Nickel nanoparticle aggregate, its manufacturing method, and nickel nanoparticle composite substrate

By forming nickel nanoparticle aggregates through controlled exposure to water or hydrogen peroxide, the method achieves strong bonding at low temperatures, overcoming the limitations of high-temperature requirements in existing technologies and expanding substrate compatibility.

JP7573378B2Active Publication Date: 2024-10-25NIPPON STEEL CHEM & MATERIAL CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020093890
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-29
Publication Date
2024-10-25
Estimated Expiration
2040-05-29

AI Technical Summary

Technical Problem

Existing methods for bonding nickel nanoparticles require high temperatures, making them unsuitable for applications on plastic substrates and compromising the inherent properties of metals due to the presence of organic matter, which affects bonding strength and performance.

Method used

The formation of nickel nanoparticle aggregates by minimizing contact with water and solvents containing hydroxyl groups, using a small amount of water or hydrogen peroxide to generate nickel hydroxide, allowing strong aggregation at low temperatures.

Benefits of technology

Enables bonding at 150°C or lower, facilitating the use of nickel nanoparticle aggregates on both high and low heat-resistant substrates, including resin substrates, enhancing their applicability in electronic components and composite substrates.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573378000004
    Figure 0007573378000004
  • Figure 0007573378000005
    Figure 0007573378000005
  • Figure 0007573378000006
    Figure 0007573378000006
Patent Text Reader

Abstract

To provide a nickel nanoparticle aggregate that strongly aggregates at a low temperature of 150°C or lower.SOLUTION: A nickel nanoparticle paste having nickel nanoparticles with an average particle size of 5-100 nm and a binder resin dispersed in a nonpolar solvent is brought into contact with water or 1 wt.% or more hydrogen peroxide solution, thereby causing a coat to form on the nickel nanoparticles and causing the nickel nanoparticles to be aggregated directly or through the coat, resulting in a nickel nanoparticle aggregate.SELECTED DRAWING: Figure 2
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a nickel nanoparticle aggregate that enables low-temperature bonding by generating nickel hydroxide on the surface of nickel nanoparticles, a method for producing the same, and a nickel nanoparticle composite substrate. [Background technology]

[0002] Metal nanoparticles have physical and chemical properties that differ from those of bulk metals, and are therefore used in a variety of applications, such as bonding materials for semiconductor devices, electromagnetic shielding materials, optical materials, and brazing materials.

[0003] Nickel nanoparticles are known to be obtained by solid-phase or liquid-phase reactions. Known solid-phase reactions include chemical vapor deposition of nickel chloride and thermal decomposition of nickel formate. Liquid-phase reactions include a method of directly reducing a metal salt with a strong reducing agent such as sodium borohydride (e.g., Patent Document 1), a method of adding a reducing agent such as hydrazine in the presence of a strong alkali to form a precursor and then thermally decomposing the precursor (e.g., Patent Document 2), and a method of synthesizing a metal complex containing a metal salt or an organic ligand by thermal decomposition in a pressure vessel together with a solvent (e.g., Patent Document 3).

[0004] In general, when nickel nanoparticles are used, bonding is performed at a temperature of 300°C or higher using hydrogen gas (inert gas base) with an explosion limit concentration of 5% or less. Even when ultrafine particles of 10 to 50 nm are used, bonding is difficult unless the temperature is 200°C or higher (for example, Patent Document 4), and the material cannot be used in applications requiring plastic substrates, such as electromagnetic shielding materials, optical materials, and bonding materials.

[0005] As a low-temperature bonding method, a method has been proposed in which complexes of metals with different ionization tendencies are used to bond the materials at temperatures between 25°C and 200°C. However, this method is not preferred because it contains a large amount of organic matter, which not only makes it difficult to obtain sufficient bonding strength, but also reduces the inherent performance of the metal (e.g., Patent Document 5). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-193118 A [Patent Document 2] JP 2008-95146 A [Patent Document 3] JP 2010-105149 A [Patent Document 4] Patent No. 6061427 [Patent Document 5] JP 2010-29871 A Summary of the Invention [Problem to be solved by the invention]

[0007] It is an object of the present invention to provide nickel nanoparticle aggregates that are tightly aggregated at low temperatures, for example below 150°C. [Means for solving the problem]

[0008] As a result of intensive research, the inventors have found that nickel nanoparticles produced by minimizing contact with water or a solvent containing a hydroxyl group tend to form strong aggregates in the presence of a very small amount of water or a chemical substance having a hydroxyl group, such as alcohol. This behavior is presumed to occur when a hydroxyl group such as water or alcohol is present, after which nickel hydroxide is generated, and the water generated is further coordinated to the adjacent nickel by condensation with the adjacent nickel hydroxide, thereby generating nickel oxide and nickel hydroxide. It is presumed that strong aggregates are formed by repeating this reaction. By utilizing this phenomenon, it has been found that strong aggregates can be formed in a short time by impregnating nickel nanoparticles produced by the above-mentioned method with a small amount of water or hydrogen peroxide and drying them, and the present invention has been completed.

[0009] In other words, the nickel nanoparticle aggregate of the present invention is obtained by contacting a nickel nanoparticle paste in which nickel nanoparticles having an average particle size of 5 to 100 nm and a binder resin are dispersed in a non-polar solvent with water or 1 wt% or more of hydrogen peroxide solution, thereby forming a coating on the surface of the nickel nanoparticles and agglomerating the nickel nanoparticles together directly or via the coating.

[0010] The nickel nanoparticle aggregate of the present invention may be obtained by drying the nickel nanoparticle paste and then contacting it with the water or 1 wt % or more of hydrogen peroxide solution.

[0011] In the nickel nanoparticle aggregate of the present invention, the nickel nanoparticles may be nickel nanoparticles having a calculated value V of 3 or more as calculated by the following formula (1): V = A × D 3 / S / 10000000 ···(1) {In the formula, A means the amount of nickel dimethylglyoxime detected [ppm] as determined by the nickel measurement method specified in JIS K 0102 59.1, and S means the specific surface area [m 2 / g], and D means the average particle size [nm] of nickel particles measured by scanning electron microscope (SEM).}

[0012] In the nickel nanoparticle aggregate of the present invention, the nickel nanoparticles may be made of nickel alone or an alloy of nickel with one or more metals selected from lithium, copper, iron, cobalt, gold, platinum and palladium.

[0013] In the nickel nanoparticle aggregate of the present invention, 99 wt % or more of the metal component contained in the nickel nanoparticles may be nickel.

[0014] The nickel nanoparticle composite substrate of the present invention comprises a substrate and the above-mentioned nickel nanoparticle aggregate laminated on the substrate.

[0015] The method for producing nickel nanoparticle aggregates of the present invention includes the steps of preparing a nickel nanoparticle paste in which nickel nanoparticles having an average particle size of 5 to 100 nm and a binder resin are dispersed in a non-polar solvent; A step of contacting the nickel nanoparticle paste with water or 1 wt % or more hydrogen peroxide solution to form a coating on the surface of the nickel nanoparticles and aggregate the nickel nanoparticles directly or via the coating; Includes. Effect of the Invention

[0016] The nickel nanoparticles used in the present invention are manufactured so that nickel cations are easily generated on the surface of the nickel nanoparticles in a solution containing a small amount of water or hydroxyl groups, and thus easily react with water or hydroxyl groups to form strong aggregates by drying at low temperatures, for example, below 150° C. Therefore, the nickel nanoparticle aggregates of the present invention have a lower aggregation temperature compared to conventional techniques, and therefore can be formed not only on inorganic substrates with high heat resistance, such as metal substrates, glass substrates, and ceramic substrates, but also on resin substrates with lower heat resistance than inorganic substrates. Therefore, the nickel nanoparticle aggregate of the present invention is useful as a bonding material for bonding various members. In addition, by using the nickel nanoparticle aggregate of the present invention, a composite substrate of nickel nanoparticles and a substrate can be obtained at a low temperature, and therefore the nickel nanoparticle aggregate can be widely used as a material for various electronic components. [Brief description of the drawings]

[0017] [Figure 1] 1 is a scanning electron microscope (SEM) image (50,000x) of the dried paste prepared in Example 1. [Diagram 2] 1 is an SEM image (50,000x) of the aggregates prepared in Example 1. [Diagram 3] 1 is an SEM image (50,000x) of the dried paste prepared in Example 2. [Figure 4] 1 is an SEM image (50,000x) of the aggregates prepared in Example 2. [Diagram 5]1 is a SEM image (100,000x) of the dried paste prepared in Example 3. [Figure 6] 1 is an SEM image (110,000x) of the aggregates prepared in Example 3. [Figure 7] 1 is an SEM image (50,000x) of the aggregates prepared in Example 4. [Figure 8] 1 is an SEM image (50,000x) of the aggregates prepared in Example 5. [Figure 9] 1 is an SEM image (50,000 times) of the dried paste prepared in Comparative Example 1. [Figure 10] 1 is an SEM image (magnification: 50,000 times) of the paste prepared in Comparative Example 1 after treatment with hydrogen peroxide water. [Figure 11] 1 is an SEM image (50,000 times) of the dried paste prepared in Comparative Example 2. [Figure 12] 1 is an SEM image (magnification: 50,000 times) of the paste prepared in Comparative Example 2 after treatment with hydrogen peroxide water. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0018] An embodiment of the present invention will be described below. The nickel nanoparticle aggregate of the present invention is obtained by contacting a nickel nanoparticle paste in which nickel nanoparticles having an average particle size of 5 to 100 nm and a binder resin are dispersed in a non-polar solvent with water or 1 wt % or more of hydrogen peroxide solution, thereby forming a coating on the surfaces of the nickel nanoparticles and aggregating the nickel nanoparticles together directly or via the coating.

[0019] Here, the nickel nanoparticles may be particles produced by known methods, such as particles synthesized by a gas phase method or particles synthesized by a liquid phase method, as long as they have the above-mentioned average particle diameter. However, particles synthesized by a liquid phase method are preferred because nickel cations are easily generated by the liquid phase method.

[0020] Moreover, the nickel nanoparticles are preferably those having a calculated value V of 3 or more as calculated by the following formula (1). V = A × D3 / S / 10000000 ···(1) {In the formula, A means the amount of nickel dimethylglyoxime detected [ppm] as determined by the nickel measurement method specified in JIS K 0102 59.1, and S means the specific surface area [m 2 / g], and D means the average particle size [nm] of nickel particles measured by scanning electron microscope (SEM).} This range has the advantage that nickel cations that form the coating are generated in sufficient amounts, making it easier to form aggregates.

[0021] In addition, the nickel nanoparticle aggregate of the present invention requires that nickel hydroxide is generated on the surface of the nickel nanoparticles in order to form the aggregate. Therefore, the material of the nickel nanoparticles is preferably nickel alone or an alloy of nickel and one or more metals selected from lithium, copper, iron, cobalt, gold, platinum and palladium, which can generate nickel hydroxide on the particle surface. For the reasons mentioned above, it is preferable that the nickel concentration in the nickel nanoparticles is high, and specifically, it is preferable that 99 wt % or more of the metal components contained in the nickel nanoparticles is nickel.

[0022] A preferred method for producing nickel nanoparticles will be exemplified below. The nickel nanoparticles used in the present embodiment are prepared by the following steps A and B: A) a step of mixing a nickel salt and a reducing agent to obtain a complex reaction solution; B) heating the complexation reaction solution to reduce the nickel component in the complexation reaction solution and obtain a slurry of nickel nanoparticles; Preferably, the method further comprises the following step C: C) washing the nickel nanoparticle slurry with a washing solvent; In order to control the particle size of the nickel nanoparticles to be synthesized, a predetermined amount of an organometallic compound may be added at any timing between step A and heating the complexing reaction solution in step B.

[0023] [Process A] Step A is a step of mixing a nickel salt and a reducing agent to obtain a nickel complexation reaction solution.

[0024] <Nickel salt> The nickel salt may be a known nickel salt. Here, the nickel salt may be, for example, an organic acid nickel salt such as a nickel carboxylate, or an inorganic metal salt such as a nickel chloride, a nickel sulfate, a nickel nitrate, or a nickel carbonate, and may be selected from one or more of these metal salts. Among these, nickel carboxylates having 1 to 12 carbon atoms excluding the COOH group are preferred, and nickel acetate and nickel formate are preferred, because they are easy to control the particle size and particle size distribution.

[0025] <Reducing agent> The reducing agent used in the present embodiment is not particularly limited as long as it can form a complex with a metal, but for example, a primary amine is preferably used. A primary amine is preferable because it can form a complex with a metal and can effectively exert a reducing ability on a nickel complex. On the other hand, a secondary amine has a large steric hindrance, which may hinder the good formation of a nickel complex, and a tertiary amine does not have a reducing ability of a metal, so neither can be used alone, but when using a primary amine, these can be used in combination within a range that does not interfere with the shape of the nickel nanoparticles to be generated.

[0026] The reducing agent may be a solid or liquid at room temperature. Here, room temperature refers to 20°C ± 15°C. A primary amine that is liquid at room temperature also functions as an organic solvent when forming a metal complex. There is no problem with a primary amine that is solid at room temperature, as long as it becomes liquid when heated to 100°C or higher or can be dissolved using an organic solvent.

[0027] The primary amine may be an aromatic primary amine, but an aliphatic primary amine is preferred from the viewpoint of ease of nickel complex formation in the reaction solution. The aliphatic primary amine can control the dispersibility of the nickel nanoparticles produced by, for example, adjusting the length of its carbon chain, and is advantageous in applications requiring dispersibility. From the viewpoint of controlling the aggregation of nickel nanoparticles in a slurry state, it is preferred to select and use an aliphatic primary amine having a carbon number of about 6 to 20. Examples of such amines include octylamine, trioctylamine, dioctylamine, hexadecylamine, dodecylamine, tetradecylamine, stearylamine, oleylamine, myristylamine, and laurylamine. Oleylamine and dodecylamine are particularly preferred because they exist in a liquid state under the temperature conditions in the nickel nanoparticle production process, and therefore the reaction can proceed efficiently in a uniform solution. Oleylamine is more preferred.

[0028] Since the primary amine functions as a surface modifier during the production of nickel nanoparticles, secondary aggregation in a slurry state can be suppressed even after the removal of the primary amine. In addition, the primary amine is preferably liquid at room temperature from the viewpoint of ease of processing operations in a washing step for separating the solid components of the produced nickel nanoparticles from the solvent or unreacted primary amine after the reduction reaction in step B. The amount of the primary amine is preferably used at a ratio of valence of the metal x 1 mol or more, more preferably valence x 1.1 mol or more, and even more preferably valence x 2 mol or more, relative to 1 mol of the metal. If the amount of the primary amine is less than valence of the metal x 1 mol, it becomes difficult to control the particle size of the obtained nickel nanoparticles, and the particle size tends to vary. In addition, there is no particular upper limit to the amount of the primary amine, but from the viewpoint of productivity, for example, it is preferable to use valence of the metal x 10 mol or less.

[0029] The conditions for forming the complexing reaction solution in step A, that is, the conditions for mixing the nickel salt and the reducing agent, will be described using an example in which nickel carboxylate is used as the nickel salt and a primary amine is used as the reducing agent. In this case, the complexing reaction can proceed at room temperature, but in order to perform the complexing reaction sufficiently and more efficiently, it is preferable to heat the reaction to a temperature within the range of, for example, 100°C to 165°C. The heating temperature is preferably a temperature exceeding 100°C, more preferably a temperature of 105°C or higher, so that the ligand substitution reaction between the coordinated water coordinated to the nickel carboxylate and the primary amine is efficiently performed, the water molecule as the complex ligand can be dissociated, and the water can be removed from the system, so that the complex with the amine can be efficiently formed. In addition, when nickel formate dihydrate is used as nickel carboxylate, it has a complex structure in which two coordinated water molecules and two formic acids as bidentate ligands are present at room temperature, so in order to efficiently form a complex by ligand substitution of these two coordinated water molecules with a primary amine, it is preferable to heat at a temperature higher than 100°C to dissociate the water molecules as complex ligands. The heating time can be appropriately determined depending on the heating temperature and the content of each raw material. There is no particular upper limit to the heating time, but unnecessarily long heat treatment is wasteful from the viewpoint of saving energy consumption and process time.

[0030] The heating method in step A is not particularly limited, and may be, for example, heating with a heat medium such as oil temperature control or an electric heater, or heating by microwave irradiation or ultrasonic irradiation.

[0031] In step A, an organic solvent other than the primary amine may be added to allow the reaction in the homogeneous solution to proceed more efficiently. When using an organic solvent, the organic solvent may be mixed simultaneously with the nickel salt and the reducing agent, but it is more preferable to mix the nickel salt and the reducing agent first to form a complex and then add the organic solvent, since the reducing agent is efficiently coordinated to the nickel atom. The organic solvent that can be used is not particularly limited as long as it does not inhibit the complex formation between the nickel salt and the reducing agent and does not oxidize the generated nickel, and for example, a saturated or unsaturated hydrocarbon-based organic solvent having 7 to 30 carbon atoms can be used. In addition, from the viewpoint of being able to use it even under heated conditions, it is preferable to select an organic solvent having a boiling point of 170°C or higher. A specific example of such an organic solvent is paraffin oil.

[0032] [Process B] In step B, the nickel complex reaction solution obtained by the complex formation reaction is heated, and the nickel in the complex reaction solution is reduced to obtain a slurry of nickel nanoparticles. The heating temperature in step B varies depending on the particle size and particle size distribution of the nickel nanoparticles obtained, but it is preferable to maintain the temperature at which an endothermic reaction occurs. If the temperature is sufficiently high beyond the reaction temperature, the catalytic action of the generated nickel decomposes the hydrocarbons, and carbon precipitates and covers the surface of the nickel nanoparticles, suppressing the generation of nickel ions on the nickel surface and reducing the bonding property, which is not preferable.

[0033] The heating time is not particularly limited, but it is preferable to measure the nickel concentration of the reaction solution using, for example, a nickel concentration meter Ni-5Z manufactured by Kasahara Chemical Industry Co., Ltd., and heat until nickel is no longer detected. If the heating time is shorter than this, it is difficult to obtain particles with the desired particle size, and further, dispersibility is likely to decrease, which is not preferable. In addition, the upper limit of the heating time is not particularly limited because the heating time varies depending on the particle size, but long heating after the reaction is completed is not preferable because carbon is precipitated on the nickel surface, the generation of nickel ions is suppressed, and the coagulation property is decreased.

[0034] The production process in step B uses a batch method or a continuous reactor for heating a stainless steel vessel, and examples of the heating means include a heating method using a heat medium such as oil temperature control, electricity, microwaves, and ultrasonic waves. From the viewpoint of production cost, a heating method using a heat medium such as oil temperature control and electricity is preferably used. Heating by microwave irradiation or ultrasonic irradiation may also be used.

[0035] In step B, in order to improve the dispersibility of the nickel nanoparticles or to impart functions such as rust inhibitors to prevent oxidation, dispersants or additives for imparting functions can be added within a range that does not interfere with bonding.

[0036] [Addition of organometallic compounds] The organometallic compound used in this embodiment is not particularly limited as long as it has the same properties (nucleophilicity) as the nucleophilic reagent and acts on the metal complex. From the viewpoints of ease of control of the particle size and particle size distribution of the nickel nanoparticles, safety, simplicity, and productivity, preferred organometallic compounds include alkali metal-based organometallic compounds in which an organic group such as an alkyl group or an alkoxy group is coordinated to an alkali metal, and alkaline earth metal-based organometallic compounds in which the organic group is coordinated to an alkaline earth metal. Hereinafter, the alkali metal-based organic compounds and the alkaline earth metal-based organic compounds are collectively referred to as "the present organometallic compounds". The present organometallic compounds may be organometallic halides containing halides such as chlorine, bromine, and iodine. In this case, they are also referred to as alkali metal-based organometallic halides and alkaline earth metal-based organometallic halides, respectively. An alkali metal-based organometallic halide is one form of an alkali metal-based organometallic compound, and an alkaline earth metal-based organometallic halide is one form of an alkaline earth metal-based organometallic compound.

[0037] Examples of the alkali metal constituting the alkali metal-based organometallic compound include lithium, sodium, potassium, rubidium, and cesium, and organolithium compounds containing highly reactive lithium are preferably used. In addition, examples of the alkaline earth metal constituting the alkaline earth metal-based organometallic compound include beryllium, magnesium, calcium, strontium, and barium, and organomagnesium halides containing magnesium, which has good reactivity, are preferably used. Note that, since alkylaluminum, in which an alkyl group is coordinated to aluminum, is highly flammable, from the viewpoints of safety and simplicity, alkali metal-based and alkaline earth metal-based organometallic compounds are more preferably used.

[0038] The present organometallic compound is preferably used as a diluted solution diluted with an organic solvent such as tetrahydrofuran, hexane, toluene, cyclohexane, butyl ether, dibutyl ether, etc. There is no limitation on the concentration of the diluted solution, but in cases where a small amount affects the particle size, a low concentration is preferable because it is easier to control.

[0039] As the alkali metal-based organometallic compound, inexpensive and versatile n-butyllithium or phenyllithium is preferably used, and a toluene or n-hexane solution of these is particularly preferable from the viewpoints of safety and simplicity. As the alkaline earth metal-based organometallic compound, ethylmagnesium chloride, ethylmagnesium bromide, butylmagnesium chloride, 2-butylmagnesium chloride-lithium chloride complex, and butylmagnesium bromide are preferably used, and tetrahydrofuran solutions of these are particularly preferably used.

[0040] The amount of the organometallic compound to be added is not particularly limited, as it may be selected according to the desired particle size. Specifically, the amount of the organometallic compound to be added is as shown below.

[0041] The organometallic compound may be added at any timing between step A and heating the complexing reaction solution in step B. For example, the organometallic compound may be added after mixing the nickel salt and the reducing agent in step A to remove excess moisture, or after preparing the complexing reaction solution. In addition, since the organometallic compound is easily deactivated by moisture and loses its effect, it is preferable to add it just before heating the complexing reaction solution in step B. By adding the organometallic compound, the particle size of the nickel nanoparticles can be significantly reduced. Although the mechanism of action is not yet clear, it is presumed that the organometallic compound having nucleophilicity acts on the nickel complex to promote the generation of nickel nuclei. Since the effect is deactivated by the influence of moisture absorption, making it difficult to control the particle size distribution, it is preferable to add the organometallic compound just before heating the complexing reaction solution in step B.

[0042] [Nickel nanoparticles] In this manner, a synthetic liquid slurry containing nickel nanoparticles can be obtained. The obtained nickel nanoparticle synthetic liquid slurry is preferably washed and replaced with a washing solvent to prevent the activity of nickel ions on the surface of the nickel nanoparticles from decreasing after, for example, standing and separating the slurry and removing the supernatant (step C). The washing solvent used in step C preferably does not contain a hydroxyl group. Therefore, it is preferable to use a solvent that does not contain 0.1 wt% or more of water as the washing solvent, and organic solvents such as toluene, xylene, hexane, and cyclohexane that satisfy this condition can be preferably used. Note that hydrophilic alcohols with a carbon number of 3 or less usually contain 0.1 wt% or more of water, and are therefore not preferable as washing solvents. The nickel nanoparticles may contain small amounts of elements other than metal elements, such as oxygen, hydrogen, carbon, and nitrogen, or may be alloys of these elements. Furthermore, the nickel nanoparticles may be composed of a single nickel nanoparticle, or may be a mixture of two or more types of nickel nanoparticles.

[0043] Furthermore, the metal components contained in the nickel nanoparticles may include alkali metals such as lithium, sodium, potassium, rubidium, and cesium; base metals such as copper, iron, and cobalt; and precious metals such as platinum, gold, palladium, and silver.

[0044] In the present method for producing nickel nanoparticles, there is no particular limit to the average particle size of the resulting nickel nanoparticles, but the average particle size can be controlled to a desired size within the range of, for example, 5 nm to 100 nm by adding the present organometallic compound.

[0045] [Nickel nanoparticle ink or paste composition] In order to make the slurry containing the obtained nickel nanoparticles into an ink or paste as described above, it is preferable to use a solvent that does not contain water or a hydrophilic alcohol having 3 or less carbon atoms, and for example, aliphatic hydrocarbons such as decane, tetradecane, paraffin oil, and petroleum-based hydrocarbons, alicyclic hydrocarbons such as cyclohexane, methylcyclohexane, ethylcyclohexane, and decahydronaphthalene, aromatic hydrocarbons such as toluene, xylene, and ethylbenzene, esters such as ethyl acetate, butyl acetate, dihydroterpinyl acetate, isobornyl acetate, isobornyl proquinate, isobornyl butyrate, and isobornyl isobutyrate, long-chain esters such as α-terpineol and butyl carbitol, and non-aqueous solvents such as esters of long-chain alcohols and carboxylic acids are preferred. Among these, it is more preferable to use non-polar solvents such as aliphatic hydrocarbons and alicyclic hydrocarbons.

[0046] There are no particular limitations on the dispersant used to make the ink or paste in this embodiment, but since a non-aqueous solvent is preferably used, a non-aqueous polymer dispersant is preferred, and a commercially available dispersant may also be used.

[0047] The weight-average molecular weight of the non-aqueous polymer dispersant used in the present embodiment is preferably within the range of 1,000 to 200,000, more preferably within the range of 5,000 to 100,000. If the weight-average molecular weight is less than the lower limit, the dispersion stability in a low-polarity solvent may be insufficient, and if it exceeds the upper limit, the viscosity may become too high, making handling difficult.

[0048] Suitable examples of commercially available non-aqueous polymer dispersants that can be used include Solsperse 3000 (trade name), Solsperse 8000 (trade name), Solsperse 9000 (trade name), Solsperse 11200 (trade name), Solsperse 13940 (trade name), and Solsperse 13240 (trade name), all manufactured by Lubrizol Japan; and DISPERBYK-161 (trade name), DISPERBYK-163 (trade name), DISPERBYK-2164 (trade name), and DISPERBYK-2155 (trade name), all manufactured by BYK-Chemie Japan.

[0049] The amount of the non-aqueous polymer dispersant used in this embodiment varies depending on the particle size, but is preferably within the range of 0.01 to 10 parts by mass, and more preferably within the range of 0.1 to 5 parts by mass, relative to 100 parts by mass of nickel nanoparticles. If the amount added is less than the lower limit, dispersibility in the paste tends to decrease, and if it exceeds the upper limit, aggregation tends to occur easily in the paste.

[0050] There is no particular limitation on the binder resin used in the present embodiment, and any resin may be used as long as it can adjust the viscosity characteristics and form a good coating film. The type and amount of binder resin to be added vary depending on the solvent used, so they may be appropriately adjusted.

[0051] [Agglutination method] The nickel nanoparticle aggregate of the present invention is obtained by contacting the nickel nanoparticle paste obtained as described above with water or 1 wt % or more hydrogen peroxide solution (hereinafter referred to as the "aggregation liquid") to bond the nickel nanoparticles together directly or via their coatings. The flocculation liquid must be a solution that easily reacts with nickel ions on the surface of the nickel nanoparticles to generate hydroxyl groups. For example, water or 1 wt% or more of hydrogen peroxide solution can be used as the flocculation liquid. By spraying the flocculation liquid onto a film formed by applying the nickel nanoparticle ink or paste onto a substrate using a sprayer or the like and contacting the nickel nanoparticles, a coating of nickel hydroxide or nickel oxide is formed on the surface of the nickel nanoparticles, and the nickel nanoparticles are aggregated directly or through the coating to form nickel nanoparticle aggregates. When hydrogen peroxide solution is used as the flocculation liquid, the concentration may be 1 wt% or more, and is preferably within the range of 30 wt% to 35 wt%. In addition, it is preferable to dry the nickel nanoparticle paste before contacting it with the flocculation liquid to reduce the content of the non-polar solvent in the nickel nanoparticle paste. The nickel nanoparticle paste can be dried at room temperature, but it is preferable to heat treat it at a temperature of, for example, 150°C or less, preferably within the range of 70°C to 150°C. In addition, although nickel nanoparticles can be aggregated at room temperature, the time required for aggregation can be shortened by contacting the nickel nanoparticles with water or 1 wt % or more of hydrogen peroxide solution and then heat treating the nickel nanoparticles at a temperature of, for example, 150° C. or lower, preferably within a range of 70° C. to 150° C. When nickel nanoparticle aggregates are formed on a resin substrate, the heat treatment temperature is more preferably within a range of 70° C. to 120° C. in order to prevent damage to the resin substrate.

[0052] There is no particular restriction on the method of contacting the flocculating liquid, but if a large amount is used and the flocculating liquid is immersed for a long time, granular deposits that are thought to be nickel hydroxide will occur on the surface of the nickel nanoparticles, making it difficult to form a coating. In addition, if the amount of nickel hydroxide precipitates too much, it is not preferable because nickel's inherent properties such as magnetism and conductivity will be lost. Therefore, it is preferable to contact an appropriate amount of the flocculating liquid with the nickel nanoparticle paste by a method such as spraying or coating. In addition, as described above, it is preferable to heat treat the nickel nanoparticles at 70°C or higher after contacting the flocculating liquid with the nickel nanoparticles.

[0053] The substrate may be an inorganic substrate having high heat resistance such as a metal substrate, a glass substrate, or a ceramic substrate, and may also be a resin substrate having lower heat resistance than an inorganic substrate. Known resins may be used for the resin substrate, such as nylon resin, epoxy resin, acrylic resin, polyethylene terephthalate, polyimide, polycarbonate, and liquid crystal polymer. By applying the nickel nanoparticle paste onto these substrates, drying the paste, contacting the substrate with the aggregating liquid, and drying the paste, nickel nanoparticle aggregates are formed on the substrates, and a composite of nickel nanoparticles and the substrate (nickel nanoparticle composite substrate) can be suitably obtained. EXAMPLES

[0054] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In the following examples, unless otherwise specified, measurements and evaluations were performed according to the following methods.

[0055] [Measurement of average particle size] The average particle size was measured by taking a photograph of the sample using a SEM (scanning electron microscope), randomly selecting 200 particles from the sample, determining the area of ​​each, and calculating the average particle size of the primary particles based on the particle size when converted to a perfect sphere. The CV value (coefficient of variation) was calculated by dividing the standard deviation by the average particle size. The smaller the CV value, the more uniform the particle size.

[0056] [Application of nickel nanoparticle paste] Two slides (76mm x 26mm x t1.1mm) made by Matsunami Glass Industry Co., Ltd. were wiped with absorbent cotton soaked in acetone to remove dirt and then dried. Approximately 0.05g of nickel nanoparticle paste was weighed out in the center of one slide and sandwiched between the other slide. The paste was then spread while applying pressure so that it did not spill out from the sides, and the slides were slid in parallel directions to obtain a smooth coating surface.

[0057] [Evaluation of cohesion] A solution containing 30-35 wt% hydrogen peroxide (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) or an isopropanol solution containing 10 wt% water was sprayed onto the nickel nanoparticle paste applied to a glass slide using a spray bottle, and the sample was allowed to soak for approximately 1 minute. The sample was then dried in a tabletop oven at 80°C, and its coagulation was evaluated using an optical microscope and an electron microscope.

[0058] [Quantitative determination of nickel] The amount of nickel dimethylglyoxime detected was determined by the nickel measurement method specified in JIS K 0102 59.1, and this was taken as the amount of nickel ions detected.

[0059] [Measurement of specific surface area] The specific surface area of ​​nickel particles [m 2 / g] was measured.

[0060] [Elemental analysis] 1. H, C, and N were measured according to JIS8819 Coal and cokes - Elemental analysis using an instrumental analyzer. 2.O was measured according to JIS8813 Coal and cokes - Elemental analysis method.

[0061] [Calculated value V] The calculated value V was determined based on the following formula (1). V = A × D 3 / S / 10000000 ···(1) {In the formula, A means the amount of nickel dimethylglyoxime detected [ppm] as determined by the nickel measurement method specified in JIS K 0102 59.1, and S means the specific surface area [m 2 / g], and D means the average particle size [nm] of nickel particles measured by scanning electron microscope (SEM).}

[0062] [Organometallic compound] Organometallic compound (1): Fujifilm Wako Pure Chemical Industries, Ltd., phenyllithium in approximately 19% dibutyl ether solution (approximately 1.9 mol / L)

[0063] The materials used to prepare the nickel nanoparticle slurry and their abbreviations are as follows:

[0064] Solvent (1): Decahydronaphthalene (Fujifilm Wako Pure Chemical Industries, Ltd.; Grade 1) Solvent (2): Terpineol

[0065] Dispersant (1): Aliphatic polymer dispersant (manufactured by Lubrizol Japan, product name: Solsperse 9000) Dispersant (2): Polyester-based polymer dispersant (manufactured by Lubrizol Japan, product name: Solsperse 13240)

[0066] Binder resin (1): aliphatic saturated hydrocarbon resin (manufactured by Arakawa Chemical Industries, Ltd., product name: Alcon P-100) / decahydronaphthalene=2 / 1 parts by weight Binder resin (2): Cellulosic resin / terpineol=1 / 10 parts by weight (manufactured by Nisshin Chemical Industry Co., Ltd., product name: EC-100FTP)

[0067] (Synthesis Example 1) 246.8 g of nickel acetate tetrahydrate was added to 600 g of oleylamine, and heated at 140 ° C for 3 hours under nitrogen flow to obtain complexation reaction solution 1 (nickel ion concentration: 7.5 wt%). After cooling this complexation reaction solution 1 to about 60 ° C, 0.10 g of organometallic compound (1) was added, reacted at 215 ° C for 7 minutes, and then rapidly cooled to obtain nickel nanoparticle slurry 1. The analysis results of the obtained nickel nanoparticle slurry 1 are shown in Tables 1 and 2. In addition, a part of the obtained nickel nanoparticles 1 was dried at 80 ° C for 1 hour, sprayed with an isopropanol solution containing 10 wt % water with a spray bottle, and dried at 80 ° C for 1 hour. The analysis results are shown in Table 3.

[0068] (Synthesis Example 2) 246.8 g of nickel acetate tetrahydrate was added to 600 g of oleylamine, and heated at 140 ° C for 3 hours under nitrogen flow to obtain a complexation reaction solution 2 (nickel ion concentration: 7.5 wt%). After cooling this complexation reaction solution 2 to about 60 ° C, 1.10 g of organometallic compound (1) was added, reacted at 212 ° C for 5 minutes, and then quenched to obtain nickel nanoparticle slurry 2. The analysis results of the obtained nickel nanoparticle slurry 2 are shown in Tables 1 and 2. In addition, a part of the obtained nickel nanoparticles 2 was dried at 80 ° C for 1 hour, sprayed with an isopropanol solution containing 10 wt % water with a spray bottle, and dried at 80 ° C for 1 hour. The analysis results are shown in Table 3.

[0069] (Synthesis Example 3) 246.8 g of nickel acetate tetrahydrate was added to 600 g of oleylamine, and heated at 140 ° C for 3 hours under nitrogen flow to obtain complexation reaction solution 1 (nickel ion concentration: 7.5 wt%). After cooling this complexation reaction solution 1 to about 60 ° C, 3.0 g of organometallic compound (1) was added, reacted at 212 ° C for 5 minutes, and then quenched to obtain nickel nanoparticle slurry 3. The analysis results of the obtained nickel nanoparticle slurry 3 are shown in Tables 1 and 2. In addition, a part of the obtained nickel nanoparticles 3 was dried at 80 ° C for 1 hour, sprayed with an isopropanol solution containing 10 wt % water with a spray bottle, and dried at 80 ° C for 1 hour. The analysis results are shown in Table 3.

[0070] (Synthesis Example 4) 246.8 g of nickel acetate tetrahydrate was added to 600 g of oleylamine, and heated at 140 ° C for 3 hours under nitrogen flow to obtain complexation reaction solution 1 (nickel ion concentration: 7.5 wt%). After cooling this complexation reaction solution 1 to about 60 ° C, 0.10 g of organometallic compound (1) was added, reacted at 215 ° C for 30 minutes, and then quenched to obtain nickel nanoparticle slurry 4. The analysis results of the obtained nickel nanoparticle slurry 4 are shown in Tables 1 and 2. In addition, a part of the obtained nickel nanoparticles 4 was dried at 80 ° C for 1 hour, sprayed with an isopropanol solution containing 10 wt % water with a spray bottle, and dried at 80 ° C for 1 hour. The analysis results are shown in Table 3.

[0071] [Table 1]

[0072] [Table 2]

[0073] [Table 3]

[0074] Example 1 The nickel nanoparticle slurry 1 obtained in Synthesis Example 1 was precipitated with a neodymium magnet, the supernatant was discarded, about 50 g of toluene washing solvent was added, and the mixture was shaken for 10 minutes using a shaker, and then the mixture was precipitated with a neodymium magnet and the supernatant was discarded, which was repeated three times to obtain a nickel nanoparticle toluene slurry. About 1 g of nickel nanoparticles was collected from this slurry, 0.2 g of dispersant (1) was added, and the mixture was treated with ultrasound for 10 minutes, after which the supernatant was discarded using a neodymium magnet, about 15 cc of solvent (1) was added, and the mixture was subjected to ultrasound for 10 minutes and the supernatant was discarded three times to obtain a nickel nanoparticle decahydronaphthalene slurry. The nickel nanoparticle solid content of this slurry was adjusted to 85%, and then 0.05 g of binder resin (1) was added, and the mixture was stirred for 10 minutes using a stirring device (trade name: Rentaro, manufactured by Thinky Corporation) to obtain paste 1. This paste 1 was applied to a slide glass and dried at 80°C. The state of this dried paste was observed by SEM and the result is shown in FIG. 1. After drying, 30-35 wt% hydrogen peroxide was sprayed onto the surface, dried at 80°C, and observed with an SEM. The results are shown in Figure 2. Comparing Figures 1 and 2, it was confirmed that a film presumably made of nickel hydroxide or nickel oxide had formed around the nickel nanoparticles in Figure 2, and that favorable agglomerations had been formed.

[0075] Example 2 A dry paste and an aggregate were prepared in the same manner as in Example 1, except that nickel nanoparticle slurry 2 was used, and the results of observing them with an SEM are shown in Figure 3 (dried paste) and Figure 4 (aggregate). Comparing Figures 3 and 4, it was confirmed that a coating was formed around the nickel nanoparticles in Figure 4, and good aggregates were formed.

[0076] Example 3 A dried paste and an aggregate were prepared in the same manner as in Example 1, except that nickel nanoparticle slurry 3 was used, and the results of observing them with an SEM are shown in Figure 5 (dried paste) and Figure 6 (aggregate). Comparing Figures 5 and 6, it was confirmed that a coating was formed around the nickel nanoparticles in Figure 6, and good aggregates were formed.

[0077] Example 4 A dried paste and an aggregate were prepared in the same manner as in Example 1, except that the solvent (1) in Example 1 was changed to the solvent (2), the dispersant (1) to the dispersant (2), and the binder resin (1) to the binder resin (2), and the amount of the binder resin (2) used was changed to 0.03 g. The results of observing the obtained aggregate with an SEM are shown in FIG. 7. It was confirmed from FIG. 7 that a coating was formed around the nickel nanoparticles, and a good aggregate was formed.

[0078] Example 5 A dry paste and an aggregate were prepared in the same manner as in Example 1, except that the 30-35% hydrogen peroxide solution used in the evaluation of the bondability in Example 1 was replaced with an isopropanol solution containing 10 wt% water. The results of observing the obtained aggregate with an SEM are shown in Figure 8. From Figure 8, it was confirmed that a coating was formed around the nickel nanoparticles, and a good aggregate was formed.

[0079] Comparative Example 1 Nickel nanoparticles were separately synthesized in the same manner as in Synthesis Example 1, and a nickel nanoparticle slurry with an average particle size of 43.5 nm was obtained. The analysis results of the obtained nickel nanoparticle slurry 2 are shown in Table 2. Using this nickel nanoparticle slurry, a dried paste was prepared in the same manner as in Example 1, except that the toluene washing solvent was changed to a methanol / toluene = 1 / 4 mixed solvent, and an attempt was made to prepare an aggregate by further treating it with hydrogen peroxide. The results of observation with an SEM are shown in Figure 9 (dried paste) and Figure 10 (after hydrogen peroxide treatment). From a comparison of Figures 9 and 10, it was confirmed that no coating was formed on the surface of the nickel nanoparticles, and no aggregates were obtained. In addition, a portion of the obtained nickel nanoparticles was dried at 80°C for 1 hour, and then an isopropanol solution containing 10 wt% water was sprayed onto the nanoparticles using a spray bottle. The nanoparticles were then dried at 80°C for 1 hour, and the analysis results are shown in Table 3.

[0080] Comparative Example 2 A dried paste was prepared in the same manner as in Example 1, except that nickel nanoparticle slurry 4 was used, and then treated with hydrogen peroxide to prepare an aggregate. The results of observation with an SEM are shown in Figure 11 (dried paste) and Figure 12 (paste after hydrogen peroxide treatment). Comparing Figures 11 and 12, it was confirmed that some areas had a coating and some did not, and good aggregates could not be obtained.

[0081] Although the embodiment of the present invention has been described in detail above for the purpose of illustration, the present invention is not limited to the above embodiment.

Claims

1. The nickel nanoparticles have an average particle size of 5 to 100 nm and have a coating of nickel hydroxide and / or nickel oxide on the surface thereof, and the nickel nanoparticles are aggregated together directly or via the coating, The nickel nanoparticles are nickel nanoparticles having a calculated value V of 3 or more as calculated by the following formula (1). V=A×D 3 / S / 10000000...(1) {In the formula, A means the amount of nickel dimethylglyoxime detected [ppm] detected by the nickel measurement method specified in JIS K 0102 59.1, S means the specific surface area [m 2 / g] of nickel particles measured by a gas adsorption method, and D means the average particle diameter [nm] of nickel particles measured by a scanning electron microscope (SEM).}

2. 2. The nickel nanoparticle aggregate of claim 1, wherein the nickel nanoparticles are composed of nickel alone or an alloy of nickel with one or more metals selected from lithium, copper, iron, cobalt, gold, platinum and palladium.

3. The nickel nanoparticle aggregate according to claim 1 or 2, wherein 99 wt % or more of the metal component contained in the nickel nanoparticle is nickel.

4. A substrate; A nickel nanoparticle composite substrate comprising the nickel nanoparticle aggregate according to claim 1 laminated on the substrate.

5. A step of preparing a nickel nanoparticle paste in which nickel nanoparticles having an average particle size of 5 to 100 nm and a binder resin are dispersed in a non-polar solvent; A step of contacting the nickel nanoparticle paste with water or hydrogen peroxide solution to form a coating on the surface of the nickel nanoparticles and agglomerate the nickel nanoparticles directly or via the coating; A method for producing nickel nanoparticle aggregates comprising:

Citation Information

Patent Citations

  • Sheet payoff device

    JP1985061427A

  • Method of producing metallic fine particle

    JP2003193118A

  • Spherical nickel microparticle, production method therefor, and electroconductive particle for anisotropic electroconductive film

    JP2008095146A

  • Joining method and joined body

    JP2010029871A

  • Semiconductor nanoparticle and production method of the same

    JP2010105149A