Bound stopper and manufacturing method thereof
A polyurethane elastomer foam composition with specific components addresses the challenge of achieving high mechanical strength and durability in bound stoppers by controlling density and cell diameter, resulting in a durable and easily manufacturable stopper for vehicle shock absorbers.
Patent Information
- Application Number
- JP2020145542
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-08-31
- Publication Date
- 2024-10-25
- Estimated Expiration
- 2040-08-31
AI Technical Summary
Existing methods for manufacturing bound stoppers for vehicle shock absorbers face challenges in controlling the skin layer density and foam cell diameter, making it difficult to achieve high mechanical strength and durability against fatigue failure under repeated loads.
A polyurethane elastomer foam composition is used, comprising a urethane prepolymer with terminal isocyanate groups derived from polytetramethylene ether glycol and diphenylmethane diisocyanate, along with polycaprolactone diol, to create a bound stopper with controlled density and cell diameter, ensuring high mechanical strength and durability.
The solution results in a bound stopper with enhanced mechanical strength and durability, capable of withstanding repeated heavy loads without requiring complex reaction control, and is easier to manufacture.
Smart Images

Figure 0007573393000001 
Figure 0007573393000002 
Figure 0007573393000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a bound stopper that is attached to a piston rod of a shock absorber for a vehicle and a method for manufacturing the same. [Background technology]
[0002] As shown in Fig. 5, a shock absorber 70 for a vehicle has a bound stopper 75 attached to a piston rod 72 of a cylinder. Reference numeral 71 denotes a cylinder body, and reference numeral 73 denotes a spring. The bound stopper 75 is made of an elastic foam molded into a bellows shape, and when the shock absorber 70 expands or contracts due to impact or vibration from the road surface and the cylinder body 71 collides with the bound stopper 75, the bound stopper 75 is compressed and deformed to absorb the impact.
[0003] The bound stopper 75 is subjected to repeated collisions with the cylinder body and the resulting compressive deformation, and therefore is required to have high mechanical strength and durability against fatigue failure and settling when subjected to repeated heavy loads.
[0004] Conventionally, as a bound stopper that aims to reduce costs while providing durability and resistance to settling under high loads and large deformations, a polyurethane foam has been proposed that is made by injecting a urethane raw material containing a polyester polyol as the polyol component and diphenylmethane diisocyanate as the isocyanate component into a mold and heating it to 70°C or higher for primary vulcanization, and then removing the molded body from the mold and heating it for secondary vulcanization, whereby the density (Da) and foam cell diameter (Ra) of the skin layer and the density (Db) and foam cell diameter (Rb) of the core satisfy specific formulas and relationships (Patent Document 1). [Prior art documents] [Patent documents]
[0005] [Patent Document 1] JP 2015-183832 A Summary of the Invention [Problem to be solved by the invention]
[0006] However, the primary and secondary vulcanization processes must be performed so that the density (Da) and foam cell diameter (Ra) of the skin layer and the density (Db) and foam cell diameter (Rb) of the core layer satisfy specific formulas and relationships, making it difficult to control the reaction.
[0007] The present invention has been made in consideration of the above-mentioned points, and an object of the present invention is to provide a bound stopper that has high mechanical strength, excellent durability against fatigue failure and settling when repeatedly subjected to large loads, and is easy to manufacture, and a method for manufacturing the same. [Means for solving the problem]
[0008] First aspect of the invention The present invention relates to a polyurethane elastomer foam bound stopper to be attached to a piston rod of a shock absorber for a vehicle, the bound stopper being made of a polyurethane elastomer foam obtained from a polyurethane elastomer foam composition containing at least an isocyanate component and a foaming agent, the isocyanate component being a urethane prepolymer having an isocyanate group at a terminal thereof, the urethane prepolymer being obtained from a polyol component containing polytetramethylene ether glycol and diphenylmethane diisocyanate.
[0009] Second aspect of the invention teeth, First aspect of the invention The polyol component contains the polytetramethylene ether glycol and polycaprolactone diol.
[0010] Third aspect of the invention teeth, First aspect of the invention or Second aspect of the invention The urethane prepolymer has an NCO% of 3.0 to 6.0%.
[0011] Fourth aspect of the invention teeth, First aspect of the invention from Third aspect of the invention Either one of Aspects With a density of 0.3 to 0.7 g / cm 3 It is characterized by having a tensile strength of 3.0 MPa or more.
[0012] Fifth aspect of the invention The present invention relates to a method for producing a bound stopper made of a polyurethane elastomer foam to be attached to a piston rod of a shock absorber for a vehicle, the method comprising: injecting a polyurethane elastomer foam composition, which contains a urethane prepolymer having an isocyanate group at its terminal, obtained from a polyol component containing polytetramethylene ether glycol and diphenylmethane diisocyanate, and a foaming agent, into a mold and foaming the composition to form a bound stopper made of the polyurethane elastomer foam.
[0013] Sixth aspect of the invention teeth, Fifth aspect of the invention The polyol component contains the polytetramethylene ether glycol and polycaprolactone diol.
[0014] Seventh aspect of the invention teeth, Fifth aspect of the invention or Sixth aspect of the invention The urethane prepolymer has an NCO% of 3.0 to 6.0%. Effect of the Invention
[0015] The bound stopper of the present invention is composed of a polyurethane elastomer foam obtained from a polyurethane elastomer foam composition containing at least an isocyanate component and a foaming agent. The isocyanate component is a urethane prepolymer having an isocyanate group at its end, which is obtained from a polyol component containing polytetramethylene ether glycol and diphenylmethane diisocyanate, and therefore the mechanical strength of the bound stopper can be increased, and durability when a large load is repeatedly applied can be improved.
[0016] The polyol component may include polytetramethylene ether glycol and polycaprolactone diol. By including polycaprolactone diol together with polytetramethylene ether glycol in the polyol component, the viscosity of the urethane prepolymer having an isocyanate group at its end can be reduced, making it less likely to develop defects such as underfill and air pockets that tend to occur in foams due to high viscosity.
[0017] Furthermore, according to the manufacturing method of the present invention, it is not necessary to perform the complicated reaction control required by the primary and secondary vulcanization processes used in conventional technology in order to make the density (Da) and foam cell diameter (Ra) of the skin layer and the density (Db) and foam cell diameter (Rb) of the core layer satisfy specific formulas and relationships, making it easy to manufacture a bound stopper that has high mechanical strength and improved durability when repeatedly subjected to large loads. [Brief description of the drawings]
[0018] [Figure 1] FIG. 2 is a cross-sectional view of a bound stopper according to an embodiment of the present invention. [Diagram 2] 1A and 1B are cross-sectional views of a mold used in manufacturing the bound stopper of the present invention and a cross-sectional view of the mold during foaming. [Diagram 3] 4 is a cross-sectional view of a mold during demolding in the manufacture of the bound stopper of the present invention. FIG. [Figure 4] 1 is a table showing the compositions and physical properties of each of the examples and comparative examples. [Diagram 5] FIG. 4 is a cross-sectional view showing a state in which the bound stopper is attached. BEST MODE FOR CARRYING OUT THEINVENTION
[0019] The bound stopper 10 according to one embodiment of the present invention shown in FIG. 1 is attached to a piston rod 72 of a shock absorber of a vehicle, similar to the bound stopper 75 shown in FIG.
[0020] The bound stopper 10 is made of a cylindrical polyurethane elastomer foam with a side outer peripheral surface 10a molded into a bellows shape, and has a through hole 11 formed in the center to allow the piston rod of the shock absorber to pass through. The bound stopper 10 is formed so that the upper part 10b has a larger outer diameter than the lower part 10c. The length and diameter of the bound stopper 10 are determined according to the shock absorber.
[0021] The density of the polyurethane elastomer foam constituting the bound stopper 10 (in accordance with JIS K7222:2005) is 0.3 to 0.7 g / cm 3 The density is preferably 0.3 g / cm 3 If the density is less than 0.7 g / cm, the physical properties of the polyurethane elastomer foam will be deteriorated and the durability against repeated compression will be poor. 3 If it exceeds this value, the foaming pressure during foam molding of the polyurethane elastomer foam becomes too high, making molding difficult.
[0022] The tensile strength (in accordance with JIS K6251:2017) of the polyurethane elastomer foam constituting the bound stopper 10 is preferably 3.0 MPa or more, and more preferably 3.5 MPa or more and 5.0 MPa or less.
[0023] The polyurethane elastomer foam constituting the bound stopper 10 is obtained from a polyurethane elastomer foam composition. The polyurethane elastomer foam composition contains at least an isocyanate component and a foaming agent.
[0024] The isocyanate component is composed of a urethane prepolymer having an isocyanate group at the end, which is obtained from a polyol component containing polytetramethylene ether glycol (PTMG) and diphenylmethane diisocyanate.
[0025] Polytetramethylene ether glycol (PTMG) has the rational formula [HO-(CH2CH2CH2CH2O) n -H]. The polyol component may include polycaprolactone diol (PCL) along with polytetramethylene ether glycol. Polycaprolactone diol is obtained by ring-opening polymerization of ε-caprolactone. The weight ratio of polytetramethylene ether glycol (PTMG) to polycaprolactone diol (PCL) is preferably PTMG:PCL=100:0 to 10:90. The polyol used preferably has a weight average molecular weight (Mw) of 800 to 5000, more preferably 1000 to 3000, and a hydroxyl value of 20 to 200 mgKOH / g, more preferably 35 to 180 mgKOH / g.
[0026] Diphenylmethane diisocyanate (MDI) includes 2,2'-diphenylmethane diisocyanate, 2,4'-diphenylmethane diisocyanate, 4,4'-diphenylmethane diisocyanate, and polymeric MDI (crude MDI). 4,4'-diphenylmethane diisocyanate is also called monomeric MDI or pure MDI. Polymeric MDI (crude MDI) is a mixture of monomeric MDI and high molecular weight polyisocyanate. Among them, 4,4'-diphenylmethane diisocyanate is preferred. The diphenylmethane diisocyanate used in the present invention is less expensive than 1,5-naphthalene diisocyanate (NDI). In addition, compared to NDI, it is produced in a larger amount worldwide and can be procured globally.
[0027] The NCO% of the urethane prepolymer having an isocyanate group at its end is preferably 3.0 to 6.0%. If the NCO% is less than 3.0%, sufficient strength is not obtained and durability is also deteriorated. On the other hand, if the NCO% is more than 6.0%, the flexibility is reduced and the prepolymer becomes hard, brittle, and durability is reduced, and the prepolymer is too hard to be removed from the mold.
[0028] The urethane prepolymer having an isocyanate group at its end, which is used in the present invention, can be obtained by a known method for producing a urethane prepolymer. Specifically, a predetermined amount of polyol is charged into a tank or the like, heated to a predetermined temperature (e.g., 130°C), and while maintaining the heated temperature and filling the tank with nitrogen, a predetermined amount of diphenylmethane diisocyanate is charged and reacted while stirring, thereby obtaining the urethane prepolymer having an isocyanate group at its end, which is used in the present invention.
[0029] The blowing agent contained in the polyurethane elastomer foam composition may be water, a fluorocarbon substitute, or a hydrocarbon such as pentane, either alone or in combination. In the case of water, carbon dioxide gas is generated during the reaction of the isocyanate component, and the foaming is caused by the carbon dioxide gas. The amount of water used as the blowing agent is preferably about 0.2 to 5 parts by weight per 100 parts by weight of the urethane prepolymer having an isocyanate group at its end.
[0030] The polyurethane elastomer foam composition may contain additives such as a catalyst, a foam stabilizer, a hydrolysis stabilizer, a crosslinking agent, a flame retardant, a colorant, a stabilizer, and a filler.
[0031] The catalyst may be a known urethanization catalyst or a retardation catalyst (temperature-sensitive catalyst). Examples of the urethanization catalyst include amine catalysts such as triethylamine, triethylenediamine, diethanolamine, dimethylaminomorpholine, N-ethylmorpholine, and tetramethylguanidine, tin catalysts such as stannous octoate and dibutyltin dilaurate, and metal catalysts such as phenylmercury propionate and lead octenate (also called organometallic catalysts). The retardation catalyst is an amine salt in which the active group of the urethanization catalyst is blocked with an acid such as formic acid or octylic acid, and examples of the retardation catalyst include phenol salts of diazabicycloalkenes, octylic acid salts of diazabicycloalkenes, and tertiary amine salts.
[0032] The foam stabilizer may be any foam stabilizer that is used for polyurethane foam, and examples of such foam stabilizers include silicone foam stabilizers, fluorine-containing compound foam stabilizers, and known surfactants. If the foam stabilizer is added during the preparation of the urethane prepolymer having an isocyanate group at its end, it will be uniformly dispersed in the urethane prepolymer having an isocyanate group at its end, improving the foam stabilizing power and allowing the production of a polyurethane foam with fine and uniform cells.
[0033] Examples of the hydrolysis stabilizer include carbodiimide compounds. In particular, when a polyester polyol is used as the polyol component, the hydrolysis resistance of the polyurethane foam can be improved by adding a hydrolysis stabilizer. Since a carbodiimide group is reactive with an active hydrogen group, it is preferable to add the carbodiimide group together with a blowing agent during the production of the polyurethane foam.
[0034] Examples of the crosslinking agent include ethylene glycol, diethylene glycol, propylene glycol, dipropylene glycol, 1,4-butanediol, glycerin, trimethylolpropane, etc. The crosslinking agent is preferably blended when preparing a urethane prepolymer having an isocyanate group at its end, and by mixing the crosslinking agent in a molten state together with a polyol component and a polyrotaxane, the crosslinking agent can be uniformly dispersed in the urethane prepolymer.
[0035] Examples of the flame retardant include halogenated compounds such as polyvinyl chloride, chloroprene rubber, and chlorinated polyethylene, condensed phosphoric acid compounds such as phosphoric acid esters and halogenated phosphoric acid esters, organic compounds such as melamine resins and urea resins, and inorganic compounds such as antimony oxide and aluminum hydroxide. If the flame retardant is added during the preparation of a urethane prepolymer having an isocyanate group at its terminal, it can be uniformly dispersed in the urethane prepolymer.
[0036] Examples of the colorant include pigments, dyes, etc. If the colorant is added during the preparation of the urethane prepolymer having an isocyanate group at its end, it can be uniformly dispersed in the urethane prepolymer.
[0037] Examples of the stabilizer include an antioxidant, an ultraviolet absorber, a light stabilizer, etc. If the stabilizer is added during the preparation of the urethane prepolymer having an isocyanate group at its end, it can be uniformly dispersed in the urethane prepolymer.
[0038] The isocyanate index (INDEX) is preferably 90 to 120. If the isocyanate index is less than 90, the degree of crosslinking is small, and the polyurethane foam does not obtain sufficient mechanical strength, and the polyurethane foam is more likely to collapse when subjected to repeated load, while if the isocyanate index is more than 120, the degree of crosslinking is large, and the polyurethane foam becomes hard and has low elasticity. A more preferable isocyanate index is 95 to 115. The isocyanate index is an index used in the field of polyurethane foams, and is a numerical value [NCO group equivalent / active hydrogen group equivalent×100] that represents the equivalent ratio of isocyanate groups to active hydrogen groups in a polyurethane elastomer foam composition, expressed as a percentage.
[0039] The method for producing the bound stopper will be described below. The production of the bound stopper comprises a step of preparing a urethane prepolymer having an isocyanate group at its end, a step of injecting and foaming a polyurethane elastomer foam composition into a mold, and a step of demolding.
[0040] In the process of preparing a urethane prepolymer having an isocyanate group at its end, a predetermined amount of polyol and a predetermined amount of diphenylmethane diisocyanate are mixed while being heated to a predetermined temperature (e.g., 130°C) to prepare a urethane prepolymer having an isocyanate group at its end.
[0041] In the step of injecting and foaming the polyurethane elastomer foam composition into a mold, the polyurethane elastomer foam composition, which contains at least a urethane prepolymer having an isocyanate group at its terminal, a foaming agent, and appropriate additives, is injected into a mold and foamed to form a bound stopper made of the polyurethane foam.
[0042] 2(2-A) shows one embodiment of a bound stopper mold 30. The mold 30 comprises a lower mold 31, a middle mold 33, and an upper mold . The lower die 31 is made up of a first lower die 31a and a second lower die 31b which can be separated into left and right halves, and has die surfaces 311a, 311b which form the side outer peripheral surface 10a of the bound stopper 10. The middle die 33 is substantially rod-shaped and has a die surface 33a on its outer periphery that forms the through hole 11 of the bound stopper 10, and is disposed between the first lower die 31a and the second lower die 31b. The lower die 31 and the middle die 33 are combined to form a cavity 34 between the die surface 311a of the first lower die 31a and the die surface 311b of the second lower die 31b and the die surface 33a of the middle die 33.
[0043] After the polyurethane elastomer foam composition is injected into the cavity 34, as shown in Fig. 2 (2-B), an upper mold 35 is placed over the cavity 34 to close the mold, and the polyurethane elastomer foam composition 40 is reacted and foamed. The mold is left in the closed state for a predetermined time to cure (primary cure), and a bound stopper 10 made of a polyurethane foam is formed. The primary cure is preferably performed at 60 to 120°C for 10 to 120 minutes.
[0044] In the demolding step, as shown in FIG. 3, the upper mold 35 is removed, the first lower mold 31a and the second lower mold 31b are opened, and the middle mold 33 is separated. The middle mold 33 separated from the first lower mold 31a and the second lower mold 31b is in a state of being fitted into the through hole 11 of the bound stopper 10 made of the polyurethane foam. Thereafter, the bound stopper 10 is wiped off from the middle mold 33 by utilizing its elasticity, and the bound stopper 10 is obtained. It is preferable that the bound stopper 10 is subjected to a secondary cure after demolding. The secondary cure is preferably performed at 90 to 180° C. for 8 to 24 hours. EXAMPLES
[0045] <Preparation of urethane prepolymer having isocyanate groups at its terminals> Urethane prepolymers having an isocyanate group at the end thereof for use in Examples 1 to 11 and Comparative Example 1 were prepared from PTMG-1 to 3 as polyols shown in FIG. 4, PCL, an ester polyol, and an isocyanate. PTMG-1 to 3, PCL, ester polyol and isocyanate consist of the following:
[0046] PTMG-1 PTMG-1 is polytetramethylene ether glycol, Mw: 2000, bifunctional, hydroxyl value: 56 mgKOH / g, product number: PTMG2000, manufactured by Mitsubishi Chemical Corporation. PTMG-2 PTMG-2 is polytetramethylene ether glycol, Mw: 1000, bifunctional, hydroxyl value: 112 mgKOH / g, product number: PTMG1000, manufactured by Mitsubishi Chemical Corporation. PTMG-3 PTMG-3 is polytetramethylene ether glycol, Mw: 3000, bifunctional, hydroxyl value: 37 mgKOH / g, product number: PTMG3000, manufactured by Mitsubishi Chemical Corporation. · PCL PCL is polycaprolactone diol, Mw: 2000, bifunctional, hydroxyl value: 56 mgKOH / g, product name: Plaxel 220N, manufactured by Daicel Corporation. Ester polyol The ester polyol was a condensation polyester polyol made of adipic acid (AA) and ethylene glycol (EG), with Mw of 2000, functionality of 2, and hydroxyl value of 56 mg KOH / g, product name Polylite OD-X-102, manufactured by DIC Corporation. Isocyanates The isocyanate used was 4,4'-diphenylmethane diisocyanate (monomeric MDI), NCO %: 33.6%, product name: Millionate MT, manufactured by Tosoh Corporation.
[0047] The above polyol and isocyanate were used in the ratios shown in Examples 1 to 11 and Comparative Example 1 in FIG. 4 to prepare urethane prepolymers having isocyanate groups at their ends as follows.
[0048] Into a 20 L metal reaction vessel, the specified amounts of polyol and isocyanate corresponding to Examples 1 to 11 and Comparative Example 1 were charged, and after charging, the mixture was heated to 130°C and mixed for 20 minutes. Thereafter, the reaction vessel was left at room temperature and slowly cooled to produce a urethane prepolymer (Liquid B) having an isocyanate group at its end.
[0049] <Preparation of test pieces> Using the prepared urethane prepolymer having an isocyanate group at its end (liquid B) and the following foaming liquid (liquid A), test pieces of Examples 1 to 11 and Comparative Example 1 were prepared by the methods described below. Foaming liquid (liquid A): Contains a compound having an active hydrogen group, a surfactant, and a catalyst. The ratio of each component in the foaming liquid (liquid A) is: compound with active hydrogen group: surfactant: catalyst = 700 : 400 : 5 Compound with active hydrogen group: mixture of castor oil and water, product number: Advade SV (castor oil and water weight ratio 50:50), manufactured by Rhein Chemie Japan Surfactant; Product name: Brownon O-200SA, manufactured by Ito Oil Mills Catalyst: Product name: Adcat PP, manufactured by Rhein Chemie Japan
[0050] A polyurethane elastomer foam composition was prepared by blending a urethane prepolymer having an isocyanate group at its end, the temperature of which was adjusted to 80°C, and a foaming liquid, the temperature of which was adjusted to 40°C, in the ratios shown in FIG. 4 for Examples 1 to 11 and Comparative Example 1. The polyurethane elastomer foam composition was mixed and then poured into a test piece mold, the temperature of which was adjusted to 80°C, in the amount shown in FIG. 4. The test piece mold had a cavity of 200×110×30 mm. After the polyurethane elastomer foam composition was poured into the mold, it was foamed in the mold and cured at 80°C for 30 minutes (primary curing), and the obtained polyurethane foam was demolded. The polyurethane foam after demolding was further cured at 100°C for 12 hours (secondary curing) to obtain test pieces of Examples 1 to 11 and Comparative Example 1.
[0051] <Product creation> The products (bound stoppers) of Examples 1 to 11 and Comparative Example 1 were obtained in the same manner as in the production of the test pieces, except that the production mold (cavity volume 152 ml) shown in Figures 2 and 3 was used and the injection amount into the production mold was the injection amount of each example and comparative example shown in Figure 4.
[0052] The density and tensile strength of the test pieces of each of the examples and comparative examples were measured, and the durability of the products was also measured. The measurement results are shown in Figure 4.
[0053] The density was measured in accordance with JIS K7222:2005 using a test piece (200×110×30 mm) as a measurement sample (with skin layers on all top, bottom and side surfaces).
[0054] Tensile strength was measured in accordance with JIS K6251:2017 by slicing a measurement sample of No. 2 dumbbell size and thickness of 2 mm (no skin layer on the top, bottom or sides) from the test piece. Tensile strength was judged as "x" when it was less than 3 MPa, and "good" when it was 3 MPa or more.
[0055] In measuring durability, the product (bound stopper 10) is inserted into the shaft, and the upper surface of the upper part 10b and the lower surface of the lower part 10c of the inserted product are sandwiched and fixed between disk-shaped plates. A load cell is placed on the upper surface of the disk-shaped plate at the top of the product, and a repeated compression test is performed in which the product is repeatedly compressed from the lower surface of the disk-shaped plate at the bottom of the product under measurement conditions of 6KN x 1Hz. If the number of repeated compressions at which the product cracks occurs is less than 80,000 times, it is judged as "X", if it is between 80,000 and less than 100,000 times, it is judged as "△", and if it is 100,000 times or more, it is judged as "O". In addition, if either the tensile strength judgment or the durability judgment was "X", the overall judgment was "X". If both judgments were "△" or "△" and "◯", the overall judgment was "△". If both judgments were "◯", the overall judgment was "◯".
[0056] In Example 1, a polyurethane elastomer foam composition with an isocyanate index of 100 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 3.1%, which was made from 1000 g of PTMG-1 and 240 g of 4,4'-diphenylmethane diisocyanate, and 2.0 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to prepare a test piece and a product. Example 1 has a density of 0.50 g / cm 3 The tensile strength was 3.5 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0057] In Example 2, a polyurethane elastomer foam composition with an isocyanate index of 105 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.1%, which was made from 1000 g of PTMG-1 and 280 g of 4,4'-diphenylmethane diisocyanate, and 2.5 g of foaming liquid. The amounts of this composition injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to produce a test piece and a product. Example 2 has a density of 0.50 g / cm 3 The tensile strength was 3.8 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0058] In Example 3, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 1000 g of PTMG-1 and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to produce a test piece and a product. Example 3 has a density of 0.50 g / cm 3The tensile strength was 4.2 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0059] In Example 4, a polyurethane elastomer foam composition with an isocyanate index of 104 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 6.0%, which was made from 1000 g of PTMG-1 and 370 g of 4,4'-diphenylmethane diisocyanate, and 3.7 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to produce a test piece and a product. Example 4 has a density of 0.50 g / cm 3 The tensile strength was 4.8 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0060] In Example 5, a polyurethane elastomer foam composition with an isocyanate index of 104 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 5.0%, which was made from 1,000 g of PTMG-2 and 470 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to produce a test piece and a product. Example 5 has a density of 0.50 g / cm 3 The tensile strength was 4.9 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0061] In Example 6, a polyurethane elastomer foam composition with an isocyanate index of 102 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 1000 g of PTMG-3 and 270 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to produce a test piece and a product. Example 6 has a density of 0.50 g / cm 3 The tensile strength was 4.4 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0062] In Example 7, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 500 g of PTMG-1, 500 g of PCL, and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. 330 g and 76 g were injected into a test piece mold and a product mold, respectively, to prepare a test piece and a product. Example 7 has a density of 0.50 g / cm 3 The tensile strength was 4.0 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0063] In Example 8, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 1000 g of PTMG-1 and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. 211 g and 49 g were injected into the test piece mold and the product mold, respectively, to produce a test piece and a product. Example 8 has a density of 0.32 g / cm 3The tensile strength was 3.1 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0064] In Example 9, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 1000 g of PTMG-1 and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. 271 g and 62 g were injected into the test piece mold and the product mold, respectively, to produce a test piece and a product. Example 9 has a density of 0.41 g / cm 3 The tensile strength was 3.8 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0065] In Example 10, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 1,000 g of PTMG-1 and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 403 g and 93 g, respectively, to prepare a test piece and a product. Example 10 has a density of 0.61 g / cm 3 The tensile strength was 4.8 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0066] In Example 11, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 100 g of PTMG-1, 900 g of PCL, and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. The amounts injected into the test piece mold and the product mold were 330 g and 76 g, respectively, to prepare a test piece and a product. Example 11 has a density of 0.50 g / cm 3 The tensile strength was 3.8 MPa, the tensile strength was rated as "good", and the durability test was performed 100,000 times without any cracks, the durability was rated as "good", and the overall judging was "good".
[0067] In Comparative Example 1, a polyurethane elastomer foam composition with an isocyanate index of 103 was prepared from 100 g of a urethane prepolymer having an isocyanate group at its terminal and an NCO% (theoretical value) of 4.9%, which was made from 1000 g of ES polyol and 320 g of 4,4'-diphenylmethane diisocyanate, and 3.1 g of foaming liquid. 330 g and 76 g were injected into a test piece mold and a product mold, respectively, to produce a test piece and a product. The comparative example has a density of 0.50 g / cm 3 The tensile strength was 2.9 MPa, so the tensile strength was rated as ``X'', and in the durability cycle test, a crack occurred after 75,000 cycles, so the durability was rated as ``X'', and the overall verdict was ``X''.
[0068] As described above, each of the examples has high mechanical strength (tensile strength) and excellent durability when subjected to repeated heavy loads. Furthermore, since the manufacture of each of the examples does not require complex reaction control, it is possible to easily manufacture a bound stopper having high mechanical strength and improved durability when subjected to repeated heavy loads. [Explanation of symbols]
[0069] 10 Bound Stopper 30 Mold 31 Lower mold 33 Medium 35 Upper type
Claims
1. A bound stopper made of polyurethane elastomer foam that is attached to a piston rod of a shock absorber for a vehicle, The polyurethane elastomer foam is obtained from a polyurethane elastomer foam composition including at least an isocyanate component and a foaming agent. The bound stopper is characterized in that the isocyanate component is a urethane prepolymer having an isocyanate group at its end, obtained from a polyol component containing polytetramethylene ether glycol and diphenylmethane diisocyanate (excluding those using polyrotaxanes containing cyclic molecules having active hydrogen groups as constituents).
2. 2. The bound stopper according to claim 1, wherein the polyol component includes the polytetramethylene ether glycol and polycaprolactone diol.
3. Density: 0.3 to 0.7 g / cm 3 3. The bound stopper according to claim 1, wherein the bound stopper has a tensile strength of 3.0 MPa or more.
4. A method for manufacturing a bound stopper made of polyurethane elastomer foam and attached to a piston rod of a shock absorber for a vehicle, comprising the steps of: A method for producing a bound stopper, comprising: injecting a composition for a polyurethane elastomer foam, the composition comprising: a urethane prepolymer having an isocyanate group at its terminal, obtained from a polyol component containing polytetramethylene ether glycol and diphenylmethane diisocyanate (excluding those using a polyrotaxane containing a cyclic molecule having an active hydrogen group as a constituent); and a foaming agent; into a mold and foaming the composition to form a bound stopper made of the polyurethane elastomer foam.
5. The method for manufacturing a bound stopper according to claim 4, wherein the polyol component contains the polytetramethylene ether glycol and polycaprolactone diol.
Citation Information
Patent Citations
Bumper spring made of urethane
JP2004293697A
Aqueous mold release agent, and method for production of flexible or semi-rigid polyurethane foam molded article using the agent
JP2015116801A
Urethane-based bumper spring and manufacturing method thereof
JP2015183832A
Fiber, fabric, nonwoven fabric, film, sheet and clothing
JP2016020549A
Bound stopper and manufacturing method thereof
JP2019070423A