Apparatus with laminated glazing for vehicles and associated near infrared viewing system - Patents.com
The laminated glazing system with optimized glass compositions and anti-reflection coatings improves near-infrared transmission and reduces heat absorption, addressing inefficiencies in existing systems and enhancing comfort and economy.
Patent Information
- Application Number
- JP2022517712
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-09-20
- Filing Date
- 2020-09-18
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-09-18
AI Technical Summary
Existing laminated glazing systems for vehicles, particularly those incorporating LIDAR, suffer from suboptimal performance in near-infrared transmission and reflection, leading to reduced efficiency and increased heat absorption, which affects comfort and economy.
A laminated glazing design featuring a first glass sheet with reduced iron oxide content and an anti-reflection coating, combined with a second glass sheet having higher iron oxide content and strategically placed through holes, optimized for near-infrared transmission and reflection management.
Enhances near-infrared transmission by up to 3% while reducing heat absorption, improving comfort and reducing material costs by eliminating the need for a second extra-clear glass sheet.
Smart Images

Figure 0007573347000001 
Figure 0007573347000002 
Figure 0007573347000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminated glazing, in particular a windshield, in particular in road and rail vehicles, in association with a viewing system in the near infrared. The invention also describes an apparatus for combining said glazing with a viewing system. [Background technology]
[0002] Glazing and related technology for autonomous vehicles is constantly evolving, among other things, to improve safety.
[0003] Laser remote sensing or LIDAR is an acronym for the English expression "light detection and ranging" or "laser detection and ranging" and is available in autonomous vehicles at the headlights.
[0004] More recently, WO 2018 / 0153012 proposes placing a LIDAR operating in the near infrared, between 750 nm and 1050 nm, behind a laminated windshield having two pieces of extra clear glass and an infrared filter. [Prior art documents] [Patent documents]
[0005] [Patent Document 1] International Publication No. 2018 / 0153012 Summary of the Invention
[0006] The performance of this viewing device (glazing combined with LIDAR) leaves room for improvement.
[0007] More broadly, the invention also covers devices using infrared and visible range, ie, multispectral, viewing systems.
[0008] More specifically, the invention relates to laminated glazing (and / or convex glazing), in particular for road vehicles (passenger cars, trucks, public transport: buses, coaches, etc.) or rail vehicles (in particular for metro, tramways, in particular with a maximum speed of up to 90 km / h or up to 70 km / h), in particular convex, in particular for windscreens, but also rear windows, but also for side windows, of a certain thickness E1, for example in the sub-centimeter range, in particular for road vehicle windscreens up to 5 mm, The glazing comprises: a first glass sheet intended to be an exterior glazing, in particular of convex shape, having an outer first main surface F1 and an inner second main surface F2 oriented towards the passenger compartment, which in the case of a motor vehicle preferably has a thickness of at most 4 mm, or even at most 3 mm or 2.5 mm, in particular 2.1 mm, 1.9 mm, 1.8 mm, 1.6 mm and 1.4 mm, also preferably at least 0.7 mm or 1 mm, a laminate interlayer (single or multi-ply), preferably made of a thermoplastic polymeric material and even better made of polyvinyl butyral (PVB), possibly coloured neutral, clear, extra clear or especially grey or green, with a thickness of preferably at most 1.8 mm, better at most 1.2 mm or even at most 0.9 mm (or even better at least 0.3 mm or even at least 0.6 mm) for road vehicles, the laminate interlayer having a cross section that decreases in a wedge shape from the top to the bottom of the laminated glazing (in particular the windscreen), possibly for sound insulation and / or possibly for a head-up display (HUD, for Head Up Display in English), the laminate interlayer having a main surface Fa oriented towards F2 and a main surface Fb opposite to Fa, a second glass sheet, preferably convex and in particular tinted, intended to be an inner glazing, having a third main surface F3 on the F2 side and an inner fourth main surface F4 oriented towards the vehicle interior, which in the case of road vehicles preferably has a thickness thinner than the thickness of the first glazing, and even at most 3 mm or 2 mm, in particular 1.9 mm, 1.8 mm, 1.6 mm and 1.4 mm, or even at most 1.3 mm, and preferably at least 0.7 mm, the thickness of the first and second glass sheets being preferably strictly less than 5 or 4 mm, even less than 3.7 mm.
[0009] The first glass sheet has, on its face F2, an anti-reflective coating, preferably localized and at at least one wavelength referred to as the operating wavelength in the infrared in the range extending from 800 nm to 1800 nm, in particular from 850 nm to 1600 nm, with a free surface (the surface not covered by the laminate interlayer and the second glass sheet) with holes penetrating through the thickness of the interlayer and through the thickness of the second glass sheet.
[0010] The first glass sheet is based in particular on silica, soda lime, soda lime silica (preferred), or aluminosilicate, or borosilicate, and has a weight content of total iron oxide (expressed in the form of Fe2O3) of max. 0.05% (500 ppm), preferably max. 0.03% (300 ppm) or max. 0.015% (150 ppm) and in particular 0.005% or more.
[0011] The second glass sheet is in particular based on silica, soda lime, preferably soda lime silica (like the first glass sheet), but also on aluminosilicates or borosilicates, and has a weight content of total iron oxide (expressed in the form Fe2O3) of at least 0.4% and preferably at most 1.5%.
[0012] Thus, according to the invention, in order to reach a high transmission level, the following are selected: 1) Extra clear outer glass targeted at near infrared light; 2) the inner glass, which is more absorbent in the targeted near infrared and is necessarily hollowed out; 3) A recessed stack interlayer to enable the use of an anti-reflective coating on the F2 surface in the targeted near infrared.
[0013] This solution outperforms prior art solutions based on two complete pieces of extra clear glass.
[0014] This solution also improves comfort (heat inside the vehicle), aesthetics, and is more economical by avoiding the use of a second extra clear glass.
[0015] The invention is particularly suitable for glazing (windshields, rear windows, etc.) in autonomous or semi-autonomous vehicles of levels L2+, L3, L4 and L5 ("full" autonomy), as well as in vehicles such as robotaxis and shuttle types.
[0016] Iron oxide is present as an impurity in most of the natural raw materials used in glass products (sand, feldspar, limestone, dolostone, etc.) and absorbs in the visible and near-ultraviolet light range (ferric ion, Fe 3+ absorption due to ferrous ions, Fe 2+ absorption due to SiO 2 ), and therefore the iron oxide in the first glass sheet is reduced.
[0017] In the second glass sheet a higher iron oxide content can therefore be chosen.
[0018] Advantageously, the assembly of the first glass sheet and said anti-reflective coating exhibits: a total transmittance of at least 90.0%, 91.0%, or even 92.0% or 92.3%, in particular at an operating wavelength of 905±5 nm and / or 1550±5 nm, measured normal (90°) or even preferably at 60° or even up to 60° to the (local) plane of the first sheet, e.g. the F2-side and / or the F1-side and / or the anti-reflective coating increases the total transmittance of the first glass sheet, measured normal (90°) or even preferably at 60° or even up to 60° to the (local) plane of the first sheet, e.g. the F2 side and / or the F1 side, by at least 1%, 2% or 2.5% or even 3.0% at the operating wavelength.
[0019] The angle of glazing, especially windshields on road vehicles, can typically be 21° to 36° with respect to the ground, with an average of 30°. Therefore, high transmission at 60° is particularly advantageous, since if the windshield is at 30° from the ground, that is the angle of incidence of the LIDAR beam on the windshield.
[0020] The transmittance in the infrared is measured using a Fourier spectrometer, such as a Bruker Vertex-70.
[0021] Naturally, if a multispectral viewing system is used, it is also desirable that the assembly of the first glass sheet and said anti-reflective coating exhibit: a total transmittance of at least 90%, 91% or even 92% at another operating wavelength, in particular in the visible range of 500 nm to 600 nm, measured normal or even preferably from 90° to 60° to the plane of the first sheet, e.g. the F2 and / or F1 side; and / or the anti-reflective coating increases the total transmittance of the first glass sheet, measured normal or even preferably from 90° to 60° relative to the plane of the first sheet, e.g. the F2 side and / or the F1 side, by at least 1%, 2% or 2.5% or even 3.0% at the second operating wavelength.
[0022] The transmittance of glass in the visible range is often expressed as a quantity called "T L ", a light transmission coefficient called light transmittance is defined, which is calculated according to standard ISO 9050:2003, i.e. taking into account the D65 illuminant as defined by standard ISO / CIE 10526 and the CIE 1931 colorimetric standard observer as defined by standard ISO / CIE 10527, from 380 to 780 nm, and is returned to a glass thickness of 3.2 mm or 4 mm.
[0023] Consequently, the light transmittance T of the laminated glazing in the non-perforated zone (the central zone of the windshield) L is preferably at least 70% or 75%, 80% or 85%, 88%.
[0024] The second glass sheet is inter alia green, blue or grey. The second glass sheet can be green with Fe2O3, or alternatively blue with CoO and Se, or grey with Se and CoO.
[0025] Mention may be made, inter alia, of the Applicant's glasses designated TSAnx (0.5-0.6% iron), TSA2+, TSA3+ (0.8-0.9% iron), TSA4+ (1% iron), TSA5+, which are green in colour.
[0026] TSA3+ (2.1 mm), for example, has a total transmittance of approximately 40% at 905 nm and approximately 50% at 1550 nm.
[0027] The second glass sheet may exhibit a redox, defined as the ratio between the weight content of FeO (ferrous iron) and the weight content of total iron oxide (expressed in the form of Fe2O3), of between 0.22 and 0.35 or 0.30.
[0028] The second glass sheet may have a chemical composition comprising the following components in varying contents within weight limits defined as follows: SiO264~75% Al2O30-5% B2O30~5% CaO 2~15% MgO 0~5% Na2O 9~18% K2O 0~5% SO30.1~0.35% Fe2O3 (total iron) at least 0.4% or even 0.4-1.5% In some cases, redox 0.22-0.3% And especially less than 0.1% impurities.
[0029] The through hole thus consists of: a first hole through the laminate intermediate layer (single or multi-layer) of width D1 - and a second hole through the second glass sheet, of width D2. The first and second holes have a common or close axis of symmetry and preferably the same width (before lamination or even after lamination).
[0030] The through holes (first and second holes) can be: - closed holes (surrounded by the wall of the second glass sheet), i.e. holes located inside the glazing and in particular at least 3 cm or 5 cm away from the nearest glazing edge - (peripheral) Forming a notch, patent or open.
[0031] The through holes are preferably located in the peripheral zone of the laminated glazing, preferably at the upper longitudinal edge and / or in the peripheral central region, and the anti-reflective coating is locally located in this peripheral region.
[0032] The through holes have a given shape, for example trapezoidal or rectangular or round or oval, in particular with a convex cross section. The anti-reflection coating can have a similar shape.
[0033] If necessary, it is possible to envisage a plurality of through holes (two or three holes) of the same shape and / or dimensions in the intermediate layer and in the second glass sheet, for example side-by-side in this peripheral zone in particular. The F2 surface then has a common anti-reflection coating with a free surface for all holes, or a separate local anti-reflection (AR) coating for each hole, and for example the local AR coatings have different thicknesses.
[0034] The shape and dimensions of the through holes are set in accordance with the prior art so as to effectively and selectively collect the entirety of the radiation penetrating the glazing (windshield, rear window, etc.) and, in particular in the case of LIDAR, the entirety of the reflected light originating from a range of solid angles that are outside the vehicle and originate from the zone in front of the vehicle that is to be captured through the LIDAR.
[0035] For example, the hole may be the same shape as an infrared viewing system such as LIDAR.
[0036] The holes (open or closed) can particularly preferably be of trapezoidal, or also circular or oval or ellipsoidal or also rectangular, square, etc., especially of convex cross section.
[0037] If the hole is a notch, part of this notch will be obscured by the frame of the glazing and therefore will not function for the viewing system, as will a hole that is closed and too close to the edge.
[0038] If the hole is closed, the edge of the hole closest to the edge of the glazing (preferably in the upper longitudinal direction and especially in the central zone) is preferably at least 2 cm or 3 cm or better still 5 cm away from this edge of the glazing (of the second sheet).
[0039] The hole can be in the central zone of the upper longitudinal edge of the windshield, i.e. in the usual zone of the interior rear-view mirror (adjacent to the hole or in some vehicles the rear-view mirror is removed), a zone where the masking layer of the F2 and / or Fa surfaces is generally thicker than on the lateral zones (passenger, driver, etc.) along the upper edge.
[0040] Preferably, the holes have a cross section, especially of the trapezoidal or disc or oval type, - the smaller dimension of which is at least 5 cm (for example to fit the dimensions of an infrared viewing system) - and preferably the larger dimension (especially the larger side or diameter) is at most 40 cm, 30 cm, 25 cm, 20 cm (for mechanical reasons). Also preferably, the anti-reflective coating occupies a surface area encompassing the hole and is a maximum of 40cm or 30cm in length.
[0041] In particular, the cross section is quadrilateral, in particular rectangular or trapezoidal, with: - the so-called upper first (large) side or upper longitudinal edge (closest to the upper longitudinal edge of the glazing), which is preferably parallel to the upper longitudinal edge of the glazing and which is preferably at most 30 cm, 20 cm or 15 cm or 12 cm long and in particular spaced at least 5 cm or 6 cm from the edge (of the upper longitudinal edge of the glazing); - the so-called lower second (large) side or lower longitudinal edge (farthest from the edge of the upper longitudinal edge of the glazing and closer to the central zone), which is preferably parallel to the edge of the upper longitudinal edge of the glazing and which is preferably at most 35 cm or 30 cm or 25 cm or 20 cm long, and which is preferably longer than the length of the first large side - a height (between said first and second large sides) which is preferably at least 5 cm or even at most 15 cm.
[0042] Optionally, the through holes are along the lateral edges.
[0043] In the case of a rear window, the through-holes can be peripheral, along the (especially upper) longitudinal edges or along the lateral edges.
[0044] By necessity, the through hole is an empty space, or at least a space that is not filled (in its center) with any material that is absorptive in the targeted near infrared, which might be between the anti-reflective coating and the infrared viewing system.
[0045] However, it is possible to prepare inserts (closed, open), for example made of flexible polymeric material (polycarbonate, polyamide, polyolefin, polypropylene, etc.), in particular up to 1.5 cm wide, of ring type (monolithic or made of several separate or connected pieces, etc.), which inserts: - attached (in particular by gluing or by force) to the wall of the second glass sheet which defines (at the top) the hole - and also in contact with the wall of the laminate interlayer and also on the F2 surface.
[0046] The insert can extend beyond the hole, particularly onto the F4 face.
[0047] This insert is used for: - for placing in the hole all or part of an infrared viewing system or intermediate optical components between the anti-reflection coating and the infrared viewing system; - for locating all or part of the fixing means of an infrared viewing system in the hole.
[0048] If the holes in the intermediate layer are made before lamination and an insert is placed at the intermediate layer before lamination (especially at up to 150° C. and especially under pressure), this insert serves to avoid or reduce creep of the intermediate layer on the free surface of the antireflective coating.
[0049] In particular the local anti-reflection coating may extend between the F2 and Fa planes, preferably by a maximum of 100 mm, 50 mm, 30 mm or 20 mm or 10 mm.
[0050] Anti-reflective coatings may include a stack of thin dielectric layers (eg, oxides and / or nitrides of metals or silicon) with alternating high and low refractive indices (at the operating wavelength).
[0051] The anti-reflective coating preferably comprises a porous silica (functional) layer, preferably a sol-gel.
[0052] In a first embodiment, the pores are the interstices of a loose stack of nanometric beads, especially of silica, which layers are described, for example, in US Patent Application Publication No. 2004 / 0258929.
[0053] In a second embodiment, the porous layer is obtained by deposition of a condensed silica sol (silica oligomers) densified by NH3 type vapors, this layer being described for example in WO 2005 / 049757.
[0054] In a third embodiment, the porous layer can also be of the sol-gel type, as described in EP 1 329 433. The porous layer can also be obtained using other known foaming agents, such as micelles of cationic surface-active molecules in solution and optionally in hydrolyzed form, or micelles of anionic surfactants, micelles of nonionic surfactants, or amphiphilic molecules, such as block copolymers.
[0055] In a fourth embodiment, the porous layer can also be of the sol-gel type, as described in WO 2008 / 059170. The porous layer can thus be obtained using a foaming agent, which is preferably a polymeric bead.
[0056] The anti-reflective coating, especially of porous silica, according to the invention may advantageously have a thickness of 10 nm to 10 μm (these limits being included), in particular 50 nm to 1 μm or even more preferably 70 to 500 nm.
[0057] The porous silica layer may have closed pores of at least 20 nm, 50 nm or 80 nm, and the functional layer may optionally have pores that increase in density towards the free surface.
[0058] The pores may be elongated in shape, in particular rice grain shaped, and even more preferably the pores may be approximately spherical or ovoid in shape.
[0059] It is preferred that the majority of the closed pores, even at least 80% of them, have approximately the same predetermined shape, in particular elongated, approximately spherical or ovoid.
[0060] The porous silica can be doped to improve its hydrolysis behavior even further, for example in the case of applications where good resistance is required (front, exterior, etc.). The dopant elements can preferably be selected from among Al, Zr, B, Sn, Zn. The dopants are introduced to replace Si atoms in a molar percentage that can preferably reach 10%, even more preferably up to 5%.
[0061] The anti-reflective coating may have a chemically protective underlayer, in particular a dense silica layer, in particular from sol-gel, for example up to 200 nm thick, on which the sol-gel porous silica functional layer rests.
[0062] The underlayer may be based on silica or on an at least partially oxidized derivative of silicon selected from among silicon dioxide, substoichiometric silicon oxide, silicon oxycarbide, silicon oxynitride, or silicon oxycarbonitride.
[0063] The underlayer has been found to be beneficial when the underlying surface is made of soda-lime-silica glass, since the underlayer acts as a barrier to alkali.
[0064] The underlayer thus preferably comprises Si, O, possibly carbon and nitrogen. However, the underlayer may also comprise a minor material compared to silicon, for example a metal such as Al, Zn or Zr. The underlayer can be applied by sol-gel or by pyrolysis, in particular by vapor phase pyrolysis (CVD).
[0065] This technique just described is quite straightforward, particularly in the case of glass substrates, by direct deposition onto float glass ribbons. x C yThis allows to obtain a layer or a SiO2 layer. However, it is also possible to carry out deposition by vacuum techniques, for example by cathodic sputtering from a (possibly doped) Si target or from a silicon suboxide target (for example in an oxidizing and / or nitriding reactive atmosphere). This underlayer preferably has a thickness of at least 5 nm, in particular from 10 nm to 200 nm, for example from 80 nm to 120 nm.
[0066] The antireflective coating can also have an overlying layer, provided that it does not impair the antireflective properties.
[0067] An anti-reflective coating can also be placed on the F1 surface in front of the anti-reflective coating on the F2 surface.
[0068] The anti-reflective coating may have the same shape as the cross-section of the holes, for example trapezoidal or also rectangular.
[0069] A priori less preferred, the anti-reflection coating can be only in a central zone in front of said through hole, without protruding beyond the through hole and preferably spaced at most 1 cm from the edge of the through hole, for example the free surface within the through hole has a length and / or side of at least 5 cm, 10 cm, 15 cm or preferably at most 30 cm.
[0070] The glazing may have an opaque masking layer, in particular enamel (e.g. black) on the F2 and / or Fa surfaces (e.g. black ink, in particular on Fa) between the F2 and Fa surfaces, in particular along the edges of the through holes between the F2 and Fa surfaces, preferably in the peripheral zone along the longitudinal edge of the glazing but also in the central zone, and an anti-reflective coating (in particular a porous silica layer or an optional dense silica underlayer) is in contact with the opaque masking layer.
[0071] The masking layer may, for example, be on the F2 plane and the anti-reflective coating may be above the masking layer or below the masking layer and / or the masking layer may be on the Fa plane and the anti-reflective coating may be in contact with the masking layer.
[0072] The masking layer has a gap along the through hole (at least in the central zone) and preferably extends into the through hole by up to 30 mm or 20 mm or 10 mm or 5 mm, and / or leaves an anti-reflective coating with a free surface at the hole, the free surface (not coated with masking layer) having a length of at least 5 cm, 10 cm, 15 cm or preferably up to 30 cm.
[0073] This masking layer will obscure the infrared viewing system and, for example, its case.
[0074] The masking layer can be a layer printed onto a laminate interlayer, for example onto the PVB.
[0075] The anti-reflective coating (particularly the porous silica layer or any dense silica underlayer) can also be spaced apart from the masking layer (eg on the F2 surface, particularly enamel), or at least does not cover it.
[0076] The opaque masking layer is preferably a continuous layer (all solid color, with a solid edge or, in a variant, with a graduated edge (a collection of patterns)).
[0077] The masking layer may be 2mm or 3mm (less than 5mm) from the (nearest) edge of the glazing.
[0078] The masking layer may be a screen, especially made of black enamel, framing the glazing (windscreen, etc.) Gaps are therefore created in this masking layer.
[0079] Another masking layer (such as enamel, especially black) may be present on the F3 or F4 face, especially facing the masking layer (and of the same nature, for example enamel, especially black).
[0080] The glazing may have metal wires, especially for heating, on the Fb side, especially fixed on the Fb side and preferably not in said holes.
[0081] It may be desirable to avoid heating lines in front of the holes.
[0082] The heating wire has in particular a thickness of less than or equal to 0.1 mm and is preferably made of copper, tungsten, gold, silver or aluminium or an alloy of at least two of these metals.
[0083] In one embodiment, the heating zone of the glazing comprises a number of individual metal wires, called "heating wires", which are connected between each other by "bus" bars. A heating current passes through these individual metal wires. The wires are advantageously very thin so as not to impair or only to a very small extent the transparency of the glazing. The metal wires preferably have a thickness of less than or equal to 0.1 mm, in particular between 0.02 and 0.04 mm, and ideally between 0.024 mm and 0.029 mm. The metal wires preferably comprise copper, tungsten, gold, silver or aluminium or an alloy of at least two of these metals. The alloy may also comprise molybdenum, rhenium, osmium, iridium, palladium or platinum.
[0084] The metal wires are preferably electrically insulated.
[0085] As regards the glass of the first glass sheet and / or the second glass sheet, it is preferably a soda-lime-silica type glass.
[0086] The inner and / or outer glass may have undergone a chemical or thermal treatment of the hardening, annealing or tempering type (especially for better mechanical strength) or may be semi-tempered.
[0087] The glass of the first glass sheet and / or the second glass sheet may preferably be of the float type, i.e. obtained by a process consisting in flowing molten glass over a bath of molten tin ("float" bath). By "atmosphere" side and "tin" side are meant the side that was in contact with the atmosphere prevailing in the float bath and the side that was in contact with the molten tin, respectively. The tin side contains a small amount of tin at the surface after diffusion into the structure of the glass.
[0088] The F2 surface with its anti-reflective coating can be either a "tin" surface or an "atmosphere" surface.
[0089] The first glass sheet may be, for example, a soda-lime-silica glass such as Diamant® from Saint-Gobain Glass, or Optiwhite® from Pilkington, or B270® from Schott, or Sunmax® glass from AGC, or glasses of other compositions described in WO 04 / 025334. Planiclear® from Saint-Gobain Glass may also be chosen.
[0090] Using common natural raw materials, the total iron oxide content is approximately 0.1% (1000 ppm) by weight. To reduce the iron oxide content, particularly pure raw materials can be selected.
[0091] In the present invention, in order to increase the near-infrared transmittance of the glass, the Fe2O3 (total iron) content of the first glass sheet is preferably less than 0.015%, furthermore 0.012% or less, particularly 0.010%. In order not to impose too much disadvantage on the cost of the glass, the Fe2O3 content is preferably 0.005% or more, particularly 0.008%.
[0092] To further increase the transmittance of the first glass sheet in the infrared, the ferrous content can be reduced in favor of the ferric content, i.e. the iron present in the glass can be oxidized. Thus, one aims for a glass with a "redox" that is as low as possible, ideally zero or close to zero. This number can vary between 0 and 0.9, with a redox of zero corresponding to a fully oxidized glass.
[0093] Glasses containing small amounts of iron oxide, especially less than 200 ppm or even less than 150 ppm, have a natural tendency to have high redox values, greater than 0.4 or even greater than 0.5, possibly due to adjustment of the iron redox equilibrium with the iron oxide content.
[0094] The redox of the first glass sheet is preferably 0.15 or more, and more preferably 0.2 to 0.30, and more preferably 0.25 to 0.30, since a redox that is too low will cause a reduction in the life of the furnace.
[0095] In the glasses according to the invention (first and second sheets), the silica SiO2 is generally kept within a narrow range for the following reasons: above 75%, the viscosity of the glass and its susceptibility to devitrification increase greatly, which makes its melting and its pouring onto a molten tin bath more difficult; below 60%, especially below 64%, the hydrolytic resistance of the glass rapidly deteriorates. The preferred content is 65-75%, especially 71-73%.
[0096] The first glass sheet may have a chemical composition including the following components in contents that vary within the weight limits defined as follows: SiO260~75% Al2O30-10% B2O3 0-5%, preferably 0% CaO 5~15% MgO 0~10% Na2O 5~20% K2O 0~10% BaO 0-5%, preferably 0% SO30.1~0.4% Fe2O3 (total iron) 0~0.015% and redox 0.1-0.3.
[0097] Throughout this specification percentages are by weight.
[0098] The glass sheet is preferably formed by floating in a tin bath. Other types of forming methods can be used, such as the pull-up method, the "down-draw" method (pull-up from below), the roll-out method, the Furcol method, etc.
[0099] The glass composition of the first glass sheet may contain, in addition to inevitable impurities contained in particular in the raw materials, small proportions (up to 1%) of other components, such as substances that serve the melting or fining of the glass (such as Cl) or also constituents resulting from the melting of refractories that serve the construction of the furnace (such as ZrO2). For the reasons already mentioned, the composition according to the invention preferably does not contain oxides such as Sb2O3, As2O3 or CeO2.
[0100] The composition of the first glass sheet preferably does not contain any infrared absorbing agents (especially for wavelengths between 800 and 1800 nm). In particular, the composition according to the invention preferably does not contain any of the following substances: oxides of transition elements such as CoO, CuO, Cr2O3, NiO, MnO2, V2O5, oxides of rare earths such as CeO2, La2O3, Nd2O3, Er2O3, or also colorants in the elemental state such as Se, Ag, Cu. Among other substances that are preferably excluded, oxides of the following elements are also present: Sc, Y, Pr, Sm, Eu, Gd, Tb, Dy, Ho, Tm, Yb, Lu. These substances very often have a very strong and undesirable coloring effect, which appears at very low contents, sometimes on the order of a few ppm or even less (1 ppm = 0.0001%). Their presence thus very significantly reduces the transmittance of the glass.
[0101] Preferably, the first glass sheet has a chemical composition comprising the following components in contents that vary within the weight limits defined as follows: SiO260~75% Al2O30-10% B2O3 0-5%, preferably 0% CaO 5~15% MgO 0~10% Na2O 5~20% K2O 0~10% BaO 0-5%, preferably 0% SO30.2>~0.4% Fe2O3 (total iron) 0~0.015% and redox 0.2-0.30.
[0102] The first glass sheet may have a chemical composition including the following components in contents that vary within the weight limits defined as follows: SiO260~75% Al2O30-10% B2O3 0-5%, preferably 0% CaO 5~15% MgO 0~10% Na2O 5~20% K2O 0~10% BaO 0-5%, preferably 0% SO30.1~0.4% Fe2O3 (total iron) 0~0.02% and redox 0.15-0.3.
[0103] In the present invention, the Fe2O3 (total iron) content is preferably less than 0.015%, further 0.012% or less, and especially 0.010%, in order to increase the near infrared transmittance of the glass. In order not to impose too much disadvantage on the cost of the glass, the Fe2O3 content is preferably 0.005% or more, and especially 0.008%.
[0104] The redox is preferably 0.15 or more, and more preferably 0.2 to 0.30, and even more preferably 0.25 to 0.30, because too low a redox can cause a shortened furnace life.
[0105] In the glasses according to the invention, the silica SiO2 is generally kept within a narrow range for the following reasons: above 75%, the viscosity of the glass and its susceptibility to devitrification increase greatly, which makes its melting and its pouring onto a molten tin bath more difficult; below 60%, especially below 64%, the hydrolytic resistance of the glass rapidly deteriorates. The preferred content is 65-75%, especially 71-73%.
[0106] Another preferred composition according to the invention is reproduced below: SiO265~75% Al2O30-3% CaO 7~12% MgO 2~5% Na2O 10~15% K2O 0~5% SO30.1~0.3% Fe2O3 (total iron) 0~0.015% or less and redox 0.1-0.3.
[0107] Another preferred composition according to the invention is reproduced below: SiO265~75% Al2O30-5% CaO 7~12% MgO 1~5% Na2O 10~15% K2O 0~5% SO30.2~0.4% Fe2O3 (total iron) 0~0.015% or less and redox 0.1-0.3.
[0108] Without departing from the scope of the invention, the interlayer may of course comprise an assembly of several thermoplastic sheets with different properties, in particular PVB sheets with different hardness, for example to ensure the function of sound insulation, as described, for example, in US 6,132,882. Likewise, one of the glass sheets may be thinned compared to the thicknesses conventionally used.
[0109] The intermediate layer may, according to the invention, be wedge-shaped, in particular for HUD (Head Up Display) applications. Likewise, one of the sheets of the intermediate layer may be entirely colored.
[0110] Besides PVB, other commonly used laminate interlayers include polyurethanes (PU) for flexible applications, thermoplastic resins without plasticizers such as ethylene vinyl acetate (EVA) copolymers, and ionomer resins. These plastics have a thickness of, for example, 0.2 mm to 1.1 mm, in particular 0.3 to 0.7 mm.
[0111] The laminate interlayer may include another functional plastic film (transparent, clear or colored), for example a poly(ethylene terephthalate) PET film carrying a conductive athermal layer, for example PVB / functional film / PVB between the F2 and F3 faces.
[0112] The transparent plastic film may be 10 to 100 μm thick. More broadly, the transparent plastic film may be polyamide, polyester, polyolefin (PE: polyethylene, PP: polypropylene), polystyrene, polyvinyl chloride (PVC), polyethylene terephthalate (PET), polymethyl methacrylate (PMMA), polycarbonate (PC). Clear films, especially PET, are preferred.
[0113] Coated PET clear films, for example XIR from Eastman, composite extruded films made of PET-PMMA, for example SRF 3M® type, can be used, but also many other films (for example made of PC, PE, PEN, PMMA, PVC) which are as visually transparent as possible and do not change in the autoclave with regard to surface and viscosity.
[0114] In order to limit the temperature rise in the vehicle interior or to limit the use of air conditioning, at least one of the glass sheets (preferably the outer glass) is tinted and the laminated glazing may also have a layer which reflects or absorbs solar radiation, preferably on the F4 side or on the F2 or F3 side, in particular a transparent conductive oxide layer called a TCO layer (on the F4 side) or even a stack of thin layers comprising at least one TCO layer, or a stack of thin layers comprising at least one silver layer (on F2 or F3), the or each silver layer being arranged between dielectric layers.
[0115] It is possible to combine (silver-containing) layers on the F2 and / or F3 sides with a TCO layer on the F4 side.
[0116] The TCO (Transparent Conductive Oxide) layer is preferably a fluorine doped tin oxide (SnO2:F) layer or an indium tin oxide (ITO) layer.
[0117] Again, the most demanding application is where the glazing is the windshield of a road vehicle (automobile) or even a (low speed) rail vehicle.
[0118] The glazing may therefore have an athermal functional layer on the F2 surface, in particular an electrically conductive, possibly heating, in particular a silver stack, which is absent in said through-holes at least in the central zone and is located along the edges of the through-holes between the F2 surface and the Fa surface, and an anti-reflective coating may optionally be in contact with the functional layer, in particular above or below the athermal functional layer.
[0119] The present invention also relates to an apparatus comprising: - Glazing as previously described - an infrared viewing system, multispectral at said operating wavelengths and particularly in the visible range of 500-600 nm, positioned within the vehicle interior behind said glazing to receive and / or transmit radiation after passing through the first glass sheet at said through hole.
[0120] Advantageous, but non-limiting, particular embodiments of the invention are described below which can of course be combined with one another if desired. [Brief description of the drawings]
[0121] [Figure 1] 1 shows a cross-sectional view of a windshield 100 in a first embodiment of the present invention using an infrared viewing system such as a LIDAR. [Diagram 2] The windshield 100 in FIG. 1 is shown in a front view (vehicle compartment side). [Diagram 3] 2 shows a cross-sectional view of a windshield 200 according to the present invention, in cross section using an infrared viewing system such as a LIDAR in a second embodiment of the present invention. [Figure 4] The windshield 200 in FIG. 3 is shown in a front view (vehicle compartment side). DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0122] 1 shows a windshield 100 according to the present invention in cross-section with an infrared viewing system such as LIDAR at 905 nm or 1550 nm, which can also be a multispectral system capable of operating in the visible range up to 1800 nm.
[0123] This viewing system 7 is placed behind the windshield, facing a zone preferably located in the upper and central part of the windshield. In this zone, the infrared viewing system 7 is oriented at a certain angle with respect to the windshield surface (F2 plane). In particular, the LIDAR can be oriented directly towards the image collection zone along a direction close to parallel to the ground, i.e. along a direction slightly inclined towards the road. In other words, the LIDAR 7 can be oriented towards the road along a slight angle with a field of view adapted to perform its function.
[0124] The windshield is a conventional laminated glazing including: an outer glass sheet 1 having an outer surface F1 and an inner surface F2; and an inner glass sheet 1' having an outer surface F3 and an inner surface F4 facing the passenger compartment, for example having a thickness of 1.6 mm or even less. The two glass sheets are joined to each other by an interlayer 3 made of a thermoplastic material, preferably clear, of sub-millimeter thickness, typically made of polyvinyl butyral (PVB), possibly with a wedge-shaped decreasing cross section from top to bottom of the laminated glazing, for example a PVB (Solutia or Eastman RC41) of approximately 0.76 mm thickness or, if necessary as a variant, a sound-insulating PVB (3- or 4-ply), for example an interlayer made of three PVB sheets, for example of approximately 0.81 mm thickness.
[0125] In the well-known conventional manner, the windshield is obtained by thermal lamination of components 1, 2 and 3. A 0.76 mm clear PVB is selected.
[0126] The first glass sheet has on its face F2 an anti-reflective coating 2 at at least one wavelength referred to as operating wavelength in the infrared between 800 nm and 1800 nm, in particular between 850 nm and 1600 nm, and has a free surface (the surface not covered by the laminate interlayer and the second glass sheet) with a hole 4 penetrating through the thickness of the interlayer and through the thickness of the second glass sheet, i.e. a hole defined by walls 40 and 40'.
[0127] The first glass sheet 1 is in particular based on silica, soda lime, soda lime silica (preferred), aluminosilicates, borosilicates and has a total iron oxide (expressed in the form of Fe2O3) content by weight of max. 0.05% (500 ppm), preferably max. 0.03% (300 ppm) or max. 0.015% (150 ppm) and in particular 0.005% or more. The first glass sheet can have a redox of 0.15 or more, in particular 0.2 to 0.30, in particular 0.25 to 0.30.
[0128] In particular, 1.95 mm OPTWHITE glass is selected.
[0129] The second glass sheet 1' is in particular based on silica, soda lime, preferably soda lime silica (like the first glass sheet), but also on aluminosilicates or borosilicates, and has a total iron oxide weight content of at least 0.4% and preferably at most 1.5%. The second glass sheet can have a redox of 0.22 to 0.35 or 0.30.
[0130] Mention may be made, inter alia, of the Applicant's glasses designated TSAnx (0.5-0.6% iron), TSA2+, TSA3+ (0.8-0.9% iron), TSA4+ (1% iron), TSA5+, which are green in colour.
[0131] For example, 1.6 mm TSA3+ glass is selected.
[0132] Using 1.95mm OPTWHITE glass with a 110nm anti-reflection coating, we obtain the following total transmission at facet F2: At -90°, 92.5% at 905nm and 92.0% at 1550nm At -60°, 91.7% at 905nm and 91.5% at 1550nm.
[0133] According to the invention, in the peripheral central region along the upper longitudinal edge, the windshield therefore has a hole 4 passing through the thickness of the laminate interlayer 3 and through the thickness of the second glass sheet 1', i.e. a hole defined by their respective side walls 40' and 40.
[0134] As shown in Figures 1 and 2, the holes here are in particular - of trapezoidal cross section - closed holes (holes surrounded by the wall of the glass sheet), i.e. holes in the glazing, which have: - the so-called upper first large side, i.e. the upper longitudinal edge, closest to the upper longitudinal edge edge 10 of the glazing, which is parallel to this edge and has a length of at most 20 cm, e.g. 10.6 cm, and is spaced at least 5 cm or 6 cm from the edge (of this large side); - the so-called lower second major side, i.e. the lower longitudinal edge (farthest from the upper longitudinal edge 10 and closer to the central zone), which is parallel to the first major side and has a length of at most 25 cm or 20 cm and preferably longer than the length of the first major side, for example 17.5 cm; - a height (between these major sides) of at least 5 cm, here 10 cm.
[0135] An infrared viewing system 7 faces the through hole 4 .
[0136] The through hole 4 can alternatively be a notch, ie a through hole which preferably opens onto the roof side.
[0137] The through hole 4 can also be in another area of the windscreen 100 or even in another glazing of the vehicle, in particular the rear window.
[0138] The anti-reflection coating 2 is also local: here it is rectangular in shape in this peripheral area and its edge 20 extends a maximum of 10 mm beyond the wall defining the hole 4, between the face 12 and the face Fa.
[0139] The windshield 100 has on its F2 face 12 an opaque masking layer 5, for example black, such as an enamel layer or lacquer, which forms the peripheral frame of the windshield (or rear window), and the windshield has, with the through-holes in the peripheral zone, gaps 51' large enough not to interfere with the performance of the LIDAR 7, but suitable to conceal the case 8 (plastic, metal, etc.) of the LIDAR 7. The case 8 can be glued to the F4 face and to the roof 9 by means of an adhesive 6.
[0140] Here, the anti-reflection coating is on the F2 surface and also slightly covers the masking layer.
[0141] The windshield 100 may have a set of nearly invisible metal lines, e.g. 50 μm, in the form of straight lines or not, located (across the entire surface) on the Fb side of the F3 side of the laminate interlayer 3. These lines are not in the through holes 4.
[0142] FIG. 3 illustrates a cross-sectional view of a windshield 200 using an infrared viewing system such as a LIDAR in accordance with a second embodiment of the present invention.
[0143] FIG. 4 shows the windshield 200 of FIG. 3 in a front view (facing the vehicle compartment).
[0144] Only the differences from the first embodiment are described below.
[0145] The anti-reflection coating 2 on the F2 surface is now underneath a masking layer.
[0146] The anti-reflective coating 2 has a shape similar to that of the cross-section of the hole, i.e. here a trapezoid in this peripheral region (not visible and therefore shown by dotted lines in FIG. 4), and its edge 20 protrudes 10 mm beyond the wall defining the hole 4, between the faces 12 and Fa.
[0147] In the through hole is fitted an insert 90, which is attached (in particular by gluing or by force) to the wall 40 of the second glass sheet which defines the hole (at the top) and which is also in contact with the wall 40' of the laminate interlayer and borders the anti-reflective coating, for example of the ring type, maximum 1.5 cm wide, made of a flexible polymeric material (such as polycarbonate).
[0148] This insert 90 can be used for mechanical reinforcement and / or for fixation of the LIDAR. It can also be used in the first embodiment.
[0149] The insert can extend beyond the hole, particularly onto the F4 face.
[0150] In relation to the embodiment shown, possible variations (not exhaustive) are as follows, which can possibly be combined: - The anti-reflective coating does not extend beyond the through-hole and is preferably spaced a maximum of 1 cm from the edge of the through-hole The anti-reflective coating is spaced apart from the masking layer (eg on face F2, in particular enamel) or at least does not cover it. The anti-reflective coating comprises a chemically protective underlayer, which is in particular a dense silica layer, in particular a sol-gel based, on top of which is a sol-gel porous silica functional layer. The F2 surface has an athermal functional layer below or above the enamel, and an anti-reflective coating is optionally in contact with the functional layer, in particular above or below the athermal functional layer. [Explanation of symbols]
[0151] 1. First Glass Sheet 1' Second glass sheet 2. Anti-reflective coating 3. Middle Tier 4 Through holes 5 Masking Layers 7 Infrared Viewing System 8 Cases 9 Roof 10 Upper longitudinal edge edge 51' Gap 90 Insert 100 Windshield 200 Windshield
Claims
1. 1. A vehicle glazing of a predetermined thickness, comprising: a first glass sheet (1) intended to be an outer glazing, having an outer first main face F1 (11) and an inner second main face F2 (12) oriented towards the vehicle interior; - a laminate intermediate layer (3) made of a polymeric material, having a main surface Fa oriented toward F2 and a main surface Fb opposite to Fa; a second glass sheet (1') intended to be an inner glazing, with a third main face F3 (13) on the F2 side and an inner fourth main face F4 (14) directed towards the passenger compartment; having A first glass sheet has, on its F2 side, an anti-reflective coating (2) at at least one wavelength, referred to as the operating wavelength in the infrared, in the range extending from 800 nm to 1800 nm, with a free surface (20) due to a through hole (4) in the thickness of the laminate interlayer and in the thickness of the second glass sheet, the first glass sheet having a total iron oxide weight content of maximum 0.05%; 13. A vehicle glazing, wherein the second glass sheet has a total iron oxide content by weight of at least 0.4%.
2. 2. Vehicle glazing according to claim 1, characterized in that the assembly of the first glass sheet (1) and the anti-reflective coating (2) exhibits a total transmittance at the operating wavelength, measured at 90°, of at least 90.0%.
3. 3. Vehicle glazing according to claim 1 or 2, characterized in that the through holes (4) are in the peripheral area and that the anti-reflective coating is locally in said peripheral area.
4. 3. Vehicle glazing according to claim 1 or 2, characterized in that the through hole (4) has a cross-section the smaller dimension of which is at least 5 cm and the larger dimension of which is at most 30 cm.
5. 3. Vehicle glazing according to claim 1 or 2, characterized in that the through-holes (4) are closed and spaced at least 2 cm from the nearest glazing edge.
6. Vehicle glazing as described in claim 1 or 2, characterized in that an insert (90) is attached to the through hole in a wall (40) of the second glass sheet which defines at least a portion of the through hole.
7. 3. Vehicle glazing according to claim 1 or 2, characterized in that the anti-reflective coating (2) locally extends beyond the through-hole (4) between the faces F2 and Fa.
8. 3. Vehicle glazing according to claim 1 or 2, characterized in that the anti-reflective coating comprises a porous silica layer.
9. 3. Vehicle glazing according to claim 1 or 2, characterized in that the anti-reflective coating comprises a chemically protective underlayer surmounted by a porous silica functional layer.
10. 3. Vehicle glazing according to claim 1 or 2, characterized in that it has an opaque masking layer (5) on the F2 face and / or on the Fa face (31), which is a masking layer between the F2 face and the Fa face, which is present along the edge of the through hole between the F2 face and the Fa face, the anti-reflective coating being in contact with the opaque masking layer, which has a gap (51') along the through hole leaving a free surface of the anti-reflective coating (2).
11. 11. Vehicle glazing according to claim 10, characterized in that the masking layer (5) is on the F2 side and the anti-reflective coating (2) is on top of or underneath the masking layer and / or the masking layer is on the Fa side and the anti-reflective coating is in contact with the masking layer.
12. 3. Vehicle glazing according to claim 1 or 2, characterized in that it has an opaque masking layer (5) on the F2 face and / or on the Fa face (31), the masking layer being present between the F2 face and the Fa face along the edge of the through hole between the F2 face and the Fa face, and the anti-reflective coating is spaced from the masking layer or at least does not cover it.
13. 3. The vehicle glazing according to claim 1 or 2, further comprising a metal wire on the Fb surface side.
14. 3. Vehicle glazing according to claim 1 or 2, characterized in that it comprises an athermal functional layer on the F2 side which is absent in the through-holes at least in the central zone and which is present along the edges of the through-holes between the F2 side and the Fa side.
15. 3. Vehicle glazing according to claim 1 or 2, characterized in that the laminate interlayer comprises PVB (3).
16. Vehicle glazing as described in claim 1 or 2, characterized in that the assembly of the first glass sheet (1) and the anti-reflective coating (2) exhibits a total transmittance of at least 90.0% at operating wavelengths of 905±5 nm and / or 1550±5 nm, measured at 90°.
17. Vehicle glazing as described in claim 4, characterized in that the cross section is trapezoidal or rectangular, or disc-shaped or oval.
18. Vehicle glazing as claimed in claim 9, characterized in that the chemically protective undercoat layer is a high density silica layer.
19. Vehicle glazing according to claim 18, characterized in that the high density silica layer is obtained by a sol-gel process.
20. Vehicle glazing as described in claim 13, characterized in that it has a heating metal wire on the Fb surface side.
21. The vehicle glazing of claim 14, wherein the functional layer is a stack comprising silver.
22. Vehicle glazing as described in claim 15, characterized in that the laminate interlayer has PVB / functional film / PVB.
23. Vehicle glazing as described in claim 22, characterized in that the functional film is a polymeric film having an athermal coating.
24. The vehicle glazing according to any one of claims 1 to 23. an infrared viewing system (7) at said operating wavelength, arranged in the vehicle interior behind said glazing to receive and / or transmit radiation after passing through the first glass sheet at said through hole; An apparatus comprising:
Citation Information
Patent Citations
Glass pane with detector for electromagnetic radiation
JP2011502090A
Bracket-equipped laminated plate
WO2017188412A1
Camera lens
WO2018153012A1
Glass for autonomous car
WO2018178278A1
Glass for autonomous car
WO2018178286A1