Optical film, optical laminate and image display device

JP7573609B2Active Publication Date: 2024-10-25FUJIFILM CORP

Patent Information

Application Number
JP2022528864
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2021-05-27
Filing Date
2021-06-02
Publication Date
2024-10-25
Estimated Expiration
2041-06-02

AI Technical Summary

Benefits of technology

【0009】 本発明によれば、透過率中心軸方向から見た場合の色味、および、透過率中心軸から傾いた方向から見た場合の色味を、ともにニュートラルにすることができる光学フィルム、ならびにこれを用いた光学積層体および画像表示装置を提供することができる。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007573609000001
    Figure 0007573609000001
  • Figure 0007573609000002
    Figure 0007573609000002
  • Figure 0007573609000003
    Figure 0007573609000003
Patent Text Reader

Abstract

The present invention addresses the problem of providing an optical film, and providing an optical laminate and an image display device that use the same, the optical film making it possible to make both the color thereof when viewed from the direction of a transmittance center axis and the color thereof when viewed from a direction inclined from the transmittance center axis neutral. This optical film comprises a light absorption anisotropic layer in which an angle θ formed by the transmittance center axis and the normal direction of a layer surface is 0-45°, and a color adjustment layer including at least one type of organic dye component.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to an optical film, an optical laminate, and an image display device. [Background technology]

[0002] A technique for using a light absorbing anisotropic layer having an absorption axis in the thickness direction in combination with a liquid crystal display device to prevent people from looking into the display device or to control the viewing angle is known. For example, Patent Document 1 proposes a polarizing element related to a viewing angle control system using a film containing a dichroic material and having an angle of 0° to 45° between the absorption axis and the normal line of the film surface. [Prior art documents] [Patent documents]

[0003] [Patent Document 1] JP 2009-145776 A Summary of the Invention [Problem to be solved by the invention]

[0004] The present inventors have investigated optical films having an optically absorptive anisotropic layer containing a dichroic material and have found that the optical film has excellent processability since it can be thinned. However, they have also found that it is difficult to control the color of the optical film to be neutral both when viewed from the direction of the central axis of transmittance of the optically absorptive anisotropic layer and when viewed from a direction tilted from the central axis of transmittance because the orientation of the dichroic material in the visible range is not uniform.

[0005] Therefore, an object of the present invention is to provide an optical film that can neutralize both the color when viewed from the direction of the central axis of transmittance and the color when viewed from a direction tilted from the central axis of transmittance, as well as an optical laminate and an image display device that use the same. [Means for solving the problem]

[0006] As a result of intensive research aimed at solving the above-mentioned problems, the inventors have discovered that an optical film having a predetermined light absorption anisotropic layer and a color-adjusting layer containing at least one organic dye compound can neutralize both the color when viewed from the direction of the central axis of transmittance and the color when viewed from a direction tilted from the central axis of transmittance, and have thus completed the present invention.

[0007] That is, it has been found that the above object can be achieved by the following configuration.

[0008] [1] An optical film comprising a light absorbing anisotropic layer in which the angle θ between the transmittance central axis and the normal direction to the layer surface is 0 to 45°, and a color adjusting layer containing at least one organic dye compound. [2] The optical film according to [1], wherein the light absorption anisotropic layer contains a liquid crystalline compound and at least one dichroic dye compound. [3] The optical film according to [1] or [2], wherein the optically absorptive anisotropic layer satisfies both of the following formulas (1) and (2). [4] The optical film according to [2] or [3], wherein at least one of the dichroic dye compounds contained in the light absorption anisotropic layer is represented by the following formula (3). [5] The optical film according to any one of [1] to [4], wherein the color-adjusting layer satisfies any one of requirements 1 to 3 described below. [6] The optical film according to any one of [1] to [5], wherein the organic colorant compound contained in the color-adjusting layer has an absorption peak wavelength of 500 to 650 nm. [7] The optical film according to any one of [1] to [6], wherein the organic colorant compound contained in the color-adjusting layer has at least one of a benzene ring and a heterocyclic ring structure in the molecule. [8] The optical film according to any one of [1] to [7], wherein the organic colorant compound contained in the color-adjusting layer has an anthraquinone structure. [9] The optical film according to any one of [1] to [8], which satisfies the formula (7) described below.

[10] The optical film according to any one of [1] to [9], which has a transmittance of 65% or more for light having a wavelength of 550 nm in a direction along the transmittance central axis.

[11] An optical laminate comprising the optical film according to any one of [1] to

[10] and a polarizer layer in which a dichroic material is oriented horizontally to the film surface.

[12] An optical laminate comprising the optical film according to any one of [1] to

[10] and a concave-convex layer having an arithmetic average roughness Ra of 35 to 125 nm.

[13] An image display device comprising the optical film according to any one of [1] to

[10] , or the optical laminate according to

[11] or

[12] . Effect of the Invention

[0009] According to the present invention, it is possible to provide an optical film that can neutralize both the color when viewed from the direction of the central axis of transmittance and the color when viewed from a direction tilted from the central axis of transmittance, as well as an optical laminate and an image display device using the same. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0010] The present invention will be described in detail below. The following description of the components may be based on representative embodiments of the present invention, but the present invention is not limited to such embodiments. In this specification, a numerical range expressed using "to" means a range that includes the numerical values ​​before and after "to" as the lower and upper limits. In this specification, parallel and orthogonal do not mean parallel and orthogonal in the strict sense, but mean a range of parallel ±5° and orthogonal ±5°, respectively. In this specification, unless otherwise specified, visible light means electromagnetic waves with a wavelength of 380 to 800 nm. In this specification, room temperature means 20 to 28° C. unless otherwise specified.

[0011] In this specification, the liquid crystal composition and liquid crystal compound conceptually include those that no longer exhibit liquid crystallinity due to curing or the like.

[0012] In the present specification, each component may be used alone or in combination of two or more substances corresponding to each component. When two or more substances are used in combination for each component, the content of the component refers to the total content of the substances used in combination, unless otherwise specified. In this specification, "(meth)acrylate" is a notation representing "acrylate" or "methacrylate", "(meth)acryl" is a notation representing "acryl" or "methacryl", and "(meth)acryloyl" is a notation representing "acryloyl" or "methacryloyl".

[0013] The substituent W in this specification will be explained. Examples of the substituent W include an alkyl group (preferably an alkyl group having 1 to 20 carbon atoms, more preferably an alkyl group having 1 to 12 carbon atoms, and particularly preferably an alkyl group having 1 to 8 carbon atoms, such as a methyl group, an ethyl group, an isopropyl group, a tert-butyl group, an n-octyl group, an n-decyl group, an n-hexadecyl group, a cyclopropyl group, a cyclopentyl group, and a cyclohexyl group), an alkenyl group (preferably an alkenyl group having 2 to 20 carbon atoms, more preferably an alkenyl group having 2 to 12 carbon atoms, and particularly preferably an alkenyl group having 2 to 8 carbon atoms, such as a vinyl group, an aryl group, a 2-butene group, and the like). Examples of the aryl group include a phenyl group, a 2-pentenyl group, and the like), an alkynyl group (preferably an alkynyl group having 2 to 20 carbon atoms, more preferably an alkynyl group having 2 to 12 carbon atoms, and particularly preferably an alkynyl group having 2 to 8 carbon atoms, and examples of the aryl group include a propargyl group and a 3-pentenyl group), an aryl group (preferably an aryl group having 6 to 30 carbon atoms, more preferably an aryl group having 6 to 20 carbon atoms, and particularly preferably an aryl group having 6 to 12 carbon atoms, and examples of the aryl group include a phenyl group, a 2,6-diethylphenyl group, a 3,5-ditrifluoromethylphenyl group, a styryl group, a naphthyl group, and a biphenyl group). a substituted or unsubstituted amino group (preferably having 0 to 20 carbon atoms, more preferably having 0 to 10 carbon atoms, and particularly preferably having 0 to 6 carbon atoms; examples of which include an unsubstituted amino group, a methylamino group, a dimethylamino group, a diethylamino group, and an anilino group), an alkoxy group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 15 carbon atoms, and examples of which include a methoxy group, an ethoxy group, and a butoxy group), an oxycarbonyl group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 15 carbon atoms, and particularly preferably having 2 to 10 carbon atoms, for example, a methoxycarbonyl group, an ethoxycarbonyl group, a phenoxycarbonyl group, etc.), an acyloxy group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms, for example, an acetoxy group, a benzoyloxy group, an acryloyl group, and a methacryloyl group, etc.), an acylamino group (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms, for example, an acetylamino group, a benzoylamino group, etc.),Alkoxycarbonylamino groups (preferably having 2 to 20 carbon atoms, more preferably having 2 to 10 carbon atoms, and particularly preferably having 2 to 6 carbon atoms; for example, methoxycarbonylamino groups, etc.), aryloxycarbonylamino groups (preferably having 7 to 20 carbon atoms, more preferably having 7 to 16 carbon atoms, and particularly preferably having 7 to 12 carbon atoms; for example, phenyloxycarbonylamino groups, etc.), sulfonylamino groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; for example, methanesulfonylamino groups, and a benzenesulfonylamino group), a sulfamoyl group (preferably having 0 to 20 carbon atoms, more preferably having 0 to 10 carbon atoms, and particularly preferably having 0 to 6 carbon atoms, such as a sulfamoyl group, a methylsulfamoyl group, a dimethylsulfamoyl group, and a phenylsulfamoyl group), a carbamoyl group (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms, such as an unsubstituted carbamoyl group, a methylcarbamoyl group, a diethylcarbamoyl group, and a phenylcarbamoyl group). and the like), alkylthio groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples of such groups include a methylthio group and an ethylthio group), arylthio groups (preferably having 6 to 20 carbon atoms, more preferably having 6 to 16 carbon atoms, and particularly preferably having 6 to 12 carbon atoms; examples of such groups include a phenylthio group), sulfonyl groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples of such groups include a mesyl group and a tosyl group), sulfinyl groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples thereof include a methanesulfinyl group and a benzenesulfinyl group), ureido groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples thereof include an unsubstituted ureido group, a methylureido group, and a phenylureido group), phosphoramido groups (preferably having 1 to 20 carbon atoms, more preferably having 1 to 10 carbon atoms, and particularly preferably having 1 to 6 carbon atoms; examples thereof include a diethyl phosphoramido group,and phenylphosphoramide groups, etc.), a hydroxy group, a mercapto group, a halogen atom (for example, a fluorine atom, a chlorine atom, a bromine atom, and an iodine atom), a cyano group, a nitro group, a hydroxamic acid group, a sulfino group, a hydrazino group, an imino group, an azo group, a heterocyclic group (preferably a heterocyclic group having 1 to 30 carbon atoms, more preferably a heterocyclic group having 1 to 12 carbon atoms, for example, a heterocyclic group having a heteroatom such as a nitrogen atom, an oxygen atom, or a sulfur atom, for example, an epoxy group, an oxetanyl group, imidazolyl group, pyridyl group, quinolyl group, furyl group, piperidyl group, morpholino group, maleimide group, benzoxazolyl group, benzimidazolyl group, benzthiazolyl group, etc.), silyl group (preferably a silyl group having 3 to 40 carbon atoms, more preferably a silyl group having 3 to 30 carbon atoms, particularly preferably a silyl group having 3 to 24 carbon atoms, for example, a trimethylsilyl group, a triphenylsilyl group, etc.), carboxy group, sulfonic acid group, phosphate group, etc., are included.

[0014] The optical film, the optical laminate, and the image display device will be described below. In the following, a state in which "the color when viewed from the direction of the central axis of transmittance and the color when viewed from a direction tilted from the central axis of transmittance are both neutral" is also referred to as "excellent wide-angle color suppression ability."

[0015] <Optical film> The optical film of the present invention comprises a light absorptive anisotropic layer in which the angle θ between the transmittance central axis and the normal direction to the layer surface is 0 to 45°, and a color-adjusting layer containing at least one organic dye compound. Here, the mechanism by which the optical film of the present invention can neutralize both the color when viewed from the direction of the central axis of transmittance and the color when viewed from a direction tilted from the central axis of transmittance is not necessarily clear, but the inventors speculate as follows. In the optically absorptive anisotropic layer of the optical film, the color tone when viewed from both of the above-mentioned directions is not neutral. It is presumed that the color tone is caused by the orientation of the substance contained in the optically absorptive anisotropic layer. Here, it is considered that the color tone can be reduced by the color tone adjusting layer containing at least one organic dye compound, and the color tone when viewed from both of the above-mentioned directions can be made neutral.

[0016] The optical film of the present invention may have a transparent substrate film, an alignment film, a barrier layer, an adhesive layer and an adhesion layer in addition to the light absorption anisotropic layer and the color adjusting layer. The light absorption anisotropic layer, the color adjusting layer, the transparent substrate film, the alignment film, and the barrier layer will be described in detail below. The method for producing the optical film will be described in detail below. The pressure-sensitive adhesive layer and the adhesive layer will be described in the method for producing the optical film.

[0017] [Light-absorbing anisotropic layer] In the light absorptive anisotropic layer of the optical film of the present invention, the angle between the transmittance central axis and the normal direction to the layer surface is 0° to 45°. Here, the transmittance central axis means the direction showing the highest transmittance when the transmittance is measured by changing the tilt angle (polar angle) and tilt direction (azimuth angle) with respect to the normal direction of the optically absorptive anisotropic layer surface. Specifically, the Mueller matrix at a wavelength of 550 nm is actually measured using AxoScan OPMF-1 (manufactured by Optoscience). More specifically, in the measurement, the azimuth angle at which the transmittance central axis is tilted is first found, and then, in a plane including the normal direction of the optically absorptive anisotropic layer along that azimuth angle (a plane including the transmittance central axis and perpendicular to the layer surface), the polar angle, which is the angle with respect to the normal direction of the optically absorptive anisotropic layer surface, is changed from 0 to 90° in 5° increments to measure the Mueller matrix at a wavelength of 550 nm, and the transmittance of the optically absorptive anisotropic layer is derived. As a result, the direction with the highest transmittance is taken as the transmittance central axis. By adjusting the angles between the central axis of transmittance of the light absorbing anisotropic layer and the normal direction to the layer surface, the viewing angle center of the liquid crystal display device can be shifted not only up, down, left, right, but also in an oblique direction from the front. In order to control the central axis of the transmission axis of the light-absorption anisotropic layer, it is preferable to align the dichroic substance, and it is more preferable to align the dichroic substance by utilizing the orientation of the liquid crystal compound. Therefore, it is preferable that the light-absorption anisotropic layer contains a liquid crystal compound and a dichroic substance. One example is a light absorbing anisotropic layer in which at least one organic dichroic dye is oriented perpendicular to the in-plane direction. The optically absorptive anisotropic layer is preferably produced using a composition for forming an optically absorptive anisotropic layer, which will be described later. The composition for forming an optically absorptive anisotropic layer preferably contains a liquid crystal compound and a dichroic substance. The composition for forming the optically absorptive anisotropic layer and the forming method using the same will be described in detail later.

[0018] (liquid crystal compound) The optically absorptive anisotropic layer of the optical film of the present invention preferably contains a liquid crystalline compound. By containing a liquid crystalline compound when forming the optically absorptive anisotropic layer, the degree of orientation of the dichroic material in the optically absorptive anisotropic layer can be increased while suppressing precipitation of the dichroic material. The liquid crystal compound refers to a liquid crystal compound that does not exhibit dichroism at least for visible light. As the liquid crystal compound, either a low molecular weight liquid crystal compound or a polymeric liquid crystal compound can be used, and it is also preferable to use both in combination. Here, the term "low molecular weight liquid crystal compound" refers to a liquid crystal compound that does not have a repeating unit in its chemical structure. Also, the term "polymeric liquid crystal compound" refers to a liquid crystal compound that has a repeating unit in its chemical structure.

[0019] -Low molecular liquid crystal compounds- Examples of the low molecular weight liquid crystal compound include the liquid crystal compounds described in JP-A-2013-228706.

[0020] -Polymer liquid crystal compound- Examples of the polymeric liquid crystal compound include the thermotropic liquid crystal polymer described in JP 2011-237513 A. In addition, the polymeric liquid crystal compound preferably has a repeating unit having a crosslinkable group at the end, in terms of the strength (particularly bending resistance) of the light absorption anisotropic film being excellent. Examples of the crosslinkable group include the polymerizable groups described in paragraphs

[0040] to

[0050] of JP 2010-244038 A. Among them, in terms of improving reactivity and synthesis suitability, acryloyl group, methacryloyl group, epoxy group, oxetanyl group, and styryl group are preferred, and acryloyl group and methacryloyl group are more preferred.

[0021] In the case where the light absorption anisotropic layer in the present invention contains a polymeric liquid crystal compound, Preferably, the liquid crystal layer forms a nematic liquid crystal phase. The temperature range in which the liquid crystal exhibits a nematic liquid crystal phase is preferably from room temperature to 450° C., and from the viewpoint of ease of handling and / or suitability for production, it is preferably 50 to 400° C.

[0022] The content of the liquid crystal compound is preferably 25 to 2000 parts by mass, more preferably 100 to 1300 parts by mass, and even more preferably 200 to 900 parts by mass, relative to 100 parts by mass of the dichroic substance. When the content of the liquid crystal compound is within the above range, the degree of orientation of the dichroic substance in the light absorptive anisotropic layer is further improved. The liquid crystal compound may be contained alone or in combination with two or more kinds. When two or more kinds of liquid crystal compounds are contained, the content of the liquid crystal compounds means the total content of the liquid crystal compounds.

[0023] The liquid crystalline compound is preferably a polymeric liquid crystalline compound containing a repeating unit represented by the following formula (1L) (hereinafter also referred to as "repeating unit (1L)"), in that the degree of orientation of the dichroic substance in the light absorption anisotropic layer is superior.

[0024] [ka]

[0025] In the above formula (1L), P1 represents the main chain of the repeating unit, L1 represents a single bond or a divalent linking group, SP1 represents a spacer group, M1 represents a mesogenic group, and T1 represents a terminal group.

[0026] Specific examples of the main chain of the repeating unit represented by P1 include groups represented by the following formulae (P1-A) to (P1-D). Among these, the group represented by the following formula (P1-A) is preferred from the viewpoints of the variety of monomers that serve as raw materials and ease of handling.

[0027] [ka]

[0028] In formulae (P1-A) to (P1-D), "*" represents the bonding position with L1 in formula (1L). 1 , R 2 , R 3 and R 4 each independently represents a hydrogen atom, a halogen atom, an alkyl group having 1 to 10 carbon atoms, or an alkoxy group having 1 to 10 carbon atoms. The alkyl group may be a straight-chain or branched alkyl group, or an alkyl group having a cyclic structure (cycloalkyl group). The alkyl group preferably has 1 to 5 carbon atoms. The group represented by formula (P1-A) is preferably one unit of a partial structure of a poly(meth)acrylic acid ester obtained by polymerization of a (meth)acrylic acid ester. The group represented by formula (P1-B) is preferably an ethylene glycol unit formed by ring-opening polymerization of the epoxy group of a compound having an epoxy group. The group represented by the formula (P1-C) is preferably a propylene glycol unit formed by ring-opening polymerization of the oxetane group of a compound having an oxetane group. The group represented by formula (P1-D) is preferably a siloxane unit of a polysiloxane obtained by condensation polymerization of a compound having at least one of an alkoxysilyl group and a silanol group. Here, the compound having at least one of an alkoxysilyl group and a silanol group is preferably a compound represented by the formula SiR 4 (OR 5 )2-, wherein R 4 is R in (P1-D) 4 Synonymous with R 5 each independently represents a hydrogen atom or an alkyl group having 1 to 10 carbon atoms.

[0029] L1 is a single bond or a divalent linking group. The divalent linking group represented by L1 is -C(O)O-, -OC(O)-, -O-, -S-, or -C(O)NR 3 -, -NR 3 C(O)-, -SO2-, and -NR 3 R 4 In the formula, R 3 and R 4 each independently represents a hydrogen atom or an alkyl group having 1 to 6 carbon atoms which may have a substituent W. When P1 is a group represented by formula (P1-A), L1 is preferably a group represented by -C(O)O- in that the degree of orientation of the dichroic material in the light absorption anisotropic layer is superior. When P1 is a group represented by any of the formulae (P1-B) to (P1-D), L1 is preferably a single bond in that the degree of orientation of the dichroic material in the light absorption anisotropic layer is superior.

[0030] The spacer group represented by SP1 preferably contains at least one structure selected from the group consisting of an oxyethylene structure, an oxypropylene structure, a polysiloxane structure, and a fluorinated alkylene structure, in terms of ease of expressing liquid crystallinity and / or availability of raw materials. Here, when SP1 represents an oxyethylene structure, *-(CH2-CH2O) n1A group represented by -* is preferred. In the formula, n1 represents an integer of 1 to 20, and * represents the bonding position with L1 or M1 in the above formula (1L). n1 is preferably an integer of 2 to 10, more preferably an integer of 2 to 4, and most preferably 3, in that the degree of orientation of the dichroic material in the light absorptive anisotropic layer is superior. In addition, when SP1 represents an oxypropylene structure, the degree of orientation of the dichroic material in the light absorption anisotropic layer is more excellent, and therefore, *-(CH(CH3)-CH2O) n2 A group represented by -* is preferred, in which n2 represents an integer of 1 to 3, and * represents the bonding position to L1 or M1. In addition, when SP1 represents a polysiloxane structure, the degree of orientation of the dichroic material in the light absorption anisotropic layer is more excellent, and therefore, *-(Si(CH3)2-O) n3 A group represented by -* is preferred, in which n3 represents an integer of 6 to 10, and * represents the bonding position to L1 or M1. In addition, the fluorinated alkylene structure represented by SP1 has a better degree of orientation of the dichroic material in the light absorption anisotropic layer, and therefore, *-(CF2-CF2) n4 A group represented by -* is preferred, in which n4 represents an integer of 6 to 10, and * represents the bonding position to L1 or M1.

[0031] The mesogenic group represented by M1 is a group that represents the main skeleton of the liquid crystal molecule that contributes to the formation of liquid crystal. The liquid crystal molecule exhibits liquid crystallinity, which is an intermediate state (mesophase) between the crystalline state and the isotropic liquid state. There are no particular limitations on the mesogenic group, and reference can be made, for example, to the description of "Flussige Kristalle in Tabellen II" (VEB Deutsche Verlag fur Grundstoff Industrie, Leipzig, published in 1984), particularly pages 7 to 16, and the description of "Liquid Crystal Handbook" edited by the Liquid Crystal Handbook Editorial Committee (Maruzen, published in 2000), particularly chapter 3. As the mesogenic group, for example, at least one group having a cyclic structure selected from the group consisting of an aromatic hydrocarbon group, a heterocyclic group, and an alicyclic group is preferable. The mesogenic group preferably has an aromatic hydrocarbon group, more preferably has 2 to 4 aromatic hydrocarbon groups, and even more preferably has 3 aromatic hydrocarbon groups, in order to achieve a better degree of orientation of the dichroic substance in the light absorption anisotropic layer.

[0032] As the mesogenic group, from the viewpoints of expression of liquid crystallinity, adjustment of the liquid crystal phase transition temperature, availability of raw materials and suitability for synthesis, as well as a superior degree of orientation of the dichroic substance in the light absorption anisotropic layer, a group represented by the following formula (M1-A) or the following formula (M1-B) is preferred, and a group represented by formula (M1-B) is more preferred.

[0033] [ka]

[0034] In formula (M1-A), A1 is a divalent group selected from the group consisting of aromatic hydrocarbon groups, heterocyclic groups, and alicyclic groups. These groups may be substituted with an alkyl group, a fluorinated alkyl group, an alkoxy group, or a substituent W. The divalent group represented by A1 is preferably a 4- to 6-membered ring. In addition, the divalent group represented by A1 may be a monocyclic ring or a condensed ring. * indicates the binding position to SP1 or T1.

[0035] Examples of the divalent aromatic hydrocarbon group represented by A1 include a phenylene group, a naphthylene group, a fluorene-diyl group, an anthracene-diyl group, and a tetracene-diyl group. In terms of the diversity of mesogenic skeleton designs and / or the availability of raw materials, a phenylene group or a naphthylene group is preferred, and a phenylene group is more preferred.

[0036] The divalent heterocyclic group represented by A1 may be either aromatic or non-aromatic, but is preferably a divalent aromatic heterocyclic group in that it further improves the degree of orientation of the dichroic material in the light absorption anisotropic layer. The atoms other than carbon constituting the divalent aromatic heterocyclic group include a nitrogen atom, a sulfur atom, and an oxygen atom. When the aromatic heterocyclic group has a plurality of atoms other than carbon constituting the ring, these atoms may be the same or different. Specific examples of divalent aromatic heterocyclic groups include, for example, a pyridylene group (pyridine-diyl group), a pyridazine-diyl group, an imidazole-diyl group, a thienylene group (thiophene-diyl group), a quinolylene group (quinoline-diyl group), an isoquinolylene group (isoquinoline-diyl group), an oxazole-diyl group, a thiazole-diyl group, an oxadiazole-diyl group, a benzothiazole-diyl group, a benzothiadiazole-diyl group, a phthalimido-diyl group, a thienothiazole-diyl group, a thiazolothiazole-diyl group, a thienothiophene-diyl group, and a thienoxazole-diyl group.

[0037] Specific examples of the divalent alicyclic group represented by A1 include a cyclopentylene group and a cyclohexylene group.

[0038] In formula (M1-A), a1 represents an integer of 1 to 10. When a1 is 2 or more, multiple A1 may be the same or different.

[0039] In formula (M1-B), A2 and A3 are each independently a divalent group selected from the group consisting of an aromatic hydrocarbon group, a heterocyclic group, and an alicyclic group. Specific examples and preferred embodiments of A2 and A3 are the same as those of A1 in formula (M1-A), and therefore the description thereof is omitted. In formula (M1-B), a2 represents an integer of 1 to 10, and when a2 is 2 or more, multiple A2 may be the same or different, multiple A3 may be the same or different, and multiple LA1 may be the same or different. a2 is preferably an integer of 2 or more, and more preferably 2, in that the degree of orientation of the dichroic material in the light absorptive anisotropic layer is more excellent. In formula (M1-B), when a2 is 1, LA1 is a divalent linking group. When a2 is 2 or more, each of the multiple LA1 is independently a single bond or a divalent linking group, and at least one of the multiple LA1 is a divalent linking group. When a2 is 2, it is preferable that one of the two LA1 is a divalent linking group and the other is a single bond, in terms of a better degree of orientation of the dichroic material in the light absorption anisotropic layer.

[0040] In formula (M1-B), the divalent linking group represented by LA1 is -O-, -(CH2) g -, -(CF2) g -, -Si(CH3)2-, -(Si(CH3)2O) g -, -(OSi(CH3)2) g -(g represents an integer from 1 to 10.), -N(Z)-, -C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z)2-C (Z')2-, -C(O)-, -OC(O)-, -C(O)O-, -OC(O)O-, -N(Z)C(O)-, -C(O)N(Z)-, -C (Z)=C(Z')-C(O)O-, -OC(O)-C(Z)=C(Z')-, -C(Z)=N-, -N=C(Z)-, -C(Z)=C(Z ')-C(O)N(Z”)-, -N(Z”)-C(O)-C(Z)=C(Z')-, -C(Z)=C(Z')-C(O)-S-, -SC(O) Examples of such groups include -C(Z)=C(Z')-, -C(Z)=NN=C(Z')- (Z, Z', and Z" independently represent a hydrogen atom, an alkyl group having 1 to 4 carbon atoms, a cycloalkyl group, an aryl group, a cyano group, or a halogen atom), -C≡C-, -N=N-, -S-, -S(O)-, -S(O)(O)-, -(O)S(O)O-, -O(O)S(O)O-, -SC(O)-, and -C(O)S-. Of these, -C(O)O- is preferred because it provides a superior degree of orientation of the dichroic material in the light absorption anisotropic layer. LA1 may be a group consisting of a combination of two or more of these groups.

[0041] Specific examples of M1 include the following structures: In the following specific examples, "Ac" represents an acetyl group.

[0042] [ka]

[0043] [ka]

[0044] Examples of the terminal group represented by T1 include a hydrogen atom, a halogen atom, a cyano group, a nitro group, a hydroxy group, an alkyl group having 1 to 10 carbon atoms, an alkoxy group having 1 to 10 carbon atoms, an alkylthio group having 1 to 10 carbon atoms, an alkoxycarbonyloxy group having 1 to 10 carbon atoms, an alkoxycarbonyl group having 1 to 10 carbon atoms (ROC(O)-: R is an alkyl group), an acyloxy group having 1 to 10 carbon atoms, an acylamino group having 1 to 10 carbon atoms, an alkoxycarbonylamino group having 1 to 10 carbon atoms, a sulfonylamino group having 1 to 10 carbon atoms, a sulfamoyl group having 1 to 10 carbon atoms, a carbamoyl group having 1 to 10 carbon atoms, a sulfinyl group having 1 to 10 carbon atoms, a ureido group having 1 to 10 carbon atoms, and a (meth)acryloyloxy group-containing group. Examples of the (meth)acryloyloxy group-containing group include a group represented by -LA (L represents a single bond or a linking group. Specific examples of the linking group are the same as those of L1 and SP1 described above. A represents a (meth)acryloyloxy group). T1 is preferably an alkoxy group having 1 to 10 carbon atoms, more preferably an alkoxy group having 1 to 5 carbon atoms, and even more preferably a methoxy group, in that the degree of orientation of the dichroic material in the light absorption anisotropic layer is superior. These terminal groups may be further substituted with these groups or the above-mentioned crosslinkable groups. The number of atoms in the main chain of T1 is preferably 1 to 20, more preferably 1 to 15, even more preferably 1 to 10, and particularly preferably 1 to 7, in terms of a better degree of orientation of the dichroic material in the light absorption anisotropic layer. When the number of atoms in the main chain of T1 is 20 or less, the degree of orientation of the dichroic material in the light absorption anisotropic layer is improved. Here, the "main chain" in T1 means the longest molecular chain bonded to M1, and hydrogen atoms are not counted in the number of atoms in the main chain of T1. For example, when T1 is an n-butyl group, the number of atoms in the main chain is 4, and when T1 is a sec-butyl group, the number of atoms in the main chain is 3.

[0045] The content of the repeating unit (1L) is preferably 20 to 100% by mass relative to 100% by mass of all repeating units contained in the polymeric liquid crystal compound, in that the degree of orientation of the dichroic material in the light absorption anisotropic layer is superior. In the present invention, the content of each repeating unit contained in the polymeric liquid crystal compound is calculated based on the charged amount (mass) of each monomer used to obtain each repeating unit. The repeating unit (1L) may be contained in the polymer liquid crystal compound in one kind or in two or more kinds. In particular, it is preferable that the polymer liquid crystal compound contains two kinds of repeating units (1L) in order to obtain a better degree of orientation of the dichroic material in the light absorption anisotropic layer.

[0046] When the polymer liquid crystal compound contains two types of repeating units (1L), it is preferable that the terminal group represented by T1 in one (repeating unit A) is an alkoxy group and the terminal group represented by T1 in the other (repeating unit B) is a group other than an alkoxy group, in order to obtain a better degree of orientation of the dichroic material in the light absorption anisotropic layer. The terminal group represented by T1 in the above repeating unit B is preferably an alkoxycarbonyl group, a cyano group, or a group containing a (meth)acryloyloxy group, from the viewpoint of achieving a better degree of orientation of the dichroic substance in the light absorption anisotropic layer, and more preferably an alkoxycarbonyl group or a cyano group. The ratio (A / B) of the content of the repeating unit A in the polymer liquid crystalline compound to the content of the repeating unit B in the polymer liquid crystalline compound is preferably 50 / 50 to 95 / 5, more preferably 60 / 40 to 93 / 7, and even more preferably 70 / 30 to 90 / 10, in order to achieve a better degree of orientation of the dichroic material in the light absorption anisotropic layer.

[0047] The polymeric liquid crystal compound may have a repeating unit having no mesogenic group in addition to the repeating unit (1L). An example of the repeating unit having no mesogenic group is a repeating unit in which M1 in formula (1L) is a single bond. When the polymer liquid crystal compound has a repeating unit that does not have a mesogenic group, the amount of the repeating unit is preferably more than 0% by mass and not more than 30% by mass, and more preferably more than 10% by mass and not more than 20% by mass, relative to 100% by mass of all repeating units contained in the polymer liquid crystal compound, in order to obtain a better degree of orientation of the dichroic material in the light absorption anisotropic layer.

[0048] -Weight average molecular weight- The weight average molecular weight (Mw) of the polymer liquid crystal compound is preferably 1,000 to 500,000, and more preferably 2,000 to 300,000, in order to provide a better degree of orientation of the dichroic material in the light absorption anisotropic layer. When the Mw of the polymer liquid crystal compound is within the above range, the polymer liquid crystal compound is easy to handle. In particular, from the viewpoint of suppressing cracks during application, the weight average molecular weight (Mw) of the polymeric liquid crystal compound is preferably 10,000 or more, and more preferably 10,000 to 300,000. In terms of the temperature latitude of the orientation degree, the weight average molecular weight (Mw) of the polymer liquid crystal compound is preferably less than 10,000, and more preferably 2,000 or more and less than 10,000. Here, the weight average molecular weight and number average molecular weight in the present invention are values ​​measured by gel permeation chromatography (GPC). Solvent (eluent): N-methylpyrrolidone ·Device name: TOSOH HLC-8220GPC Column: Three TOSOH TSKgel SuperAWM-H (6 mm x 15 cm) columns connected together Column temperature: 25℃ Sample concentration: 0.1% by mass ·Flow rate: 0.35mL / min Calibration curve: TOSOH TSK standard polystyrene Calibration curve using 7 samples with Mw = 2,800,000 to 1,050 (Mw / Mn = 1.03 to 1.06)

[0049] (dichroic substance) The light absorptive anisotropic layer of the present invention preferably contains a dichroic material. The dichroic material means a material that has different absorbance depending on the direction. The dichroic material is not particularly limited, and examples thereof include visible light absorbing materials (e.g., dichroic dye compounds and dichroic azo dye compounds), luminescent materials (e.g., fluorescent materials and phosphorescent materials), ultraviolet absorbing materials, infrared absorbing materials, nonlinear optical materials, carbon nanotubes, and inorganic materials (e.g., quantum rods), and conventionally known dichroic materials (dichroic dye compounds) can be used.

[0050] Among these, dichroic dye compounds are preferred, and dichroic azo dye compounds are more preferred. The dichroic azo dye compound is not particularly limited, and any conventionally known dichroic azo dye compound can be used, but the compounds described below are preferably used. The dichroic azo dye compound will now be described.

[0051] The dichroic azo dye compound may or may not exhibit liquid crystallinity. When the dichroic azo dye compound exhibits liquid crystallinity, it may exhibit either nematic or smectic properties. The temperature range in which the liquid crystal phase is exhibited is preferably from room temperature to 300° C., and more preferably from 50 to 200° C. in terms of handling and manufacturing suitability.

[0052] In terms of adjusting color, the light absorption anisotropic layer preferably contains at least one dye compound having a maximum absorption wavelength in the wavelength range of 560 to 700 nm (hereinafter also referred to as a "first dichroic azo dye compound") and at least one dye compound having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm (hereinafter also referred to as a "second dichroic azo dye compound"). Specifically, it is more preferable for the light absorption anisotropic layer to contain at least a dichroic azo dye compound represented by formula (3) described below and a dichroic azo dye compound represented by formula (4) described below.

[0053] In addition, three or more dichroic azo dye compounds may be used in combination. For example, in order to make the light absorption anisotropic layer closer to black, it is preferable to use a first dichroic azo dye compound, a second dichroic azo dye compound, and at least one dye compound having a maximum absorption wavelength in the wavelength range of 380 nm or more and less than 455 nm (hereinafter also referred to as a "third dichroic azo dye compound") in combination.

[0054] In order to improve pressure resistance, the dichroic azo dye compound preferably has a crosslinkable group. Examples of the crosslinkable group include a (meth)acryloyl group, an epoxy group, an oxetanyl group, and a styryl group, and among these, a (meth)acryloyl group is preferable.

[0055] -First dichroic azo dye compound- As described above, the first dichroic azo dye compound is a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 to 700 nm. The first dichroic azo dye compound is preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 to 700 nm, and from the viewpoint of adjusting the color of the polarizer, is more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 to 650 nm, and is even more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 560 to 640 nm. The maximum absorption wavelength (nm) of the dichroic azo dye compound in this specification is determined from an ultraviolet-visible light spectrum in the wavelength range of 380 to 800 nm measured with a spectrophotometer using a solution in which the dichroic azo dye compound is dissolved in a good solvent. The first dichroic azo dye compound is preferably a compound having a chromophore and a side chain bonded to an end of the chromophore. Specific examples of the chromophore include an aromatic ring group (e.g., an aromatic hydrocarbon group, an aromatic heterocyclic group), an azo group, etc., and a structure having both an aromatic ring group and an azo group is preferred, and a bisazo structure having an aromatic heterocyclic group (preferably a thienothiazole group) and two azo groups is more preferred. The side chain is not particularly limited, and may be L of formula (3) described later. 3 , R 2 or L 4 Examples of the group include a group represented by the following formula:

[0056] The first dichroic azo dye compound is preferably a compound represented by the following formula (3), in that the degree of orientation of the dichroic azo dye compound in the light absorption anisotropic layer to be formed is further improved.

[0057] [ka]

[0058] In formula (3), A 4 represents a divalent aromatic group which may have a substituent. In formula (3), L 3 and L 4 each independently represents a substituent. In formula (3), E represents any one of a nitrogen atom, an oxygen atom, and a sulfur atom. In formula (3), R 1 represents a hydrogen atom, a halogen atom, an alkyl group which may have a substituent, or an alkoxy group which may have a substituent. In formula (3), R 2 represents a hydrogen atom or an alkyl group which may have a substituent. In formula (3), R 3represents a hydrogen atom or a substituent. In formula (3), n represents 0 or 1. However, when E is a nitrogen atom, n is 1, and when E is an oxygen atom or a sulfur atom, n is 0. The above-mentioned substituent is preferably the substituent W.

[0059] In formula (3), A 4 The "divalent aromatic group which may have a substituent" represented by the formula (I) will be explained below. Examples of the substituent include the substituent group G described in paragraphs

[0237] to

[0240] of JP2011-237513A. Among them, preferred examples include a halogen atom, an alkyl group, an alkoxy group, an alkoxycarbonyl group (e.g., methoxycarbonyl, ethoxycarbonyl, etc.), an aryloxycarbonyl group (e.g., phenoxycarbonyl, 4-methylphenoxycarbonyl, 4-methoxyphenylcarbonyl, etc.), etc., more preferred examples are alkyl groups, and even more preferred examples are alkyl groups having 1 to 5 carbon atoms. On the other hand, examples of the divalent aromatic group include a divalent aromatic hydrocarbon group and a divalent aromatic heterocyclic group. Examples of the divalent aromatic hydrocarbon group include arylene groups having 6 to 12 carbon atoms, specifically, phenylene groups, cumenylene groups, mesitylene groups, tolylene groups, xylylene groups, etc. Among these, the phenylene group is preferable.

[0060] In formula (3), L 3 and L 4Examples of the substituent represented by include the substituent W. Among them, the substituent is preferably an alkyl group which may have a substituent, an alkenyl group which may have a substituent, an alkynyl group which may have a substituent, an aryl group which may have a substituent, an alkoxy group which may have a substituent, an oxycarbonyl group which may have a substituent, an acyloxy group which may have a substituent, an acylamino group which may have a substituent, an amino group which may have a substituent, an alkoxycarbonylamino group which may have a substituent, a sulfonylamino group which may have a substituent, a sulfamoyl group which may have a substituent, a carbamoyl group which may have a substituent, an alkylthio group which may have a substituent, a sulfonyl group which may have a substituent, an ureido group which may have a substituent, a nitro group, a hydroxy group, a cyano group, an imino group, an azo group, a halogen atom, or a heterocyclic group, and more preferably an alkyl group which may have a substituent, an alkenyl group which may have a substituent, an aryl group which may have a substituent, an alkoxy group which may have a substituent, an oxycarbonyl group which may have a substituent, an acyloxy group which may have a substituent, an amino group which may have a substituent, a nitro group, an imino group, or an azo group. L 3 and L 4 At least one of L 3 and L 4 It is more preferable that both of the above groups contain a crosslinkable group. Specific examples of the crosslinkable group include the polymerizable groups described in paragraphs

[0040] to

[0050] of JP2010-244038A. From the viewpoints of reactivity and synthetic suitability, an acryloyl group, a methacryloyl group, an epoxy group, an oxetanyl group, or a styryl group is preferable, and an acryloyl group or a methacryloyl group is more preferable.

[0061] In formula (3), E represents any one of a nitrogen atom, an oxygen atom, and a sulfur atom, and is preferably a nitrogen atom from the viewpoint of synthetic suitability.

[0062] In formula (3), R1 represents any one of a hydrogen atom, a halogen atom, an optionally substituted alkyl group, and an optionally substituted alkoxy group or a group thereof, and is preferably a hydrogen atom or an optionally substituted alkyl group. Examples of the substituent include a halogen atom. The alkyl group may be a linear, branched, or cyclic alkyl group having 1 to 8 carbon atoms. Of these, a linear alkyl group having 1 to 6 carbon atoms is preferred, a linear alkyl group having 1 to 3 carbon atoms is more preferred, and a methyl group or an ethyl group is even more preferred. The alkoxy group includes an alkoxy group having 1 to 8 carbon atoms. Among them, an alkoxy group having 1 to 6 carbon atoms is preferable, an alkoxy group having 1 to 3 carbon atoms is more preferable, and a methoxy group or an ethoxy group is further preferable.

[0063] In formula (3), R 2 represents a hydrogen atom or an alkyl group which may have a substituent, and is preferably an alkyl group which may have a substituent. R 2 Specific examples and preferred embodiments of the "alkyl group which may have a substituent" represented by R 1 Since this is the same as the "alkyl group which may have a substituent" in the above, the explanation thereof will be omitted.

[0064] In formula (3), R 3 represents a hydrogen atom or a substituent. R 3 Specific examples and preferred embodiments of the "substituent" represented by are the same as the substituents in the above-mentioned "divalent aromatic group which may have a substituent", and preferred embodiments are also the same, so description thereof will be omitted.

[0065] In terms of light resistance, L 3 is preferably an electron-withdrawing group, R 2 and L 4 is preferably a group having low electron donating property. Specific examples of such groups include L 3Examples of the alkyl group include an alkylsulfonyl group, an alkylcarbonyl group, an alkyloxycarbonyl group, an acyloxy group, an alkylsulfonylamino group, an alkylsulfamoyl group, an alkylsulfinyl group, and an alkylureido group. 2 and L 4 Examples of the group include the group having the following structure. In addition, the group having the following structure corresponds to R 2 and L 4 is shown including the nitrogen atom to which it is bonded.

[0066] [ka]

[0067] Specific examples of the first dichroic azo dye compound are shown below, but the invention is not limited thereto.

[0068] [ka] JPEG0007573609000009.jpg161127

[0069] -Second dichroic azo dye compound- The second dichroic azo dye compound is a compound different from the first dichroic azo dye compound, specifically, the chemical structure thereof is different. As described above, the second dichroic azo dye compound is a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm. From the viewpoint of adjusting the color of the polarizer, the second dichroic azo dye compound is preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 nm or more and less than 560 nm, more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 to 555 nm, and even more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 455 to 550 nm. In particular, by using a first dichroic azo dye compound having a maximum absorption wavelength of 560 to 700 nm and a second dichroic azo dye compound having a maximum absorption wavelength of 455 nm or more and less than 560 nm, it becomes easier to adjust the color of the polarizer. The second dichroic azo dye compound is preferably a compound having a chromophore which is the core of the dichroic azo dye compound, and a side chain bonded to an end of the chromophore. Specific examples of the chromophore include aromatic ring groups (e.g., aromatic hydrocarbon groups, aromatic heterocyclic groups) and azo groups. A structure having both an aromatic hydrocarbon group and an azo group is preferred, and a bisazo or trisazo structure having an aromatic hydrocarbon group and two or three azo groups is more preferred. The side chain is not particularly limited, and examples thereof include groups represented by R4, R5, or R6 in formula (4) described below.

[0070] The second dichroic azo dye compound is preferably a compound represented by formula (4) in that the degree of alignment of the polarizer is further improved.

[0071] Formula (4) [ka]

[0072] In formula (4), n represents 1 or 2. In formula (4), Ar3, Ar4 and Ar5 each independently represent a phenylene group which may have a substituent, or a heterocyclic group which may have a substituent. The substituent is not particularly limited, but may be, for example, the substituent W. The heterocyclic group may be either aromatic or non-aromatic. Examples of the atoms other than carbon that constitute the aromatic heterocyclic group include a nitrogen atom, a sulfur atom, and an oxygen atom. When the aromatic heterocyclic group has a plurality of atoms that constitute the ring other than carbon, these atoms may be the same or different. Specific examples of aromatic heterocyclic groups include a pyridylene group (pyridine-diyl group), a pyridazine-diyl group, an imidazole-diyl group, a thienylene group (thiophene-diyl group), a quinolylene group (quinoline-diyl group), an isoquinolylene group (isoquinoline-diyl group), an oxazole-diyl group, a thiazole-diyl group, an oxadiazole-diyl group, a benzothiazole-diyl group, a benzothiadiazole-diyl group, a phthalimido-diyl group, a thienothiazole-diyl group, a thiazolothiazole-diyl group, a thienothiophene-diyl group, and a thienoxazole-diyl group.

[0073] In formula (4), R4 is defined as L in formula (3). 3 is the same as: In formula (4), R5 and R6 are defined as R 2 and L 4 is the same as:

[0074] In terms of light resistance, R4 is preferably an electron-withdrawing group, and R5 and R6 are preferably groups having low electron-donating properties. Specific examples of such groups in which R4 is an electron-withdrawing group include L 3 is an electron-withdrawing group, and specific examples when R5 and R6 are groups with low electron-donating properties are 2 and L 4 is a group having low electron donating property.

[0075] Specific examples of the second dichroic azo dye compound are shown below, but the invention is not limited thereto.

[0076] [ka] JPEG0007573609000012.jpg155111 JPEG0007573609000013.jpg160105 JPEG0007573609000014.jpg167111

[0077] -Difference in logP values- The logP value is one of the indices that express the hydrophilic and hydrophobic properties of a chemical structure. The absolute value of the difference between the logP value of the side chain of the first dichroic azo dye compound and the logP value of the side chain of the second dichroic azo dye compound (hereinafter also referred to as "logP difference") is preferably 2.30 or less, more preferably 2.0 or less, even more preferably 1.5 or less, and particularly preferably 1.0 or less. If the logP difference is 2.30 or less, the affinity between the first dichroic azo dye compound and the second dichroic azo dye compound is increased, making it easier to form an array structure, and therefore the degree of orientation of the dichroic azo dye compounds is further improved. When the first dichroic azo dye compound or the second dichroic azo dye compound has a plurality of side chains, it is preferable that at least one of the logP differences satisfies the above value. Here, the side chain of the first dichroic azo dye compound and the second dichroic azo dye compound means a group bonded to the end of the above-mentioned chromophore. For example, when the first dichroic azo dye compound is a compound represented by formula (3), L 3 , L 4 and R 2 is a side chain, and when the second dichroic azo dye compound is a compound represented by formula (4), R4, R5 and R6 in formula (4) are side chains. In particular, when the first dichroic azo dye compound is a compound represented by formula (3) and the second dichroic azo dye compound is a compound represented by formula (4), L 3 The difference between the logP values ​​of R and R4, L 3 The difference between the logP values ​​of R and R5, L 4 The difference in logP value between R4 and L 4 It is preferable that at least one of the logP value differences between R1 and R2 satisfies the above value.

[0078] The logP value may also be called the hydrophilicity / hydrophobicity parameter. The logP value may be calculated using software such as ChemBioDraw Ultra or HSPiP (Ver. 4.1.07). It may also be experimentally determined by the method of OECD Guidelines for the Testing of Chemicals, Section 1, Test No. 117, etc. In this specification, unless otherwise specified, the value calculated by inputting the structural formula of a compound into HSPiP (Ver. 4.1.07) is used as the logP value.

[0079] -Third dichroic azo dye compound- The third dichroic azo dye compound is a dichroic azo dye compound other than the first dichroic azo dye compound and the second dichroic azo dye compound, and specifically, has a different chemical structure from the first dichroic azo dye compound and the second dichroic azo dye compound. If the light absorption anisotropic layer contains the third dichroic azo dye compound, there is an advantage that the color of the light absorption anisotropic layer can be easily adjusted. As described above, the third dichroic azo dye compound is a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 380 nm or more and less than 455 nm. From the viewpoint of adjusting the color of the polarizer, the third dichroic azo dye compound is preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 380 nm or more and less than 455 nm, more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 400 to 455 nm, and even more preferably a dichroic azo dye compound having a maximum absorption wavelength in the wavelength range of 410 to 455 nm.

[0080] The third dichroic azo dye compound preferably contains a dichroic azo dye compound represented by the following formula (6).

[0081] [ka]

[0082] In formula (6), A and B each independently represent a crosslinkable group or a monovalent substituent. In formula (6), a and b each independently represent 0 or 1. In terms of excellent alignment degree at 420 nm, it is preferable that a and b are both 0. In formula (6), L1 represents a monovalent substituent when a = 0, and L1 represents a single bond or a divalent linking group when a = 1. Furthermore, L2 represents a monovalent substituent when b = 0, and L2 represents a single bond or a divalent linking group when b = 1. In formula (6), Ar1 represents an (n1+2)-valent aromatic hydrocarbon group or heterocyclic group, Ar2 represents an (n2+2)-valent aromatic hydrocarbon group or heterocyclic group, and Ar3 represents an (n3+2)-valent aromatic hydrocarbon group or heterocyclic group. In formula (6), R1, R2, and R3 each independently represent a monovalent substituent. When n1≧2, multiple R1s may be the same or different from each other, when n2≧2, multiple R2s may be the same or different from each other, and when n3≧2, multiple R3s may be the same or different from each other. In formula (6), k represents an integer of 1 to 4. When k≧2, multiple Ar2's may be the same or different, and multiple R2's may be the same or different. In formula (6), n1, n2, and n3 each independently represent an integer of 0 to 4, provided that when k=1, n1+n2+n3≧0, and when k≧2, n1+n2+n3≧1.

[0083] In formula (6), examples of the crosslinkable groups represented by A and B include the polymerizable groups described in paragraphs

[0040] to

[0050] of JP 2010-244038 A. Among these, from the viewpoint of improving reactivity and synthesis suitability, acryloyl, methacryloyl, epoxy, oxetanyl, and styryl groups are preferred, and from the viewpoint of further improving solubility, acryloyl and methacryloyl groups are more preferred.

[0084] In formula (6), examples of the monovalent substituents represented by A and B include the substituent W.

[0085] The monovalent substituents represented by L1 and L2 are preferably groups introduced to increase the solubility of the dichroic substance, or groups having electron donating or electron withdrawing properties introduced to adjust the color tone of the dye. Examples of the substituents include the substituent W. The substituent W may be further substituted with a substituent W. When there are two or more substituents, they may be the same or different. If possible, they may be bonded to each other to form a ring. Examples of the group in which the above-mentioned substituent W is further substituted by the above-mentioned substituent W include a group in which an alkoxy group is substituted by an alkyl group, R B -(OR A ) na - group, and a group in which the carboxy group is substituted with an alkyl group; R B -OCO-R A -group, where R A represents an alkylene group having 1 to 5 carbon atoms, R B represents an alkyl group having 1 to 5 carbon atoms, and na represents an integer of 1 to 10 (preferably 1 to 5, more preferably 1 to 3). Among them, examples of the monovalent substituent represented by L1 and L2 include an alkyl group, an alkenyl group, an alkoxy group, and a group in which these groups are further substituted with these groups (for example, the above-mentioned R B -(OR A ) na - group, and R B -OCO-R A -group), and alkyl groups, alkoxy groups, and groups in which these groups are further substituted with these groups (for example, the above-mentioned R B -(OR A ) na - group, and R B -OCO-R A -group) is more preferred.

[0086] Examples of the divalent linking group represented by L1 and L2 include -O-, -S-, -CO-, -COO-, -OCO-, -O-CO-O-, and -CO-NR N -, -O-CO-NR N -, -NR N -CO-NR N Examples of such groups include -, -SO2-, -SO-, an alkylene group, a cycloalkylene group, and an alkenylene group, as well as groups formed by combining two or more of these groups. Among these, a group formed by combining an alkylene group with one or more groups selected from the group consisting of -O-, -COO-, -OCO-, and -O-CO-O- is preferred, and a group formed by combining an alkylene group with -OCO- is particularly preferred. Here, R N represents a hydrogen atom or an alkyl group. N If there are multiple R N may be the same or different from each other.

[0087] From the viewpoint of further improving the solubility of the dichroic substance, the number of atoms in the main chain of at least one of L1 and L2 is preferably 3 or more, more preferably 5 or more, further preferably 7 or more, and particularly preferably 10 or more. The upper limit of the number of atoms in the main chain is preferably 20 or less, and more preferably 12 or less. On the other hand, in order to further improve the degree of orientation of the dichroic material in the light absorption anisotropic layer, the number of atoms in the main chain of at least one of L1 and L2 is preferably 1 to 5. Here, when A in formula (6) is present, the "main chain" in L1 refers to a portion necessary for directly connecting the "O" atom connected to L1 and "A", and the "number of atoms in the main chain" refers to the number of atoms constituting the above portion. Similarly, when B in formula (6) is present, the "main chain" in L2 refers to a portion necessary for directly connecting the "O" atom connected to L2 and "B", and the "number of atoms in the main chain" refers to the number of atoms constituting the above portion. Note that the "number of atoms in the main chain" does not include the number of atoms in the branched chain described below. In addition, when A is not present, the "number of atoms in the main chain" in L1 refers to the number of atoms in L1 that does not include branched chains. When B is not present, the "number of atoms in the main chain" in L2 refers to the number of atoms in L2 that does not include branched chains. Specifically, in the following formula (D1), the number of atoms in the main chain of L1 is 5 (the number of atoms in the dotted frame on the left side of the following formula (D1)), and the number of atoms in the main chain of L2 is 5 (the number of atoms in the dotted frame on the right side of the following formula (D1)). In addition, in the following formula (D10), the number of atoms in the main chain of L1 is 7 (the number of atoms in the dotted frame on the left side of the following formula (D10)), and the number of atoms in the main chain of L2 is 5 (the number of atoms in the dotted frame on the right side of the following formula (D10)).

[0088] [ka]

[0089] L1 and L2 may have a branched chain. Here, when A is present in formula (6), the "branched chain" in L1 refers to a portion other than the portion necessary for directly linking the "O" atom linked to L1 in formula (6) to "A". Similarly, when B is present in formula (6), the "branched chain" in L2 refers to a portion other than the portion necessary for directly linking the "O" atom linked to L2 in formula (6) to "B". In addition, when A is not present in formula (6), the "branched chain" in L1 refers to a portion other than the longest atomic chain (i.e., the main chain) extending from the "O" atom connecting to L1 in formula (6). Similarly, when B is not present in formula (6), the "branched chain" in L2 refers to a portion other than the longest atomic chain (i.e., the main chain) extending from the "O" atom connecting to L2 in formula (6). The number of atoms in the branched chain is preferably 3 or less. The number of atoms in the branched chain is advantageous in that the degree of orientation of the dichroic material in the light absorption anisotropic layer is improved. Note that the number of atoms in the branched chain does not include the number of hydrogen atoms.

[0090] In formula (6), Ar1 represents an (n1+2)-valent (e.g., trivalent when n1 is 1), Ar2 represents an (n2+2)-valent (e.g., trivalent when n2 is 1), and Ar3 represents an (n3+2)-valent (e.g., trivalent when n3 is 1) aromatic hydrocarbon group or heterocyclic group. Here, Ar1 to Ar3 can be said to be divalent aromatic hydrocarbon groups or divalent heterocyclic groups substituted with n1 to n3 substituents (R1 to R3 described below), respectively. The divalent aromatic hydrocarbon group represented by Ar1 to Ar3 may be a single ring or may have a condensed ring structure of two or more rings. From the viewpoint of further improving the solubility, the number of rings in the divalent aromatic hydrocarbon group is preferably 1 to 4, more preferably 1 or 2, and even more preferably 1 (i.e., a phenylene group). Specific examples of the divalent aromatic hydrocarbon group include a phenylene group, an azulene-diyl group, a naphthylene group, a fluorene-diyl group, an anthracene-diyl group, and a tetracene-diyl group. From the viewpoint of further improving solubility, the phenylene group and the naphthylene group are preferred, and the phenylene group is more preferred. Specific examples of the third dichroic dye compound are shown below, but the present invention is not limited thereto. In the following specific examples, n represents an integer of 1 to 10.

[0091] [ka]

[0092] [ka]

[0093] It is also preferable that the third dye has a structure having no radical polymerizable group. When the third dye has a structure having no radical polymerizable group, the degree of orientation is excellent when the wavelength for measuring the degree of orientation described below is 420 nm. Examples of the structure having no radical polymerizable group include the following structures. [ka] JPEG0007573609000020.jpg12119

[0094] The third dichroic azo dye compound is more preferably a dichroic azo dye compound having a structure represented by the following formula (1-1), in that it has a particularly excellent degree of orientation when the wavelength for measuring the degree of orientation, as described below, is 420 nm.

[0095] [ka]

[0096] In formula (1-1), R1, R3, n1, n3, L1 and L2 are defined the same as R1, R3, n1, n3, L1 and L2 in formula (6), respectively. In formula (1-1), R4 and R5 are defined the same as the substituent W. In formula (1-1), R 21 and R 22 Each of the definitions is independently the same as that of R2 in formula (6). In formula (1-1), n21 and n22 are each independently defined as n2 in formula (6). n1+n21+n22+n3≧1, and n1+n21+n22+n3 is preferably an integer of 1 to 9, and more preferably an integer of 1 to 5.

[0097] Specific examples of the third dichroic azo dye compound are shown below, but the present invention is not limited to these.

[0098] [ka]

[0099] [ka]

[0100] [ka]

[0101] [Composition for forming optically absorptive anisotropic layer] The optically absorptive anisotropic layer of the optical film of the present invention is preferably prepared using a composition for forming an optically absorptive anisotropic layer, which contains, for example, a liquid crystalline compound and a dichroic substance. The composition for forming the optically absorptive anisotropic layer may contain components other than the liquid crystal compound and the dichroic substance, such as a solvent, an interface improver, a vertical alignment agent, a polymerizable component, a polymerization initiator (e.g., a radical polymerization initiator), a leveling agent suitable for vertical alignment, etc. In this case, the optically absorptive anisotropic layer in the present invention contains a solid component other than the liquid component (solvent, etc.). Components that may be contained in the composition for forming an optically absorptive anisotropic layer will be described below. The liquid crystal compound and the dichroic substance can be those described above, and the preferred embodiments are also as described above.

[0102] (solvent) The composition for forming an optically absorptive anisotropic layer preferably contains a solvent. Examples of the solvent include ketones (e.g., acetone, 2-butanone, methyl isobutyl ketone, cyclopentanone, and cyclohexanone), ethers (e.g., dioxane, tetrahydrofuran, 2-methyltetrahydrofuran, cyclopentyl methyl ether, tetrahydropyran, and dioxolane), aliphatic hydrocarbons (e.g., hexane), alicyclic hydrocarbons (e.g., cyclohexane), aromatic hydrocarbons (e.g., benzene, toluene, xylene, and trimethylbenzene), halogenated carbons (e.g., dichloromethane, trichloromethane, dichloroethane, dichlorobenzene, and chlorotoluene), esters (e.g., acetic acid, Examples of the organic solvent include organic solvents such as methyl, ethyl acetate, butyl acetate, and ethyl lactate, alcohols (e.g., ethanol, isopropanol, butanol, cyclohexanol, isopentyl alcohol, neopentyl alcohol, diacetone alcohol, and benzyl alcohol), cellosolves (e.g., methyl cellosolve, ethyl cellosolve, and 1,2-dimethoxyethane), cellosolve acetates, sulfoxides (e.g., dimethyl sulfoxide), amides (e.g., dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and N-ethylpyrrolidone), and heterocyclic compounds (e.g., pyridine), as well as water. These solvents may be used alone or in combination of two or more. Of these solvents, ketones (particularly cyclopentanone and cyclohexanone), ethers (particularly tetrahydrofuran, cyclopentyl methyl ether, tetrahydropyran, and dioxolane), alcohols (particularly benzyl alcohol), and amides (particularly dimethylformamide, dimethylacetamide, N-methylpyrrolidone, and N-ethylpyrrolidone) are preferred. When the liquid crystal composition contains a solvent, the content of the solvent is preferably from 80 to 99 mass %, more preferably from 83 to 98 mass %, and further preferably from 85 to 96 mass %, based on the total mass of the liquid crystal composition. When two or more solvents are contained, the content of the solvents means the total content of the solvents.

[0103] (Interface improver) The composition for forming the optically absorptive anisotropic layer preferably contains an interfacial improving agent. As the interface improver, the interface improvers described in the Examples section below can be used. When the coloring composition contains an interface improving agent, the content of the interface improving agent is preferably 0.001 to 5 parts by mass per 100 parts by mass of the total of the dichroic dye compound and the liquid crystal compound in the coloring composition.

[0104] (Vertical alignment agent) The composition for forming an optically absorptive anisotropic layer preferably contains a vertical alignment agent. The vertical alignment agent refers to a substance that has the effect of vertically aligning a dichroic substance. Examples of the vertical alignment agent include boronic acid compounds and onium salts.

[0105] The boronic acid compound is preferably a compound represented by formula (30).

[0106] Formula (30) [ka]

[0107] In formula (30), R 1 and R 2 each independently represents a hydrogen atom, a substituted or unsubstituted aliphatic hydrocarbon group, a substituted or unsubstituted aryl group, or a substituted or unsubstituted heterocyclic group. R 3 represents a substituent containing a functional group capable of bonding to a (meth)acrylic group. 3 is preferably a substituted or unsubstituted aliphatic hydrocarbon group, an aryl group or a heterocyclic group having a functional group capable of bonding to a (meth)acrylic group. Examples of functional groups that can be bonded to an acrylic group include polymerizable groups such as vinyl groups, acrylate groups, methacrylate groups, acrylamide groups, styryl groups, vinyl ketone groups, butadiene groups, vinyl ether groups, oxiranyl groups, aziridinyl groups, and oxetane groups. Among these, vinyl groups, acrylate groups, methacrylate groups, styryl groups, oxiranyl groups, and oxetane groups are preferred, and vinyl groups, acrylate groups, acrylamide groups, and styryl groups are more preferred. Specific examples of the boronic acid compound include boronic acid compounds represented by general formula (I) described in paragraphs 0023 to 0032 of JP-A No. 2008-225281. As the boronic acid compound, the compounds exemplified below are also preferred.

[0108] [ka]

[0109] The onium salt is preferably a compound represented by the formula (31).

[0110] Formula (31) [ka]

[0111] In formula (31), ring A represents a quaternary ammonium ion consisting of a nitrogen-containing heterocycle. X represents an anion. 1 represents a divalent linking group. 2 represents a single bond or a divalent linking group. 1 represents a divalent linking group having a 5- or 6-membered ring as a partial structure. Z represents a divalent linking group having 2 to 20 alkylene groups as a partial structure. P 1 and P 2 each independently represents a monovalent substituent having a polymerizable ethylenically unsaturated bond. Specific examples of the onium salt include the onium salts described in paragraphs 0052 to 0058 of JP-A No. 2012-208397, the onium salts described in paragraphs 0024 to 0055 of JP-A No. 2008-026730, and the onium salts described in JP-A No. 2002-37777.

[0112] The content of the vertical alignment agent in the composition for forming an optically absorptive anisotropic layer is preferably from 0.1 to 400% by mass, more preferably from 0.5 to 350% by mass, based on the total mass of the liquid crystal compound. The vertical alignment agent may be used alone or in combination of two or more kinds. When two or more kinds of vertical alignment agents are used, the total amount thereof is preferably within the above range.

[0113] -Leveling agent suitable for vertical alignment- When a dichroic material is vertically aligned using a composition for forming an optically absorptive anisotropic layer that contains a vertical alignment agent, the composition for forming an optically absorptive anisotropic layer preferably contains the following leveling agent. When the composition for forming an optically absorptive anisotropic layer contains a leveling agent, surface roughness caused by dry air applied to the surface of the anisotropic light absorbing layer is suppressed, and the dichroic material is more uniformly aligned. The leveling agent is not particularly limited, and is preferably a leveling agent containing a fluorine atom (fluorine-based leveling agent) or a leveling agent containing a silicon atom (silicon-based leveling agent), and more preferably a fluorine-based leveling agent.

[0114] Examples of fluorine-based leveling agents include fatty acid esters of polyvalent carboxylic acids in which a part of the fatty acid is substituted with a fluoroalkyl group, and polyacrylates having a fluoro substituent. In particular, when rod-shaped compounds are used as the dichroic material and liquid crystal compound, a leveling agent containing a repeating unit derived from the compound represented by formula (40) is preferred in terms of promoting the vertical alignment of the dichroic material and liquid crystal compound.

[0115] Formula (40) [ka]

[0116] R 0 represents a hydrogen atom, a halogen atom, or a methyl group. L represents a divalent linking group. L is preferably an alkylene group having 2 to 16 carbon atoms, and any non-adjacent -CH2- in the alkylene group may be substituted with -O-, -COO-, -CO-, or -CONH-. n represents an integer of 1 to 18.

[0117] The leveling agent having a repeating unit derived from the compound represented by formula (40) may further contain other repeating units. The other repeating units include a repeating unit derived from a compound represented by formula (41).

[0118] Formula (41) [ka]

[0119] R 11 represents a hydrogen atom, a halogen atom, or a methyl group. X is an oxygen atom, a sulfur atom, or -N(R 13 )-. R 13 represents a hydrogen atom or an alkyl group having 1 to 8 carbon atoms. R 12 represents a hydrogen atom, an alkyl group which may have a substituent, or an aromatic group which may have a substituent. The number of carbon atoms in the alkyl group is preferably 1 to 20. The alkyl group may be linear, branched, or cyclic. Examples of the substituent that the alkyl group may have include a poly(alkyleneoxy) group and a polymerizable group. Examples of the polymerizable group are as described above.

[0120] When the leveling agent contains a repeating unit derived from the compound represented by formula (40) and a repeating unit derived from the compound represented by formula (41), the content of the repeating unit derived from the compound represented by formula (40) is preferably 10 to 95 mol %, and more preferably 15 to 90 mol %, based on the total repeating units contained in the leveling agent. When the leveling agent contains a repeating unit derived from the compound represented by formula (40) and a repeating unit derived from the compound represented by formula (41), the content of the repeating unit derived from the compound represented by formula (41) is preferably 10 to 90 mol %, and more preferably 20 to 80 mol %, based on the total repeating units contained in the leveling agent.

[0121] Further, the leveling agent may also include a leveling agent containing a repeating unit derived from a compound represented by formula (42) instead of the repeating unit derived from the compound represented by formula (40) described above.

[0122] Formula (42) [ka]

[0123] R 2 represents a hydrogen atom, a halogen atom, or a methyl group. L 2 represents a divalent linking group. n represents an integer of 1 to 18.

[0124] Specific examples of the leveling agent include the compounds exemplified in paragraphs 0046 to 0052 of JP-A No. 2004-331812 and the compounds described in paragraphs 0038 to 0052 of JP-A No. 2008-257205.

[0125] The content of the leveling agent in the composition is preferably from 0.001 to 10% by mass, and more preferably from 0.01 to 5% by mass, based on the total mass of the liquid crystal compound. The leveling agent may be used alone or in combination of two or more kinds. When two or more kinds of leveling agents are used, the total amount thereof is preferably within the above range.

[0126] (Polymerizable component) The composition for forming the optically absorptive anisotropic layer preferably contains a polymerizable component. Examples of the polymerizable component include a compound containing acrylate (e.g., an acrylate monomer). In this case, the light absorption anisotropic layer in the present invention contains a polyacrylate obtained by polymerizing the compound containing the acrylate. Specifically, the compound described in paragraph 0058 of JP2017-122776A can be mentioned. When the composition for forming an optically absorptive anisotropic layer contains a polymerizable component, the content of the polymerizable component is preferably 3 to 20 parts by mass per 100 parts by mass of the total of the dichroic substance and the liquid crystal compound in the composition for forming an optically absorptive anisotropic layer.

[0127] (Polymerization initiator) The composition for forming the optically absorptive anisotropic layer preferably contains a polymerization initiator. The polymerization initiator is not particularly limited, but is preferably a compound having photosensitivity, that is, a photopolymerization initiator. As the photopolymerization initiator, various compounds can be used without any particular limitation. Examples of the photopolymerization initiator include α-carbonyl compounds (U.S. Pat. Nos. 2,367,661 and 2,367,670), acyloin ethers (U.S. Pat. No. 2,448,828), α-hydrocarbon-substituted aromatic acyloin compounds (U.S. Pat. No. 2,722,512), polynuclear quinone compounds (U.S. Pat. Nos. 3,046,127 and 2,951,758), and combinations of triaryl imidazole dimers and p-aminophenyl ketones (U.S. Pat. No. 3,549,367). ), acridine and phenazine compounds (JP 60-105667 A and U.S. Pat. No. 4,239,850 A), oxadiazole compounds (U.S. Pat. No. 4,212,970 A), o-acyloxime compounds (JP 2016-27384 A

[0065] ), and acylphosphine oxide compounds (JP 63-40799 A, JP 5-29234 A, JP 10-95788 A, and JP 10-29997 A). As such a photopolymerization initiator, commercially available products can also be used, such as IRGACURE 184, IRGACURE 907, IRGACURE 369, IRGACURE 651, IRGACURE 819, IRGACURE 2959, IRGACURE OXE-01, and IRGACURE OXE-02, all of which are manufactured by BASF.

[0128] When the composition for forming an optically absorptive anisotropic layer contains a polymerization initiator, the content of the polymerization initiator is preferably 0.01 to 30 parts by mass, more preferably 0.1 to 15 parts by mass, relative to 100 parts by mass of the total of the dichroic substance and the polymer liquid crystal compound in the composition for forming an optically absorptive anisotropic layer. When the content of the polymerization initiator is 0.01 part by mass or more, the durability of the optically absorptive anisotropic film becomes good, and when it is 30 parts by mass or less, the degree of orientation of the dichroic substance in the optically absorptive anisotropic layer becomes better. The polymerization initiator may be used alone or in combination of two or more. When two or more polymerization initiators are used, the total amount thereof is preferably within the above range.

[0129] (Dichroic substance content) The content of the dichroic substance is preferably 10 to 30% by mass, more preferably 15 to 30% by mass, further preferably 18 to 28% by mass, and particularly preferably 20 to 26% by mass, based on the total solid content mass of the optically absorptive anisotropic layer. The total solid content mass means the mass of the optically absorptive anisotropic layer-forming composition excluding the solvent component. If the content of the dichroic material is within the above range, a light absorbing anisotropic layer with a high degree of orientation can be obtained even when the light absorbing anisotropic layer is made into a thin film, and therefore a light absorbing anisotropic layer with excellent flexibility can be easily obtained. The content of the first dichroic azo dye compound is preferably 40 to 90 parts by mass, and more preferably 45 to 75 parts by mass, relative to 100 parts by mass of the total content of the dichroic substances. The content of the second dichroic azo dye compound is preferably from 6 to 50 parts by mass, and more preferably from 8 to 35 parts by mass, based on 100 parts by mass of the total content of the dichroic substances. The content of the third dichroic azo dye compound is preferably from 3 to 50 parts by mass, and more preferably from 5 to 40 parts by mass, based on 100 parts by mass of the dichroic azo dye compound. The content ratio of the first dichroic azo dye compound, the second dichroic azo dye compound, and the third dichroic azo dye compound used as necessary can be set arbitrarily in order to adjust the color of the light absorption anisotropic layer. However, the content ratio of the second dichroic azo dye compound to the first dichroic azo dye compound (second dichroic azo dye compound / first dichroic azo dye compound) is preferably 0.1 to 10, more preferably 0.2 to 5, and even more preferably 0.3 to 0.8, in terms of moles. If the content ratio of the second dichroic azo dye compound to the first dichroic azo dye compound is within the above range, the degree of orientation can be increased.

[0130] [Properties of the optically absorptive anisotropic layer] The light absorption anisotropic layer of the present invention has a transmittance inclined by 30° from the central axis of transmittance (hereinafter, unless otherwise specified, the transmittance at a wavelength of 550 nm is shown) of preferably 60% or less, more preferably 40% or less, and even more preferably 20% or less. This makes it possible to increase the contrast between the center of transmittance and the illuminance in a direction shifted from the center of transmittance, and to sufficiently narrow the viewing angle.

[0131] The transmittance of the central axis of the optically absorptive anisotropic layer used in the present invention is preferably 65% ​​or more, more preferably 75% or more, and even more preferably 85% or more. The upper limit is not particularly limited, but may be less than 100%. When the transmittance is within the above range, the illuminance at the viewing angle center of the image display device using the optically absorptive anisotropic layer can be increased, and the visibility can be improved.

[0132] In the liquid crystal display device of the present invention, in order to achieve a reduction in the illuminance in the peripheral portion while minimizing the reduction in the illuminance in the center of the viewing angle, the degree of orientation of the optically absorptive anisotropic layer measured at a wavelength of 550 nm is preferably 0.80 or more, more preferably 0.90 or more, and even more preferably 0.95 or more. In this specification, the degree of orientation measured at a wavelength of λ nm is defined as follows. During measurement, the polar angle, which is the angle with respect to the normal direction of the light absorbing anisotropic layer, is changed from 0 to 90° in 5° increments, and the Mueller matrix at a wavelength of 550 nm at each polar angle is measured to derive the minimum transmittance (Tmin). Next, after removing the influence of surface reflection, Tmin at the polar angle at which Tmin is highest is defined as Tm(0), and Tmin at the direction 40° larger than the polar angle at which Tmin is highest is defined as Tm(40). The absorbance is calculated from the obtained Tm(0) and Tm(40) using the following formula, and A(0) and A(40) are calculated. A = -log(Tm) Here, Tm represents the transmittance and A represents the absorbance. From the calculated A(0) and A(40), the degree of orientation S at a wavelength of 550 nm, defined by the following formula, is calculated. S=(4.6×A(40)-A(0)) / (4.6×A(40)+2×A(0)) By changing the wavelength from 550 nm to 420 nm or 650 nm, the degree of orientation S at wavelengths of 420 nm and 650 nm is calculated.

[0133] The optical film using the light absorptive anisotropic layer of the present invention can have a high transmittance along the central axis of transmittance and a low transmittance in a direction shifted from the central axis of transmittance. This is presumably due to the following reasons. In order to reduce the transmittance in a direction shifted from the central axis of transmittance, the thickness of the light absorbing anisotropic layer can be increased, but at the same time, the transmittance along the central axis of transmittance is reduced. Here, if the degree of orientation measured at a wavelength of 550 nm is set to 0.95 or more, it is considered that the dichroic material is the main contributor to the degree of orientation measured at a wavelength of 550 nm, and therefore the frequency of dichroic materials whose absorption axes are shifted from the central axis of transmittance is considered to decrease. As a result, it is possible to suppress the absorption by the dichroic material when viewed from the central axis of transmittance, and as a result, it is presumed that the transmittance along the central axis of transmittance can be increased.

[0134] It is also preferable that the optically absorptive anisotropic layer satisfies both of the following formulae (1) and (2). S P (420 nm) P (550nm) Formula (1) S P (420 nm) P (650nm) Formula (2) Here, the above S P (λ) represents the degree of orientation of the optically absorbing anisotropic layer measured at a wavelength of λ nm.

[0135] The thickness of the optically absorptive anisotropic layer is not particularly limited, but from the viewpoint of flexibility when the optical laminate of the present invention described later is used in a polarizing element, it is preferably 100 to 8000 nm, and more preferably 300 to 5000 nm.

[0136] [Method of forming optically absorptive anisotropic layer] ​​The method for forming the optically absorptive anisotropic layer is not particularly limited, and examples thereof include a method including, in this order, a step of forming a coating film by applying the above-mentioned composition for forming an optically absorptive anisotropic layer (hereinafter also referred to as a "coating film forming step") and a step of orienting the liquid crystalline component or dichroic material contained in the coating film (hereinafter also referred to as an "orientation step"). The liquid crystal component is a component including not only the above-mentioned liquid crystal compound but also a dichroic substance having liquid crystallinity when the above-mentioned dichroic substance has liquid crystallinity.

[0137] As a technique for orienting an organic dichroic dye in a desired direction, a technique for producing a polarizer using an organic dichroic dye, a technique for producing a guest-host liquid crystal cell, etc., can be referred to. For example, the techniques used in the methods for producing dichroic polarizing elements described in JP-A-11-305036 and JP-A-2002-90526 and the methods for producing guest-host type liquid crystal displays described in JP-A-2002-99388 and JP-A-2016-27387 can also be used to produce the light absorption anisotropic layer used in the present invention.

[0138] For example, by utilizing the technique of a guest-host type liquid crystal cell, the organic dichroic dye molecules can be aligned in the desired orientation as described above in association with the alignment of the host liquid crystal. Specifically, the light absorption anisotropic layer used in the present invention can be produced by mixing the organic dichroic dye as the guest with a rod-shaped liquid crystal compound as the host liquid crystal, aligning the host liquid crystal, and aligning the organic dichroic dye molecules along the alignment of the liquid crystal molecules, and fixing the alignment state.

[0139] In order to prevent the light absorption characteristics of the light absorption anisotropic layer used in the present invention from varying depending on the usage environment, it is preferable to fix the orientation of the organic dichroic dye by forming a chemical bond. For example, the orientation can be fixed by promoting polymerization of the host liquid crystal, the organic dichroic dye, or a polymerizable component added as required.

[0140] Alternatively, a guest-host type liquid crystal cell having a liquid crystal layer containing at least an organic dichroic dye and a host liquid crystal between a pair of substrates may itself be used as the light absorption anisotropic layer used in the present invention. The orientation of the host liquid crystal (and the orientation of the organic dichroic dye molecules associated therewith) can be controlled by an alignment film formed on the inner surface of the substrate, and the alignment state is maintained unless an external stimulus such as an electric field is applied, making it possible to keep the light absorption characteristics of the light absorption anisotropic layer used in the present invention constant.

[0141] In addition, a polymer film that satisfies the light absorption characteristics required for the light absorption anisotropic layer used in the present invention can be prepared by permeating an organic dichroic dye into a polymer film and orienting the organic dichroic dye along the orientation of the polymer molecules in the polymer film. Specifically, the polymer film can be prepared by applying a solution of the organic dichroic dye to the surface of the polymer film and permeating the film. The orientation of the organic dichroic dye can be adjusted by the orientation of the polymer chain in the polymer film, its properties (chemical and physical properties of the polymer chain or its functional groups, etc.), the coating method, etc. Details of this method are described in JP-A-2002-90526.

[0142] The coating film forming step, the orientation step, and other steps will be described below.

[0143] (Coating film formation process) The coating film forming step is a step of forming a coating film by applying a composition for forming an optically absorptive anisotropic layer. By using a composition for forming an optically absorptive anisotropic layer that contains the above-mentioned solvent, or by using a composition for forming an optically absorptive anisotropic layer that has been made into a liquid such as a molten liquid by heating or the like, it becomes easy to apply the composition for forming an optically absorptive anisotropic layer. Examples of methods for applying the composition for forming the optically absorptive anisotropic layer include known methods such as roll coating, gravure printing, spin coating, wire bar coating, extrusion coating, direct gravure coating, reverse gravure coating, die coating, spraying, and inkjet methods.

[0144] (Orientation process) The alignment step is a step of aligning the liquid crystal component contained in the coating film. This results in a light absorption anisotropic layer. The alignment step may include a drying treatment, a heating treatment, and a cooling treatment. Each of the above treatments will be described below. The orientation step may include a drying treatment. By the drying treatment, components such as a solvent can be removed from the coating film. The drying treatment may be performed by leaving the coating film at room temperature for a predetermined time (for example, natural drying), or may be performed by heating and / or blowing air. Here, the liquid crystal component contained in the composition for forming an optically absorptive anisotropic layer may be aligned by the above-mentioned coating film forming process or drying treatment. For example, in an embodiment in which the composition for forming an optically absorptive anisotropic layer is prepared as a coating liquid containing a solvent, the coating film is dried to remove the solvent from the coating film, thereby obtaining a coating film having optical absorption anisotropy (i.e., an optically absorptive anisotropic film). When the drying treatment is carried out at a temperature equal to or higher than the transition temperature of the liquid crystal component contained in the coating film to a liquid crystal phase, the heating treatment described below does not need to be carried out.

[0145] The transition temperature of the liquid crystal component contained in the coating film to the liquid crystal phase is preferably 10 to 250°C, more preferably 25 to 190°C, from the viewpoint of manufacturability, etc. If the transition temperature is 10°C or higher, cooling treatment or the like is not required to lower the temperature to the temperature range in which the liquid crystal phase is exhibited, which is preferable. In addition, if the transition temperature is 250°C or lower, a high temperature is not required even when the film is once in an isotropic liquid state at a temperature higher than the temperature range in which the liquid crystal phase is exhibited, which is preferable, since waste of thermal energy and deformation and deterioration of the substrate can be reduced.

[0146] The alignment step preferably includes a heat treatment, which allows the liquid crystal component contained in the coating film to be aligned, so that the coating film after the heat treatment can be suitably used as an optically absorptive anisotropic film. From the viewpoint of manufacturability, the heat treatment temperature is preferably from 10 to 250° C., more preferably from 25 to 190° C. The heating time is preferably from 1 to 300 seconds, more preferably from 1 to 60 seconds.

[0147] The alignment step may include a cooling treatment carried out after the heating treatment. The cooling treatment is a treatment for cooling the coated film after heating to about room temperature (20 to 25°C). This makes it possible to fix the alignment of the liquid crystal component contained in the coated film. The cooling means is not particularly limited and can be carried out by a known method. By the above steps, an optically absorptive anisotropic film can be obtained. In this embodiment, the method for aligning the liquid crystal component contained in the coating film includes drying treatment and heating treatment, but is not limited thereto and can be carried out by any known alignment treatment.

[0148] (Other processes) The method for forming the optically absorptive anisotropic layer may include a step of curing the optically absorptive anisotropic layer (hereinafter also referred to as a "curing step") after the above-mentioned alignment step. The curing step is carried out by heating and / or light irradiation (exposure) when the light absorption anisotropic layer has a crosslinkable group (polymerizable group), for example. Among these, the curing step is preferably carried out by light irradiation. The light source used for curing may be various light sources such as infrared light, visible light, or ultraviolet light, but ultraviolet light is preferred. In addition, ultraviolet light may be irradiated while heating during curing, or ultraviolet light may be irradiated through a filter that transmits only specific wavelengths. When the exposure is performed with heating, the heating temperature during exposure is preferably 25 to 140° C., although it depends on the transition temperature to a liquid crystal phase of the liquid crystal component contained in the liquid crystal film. The exposure may be carried out under a nitrogen atmosphere. When the curing of the liquid crystal film proceeds by radical polymerization, it is preferable to carry out the exposure under a nitrogen atmosphere, since this reduces the inhibition of polymerization caused by oxygen.

[0149] The thickness of the optically absorptive anisotropic layer is not particularly limited, but from the viewpoint of flexibility when the laminate of the present invention described below is used in a polarizing element, it is preferably 100 to 8000 nm, and more preferably 300 to 5000 nm.

[0150] (Patterning of optically absorptive anisotropic layer) The optically absorptive anisotropic layer of the present invention may be an optically absorptive anisotropic layer having Region A and Region B in its plane, with the oblique transmittance as viewed from a polar angle of 30° (hereinafter referred to as the polar angle 30° transmittance) being different between Region A and Region B. In this case, it is preferable that the optically absorptive anisotropic layer has a polar angle 30° transmittance of 10% or less in Region A and a polar angle 30° transmittance of 80% or more in Region B. By patterning the above-mentioned regions, it is possible to strengthen or weaken the viewing angle dependency. This makes it possible to display highly confidential information only in the regions with strengthened viewing angle dependency. In addition, by freely controlling the viewing angle dependency as a display device, it is possible to design a display device with excellent design. In order to prevent light leakage from the light-emitting part to the surrounding area in a display device such as μLED, it is also possible to increase the contrast between light and dark on the screen by patterning the areas other than the light-emitting part to have a high polar angle 30° transmittance and the light-emitting part to have a low polar angle 30° transmittance.

[0151] -Pattern formation method- The method for forming a patterned light absorption anisotropic layer having two or more different regions in the plane is not particularly limited, and various known methods such as those described in WO2019 / 176918 can be used. Examples include a method for controlling the thickness of the patterned light absorption anisotropic layer in the plane, a method for unevenly distributing a dichroic dye compound in the patterned light absorption anisotropic layer, and a method for post-processing an optically uniform patterned light absorption anisotropic layer. Methods for controlling the thickness of the patterned optically absorptive anisotropic layer in-plane include a method using lithography, a method using imprinting, and a method for forming a patterned optically absorptive anisotropic layer on a substrate having a concave-convex structure. Methods for unevenly distributing the dichroic dye compound in the patterned optically absorptive anisotropic layer include a method for extracting the dichroic dye compound by immersion in a solvent (bleaching). Furthermore, a method for post-processing an optically uniform patterned optically absorptive anisotropic layer includes a method for cutting a part of a flat optically absorptive anisotropic layer by laser processing or the like.

[0152] [Color adjustment layer] The optical film of the present invention has a color-adjusting layer containing at least one organic colorant compound. Hereinafter, the explanation of how the color-adjusting layer provides an optical film with excellent wide-angle color suppression properties (principle of color adjustment), the organic dye compound contained in the color-adjusting layer, and the properties of the color-adjusting layer will be described in detail.

[0153] (Principle of color adjustment) The color control of an optical film containing a dichroic material is usually performed by adjusting the amount and / or the ratio of the dichroic material added to the film. However, when the degree of orientation calculated by wavelength changes, it is difficult to obtain an optical film with excellent wide-angle color suppression by only adjusting the amount and / or the ratio of the dichroic material added. For example, when using a dichroic substance having the above-mentioned thienothiazole skeleton, the substance may have different absorption wavelengths in multiple directions, which can cause a problem of reducing the degree of orientation measured at wavelengths outside the main absorption wavelength range of the dichroic substance. Specifically, for example, when a dichroic dye compound having a thienothiazole skeleton is used in a light absorption anisotropic layer, the degree of orientation measured in the short wavelength region decreases, and when the degree of orientation measured at each wavelength is S(λ), it becomes easier to satisfy the relationship between the above formulas (1) and (2). When the relationship between equations (1) and (2) is satisfied, S P (420nm) is S P (550 nm) and S P(650 nm), the degree of orientation appears to be low only in the short wavelength region. In this case, even if multiple dichroic substances are blended to make the color neutral when viewed from the transmittance central axis direction, the color will not be neutral when viewed from an oblique direction. In other words, when the relationship of formula (1) and formula (2) is satisfied, it is difficult to obtain an optical film with excellent wide-angle color suppression performance by only adjusting the amount and / or the ratio of the dichroic substances added in the optical film.

[0154] Furthermore, when multiple dichroic materials are contained in an optical film, even if the ease of orientation of each dichroic material in the optical film differs, the degree of orientation calculated depending on the wavelength at which the degree of orientation is measured may change, making it difficult to obtain an optical film with excellent wide-angle color suppression properties by simply adjusting the amount and / or the ratio of the amounts of dichroic materials added in the optical film.

[0155] In the present invention, when the color in the transmittance central axis direction is made neutral by adjusting the amount and / or the ratio of the dichroic substance added in the light absorption anisotropic layer, the color change when viewed from a diagonal direction of the transmittance central axis may become large. Here, by adjusting the amount and / or the ratio of the dichroic substance added and adjusting the color using a color adjusting layer that satisfies any one of the following requirements 1 to 3, it becomes easy to suppress the color change when viewed in the transmittance central axis direction and from a diagonal direction, that is, it is considered that an optical film with better wide-angle color suppression properties can be obtained. In this case, when the color-adjusting layer satisfies any one of the following requirements 1 to 3, the color-adjusting layer exhibits small color change when viewed in the transmittance central axis direction and from an oblique direction, and offsets the color change of the light-absorption anisotropic layer, resulting in an optical film with better wide-angle color suppression properties. Requirement 1:S C (420nm)<0.1 Requirement 2:S C (550nm)<0.1 Requirement 3:S C (650nm)<0.1 However, S C(λ nm) represents the degree of orientation of the color-adjusting layer measured at a wavelength of λ nm.

[0156] (Organic dye compound contained in color adjusting layer) The color-adjusting layer contains at least one organic colorant compound. Examples of structures possessed by the dye compound contained in the color-adjusting layer include an azo structure, a methine structure, an anthraquinone structure, a triarylmethane structure, an oxazine structure, an azomethine structure, a phthalocyanine structure, a porphyrin structure, a perylene structure, a pyrrolopyrrole structure, and a squarylium structure. Here, in terms of excellent absorption waveform, heat resistance, and light resistance, the methine structure, the azomethine structure, the azo structure, the phthalocyanine structure, and the anthraquinone structure are preferred, compounds having an azo structure, a phthalocyanine structure, and an anthraquinone structure are more preferred, and compounds having an anthraquinone structure are even more preferred. Specific examples of compounds having the above structure include the dye compounds described in Functional Dyes, co-authored by Makoto Okawahara, Masaru Matsuoka, Kosuke Hirashima, and Teijiro Kitao, Kodansha, 1992, and Electronics Related Materials, edited by Sumio Tokita, CMC Co., Ltd., 1998.

[0157] It is also preferable that the dye compound contained in the color-adjusting layer has at least one of a benzene ring and a heterocyclic ring structure in the molecule. The structure having a benzene ring may be any structure that includes a benzene ring as part of the structure, and examples of the structure having a benzene ring include a benzene ring, a naphthalene ring, an anthracene ring, a phenanthrene ring, a fluorene ring, and a pyrene ring, as well as an anthraquinone structure, an oxazine structure, a phthalocyanine structure, a porphyrin structure, and a perylene structure. Examples of the structure having a heterocycle include a ring structure containing a heteroatom other than carbon. The structure having a heterocycle may or may not have aromaticity, and is preferably aromatic. Examples of the structure having a heterocycle include a pyrrole ring, a furan ring, a thiophene ring, an imidazole ring, a pyrazole ring, an oxazole ring, a benzimidazole ring, an indole ring, a purine ring, and a benzotriazole ring, as well as an oxazine structure, a phthalocyanine structure, and a porphyrin structure.

[0158] The absorption peak wavelength of the dye compound contained in the color-adjusting layer used in the present invention is preferably 500 to 650 nm, more preferably 550 to 600 nm. By setting the absorption peak wavelength of the dye compound in this range, the color of the optical film in the present invention can be adjusted to be more neutral.

[0159] In this specification, the absorption peak wavelength of a dye compound refers to the maximum absorption wavelength in the absorption spectrum measured by the following method. A solution is prepared by dissolving 1.0 mg of the dye compound to be measured in 100 ml of chloroform or 100 ml of water. Next, the prepared solution is placed in a quartz cell (1 cm long square cell), and the absorbance of the solution is measured in the wavelength range of 200 to 800 nm using a UV-Vis-Infrared Spectrophotometer U-3150 (Shimadzu Corporation). Next, in the obtained absorption spectrum, the maximum absorption wavelength is determined.

[0160] Specific examples of the dye compound that can be used in the present invention are shown below, but the present invention is not limited to these.

[0161] - Compounds with anthraquinone structure - [ka]

[0162] - Compounds with azo structure - [ka]

[0163] -Compounds having a triarylmethane structure- [ka]

[0164] - Compounds having an oxazine structure - [ka]

[0165] - Compounds having a phthalocyanine structure - [ka]

[0166] (Properties of color-adjusting layer) Moreover, the color-adjusting layer preferably satisfies any one of the following requirements 1 to 3, more preferably satisfies two of the following requirements 1 to 3, and even more preferably satisfies all of the requirements 1 to 3. Requirement 1:S C (420nm)<0.1 Requirement 2:S C (550nm)<0.1 Requirement 3:S C (650nm)<0.1 In addition, S C (λ nm) represents the degree of orientation of the color-adjusting layer measured at a wavelength of λ nm. The degree of orientation measured at a wavelength of λ nm is the same as that of the light-absorption anisotropic layer, and is obtained by measuring the color-adjusting layer. When a color-adjusting layer is laminated to obtain an optical film, the color-adjusting layer before transfer lamination may be used for measurement, or the color-adjusting layer may be formed on another substrate and used for measurement, or the color-adjusting layer may be separated from the laminated optical film and used for measurement. In this specification, the orientation degree is described when the color-adjusting layer is separated from the laminated optical film and used as the measured object.

[0167] The color-adjusting layer satisfies any one of the above requirements 1 to 3, but may also satisfy all of the requirements 1 to 3, or may satisfy two selected from the requirements 1 to 3. In addition, the above requirements that the color-adjusting layer must satisfy are preferably appropriately selected depending on the degree of orientation of the dichroic material contained in the light-absorption anisotropic layer. Below, examples of the relationship between the degree of orientation of the light-absorption anisotropic layer and the combination of preferred requirements that the color-adjusting layer must satisfy for that relationship are shown. For example, the following combination 1: P (420 nm) P (650 nm): Requirement 3" is that the light absorption anisotropic layer contains the first dichroic azo dye compound and the third dichroic azo dye compound, and the S P (420nm) is the above S P If it is smaller than 650 nm, it means that it is preferable that the color-adjusting layer satisfies requirement 3. Combination 1: S P (420 nm) P (650nm): Requirement 3 Combination 2: S P (420 nm) P (550nm): Requirement 2 Combination 3: S P (550 nm) P (420nm): Requirement 1 Combination 4: S P (550 nm) P (650nm): Requirement 3 Combination 5: S P (650 nm) P (420nm): Requirement 1 Combination 6: S P (650 nm) P (550nm): Requirement 2 Among the above combinations, combinations 1, 2, 5 and 6 are preferred, and combinations 1 and 5 are more preferred.

[0168] Moreover, it is preferable that the color-adjusting layer satisfies the following formula (7). 0.005≦(c(C)×d(C)) / (c(P)×d(P))≦0.06 Equation (7) ​​​​​​​In formula (7), c(C) represents the mass ratio of the organic dye compound in the color-adjusting layer to the total mass of the color-adjusting layer. In the formula (7), d(C) represents the film thickness (μm) of the color-adjusting layer. In formula (7), c(P) represents the mass ratio of the dichroic dye compound in the optically absorptive anisotropic layer to the total mass of the optically absorptive anisotropic layer. In formula (7), d(P) represents the film thickness (μm) of the optically absorptive anisotropic layer. In the above formula (7), the lower limit is more preferably 0.01 or more, and the upper limit is more preferably 0.03 or less. When the color-adjusting layer satisfies formula (7), the color when viewed from the transmittance central axis direction can be made neutral, and the transmittance in the transmittance central axis direction can be increased. In this specification, the film thickness can be measured by cutting a cross section of the obtained optical film using a microtome cutter, and observing and measuring the length with a scanning electron microscope (SEM).

[0169] The color-adjusting layer may have only the function of a color-adjusting layer, or may have the function integrated with other layers. That is, the light-absorption anisotropic layer, the transparent substrate film, the alignment film, and the barrier layer may all have the function of a color-adjusting layer. When the color adjusting layer of the optical film is a layer separate from the light absorbing anisotropic layer, the lamination position of the color adjusting layer in the optical film is not particularly limited, but it is preferable that the color adjusting layer is in direct contact with the light absorbing anisotropic layer and is provided on the viewing side of the light absorbing anisotropic layer.

[0170] [Transparent substrate film] The transparent substrate film is not particularly limited, and examples thereof include known transparent resin films, known transparent resin plates, and known transparent resin sheets. Examples of transparent resin films include cellulose acylate films (e.g., cellulose triacetate film (refractive index 1.48), cellulose diacetate film, cellulose acetate butyrate film, cellulose acetate propionate film), polyethylene terephthalate film, polyethersulfone film, polyacrylic resin film, polyurethane resin film, polyester film, polycarbonate film, polysulfone film, polyether film, polymethylpentene film, polyether ketone film, and (meth)acrylonitrile film.

[0171] Among these, a cellulose acylate film, which is generally used as a protective film for a polarizing plate, is preferred, and a cellulose triacetate film is more preferred, because it has high transparency, little optical birefringence, and is easy to manufacture. The transparent substrate film usually has a thickness of 20 μm to 100 μm.

[0172] [Alignment film] The optical film of the present invention may have an alignment layer between the transparent substrate film and the light absorptive anisotropic layer. The alignment film is not particularly limited as long as it can make the dichroic dye compound have a desired alignment state on the alignment film. For example, a film formed from a multifunctional acrylate compound and a polyvinyl alcohol film are included, and a polyvinyl alcohol film is preferred. The polyvinyl alcohol used in the polyvinyl alcohol film may be a modified polyvinyl alcohol.

[0173] [Barrier layer] The optical layered body of the present invention may have a barrier layer in addition to the light absorption anisotropic layer. Here, the barrier layer is also called a gas barrier layer (oxygen barrier layer), and has the function of protecting the polarizing element of the present invention from gases such as oxygen in the atmosphere, moisture, or compounds contained in adjacent layers. For the barrier layer, reference can be made to the descriptions in, for example, paragraphs

[0014] to

[0054] of JP 2014-159124 A, paragraphs

[0042] to

[0075] of JP 2017-121721 A, paragraphs

[0045] to

[0054] of JP 2017-115076 A, paragraphs

[0010] to

[0061] of JP 2012-213938 A, and paragraphs

[0021] to

[0031] of JP 2005-169994 A.

[0174] [Refractive index adjustment layer] In the optical laminate of the present invention, the above-mentioned light-absorption anisotropic layer has a dichroic material, and internal reflection due to the high refractive index of the light-absorption anisotropic layer may become a problem. In that case, it is preferable that a refractive index adjustment layer is present. The refractive index adjustment layer is a layer disposed so as to be in contact with the light-absorption anisotropic layer, and it is preferable that the in-plane average refractive index at a wavelength of 550 nm is 1.55 or more and 1.70 or less. It is preferable that the refractive index adjustment layer is a refractive index adjustment layer for performing so-called index matching.

[0175] [Optical film properties] The optical film of the present invention has a transmittance in the central axis direction of preferably 65% ​​or more, more preferably 75% or more, and even more preferably 85% or more. There is no particular upper limit, but it may be less than 100%.

[0176] The thickness of the optical film of the present invention is preferably from 30 to 90 μm, more preferably from 35 to 70 μm, and further preferably from 40 to 50 μm.

[0177] <Method of manufacturing optical film> The optical film of the present invention can be produced by any known method, and is not particularly limited. Each step in the production can also be performed by any known method, and is not particularly limited. An example of a method for producing the optical film of the present invention includes a method comprising, in this order, a step of applying a composition for forming an alignment film onto the transparent substrate film to form an alignment film, a step of applying the composition for forming a light absorbing anisotropic layer onto the alignment film and orienting a dichroic dye compound contained in the coating film to obtain the light absorbing anisotropic layer, and a step of forming the color adjusting layer adjacent to the light absorbing anisotropic layer. Hereinafter, layers that may be provided when producing the optical film will be described. Specifically, the adhesive layer and the bonding layer will be described.

[0178] [Adhesive layer] In producing the optical film, an adhesive layer may be provided. The adhesive layer in the present invention is preferably a transparent, optically isotropic adhesive similar to those used in ordinary liquid crystal displays, and a pressure-sensitive adhesive is usually used.

[0179] In addition to the base material (adhesive), conductive particles, and thermally expandable particles used as necessary, the adhesive layer in the present invention may contain additives such as crosslinkers (e.g., isocyanate-based crosslinkers, epoxy-based crosslinkers, etc.), tackifiers (e.g., rosin derivative resins, polyterpene resins, petroleum resins, oil-soluble phenolic resins, etc.), plasticizers, fillers, antioxidants, surfactants, UV absorbers, light stabilizers, and antioxidants.

[0180] The thickness of the adhesive layer is usually 20 to 500 μm, and preferably 20 to 250 μm. If it is less than 20 μm, the necessary adhesive strength and / or rework suitability may not be obtained, and if it exceeds 500 μm, the adhesive may protrude or ooze out from the peripheral edge of the image display device.

[0181] The adhesive layer can be formed by any suitable method, such as a method in which a coating liquid containing a base material, conductive particles, and, if necessary, heat-expandable particles, additives, solvents, etc. is directly applied onto the protective member support 110 and then pressure-bonded via a release liner, or a method in which a coating liquid is applied onto a suitable release liner (such as release paper) to form a heat-expandable adhesive layer, and then this is pressure-transferred (adhered) onto the protective member support 110.

[0182] As another example of the protective member, a configuration in which conductive particles are added to the configuration of the heat-peelable adhesive sheet described in JP-A-2003-292916 can be used. Furthermore, as the protective member, a commercially available product such as "REVALPHA" manufactured by Nitto Denko Corporation, in which conductive particles are scattered on the surface of the adhesive layer, may be used. There is no particular limitation on the method for forming the adhesive layer, and the details will be described later in the section on the method for forming the adhesive layer.

[0183] [Adhesive layer] In the production of the optical film, an adhesive layer may be provided. The adhesive layer means a layer formed of an adhesive. The adhesive exhibits adhesiveness by drying or reacting after lamination. An example of an adhesive that exhibits adhesiveness upon drying is a polyvinyl alcohol adhesive (PVA adhesive). Examples of curable adhesives that exhibit adhesive properties through a reaction include active energy ray curable adhesives such as (meth)acrylate adhesives, and cationic polymerization curable adhesives. Note that (meth)acrylate means acrylate and / or methacrylate. Examples of the curable component in the (meth)acrylate adhesive include a compound having a (meth)acryloyl group and a compound having a vinyl group. In addition, as the cationic polymerization curing adhesive, a compound having an epoxy group and / or an oxetanyl group can also be used. The compound having an epoxy group is not particularly limited as long as it has at least two epoxy groups in the molecule, and various commonly known curable epoxy compounds can be used. Examples of preferred epoxy compounds include a compound having at least two epoxy groups and at least one aromatic ring in the molecule (aromatic epoxy compound), and a compound having at least two epoxy groups in the molecule, at least one of which is formed between two adjacent carbon atoms constituting an alicyclic ring (alicyclic epoxy compound). Among these, from the viewpoint of resistance to thermal deformation, an ultraviolet-curing adhesive that is cured by exposure to ultraviolet light is preferably used.

[0184] [Formation method] A method for forming the adhesive layer and / or the pressure-sensitive adhesive layer will be described. The adhesive layer and / or each layer of the pressure-sensitive adhesive layer may contain a compound having ultraviolet absorbing ability, such as a salicylic acid ester compound, a benzophenol compound, a benzotriazole compound, a cyanoacrylate compound, a nickel complex compound, etc. The adhesive layer and / or the pressure-sensitive adhesive layer may be treated by irradiating with ultraviolet light.

[0185] The application of the adhesive layer and / or the bonding layer to the optical film can be performed by a suitable method. For example, the base polymer or polymer composition of the adhesive layer or the bonding layer is dispersed or dissolved in a solvent containing a suitable solvent such as toluene and ethyl acetate to prepare a 10 to 40 mass% adhesive solution. The prepared solution can be applied directly onto the film by a suitable spreading method such as casting or coating, and the adhesive layer or the bonding layer can be formed on a substrate other than the optical film and then transferred.

[0186] The adhesive layer and / or the bonding layer can be formed by superposing layers of different compositions and types. The adhesive layer and / or the bonding layer may be provided on one side or both sides of the optical film. When the adhesive layer and / or the bonding layer are provided on both sides of the optical film, the adhesive layer and / or the bonding layer may have different compositions, types and thicknesses on both sides of the film.

[0187] The optical film may have a protective film, and the protective film may be subjected to a surface modification treatment before the adhesive or pressure-sensitive adhesive is applied in order to improve adhesion, etc. Specific examples of the surface modification treatment include a corona treatment, a plasma treatment, a primer treatment, and a saponification treatment.

[0188] <Optical laminate> The optical laminate of the present invention is an optical laminate obtained by laminating the optical film of the present invention in which the angle θ between the transmittance central axis and the film normal is 0° to 45° and a polarizer layer in which a dichroic material is oriented horizontally to the film surface. This makes it possible to reduce the transmittance of light in a direction oblique to the transmittance central axis, and by narrowing the viewing angle, the optical laminate can be used for applications such as privacy films. The polarizer layer in which the dichroic material is horizontally aligned is not particularly limited. The polarizer layer may be a polarizer in which the dichroic material is dyed in polyvinyl alcohol or other polymer resin and stretched to be horizontally aligned, or a polarizer in which the dichroic material is horizontally aligned by utilizing the orientation of a liquid crystal compound as in the light absorption anisotropic layer of the present invention. Among them, a polarizer in which the dichroic material is horizontally aligned by utilizing the orientation of a liquid crystal compound is preferred. Polarizers in which a dichroic material is oriented by utilizing the orientation properties of liquid crystals have many advantages, such as the ability to make them extremely thin, with a thickness of approximately 0.1 to 5 μm, the fact that they are less likely to crack when bent as described in JP 2019-194685 A, the fact that they are less susceptible to thermal deformation, and the fact that they have excellent durability even in polarizing plates with high transmittance of over 50% as described in JP 6483486 A. Taking advantage of these advantages, the optical laminate of the present invention can be used in applications requiring high brightness and / or small size and light weight, in fine optical systems, for molding into parts with curved surfaces, and for flexible applications.

[0189] The thickness of the optical layered body of the present invention is preferably 40 to 150 μm, more preferably 45 to 100 μm, and even more preferably 50 to 70 μm, from the viewpoints of application to molding into parts having curved surfaces and application to flexible uses.

[0190] [Optical laminate with unevenness] The optical laminate of the present invention has a structure that prevents defects caused by contact between smooth surfaces. In order to prevent blocking, it is preferable to provide surface irregularities with an arithmetic surface roughness Ra of 35 to 125 nm. The arithmetic surface roughness Ra of the surface irregularities is more preferably 50 to 110 nm, and even more preferably 65 to 95 nm. By making the arithmetic surface roughness Ra 35 nm or more, it is possible to prevent the films from sticking together when the optical films are stacked, and to make it difficult for traces of film adhesion to remain. Furthermore, by making the arithmetic surface roughness Ra 125 nm or less, it is possible to maintain the narrowed viewing angle by the optical film of the present invention, particularly when used for privacy film applications.

[0191] The arithmetic mean roughness Ra is the arithmetic mean roughness conforming to JIS B0601:2001. The arithmetic mean roughness Ra can be measured using a stylus-type surface roughness meter (such as Mitutoyo's surface roughness measuring instrument SJ-401). In this specification, the arithmetic mean roughness Ra measured using a stylus-type surface roughness meter (Mitutoyo's surface roughness measuring instrument SJ-401) is described.

[0192] The method of imparting the surface roughness may be to laminate another optical film having a surface unevenness, to further laminate a surface unevenness layer, or to directly impart unevenness to the barrier layer or the like on the outermost surface of the optical laminate of the present invention. For example, examples of other optical films having a surface unevenness include (A) styrene-methyl methacrylate copolymer resin particles having an average particle size of 1.0 to 3.0 μm and a refractive index of 1.50 to 1.54, (B) a curable compound having two or more curable groups in the molecule, (C) a smectite clay-organic complex obtained by intercalating a quaternary ammonium salt represented by the following general formula (1R) into a smectite clay, and (D) an antiglare film formed from a compound containing a volatile organic solvent, as described in Japanese Patent No. 5909454. General formula (1R) [(R 1 )3(R 2 )N] + X - (1R) (In the formula, R 1 and R 2 are not the same, R 1 represents an alkyl group, an alkenyl group, or an alkynyl group having 4 to 24 carbon atoms; R 2 represents an alkyl group, an alkenyl group, or an alkynyl group having 1 to 10 carbon atoms; X - represents an anion.) The other optical film having the above-mentioned surface irregularities may be attached using an adhesive, or only the surface irregularity layer described in Japanese Patent No. 5909454 may be coated on the outermost layer of the optical film of the present invention.

[0193] Another example of an optical film having surface irregularities is a film having a surface irregularity layer having a phase separation structure, which is formed of a polymer composed of a (meth)acrylic resin having a polymerizable group and a cellulose derivative, a curable resin precursor, and a cured product of a curable composition containing a fluorine-based leveling agent composed of a resin having a radical polymerizable group and a branched fluoroaliphatic hydrocarbon group, as described in Japanese Patent No. 6093153. The optical film may be bonded using an adhesive, or only the surface irregularity layer having a phase separation structure may be further coated on the optical film of the present invention.

[0194] The above-mentioned surface-convex film preferably has low internal scattering, and the internal haze is preferably 5% or less, more preferably 3% or less, and even more preferably 1% or less. By making the internal haze 5% or less, the narrowed viewing angle can be maintained by the optical film of the present invention, especially when used for privacy film applications.

[0195] <Image display device> The image display device of the present invention has the above-mentioned optical film of the present invention or the above-mentioned optical laminate of the present invention. The display element used in the image display device of the present invention is not particularly limited, and examples thereof include a liquid crystal cell, an organic electroluminescence (hereinafter abbreviated as "EL") display panel, and a plasma display panel. Among these, a liquid crystal cell or an organic EL display panel is preferred, and a liquid crystal cell is more preferred. That is, as the image display device of the present invention, a liquid crystal display device using a liquid crystal cell as a display element, and an organic EL display device using an organic EL display panel as a display element are preferred, and a liquid crystal display device is more preferred.

[0196] [Liquid crystal display device] A preferred embodiment of the liquid crystal display device, which is one example of the image display device of the present invention, is one having the optical film of the present invention described above and a liquid crystal cell. A more preferred embodiment of the liquid crystal display device is one having the optical laminate of the present invention described above (not including a λ / 4 plate) and a liquid crystal cell. In the present invention, it is preferable to use the optical laminate of the present invention as the front side polarizing element among the polarizing elements provided on both sides of the liquid crystal cell, and it is more preferable to use the optical laminate of the present invention as the front side and rear side polarizing elements. The liquid crystal cell constituting the liquid crystal display device will be described in detail below.

[0197] (Liquid crystal cell) The liquid crystal cell used in the liquid crystal display device is preferably in VA (Vertical Alignment) mode, OCB (Optically Compensated Bend) mode, IPS (In-Plane-Switching) mode, or TN (Twisted Nematic) mode, but is not limited to these. In a TN mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially horizontally when no voltage is applied, and further aligned in a twisted manner at an angle of 60 to 120°. TN mode liquid crystal cells are most commonly used as color TFT (Thin Film Transistor) liquid crystal display devices, and are described in many publications. In a VA mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied. VA mode liquid crystal cells include (1) a narrow-sense VA mode liquid crystal cell (described in JP-A-2-176625) in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and substantially horizontally when voltage is applied, (2) a VA mode multi-domain (MVA mode) liquid crystal cell (described in SID97, Digest of tech. Papers (Proceedings) 28 (1997) 845) in order to expand the viewing angle, (3) a mode (n-ASM mode) liquid crystal cell in which rod-shaped liquid crystal molecules are aligned substantially vertically when no voltage is applied and are aligned in a twisted multi-domain when voltage is applied (described in Proceedings of the Japan Liquid Crystal Discussion Society 58-59 (1998)), and (4) a SURVIVAL mode liquid crystal cell (announced at LCD International 98). The VA mode liquid crystal cell may be any of PVA (Patterned Vertical Alignment) type, optical alignment type, and PSA (Polymer-Sustained Alignment) type. Details of these modes are described in JP-A-2006-215326 and JP-A-2008-538819. In the IPS mode liquid crystal cell, rod-shaped liquid crystal molecules are aligned substantially parallel to the substrate, and the liquid crystal molecules respond in a planar manner when an electric field parallel to the substrate surface is applied. In the IPS mode, the black display is achieved when no electric field is applied, and the absorption axes of the pair of upper and lower polarizing plates are perpendicular to each other. Methods of reducing light leakage during black display in an oblique direction and improving the viewing angle using an optical compensation sheet are disclosed in JP-A-10-54982, JP-A-11-202323, JP-A-9-292522, JP-A-11-133408, JP-A-11-305217, JP-A-10-307291, etc.

[0198] [Organic EL display device] A suitable embodiment of an organic EL display device, which is one example of the image display device of the present invention, includes, from the viewing side, the above-mentioned polarizer of the present invention, a λ / 4 plate, and an organic EL display panel, in this order. More preferably, the optical laminate of the present invention having a λ / 4 plate and an organic EL display panel are arranged in this order from the viewing side. In this case, the optical laminate is arranged in the following order from the viewing side: a substrate, an alignment film, the polarizer of the present invention, a barrier layer that is provided if necessary, and the λ / 4 plate. The organic EL display panel is a display panel configured using an organic EL element having an organic light-emitting layer (organic electroluminescence layer) sandwiched between electrodes (cathode and anode). The configuration of the organic EL display panel is not particularly limited, and a known configuration may be adopted.

[0199] [Curved image display device] Examples of the curved image display device of the present invention are disclosed in JP-A-2017-181821, JP-A-2017-181819, JP-A-2017-102456, JP-A-2014-95901, and the like. EXAMPLES

[0200] The present invention will be specifically described below based on examples. The materials, reagents, amounts of substances and their ratios, operations, etc. shown in the following examples can be appropriately changed without departing from the spirit of the present invention. Therefore, the present invention is not limited to the following examples.

[0201] <Example 1> [Formation of alignment film] The surface of a cellulose acylate film (TAC substrate with a thickness of 40 μm; TG40, Fujifilm Corporation) was saponified with an alkaline solution, and the following composition for forming an alignment film 1 was applied thereon with a wire bar. The support on which the coating film was formed was dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds to form an alignment film AL1, and a TAC film 1 with an alignment film was obtained. The thickness of the alignment film AL1 was 1 μm.

[0202] ------------------------------------------------------------------ (Orientation film forming composition 1) ------------------------------------------------------------------ 3.80 parts by weight of modified polyvinyl alcohol PVA-1 (see below) ·IRGACURE 2959 0.20 parts by mass ·Water 70 parts by mass Methanol 30 parts by weight ------------------------------------------------------------------

[0203] Modified Polyvinyl Alcohol PVA-1 [ka]

[0204] [Formation of Optically Absorbing Anisotropic Layer P1] Onto the obtained TAC film 1 with the alignment layer, the following composition for forming an optically absorptive anisotropic layer P1 was continuously applied with a wire bar, heated at 120° C. for 60 seconds, and then cooled to room temperature (23° C.). It was then heated at 80° C. for 60 seconds and cooled again to room temperature. Then, an LED lamp (center wavelength 365 nm) was used, and the illuminance was 200 mW / cm 2 By irradiating the liquid crystal display for 2 seconds under the irradiation conditions, an optically absorptive anisotropic layer P1 was formed on the alignment film AL1. The optically absorptive anisotropic layer P1 had a thickness of 3.5 μm.

[0205] ------------------------------------------------------------------ Composition of optically absorptive anisotropic layer forming composition P1 ------------------------------------------------------------------ 0.63 parts by weight of the following dichroic substance D-1 0.17 parts by weight of the following dichroic substance D-2 1.13 parts by weight of the following dichroic substance D-3 8.18 parts by weight of the following polymeric liquid crystal compound P-1 IRGACURE OXE-02 (BASF) 0.16 parts by weight 0.12 parts by weight of the following compound E-1 0.12 parts by weight of the following compound E-2 0.005 parts by weight of the following surfactant F-1 Cyclopentanone 85.00 parts by mass Benzyl alcohol 4.50 parts by weight ------------------------------------------------------------------

[0206] Dichroic substance D-1 [ka]

[0207] Dichroic substance D-2 [ka]

[0208] Dichroic substance D-3 [ka]

[0209] Polymer liquid crystal compound P-1 [ka]

[0210] Compound E-1 [ka]

[0211] Compound E-2 [ka]

[0212] Surfactant F-1 [ka]

[0213] [Formation of color-adjusting layer C1] On the obtained light absorption anisotropic layer P1, the following composition C1 for forming a color adjusting layer was continuously applied with a wire bar to form a coating film. Next, the support on which the coating film was formed was dried with hot air at 60° C. for 60 seconds and then with hot air at 100° C. for 120 seconds to form a color-adjusting layer C1, and thus an optical film 1. The film thickness of the color-adjusting layer was 0.5 μm. ------------------------------------------------------------------ (Color Adjusting Layer Forming Composition C1) ------------------------------------------------------------------ 3.80 parts by weight of the modified polyvinyl alcohol PVA-1 ·IRGACURE 2959 0.20 parts by mass 0.08 parts by weight of the following dye compound G-1 ·Water 70 parts by mass Methanol 30 parts by weight ------------------------------------------------------------------

[0214] Pigment compound G-1 [ka]

[0215] [Preparation of optical laminate A1] Polarizing plate 1 having a polarizer with a thickness of 8 μm and one surface of the polarizer exposed was produced in the same manner as in polarizing plate 02 with a one-side protective film described in WO 2015 / 166991. The surface of the polarizing plate 1 on which the polarizer was exposed and the surface of the light absorption anisotropic layer of the prepared optical film 1 were subjected to a corona treatment, and then bonded together using the following PVA adhesive 1 to prepare an optical laminate A1.

[0216] (Preparation of PVA adhesive 1) 100 parts of a polyvinyl alcohol resin containing acetoacetyl groups (average degree of polymerization: 1200, degree of saponification: 98.5 mol%, degree of acetoacetylation: 5 mol%) was dissolved in pure water at a temperature of 30°C to prepare an aqueous solution with a solid content of 3.7%.

[0217] [Fabrication of image display device I1] An iPad Air (registered trademark) Wi-Fi model 16GB (manufactured by APPLE), which is an IPS mode liquid crystal display device, was disassembled and the liquid crystal cell was taken out. The viewer-side polarizing plate was peeled off from the liquid crystal cell, and the optical laminate A1 prepared above was attached to the surface from which the viewer-side polarizing plate was peeled off, with the polarizing plate 1 side facing the liquid crystal cell side, using the following adhesive sheet 1. At this time, the polarizing plate 1 was attached so that the direction of the absorption axis was the same as the absorption axis of the viewer-side polarizing plate attached to the product. After lamination, the product was reassembled to prepare an image display device I1.

[0218] (Preparation of adhesive sheet 1) The acrylate-based polymer was prepared according to the following procedure. In a reaction vessel equipped with a cooling tube, a nitrogen inlet tube, a thermometer, and a stirrer, 95 parts by mass of butyl acrylate and 5 parts by mass of acrylic acid were mixed and polymerized by a solution polymerization method to obtain an acrylate polymer PL1 having an average molecular weight of 2,000,000 and a molecular weight distribution (Mw / Mn) of 3.0.

[0219] Next, in addition to the obtained acrylate-based polymer PL1 (100 parts by mass), Coronate L (a 75% by mass ethyl acetate solution of trimethylolpropane adduct of tolylene diisocyanate, number of isocyanate groups in one molecule: 3, manufactured by Nippon Polyurethane Industry Co., Ltd.) (1.0 part by mass), and a silane coupling agent KBM-403 (manufactured by Shin-Etsu Chemical Co., Ltd.) (0.2 parts by mass) were mixed, and finally ethyl acetate was added so that the total solid concentration was 10% by mass to prepare a composition for forming an adhesive. This composition was applied to a separate film surface-treated with a silicone-based release agent using a die coater and dried for 1 minute in an environment of 90 ° C. to obtain an acrylate-based adhesive sheet. The thickness of the adhesive sheet was 25 μm, and the storage modulus was 0.1 MPa.

[0220] <Example 2> An optical film 2 of Example 2 was produced in the same manner as in Example 1, except that in the optical film 1 of Example 1, the color-adjusting layer-forming composition C1 was changed to the color-adjusting layer-forming composition C2. ------------------------------------------------------------------ (Color Adjusting Layer Forming Composition C2) ------------------------------------------------------------------ 3.80 parts by weight of the modified polyvinyl alcohol PVA-1 ·IRGACURE 2959 0.20 parts by mass 0.01 parts by weight of the following dye compound G-2 ·Water 70 parts by mass Methanol 30 parts by weight ------------------------------------------------------------------

[0221] Pigment compound G-2 [ka]

[0222] <Example 3> An optical film 3 was produced in the same manner as in Example 1, except that a composition for forming an optically absorptive anisotropic layer P2 was used in which the dichroic material D-3 in the composition for forming an optically absorptive anisotropic layer P1 in Example 1 was changed to the dichroic material D-4.

[0223] Dye compound D-4 [ka]

[0224] <Example 4> An optical film 4 was produced in the same manner as in Example 1, except that the optically absorptive anisotropic layer-forming composition P1 of Example 1 was replaced with the optically absorptive anisotropic layer-forming composition P3. ------------------------------------------------------------------ Composition of the optically absorptive anisotropic layer forming composition P3 ------------------------------------------------------------------ 0.63 parts by weight of the above dichroic substance D-1 0.17 parts by weight of the above dichroic substance D-2 1.13 parts by weight of the following dichroic substance D-5 5.45 parts by weight of the following liquid crystal compound L-1 2.72 parts by weight of the following liquid crystal compound L-2 IRGACURE OXE-02 (BASF) 0.16 parts by weight 0.12 parts by weight of the above compound E-1 0.12 parts by weight of the above compound E-2 0.005 parts by weight of the above surfactant F-1 Cyclopentanone 85.00 parts by mass Benzyl alcohol 4.50 parts by weight ------------------------------------------------------------------

[0225] Dichroic substance D-5 [ka]

[0226] Liquid crystal compound L-1 [ka]

[0227] Liquid crystal compound L-2 [ka]

[0228] <Example 5> An optical film 5 was produced in the same manner as in Example 1, except that in the optical film 1 of Example 1, the color-adjusting layer-forming composition C1 was changed to the color-adjusting layer-forming composition C3. ------------------------------------------------------------------ (Color adjustment layer forming composition C3) ------------------------------------------------------------------ 3.80 parts by weight of the modified polyvinyl alcohol PVA-1 ·IRGACURE 2959 0.20 parts by mass 0.16 parts by weight of the following dye compound G-3 ·Water 70 parts by mass Methanol 30 parts by weight ------------------------------------------------------------------

[0229] Pigment compound G-3 [ka]

[0230] <Comparative Example 1> Optical film 6 was produced in the same manner as in Example 1, except that in the optical film 1 of Example 1, no color-adjusting layer was provided.

[0231] <Comparative Example 2> Optical film 7 was prepared in the same manner as in optical film 6 of Comparative Example 1, except that the composition for forming an optically absorptive anisotropic layer in Comparative Example 1 was changed to the following P4. ------------------------------------------------------------------ Composition of optically absorptive anisotropic layer forming composition P4 ------------------------------------------------------------------ 0.75 parts by weight of the dichroic substance D-1 0.34 parts by weight of the above dichroic substance D-2 1.13 parts by weight of the above dichroic substance D-3 7.88 parts by weight of the polymer liquid crystal compound P-1 IRGACURE OXE-02 (BASF) 0.16 parts by weight 0.12 parts by weight of the above compound E-1 0.12 parts by weight of the above compound E-2 0.005 parts by weight of the above surfactant F-1 Cyclopentanone 85.00 parts by mass Benzyl alcohol 4.50 parts by weight ------------------------------------------------------------------

[0232] <Comparative Example 3> Optical film 8 was produced in the same manner as in Example 3, except that in the optical film 3 of Example 3, no color-adjusting layer was provided.

[0233] <Example 6> [Formation of photo-alignment layer] In the same manner as in Example 1, a TAC film 1 with an alignment layer was prepared, and the following composition liquid E1 for forming a photoalignment layer was applied onto the alignment layer AL1 and dried at 60° C. for 2 minutes. Thereafter, the resulting coating film was exposed to ultraviolet light (irradiation dose 2000 mJ / cm 2 ) using an ultraviolet light exposure device. 2) was irradiated from a direction at a polar angle of 15° with respect to the film normal direction as a reference, to produce a photo-alignment layer E1 with a thickness of 0.03 μm.

[0234] [Preparation of composition liquid E1 for forming photo-alignment layer] A composition liquid E1 for forming a photo-alignment layer was prepared with the following composition, and dissolved for 1 hour while stirring. After dissolution, the solution was filtered through a 0.45 μm filter to obtain a photoalignment layer forming composition liquid E1. ---------------------------------------------------------------------------------- Composition liquid E1 for forming photo-alignment layer ---------------------------------------------------------------------------------- 0.3 parts by weight of the following photoalignment material E-3 2-Butoxyethanol 41.6 parts by weight Dipropylene glycol monomethyl ether 41.6 parts by weight ·Pure water 16.5 parts by mass ----------------------------------------------------------------------------------

[0235] Photo-alignment material E-3 [ka]

[0236] [Formation of optically absorptive anisotropic layer P9] Onto the obtained photoalignment layer E1, the composition for forming an optically absorptive anisotropic layer P1 was continuously applied with a wire bar, heated at 120° C. for 60 seconds, and then cooled to room temperature (23° C.). It was then heated at 80° C. for 60 seconds and cooled again to room temperature. After that, an LED lamp (center wavelength 365 nm) was used to illuminate the sample at an intensity of 200 mW / cm 2 By irradiating the liquid crystal display AL1 for 2 seconds under the irradiation conditions described above, an optically absorptive anisotropic layer P9 was formed on the alignment film AL1. The optically absorptive anisotropic layer P9 had a thickness of 3.5 μm. The angle between the central axis of transmittance of the optically absorptive anisotropic layer P9 and the normal to the film was 15 degrees.

[0237] [Formation of color-adjusting layer C9] On the obtained light absorption anisotropic layer P9, the color adjusting layer forming composition C1 was applied, and an optical film 9 was obtained in the same manner as in Example 1.

[0238] <Examples 7 to 10> Optical films 10 to 13 were produced in the same manner as in Example 1, except that in the optical film 1 of Example 1, the thickness d(C) of the color-adjusting layer was changed and the value represented by c(C)×d(C)) / (c(P)×d(P) in the above formula (7) was adjusted to the values ​​shown in Table 2.

[0239] <Example 11> In the optical film 1 of Example 1, after forming the light absorbing anisotropic layer P1, an alignment film was formed again using the composition 1 for forming an alignment film in the same manner as the alignment film AL1, and then the composition C1 for forming a color adjusting layer was changed to the composition C4 for forming a color adjusting layer. In the same manner as in Example 1, the optical film 14 of Example 11 was produced. ------------------------------------------------------------------ (Color adjustment layer forming composition C4) ------------------------------------------------------------------ 1.13 parts by weight of the above dichroic substance D-3 9.22 parts by weight of the polymer liquid crystal compound P-1 IRGACURE OXE-02 (BASF) 0.16 parts by weight Surfactant F-1 0.005 parts by weight Cyclopentanone 85.00 parts by mass Benzyl alcohol 4.50 parts by weight ------------------------------------------------------------------

[0240] <Evaluation> [Evaluation of the degree of orientation] (Light absorption anisotropic layer) The degree of orientation of the obtained optically absorptive anisotropic layer at a wavelength of 550 nm was calculated by the following method. During the measurement, the polar angle, which is the angle with respect to the normal direction of the light absorbing anisotropic layer, was changed from 0 to 90° in 5° increments, and the Mueller matrix at a wavelength of 550 nm was measured at each polar angle to derive the minimum transmittance (Tmin). Next, after removing the influence of surface reflection, Tmin at the polar angle at which Tmin is highest is defined as Tm(0), and Tmin at the direction 40° larger than the polar angle at which Tmin is highest is defined as Tm(40). The absorbance (A) was calculated from the obtained Tm(0) and Tm(40) using the following formula, and A(0) and A(40) were calculated. A = -log(Tm) Here, Tm represents the transmittance and A represents the absorbance. From the calculated A(0) and A(40), the degree of orientation S at a wavelength of 550 nm is defined by the following formula: P was calculated. S P =(4.6×A(40)-A(0)) / (4.6×A(40)+2×A(0)) By changing the wavelength from 550 nm to 420 nm or 650 nm, the degree of orientation S at the wavelengths of 420 nm and 650 nm P was calculated.

[0241] (Color adjustment layer) From the obtained optical film, only the color-adjusting layer was transferred onto a cellulose acylate film (TAC substrate having a thickness of 40 μm; TG40, Fujifilm Corporation) via an adhesive. C Using this transferred film, the optical absorption anisotropy was measured in the same manner as for the optical absorption anisotropic layer.

[0242] [Transmittance and color evaluation] The image display device I1 thus produced was measured using a measuring device (EZ-Contrast XL88, manufactured by ELDIM) to measure the luminance Y(0)A1 of the transmittance central axis of the white display screen, the luminance Y(30)A1 in a direction shifted by 30° from the transmittance central axis (diagonal direction) on the plane between the transmittance central axis and the film normal, and the color tone a of the transmittance central axis. * (0) A1, b *(0) A1, color tone a in the direction shifted 30° from the central axis of transmittance on the plane between the central axis of transmittance and the film normal * (30) A1, b * (30)A1 was measured. In addition, in the preparation of the image display device I1, an image display device B was prepared in the same manner as in Example 1, except that an optical laminate without a light absorbing anisotropic layer was attached to the liquid crystal cell, and the luminance Y(0)B of the white display screen at a polar angle of 0° (front direction) was measured in the same manner as described above. The front transmittance T(0) was calculated by comparing with the luminance of the image display device B without a light absorbing anisotropic layer. Specifically, the calculation was performed using the following formula. T(0)=Y(0)A1 / Y(0)B The transmittance and color were evaluated according to the following evaluation criteria.

[0243] (Transmittance evaluation criteria) A:T(0) is 75% or more B: T(0) is 65% or more but less than 75% C:T(0) is less than 65%

[0244] (Color evaluation criteria) A:|a * (0)| is less than 3 B:|a * (0)| is 3 or more but less than 5 C:|a * (0)| is 5 or more Also, b * (0), a * (30), and b * (30) was evaluated in the same manner.

[0245] Further, image display devices I2 to I8 were produced by replacing the optical film 1 with the optical films 2 to 8, respectively, and the transmittance and color were evaluated in the same manner.

[0246] The evaluation results are shown in Table 1.

[0247] In Table 1, "polar angle" represents the angle of the central axis of transmittance of the optical film with respect to the normal direction of the optical film. In Table 1, the "A" notation in the "Orientation" column indicates the above method. 420 The degree of orientation of the color-adjusting layer measured at 550 nm, 650 nm, and 750 nm S C However, all of the above were less than 0.1. In other words, the "A" in the "Orientation degree" column indicates that all of the above requirements 1 to 3 are satisfied. In addition, in Table 1, the "B" in the "Orientation degree of color-adjusting layer" column indicates that 420 The degree of orientation of the color-adjusting layer measured at 550 nm, 650 nm, and 750 nm S C This indicates that either of the above was 0.1 or greater. In Table 1, “S P ( 420 )," "S P (550)" and "S P (650)" are 420 The results show the degree of orientation of the optical film measured at 550 nm, 550 nm, and 650 nm. In Table 1, “S P ( 420 ) P (550)" and "S P ( 420 ) P The "A" notation in the "(650)" column indicates that the inequality holds, and the "B" notation indicates that the inequality does not hold. P ( 420 ) P (550)" and "S P ( 420 ) P (650)" corresponds to the above formulas (1) and (2), respectively.

[0248] [Table 1]

[0249] Comparing the results of the Examples and Comparative Examples in Table 1, it was confirmed that the optical films of the Examples were excellent in wide-angle color suppression. Comparing the results of the Examples in Table 1, it was confirmed that when the light absorptive anisotropic layer satisfies the above formulas (1) and (2), the optical film has superior transmittance.​​​​ From Table 1, it was confirmed that when at least one of the dichroic dye compounds contained in the light absorption anisotropic layer is a dichroic dye compound represented by the above formula (3), the optical film has superior transmittance. From Table 1, it was confirmed that when the color-adjusting layer satisfies the above requirements 1 to 3, the optical film has superior wide-angle color suppression properties. It was confirmed from Table 1 that when the absorption peak wavelength of the organic colorant compound contained in the color-adjusting layer is 500 to 650 nm, the optical film has superior wide-angle color suppression properties.

[0250] Table 2 shows the results of evaluation of Examples 1, 7 to 10, and Comparative Example 1 with respect to the above formula (7) and color tone. The degree of orientation of the color-adjusting layer was 0 when measured at any of 420 nm, 550 nm, and 650 nm. In Table 2, the notation "(c(C)×d(C)) / (c(P)×d(P))" is the value corresponding to the above formula (7).

[0251] [Table 2]

[0252] From Table 2, it was confirmed that when the optical film satisfies the above formula (7), the optical film has superior wide-angle color suppression properties.

[0253] (Confirmation of suitability for curved surface processing) [Suitability for curved surface processing] The optical laminate A1 produced in Example 1 was attached to the display screen of a smartphone (Galaxy Note9, manufactured by Samsung) having a curved surface, with the optical film 1 side facing the display screen, using a commercially available adhesive SK2057 (manufactured by Soken Chemical & Engineering Co., Ltd.) The optical laminate A1 had a film thickness of 100 μm or less and was highly flexible, and could be neatly attached to the curved surface of the display screen without any air bubbles. Next, a louver-type optical film (3M (trademark) Security / Privacy Filter PF12 H2 series) that has the same performance as the optical film of the present invention and is widely used on the market was attached to the display screen of the smartphone using a commercially available adhesive SK2057 (manufactured by Soken Chemical Industries, Ltd.) The louver-type optical film had a thickness of 500 μm and low flexibility, and air bubbles were trapped in the curved parts of the display screen, making it impossible to attach it neatly.

[0254] [Evaluation of patterned products] An optically absorptive anisotropic layer having the above-mentioned patterns of region A and region B was prepared as follows and evaluated.

[0255] (Formation of patterned light absorbing anisotropic layer) The optically absorptive anisotropic layer-forming composition P1 was continuously applied onto the alignment film AL1 of Example 1 with a wire bar to form a coating layer P1. Next, the coating layer P1 was heated at 140° C. for 30 seconds, and then cooled to room temperature (23° C.). It was then heated at 80° C. for 60 seconds and cooled again to room temperature. Then, light emitted from a high-pressure mercury lamp was passed through a mask at an illuminance of 28 mW / cm 2 By irradiating for 60 seconds under the irradiation conditions, a light absorbing anisotropic layer having a cured region and an uncured region of the liquid crystal compound in the plane was produced on the alignment film AL1. The mask had a mask pattern having a rectangular light transmitting region of 10 mm length x 50 mm width as region A, a light shielding region (region B) and a light transmitting region. The film having a polarizing layer with a cured region (region A) and an uncured region (region B) of the liquid crystal compound within the plane thus prepared was immersed in ethanol for 3 minutes to wash and remove the unpolymerized liquid crystal compound, thereby forming a patterned optical film 10 having a patterned light absorption anisotropic layer having regions A and B with different polarization degrees within the plane. Region A had a polar angle 30° transmittance of 10% or less and a front transmittance of 80% or more. Region B had both a polar angle 30° transmittance and a front transmittance of 80% or more. -Preparation of optical laminate A10- The surface of the polarizing plate 1 on which the polarizer was exposed and the surface of the light absorption anisotropic layer of the patterned optical film 10 prepared above were bonded together using the pressure-sensitive adhesive sheet 1 to prepare an optical laminate A10.

[0256] -Production of image display device I10- An image display device I10 was produced in the same manner as the image display device I1, except that the optical laminate A1 was replaced with the optical laminate A10. Only the area A had a narrow viewing angle and was clearly visible only from the front.

[0257] [Evaluation of surface textured products] The optical laminate having the above-mentioned surface irregularities was produced and evaluated as follows.

[0258] (Production of image display device I11) In order to impart a surface roughness of Ra 90 nm, the surface roughness film described in Example 3 of Japanese Patent No. 6093153 was attached to the exposed polarizer surface of the polarizing plate 1 using the above-mentioned adhesive sheet 1 to produce an optical laminate A11. An image display device I11 was produced in the same manner as the image display device I1, except that the optical laminate A1 was changed to the optical laminate A11.

[0259] (Production of image display device I12) In order to impart a surface roughness of Ra 50 nm, the surface roughness film described in Example 101 of Japanese Patent No. 5,909,454 was attached to the exposed polarizer surface of the polarizing plate 1 using the above-mentioned adhesive sheet 1 to produce an optical laminate A12. An image display device I12 was produced in the same manner as the image display device I1, except that the optical laminate A1 was changed to the optical laminate A12.

[0260] (Production of image display device I13) In order to impart a surface roughness of Ra 130 nm, the surface roughness film described in Example 7 of Japanese Patent No. 6,093,153 was attached to the exposed polarizer surface of polarizing plate 1 using the above-mentioned adhesive sheet 1 to produce optical laminate A13. An image display device I13 was produced in the same manner as the image display device I1, except that the optical laminate A1 was changed to the optical laminate A13.

[0261] (Evaluation: Anti-blocking property) For each optical laminate of the Examples, the adhesion when the outermost surfaces of the optical laminates were bonded together was evaluated according to the following criteria. The bonded optical laminates are optical laminates of the same Example. For example, the optical laminate A1 was obtained by bonding two optical laminates A1 together. By bonding optical laminates of the same Example together in this way and evaluating them, the anti-blocking property of the optical laminate can be evaluated more accurately without being affected by the physical properties of the other surfaces to be bonded, compared to the case where the anti-blocking property is evaluated by bonding them to other surfaces. The anti-blocking property was evaluated according to the following evaluation criteria.

[0262] -Evaluation criteria for anti-blocking properties- A: There is no sticking feeling at all. B: Almost no sticking feeling. C: Strong adhesion.

[0263] (Evaluation: Narrow viewing angle) For each image display device of the Examples, the narrow viewing angle property when viewed from the front and when viewed tilted 20 degrees to the side was evaluated according to the following criteria.

[0264] - Evaluation criteria for narrow viewing angle - A: There is a clear difference in visibility from the front and at an angle. B: There is a clear difference in visibility between the front and diagonal directions. C: It can be seen from an angle.

[0265] The evaluation results of the anti-blocking properties of the optical laminates A1, A11, A12, and A13, and the narrow viewing angle properties of the image display devices I1, I11, I12, and I13 are shown in Table 3 as Examples 1, 11, 12, and 13, respectively. [Table 3]

[0266] From Table 3, it was confirmed that when the arithmetic surface roughness Ra of the surface irregularities of the optical laminate of the present invention is 50 nm or more, the anti-blocking property when the films are laminated is superior. On the other hand, it was confirmed that when the arithmetic surface roughness Ra of the surface irregularities is less than 130 nm, the narrow viewing angle property is superior.

Claims

1. The present invention has a light absorbing anisotropic layer having an angle θ between a transmittance central axis and a normal direction of the layer surface of 0 to 45°, and a color adjusting layer containing at least one organic dye compound, the light absorption anisotropic layer contains a liquid crystal compound and at least one dichroic dye compound, The optically absorptive anisotropic layer satisfies both of the following formulas (1) and (2): An optical film satisfying the following formula (7): S P (420 nm) <S P (550nm) Formula (1) S P (420 nm) <S P (650nm) Formula (2) However, S P (λ nm) represents the degree of orientation of the optically absorptive anisotropic layer measured at a wavelength of λ nm. 0.005≦(c(C)×d(C)) / (c(P)×d(P))≦0.06 Formula (7) In the formula (7), c(C) represents the mass ratio of the organic dye compound in the color-adjusting layer to the total mass of the color-adjusting layer. In the formula (7), d(C) represents the film thickness (μm) of the color-adjusting layer. In the formula (7), c(P) represents the mass ratio of the dichroic dye compound in the optically absorptive anisotropic layer to the total mass of the optically absorptive anisotropic layer. In the formula (7), d(P) represents the film thickness (μm) of the optically absorptive anisotropic layer.

2. The optical film according to claim 1 , wherein at least one of the dichroic dye compounds contained in the light absorption anisotropic layer is represented by the following formula (3): [Formula 1] In the formula (3), A 4 represents a divalent aromatic group which may have a substituent. In the formula (3), L 3 and L 4 each independently represents a substituent. In the formula (3), E represents any one of a nitrogen atom, an oxygen atom, and a sulfur atom. In the formula (3), R 1 represents a hydrogen atom, a halogen atom, an alkyl group which may have a substituent, or an alkoxy group which may have a substituent. In the formula (3), R 2 represents a hydrogen atom or an alkyl group which may have a substituent. In the formula (3), R 3 represents a hydrogen atom or a substituent. In the formula (3), n represents 0 or 1. However, when E is a nitrogen atom, n is 1, and when E is an oxygen atom or a sulfur atom, n is 0.

3. 3. The optical film according to claim 1, wherein the color-adjusting layer satisfies any one of the following requirements 1 to 3, satisfies two of the following requirements 1 to 3, or satisfies all of the following requirements 1 to 3. Requirement 1: S C (420nm)<0.1 Requirement 2: S C (550nm)<0.1 Requirement 3: S C (650nm)<0.1 However, S C (λ nm) represents the degree of orientation of the color-adjusting layer measured at a wavelength of λ nm.

4. 4. The optical film according to claim 1, wherein the organic dye compound contained in the color-adjusting layer has an absorption peak wavelength of 500 to 650 nm.

5. 5. The optical film according to claim 1, wherein the organic colorant compound contained in the color-adjusting layer has at least one of a benzene ring and a heterocyclic ring structure in the molecule.

6. 6. The optical film according to claim 1, wherein the organic dye compound contained in the color-adjusting layer has an anthraquinone structure.

7. 7. The optical film according to claim 1, wherein the transmittance of light having a wavelength of 550 nm in a direction along the central transmittance axis is 65% or more.

8. 8. An optical laminate comprising the optical film according to claim 1 and a polarizer layer in which a dichroic material is oriented horizontally to the film surface.

9. An optical laminate comprising the optical film according to any one of claims 1 to 7 and a concave-convex layer having an arithmetic mean roughness Ra of 35 to 125 nm.

10. An image display device comprising the optical film according to any one of claims 1 to 7, or the optical laminate according to claim 8 or 9.

Citation Information

Patent Citations

  • Viewing angle control system and image display device

    JP2009145776A

  • Light absorption anisotropic film, three-dimensional light absorption anisotropic film, and manufacturing method of the same

    JP2016027387A

  • Laminate and article

    JP2018045175A

  • Metal-containing polyazo dyestuffs

    US3005814A

Cited By

  • Optical film, optical laminate, and image display device

    JP2024103795A

  • Optical film, optical laminate, and image display device

    US12668744B2