Apparatus for producing non-aqueous electrolyte and method for producing non-aqueous electrolyte
The use of a styrene-based weakly basic anion exchange resin with specific ion exchange capacity addresses the challenge of purifying non-aqueous electrolytes by adsorbing acidic impurities, ensuring effective purification and preventing group conversion, thus maintaining battery performance.
Patent Information
- Application Number
- JP2018199868
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2018-10-24
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2038-10-24
AI Technical Summary
Existing methods for removing acidic impurities like hydrofluoric acid from non-aqueous electrolytes used in lithium-ion batteries are ineffective due to the modification of tertiary amino groups to quaternary ammonium groups, leading to reduced battery capacity and corrosion.
A non-aqueous electrolyte manufacturing apparatus and method using a styrene-based weakly basic anion exchange resin with a tertiary amino group and a total ion exchange capacity of 0.1 to 3.0 eq/L-R, which effectively adsorbs and purifies acidic impurities while minimizing the conversion to quaternary ammonium groups.
The apparatus and method enable easy purification of non-aqueous electrolytes by effectively suppressing the modification of tertiary amino groups to quaternary ammonium groups, thereby maintaining battery performance and preventing corrosion.
Smart Images

Figure 0007573355000004 
Figure 0007573355000005 
Figure 0007573355000001
Abstract
Description
[Technical field]
[0001] The present invention relates to an apparatus for producing a non-aqueous electrolyte solution and a method for producing a non-aqueous electrolyte solution. [Background technology]
[0002] In lithium ion batteries, a non-aqueous electrolyte solution in which a lithium-based electrolyte such as lithium hexafluorophosphate (LiPF6) is dissolved in an organic non-aqueous solvent is used as the electrolyte solution.
[0003] However, trace amounts of water remain in the solvent and lithium-based electrolyte constituting the electrolytic solution. This water reacts with the lithium-based electrolyte such as LiPF6 to produce hydrogen fluoride (HF) and the like, for example, as shown in the following reaction formulas (1) to (3). (1) LiPF6+H2O → LiF+2HF+POF3 (2) POF3+H2O → POF2(OH)+HF (3)POF2(OH)+H2O → POF(OH)2+HF
[0004] If acidic impurities such as hydrogen fluoride (hydrofluoric acid) are present in the electrolyte, they can reduce the battery capacity and charge / discharge cycle characteristics of the lithium-ion battery, and can make the inside of the battery more susceptible to corrosion (see Patent Document 1 (JP 2011-71111 A), etc.). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2011-71111 A Summary of the Invention [Problem to be solved by the invention]
[0006] For this reason, a method for removing acidic impurities such as hydrofluoric acid from the electrolyte has been desired. One possible method for removing such acidic impurities is to bring the electrolyte for a lithium ion battery into contact with a weakly basic anion exchange resin that contains an anion exchange group having a tertiary amine structure (a tertiary amino group).
[0007] However, the present inventors have found through their investigations that when the weakly basic anion exchange resin is brought into contact with an electrolyte for a lithium ion battery, a quaternization reaction occurs in which the tertiary amino group is modified into a quaternary ammonium group by the carbonate solvent in the electrolyte. When the anion exchange group is modified by the above-mentioned quaternization reaction, the adsorptivity is improved and the group becomes more likely to adsorb not only acidic impurities in the electrolyte but also other components, making it difficult to selectively remove the acidic impurities.
[0008] Under such circumstances, an object of the present invention is to provide an apparatus for producing a nonaqueous electrolyte solution that can easily perform purification treatment while effectively suppressing the degeneration of tertiary amino groups, which are weakly basic anion exchange groups, into quaternary ammonium groups, when acidic impurities, such as hydrofluoric acid, contained in a nonaqueous electrolyte solution, such as an electrolyte solution for a lithium ion battery, are adsorbed and purified by a weakly basic anion exchange resin having an amino group, and to provide a method for producing a nonaqueous electrolyte solution.
[0009] As a result of intensive research into achieving the above-mentioned object, the present inventors have found that the above technical problems can be solved by a production apparatus for a non-aqueous electrolyte, the production apparatus having an ion exchange section containing a weakly basic anion exchange resin for obtaining a non-aqueous electrolyte by passing an alkali metal salt electrolyte-containing liquid in which an alkali metal salt electrolyte is dispersed in a carbonate ester, the weakly basic anion exchange resin having a styrene-based resin base and a tertiary amino group as a weakly basic anion exchange group, and having a total ion exchange capacity of 0.1 to 3.0 eq / LR before treatment with the alkali metal salt electrolyte-containing liquid, and have completed the present invention based on this finding.
[0010] That is, the present invention provides (1) In carbonate ester Can decompose to produce acids an ion exchange unit containing a weakly basic anion exchange resin for passing an alkali metal salt electrolyte-containing liquid in which an alkali metal salt electrolyte is dissolved to obtain a non-aqueous electrolyte; The weakly basic anion exchange resin has a styrene-based resin as a base, a tertiary amino group as a weakly basic anion exchange group, and a total ion exchange capacity of 0.1 to 3.0 eq / LR before treatment with an alkali metal salt electrolyte-containing liquid. An apparatus for producing a non-aqueous electrolyte, (2) The apparatus for producing a non-aqueous electrolyte according to (1) above, wherein the styrene-based resin is a styrene-divinylbenzene copolymer. (3) The apparatus for producing a non-aqueous electrolyte according to (1) or (2), wherein the non-aqueous electrolyte is an electrolyte for a lithium ion battery. (4) A method for producing a nonaqueous electrolyte, comprising the steps of: In carbonate ester Can decompose to produce acids an acid adsorption step of passing an alkali metal salt electrolyte-containing liquid in which an alkali metal salt electrolyte is dissolved through an ion exchange section containing a weakly basic anion exchange resin to obtain nonaqueous electrolysis, The weakly basic anion exchange resin has a styrene-based resin as a base, a tertiary amino group as a weakly basic anion exchange group, and a total ion exchange capacity of 0.1 to 3.0 eq / LR before treatment with an alkali metal salt electrolyte-containing liquid. A method for producing a non-aqueous electrolyte solution, (5) The method for producing a non-aqueous electrolyte solution according to (4) above, wherein the styrene-based resin is a styrene-divinylbenzene copolymer. (6) The method for producing a nonaqueous electrolyte solution according to (4) or (5), wherein the nonaqueous electrolyte solution is an electrolyte solution for a lithium ion battery. This provides: Effect of the Invention
[0011] According to the present invention, it is possible to provide an apparatus for producing a nonaqueous electrolyte that can easily perform purification treatment while effectively suppressing the degeneration of tertiary amino groups, which are weakly basic anion exchange groups, into quaternary ammonium groups when acidic impurities such as hydrofluoric acid contained in the nonaqueous electrolyte are adsorbed and purified by a weakly basic anion exchange resin having amino groups, and it is also possible to provide a method for producing a nonaqueous electrolyte. [Brief description of the drawings]
[0012] [Figure 1] FIG. 2 is a diagram illustrating a configuration of an apparatus for producing a nonaqueous electrolyte according to the present invention. [Diagram 2] 1 is a diagram showing an example of an apparatus for producing a nonaqueous electrolyte according to the present invention; DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] The apparatus for producing a non-aqueous electrolyte according to the present invention includes an ion exchange unit containing a weakly basic anion exchange resin, and configured to pass an alkali metal salt electrolyte-containing liquid in which an alkali metal salt electrolyte is dispersed in a carbonate ester to obtain a non-aqueous electrolyte, The weakly basic anion exchange resin has a styrene-based resin as a base, a tertiary amino group as a weakly basic anion exchange group, and a total ion exchange capacity of 0.1 to 3.0 eq / LR before treatment with an alkali metal salt electrolyte-containing liquid. It is characterized by the above.
[0014] FIG. 1 shows an example of the configuration of a non-aqueous electrolyte manufacturing apparatus according to the present invention.
[0015] As shown in FIG. 1, a nonaqueous electrolyte manufacturing apparatus 1 according to the present invention has an ion exchange unit 2 containing a weakly basic anion exchange resin, for passing an alkali metal salt electrolyte-containing solution S in which an alkali metal salt electrolyte such as a lithium-based electrolyte is dispersed in a carbonate ester to obtain a nonaqueous electrolyte.
[0016] In the apparatus for producing a non-aqueous electrolyte according to the present invention, the carbonate ester may be at least one selected from cyclic carbonate esters and chain carbonate esters.
[0017] Examples of the cyclic carbonate ester include one or more selected from ethylene carbonate, propylene carbonate, and the like. Examples of the chain carbonate ester include one or more selected from dimethyl carbonate, diethyl carbonate, ethyl methyl carbonate, and the like.
[0018] In the nonaqueous electrolyte manufacturing apparatus according to the present invention, the alkali metal salt electrolyte may be a lithium-based electrolyte, and the lithium-based electrolyte may be one or more selected from LiPF, LiClO, LiBF, LiAsF, LiSbF, LiAlCl, LiCFSO, etc., with LiPF being preferred in terms of battery performance. In the non-aqueous electrolyte production apparatus according to the present invention, the non-aqueous electrolyte is preferably an electrolyte for lithium ion batteries.
[0019] In the nonaqueous electrolyte manufacturing apparatus according to the present invention, the concentration of the alkali metal salt in the alkali metal salt electrolyte-containing solution is preferably 0.5 to 2.0 mol / L, more preferably 0.5 to 1.2 mol / L, and even more preferably 0.8 to 1.2 mol / L.
[0020] The method for preparing the alkali metal salt electrolyte-containing liquid is not particularly limited. For example, the liquid can be prepared by adding and dissolving an alkali metal salt electrolyte in a carbonate ester under an inert gas atmosphere.
[0021] The apparatus for producing a non-aqueous electrolyte according to the present invention has an ion exchange section containing a weakly basic anion exchange resin, through which an alkali metal salt electrolyte-containing liquid (unrefined non-aqueous electrolyte) passes.
[0022] In the apparatus for producing a non-aqueous electrolyte according to the present invention, the weakly basic anion exchange resin used in the ion exchange section has a styrene-based resin as a base.
[0023] In the present application, the styrene-based resin means a resin in which styrene or a styrene derivative is homopolymerized or copolymerized, and which contains 50 mass % or more of structural units derived from styrene or a styrene derivative.
[0024] The styrene derivative may be one or more selected from α-methylstyrene, vinyltoluene, chlorostyrene, ethylstyrene, i-propylstyrene, dimethylstyrene, bromostyrene, and the like.
[0025] The styrene-based resin may be a copolymer with other copolymerizable vinyl monomers, so long as it is mainly composed of a homopolymer or copolymer of styrene or a styrene derivative. Examples of such vinyl monomers include one or more selected from polyfunctional monomers such as divinylbenzenes, such as o-divinylbenzene, m-divinylbenzene, and p-divinylbenzene, alkylene glycol di(meth)acrylates, such as ethylene glycol di(meth)acrylate and polyethylene glycol di(meth)acrylate, (meth)acrylonitrile, methyl (meth)acrylate, and the like.
[0026] The other copolymerizable vinyl monomers are preferably ethylene glycol di(meth)acrylate, polyethylene glycol di(meth)acrylate having an ethylene polymerization number of 4 to 16, and divinylbenzene, more preferably divinylbenzene and ethylene glycol di(meth)acrylate, and even more preferably divinylbenzene.
[0027] In the apparatus for producing a non-aqueous electrolyte according to the present invention, the weakly basic anion exchange resin used in the ion exchange section has a tertiary amino group as the weakly basic anion exchange group.
[0028] The tertiary amino group is represented by the following general formula (I): [ka] (However, R 1 Groups and R 2 The groups are hydrocarbon groups having 1 to 3 carbon atoms and may be the same or different, and * indicates a bonding site with the substrate or a bonding group for bonding to the substrate.) Examples of the above-mentioned formulas are given below.
[0029] In the weakly basic anion exchange group represented by the above general formula (I), R 1 Groups and R 2 The group is a hydrocarbon group having 1 to 3 carbon atoms. R 1 Group or R 2 The group may be one or more selected from an alkyl group and an alkenyl group, and is preferably an alkyl group. R 1 Group or R 2 Specific examples of the group include one or more groups selected from a methyl group, an ethyl group, a propyl group, and a propylene group, with a methyl group being preferred. In the weakly basic anion exchange group represented by the above general formula (I), R 1 Groups and R 2 The groups may be the same or different.
[0030] Examples of the weakly basic anion exchange group represented by the above general formula (I) include a dimethylamino group, a diethylamino group, and a dipropylamino group, with the dimethylamino group being preferred.
[0031] In the above general formula (I), * indicates the binding site between the weakly basic anion exchange group represented by the above general formula (I) and the substrate or a binding group for binding to the substrate.
[0032] The weakly basic anion exchange group represented by the above general formula (I) is appropriately bonded to a substrate made of a styrene-based resin by bonding with a bonding group R 3It is preferable that the bond is via a group. [ka] (However, R 1 Groups and R 2 R 3 The group is a hydrocarbon group having 1 to 3 carbon atoms, and * indicates the bonding site with the substrate.
[0033] Above R 1 Groups and R 2 Examples of the group include the same as those mentioned above. Above R 3 The group is a hydrocarbon group having 1 to 3 carbon atoms, and R 3 The group may be at least one selected from an alkylene group and an alkenylene group, and is preferably an alkylene group. R 3 Specific examples of the group include one or more selected from a methylene group (-CH2-), an ethylene group (-CH2CH2CH2-), a propylene group (-CH2CH2CH2-), etc., with a methylene group being preferred.
[0034] The weakly basic anion exchange group represented by the above general formula (I) can be introduced into a styrene-based resin by introducing it as a substituent into styrene or a styrene derivative.
[0035] In the nonaqueous electrolyte manufacturing apparatus according to the present invention, the weakly basic anion exchange resin used in the ion exchange section has a total ion exchange capacity of 0.1 to 3.0 eq / LR before treatment with the alkali metal salt electrolyte-containing liquid.
[0036] In the nonaqueous electrolyte manufacturing apparatus according to the present invention, the weakly basic anion exchange resin used in the ion exchange section has a total ion exchange capacity before treatment with the alkali metal salt electrolyte-containing liquid of 0.1 to 3.0 eq / LR, preferably 0.5 to 2.5 eq / LR, and more preferably 1.0 to 2.0 eq / LR.
[0037] In the present application, the total ion exchange capacity means a value calculated by the method described below. In a weakly basic anion exchange resin in which amino groups serve as the weakly basic anion exchange groups, the total ion exchange capacity refers to the combined ion exchange capacity of primary amino groups, secondary amino groups, tertiary amino groups and quaternary ammonium groups.
[0038] The nonaqueous electrolyte manufacturing apparatus according to the present invention employs as a weakly basic anion exchange resin a styrene-based resin base, which has a tertiary amino group as a weakly basic anion exchange group, and which has a total ion exchange capacity within the above range before treatment with an alkali metal salt electrolyte-containing liquid. This makes it possible to easily perform purification treatment while effectively suppressing the modification of the tertiary amino group, which is a weakly basic anion exchange group, to a quaternary ammonium group when adsorbing and purifying acidic impurities such as hydrofluoric acid contained in an alkali metal salt electrolyte-containing liquid with the weakly basic anion exchange resin having an amino group.
[0039] In this application, the total ion exchange capacity is defined as the sum of the amino group exchange capacity and the neutral salt decomposition capacity when the anion exchange resin is completely converted to a chloride ion form with hydrochloric acid in a wet state and before treatment with an alkali metal salt electrolyte-containing liquid, the excess hydrochloric acid is washed away with ethanol, and the amount of chloride ions that flow out when ammonia water is passed through is defined as the amino group exchange capacity, and the amount of chloride ions that flow out when a sodium nitrate solution is then passed through is defined as the neutral salt decomposition capacity.
[0040] The weakly basic anion exchange resin contained in the ion exchange section may have any of a gel type structure, a macroporous (MR) type structure, and a porous type structure, and is preferably one having a macroporous type structure.
[0041] The size of the weakly basic anion exchange resin is not particularly limited, but the harmonic mean diameter is preferably The thickness is preferably 300 to 1000 μm, more preferably 400 to 800 μm, and further preferably 500 to 700 μm.
[0042] Such a weakly basic anion exchange resin may be a commercially available product, and examples thereof include one or more types selected from Diaion WA30 manufactured by Mitsubishi Chemical Corporation and ORLITE DS-6 manufactured by Organo Corporation.
[0043] In the non-aqueous electrolyte manufacturing apparatus according to the present invention, the form of the weakly basic anion exchange resin contained in the ion exchange unit is not particularly limited as long as it allows contact between the alkali metal salt electrolyte-containing liquid and the weakly basic anion exchange resin. For example, the ion exchange unit may be a column or tank packed with a weakly basic anion exchange resin through which the alkali metal salt electrolyte-containing liquid can pass. The ion exchange unit may also be provided with a pump for passing the alkali metal salt electrolyte-containing liquid.
[0044] In the nonaqueous electrolyte manufacturing apparatus according to the present invention, the liquid passing speed (liquid hourly space velocity) at which the alkali metal salt electrolyte-containing liquid is passed through the weakly basic anion exchange device in the ion exchange unit may be appropriately selected from the speeds at which acidic impurities in the alkali metal salt electrolyte-containing liquid can be removed.
[0045] In the treatment with the weakly basic anion exchange resin, for example, first, the weakly basic anion exchange resin is washed in advance with the carbonate ester solvent constituting the alkali metal salt electrolyte-containing liquid to be treated, and then dried under reduced pressure at about 40 to 80°C. Next, the weakly basic anion exchange resin is swelled again with the carbonate ester solvent constituting the alkali metal salt electrolyte-containing liquid to be treated, and then packed into a column. After that, the electrolyte to be treated is preferably subjected to backwashing and extrusion operations according to the usual method, and then subjected to SV (flow rate / ion exchange resin volume ratio) of 1 to 100 hr. -1 , more preferably SV2 to 50hr -1 , and more preferably SV5 to 20 hr -1This can be done by passing the solution through the column.
[0046] In the non-aqueous electrolyte manufacturing apparatus according to the present invention, the content of acidic impurities such as hydrofluoric acid in the acid adsorption treatment solution obtained from the ion exchange unit is preferably 20 ppm by mass or less, more preferably 10 ppm by mass or less, and even more preferably 5 ppm by mass or less. In the present application, the amount of acidic impurities refers to a value measured by neutralization titration.
[0047] According to the present invention, by adopting a weakly basic anion exchange resin contained in an ion exchange section that has a styrene-based resin as a base, has tertiary amino groups as weakly basic anion exchange groups, and has a total ion exchange capacity calculated by the above formula within the above range, it is possible to provide an apparatus for producing a nonaqueous electrolyte that can easily perform a purification process while effectively suppressing the degeneration of the tertiary amino groups, which are weakly basic anion exchange groups, into quaternary ammonium groups, when adsorbing acidic impurities such as hydrofluoric acid contained in the nonaqueous electrolyte with the weakly basic anion exchange resin having amino groups for purification.
[0048] Next, a method for producing the nonaqueous electrolyte according to the present invention will be described. The method for producing a non-aqueous electrolyte according to the present invention includes an acid adsorption step of passing an alkali metal salt electrolyte-containing liquid, in which an alkali metal salt electrolyte is dispersed in a carbonate ester, through an ion exchange unit containing a weakly basic anion exchange resin to obtain a non-aqueous electrolyte, the weakly basic anion exchange resin having a styrene-based resin base, a tertiary amino group as a weakly basic anion exchange group, and a total ion exchange capacity of 0.1 to 3.0 eq / LR before treatment with the alkali metal salt electrolyte-containing liquid.
[0049] The method for producing a non-aqueous electrolyte solution according to the present invention is essentially a method for producing a non-aqueous electrolyte solution using the production apparatus according to the present invention, and therefore the details of the production method are the same as those described above in relation to the use of the production apparatus according to the present invention.
[0050] According to the present invention, by adopting a weakly basic anion exchange resin contained in an ion exchange section that has a styrene-based resin as a base, has a tertiary amino group as a weakly basic anion exchange group, and has a total ion exchange capacity within the above range before treatment with an alkali metal salt electrolyte-containing liquid, it is possible to provide a method for producing a non-aqueous electrolyte that can be easily purified while effectively suppressing the modification of the tertiary amino group, which is a weakly basic anion exchange group, to a quaternary ammonium group when acidic impurities such as hydrofluoric acid contained in the non-aqueous electrolyte are adsorbed by the weakly basic anion exchange resin having a tertiary amino group for purification treatment. EXAMPLES
[0051] The present invention will now be described in more detail with reference to examples, but these are merely illustrative and do not limit the present invention.
[0052] Example 1 An electrolyte solution was prepared using an apparatus for producing an electrolyte solution for lithium ion batteries as the nonaqueous electrolyte solution producing apparatus 1 shown in FIG. That is, first, as shown in FIG. 2, a column packed with a weakly basic anion exchange resin having a styrene-divinylbenzene base and a dimethylamino group as a weakly basic anion exchange group was prepared as an ion exchange section 2 constituting an apparatus for producing a nonaqueous electrolyte (apparatus for producing an electrolyte for a lithium ion battery) 1. Next, an electrolyte S, which was prepared by dissolving LiPF6 at 1 mol / L in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, was pumped into the column at 10 h -1 The electrolyte was passed through the tank at a flow rate of 1500 g for 15 days, and the electrolyte after passing through the tank was stored in the tank T. The total ion exchange capacity of the weakly basic anion exchange resin was measured before and after the above-mentioned liquid passing through it by the following method. The results are shown in Table 1.
[0053] <Method for measuring total ion exchange capacity> After the anion exchange resin is completely converted to the chloride ion form with hydrochloric acid, excess hydrochloric acid is washed away with ethanol, and the amount of chloride ions that flow out when ammonia water is passed through is taken as the amino group exchange capacity, and the amount of chloride ions that flow out when sodium nitrate solution is then passed through is taken as the neutral salt decomposition capacity. The sum of the amino group exchange capacity and the neutral salt decomposition capacity is taken as the total ion exchange capacity.
[0054] The total ion exchange capacity indicates the amount of all ion exchange groups (the total amount of primary amino groups to tertiary amino groups and quaternary ammonium groups), and the neutral salt decomposition capacity indicates the amount of quaternary ammonium groups. In Table 1, the neutral salt decomposition capacity and amino group exchange capacity before and after the electrolyte treatment are also shown. Table 1 also shows the proportion of quaternary ammonium groups in the total amount of functional groups calculated according to the following formula. Proportion of quaternary ammonium groups in the total amount of functional groups (%) = (neutral salt decomposition capacity (eq / LR) / total ion exchange capacity (eq / LR)) x 100
[0055] (Examples 2 to 4) The lithium ion battery electrolyte manufacturing apparatus 1 was constructed in the same manner as in Example 1, except that the weakly basic anion exchange resin packed in the column constituting the ion exchange unit 2 was a weakly basic anion exchange resin based on styrene-divinylbenzene and having a dimethylamino group as a weakly basic anion exchange group, and had a total ion exchange capacity shown in Table 1. Next, in the same manner as in Example 1, an electrolyte S, which was prepared by dissolving LiPF6 at 1 mol / L in a mixed solvent of ethylene carbonate and dimethyl carbonate in a volume ratio of 1:1, was pumped into the column at 10 h -1 The electrolyte was passed through the tank at a flow rate of 1500 g for 15 days, and the electrolyte after passing through the tank was stored in the tank T. The total ion exchange capacity of the weakly basic anion exchange resin before and after the above-mentioned liquid passing was measured in the same manner as in Example 1. The results are shown in Table 1. In Table 1, the neutral salt decomposition capacity, amino group exchange capacity, and the proportion of quaternary ammonium groups in the total amount of functional groups before and after the electrolyte treatment are also shown, as in Example 1.
[0056] Comparative Example 1 The weakly basic anion exchange resin was based on an acrylic resin and had a dimethylamino group as the weakly basic anion exchange group. In the same manner as in Example 1, except that the weakly basic anion exchange resin was based on an acrylic resin and had a dimethylamino group as the weakly basic anion exchange group, the electrolyte S was passed through a column packed with the weakly basic anion exchange resin, and the total ion exchange capacity and neutral salt decomposition capacity of the weakly basic anion exchange resin were measured before and after passing the electrolyte S through the column. The results are shown in Table 1.
[0057] [Table 1]
[0058] From Table 1, it can be seen that in Examples 1 to 4, the treatment for removing acidic impurities from a lithium-based electrolyte-containing solution in which a lithium-based electrolyte is dispersed in a carbonate ester is carried out by using a resin having a styrene-based resin as a base, a tertiary amino group as a weakly basic anion exchange group, and an amino group exchange capacity calculated by the above formula within the above range. When acidic impurities such as hydrofluoric acid contained in the electrolyte for a lithium ion battery are adsorbed and purified by a weakly basic anion exchange resin having a tertiary amino group, the denaturation of the tertiary amino group, which is a weakly basic anion exchange group, to a quaternary ammonium group can be effectively suppressed, and the purification treatment can be easily carried out.
[0059] On the other hand, from Table 1, it can be seen that in Comparative Example 1, the treatment for removing acidic impurities from the lithium-based electrolyte-containing liquid in which the lithium-based electrolyte is dispersed in the carbonate ester is not performed using the specific weakly basic anion exchange resin, and therefore it is difficult to suppress the modification of tertiary amino groups to quaternary ammonium groups (quaternization reaction). [Industrial Applicability]
[0060] According to the present invention, it is possible to provide an apparatus for producing a nonaqueous electrolyte that can easily perform purification treatment while effectively suppressing the degeneration of tertiary amino groups, which are weakly basic anion exchange groups, into quaternary ammonium groups when acidic impurities such as hydrofluoric acid contained in the nonaqueous electrolyte are adsorbed and purified by a weakly basic anion exchange resin having amino groups, and it is also possible to provide a method for producing a nonaqueous electrolyte. [Explanation of symbols]
[0061] 1. Nonaqueous electrolyte manufacturing equipment 2. Acid Absorber
Claims
1. an ion exchange section containing a weakly basic anion exchange resin for passing an alkali metal salt electrolyte-containing liquid in which an alkali metal salt electrolyte capable of decomposing into a carbonate ester to generate an acid is dissolved, to obtain a nonaqueous electrolyte; The weakly basic anion exchange resin has a styrene-based resin as a base, a tertiary amino group as a weakly basic anion exchange group, and a total ion exchange capacity before treatment with an alkali metal salt electrolyte-containing liquid of 0.1 to 3.0 eq / L-R. The apparatus for producing a non-aqueous electrolyte solution is characterized in that
2. 2. The apparatus for producing a non-aqueous electrolyte according to claim 1, wherein the styrene-based resin is a styrene-divinylbenzene copolymer.
3. 3. The apparatus for producing a non-aqueous electrolyte according to claim 1, wherein the non-aqueous electrolyte is an electrolyte for a lithium ion battery.
4. A method for producing a non-aqueous electrolyte solution, comprising the steps of: an acid adsorption step of passing an alkali metal salt electrolyte-containing solution, in which an alkali metal salt electrolyte capable of being decomposed into a carbonate ester to generate an acid, through an ion exchange unit containing a weakly basic anion exchange resin to obtain a non-aqueous electrolyte; The weakly basic anion exchange resin has a styrene-based resin as a base, a tertiary amino group as a weakly basic anion exchange group, and a total ion exchange capacity before treatment with an alkali metal salt electrolyte-containing liquid of 0.1 to 3.0 eq / L-R. The present invention relates to a method for producing a non-aqueous electrolyte solution.
5. 5. The method for producing a non-aqueous electrolyte according to claim 4, wherein the styrene-based resin is a styrene-divinylbenzene copolymer.
6. 6. The method for producing a non-aqueous electrolyte solution according to claim 4, wherein the non-aqueous electrolyte solution is an electrolyte solution for a lithium ion battery.
Citation Information
Patent Citations
Manufacture of pure boric acid
JP1988035413A
Method for removing acid from lithium salt solution
JP2000505042A
Zeolite for processing nonaqueous electrolyte and method for processing nonaqueous electrolyte
JP2011071111A
Recovery of iodide from chemical process wastewater
US6379556B1