Non-aqueous electrolyte secondary battery

The nonaqueous electrolyte secondary battery with a specific porosity distribution in the negative electrode active material layer and a phosphate ester compound in the electrolyte addresses capacity loss after high-temperature storage by reducing electrolyte decomposition, ensuring capacity retention and resistance stability.

JP7572967B2Active Publication Date: 2024-10-24PANASONIC ENERGY CO LTD
View PDF 10 Cites 0 Cited by

Patent Information

Application Number
JP2021562585
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-12-06
Filing Date
2020-11-25
Publication Date
2024-10-24
Estimated Expiration
2040-11-25

AI Technical Summary

Technical Problem

Nonaqueous electrolyte secondary batteries experience a decrease in battery capacity after high-temperature storage due to decomposition reactions at the positive and negative electrodes.

Method used

A nonaqueous electrolyte secondary battery design that includes a negative electrode active material layer with specific porosity distribution and a non-aqueous electrolyte containing a phosphate ester compound, which suppresses decomposition reactions at both electrodes.

Benefits of technology

The design effectively prevents a decrease in battery capacity after high-temperature storage by minimizing electrolyte decomposition, maintaining capacity retention and reducing resistance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572967000006
    Figure 0007572967000006
  • Figure 0007572967000007
    Figure 0007572967000007
  • Figure 0007572967000008
    Figure 0007572967000008
Patent Text Reader

Abstract

A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure comprises a positive electrode, a negative electrode (12) and a nonaqueous electrolyte solution; the negative electrode (12) comprises a negative electrode collector (40) and a negative electrode active material layer (42) that is provided on the negative electrode collector (40); the negative electrode active material layer (42) contains, as negative electrode active materials, graphite particles A and graphite particles B; the graphite particles A have an internal void fraction of 5% or less; the graphite particles B have an internal void fraction of from 8% to 20%; if the negative electrode active material layer (42) is halved in the thickness direction, a region (42b) on the half closer to the outer surface contains more graphite particles A than a region (42a) on the half closer to the negative electrode collector; and the nonaqueous electrolyte solution contains a phosphoric acid ester compound represented by general formula (I). (In the formula, each of R1, R2 and R3 independently represents an alkyl group, an alkenyl group or an alkynyl group; and at least one of R1, R2 and R3 represents an alkenyl group or an alkynyl group.)
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]

[0002] 2. Description of the Related Art Non-aqueous electrolyte secondary batteries that use a carbon material as a negative electrode active material are widely used as high energy density secondary batteries.

[0003] For example, Patent Document 1 discloses a non-aqueous electrolyte secondary battery that uses densified carbon having an internal porosity of 5% or less as a carbon material.

[0004] For example, Patent Document 2 discloses a nonaqueous electrolyte secondary battery that uses carbon materials including carbon material A having an internal porosity of 1% or more and less than 23% and carbon material B having an internal porosity of 23% or more and 40% or less. [Prior art documents] [Patent documents]

[0005] [Patent Document 1] Japanese Patent Application Publication No. 9-320600 [Patent Document 2] JP 2014-67638 A Summary of the Invention [Problem to be solved by the invention]

[0006] An object of the present disclosure is to provide a nonaqueous electrolyte secondary battery capable of suppressing a decrease in battery capacity after high-temperature storage. [Means for solving the problem]

[0007] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure comprises a positive electrode, a negative electrode, and a nonaqueous electrolyte, the negative electrode comprising a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer including graphite particles A and graphite particles B as negative electrode active materials, the graphite particles A having an internal porosity of 5% or less and the graphite particles B having an internal porosity of 8% to 20%, the graphite particles A being contained in a larger amount in an outer surface half region than in an anode current collector half region when the negative electrode active material layer is divided into two equal parts in a thickness direction, and the nonaqueous electrolyte includes a phosphate ester compound represented by the following general formula (I): [ka] (In the formula, R1, R2, and R3 are each independently an alkyl group, an alkenyl group, or an alkynyl group, and at least one of R1, R2, and R3 is an alkenyl group or an alkynyl group.) Effect of the Invention

[0008] According to one embodiment of the present disclosure, it is possible to suppress a decrease in battery capacity after high-temperature storage. [Brief description of the drawings]

[0009] [Figure 1] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment of the present invention. [Diagram 2] FIG. 2 is a cross-sectional view of a negative electrode according to an embodiment of the present invention. [Diagram 3] FIG. 3 is a cross-sectional view of a graphite particle in a negative electrode active material layer. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] A nonaqueous electrolyte secondary battery according to one embodiment of the present disclosure comprises a positive electrode, a negative electrode, and a nonaqueous electrolyte, the negative electrode comprising a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, the negative electrode active material layer including graphite particles A and graphite particles B as negative electrode active materials, the graphite particles A having an internal porosity of 5% or less and the graphite particles B having an internal porosity of 8% to 20%, the graphite particles A being contained in a larger amount in an outer surface half region than in an anode current collector half region when the negative electrode active material layer is divided into two equal parts in a thickness direction, and the nonaqueous electrolyte including a phosphate ester compound represented by the following general formula (I): [ka] (In the formula, R1, R2, and R3 are each independently an alkyl group, an alkenyl group, or an alkynyl group, and at least one of R1, R2, and R3 is an alkenyl group or an alkynyl group.)

[0011] It is believed that the non-aqueous electrolyte solution containing the phosphate ester compound suppresses the decomposition reaction of the non-aqueous electrolyte solution at the positive electrode in a high-temperature environment compared to the non-aqueous electrolyte solution not containing the phosphate ester compound. In addition, as in the present disclosure, the graphite particles A having an internal porosity of 5% or less are contained more in the outer surface half of the negative electrode active material layer than in the negative electrode current collector half of the negative electrode active material layer, so that the reactivity at the outer surface of the negative electrode active material layer is suppressed, and therefore the decomposition reaction of the non-aqueous electrolyte solution at the negative electrode in a high-temperature environment is suppressed. Thus, according to the present disclosure, the decomposition reaction of the non-aqueous electrolyte solution at the positive and negative electrodes in a high-temperature environment is suppressed, so that it is believed that it is possible to suppress the decrease in battery capacity after high-temperature storage.

[0012] Hereinafter, an example of an embodiment will be described in detail with reference to the drawings. Note that the nonaqueous electrolyte secondary battery of the present disclosure is not limited to the embodiment described below. Also, the drawings referred to in the description of the embodiment are schematic.

[0013] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. The nonaqueous electrolyte secondary battery 10 shown in FIG. 1 includes a wound electrode body 14 formed by winding a positive electrode 11 and a negative electrode 12 with a separator 13 therebetween, a nonaqueous electrolyte, insulating plates 18 and 19 respectively arranged above and below the electrode body 14, and a battery case 15 for accommodating the above-mentioned components. The battery case 15 is composed of a bottomed cylindrical case body 16 and a sealing body 17 for closing the opening of the case body 16. Note that, instead of the wound electrode body 14, an electrode body of another form may be applied, such as a laminated electrode body formed by alternately stacking positive and negative electrodes with a separator interposed therebetween. In addition, examples of the battery case 15 include a metallic outer can such as a cylindrical, square, coin, or button-shaped one, and a pouch outer body formed by laminating a resin sheet and a metal sheet.

[0014] The case body 16 is, for example, a metallic outer can having a cylindrical shape with a bottom. A gasket 28 is provided between the case body 16 and the sealing body 17 to ensure airtightness inside the battery. The case body 16 has a protruding portion 22 that supports the sealing body 17, for example, a part of the side surface of the case body 16 protruding inward. The protruding portion 22 is preferably formed in an annular shape along the circumferential direction of the case body 16, and supports the sealing body 17 on its upper surface.

[0015] The sealing body 17 has a structure in which a filter 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the nonaqueous electrolyte secondary battery 10 increases due to heat generation caused by an internal short circuit or the like, for example, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.

[0016] 1, a positive electrode lead 20 attached to a positive electrode 11 passes through a through hole in an insulating plate 18 and extends toward a sealing body 17, and a negative electrode lead 21 attached to a negative electrode 12 passes outside an insulating plate 19 and extends toward the bottom side of a case body 16. The positive electrode lead 20 is connected to the underside of a filter 23, which is the bottom plate of the sealing body 17, by welding or the like, and a cap 27, which is the top plate of the sealing body 17 and is electrically connected to the filter 23, serves as a positive electrode terminal. The negative electrode lead 21 is connected to the inner bottom surface of the case body 16 by welding or the like, and the case body 16 serves as a negative electrode terminal.

[0017] Each of the components of the nonaqueous electrolyte secondary battery 10 will now be described in detail.

[0018] [Negative electrode] 2 is a cross-sectional view of a negative electrode according to an embodiment of the present invention. The negative electrode 12 includes a negative electrode current collector 40 and a negative electrode active material layer 42 provided on the negative electrode current collector 40.

[0019] The negative electrode current collector 40 may be, for example, a foil of a metal such as copper that is stable in the potential range of the negative electrode, or a film having such a metal disposed on its surface.

[0020] The negative electrode active material layer 42 contains graphite particles as the negative electrode active material. The negative electrode active material layer 42 preferably contains a binder and the like. The negative electrode 12 can be produced, for example, by preparing a negative electrode mixture slurry containing the negative electrode active material, the binder and the like, applying the negative electrode mixture slurry onto the negative electrode current collector 40, drying the slurry to form the negative electrode active material layer 42, and rolling the negative electrode active material layer 42. The method for producing the negative electrode active material layer 42 will be described in detail later.

[0021] Fig. 3 is a cross-sectional view of a graphite particle in a negative electrode active material layer. As shown in Fig. 3, a graphite particle 30 has, in a cross-sectional view of the graphite particle 30, closed voids 34 that do not connect the inside of the particle to the particle surface (hereinafter, internal voids 34) and voids 36 that connect the inside of the particle to the particle surface (hereinafter, external voids 36).

[0022] The graphite particles 30 in this embodiment include graphite particles A having an internal porosity of 5% or less and graphite particles B having an internal porosity of 8% to 20%. The internal porosity of the graphite particles A may be 5% or less in order to suppress a decrease in battery capacity after high-temperature storage, but is preferably 1% to 5%, and more preferably 3% to 5%. The internal porosity of the graphite particles B may be 8% to 20%, but is preferably 10% to 18%, and more preferably 12% to 16%, in order to suppress a decrease in battery capacity after high-temperature storage. Here, the internal porosity of the graphite particles is a two-dimensional value calculated from the ratio of the area of ​​the internal voids 34 of the graphite particles to the cross-sectional area of ​​the graphite particles. The internal porosity of the graphite particles is calculated by the following procedure.

[0023] <Method for measuring internal porosity> (1) Exposing a cross section of the negative electrode active material layer. For example, a method for exposing the cross section includes cutting out a part of the negative electrode and processing it with an ion milling device (e.g., IM4000PLUS manufactured by Hitachi High-Technologies Corporation) to expose the cross section of the negative electrode active material layer. (2) A backscattered electron image of the cross section of the exposed negative electrode active material layer is taken using a scanning electron microscope at a magnification of 3,000 to 5,000 times. (3) The cross-sectional image obtained as described above is imported into a computer and binarized using image analysis software (e.g., ImageJ, manufactured by the National Institutes of Health, USA) to obtain a binary processed image in which the particle cross-sections in the cross-sectional image are colored black and voids present in the particle cross-sections are colored white. (4) From the binarized image, graphite particles A and B with a particle size of 5 μm to 50 μm are selected, and the area of ​​the graphite particle cross section and the area of ​​the internal voids present in the graphite particle cross section are calculated. Here, the area of ​​the graphite particle cross section refers to the area of ​​the region surrounded by the outer periphery of the graphite particle, that is, the area of ​​the entire cross section of the graphite particle. In addition, for voids present in the graphite particle cross section that have a width of 3 μm or less, it may be difficult to distinguish whether they are internal voids or external voids in image analysis, so voids with a width of 3 μm or less may be considered internal voids. Then, the internal void ratio of the graphite particle (area of ​​internal voids in graphite particle cross section × 100 / area of ​​graphite particle cross section) is calculated from the calculated area of ​​the graphite particle cross section and the area of ​​the internal voids in the graphite particle cross section. The internal void ratios of graphite particles A and B are the average values ​​of 10 graphite particles A and B, respectively.

[0024] The graphite particles A and B are produced, for example, as follows. <Graphite particles A with internal porosity of 5% or less> For example, the coke (precursor) as the main raw material is crushed to a predetermined size, and then the crushed coke is agglomerated with a binder, baked at a temperature of 2600°C or higher, graphitized, and sieved to obtain graphite particles A of a desired size. Here, the internal porosity can be adjusted to 5% or less depending on the particle size of the crushed precursor or the particle size of the agglomerated precursor. For example, the average particle size (volume-based median diameter D50) of the crushed precursor is preferably in the range of 12 μm to 20 μm. In addition, when the internal porosity is reduced to a range of 5% or less, it is preferable to increase the particle size of the crushed precursor. <Graphite particles B with internal porosity of 8% to 20%> For example, the coke (precursor) as the main raw material is crushed to a predetermined size, agglomerated with a binder, and then pressed into a block shape, which is then fired at a temperature of 2600°C or higher to be graphitized. The graphitized block-shaped body is crushed and sieved to obtain graphite particles B of a desired size. Here, the internal porosity can be adjusted to 8% to 20% depending on the amount of volatile components added to the block-shaped body. When a part of the binder added to the coke (precursor) volatilizes during firing, the binder can be used as the volatile component. An example of such a binder is pitch.

[0025] The graphite particles A and B used in this embodiment may be natural graphite, artificial graphite, or the like, but are not particularly limited thereto. However, in terms of ease of adjusting the internal porosity, artificial graphite is preferred. The interplanar spacing (d 002 ) is, for example, preferably 0.3354 nm or more, more preferably 0.3357 nm or more, and preferably less than 0.340 nm, more preferably 0.338 nm or less. The crystallite size (Lc(002)) of the graphite particles A and B used in this embodiment, determined by X-ray diffraction, is, for example, preferably 5 nm or more, more preferably 10 nm or more, and preferably 300 nm or less, more preferably 200 nm or less. The interplanar spacing (d 002 When the crystallite size (Lc(002)) satisfies the above range, the battery capacity of the nonaqueous electrolyte secondary battery tends to be larger than when the crystallite size (Lc(002)) does not satisfy the above range.

[0026] In this embodiment, the graphite particles A are contained more in the outer surface half region 42b than in the negative electrode current collector half region 42a when the negative electrode active material layer 42 shown in FIG. 2 is divided in half in the thickness direction. This suppresses, for example, the decomposition reaction of the nonaqueous electrolyte in the negative electrode in a high-temperature environment, thereby suppressing the decrease in battery capacity after high-temperature storage. Note that dividing the negative electrode active material layer 42 in half in the thickness direction means dividing the negative electrode active material layer 42 in half at the middle Z of the thickness of the negative electrode active material layer 42 when the stacking direction of the negative electrode current collector 40 and the negative electrode active material layer 42 is the thickness direction of the negative electrode active material layer 42. Then, of the negative electrode active material layer 42 divided in half in the thickness direction, the negative electrode active material layer 42 located closer to the negative electrode current collector 40 is defined as the negative electrode current collector half region 42a, and the negative electrode active material layer 42 located farther from the negative electrode current collector 40 is defined as the outer surface half region 42b.

[0027] In this embodiment, it is sufficient that the graphite particles A are contained more in the outer surface half region 42b than in the negative electrode current collector half region 42a, but in terms of suppressing a decrease in battery capacity after high-temperature storage, the ratio of graphite particles A to graphite particles B in the outer surface half region 42b is preferably 20:80 to 100:0 by mass, and more preferably 50:50 to 100:0. Furthermore, the ratio of graphite particles A to graphite particles B in the negative electrode current collector half region 42a is preferably 10:90 to 0:100 by mass, and more preferably 0:100.

[0028] An example of a method for producing the negative electrode active material layer 42 will be described. For example, a negative electrode active material containing graphite particles B (graphite particles A as required), a binder, and a solvent such as water are mixed to prepare a negative electrode composite material slurry for the negative electrode current collector side. Separately, a negative electrode active material containing a larger amount of graphite particles A (graphite particles B as required) than the negative electrode composite material slurry for the negative electrode current collector side is mixed with a binder and a solvent such as water to prepare a negative electrode composite material slurry for the outer surface side. Then, the negative electrode composite material slurry for the negative electrode current collector side is applied to both sides of the negative electrode current collector and dried, and then the negative electrode composite material slurry for the outer surface side is applied to both sides on the coating film of the negative electrode composite material slurry for the negative electrode current collector side and dried, thereby forming the negative electrode active material layer 42. In the above-described method, the negative electrode composite slurry for the negative electrode current collector side is applied and dried, and then the negative electrode composite slurry for the outer surface side is applied. However, a method in which the negative electrode composite slurry for the outer surface side is applied after the negative electrode composite slurry for the negative electrode current collector side is applied and before drying may be used, or the negative electrode composite slurry for the negative electrode current collector side and the negative electrode composite slurry for the outer surface side may be applied simultaneously.

[0029] The negative electrode active material may contain, in addition to the graphite particles A and B used in this embodiment, other materials capable of reversibly absorbing and releasing lithium ions, for example, a Si-based material. Examples of the Si-based material include Si, an alloy containing Si, and SiO X (X is 0.8 to 1.6) and the like. The Si-based material is a negative electrode material capable of improving the battery capacity more than graphite particles, but on the other hand, it is disadvantageous in terms of charge-discharge cycle characteristics because of its large volume expansion accompanying charge-discharge. However, in a negative electrode active material layer having a negative electrode active material containing graphite particles A and B and a Si-based material, the amount of graphite particles A in the outer surface half region is larger than that in the negative electrode current collector half region, and in some cases, the deterioration of the charge-discharge cycle characteristics can be effectively suppressed compared to the case where the graphite particles A are uniformly dispersed in the negative electrode active material layer. The content of the Si-based material is, for example, preferably 1 mass% to 10 mass%, more preferably 3 mass% to 7 mass%, relative to the mass of the negative electrode active material, from the viewpoints of improving the battery capacity and suppressing the deterioration of the charge-discharge cycle characteristics.

[0030] Other examples of the other material capable of reversibly absorbing and releasing lithium ions include metals that are alloyed with lithium, such as tin (Sn), and alloys and oxides containing metal elements such as Sn. The negative electrode active material may contain the other materials, and the content of the other materials is desirably, for example, 10% by mass or less with respect to the mass of the negative electrode active material.

[0031] Examples of the binder include fluorine-based resin, PAN, polyimide-based resin, acrylic resin, polyolefin-based resin, styrene-butadiene rubber (SBR), nitrile-butadiene rubber (NBR), carboxymethyl cellulose (CMC) or a salt thereof, polyacrylic acid (PAA) or a salt thereof (PAA-Na, PAA-K, etc., or a partially neutralized salt), polyvinyl alcohol (PVA), etc. These may be used alone or in combination of two or more kinds.

[0032] [Positive electrode] The positive electrode 11 is composed of a positive electrode current collector such as a metal foil and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode current collector may be a foil of a metal such as aluminum that is stable in the potential range of the positive electrode, or a film having the metal disposed on the surface layer. The positive electrode active material layer includes, for example, a positive electrode active material, a binder, a conductive material, and the like.

[0033] The positive electrode 11 can be produced, for example, by applying a positive electrode mixture slurry containing a positive electrode active material, a binder, a conductive material, etc. onto a positive electrode current collector, drying it to form a positive electrode active material layer, and then rolling this positive electrode active material layer.

[0034] The positive electrode active material may be, for example, a lithium transition metal oxide containing a transition metal element such as Co, Mn, or Ni. x CoO2, Li x NiO2, Li x MnO2, Li x Co y Ni 1-y O2, Li x Co y M 1-y O z , Lix Ni 1-y M y O z 、 Li x Mn2O4, Li x Mn 2-y M y O4, LiMPO4, Li2MPO4F (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3). These may be used alone or in combination of multiple types. In terms of achieving high capacity of the non-aqueous electrolyte secondary battery, the cathode active material is Li x NiO2, Li x Co y Ni 1-y O2, Li x Ni 1-y M y O z (M; at least one of Na, Mg, Sc, Y, Mn, Fe, Co, Ni, Cu, Zn, Al, Cr, Pb, Sb, B, 0 < x ≤ 1.2, 0 < y ≤ 0.9, 2.0 ≤ z ≤ 2.3), etc., and preferably contains lithium nickel composite oxides.

[0035] Examples of the conductive material include carbon-based particles such as carbon black (CB), acetylene black (AB), ketjen black, and graphite. These may be used alone or in combination of two or more types.

[0036] Examples of the binder include fluorine-based resins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide-based resins, acrylic resins, and polyolefin-based resins. These may be used alone or in combination of two or more types.

[0037] [Non-aqueous electrolyte] The nonaqueous electrolyte contains a phosphate ester compound represented by the following general formula (I): Since the nonaqueous electrolyte contains the phosphate ester compound represented by the following general formula (I), for example, the decomposition reaction of the nonaqueous electrolyte at the positive electrode in a high-temperature environment is suppressed, and therefore the decrease in battery capacity after high-temperature storage is suppressed. [ka] (In the formula, R1, R2, and R3 are each independently an alkyl group, an alkenyl group, or an alkynyl group, and at least one of R1, R2, and R3 is an alkenyl group or an alkynyl group.)

[0038] The number of carbon atoms in the alkyl group is, for example, preferably in the range of 1 to 10, and more preferably in the range of 1 to 6. The number of carbon atoms in the alkenyl group and alkynyl group is, for example, preferably in the range of 2 to 10, and more preferably in the range of 2 to 8. When the number of carbon atoms in the alkyl group, alkenyl group, and alkynyl group exceeds the above range, the viscosity of the nonaqueous electrolyte may be higher than when the number of carbon atoms is within the above range, which may lead to an increase in the resistance of the nonaqueous electrolyte secondary battery.

[0039] The hydrogen atom or carbon atom of the alkyl group, alkenyl group, and alkynyl group may be substituted with a different element or a substituent, if necessary.The different element is not particularly limited, but for example, boron, silicon, nitrogen, sulfur, fluorine, chlorine, bromine, etc.The substituent is not particularly limited, but for example, methyl group, ethyl group, propyl group, butyl group, pentyl group, phenyl group, cyano group, nitro group, hydroxy group, carboxy group, sulfo group, phosphono group, ether group, sulfide group, carbonyl group, sulfonyl group, etc.

[0040] The phosphate ester compound represented by the above general formula includes, for example, triallyl phosphate, trivinyl phosphate, tris(3-butenyl) phosphate, methyldiallyl phosphate, ethyldiallyl phosphate, propyldiallyl phosphate, methylbis(2-propynyl) phosphate, ethylbis(2-propynyl) phosphate, propylbis(2-propynyl) phosphate, butylbis(2-propynyl) phosphate, pentylbis(2-propynyl) phosphate, tris(2-propynyl) phosphate, and the like. Among these, triallyl phosphate is preferable in terms of suppressing the increase in resistance of the non-aqueous electrolyte secondary battery. These may be used alone or in combination of two or more.

[0041] The concentration of the phosphate ester compound in the non-aqueous electrolyte is preferably in the range of, for example, 0.01% by mass to 3% by mass, more preferably in the range of 0.1% by mass to 3% by mass, and still more preferably in the range of 1% by mass to 3% by mass. When the concentration of the phosphate ester compound satisfies the above range, it may be possible to further suppress the decrease in battery capacity after high-temperature storage as compared with the case where the above range is not satisfied.

[0042] The non-aqueous electrolyte contains an electrolyte salt. The electrolyte salt is preferably a lithium salt. Examples of the lithium salt include LiBF4, LiClO4, LiPF6, LiAsF6, LiSb F6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF 6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), Li B 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, borate salts such as Li2B4O7, Li(B(C2O4)F2), LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1SO2){l, m are integers of 0 or more} and other imide salts. The lithium salt may be used alone or in combination. Among these, LiPF6 is preferably used from the viewpoints of ion conductivity, electrochemical stability, and the like. The concentration of the lithium salt is preferably 0.8 to 1.8 mol per 1 L of the non-aqueous solvent.

[0043] The non-aqueous electrolyte contains, for example, a non-aqueous solvent that dissolves an electrolyte salt. For example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these can be used as the non-aqueous solvent. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is substituted with a halogen atom such as fluorine.

[0044] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone and γ-valerolactone; and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate.

[0045] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, and the like. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.

[0046] As the halogen-substituted compound, it is preferable to use a fluorinated cyclic carbonate such as fluoroethylene carbonate (FEC), a fluorinated chain carbonate, a fluorinated chain carboxylate such as methyl fluoropropionate (FMP), or the like.

[0047] [Separator] For example, a porous sheet having ion permeability and insulation is used for the separator 13. Specific examples of the porous sheet include a microporous thin film, a woven fabric, and a nonwoven fabric. The separator is preferably made of an olefin resin such as polyethylene or polypropylene, or cellulose. The separator 13 may be a laminate having a cellulose fiber layer and a thermoplastic resin fiber layer such as an olefin resin. Alternatively, the separator may be a multilayer separator including a polyethylene layer and a polypropylene layer, and a separator having a surface coated with a material such as an aramid resin or ceramic may be used. EXAMPLES

[0048] The present disclosure will be further described below with reference to examples, but the present disclosure is not limited to these examples.

[0049] <Example 1> [Preparation of positive electrode] The positive electrode active material is aluminum-containing lithium nickel cobalt oxide (LiNi 0.88 Co 0.09 Al 0.03 O2) was used. 100 parts by mass of the above positive electrode active material, 1 part by mass of acetylene black, and 0.9 parts by mass of polyvinylidene fluoride were mixed in a solvent of N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode composite slurry. This slurry was applied to both sides of an aluminum foil having a thickness of 15 μm, and the coating film was dried and then rolled with a rolling roller to produce a positive electrode in which a positive electrode active material layer was formed on both sides of the positive electrode current collector. The produced positive electrode was cut to a width of 57.6 mm and a length of 679 mm for use.

[0050] [Preparation of graphite particles A] The coke was pulverized until the average particle size (median diameter D50) was 12 μm. Pitch was added as a binder to the pulverized coke, and the coke was aggregated until the average particle size (median diameter D50) was 17 μm. The aggregate was graphitized by baking at a temperature of 2800° C., and then sieved using a 250 mesh sieve to obtain graphite particles A with an average particle size (median diameter D50) of 23 μm.

[0051] [Preparation of graphite particles B] The coke was crushed to an average particle size (median diameter D50) of 15 μm, and the crushed coke was agglomerated by adding pitch as a binder. The coke was then subjected to an isostatic pressure of 1.6 g / cm. 3 ~1.9g / cm 3A block-shaped compact having a density of 1000 nm was produced. This block-shaped compact was graphitized by firing at a temperature of 2800° C. Next, the graphitized block-shaped compact was pulverized and sieved using a 250 mesh sieve to obtain graphite particles B having an average particle size (median size D50) of 23 μm.

[0052] [Preparation of negative electrode] Graphite particles A were mixed to 40 parts by mass, graphite particles B were mixed to 55 parts by mass, and SiO was mixed to 5 parts by mass, which was used as the negative electrode active material A contained in the outer surface side half region of the negative electrode active material layer. These were mixed so that the mass ratio of negative electrode active material A: carboxymethylcellulose (CMC): styrene-butadiene copolymer rubber (SBR) was 100:1:1 to prepare a negative electrode mixture slurry on the outer surface side. In addition, graphite particles B were mixed to 95 parts by mass, and SiO was mixed to 5 parts by mass, which was used as the negative electrode active material B contained in the negative electrode current collector side half region of the negative electrode active material layer. These were mixed so that the mass ratio of negative electrode active material B: carboxymethylcellulose (CMC): styrene-butadiene copolymer rubber (SBR) was 100:1:1 to prepare a negative electrode mixture slurry on the negative electrode current collector side.

[0053] The negative electrode mixture slurry on the negative electrode current collector side was applied to both sides of a copper foil with a thickness of 8 μm, the coating was dried, and then the negative electrode mixture slurry on the outer surface side was applied on the coating, dried, and the coating was rolled with a rolling roller to produce a negative electrode in which a negative electrode active material layer was formed on both sides of the negative electrode current collector. That is, the graphite particles A: graphite particles B in the outer surface half of the negative electrode active material layer were in a mass ratio of 40:55, and the graphite particles A: graphite particles B in the negative electrode current collector half of the negative electrode active material layer were in a mass ratio of 0:100. In addition, the internal porosity of the graphite particles A and B in the produced negative electrode was measured and found to be 3% and 15%, respectively. The produced negative electrode was cut to a width of 58.6 mm and a length of 662 mm for use.

[0054] [Preparation of non-aqueous electrolyte] LiPF6 was dissolved at a concentration of 1.4 mol / L in a non-aqueous solvent in which ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75, and 3 mass% of vinylene carbonate and 1 mass% of triallyl phosphate were added to the solution to prepare a non-aqueous electrolyte.

[0055] [Preparation of non-aqueous electrolyte secondary battery] (1) An aluminum positive electrode lead was attached to the positive electrode current collector, and a nickel-copper-nickel negative electrode lead was attached to the negative electrode current collector. After that, a polyethylene separator was placed between the positive and negative electrodes and wound to prepare a wound electrode body. (2) Insulating plates were placed above and below the electrode body, the negative electrode lead was welded to the case body, and the positive electrode lead was welded to the sealing member, and the electrode body was housed within the case body. (3) After the non-aqueous electrolyte was injected into the case body under reduced pressure, the open end of the case body was crimped to a sealing member via a gasket, completing the non-aqueous electrolyte secondary battery.

[0056] <Comparative Example 1> Graphite particles B were mixed to 95 parts by mass and SiO to 5 parts by mass, and this was used as the negative electrode active material C contained in the entire region of the negative electrode active material layer. The negative electrode active material C: carboxymethyl cellulose (CMC): styrene-butadiene copolymer rubber (SBR) were mixed so that the mass ratio was 100:1:1 to prepare a negative electrode mixture slurry. This negative electrode mixture slurry was applied to both sides of a copper foil with a thickness of 8 μm, the coating film was dried, and then the coating film was rolled with a rolling roller to prepare a negative electrode in which a negative electrode active material layer was formed on both sides of the negative electrode current collector. That is, the graphite particles A: graphite particles B in the outer surface side half region of the negative electrode active material layer was 0:100 in mass ratio, and the graphite particles A: graphite particles B in the negative electrode current collector side half region of the negative electrode active material layer was also 0:100 in mass ratio. The prepared negative electrode was cut to a width of 58.6 mm and a length of 662 mm for use.

[0057] LiPF6 was dissolved at a concentration of 1.4 mol / L in a non-aqueous solvent in which ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75, and vinylene carbonate was further added at 3 mass%. This was used as a non-aqueous electrolyte. In other words, in Comparative Example 1, a non-aqueous electrolyte that did not contain a phosphate ester compound was used.

[0058] A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1 using the above negative electrode and nonaqueous electrolyte.

[0059] <Comparative Example 2> LiPF6 was dissolved at a concentration of 1.4 mol / L in a non-aqueous solvent in which ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 20:5:75, and further, 3 mass% of vinylene carbonate and 1 mass% of triethyl phosphate were added. This was used as a non-aqueous electrolyte. That is, in Comparative Example 2, a non-aqueous electrolyte containing a phosphoric acid ester compound having an alkyl group was used.

[0060] In Comparative Example 2, a nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the above nonaqueous electrolyte was used and the negative electrode fabricated in Comparative Example 1 was used.

[0061] <Comparative Example 3> A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the negative electrode fabricated in Comparative Example 1 was used.

[0062] <Comparative Example 4> A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the nonaqueous electrolyte prepared in Comparative Example 1 was used.

[0063] <Comparative Example 5> A nonaqueous electrolyte secondary battery was fabricated in the same manner as in Example 1, except that the nonaqueous electrolyte prepared in Comparative Example 2 was used.

[0064] [High temperature storage test] At an environmental temperature of 25°C, the nonaqueous electrolyte secondary batteries of Example 1 and each comparative example were charged at a constant current of 990mA (0.3 hour rate) to 4.2V, and then charged at a constant voltage of 4.2V with a cut-off current of 66mA. Thereafter, a constant current discharge was performed at a constant current of 1650mA (0.5 hour rate) to 3.0V, and the discharge capacity at this time was measured as the battery capacity before storage. Thereafter, a constant current charge was performed at a constant current of 990mA (0.3 hour rate) to 4.2V, and a constant voltage charge was performed at a constant voltage of 4.2V with a cut-off current of 66mA, and the SOC was adjusted to 100%. Then, under an environmental temperature of 25°C, the AC impedance was measured, and the resistance value at 0.02Hz was measured, which was the resistance value before storage.

[0065] Thereafter, the nonaqueous electrolyte secondary batteries of Example 1 and each comparative example were stored in a high temperature bath at 80°C for 3 days. After storage, each nonaqueous electrolyte secondary battery was removed from the thermostatic bath and left for 1 hour, and then discharged at a constant current of 1650mA (0.5 hour rate) to 3.0V at an environmental temperature of 25°C, and the discharge capacity at this time was measured as the battery capacity after high temperature storage. Thereafter, constant current charging was performed at a constant current of 990mA (0.3 hour rate) to 4.2V, and constant voltage charging was performed at a constant voltage of 4.2V with a cut-off current of 66mA, and the SOC was adjusted to 100%. Then, AC impedance was measured at an environmental temperature of 25°C, and the resistance value at 0.02Hz was measured, and this was the resistance value after storage.

[0066] The capacity retention rates after high-temperature storage of the nonaqueous electrolyte secondary batteries of Example 1 and each of the Comparative Examples were calculated using the following formula (1), and are summarized in Table 1. Here, a higher value of the capacity retention rate after high-temperature storage indicates that the decrease in battery capacity after high-temperature storage is more suppressed. Capacity retention rate after high temperature storage = (battery capacity after storage / battery capacity before storage) x 100(1)

[0067] In addition, the resistance ratios before and after high-temperature storage of the nonaqueous electrolyte secondary batteries of Example 1 and each Comparative Example were calculated using the following formula (2), and are summarized in Table 1. Here, a lower resistance ratio before and after high-temperature storage indicates that the increase in battery resistance after high-temperature storage is more suppressed. Resistance ratio before and after high-temperature storage = Resistance after storage / Resistance before storage (2)

[0068] [Table 1]

[0069] As can be seen from Table 1, the capacity retention rate after high-temperature storage in Example 1 was higher than those in Comparative Examples 1 to 5. That is, according to Example 1, it is possible to suppress the decrease in battery capacity after high-temperature storage. Furthermore, the resistance ratio before and after high-temperature storage in Example 1 was lower than those in Comparative Examples 1 to 2 and 4 to 5, and was comparable to that of Comparative Example 3. That is, by using a nonaqueous electrolyte containing a phosphate ester compound as in Example 1 and Comparative Example 3, it is possible to suppress the increase in battery resistance before and after high-temperature storage. [Explanation of symbols]

[0070] 10 nonaqueous electrolyte secondary battery, 11 positive electrode, 12 negative electrode, 13 separator, 14 electrode body, 15 battery case, 16 case body, 17 sealing body, 18, 19 insulating plate, 20 positive electrode lead, 21 negative electrode lead, 22 protruding portion, 23 filter, 24 lower valve body, 25 insulating member, 26 upper valve body, 27 cap, 28 gasket, 30 graphite particles, 34 internal gap, 36 external gap, 40 negative electrode current collector, 42 negative electrode active material layer, 42a negative electrode current collector side half region, 42b outer surface side half region.

Claims

1. A non-aqueous electrolyte secondary battery having a positive electrode, a negative electrode, and a non-aqueous electrolyte, the negative electrode has a negative electrode current collector and a negative electrode active material layer provided on the negative electrode current collector, The negative electrode active material layer contains graphite particles A and graphite particles B as negative electrode active materials, the graphite particles A have an internal porosity of 5% or less, and the graphite particles B have an internal porosity of 8% to 20%, the graphite particles A are contained in a larger amount in an outer surface half region than in an outer surface half region of the negative electrode current collector side when the negative electrode active material layer is divided into two equal parts in a thickness direction; The nonaqueous electrolyte secondary battery includes a phosphoric acid ester compound represented by the following general formula (I): [Formula 1] (In the formula, R1, R2, and R3 are each independently an alkyl group, an alkenyl group, or an alkynyl group, and at least one of R1, R2, and R3 is an alkenyl group or an alkynyl group.)

2. 2. The nonaqueous electrolyte secondary battery according to claim 1, wherein the alkenyl group and the alkynyl group each have 2 to 10 carbon atoms.

3. 3. The nonaqueous electrolyte secondary battery according to claim 1, wherein the content of the phosphate ester compound in the nonaqueous electrolyte is in the range of 0.01% by mass to 3% by mass.

4. 4. The nonaqueous electrolyte secondary battery according to claim 1, wherein the negative electrode active material comprises a Si-based material.

Citation Information

Patent Citations

  • Electrochemical battery fined carbon

    JP1997320600A

  • Electrolyte and battery

    JP2006221972A

  • Carbon material for nonaqueous secondary battery, negative electrode, and nonaqueous secondary battery

    JP2014067638A

  • Nonaqueous electrolyte and lithium ion secondary battery

    JP2015133255A

  • Carbon material for nonaqueous secondary battery and nonaqueous secondary battery