Methods and compositions for modifying additively manufactured metal or metal alloy objects

The use of organic acid and solid media formulations addresses post-printing challenges in AM metal parts by efficiently removing support material, reducing surface roughness, and enhancing structural integrity, resulting in a shiny finish.

JP7572976B2Active Publication Date: 2024-10-24POSTPROCESS TECHNOLOGIES INC
View PDF 3 Cites 0 Cited by

Patent Information

Application Number
JP2021574284
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2019-06-18
Filing Date
2020-06-18
Publication Date
2024-10-24
Estimated Expiration
2040-06-18

AI Technical Summary

Technical Problem

Current additive manufacturing (AM) technologies for metal and metal alloy parts face challenges in post-printing processing, including removal of unnecessary powder and support material, surface roughness reduction, oxidation layer removal, and stress relief, which are time-consuming and often require hazardous chemicals.

Method used

Formulations comprising organic acids and solid polishing media are used to remove unwanted material, reduce surface roughness, and modify the surface finish of AM objects through wet blasting in a controlled environment, utilizing varying temperatures, pressures, and spray nozzle operations.

Benefits of technology

The formulations effectively remove support material, reduce surface roughness from 400+ microinches to 10 microinches, eliminate oxidation layers, and enhance structural integrity by reducing stress concentrations, achieving a shiny metallic appearance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007572976000003
    Figure 0007572976000003
  • Figure 0007572976000001
    Figure 0007572976000001
  • Figure 0007572976000002
    Figure 0007572976000002
Patent Text Reader

Abstract

Disclosed are methods of using the formulations to treat manufactured metal or metal alloy objects, particularly metal or metal alloy objects manufactured by additive manufacturing. Also disclosed are methods, systems, and devices that use the formulations to remove excess material from a surface, remove support material, and / or modify the surface of a manufactured metal or metal alloy object. [Drawing] Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] (Reference Application) This patent application claims priority to U.S. Provisional Patent Application No. 62 / 863,180, filed June 18, 2019, the disclosure of which is incorporated by reference.

[0002] The present application relates generally to processes using formulations for removing material from or finishing metal or metal alloy objects formed by additive manufacturing processes, as well as systems, devices, and methods for using such formulations. [Background technology]

[0003] Additive manufacturing (AM) of metal and metal alloy parts offers advantages over traditional manufacturing methods. The design of metal or metal alloy objects can be limited by geometric constraints and require large tooling, equipment and labor costs, but a wide range of metal powders can be used to achieve a high level of design freedom. While the utility of AM techniques for prototyping metal objects is already well established, AM can also be used to produce parts for demanding applications in the aerospace, medical, dental and manufacturing industries.

[0004] Current AM technologies for metal parts include powder bed methods such as DMLS (Direct Metal Laser Sintering), EBM (Electron Beam Melting), SLM (Selective Laser Melting), or powder fed methods such as LC (Laser Cladding), LMD (Laser Metal Deposition), DMD (Direct Metal Deposition). Within each of these technologies, some of the most popular alloys being additively manufactured today include various titanium, aluminum, stainless steels (304, 316), carbon steels, nickel superalloys (e.g. Inconel® 718, Haynes® 282, Hastelloy®) (aerospace industry), AlSi10Mg (aerospace industry), Ti6Al4V (medical industry), and CoCr (dental industry).

[0005] While AM ​​has many advantages in many applications, one of the challenges that must be addressed is the processing of the part after it has been created by the printer. Different AM printing techniques and materials present different post-printing challenges. These challenges include, but are not limited to: Removal of unwanted metal particles Removal of unwanted print material Removal of unnecessary support material Reduce surface roughness Removal of oxidized surface material Polishing of parts Surface Passivation Stress relief

[0006] Current methods for treating metal and metal alloy parts range from mechanical methods such as machining, hand sanding, blasting, tumbling, abrading, electro polishing, etc., to chemical surface treatments such as descaling and pickling. These methods are time consuming, relatively expensive, require a relatively large amount of manual labor, or require the use of hazardous chemicals.

[0007] While these conventional processing methods are satisfactory for some applications, there is room for improvement, and in particular there is a need for effective methods for processing AM formed metal or metal alloy objects, and for removing support material from AM formed metal or alloy objects as well as for surface treatment. Summary of the Invention

[0008] The inventive concepts disclosed herein include a formulation composed of one or more organic acids and a solid abrasive medium, and a method of using this formulation. This formulation and method are used to remove material from or modify the surface of AM metal-based objects, including metal and metal alloy objects. For example, the formulation can be used in a chamber where the AM object is wet blasted with the formulation to remove unwanted metal or metal alloy material. The formulation can be utilized at specific temperatures, pressures, and spray nozzle operations, and various types of spray nozzles can be used while varying the distance between the spray nozzle and the object to apply the desired modification to the surface of the AM object.

[0009] <Type of AM> Using the inventive concepts disclosed herein, it is possible to modify the surface of objects formed by various additive manufacturing methods, such as powder bed methods like EBM (Electron Beam Melting), DMLS (Direct Metal Laser Sintering), and SLM (Selective Laser Melting), and powder feed methods like LC (Laser Cladding), LMD (Laser Metal Deposition), and DED (Directed Energy Deposition).

[0010] <Removal of support material> Some metal or metal alloy objects manufactured by the AM method have support materials. Using the inventive concepts disclosed herein, it is possible to remove the unnecessary support materials printed to support the structure of the AM metal or metal alloy object.

[0011] <Surface roughness> Another aspect of the present invention is directed towards reducing the surface roughness of metal or metal alloy objects manufactured by the AM method. AM metal and metal alloy objects may have a rough surface finish (measured as Ra in microinches or micrometers). Using the inventive concepts disclosed herein, it is possible to reduce the surface roughness of AM metal or metal alloy objects from an Ra of 400+ microinches during manufacturing to an Ra of about 10 microinches or the desired roughness.

[0012] <Surface Finish> The inventive concepts disclosed herein can be used to modify the surface finish of objects produced by AM processes. In some cases, the surfaces of AM metal and metal alloy objects oxidize to a dark gray or black color. The inventive concepts disclosed herein can be used to remove the oxide layer from the metal or metal alloy, partially passivate the object, and give the object a shiny, metallic-looking surface finish.

[0013] <Structural integrity> The inventive concepts disclosed herein can further be used to improve the structural integrity and strength of objects produced by AM processes. AM metal and metal alloy objects can have poor mechanical properties due to stress concentrations at their surfaces. Embodiments of the inventive concepts can be used to reduce stress concentrations at the metal or metal alloy surface. [Brief description of the drawings]

[0014] [Figure 1] FIG. 1 is a schematic diagram of a system that can be used to apply a formulation according to the present invention to additively manufacture objects. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0015] The following detailed description describes examples of the invention and inventive concepts. It should be noted that other embodiments are possible and that various modifications may be made to the invention without departing from the spirit and scope of the invention. Thus, the following more detailed descriptions of specific embodiments of the invention are presented for purposes of explanation, not for purposes of limiting the scope of the invention, and are intended to describe certain features and characteristics that are part of the invention or inventive concepts.

[0016] Unless otherwise specified herein, the term "finishing" refers to the removal of unwanted material from an AM object, which occurs after the printing stage of the object to produce a finished object. Finishing can include one or more steps, including, but not limited to, removing unwanted metal powder, removing unwanted printed material, removing unwanted support material, reducing surface roughness, removing oxidized surface material, polishing the part, passivating the surface, and / or stress relieving the AM object. "Finishing" an AM object may also be referred to as "cleaning," "surface modification," "polishing," "grinding," "milling," "smoothing," or "texturizing."

[0017] In this disclosure, unless otherwise specified herein, the term "formulation" refers to a fluid composition, which may include a fluid, slurry, mixture, colloid, suspension, chemical, liquid, detergent, or solution, any of which may be used when referring to the inventive concepts disclosed herein.

[0018] Below, numerical ranges are disclosed. The ranges state a lower limit (LLV) and an upper limit (ULV). Unless otherwise stated, the LLV, ULV, and all values ​​between the LLV and ULV are part of the range.

[0019] The inventive concepts disclosed herein include formulations and methods and systems for using the formulations to remove support material from or modify the surface of AM metal or metal alloy objects. The inventive concepts can be practiced to remove or modify metal or metal alloy materials, such as surface material, support structure material, or oxidized surface layers of objects formed by AM processes.

[0020] Metals and metal alloys to which the concepts of the present invention are applicable include, but are not limited to, one or more of the following: titanium, Ti6Al4V, aluminum, tool steels and cermets such as AlSi10Mg, Al6061, H13, superalloys such as Inconel 625, 718, stainless steels such as Stellite, BC4, 304L, 316, 320, refractory materials such as MoRe, Ta-W, CoCr, and the like.

[0021] Additionally, the inventive concepts, including methods, can be implemented at specific temperatures and / or pressures, using different types of spray nozzles with desired spray nozzle action, and / or varying the distance from the spray nozzle to the object to modify the surface of the AM object to achieve specific desired characteristics.

[0022] Formulations based on the concepts of the present invention include acidic organic compounds, such as compounds with carboxylic acid groups, organic-based alcohols in which the hydroxyl group functions as a weak acid, enol groups, and phenol groups (i.e., phenolic acids). The following are examples of acidic compounds that can be used: formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, oxalic acid, lactic acid, malic acid, citric acid, ascorbic acid, benzoic acid, carbonic acid, glycine, sarcosine, glycolic acid, phenolic acid, uric acid, taurine, p-toluenesulfonic acid, trifluoromethanesulfonic acid, aminomethylphosphonic acid, maleic acid, succinic acid, palmitic acid, itaconic acid, fumaric acid, tartaric acid, and boric acid. One or more organic acids can be present in the colloidal mixture from 0.01% up to 50.00% of the total weight of the mixture.

[0023] [ka]

[0024] Formulations according to the concepts of the present invention include solid media. The solid media provide mechanical abrasion and facilitate the finishing process. The solid media can be of various materials, shapes, and / or sizes. The solid media can be selected from the following types: glass beads, steel, stainless steel, ceramic materials, aluminum oxide / alumina, silica, zirconium, silicon carbide, plastic, garnet, copper, corncobs, walnut shells, mica, feldspar, pumice, and the like, and combinations thereof. The solid media can be of the following shapes: spherical, elongated, irregular, jagged, angular, cubic, rectangular, and / or cylindrical. The solid media can have the following dimensions: longest linear diameter of 0.1 to 1000 μm (micrometers), including all values ​​and ranges between 0.1 μm.

[0025] <First embodiment> In this first embodiment, a formulation according to the concepts of the present invention is used to finish a component made of Inconel 718. Inconel 718 (55Ni-21Cr-5Nb-3Mo) is a nickel-based superalloy. This superalloy is precipitation hardened to maintain high strength and good ductility. Inconel 718 is non-magnetic and maintains good corrosion and oxidation resistance, and is used for components that require high resistance to deformation and stress cracking up to 1300°F (704°C) and oxidation resistance up to 1800°F (982°C). Conventional methods for finishing Inconel 718 manufactured by AM processes use chemicals such as hydrofluoric acid (HF) and aqua regia (HCl / HNO3).

[0026] In one embodiment, the formulation was applied using a DECI Duo system, available from Post Process Technologies, Inc. FIG. 1 is a schematic diagram of an embodiment of the system 10. The equipment hardware portion of the DECI Duo system includes a spray chamber 25 containing two single-axis jets 28A, 28B that deliver compressed air and formulation (cleaning agent and suspended solids) 7 at software-controlled variable pressures and velocities. The chamber 25 is fitted with a 360-degree rotatable T-shaped perforated turntable 22 designed for flexible material fixturing. The rotation of the table 22 provides a third axis of motion, allowing maximum surface exposure to the part 19 being processed.

[0027] In this embodiment, the DECI Duo system uses a formulation using Thermal Atomized Fusaraid (TAF) technology developed by Post Process Technologies, Inc. The DECI Duo system and Thermal Atomized Fusaraid (TAF) technology are described in co-pending patent application Ser. No. 16 / 209778, filed Dec. 4, 2018, entitled "Method and Apparatus for Surface Finishing and Support Material Removal," the entire disclosure of which is incorporated herein by reference. A part 19 requiring support material removal and / or build material surface smoothing is placed on the turntable 22. A media pump 37 draws fluid 7 from a tank 31 having an open top surface 34 located below the turntable 22 and delivers the fluid 7 through a conduit 43A to a nozzle 28, which sprays the fluid 7 onto the part 19 with compressed air. After spraying the part 19, the fluid 7 returns to the tank 31. When used on a PostProcess DECI Duo system, the process is software controlled by PostProcess' AUTOMAT3D® platform, which is described in co-pending patent application Ser. No. 16 / 340647, filed April 9, 2019, and co-pending patent application Ser. No. 16 / 348276, filed May 8, 2019, the entire disclosures of which are incorporated herein by reference.

[0028] The specific component ingredients of the formulation can be related to the metal undergoing the finishing process and the desired finish. Thus, the formulation of this embodiment was based on the physical and chemical properties of Inconel 718 and the desired etching, passivation, and polishing needs. The formulation was a mildly acidic cleaning solution containing 2% by weight oxalic acid. This formulation enhanced the surface finishing process by etching the surface of the part, while avoiding the hazardous issues associated with traditional chemical reactions. The formulation etched the surface of the part as the first step of the finishing process. The suspended solids used in the TAF technique can effectively abrade the surface of the part. If the user's goal is a relatively smooth surface, the process can end here. However, if the user wishes to further smooth the part, a second finishing step can be performed.

[0029] The media included in the formulation of this embodiment was a ceramic zirconia based aggregate with a size of 425 μm. This media was selected taking into consideration the layer thickness and hardness associated with DMLS printing of Inconel 718. Zirconia has high toughness and is well suited for hard alloys such as Inconel. The media particle size of 425 μm correlates to the surface roughness caused by the range of layer thicknesses associated with DMLS. Additionally, this media has the advantage of being chemically inert and will not contaminate the part or the formulation. Using this formulation with TAF technology allows parts to be finished with less thermal energy, reducing the risk of affecting the grain structure of the part.

[0030] One of the benefits of using the DECI Duo system to apply the formulations is the DECI Duo's AUTOMAT3D programming platform. AUTOMAT3D programming implements agitation algorithms designed specifically for metal properties, allowing the DECI Duo system to take a predictive approach in finishing AM metal parts. The software controls the nozzle operating speed, the temperature at which the process is run, and the air and liquid pressures throughout the duration of the cycle, efficiently providing a chemical and mechanical energy source. Sensors monitor the process and ensure energy levels remain within the desired range with automatic adjustments in real time. AUTOMAT3D platform programming also allows users to digitally vary parameters, creating flexibility for a range of finishing requirements. Settings may be stored for reduced machine make time and repeatability. AUTOMAT3D programming also records run times to allow for planned preventative maintenance of the software, thereby reducing downtime.

[0031] In this embodiment, several tests of parts with different geometries, initial roughness, and final roughness were performed to create a data set. Different agitation algorithms were used. The desired results included a reduction in surface roughness and polishing, which meant a glossier part. Increasing the temperature along with the fluid and pressure was required to reduce the surface roughness caused by the layer thickness. Increasing these ranges increased the mechanical energy of the system, leading to faster removal. In this embodiment, the acidity of the formulation reacted with the surface layer of the part, resulting in a degree of passivation. This process resulted in a reduced surface roughness, faded or disappeared lines in the printed layer, a more corrosion resistant surface finish, and a glossier part.

[0032] The results in this embodiment were measured using a surface profilometer. Roughness values ​​varied depending on the part orientation and surface being measured. Measurements were taken in a direction perpendicular to the printed layer. The table below contains examples of initial and final surface roughness measurements, as well as the corresponding operator and equipment time requirements for the results obtained.

[0033] [Table 1] EXAMPLES

[0034] The following examples are presented to illustrate various variations, but are not intended to limit the scope of the inventive concepts in any way. In the following examples, objects were finished with a Post Process DECI Duo machine. The time to achieve results varied depending on the material and the desired smoothness after finishing.

[0035] <Example 1> The surface of AlSi10Mg alloy produced by additive manufacturing is modified using a colloidal mixture in a wet blasting chamber consisting of 2% by weight oxalic acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. The surface finishing of AlSi10Mg alloy is performed by maintaining the temperature of the spray chamber in the range of 70°F (21°C) to 140°F (60°C) and pressure of 0-80 psig. The surface roughness of AlSi10Mg alloy can be modified by using such a colloidal mixture, from Ra of 200-300 microinches to Ra of less than 70 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0036] <Example 2> The surface of AlSi10Mg alloy produced by additive manufacturing is modified using a colloidal mixture in a wet blasting chamber consisting of 2% by weight oxalic acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 100-300 micrometers, and 40 gallons of water. The surface finishing of AlSi10Mg alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. The surface roughness of AlSi10Mg alloy can be modified by using such a colloidal mixture, from an Ra of 200-300 microinches to an Ra of less than 100-150 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0037] <Example 3> The surface of AlSi10Mg alloy produced by additive manufacturing is modified using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1% citric acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. The surface finishing of AlSi10Mg alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. The surface roughness of AlSi10Mg alloy can be modified by using such a mixture, from an Ra of 200-300 microinches to an Ra of less than 100-150 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0038] <Example 4> The surface of AlSi10Mg alloy produced by additive manufacturing is modified using a colloidal mixture in a wet blasting chamber consisting of 1% ascorbic acid, 1% citric acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. The surface finishing of AlSi10Mg alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. The surface roughness of AlSi10Mg alloy can be modified by using such a mixture, from an Ra of 200-300 microinches to an Ra of less than 100-150 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0039] <Example 5> The surface of AlSi10Mg alloy produced by additive manufacturing is modified using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 0.2% benzoic acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. The surface finishing of AlSi10Mg alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. The surface roughness of AlSi10Mg alloy can be modified by using such a mixture, from a Ra of 200-300 microinches to a Ra of 80-120 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0040] <Example 6> The surface of AlSi10Mg alloy produced by additive manufacturing is modified using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1.0% tartaric acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of AlSi10Mg alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of AlSi10Mg alloy, from 200-300 microinches Ra to 80-120 microinches Ra. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0041] <Example 7> Surface modifications are made to Ti6Al4V alloys produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 2% oxalic acid by weight, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Ti6Al4V alloys is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-78 psig. Such mixtures can be used to modify the surface roughness of Ti6Al4V alloys, from a Ra of 200-300 microinches to a Ra of 100-150 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0042] <Example 8> Surface modifications are made to Ti6Al4V alloys produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1% ascorbic acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Ti6Al4V alloys is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of Ti6Al4V alloys, from 200-300 microinches Ra to less than 120 microinches Ra. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0043] <Example 9> Surface modifications are made to Ti6Al4V alloys produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1% citric acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Ti6Al4V alloys is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of Ti6Al4V alloys, from an Ra of 200-300 microinches to an Ra of less than 120 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0044] <Example 10> Surface modifications are made to Ti6Al4V alloys produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1% benzoic acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Ti6Al4V alloys is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of Ti6Al4V alloys, from 200-300 microinches Ra to less than 120 microinches Ra. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0045] <Example 11> Modifications are made to the surface of Inconel 718 alloy produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 2% oxalic acid by weight, 35 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Inconel 718 alloy is performed by maintaining the spray chamber at a temperature range of ambient 80°F (21°C) to 140°F (60°C) and a pressure of 50-100 psig. Such mixtures can be used to modify the surface roughness of Inconel 718 alloy, from an Ra of 150-250 microinches to an Ra of less than 75 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0046] <Example 12> Modifications are made to the surface of Inconel 718 alloy produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 4% oxalic acid by weight, 35 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Inconel 718 alloy is performed by maintaining the spray chamber at a temperature range of ambient 80°F (21°C) to 140°F (60°C) and a pressure of 50-100 psig. Such mixtures can be used to modify the surface roughness of Inconel 718 alloy, from an Ra of 150-250 microinches to an Ra of less than 75 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0047] <Example 13> Modifications are made to the surface of Inconel 718 alloy produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1.0% tartaric acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Inconel 718 alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of Inconel 718 alloy, from an Ra of 150-250 microinches to an Ra of less than 75 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0048] <Example 14> Modifications are made to the surface of Inconel 718 alloy produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 1% oxalic acid, 1.0% benzoic acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Inconel 718 alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of Inconel 718 alloy, from an Ra of 150-200 microinches to an Ra of less than 75 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0049] <Example 15> Modifications are made to the surface of Inconel 718 alloy produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 1% ascorbic acid, 1.0% citric acid, 30-40 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of Inconel 718 alloy is performed by maintaining the spray chamber at a temperature range of ambient 70°F (21°C) to 140°F (60°C) and a pressure of 0-80 psig. Such mixtures can be used to modify the surface roughness of Inconel 718 alloy, from an Ra of 150-200 microinches to an Ra of less than 75 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0050] <Example 16> Surface modifications are made to aluminum F357 alloy produced by additive manufacturing using a colloidal mixture in a wet blasting chamber consisting of 2% oxalic acid by weight, 35 pounds of spherical zirconium oxide (ZrO2) 400-600 micrometers in size, and 40 gallons of water. Surface finishing of aluminum F357 alloy is performed by maintaining the spray chamber at a temperature range of ambient 80°F (21°C) to 140°F (60°C) and a pressure of 50-100 psig. Such mixtures can be used to modify the surface roughness of aluminum F357 alloy, from an Ra of 150-250 microinches to an Ra of less than 75 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0051] <Example 17> Modifications are made to the surface of additively manufactured 316 stainless steel using a colloidal mixture in a wet blasting chamber consisting of 2% oxalic acid by weight, 35 pounds of spherical zirconium oxide (ZrO2) with a size of 400-600 micrometers, and 40 gallons of water. Surface finishing of the 316 stainless steel is performed by maintaining the spray chamber at a temperature range of ambient 80°F (21°C) to 140°F (60°C) and a pressure of 50-100 psig. The use of such a mixture alters the surface roughness of the 316 stainless steel, from a Ra of 300-350 microinches to a Ra of 50-100 microinches. The finished object has a shiny metallic appearance with no visible traces of oxidation on the surface.

[0052] In the embodiments disclosed above, the formulations of AM metal and metal alloy finishing compositions have been described for use with the DECI Duo system. However, the AM formulations are not limited to use with the DECI Duo system. Alternatively, Post Process equipment other than the DECI Duo may be used with any of the disclosed formulations. Such alternative equipment or systems may include a simple closed chamber in which the metal or metal alloy part is sprayed manually (e.g., by an attendant or human operator). Alternatively, the AM finishing formulation may be used in a closed chamber in which the part is placed and sprayed unattended for a period of time. The time to achieve the desired results will vary depending on the type of equipment used, including the number of spray nozzles and the dimensions of the chamber. The spraying may take minutes, hours, or days to achieve the desired AM part characteristics.

[0053] As a further possibility, the formulations disclosed herein may be used to treat metal or metal alloy objects manufactured by methods other than additive manufacturing. For example, the treatment formulations disclosed herein may be used to finish metal or metal alloy objects manufactured by conventional manufacturing methods such as casting or molding. When used to treat metal or metal alloy objects manufactured by means other than additive manufacturing, the formulations may be used with any of the systems, hardware, or equipment described above, including the DECI Duo system or conventional cleaning chambers.

[0054] In one embodiment, the formulation is provided with the organic acid (neat, undiluted, or concentrated) and the solid vehicle as separate components, which are mixed with water (if necessary) prior to use. Alternatively, the organic acid component of the formulation is provided as a concentrated liquid, which is mixed with the appropriate proportion of water prior to use. As a further possibility, the organic acid component of the formulation is provided as a powder, which is added to water in the appropriate proportion prior to use. In yet another embodiment, the formulation, including the organic acid, the solid vehicle, and water, is provided fully or partially premixed. As a further possibility, the organic acid component of the formulation is provided as a concentrated liquid, powder, or premixed solution, and the appropriate solid vehicle is selected for use.

[0055] Having thus described the features of the present invention and some embodiments of the present invention, the following non-limiting statements of various embodiments of the present invention follow.

[0056] <Statement A> 1. A sprayable formulation for finishing metal-based objects formed by additive manufacturing, comprising: 0.01 to 50% by weight of at least one organic acid; 0.01 to 50% by weight of a solid medium; Formulations containing water (e.g., balance water).

[0057] <Statement B> 4. The sprayable formulation of claim A, wherein the at least one organic acid is selected from formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, oxalic acid, lactic acid, malic acid, citric acid, ascorbic acid, benzoic acid, carbonic acid, glycine, sarcosine, glycolic acid, phenolic acid, uric acid, taurine, p-toluenesulfonic acid, trifluoromethanesulfonic acid, aminomethylphosphonic acid, maleic acid, succinic acid, palmitic acid, itaconic acid, fumaric acid, tartaric acid, boric acid, and the like, and combinations thereof.

[0058] <Statement C> The sprayable formulation of statement A or B, wherein the solid medium is selected from glass beads, steel, stainless steel, ceramic materials, aluminum oxide / alumina, silica, zirconium, silicon carbide, plastic, garnet, copper, corn cobs, walnut shells, mica, feldspar, pumice, and the like, and combinations thereof.

[0059] <Statement D> The sprayable formulation of any of Statements A, B, C, wherein the solid medium has a shape, appearance, and / or surface that is spherical, elongated, irregular, jagged, angular, cubic, rectangular, cylindrical, and combinations thereof.

[0060] <Statement E> The sprayable formulation according to any of statements A, B, C, D, wherein the solid medium is in the size range of 0.1 to 1000 μm (micrometers), including all values ​​and ranges between 0.1 μm.

[0061] <Statement F> The sprayable formulation according to any of the preceding statements, wherein the finishing solution is comprised of a colloidal slurry.

[0062] <Statement G> The sprayable formulation according to any of the preceding statements, wherein said metal-based object comprises a metal or metal alloy object.

[0063] <Statement H> The sprayable formulation according to any of the preceding statements, wherein the metal-based object comprises at least one of tool steels or cermets including titanium, Ti6Al4V, aluminum, AlSi10Mg, Al6061, H13, superalloys such as Inconel 625, 718, stainless steels including Stellite, BC4, 304L, 316, 320 or refractory materials including MoRe and Ta-W, CoCr, or combinations thereof.

[0064] <Statement I> The sprayable formulation according to any of the preceding statements, wherein the additive manufacturing process comprises powder bed processes including electron beam melting, direct metal laser sintering, selective laser melting, powder fed processes including laser cladding and / or laser metal deposition, and / or directed energy deposition.

[0065] <Statement J> 1. A method for finishing an additively manufactured metal-based object, comprising applying a sprayable formulation to the additively manufactured metal-based object, the sprayable formulation comprising 0.01-50 wt. % of at least one organic acid, 0.01-50 wt. % of a solid medium, and water.

[0066] <Statement K> The method of statement J, further comprising heating the chamber, wherein the formulation is provided at a temperature between 21 and 60 degrees Celsius.

[0067] <Statement L> The method of statement J or K, further comprising pressurizing the chamber, wherein the formulation is provided at a pressure of 0 to 80 psig.

[0068] <Statement M> The method of any of statements J, K, L, further comprising rotating a platform on which the additively manufactured metal-based object is placed as the formulation is being administered.

[0069] <Statement N> The method of any of statements J, K, L, and M, wherein the finishing process includes at least one of removing unwanted metal powder from the additively manufactured metal-based object, removing unwanted printed material from the additively manufactured metal-based object, removing unwanted support material from the additively manufactured metal-based object, reducing surface roughness of the additively manufactured metal-based object, removing oxidized surface material from the additively manufactured metal-based object, polishing the additively manufactured metal-based object, passivating the surface of the additively manufactured metal-based object, and stress relaxing the additively manufactured metal-based object.

[0070] <Statement O> 1. A system for finishing an additively manufactured metal-based object, comprising: A closed chamber; a platform within the closed chamber on which the additively manufactured metal-based object can be placed; and The system includes a spray nozzle positioned to direct a sprayable formulation toward the additively manufactured metal-based object placed on the platform, the sprayable formulation comprising 0.01-50% by weight of at least one organic acid, 0.01-50% by weight of a solid medium, and water.

[0071] <Statement P> 1. A method of providing a sprayable formulation for finishing an additively manufactured metal-based object, comprising: providing at least one organic acid in an amount of 0.01 to 50% by weight; Adding 0.01 to 50% by weight of a solid medium to the at least one organic acid; Adding water as needed.

[0072] <Statement Q> The method of statement P, wherein the at least one organic acid is provided in a concentrated form, further comprising adding water to the concentrated form to provide 0.01 to 50 wt. % of the at least one organic acid.

[0073] <Statement R> The method of statement P, wherein the at least one organic acid is provided in a powder form, further comprising adding water to the powder to provide 0.01-50 wt. % of the at least one organic acid.

[0074] Of course, various aspects of the invention described above, and other features and functions, or alternatives thereof, can be appropriately combined to form many other different systems or applications. Various alternatives, modifications, variations, or improvements that are not currently anticipated or foreseeable may be made by those skilled in the art in the future, and are also encompassed by the present invention. Although the embodiments of the present invention have been described above, the present invention is not limited to these embodiments. The present invention is considered to be limited only by the appended claims and the reasonable interpretation thereof. [Explanation of symbols]

[0075] The list of main items shown in Figure 1 is as follows: 7 Sprayable Fluids 10 equipment 19 Additive Manufacturing Parts 22 Turntable 25 Spray Chamber 28 Nozzles 31 Tank 34 Upper 37 Media Pump 40 Human Machine Interface (HMI) 43 Fluid conduit 46 Housing 61 Fans 67 Lattice 70 Clean-in-place (CIP) nozzle 73 Outlet 76 Slanted side 79 Port 82 Administration mechanism 85 Liquid level sensor 88 Valve 91 Heater 94 Valve 97 Vent 100 Valve 104 Air Pump 106 pH Sensor 109 Temperature Sensor 112 Pressure Sensor 115 Camera 118 CIP Pump 121 CIP System 124 CIP inlet

Claims

1. 1. A sprayable formulation for finishing metal-based objects formed by additive manufacturing, comprising: 0.01 to 50% by weight of at least one organic acid; 0.01 to 50% by weight of a solid medium; Contains water, A formulation wherein said solid medium has a size ranging from 0.1 to 1000 μm (micrometers).

2. 2. The sprayable formulation of claim 1, wherein the at least one organic acid is selected from formic acid, acetic acid, propionic acid, butyric acid, valeric acid, caproic acid, oxalic acid, lactic acid, malic acid, citric acid, ascorbic acid, benzoic acid, carbonic acid, glycine, sarcosine, glycolic acid, phenolic acid, uric acid, taurine, p-toluenesulfonic acid, trifluoromethanesulfonic acid, aminomethylphosphonic acid, maleic acid, succinic acid, palmitic acid, itaconic acid, fumaric acid, tartaric acid, boric acid, and combinations thereof.

3. 3. The sprayable formulation of claim 1 or 2, wherein the solid medium is selected from glass beads, steel, stainless steel, ceramic materials, aluminum oxide / alumina, silica, zirconium, silicon carbide, plastic, garnet, copper, corn cobs, walnut shells, mica, feldspar, pumice, and combinations thereof.

4. 4. The sprayable formulation of claim 1, 2 or 3, wherein the solid medium has a shape, appearance and / or surface that is spherical, elongated, irregular, jagged, angular, cubic, rectangular, cylindrical, and combinations thereof.

5. 5. The sprayable formulation of claim 1, 2, 3 or 4, wherein the finishing solution comprises a colloidal slurry.

6. 6. The sprayable formulation of claim 1, 2, 3, 4 or 5, wherein the metal-based object comprises a metal or metal alloy object.

7. 7. The sprayable formulation of claim 6, wherein the metal-based object comprises at least one of titanium, Ti6Al4V, aluminum, AlSi10Mg, Al6061, tool steels or cermets including H13, superalloys Inconel 625, Inconel 718, Stellite, stainless steels including BC4, 304L, 316, 320, or refractory materials including MoRe or Ta-W, CoCr, or combinations thereof.

8. 7. The sprayable formulation of claim 6, wherein the additive manufacturing process comprises a powder bed process including electron beam melting, direct metal laser sintering, selective laser melting, a powder feed process including laser cladding or laser metal deposition, or a directed energy deposition process.

9. 1. A method for finishing an additively manufactured metal-based object, comprising applying a sprayable formulation to the additively manufactured metal-based object, the sprayable formulation comprising 0.01-50% by weight of at least one organic acid, 0.01-50% by weight of a solid medium, and water, the solid medium having a size in the range of 0.1-1000 μm (micrometers).

10. 10. The method of claim 9, further comprising heating the chamber, wherein the formulation is provided at a temperature of 21 to 60 degrees Celsius.

11. 10. The method of claim 9, further comprising pressurizing the chamber, wherein the formulation is provided at a pressure of 0 to 80 psig.

12. 10. The method of claim 9, further comprising rotating a platform on which the additively manufactured metal-based object is mounted as the formulation is being dispensed.

13. 10. The method of claim 9, wherein the finishing step comprises at least one of removing unwanted metal powder from the additively manufactured metal-based object, removing unwanted printing material from the additively manufactured metal-based object, removing unwanted support material from the additively manufactured metal-based object, reducing surface roughness of the additively manufactured metal-based object, removing oxidized surface material from the additively manufactured metal-based object, polishing the additively manufactured metal-based object, passivating a surface of the additively manufactured metal-based object, and stress relaxing the additively manufactured metal-based object.

14. 1. A system for finishing an additively manufactured metal-based object, comprising: A closed chamber; a platform within the closed chamber on which the additively manufactured metal-based object can be placed; and 1. The system of claim 1, further comprising: a spray nozzle positioned to direct a sprayable formulation at the additively manufactured metal-based object mounted on the platform, the sprayable formulation comprising 0.01-50% by weight of at least one organic acid, 0.01-50% by weight of a solid medium, and water, the solid medium being in the size range of 0.1-1000 μm (micrometers).

15. A method of providing a sprayable formulation for finishing an additively manufactured metal-based object, comprising the steps of: providing 0.01 to 50% by weight of at least one organic acid; adding 0.01 to 50% by weight of a solid medium to the at least one organic acid; Add water if necessary.

11. The method of claim 10, further comprising providing the at least one organic acid in a concentrated, neat, or undiluted state, and further adding water to the concentrated, neat, or undiluted state to provide 0.01 to 50 wt. % of the at least one organic acid.

16. A method of providing a sprayable formulation for finishing an additively manufactured metal-based object, comprising the steps of: providing 0.01 to 50% by weight of at least one organic acid; adding 0.01 to 50% by weight of a solid medium to the at least one organic acid; Add water if necessary. The method includes providing the at least one organic acid in a powder form, and further adding water to the powder form to provide 0.01 to 50 weight percent of the at least one organic acid.

Citation Information

Patent Citations

  • Method for treating metal substrates

    JP2016528383A

  • Titanium implant surfaces free from alpha case and with enhanced osteoinduction

    WO2018026448A1

  • Method and apparatus for surface finishing and support material removal (DECI DUO)