Non-aqueous electrolyte secondary battery
By adding Ca and Al to lithium transition metal oxides and forming a protective film on the negative electrode, the battery's capacity retention and cycle life are enhanced, addressing the structural instability caused by high Ni content.
Patent Information
- Application Number
- JP2021558189
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-11-19
- Filing Date
- 2020-09-17
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-17
AI Technical Summary
Lithium transition metal oxides with high Ni content used as positive electrode active materials in non-aqueous electrolyte secondary batteries experience a decrease in battery capacity due to the destruction of the layered crystal structure during charging and discharging, leading to poor charge/discharge cycle characteristics.
Incorporating specific amounts of Ca and Al into the lithium transition metal oxide to stabilize the layered structure, with Ca being supplied to the negative electrode to form a protective film, enhancing the charge/discharge cycle characteristics.
The stabilization of the lithium transition metal oxide structure and suppression of side reactions improve the battery's capacity retention and cycle life.
Smart Images

Figure 0007573183000002 
Figure 0007573183000001
Abstract
Description
[Technical field]
[0001] The present disclosure relates to a non-aqueous electrolyte secondary battery. [Background technology]
[0002] In recent years, lithium transition metal oxides with a high Ni content have been attracting attention as a positive electrode active material with high energy density. For example, Patent Document 1 describes a lithium transition metal oxide having the general formula Li x Ni y Co z M m and a BET specific surface area of 0.8 m or less. 2 / g or less.
[0003] Patent Document 2 discloses a positive electrode active material for a nonaqueous electrolyte secondary battery, which has an α-NaFeO2 structure, contains one or more transition metal elements selected from the group consisting of Mn, Ni, and Co, and has an alkaline earth metal and W present on the particle surface of a lithium transition metal oxide. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2003-100295 A [Patent Document 2] JP 2018-129221 A Summary of the Invention
[0005] When a lithium transition metal oxide with a high Ni content is used as the positive electrode active material of a nonaqueous electrolyte secondary battery, the amount of Li extracted during charging is large, and there is a problem that the layered crystal structure is destroyed by repeated charging and discharging, and the battery capacity decreases. Note that the techniques disclosed in Patent Documents 1 and 2 still have room for improvement in terms of charge and discharge cycle characteristics.
[0006] A non-aqueous electrolyte secondary battery according to an embodiment of the present disclosure includes a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, and a non-aqueous electrolyte. The positive electrode active material includes a lithium transition metal oxide containing at least Ni, Ca, and Al, and having a layered structure including a Li layer into which Li reversibly enters and leaves, in which the Ni content in the lithium transition metal oxide is 80 mol% or more and 95 mol% or less with respect to the total amount of metal elements other than Li, the Ca content is more than 0 mol% and 3 mol% or less with respect to the total amount of metal elements other than Li, the Al content is more than 0 mol% and 8 mol% or less with respect to the total amount of metal elements other than Li, the ratio of metal elements other than Li present in the Li layer is 0.6 mol% or more and 2.0 mol% or less with respect to the total number of moles of metal elements other than Li contained in the lithium transition metal oxide, and the negative electrode active material has a coating containing Ca on its surface, and the ratio of Ca in the coating is 15 mass ppm or more and less than 80 mass ppm with respect to the total mass of the positive electrode active material.
[0007] According to the nonaqueous electrolyte secondary battery of one embodiment of the present disclosure, it is possible to suppress the decrease in battery capacity due to charging and discharging while having a high capacity. The positive electrode active material includes a lithium transition metal oxide having a high Ni content, and it is possible to provide a nonaqueous electrolyte secondary battery having excellent charge and discharge cycle characteristics. [Brief description of the drawings]
[0008] [Figure 1] FIG. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0009] The layered structure of the lithium transition metal oxide contained in the positive electrode active material contains a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the Li ions in the Li layer reversibly enter and exit the layered structure, which causes the charge and discharge reaction of the battery. When a lithium transition metal oxide with a high Ni content is used, many Li ions are extracted from the Li layer during charging of the battery, which can cause the layered structure to collapse and reduce the battery capacity. In particular, the surface of the lithium transition metal oxide is highly active and the layered structure is easily unstable, which can lead to the deterioration of the layered structure. In addition, as in the positive electrode, the negative electrode active material and the electrolyte can react with each other, causing the surface of the negative electrode active material to change.
[0010] Therefore, the present inventors have intensively studied to solve the above problems, and have found that the charge-discharge cycle characteristics are specifically improved by adding a predetermined amount of Ca to a lithium transition metal oxide containing Ni and Al, and replacing a part of Li in the Li layer with other metal elements. At this time, it was found that the effect is expressed when a coating is formed on the surface of the negative electrode active material by supplying Ca from the positive electrode to the negative electrode, and the Ca concentration in the coating is within a predetermined range. The structural stabilization of the Li layer by the replacement with other metal elements, the stabilization of the transition metal layer by the replacement with Al, the modification of the surface of the positive electrode active material by the addition of Ca, and the formation of a good coating containing Ca on the negative electrode active material suppress the secondary reaction between the positive electrode active material / negative electrode active material and the electrolyte, resulting in a specific synergistic effect, which is thought to have led to a significant improvement in the charge-discharge cycle characteristics.
[0011] An example of an embodiment of a nonaqueous electrolyte secondary battery according to the present disclosure will be described in detail below. A cylindrical battery in which a wound electrode body is housed in a cylindrical battery case will be exemplified below, but the electrode body is not limited to the wound type, and may be a laminate type in which a plurality of positive electrodes and a plurality of negative electrodes are alternately laminated one by one with a separator interposed therebetween. In addition, the battery case is not limited to a cylindrical shape, and may be, for example, a square shape, a coin shape, or the like, or may be a battery case made of a laminate sheet including a metal layer and a resin layer.
[0012] Fig. 1 is a cross-sectional view of a nonaqueous electrolyte secondary battery 10 according to an embodiment. As illustrated in Fig. 1, the nonaqueous electrolyte secondary battery 10 includes an electrode assembly 14, a nonaqueous electrolyte (not shown), and a battery case 15 that accommodates the electrode assembly 14 and the nonaqueous electrolyte. The electrode assembly 14 has a wound structure in which a positive electrode 11 and a negative electrode 12 are wound with a separator 13 interposed therebetween. The battery case 15 includes a cylindrical outer can 16 with a bottom, and a sealing body 17 that closes the opening of the outer can 16.
[0013] The electrode body 14 is composed of a long positive electrode 11, a long negative electrode 12, two long separators 13, a positive electrode tab 20 joined to the positive electrode 11, and a negative electrode tab 21 joined to the negative electrode 12. The negative electrode 12 is formed to have a size slightly larger than the positive electrode 11 in order to prevent lithium deposition. That is, the negative electrode 12 is formed to be longer in the longitudinal direction and width direction (short direction) than the positive electrode 11. The two separators 13 are formed to have a size at least slightly larger than the positive electrode 11, and are arranged to sandwich the positive electrode 11, for example.
[0014] The nonaqueous electrolyte secondary battery 10 includes insulating plates 18, 19 disposed above and below the electrode body 14. In the example shown in Fig. 1, a positive electrode tab 20 attached to the positive electrode 11 passes through a through hole in the insulating plate 18 and extends toward the sealing body 17, and a negative electrode tab 21 attached to the negative electrode 12 passes outside the insulating plate 19 and extends toward the bottom side of the outer can 16. The positive electrode tab 20 is connected to the lower surface of a bottom plate 23 of the sealing body 17 by welding or the like, and a cap 27 of the sealing body 17 electrically connected to the bottom plate 23 serves as a positive electrode terminal. The negative electrode tab 21 is connected to the inner bottom surface of the outer can 16 by welding or the like, and the outer can 16 serves as a negative electrode terminal.
[0015] The exterior can 16 is, for example, a cylindrical metal container with a bottom. A gasket 28 is provided between the exterior can 16 and the sealing body 17, and the internal space of the battery case 15 is sealed. The exterior can 16 has a grooved portion 22 that supports the sealing body 17 and is formed, for example, by pressing the side portion from the outside. The grooved portion 22 is preferably formed in an annular shape along the circumferential direction of the exterior can 16, and supports the sealing body 17 on its upper surface.
[0016] The sealing body 17 has a structure in which a bottom plate 23, a lower valve body 24, an insulating member 25, an upper valve body 26, and a cap 27 are laminated in this order from the electrode body 14 side. Each member constituting the sealing body 17 has, for example, a disk shape or a ring shape, and each member except the insulating member 25 is electrically connected to each other. The lower valve body 24 and the upper valve body 26 are connected to each other at their respective centers, and the insulating member 25 is interposed between their respective peripheral edges. When the internal pressure of the battery increases due to abnormal heat generation, the lower valve body 24 deforms and breaks so as to push the upper valve body 26 toward the cap 27, and the current path between the lower valve body 24 and the upper valve body 26 is interrupted. When the internal pressure further increases, the upper valve body 26 breaks, and gas is discharged from the opening of the cap 27.
[0017] The positive electrode 11, negative electrode 12, separator 13, and nonaqueous electrolyte that constitute the nonaqueous electrolyte secondary battery 10, and in particular the positive electrode active material contained in the positive electrode mixture layer 31 that constitutes the positive electrode 11, will be described in detail below.
[0018] [Positive electrode] The positive electrode 11 has a positive electrode current collector 30 and a positive electrode composite layer 31 formed on both sides of the positive electrode current collector 30. For the positive electrode current collector 30, a foil of a metal, such as aluminum or an aluminum alloy, that is stable in the potential range of the positive electrode 11, or a film having the metal disposed on the surface layer, can be used. The positive electrode composite layer 31 contains a positive electrode active material, a conductive material, and a binder. The thickness of the positive electrode composite layer 31 is, for example, 10 μm to 150 μm on one side of the positive electrode current collector 30. The positive electrode 11 can be produced by applying a positive electrode slurry containing a positive electrode active material, a conductive material, a binder, and the like to the surface of the positive electrode current collector 30, drying the coating, and then compressing it to form the positive electrode composite layer 31 on both sides of the positive electrode current collector 30.
[0019] Examples of the conductive material contained in the positive electrode mixture layer 31 include carbon materials such as carbon black, acetylene black, ketjen black, and graphite. Examples of the binder contained in the positive electrode mixture layer 31 include fluororesins such as polytetrafluoroethylene (PTFE) and polyvinylidene fluoride (PVdF), polyacrylonitrile (PAN), polyimide, acrylic resin, and polyolefin. These resins may be used in combination with carboxymethylcellulose (CMC) or a salt thereof, polyethylene oxide (PEO), or the like.
[0020] The positive electrode active material is included in the positive electrode composite layer 31 of the positive electrode 11. The positive electrode active material has a layered structure including a Li layer where Li reversibly enters and exits, and includes a lithium transition metal oxide containing at least Ni and Ca. Examples of the layered structure of the lithium transition metal oxide include a layered structure belonging to the space group R-3m and a layered structure belonging to the space group C2 / m. Among these, a layered structure belonging to the space group R-3m is preferable in terms of high capacity and stability of the crystal structure. The positive electrode active material may be mainly composed of a lithium transition metal oxide and substantially composed of only the lithium transition metal oxide. The positive electrode active material may include a composite oxide other than the lithium transition metal oxide or other compounds within a range that does not impair the object of the present disclosure.
[0021] The lithium transition metal oxide is, for example, a secondary particle formed by agglomeration of a plurality of primary particles. The particle size of the primary particles constituting the secondary particles is, for example, 0.05 μm to 1 μm. The particle size of the primary particles is measured as the diameter of a circumscribed circle in a particle image observed by a scanning electron microscope (SEM). The lithium transition metal oxide is a particle having a volume-based median diameter (D50) of, for example, 3 μm to 30 μm, preferably 5 μm to 25 μm, and particularly preferably 7 μm to 15 μm. D50 means a particle size at which the cumulative frequency is 50% from the smallest particle size in the volume-based particle size distribution, and is also called the median diameter. The particle size distribution of the lithium transition metal oxide can be measured using a laser diffraction type particle size distribution measuring device (for example, MT3000II manufactured by Microtrack Bell Co., Ltd.) using water as a dispersion medium.
[0022] In the lithium transition metal oxide, the Ni content is 80 mol% or more and 95 mol% or less, preferably 85 mol% or more and 92 mol% or less, based on the total amount of metal elements excluding Li. By making the Ni content 80 mol% or more, a battery with high energy density can be obtained. On the other hand, if the Ni content exceeds 95 mol%, the contents of Ca and other metal elements become too small to ensure the stability of the layered structure of the lithium transition metal oxide, and erosion of the particle surface cannot be suppressed.
[0023] In the lithium transition metal oxide, the content of Ca is more than 0 mol% and 3 mol% or less, preferably 1 mol% or less, based on the total amount of metal elements excluding Li. Ca has an effect of suppressing the erosion of the surface of the lithium transition metal oxide by the electrolyte due to electronic interaction, and it is considered that the cycle characteristics of the battery are improved if Ca is contained. Ca in the lithium transition metal oxide is, for example, Ca or a compound containing Ca. An example of a compound containing Ca is CaO.
[0024] Ca is preferably present on the particle surface of the lithium transition metal oxide and in its vicinity, for example, in a surface vicinity region within 30 nm from the particle surface. Since the lithium transition metal oxide is generally a secondary particle formed by agglomeration of a plurality of primary particles, Ca is preferably present at a higher concentration on the surface and in the vicinity of the primary particles, including the surface of the secondary particles, than in the center of the primary particles. That is, Ca is unevenly distributed on the surface and in its vicinity of the primary particles of the lithium transition metal oxide, and the content of Ca per unit volume is higher on the surface than inside the primary particles. Ca may be present as a compound, for example, on the particle surface of the lithium transition metal oxide or in the layered structure. The distribution of Ca in the lithium transition metal oxide can be analyzed by TEM-EDX or the like.
[0025] The content of Al in the lithium transition metal oxide is more than 0 mol% and at most 8 mol% with respect to the total amount of metal elements excluding Li, and preferably 2 mol% or more and 6 mol% or less. Since the oxidation number of Al does not change even during charge and discharge, it is considered that the structure of the transition metal layer is stabilized by being contained in the transition metal layer. However, when the content of Al exceeds 8 mol%, Al impurities are generated and the battery capacity decreases. Al may be uniformly dispersed in the layered structure of the lithium transition metal oxide, or may be present in a part of the layered structure. Further, Al may coexist with Ca in the particle surface and its vicinity of the lithium transition metal oxide, for example, in the surface vicinity region within 30 nm from the particle surface. Al in the lithium transition metal oxide may exist as Al, a compound containing Al, or a compound containing Ca and Al. Examples of the compound containing Al include Al2O3. Examples of the compound containing Ca and Al include Ca3Al2O6.
[0026] An example of a preferred lithium transition metal oxide is represented by the general formula Li a Ni x Al y M z Ca w O 2-b (wherein 0.95 < a < 1.05, 0.80 ≤ x ≤ 0.95, 0 ≤ y ≤ 0.08, 0 ≤ z ≤ 0.1, 0 < w ≤ 0.03, 0 ≤ b < 0.05, x + y + z + w = 1, and M is at least one element selected from Co, Mn, Fe, Ti, Si, Nb, Zr, Mo, and Zn) is a composite oxide. Preferably, M contains at least one of Co and Mn. The lithium transition metal oxide may contain at least one of Co and Mn, and may also contain at least one metal element selected from Fe, Ti, Si, Nb, Zr, Mo, and Zn. The molar fraction of the metal elements contained in the whole particles of the lithium transition metal oxide can be measured by an inductively coupled plasma atomic emission spectrometer (ICP-AES), an electron probe microanalyzer (EPMA), an energy dispersive X-ray analyzer (EDX), or the like.
[0027] The layered structure of the lithium transition metal oxide includes a transition metal layer such as Ni, a Li layer, and an oxygen layer, and the Li ions present in the Li layer reversibly enter and exit the Li layer, thereby allowing the charge and discharge reaction of the battery to proceed. The ratio of metal elements other than Li present in the Li layer is 0.6 mol% or more and 2.0 mol% or less, preferably 0.7 mol% or more and 1.9 mol% or less, more preferably 0.8 mol% or more and 1.8 mol% or less, relative to the total number of moles of metal elements other than Li contained in the lithium transition metal oxide. If it is within this range, the structure of the Li layer is stabilized in the state in which Li ions are extracted during charging, and the charge and discharge cycle characteristics are improved. On the other hand, if the ratio is less than 0.6 mol% or more than 2.0 mol%, the effect of improving the charge and discharge cycle characteristics cannot be obtained. The metal elements other than Li in the Li layer are considered to be mainly Ni, but may contain other metal elements.
[0028] The ratio of metal elements other than Li present in the Li layer is determined by Rietveld analysis of the X-ray diffraction pattern obtained by X-ray diffraction measurement of the lithium transition metal oxide. The X-ray diffraction pattern is obtained by a powder X-ray diffraction method under the following conditions using, for example, a powder X-ray diffractometer (manufactured by Rigaku Corporation, product name "RINT-TTR", radiation source Cu-Kα).
[0029] Measurement range: 15-120° Scan speed: 4° / min Analysis range: 30-120° Background: B-spline Profile function: Split pseudo-Voigt function Constraint condition: Li(3a)+Ni(3a)=1 Ni(3a)+Ni(3b)=y (y is the Ni content in each element) ICSD No.:98-009-4814 Rietveld analysis of the X-ray diffraction pattern can be performed using Rietveld analysis software PDXL2 (manufactured by Rigaku Corporation). In addition, it is preferable that the X-ray diffraction pattern of the lithium transition metal oxide does not have a peak derived from calcium oxide (CaO). If CaO is contained to an extent that can be detected by X-ray diffraction measurement, a decrease in charge / discharge capacity may occur.
[0030] Next, an example of a method for producing a positive electrode active material containing a lithium transition metal compound will be described.
[0031] The method for producing a positive electrode active material includes, for example, a first step of obtaining a composite oxide containing Ni and an arbitrary metal element, a second step of mixing the composite oxide obtained in the first step with a lithium compound to obtain a mixture, and a third step of firing the mixture. The ratio of metal elements other than Li in the Li layer of the layered structure of the finally obtained positive electrode active material is adjusted by controlling, for example, the mixing ratio of the raw materials in the second step and the firing temperature and time in the third step.
[0032] In the first step, for example, while stirring a solution of a metal salt containing Ni and an arbitrary metal element (Al, Co, Mn, Fe, etc.), an alkaline solution such as sodium hydroxide is dropped to adjust the pH to the alkaline side (e.g., 8.5 to 12.5), thereby precipitating (co-precipitating) a composite hydroxide containing Ni and the arbitrary metal element, and the composite hydroxide is calcined to obtain a composite oxide containing Ni and the arbitrary metal element. The calcination temperature is not particularly limited, but is, for example, in the range of 300°C to 600°C.
[0033] In the second step, the composite oxide obtained in the first step is mixed with a lithium compound and a calcium compound to obtain a mixture. Examples of the lithium compound include Li2CO3, LiOH, Li2O, LiNO3, LiNO2, Li2SO4, LiOH·H2O, LiH, and LiF. Examples of the calcium compound include Ca(OH)2, CaO, CaCO3, CaSO4, and Ca(NO3)2. The mixing ratio of the composite oxide obtained in the first step and the lithium compound is preferably such that, for example, the molar ratio of metal elements other than Li:Li is in the range of 1:0.98 to 1:1.1, in order to easily adjust each of the parameters to the ranges specified above. In addition, the mixing ratio of the composite oxide obtained in the first step and the calcium compound is preferably such that, for example, the molar ratio of metal elements other than Li:Ca is in the range of 1:0.0005 to 1:0.02, in order to easily adjust each of the parameters to the ranges specified above. In the second step, when the composite oxide obtained in the first step is mixed with the lithium compound and the calcium compound, other metal raw materials may be added as necessary. The other metal raw materials are oxides or the like containing metal elements other than the metal elements constituting the composite oxide obtained in the first step.
[0034] In the third step, the mixture obtained in the second step is fired at a predetermined temperature and time to obtain the positive electrode active material according to the present embodiment. The firing of the mixture in the third step includes a multi-stage firing process including a first firing process in which the mixture is fired in a firing furnace under oxygen flow at a first heating rate to a first set temperature of 450°C to 680°C, and a second firing process in which the fired product obtained in the first firing process is fired in a firing furnace under oxygen flow at a second heating rate to a second set temperature of more than 680°C to 800°C. Here, the first heating rate is in the range of 1.5°C / min to 5.5°C / min, and the second heating rate is slower than the first heating rate and is in the range of 0.1°C / min to 3.5°C / min. By such multi-stage firing, the ratio of metal elements other than Li present in the Li layer in the finally obtained positive electrode active material of the present embodiment can be adjusted to 0.6 mol% or more to 2.0 mol% or less. The first heating rate and the second heating rate may be set in a plurality of rates for each temperature range, so long as they are within the ranges specified above. The holding time of the first set temperature in the first firing step is preferably 5 hours or less, more preferably 3 hours or less, in terms of adjusting each of the parameters of the lithium transition metal oxide to the ranges specified above. The holding time of the first set temperature is the time during which the first set temperature is maintained after the first set temperature is reached. The holding time of the second set temperature in the second firing step is preferably 1 hour to 10 hours, more preferably 1 hour to 5 hours, in terms of adjusting each of the parameters of the lithium transition metal oxide to the ranges specified above. The holding time of the second set temperature is the time during which the second set temperature is maintained after the second set temperature is reached. When firing the mixture, in terms of adjusting each of the parameters to the ranges specified above, the firing is performed, for example, in an oxygen stream with an oxygen concentration of 60% or more, and the flow rate of the oxygen stream is set to 10 cm / s of the firing furnace. 3 The flow rate can be in the range of 0.2 mL / min to 4 mL / min per kg of mixture and 0.3 L / min or more per kg of mixture.
[0035] [Negative electrode] The negative electrode 12 has a negative electrode current collector 40 and a negative electrode composite layer 41 formed on both sides of the negative electrode current collector 40. For the negative electrode current collector 40, a foil of a metal stable in the potential range of the negative electrode 12, such as copper or a copper alloy, or a film having the metal disposed on the surface layer can be used. The negative electrode composite layer 41 contains a negative electrode active material and a binder. The thickness of the negative electrode composite layer 41 is, for example, 10 μm to 150 μm on one side of the negative electrode current collector 40. The negative electrode 12 can be produced by applying a negative electrode composite slurry containing a negative electrode active material, a binder, and the like to the surface of the negative electrode current collector 40, drying the coating, and then rolling to form the negative electrode composite layer 41 on both sides of the negative electrode current collector 40.
[0036] The negative electrode active material contained in the negative electrode mixture layer 41 is not particularly limited as long as it can reversibly absorb and release lithium ions, and includes carbon materials such as graphite. The graphite may be any of natural graphite such as flake graphite, lump graphite, and earthy graphite, lump artificial graphite, and artificial graphite such as graphitized mesophase carbon microbeads.
[0037] The negative electrode active material has a coating film containing Ca on its surface. The ratio of Ca in the coating film is 15 ppm by mass or more and less than 80 ppm by mass with respect to the total mass of the positive electrode active material. If the ratio is within this range, the charge-discharge cycle characteristics are improved.
[0038] The negative electrode active material may further contain Ni in the coating. Ni, for example, is transferred from the positive electrode and supplied to the negative electrode. Ni may be preliminarily contained in the negative electrode active material. The molar ratio of the Ca content to the Ni content in the coating is preferably 0.5≦Ca / Ni≦1.0. If it is within this range, the charge / discharge cycle characteristics are further improved. The Ca and Ni contents in the coating of the negative electrode active material can be analyzed by TEM-EDX or the like.
[0039] The negative electrode active material may include metals such as Si and Sn that are alloyed with Li, metal compounds containing Si and Sn, and lithium-titanium composite oxides. These may also be provided with a carbon coating. For example, SiO x Si-containing compounds represented by (0.5≦x≦1.6) or Li 2y SiO(2+y) Si-containing compounds in which fine particles of Si are dispersed in a lithium silicate phase represented by (0 < y < 2) may be used in combination with graphite.
[0040] As the binder contained in the negative electrode composite layer 41, fluorine-containing resins such as PTFE and PVdF, PAN, polyimide, acrylic resin, polyolefin, etc. may be used as in the case of the positive electrode 11, but preferably styrene-butadiene rubber (SBR) is used. Further, the negative electrode composite layer 41 may contain CMC or its salt, polyacrylic acid (PAA) or its salt, polyvinyl alcohol (PVA), etc.
[0041] [Separator] For the separator 13, for example, a porous sheet having ion permeability and insulation is used. Specific examples of the porous sheet include microporous thin films, woven fabrics, non-woven fabrics, etc. As the material of the separator 13, polyolefins such as polyethylene and polypropylene, cellulose, etc. are suitable. The separator 13 may have a single-layer structure or a laminated structure. Further, a resin layer with high heat resistance such as an aramid resin or a filler layer containing an inorganic compound filler may be provided on the surface of the separator 13.
[0042] [Non-aqueous electrolyte] The non-aqueous electrolyte contains, for example, a non-aqueous solvent and an electrolyte salt dissolved in the non-aqueous solvent. As the non-aqueous solvent, for example, esters, ethers, nitriles such as acetonitrile, amides such as dimethylformamide, and mixed solvents of two or more of these can be used. The non-aqueous solvent may contain a halogen-substituted product in which at least a part of the hydrogen of these solvents is substituted with a halogen atom such as fluorine. Examples of the halogen-substituted product include fluorinated cyclic carbonates such as fluoroethylene carbonate (FEC), fluorinated chain carbonates, and fluorinated chain carboxylic acid esters such as methyl fluoropropionate (FMP).
[0043] Examples of the esters include cyclic carbonates such as ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate; chain carbonates such as dimethyl carbonate (DMC), ethyl methyl carbonate (EMC), diethyl carbonate (DEC), methyl propyl carbonate, ethyl propyl carbonate, and methyl isopropyl carbonate; cyclic carboxylates such as γ-butyrolactone (GBL) and γ-valerolactone (GVL); and chain carboxylates such as methyl acetate, ethyl acetate, propyl acetate, methyl propionate (MP), and ethyl propionate (EP).
[0044] Examples of the ethers include 1,3-dioxolane, 4-methyl-1,3-dioxolane, tetrahydrofuran, 2-methyltetrahydrofuran, propylene oxide, 1,2-butylene oxide, 1,3-dioxane, 1,4-dioxane, 1,3,5-trioxane, furan, 2-methylfuran, 1,8-cineole, cyclic ethers such as crown ethers, 1,2-dimethoxyethane, diethyl ether, dipropyl ether, diisopropyl ether, dibutyl ether, dihexyl ether, ethyl vinyl ether, butyl vinyl ether, methyl phenyl ether, and the like. and chain ethers such as ethyl phenyl ether, butyl phenyl ether, pentyl phenyl ether, methoxytoluene, benzyl ethyl ether, diphenyl ether, dibenzyl ether, o-dimethoxybenzene, 1,2-diethoxyethane, 1,2-dibutoxyethane, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol dibutyl ether, 1,1-dimethoxymethane, 1,1-diethoxyethane, triethylene glycol dimethyl ether, and tetraethylene glycol dimethyl ether.
[0045] The electrolyte salt is preferably a lithium salt. Examples of lithium salts include LiBF4, LiClO4, LiPF6, LiAsF6, LiSbF6, LiAlCl4, LiSCN, LiCF3SO3, LiCF3CO2, Li(P(C2O4)F4), LiPF6-x (C n F 2n+1 ) x (1 < x < 6, n is 1 or 2), LiB 10 Cl 10 , LiCl, LiBr, LiI, lithium chloroborane, lithium lower aliphatic carboxylate, borate salts such as Li2B4O7, Li(B(C2O4)F2), LiN(SO2CF3)2, LiN(C1F 2l+1 SO2)(C m F 2m+1 SO2){l, m are integers of 0 or more}, and imide salts such as these may be mentioned. The lithium salt may be used alone or in combination of two or more. Among these, from the viewpoints of ionic conductivity, electrochemical stability, etc., it is preferable to use LiPF6. The concentration of the lithium salt is, for example, 0.8 mol to 1.8 mol per 1 L of the non-aqueous solvent. Further, vinylene carbonate or a propane sultone-based additive may be added.
[0046] [Preparation of Positive Electrode Active Material] Hereinafter, the present disclosure will be further described by way of examples and comparative examples, but the present disclosure is not limited to the following examples.
[0047] [Preparation of Positive Electrode Active Material] [Example 1] General formula Ni 0.91 Co 0.05 Al 0.04 O2, the metal composite oxide and calcium hydroxide (Ca(OH)2) were mixed so that the content of Ca was 0.1 mol% with respect to the total amount of Ni, Co, and Al, and further lithium hydroxide monohydrate (LiOH·H2O) was mixed so that the molar ratio of the total amount of Ni, Co, Al, and Ca to Li was 1:1.02. The mixture was calcined from room temperature to 650 °C at a heating rate of 2 °C / min under an oxygen stream with an oxygen concentration of 95% (flow rate of 10 L / min per 1 kg of the mixture), and then from 650 °C to 720 °C at a heating rate of 1 °C / min. The calcined product was washed with water to remove impurities, and the positive electrode active material of Example 1 was obtained. As a result of analyzing the composition of the positive electrode active material of Example 1 by ICP-AES, Li 0.99 Ni0.909 Co 0.05 Al 0.04 Ca 0.001 It was O2.
[0048] [Preparation of positive electrode] The above positive electrode active material was mixed in a ratio of 95 parts by mass, 3 parts by mass of acetylene black as a conductive material, and 2 parts by mass of polyvinylidene fluoride as a binder, and this was mixed with N-methyl-2-pyrrolidone (NMP) to prepare a positive electrode slurry. Next, the slurry was applied to a positive electrode current collector made of aluminum foil with a thickness of 15 μm, and after drying the coating film, the coating film was rolled with a rolling roller and cut into a predetermined electrode size to obtain a positive electrode in which a positive electrode composite layer was formed on both sides of the positive electrode core. In addition, an exposed portion in which the surface of the positive electrode core was exposed was provided in a part of the positive electrode. Positive electrodes were also prepared in the same manner in other examples and comparative examples.
[0049] [Preparation of negative electrode] Natural graphite was used as the negative electrode active material. The negative electrode active material, sodium carboxymethylcellulose (CMC-Na), and styrene-butadiene rubber (SBR) were mixed in an aqueous solution at a solid content mass ratio of 100:1:1 to prepare a negative electrode composite slurry. The negative electrode composite slurry was applied to both sides of a negative electrode core made of copper foil, and the coating film was dried. The coating film was then rolled using a rolling roller and cut to a predetermined electrode size to obtain a negative electrode in which a negative electrode composite layer was formed on both sides of the negative electrode core. An exposed portion was provided in part of the negative electrode, where the surface of the negative electrode core was exposed.
[0050] [Preparation of non-aqueous electrolyte] Ethylene carbonate (EC), methyl ethyl carbonate (MEC), and dimethyl carbonate (DMC) were mixed in a volume ratio of 3:3:4. Lithium hexafluorophosphate (LiPF6) was dissolved in the mixed solvent to a concentration of 1.2 mol / L to prepare a non-aqueous electrolyte.
[0051] [Preparation of test cell] An aluminum lead was attached to the exposed portion of the positive electrode, and a nickel lead was attached to the exposed portion of the negative electrode, and the positive and negative electrodes were spirally wound with a polyolefin separator interposed therebetween, and then pressed in the radial direction to produce a flat wound electrode body. This electrode body was placed in an exterior body, and the nonaqueous electrolyte was injected, and the opening of the exterior body was sealed to obtain a test cell.
[0052] [Evaluation of capacity retention rate] The test cell was subjected to the following cycle test. The discharge capacity at the first cycle and the discharge capacity at the 30th cycle of the cycle test were obtained, and the capacity retention rate was calculated by the following formula.
[0053] Capacity retention rate (%) = (30th cycle discharge capacity ÷ 1st cycle discharge capacity) × 100 <Cycle test> The test cell was charged at a constant current of 0.2 It in a temperature environment of 25°C until the battery voltage reached 4.2 V, and then charged at a constant voltage until the current value reached 1 / 100 It at 4.2 V. Then, the test cell was discharged at a constant current of 0.2 It until the battery voltage reached 2.5 V. This charge / discharge cycle was repeated 30 times.
[0054] <Examples 2 to 6 and Comparative Examples 1 to 7> Test cells were prepared in the same manner as in Example 1, except that the raw materials used, the raw material compounding ratio, and the manufacturing conditions (the molar ratio of Li to the total amount of metal elements other than Li, and the second-stage firing temperature) were changed to synthesize lithium transition metal oxides (positive electrode active materials) having the compositions shown in Table 1, and then the test cells were evaluated.
[0055] Table 1 shows the evaluation results of the capacity retention rate. Table 1 also shows the ratio of metal elements other than Li present in the Li layer to the total number of moles of metal elements other than Li, the ratio of Ca contained in the negative electrode active material to the total mass of the positive electrode active material, and the molar ratio of the Ca content to the Ni content in the coating of the negative electrode active material. Powder X-ray diffraction measurements were performed on the lithium transition metal oxides of the examples and comparative examples under the conditions described above to obtain X-ray diffraction patterns. From all the X-ray diffraction patterns of the examples and comparative examples, diffraction lines showing a layered structure were confirmed, and no peaks of CaO were confirmed.
[0056] [Table 1]
[0057] As shown in Table 1, the test cells of Examples 1-6 had higher capacity retention rates than any of the test cells of Comparative Examples 1-7. [Explanation of symbols]
[0058] 10 Nonaqueous electrolyte secondary battery 11 Positive electrode 12 Negative electrode 13 Separator 14 Electrode body 15 Battery case 16 Outer can 17 Sealing body 18,19 Insulating plate 20 Positive tab 21 Negative electrode tab 22 Grooved part 23 Bottom plate 24 Lower valve body 25 Insulating materials 26 Upper valve 27 Cap 28 Gasket 30 Positive electrode current collector 31 Positive electrode mixture layer 40 Negative electrode current collector 41 Negative electrode composite layer
Claims
1. A non-aqueous electrolyte secondary battery comprising a positive electrode including a positive electrode active material, a negative electrode including a negative electrode active material, and a non-aqueous electrolyte, The positive electrode active material includes a lithium transition metal oxide having a layered structure including a Li layer through which Li reversibly enters and exits, and containing at least Ni, Ca, and Al; In the lithium transition metal oxide, The content of Ni is 80 mol % or more and 95 mol % or less based on the total amount of metal elements excluding Li, The Ca content is more than 0 mol % and 3 mol % or less based on the total amount of metal elements excluding Li, The content of Al is more than 0 mol % and 8 mol % or less based on the total amount of metal elements excluding Li, a ratio of metal elements other than Li present in the Li layer is 0.6 mol % or more and 2.0 mol % or less with respect to the total number of moles of metal elements other than Li contained in the lithium transition metal oxide, the negative electrode active material has a Ca-containing coating on its surface, a ratio of Ca in the coating is 15 ppm by mass or more and less than 80 ppm by mass with respect to the total mass of the positive electrode active material.
2. The nonaqueous electrolyte secondary battery according to claim 1 , wherein the negative electrode active material further contains Ni in the coating.
3. 3. The nonaqueous electrolyte secondary battery according to claim 2, wherein a molar ratio of a Ca content to a Ni content in said coating is 0.5≦Ca / Ni≦1.0.
Citation Information
Patent Citations
Material used as positive electrode of lithium ion battery and preparation method therefor
CN105355878A
Electrical discharge machining device
JP1981015926A
Brake gear for winch* etc*
JP1981082796A
Positive electrode material for lithium secondary battery and manufacturing method thereof
JP2003100295A
Nonaqueous electrolyte battery
JP2013030284A