthone and thioxanthone; anthracene compounds such as anthracene and alkoxy-substituted anthracene; phenothiazine and rubrene; and the like. The photosensitizer can be used alone or in combination of two or more types.
[0076] When the composition contains a photosensitizer, the content of the photosensitizer in the composition may be appropriately determined according to the type and amount of the photopolymerization initiator and the polymerizable liquid crystal compound. The content of the photosensitizer in the composition is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 10 parts by mass or less, and even more preferably 0.5 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0077] Polymerization Inhibitor The composition may contain at least one type of polymerization inhibitor. Examples of the polymerization inhibitor include radical scavengers such as hydroquinone, alkoxy group-containing hydroquinone, alkoxy group-containing catechol (e.g., butylcatechol), pyrogallol, and 2,2,6,6-tetramethyl-1-piperidinyloxy radical; thiophenols; β-naphthylamines and β-naphthols; and the like. The composition contains a polymerization inhibitor, so that the degree of progress of the polymerization reaction of the polymerizable liquid crystal compound can be controlled.
[0078] When the composition contains a polymerization inhibitor, the content of the polymerization inhibitor in the composition is preferably 0.1 parts by mass or more and 30 parts by mass or less, more preferably 0.5 parts by mass or more and 10 parts by mass or less, and even more preferably 0.5 parts by mass or more and 8 parts by mass or less, relative to 100 parts by mass of the polymerizable liquid crystal compound.
[0079] Leveling Agent The composition may contain at least one leveling agent. The leveling agent has the function of adjusting the fluidity of the composition and making the coating film obtained by applying the composition flatter, and specifically includes a surfactant. As the leveling agent, at least one selected from the group consisting of leveling agents mainly composed of a polyacrylate compound and leveling agents mainly composed of a fluorine atom-containing compound is preferable. The leveling agent may be used alone or in combination of two or more kinds.
[0080] When the composition contains a leveling agent, the content of the leveling agent is preferably 0.05 parts by mass or more and 5 parts by mass or less, more preferably 0.05 parts by mass or more and 3 parts by mass or less, relative to 100 parts by mass of the total amount of the polymerizable liquid crystal compound and the liquid crystal polymer compound. When the content of the leveling agent is within the above range, the polymerizable liquid crystal compound and the liquid crystal polymer compound are easily horizontally aligned, and unevenness is unlikely to occur, and a smoother film, such as a polarizing film, tends to be obtained.
[0081] When the content of the leveling agent is within the above range, the polymerizable liquid crystal compound and the liquid crystalline polymer compound are easily horizontally aligned, and the obtained film tends to be smoother. When the content of the leveling agent relative to the polymerizable liquid crystal compound and the liquid crystalline polymer compound exceeds the above range, the obtained film tends to be easily uneven.
[0082] Antioxidants The composition may contain an antioxidant. The antioxidant is not particularly limited as long as the composition can exhibit the effects of the present invention, and known antioxidants can be used. From the viewpoint of having a high inhibitory effect against photodegradation of compound (1), the antioxidant is preferably a so-called primary antioxidant that has an action of preventing autoxidation by capturing radicals. Therefore, it is more preferable that the antioxidant contained in the composition is at least one selected from the group consisting of phenolic compounds, alicyclic alcohol compounds, and amine compounds. The antioxidant may be used alone or in combination of two or more kinds.
[0083] The content of the antioxidant in the composition is preferably 0.1 parts by mass or more and 15 parts by mass or less, more preferably 0.3 parts by mass or more, even more preferably 0.5 parts by mass or more, more preferably 12 parts by mass or less, and even more preferably 10 parts by mass or less, relative to 100 parts by mass of the composition. When the content of the antioxidant is equal to or more than the lower limit, the photodegradation of compound (1) can be more effectively suppressed. When the content of the antioxidant is equal to or less than the upper limit, the alignment of the polymerizable liquid crystal compound is less likely to be disturbed, and a higher effect of suppressing the photodegradation of compound (1) can be expected.
[0084] The composition may contain additives other than those described above. Examples of the additives include a release agent, a stabilizer, a colorant such as a bluing agent, a flame retardant, and a lubricant. When the composition contains other additives, the content of the other additives is preferably more than 0% and not more than 20% by mass, more preferably more than 0% and not more than 10% by mass, based on the solid content of the composition.
[0085] The composition can be produced by a conventionally known method for preparing a composition, for example, by mixing and stirring compound (1), a liquid crystal compound, and, if necessary, additives such as an antioxidant and a leveling agent.
[0086] <Compound> The compound according to this embodiment is represented by the following formula (1a) and has a maximum absorption wavelength in the wavelength range of 370 nm to 470 nm. The compound represented by the following formula (1a) (hereinafter also referred to as compound (1a)) may be used as a material for forming a polarizing film as a dichroic dye, for example. That is, compound (1a) may be an active ingredient constituting a dichroic dye. A polarizing plate having a polarizing film containing compound (1a) can achieve an excellent dichroic ratio (DR).
[0087] [ka]
[0088] In formula (1a), y represents 1 or 2, preferably 1. When y is 2, two Ar 13 may be the same or different.
[0089] R 11 and R 12 R each independently represents an alkyl group, an alkoxy group, an alkoxycarbonyl group, or an alkanoyloxy group, preferably an alkyl group, an alkoxy group, or an alkoxycarbonyl group, and more preferably an alkyl group or an alkoxy group. 11 or R 12 In the group represented by the formula (I), at least one of the hydrogen atoms of these groups may be substituted with a polymerizable group. 11 and R 12 A preferred embodiment of the formula is R 1 and R 2 is the same as:
[0090] Ar 11 , Ar 12 and Ar 13 each independently represents a divalent aromatic group selected from the group consisting of a thiazoldiyl group, a benzothiazoldiyl group, and a 1,4-phenylene group. 11 , Ar 12 and Ar 13 At least one of is a thiazoldiyl group or a benzothiazoldiyl group, preferably a benzothiazoldiyl group. Also preferably, at least Ar 11 is a benzothiazolediyl group. 11 , Ar 12 or Ar 13 The divalent aromatic group represented by the following formula (I) may be substituted with at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group.
[0091] Specific examples of compound (1a) include compounds represented by any one of formulas (1-1) to (1-36) described above, but the present invention is not limited thereto. From the viewpoint of dichroic ratio, compound (1a) is preferably at least one selected from the group consisting of compounds represented by any one of formulas (1-1) to (1-33), and more preferably at least one selected from the group consisting of compounds represented by any one of formulas (1-1) to (1-23).
[0092] Compound (1a) may have a maximum absorption wavelength (λmax) in the wavelength range of, for example, 370 nm or more and 470 nm or less. The maximum absorption wavelength of compound (1a) may be preferably 400 nm or more and 470 nm or less, more preferably 420 nm or more and 460 nm or less. The upper limit and the lower limit of the above range can be combined arbitrarily.
[0093] <Membrane> The film according to the present embodiment is formed from a composition containing compound (1) and a liquid crystal compound. The film made of the composition may be formed by applying the composition to a substrate and forming a film. In addition, when the composition contains a polymerizable liquid crystal compound, the film containing a cured product obtained by polymerizing the polymerizable liquid crystal compound may be formed by applying the composition to a substrate, forming a film, and then polymerizing and curing the polymerizable liquid crystal compound.
[0094] The composition can form a film having a high degree of orientational order, such as a polarizing film. Therefore, the film according to the present embodiment is a polarizing film formed from a composition containing compound (1) and a liquid crystal compound, and includes a polarizing film having a high degree of orientational order.
[0095] Here, in a polarizing film with a high degree of orientational order, a Bragg peak derived from a higher-order structure such as a hexatic phase or a crystalline phase is obtained in an X-ray diffraction measurement. Therefore, in a polarizing film formed from the composition, it is preferable that the polymerizable liquid crystal compound or the liquid crystalline polymer compound is oriented so as to show a Bragg peak in an X-ray diffraction measurement, and it is more preferable that the molecules of the polymerizable liquid crystal compound or the liquid crystalline polymer compound are oriented in the direction in which light is absorbed, that is, "horizontal orientation". A high degree of orientational order that shows a Bragg peak can be achieved by controlling the type of the polymerizable liquid crystal compound or the liquid crystalline polymer compound used, the amount of compound (1), etc.
[0096] The compound (1) and the liquid crystal compound constituting the composition used to form the film are as described above.
[0097] The membrane can be produced, for example, by a method comprising the following steps. Step A: forming a coating film of a composition containing compound (1), a liquid crystalline compound, and a solvent; Step B: Removing at least a portion of the solvent from the coating; Step C: raising the temperature to a temperature at which the liquid crystalline compound undergoes a phase transition to a liquid phase or higher, and then lowering the temperature to cause the liquid crystalline compound to undergo a phase transition to a smectic phase (smectic liquid crystal state); and Step D: If necessary, polymerizing the polymerizable liquid crystal compound while maintaining the smectic phase (smectic liquid crystal state).
[0098] The coating film of the composition can be formed, for example, by applying the composition onto a substrate, an alignment film described later, etc. Alternatively, the composition may be directly applied onto a retardation film or other layer constituting a polarizing plate.
[0099] The substrate is usually a transparent substrate. When the substrate is not placed on the display surface of a display element, for example, when a laminate obtained by removing the substrate from the film is placed on the display surface of a display element, the substrate does not have to be transparent. The transparent substrate means a substrate having transparency capable of transmitting light, particularly visible light, and the transparency means a property in which the transmittance of light in the wavelength range of 380 nm to 780 nm is 80% or more. A specific example of a transparent substrate is a translucent resin substrate.
[0100] Examples of resins constituting the light-transmitting resin substrate include polyolefins, cyclic olefin resins, polyvinyl alcohol, polyethylene terephthalate, polymethacrylic acid esters, polyacrylic acid esters, cellulose esters, polyethylene naphthalate, polycarbonates, polysulfones, polyethersulfones, polyether ketones, polyphenylene sulfide, and polyphenylene oxide. From the viewpoints of availability and transparency, polyethylene terephthalate, polymethacrylic acid esters, cellulose esters, cyclic olefin resins, and polycarbonates are preferred.
[0101] The properties required for the substrate vary depending on the film configuration, but generally, a substrate with as small a retardation as possible is preferred. Examples of substrates with as small a retardation as possible include cellulose ester films with no retardation, such as Zerotack (Konica Minolta Opto, Inc.) and Z-tack (FUJIFILM Corporation). Unstretched cyclic olefin resin substrates are also preferred. The surface of the substrate on which the film is not laminated may be subjected to hard coat treatment, antireflection treatment, antistatic treatment, etc.
[0102] The thickness of the substrate is usually 5 μm or more and 300 μm or less, preferably 20 μm or more and 200 μm or less, and more preferably 20 μm or more and 100 μm or less. If the thickness is equal to or more than the lower limit, the decrease in strength is suppressed and the processability tends to be good.
[0103] Examples of a method for applying the composition to a substrate or the like include known methods such as coating methods such as spin coating, extrusion, gravure coating, die coating, bar coating, and applicator methods, and printing methods such as flexography.
[0104] Next, at least a part of the solvent contained in the coating film obtained from the composition is removed by drying or the like to form a dry coating film. When the coating film contains a polymerizable liquid crystal compound, the coating film is dried under conditions in which the polymerizable liquid crystal compound does not polymerize to form a dry coating film. Examples of the drying method for the coating film include natural drying, ventilation drying, heat drying, and reduced pressure drying.
[0105] Furthermore, in order to cause the liquid crystal compound to undergo a phase transition to a liquid phase, the temperature is raised to a temperature at which the liquid crystal compound undergoes a phase transition to a liquid phase or higher, and then the temperature is lowered to cause the liquid crystal compound to undergo a phase transition to a smectic phase (smectic liquid crystal state). Such a phase transition may be performed after the solvent in the coating film is removed, or may be performed simultaneously with the removal of the solvent.
[0106] When the composition contains a polymerizable liquid crystal compound, the polymerizable liquid crystal compound is polymerized while maintaining the smectic liquid crystal state of the polymerizable liquid crystal compound, thereby forming a film containing a cured product of the polymerizable liquid crystal compound. The polymerization method is preferably a photopolymerization method. In photopolymerization, the light to be irradiated to the dried coating film is appropriately selected according to the type of photopolymerization initiator contained in the dried coating film, the type of polymerizable liquid crystal compound (particularly, the type of polymerizable group possessed by the polymerizable liquid crystal compound) and the amount thereof. Specific examples thereof include one or more types of light selected from the group consisting of visible light, ultraviolet light, infrared light, X-rays, α-rays, β-rays and γ-rays, active electron beams, etc. Among them, ultraviolet light is preferred in that the progress of the polymerization reaction is easily controlled and that photopolymerization devices widely used in this field can be used. It is preferable to select the type of polymerizable liquid crystal compound and photopolymerization initiator contained in the composition so that photopolymerization is possible by ultraviolet light. In addition, the polymerization temperature can also be controlled by irradiating light while cooling the dried coating film with an appropriate cooling means during polymerization. By adopting such a cooling means, the polymerization of the polymerizable liquid crystal compound can be performed at a lower temperature, and even if a substrate having a relatively low heat resistance is used, a film can be appropriately formed. During photopolymerization, a patterned film can be obtained by performing masking and development.
[0107] Examples of the light source of the active energy rays include a low-pressure mercury lamp, a medium-pressure mercury lamp, a high-pressure mercury lamp, an ultra-high-pressure mercury lamp, a xenon lamp, a halogen lamp, a carbon arc lamp, a tungsten lamp, a gallium lamp, an excimer laser, an LED light source emitting light in the wavelength range of 380 nm or more and 440 nm or less, a chemical lamp, a black light lamp, a microwave-excited mercury lamp, and a metal halide lamp.
[0108] The UV irradiation intensity is usually 10mW / cm 2 More than 3,000mW / cm 2The ultraviolet irradiation intensity is preferably an intensity in a wavelength region effective for activating a photopolymerization initiator. The time for irradiating light may be usually 0.1 seconds or more and 10 minutes or less, preferably 0.1 seconds or more and 5 minutes or less, more preferably 0.1 seconds or more and 3 minutes or less, and further preferably 0.1 seconds or more and 1 minute or less. When irradiating once or multiple times with such ultraviolet irradiation intensity, the integrated light amount is 10 mJ / cm 2 More than 3,000mJ / cm 2 It is preferable that:
[0109] By carrying out photopolymerization, the polymerizable liquid crystal compound is polymerized while maintaining the liquid crystal state of the smectic phase, preferably the high-order smectic phase, to form a film. The film obtained by polymerizing the polymerizable liquid crystal compound while maintaining the liquid crystal state of the smectic phase has the advantage of having higher polarization performance due to the action of the dichroic dye, compared to conventional host-guest type polarizing films, that is, films made of a liquid crystal state of a nematic phase. Furthermore, it has the advantage of being superior in strength compared to films coated with only a dichroic dye or a lyotropic liquid crystal.
[0110] The thickness of the film can be appropriately selected depending on the display device to which it is applied, and is preferably 0.5 μm or more and 10 μm or less, more preferably 1 μm or more and 5 μm or less, and further preferably 1 μm or more and 3 μm or less.
[0111] When the film is used as a polarizing film, it is preferable that the film is formed on an alignment film. The alignment film has an alignment regulating force that causes the polymerizable liquid crystal compound and the liquid crystal polymer compound to be aligned in a desired direction. The alignment film is preferably one that has solvent resistance that does not dissolve when a composition containing at least one of the polymerizable liquid crystal compound and the liquid crystal polymer compound is applied, and also has heat resistance in a heat treatment for removing the solvent or orienting the polymerizable liquid crystal compound. Examples of such alignment films include alignment films containing an alignment polymer, photo-alignment films, and groove alignment films having a concave-convex pattern or a plurality of grooves on the surface, and photo-alignment films are preferable from the viewpoint of the accuracy and quality of the alignment angle.
[0112] <Laminate> The laminate according to the present embodiment includes a film containing a composition containing the compound (1) and a liquid crystal compound as a forming material. The laminate may include a substrate and a film containing the composition as a forming material disposed on the substrate, or may include a substrate, an alignment film disposed on the substrate, and a film containing the composition as a forming material disposed on the alignment film. The film containing the composition as a forming material may constitute a polarizing film. The substrate may be a retardation film. The laminate may constitute, for example, a polarizing plate. The laminate may be manufactured, for example, by forming a film on the substrate in accordance with the above-mentioned method for manufacturing the film.
[0113] From the viewpoint of flexibility and visibility of the display device, the thickness of the laminate is preferably from 10 μm to 300 μm, more preferably from 20 μm to 200 μm, and further preferably from 25 μm to 100 μm.
[0114] When the laminate includes a retardation film as the substrate, the thickness of the retardation film can be appropriately selected depending on the display device to which it is applied.
[0115] <Display device> The display device of the present embodiment includes the laminate, and the laminate may be a polarizing plate. The display device can be obtained, for example, by bonding the laminate as a polarizing plate to the surface of the display device via a pressure-sensitive adhesive layer. The display device is a device having a display element, and is a device including a light-emitting element or a light-emitting device as a light-emitting source. Examples of the display device include a liquid crystal display device, an organic electroluminescence (EL) display device, an inorganic electroluminescence (EL) display device, an electron emission display device (e.g., a field emission display device (FED), a surface field emission display device (SED)), electronic paper (a display device using electronic ink, an electrophoretic element, etc.), a plasma display device, a projection display device (e.g., a display device having a grating light valve (GLV) display device, a digital micromirror device (DMD)), and a piezoelectric ceramic display. The liquid crystal display device includes any of a transmissive liquid crystal display device, a semi-transmissive liquid crystal display device, a reflective liquid crystal display device, a direct-view liquid crystal display device, and a projection liquid crystal display device. These display devices may be a display device that displays a two-dimensional image, or a stereoscopic display device that displays a three-dimensional image. In particular, as the display device, an organic EL display device and a touch panel display device are preferable, and an organic EL display device is particularly preferable. EXAMPLES
[0116] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples.
[0117] Synthesis Example 1 Synthesis of compound (1-1) To synthesize compound (1-1), compound (1-1-a) was first synthesized into compound (1-1-b), which was then alkylated to obtain compound (1-1).
[0118] Synthesis of compound (1-1-a) 6-Methoxybenzo[d]thiazol-2-amine (9.01g, 50.0mmol), acetic acid (30.0mL), water (70.0mL), and sulfuric acid (4.0mL, 75mmol) were mixed and cooled to 0°C to 5°C, and a 40% sulfuric acid solution of nitrosylsulfuric acid (31.8g, 100mmol) was added dropwise thereto. After that, the mixture was stirred for 30 minutes while maintaining the temperature at 0°C to 5°C, and amidosulfuric acid (4.85g, 50.0mmol) was added to prepare a diazo solution. On the other hand, sodium (phenylamino)methanesulfonate (11.6g, 55.0mmol) and water (300mL) were mixed and cooled to 0°C to 5°C, and the entire amount of the diazo solution prepared earlier was added dropwise. After the dropwise addition, the mixture was heated to room temperature, and the precipitated solid was collected by filtration and washed with acetonitrile to obtain a black solid. The obtained solid, sodium hydroxide (5.96 g, 149 mmol), and water (300 mL) were mixed and heated with stirring at 90° C. for 2 hours. The precipitated solid was collected by filtration to obtain compound (1-1-a) (8.61 g, yield 61%).
[0119] [ka]
[0120] Synthesis of compound (1-1-b) Compound (1-1-a) (5.69 g, 20.0 mmol), 35% hydrochloric acid (5.9 mL, 67 mmol), acetic acid (48.0 mL), and water (8.0 mL) were mixed and cooled to 0 to 5 ° C., and a solution of sodium nitrite (4.14 g, 60.0 mmol) in water (6.0 mL) was added dropwise thereto. After that, the mixture was stirred for 30 minutes while maintaining the temperature at 0 to 5 ° C., and amidosulfuric acid (3.88 g, 40.0 mmol) was added to prepare a diazo liquid. Meanwhile, phenol (5.64 g, 60.0 mmol), sodium acetate (9.85 g, 120 mmol), and water (140 mL) were mixed and cooled to 0 to 5 ° C., and the entire amount of the diazo liquid prepared earlier was added dropwise thereto. After the dropwise addition was completed, the temperature was raised to room temperature, and the precipitated solid was filtered off to obtain compound (1-1-b) (7.11 g, yield 91%).
[0121] [ka]
[0122] Synthesis of compound (1-1) Compound (1-1-b) (0.300 g, 0.770 mmol), 2-methylbutyl p-toluenesulfonate (0.75 g, 3.1 mmol), potassium carbonate (0.43 g, 3.1 mmol), and N,N-dimethylacetamide (5.0 g) were mixed and heated and stirred at 90° C. for 2 hours. Water was added to the reaction solution, and the precipitated solid was filtered and washed with methanol. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (1-1) (0.28 g, yield 79%).
[0123] [ka]
[0124] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.20-8.17(m,2H),8.08(d,1H),8.06-8.03(m,2H),7.98-7.94(m,2H),7.33(d,1H),7.14(dd,1H),7.05-7.01( m,2H),3.95-3.91(m,1H),3.93(s,3H),3.87-3.83(m,1H),1.98-1.86( m,1H),1.66-1.55(m,1H),1.37-1.26(m,1H),1.05(d,2H),0.98(t,3H). UV-visible spectrum: λmax = 453 nm (in acetonitrile)
[0125] Synthesis Example 2: Synthesis of Compound (1-2) Compound (1-1-b) (3.70 g, 9.50 mmol), 1-bromo-2-methylpropane (2.62 g, 19.1 mmol), potassium carbonate (3.94 g, 28.5 mmol), and N,N-dimethylacetamide (47.5 mL) were mixed and heated and stirred at 90° C. for 4 hours. Methanol was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (1-2) (1.93 g, yield 46%).
[0126] [ka]
[0127] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.21-8.17(m,2H),8.08(d,1H),8.06-8.03(m,2H),7.99-7.95(m,2H),7 .34(d,1H),7.15(dd,1H),7.05-7.01(m,2H),3.93(s,3H),3.83(d,2H),2.19-2.09(m,1H),1.07(d,6H). UV-visible spectrum: λmax = 452 nm (in acetonitrile)
[0128] Synthesis Example 3: Synthesis of compound (1-3) Compound (1-1-b) (0.586 g, 1.50 mmol), 1-bromo-3-methylbutane (0.453 g, 3.01 mmol), potassium carbonate (0.622 g, 4.50 mmol), and N,N-dimethylacetamide (7.5 mL) were mixed and heated and stirred at 100° C. for 1 hour. Methanol was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (1-3) (0.397 g, yield 57%).
[0129] [ka]
[0130] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.21-8.17(m,2H),8.08(d,1H),8.06-8.03(m,2H),7.99-7.95(m,2H),7.34(d ,1H),7.15(dd,1H),7.05-7.01(m,2H),4.10(t,2H),3.93(s,3H),1.92-1.83(m,1H),1.74(q,2H),1.00(d,6H). UV-visible spectrum: λmax = 452 nm (in acetonitrile)
[0131] Synthesis Example 4: Synthesis of compound (1-4) Compound (1-1-b) (0.585 g, 1.50 mmol), 2-propanol (0.25 mL, 3.2 mmol), triphenylphosphine (0.473 g, 1.80 mmol), 1.9 M toluene solution of diisopropyl azodicarboxylate (0.85 mL, 1.6 mmol), and THF (9.5 mL) were mixed and stirred at room temperature for 2 hours. Methanol was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (1-4) (0.268 g, yield 41%).
[0132] [ka]
[0133] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.21-8.17(m,2H),8.08(d,1H),8.06-8.03(m,2H),7.99-7.95( m,2H),7.34(d,1H),7.15(dd,1H),7.05-7.01(m,2H),4.69(sep,1H),3.93(s,3H),1.41(d,6H). UV-visible spectrum: λmax = 455 nm (in acetonitrile)
[0134] Synthesis Example 5: Synthesis of Compound (1-5) To synthesize compound (1-5), compound (1-5-a) was first synthesized via compound (1-5-b), which was then alkylated to obtain compound (1-5).
[0135] Synthesis of compound (1-5-a) 6-Ethoxybenzo[d]thiazol-2-amine (9.71g, 50.0mmol), acetic acid (70.0mL), water (70.0mL), and sulfuric acid (4.0mL, 75mmol) were mixed and cooled to 0°C to 5°C, and a 40% sulfuric acid solution of nitrosylsulfuric acid (31.8g, 100mmol) was added dropwise thereto. After that, the mixture was stirred for 30 minutes while maintaining the temperature at 0°C to 5°C, and amidosulfuric acid (4.85g, 50.0mmol) was added to prepare a diazo liquid. On the other hand, sodium (phenylamino)methanesulfonate (11.5g, 55.1mmol) and water (300mL) were mixed and cooled to 0°C to 5°C, and the entire amount of the diazo liquid prepared earlier was added dropwise. After the dropwise addition, the mixture was heated to room temperature, and the precipitated solid was collected by filtration and washed with acetonitrile to obtain a black solid. The obtained solid, sodium hydroxide (6.00 g, 150 mmol), and water (300 mL) were mixed and heated and stirred at 90° C. for 2 hours. The precipitated solid was collected by filtration to obtain compound (1-5-a) (8.48 g, yield 57%).
[0136] [ka]
[0137] Synthesis of compound (1-5-b) Compound (1-5-a) (5.97 g, 20.0 mmol), 35% hydrochloric acid (5.9 mL, 67 mmol), acetic acid (48.0 mL), and water (8.0 mL) were mixed and cooled to 0 to 5 ° C., and a solution of sodium nitrite (4.14 g, 60.0 mmol) in water (6.0 mL) was added dropwise thereto. After that, the mixture was stirred for 30 minutes while maintaining the temperature at 0 to 5 ° C., and amidosulfuric acid (3.89 g, 40.1 mmol) was added to prepare a diazo solution. Meanwhile, phenol (5.65 g, 60.0 mmol), sodium acetate (9.84 g, 120 mmol), and water (140 mL) were mixed and cooled to 0 to 5 ° C., and the entire amount of the diazo solution prepared earlier was added dropwise thereto. After the dropwise addition was completed, the temperature was raised to room temperature, and the precipitated solid was filtered off to obtain compound (1-5-b) (7.01 g, yield 87%).
[0138] [ka]
[0139] Synthesis of compound (1-5) Compound (1-5-b) (0.400 g, 0.991 mmol), 2-methylbutyl p-toluenesulfonate (0.96 g, 4.0 mmol), potassium carbonate (0.55 g, 4.0 mmol), and N,N-dimethylacetamide (5.0 g) were mixed and heated and stirred at 90° C. for 2 hours. Water was added to the reaction solution, and the precipitated solid was filtered and washed with methanol. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent to obtain compound (1-5) (0.24 g, yield 51%).
[0140] [ka]
[0141] 1H-NMR (400MHz, CDCl3): δ(ppm)=8.20-8.17(m,2H),8.07(d,1H),8.06-8.0 3(m,2H),7.98-7.94(m,2H),7.32(d,1H),7.13(dd,1H),7.05-7.01(m,2H) ,4.15(q,2H),3.95-3.91(m,1H),3.87-3.83(m,1H),1.98-1.86(m,1H),1. 66-1.55(m,1H),1.49(t,3H),1.36-1.25(m,1H),1.05(d,2H),0.98(t,3H). UV-visible spectrum: λmax = 455 nm (in acetonitrile)
[0142] Synthesis Example 6: Synthesis of compound (1-6) To synthesize compound (1-6), compound (1-6-a) was first synthesized via compound (1-6-b), which was then alkylated to obtain compound (1-6).
[0143] Synthesis of compound (1-6-a) Sodium nitrite (1.04g, 15.0mmol) was added little by little to sulfuric acid (12.0mL), and the mixture was heated and stirred at 50℃ for 15 minutes to prepare sodium nitrosyl sulfate solution. 6-n-Butylbenzo[d]thiazol-2-amine (2.06g, 10.0mmol), acetic acid (40.0mL), water (10.0mL), and sulfuric acid (0.80mL, 15mmol) were mixed and cooled to 0℃ to 5℃, and the entire amount of the sodium nitrosyl sulfate solution prepared earlier was added dropwise to the mixture. The mixture was then stirred for 15 minutes while maintaining the temperature at 0℃ to 5℃, and a solution of amidosulfuric acid (0.86g, 5.00mmol) in water (3.0mL) was added to prepare a diazo solution. On the other hand, sodium (phenylamino)methanesulfonate (3.14 g, 15.0 mmol) and water (40.0 mL) were mixed and cooled to 0 to 5°C, and the entire amount of the diazo solution prepared earlier was added dropwise. After the addition was completed, the temperature was raised to room temperature, and the precipitated solid was collected by filtration and washed with acetonitrile to obtain a black solid. The obtained solid, sodium hydroxide (2.01 g, 50.3 mmol), and water (120 mL) were mixed and heated and stirred at 90°C for 2 hours. The precipitated solid was collected by filtration to obtain compound (1-6-a) (2.36 g, yield 76%).
[0144] [ka]
[0145] Synthesis of compound (1-6-b) Compound (1-6-a) (1.20 g, 3.87 mmol), 35% hydrochloric acid (0.60 mL, 6.8 mmol), acetic acid (24.0 mL), and water (4.0 mL) were mixed and cooled to 0 to 5 ° C., and a solution of sodium nitrite (0.801 g, 11.6 mmol) in water (3.0 mL) was added dropwise thereto. After that, the mixture was stirred for 30 minutes while maintaining the temperature at 0 to 5 ° C., and a solution of amidosulfuric acid (0.751 g, 7.73 mmol) in water (6.0 mL) was added to prepare a diazo solution. Meanwhile, phenol (0.558 g, 5.93 mmol), sodium acetate (1.91 g, 23.2 mmol), and water (25.0 mL) were mixed and cooled to 0 to 5 ° C., and the entire amount of the diazo solution prepared earlier was added dropwise thereto. After the dropwise addition was completed, the temperature was raised to room temperature, and the precipitated solid was filtered off to obtain compound (1-6-b) (1.54 g, yield 96%).
[0146] [ka]
[0147] Synthesis of compound (1-6) Compound (1-6-b) (0.623 g, 1.50 mmol), methanol (0.35 mL, 8.6 mmol), triphenylphosphine (0.592 g, 2.26 mmol), 1.9 M diisopropyl azodicarboxylate toluene solution (0.95 mL, 1.8 mmol), and THF (9 mL) were mixed and stirred at room temperature for 1 hour. Methanol was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (1-6) (0.310 g, yield 48%).
[0148] [ka]
[0149] 1H-NMR (400MHz, CDCl3): δ(ppm)=8.23-8.19(m,2H),8.10(d,1H),8.07-8.04(m,2H),8.00-7.97(m,2H),7.71(d, 1H),7.37(dd,1H),7.07-7.03(m,2H),3.92(s,3H),2.78(t,2H),1.70(quin,2H),1.41(sext,2H),0.95(t,3H). UV-visible spectrum: λmax = 428 nm (in acetonitrile)
[0150] Synthesis Example 7: Synthesis of compound (1-7) Compound (1-5-b) (0.606 g, 1.50 mmol), 1-iodobutane (0.555 g, 3.02 mmol), potassium carbonate (0.624 g, 4.51 mmol), and N,N-dimethylacetamide (7.5 mL) were mixed and heated and stirred at 100° C. for 1.5 hours. Methanol was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (1-7) (0.309 g, yield 45%).
[0151] [ka]
[0152] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.20-8.17(m,2H),8.07(d,1H),8.06-8.02(m,2H),7.98-7.94(m,2H),7.31(d,1H) ),7.13(dd,1H),7.05-7.01(m,2H),4.15(q,2H),4.07(t,2H),1.86-1.79(m,2H),1.58-1.47(m,5H),1.01(t,3H). UV-visible spectrum: λmax = 456 nm (in acetonitrile)
[0153] Synthesis Example 8: Synthesis of compound (1-8) Compound (1-1-b) (0.391 g, 1.00 mmol), 1-bromo-3,7-dimethyloctane (0.444 g, 2.01 mmol), potassium carbonate (0.415 g, 3.00 mmol), and N,N-dimethylacetamide (5.0 mL) were mixed and heated and stirred at 100° C. for 1 hour. Water was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography using chloroform as a developing solvent, and further purified by reprecipitation from chloroform / methanol to obtain compound (1-8) (0.128 g, 24% yield).
[0154] [ka]
[0155] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.21-8.17(m,2H),8.08(d,1H),8.06-8.03(m,2H),7.99-7.95(m,2H),7.34(d,1H),7.15(dd,1H),7. 05-7.01(m,2H),4.15-4.06(m,2H),3.93(s,3H),1.92-1.84(m,1H),1.75-1.46(m,3H),1.40-1.15(m,6H),0.97(d,3H),0.88(d,6H). UV-visible spectrum: λmax = 452 nm (in acetonitrile)
[0156] Synthesis Example 9: Synthesis of compound (1-9) Compound (1-1-b) (0.584 g, 1.50 mmol), 1-iodohexane (0.637 g, 3.00 mmol), potassium carbonate (0.622 g, 4.50 mmol), and N,N-dimethylacetamide (7.5 mL) were mixed and heated and stirred at 100° C. for 1 hour. Methanol was added to the reaction solution, and the precipitated solid was filtered off. The obtained solid was purified by silica gel column chromatography (chloroform / hexane=9 / 1), and further purified by reprecipitation from chloroform / methanol to obtain compound (1-9) (0.403 g, yield 57%).
[0157] [ka]
[0158] 1 H-NMR (400MHz, CDCl3): δ(ppm)=8.20-8.17(m,2H),8.08(d,1H),8.06-8.03(m,2H),7.98-7.94(m,2H),7.33(d,1H),7.14 (dd,1H),7.04-7.01(m,2H),4.06(t,2H),3.93(s,3H),1.83(tt,2H),1.53-1.46(m,2H),1.39-1.34(m,4H),0.92(d,3H). UV-visible spectrum: λmax = 452 nm (in acetonitrile)
[0159] Example 1: Preparation of composition E1 containing compound (1-1) The following components were mixed and stirred at 80° C. for 1 hour to obtain composition E1. ·Polymerizable liquid crystal compound (A-6) 75 parts by mass ·Polymerizable liquid crystal compound (A-7) 25 parts by mass ·Compound (1-1) 4.0 parts by mass Polymerization initiator: 2-dimethylamino-2-benzyl-1-(4-morpholinophenyl)butan-1-one (Irgacure 369; BASF Japan) 6 parts by mass Leveling agent: polyacrylate compound (BYK-361N; manufactured by BYK-Chemie) 1.2 parts by weight Solvent: o-xylene 250 parts by weight
[0160] Polymerizable liquid crystal compound (A-6) [ka]
[0161] Polymerizable liquid crystal compound (A-7) [ka]
[0162] The polymerizable liquid crystal compound (A-6) was synthesized by the method described in Lub et al. Recl. Trav. Chim. Pays-Bas, 115, 321-328 (1996). The polymerizable liquid crystal compound (A-7) was also produced according to this method.
[0163] Examples 2 to 9: Preparation of compositions E2 to E9 Compositions E2 to E9 of Examples 2 to 9 were obtained, respectively, in the same manner as in Example 1, except that compounds (1-2) to (1-9), respectively, were used instead of compound (1-1).
[0164] Comparative Examples 1 and 2: Preparation of Compositions C1 and C2 Compositions C1 and C2 of Comparative Examples 1 and 2 were obtained in the same manner as in Example 1, except that compounds (2-1) and (2-2) represented by the following formulas were used instead of compound (1-1). Compounds (2-1) and (2-2) were prepared by referring to the description in JP-A-56-104984.
[0165] [ka]
[0166] <Manufacture of polarizing plates> 1. Formation of alignment layer A glass substrate was used as a transparent substrate. A 2% by mass aqueous solution (composition for forming an alignment layer) of polyvinyl alcohol (polyvinyl alcohol 1000 fully saponified type, manufactured by Wako Pure Chemical Industries, Ltd.) was applied onto the glass substrate by spin coating, and after drying, a film having a thickness of 100 nm was formed. Subsequently, an alignment film was formed by subjecting the surface of the obtained film to a rubbing treatment, and a substrate having an alignment film formed on the glass substrate was obtained.
[0167] 2. Formation of polarizing film The composition obtained above was applied by spin coating onto the alignment film of the substrate obtained above, and then heated and dried on a hot plate at 120°C for 3 minutes.Then, the composition was quickly cooled to below 70°C (the temperature at which the film exhibits a smectic liquid crystal phase when cooled), to obtain a laminate in which a dry film was formed on the alignment film.
[0168] Next, ultraviolet rays were irradiated using a UV irradiation device (SPOT CURE SP-7; manufactured by Ushio Inc.) at an exposure dose of 2400 mJ / cm 2 The dried film was irradiated with light at 365 nm (reference wavelength) to polymerize the polymerizable liquid crystal compound contained in the dried film while maintaining the liquid crystal state of the composition, and a polarizing film was formed from the dried film to obtain a polarizing plate.
[0169] <Evaluation> The dichroic ratio of the obtained polarizing plate was measured as follows. The absorbance (A1) in the transmission axis direction and the absorbance (A2) in the absorption axis direction at the maximum absorption wavelength (λmax) of the polarizing film of the polarizing plate were measured by the double beam method using a spectrophotometer (UV-3150 manufactured by Shimadzu Corporation) with a folder equipped with a polarizing plate. A mesh that cuts the amount of light by 50% was installed on the reference side of the folder. The ratio (A2 / A1) was calculated from the measured values of the absorbance (A1) in the transmission axis direction and the absorbance (A2) in the absorption axis direction, and was taken as the dichroic ratio (DR). The results are shown in Table 1. In Table 1, the maximum absorption wavelength of the compounds is the measured value in an acetonitrile solution, except for compound (2-2). The maximum absorption wavelength of compound (2-2) is the measured value in a chloroform solution, and is a reference value.
[0170] [Table 1]
[0171] It can be seen from Table 1 that a polarizing plate having a film made of a composition containing compound (1) can achieve an excellent dichroic ratio (DR).
Claims
1. A composition comprising a compound represented by the following formula (1) and having a maximum absorption wavelength in the wavelength range of 370 nm or more and 470 nm or less, and a liquid crystalline compound including at least one of a polymerizable liquid crystalline compound and a liquid crystalline polymer compound. [Formula 1] [In formula (1), x represents 1. R 1 and R 2 each independently represents an alkyl group, an alkoxy group, an alkoxycarbonyl group, or an alkanoyloxy group, and at least one of the hydrogen atoms of these groups may be substituted with a polymerizable group. Ar 1 , Ar 2 and Ar 3 each independently represents a divalent aromatic group selected from the group consisting of a benzothiazolediyl group and a 1,4-phenylene group; Ar 1 , Ar 2 and Ar 3 At least one of the aromatic groups is a benzothiazolediyl group, and these aromatic groups may be substituted with at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group.
2. 2. The composition according to claim 1, wherein the liquid crystal compound is a smectic liquid crystal compound.
3. In the formula (1), R 1 and R 2 The composition according to claim 1 or 2, wherein each independently represents an alkyl group, an alkoxy group, or an alkoxycarbonyl group.
4. In the formula (1), at least Ar 1 The composition according to any one of claims 1 to 3, wherein is a benzothiazolediyl group.
5. A compound represented by the following formula (1a) and having a maximum absorption wavelength in the wavelength range of 370 nm or more and 470 nm or less. [Case 2] [In formula (1a), y represents 1. R 11 and R 12 each independently represents an alkyl group, an alkoxy group, an alkoxycarbonyl group, or an alkanoyloxy group, and at least one of the hydrogen atoms of these groups may be substituted with a polymerizable group. Ar 11 , Ar 12 and Ar 13 each independently represents a divalent aromatic group selected from the group consisting of a benzothiazolediyl group and a 1,4-phenylene group; Ar 11 , Ar 12 and Ar 13 At least one of the aromatic groups is a benzothiazolediyl group, and these aromatic groups may be substituted with at least one selected from the group consisting of a halogen atom, a methyl group, a hydroxyl group, and a methoxy group.
6. In the formula (1a), at least Ar 11 The compound according to claim 5, wherein is a benzothiazolediyl group.
7. A film formed from the composition according to any one of claims 1 to 4.
8. A laminate comprising the film of claim 7.
9. A display device comprising the laminate according to claim 8 .
Citation Information
Patent Citations
Compound containing benzoxazole ring bis(azo) structure, synthetic method for compound and use of compound
CN105384693A
Bichromic pigment for yellow liquid crystal
JP1981104984A
Dichroic dye for liquid crystal
JP1985228568A
Dichroic Guest-Host Polarizers Containing Oriented Polymer Films
JP2007510946A
Polarizer and method for manufacturing the same
JP2013037353A