Anti-glare hard-coated film, method for producing anti-glare hard-coated film, optical member and image display device
The anti-glare hard coat film addresses glare and display unevenness by controlling particle sizes and surface texture, enhancing image clarity in outdoor environments.
Patent Information
- Application Number
- JP2020018382
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-02-05
- Publication Date
- 2024-10-28
- Estimated Expiration
- 2040-02-05
AI Technical Summary
Anti-glare hard coat films used in image display devices suffer from glare due to external light reflection and display unevenness, such as streaks and lateral bumps, especially when used outdoors, which can make images difficult to view.
An anti-glare hard coat film with a resin layer containing first and second particles, where the weight average particle diameters and surface irregularities are controlled to suppress reflections and prevent streaks and bumps, achieved by applying a coating solution onto a light-transmitting substrate and curing it to form a specific surface texture.
The film effectively suppresses reflections and prevents streaks and lateral bumps, ensuring clear image visibility even in outdoor conditions, maintaining high-quality display performance.
Smart Images

Figure 0007573969000003 
Figure 0007573969000001 
Figure 0007573969000002
Abstract
Description
[Technical field]
[0001] The present invention relates to a hard-coated antiglare film, a method for producing the hard-coated antiglare film, an optical member, and an image display device. [Background technology]
[0002] Various image display devices, such as cathode ray tube displays (CRT), liquid crystal displays (LCD), plasma display panels (PDP) and electroluminescence displays (ELD), are subjected to anti-glare treatment to prevent contrast reduction caused by reflection of external light, such as fluorescent lamps and sunlight, and glare of images on the surface of the image display device. In particular, as the screen size of image display devices increases, the number of image display devices equipped with anti-glare films is increasing.
[0003] There are many documents describing antiglare films, such as Patent Document 1. As an antiglare film, an antiglare hard-coated film in which the antiglare layer also serves as a hard-coat layer is also used. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2004-110461 A Summary of the Invention [Problem to be solved by the invention]
[0005] From the viewpoint of visibility, the hard-coated antiglare film must be able to suppress glare caused by reflection of external light.
[0006] For example, in recent years, the demand for public information displays (PIDs) has been increasing. PIDs are often used outdoors. When a display (image display device) is used outdoors, glare due to reflection of external light is more likely to occur than when it is used indoors. When glare occurs, it may become difficult to see the image.
[0007] In addition, antiglare hard-coated films are often produced by continuously coating a coating liquid (antiglare hard-coat layer-forming material) on a long substrate while the substrate is being transported. However, when an antiglare hard-coated film produced in this manner is used in an image display device, display unevenness may occur. The display unevenness may be, for example, a striped pattern (hereinafter sometimes referred to as "streaks") in the transport direction of the substrate (the longitudinal direction of the substrate, hereinafter sometimes referred to as "MD direction"), and a striped pattern (hereinafter sometimes referred to as "horizontal stripes") in a direction perpendicular to the MD direction (hereinafter sometimes referred to as "TD direction"). Such display unevenness is more likely to occur when the distance over which the antiglare hard-coat layer-forming material is continuously coated is long.
[0008] Therefore, an object of the present invention is to provide an anti-glare hard-coated film in which reflection is suppressed and streaks and horizontal dents are suppressed or prevented, a method for producing the anti-glare hard-coated film, an optical member, and an image display device. [Means for solving the problem]
[0009] In order to achieve the above object, the antiglare hard-coated film of the present invention comprises: An antiglare hard-coated film comprising an antiglare hard-coat layer (B) laminated on a light-transmitting substrate (A), the antiglare hard coat layer (B) is formed of a resin layer, and contains first particles and second particles inside the resin layer, a total mass of the first particles and the second particles is 2 to 25% by mass with respect to a total mass of a resin forming the resin layer, The antiglare hard coat film has an outermost surface on the side of the antiglare hard coat layer (B) formed with irregularities, The weight average particle diameter of the first particles satisfies the following formula (1), The weight average particle diameter of the second particles satisfies the following formula (2), The uneven shape of the outermost surface is characterized in satisfying the following mathematical expressions (3) and (4). 3.0 <d1≦8.5[μm] (1) 1.0≦d2≦3.0[μm] (2) Ry: 1.0≦Ry≦7.0 [μm] (3) θa: 1.0≦θa≦7.5[°] (4) In the formula (1), d1 is the weight average particle diameter [μm] of the first particles, In the formula (2), d2 is the weight average particle diameter [μm] of the second particles, In the formula (3), Ry is the maximum height [μm] of the convex portion of the concave-convex portion, In the formula (4), θa is the average inclination angle [°] of the irregularities.
[0010] The method for producing the antiglare hard-coated film of the present invention includes the steps of: The method includes forming the antiglare hard coat layer (B) on the light-transmitting substrate (A) so as to satisfy the formulas (1) to (4), the antiglare hard coat layer (B) forming step includes a coating step of applying a coating liquid onto the light-transmitting substrate (A), and a coating film forming step of drying the applied coating liquid to form a coating film, The method for producing the hard-coated antiglare film of the present invention is characterized in that the coating liquid contains the resin, the first particles, the second particles, and a solvent.
[0011] The optical member of the present invention is an optical member that includes the hard-coated antiglare film of the present invention.
[0012] The image display device of the present invention is an image display device that includes the hard-coated antiglare film of the present invention or the optical member of the present invention. Effect of the Invention
[0013] According to the present invention, it is possible to provide an antiglare hard-coated film in which reflection is suppressed and streaks and horizontal dents are suppressed or prevented, a method for producing the antiglare hard-coated film, an optical member, and an image display device. [Brief description of the drawings]
[0014] [Figure 1] FIG. 1 is a cross-sectional view showing an example of the hard-coated antiglare film of the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0015] Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the following description in any way.
[0016] In the antiglare hard-coated film of the present invention, for example, the total mass of the second particles may be 1% by mass or more relative to the total mass of the resin forming the resin layer. In the present invention, "weight" and "mass" may be read as interchangeable unless otherwise specified. For example, "parts by mass" may be read as "parts by weight", "parts by weight" may be read as "parts by weight", "% by mass" may be read as "% by weight", and "% by weight" may be read as "% by mass".
[0017] The hard-coated antiglare film of the present invention may have an external haze value caused by the unevenness of 5% or more, for example.
[0018] In the hard-coated antiglare film of the present invention, for example, the total mass of the first particles may be ⅔ or more of the total mass of the second particles.
[0019] In the hard-coated antiglare film of the present invention, for example, another layer may be further laminated on the surface of the hard-coated antiglare layer (B) opposite to the light-transmitting substrate (A).
[0020] The antiglare hard-coated film of the present invention may be, for example, such that the antiglare hard-coat layer (B) and the other layer are laminated in the above-mentioned order on the light-transmitting substrate (A), and unevenness is formed on the outermost surface of the other layer, and the unevenness satisfies the above-mentioned mathematical expressions (1) to (4).
[0021] In the method for producing the hard-coated antiglare film of the present invention, for example, in the coating step, the coating liquid may be continuously coated over a width of 1000 mm or more and a length of 500 m or more.
[0022] In the method for producing the hard-coated antiglare film of the present invention, for example, the step of forming the hard-coated antiglare layer (B) may further include a curing step of curing the coating film.
[0023] The optical member of the present invention may be, for example, a polarizing plate.
[0024] The image display device of the present invention may be, for example, a public information display.
[0025] [1. Anti-glare hard coat film] As described above, the antiglare hard-coated film of the present invention has An antiglare hard-coated film comprising an antiglare hard-coat layer (B) laminated on a light-transmitting substrate (A), the antiglare hard coat layer (B) is formed of a resin layer, and contains first particles and second particles inside the resin layer, a total mass of the first particles and the second particles is 2 to 25% by mass with respect to a total mass of a resin forming the resin layer, The antiglare hard coat film has an outermost surface on the side of the antiglare hard coat layer (B) formed with irregularities, The weight average particle diameter of the first particles satisfies the following formula (1), The weight average particle diameter of the second particles satisfies the following formula (2), The uneven shape of the outermost surface is characterized in satisfying the following mathematical expressions (3) and (4). 3.0 <d1≦8.5[μm] (1) 1.0≦d2≦3.0[μm] (2) Ry: 1.0≦Ry≦7.0 [μm] (3) θa: 1.0≦θa≦7.5[°] (4) In the formula (1), d1 is the weight average particle diameter [μm] of the first particles, In the formula (2), d2 is the weight average particle diameter [μm] of the second particles, In the formula (3), Ry is the maximum height [μm] of the convex portion of the concave-convex portion, In the formula (4), θa is the average inclination angle [°] of the irregularities.
[0026] The cross-sectional view of FIG. 1 shows an example of the configuration of the antiglare hard-coated film of the present invention. As shown in the figure, this antiglare hard-coated film 10 has an antiglare hard-coated layer (B) 12 laminated on one surface of a light-transmitting substrate (A) 11. The antiglare hard-coated layer (B) 12 contains first particles 12b1 and second particles 12b2 in a resin layer 12a. The outermost surface of the antiglare hard-coated film 10 on the side of the antiglare hard-coated layer (B) 12 (the surface of the antiglare hard-coated layer (B) 12 opposite the light-transmitting substrate (A) 11) has unevenness formed thereon. The maximum height Ry of the convex portion of the unevenness is 1.0 μm or more and 7.0 μm or less. The average inclination angle θa of the unevenness is 1.0° or more and 7.5° or less. The weight-average particle diameter d1 of the first particles 12b1 is more than 3.0 μm and 8.5 μm or less. The weight average particle diameter d2 of the second particles 12b2 is not less than 1.0 μm and not more than 3.0 μm.
[0027] FIG. 1 is merely an example, and the present invention is not limited thereto. For example, the antiglare hard-coated film of the present invention may or may not contain other fillers (filling materials) other than the first particles 12b1 and the second particles 12b2 in the resin layer 12a. Examples of the other fillers include, but are not limited to, thixotropic agents, various metal oxide particles for adjusting the refractive index, and antiblocking properties. The antiglare hard-coated layer (B) 12 may be directly laminated on the light-transmitting substrate (A) 11 without any other layer as shown in FIG. 1, or may be laminated on the light-transmitting substrate (A) 11 via one or two or more other layers. The antiglare hard-coated layer (B) 12 may not have any other layer on the surface opposite to the light-transmitting substrate (A) 11 as shown in FIG. 1, but may have one or more other layers laminated thereon.
[0028] In the antiglare hard-coated film of the present invention, the "outermost surface on the antiglare hard-coat layer (B) side" is the outermost surface on the antiglare hard-coat layer (B) side. Specifically, when the other layer is not present on the surface of the antiglare hard-coat layer (B) 12 opposite the light-transmitting substrate (A) 11 (for example, FIG. 1), the "outermost surface on the antiglare hard-coat layer (B) side" is the surface of the antiglare hard-coat layer (B) opposite the light-transmitting substrate (A). In addition, when the other layer is present on the surface of the antiglare hard-coat layer (B) 12 opposite the light-transmitting substrate (A) 11, the "outermost surface on the antiglare hard-coat layer (B) side" is the outermost surface of the other layer opposite the light-transmitting substrate (A).
[0029] As described above, the antiglare hard-coated film of the present invention suppresses reflection, and suppresses or prevents streaks and horizontal dents. Specifically, for example, the antiglare hard-coated film of the present invention can prevent reflection of external light outdoors. In addition, the antiglare hard-coated film of the present invention has high-quality display performance because streaks and horizontal dents are suppressed or prevented. In addition, the antiglare hard-coated film of the present invention can be produced, for example, by continuously applying a coating liquid (antiglare hard-coated layer (B) forming material) onto the long light-transmitting substrate (A). That is, even with such a production method, the antiglare hard-coated film of the present invention in which reflection is suppressed and streaks and horizontal dents are suppressed or prevented can be produced.
[0030] Hereinafter, the light-transmitting substrate (A), the antiglare hard coat layer (B) and the other layers will be further described with examples.
[0031] The light-transmitting substrate (A) is not particularly limited, and examples thereof include transparent plastic film substrates. The transparent plastic film substrate is not particularly limited, and is preferably one having excellent visible light transmittance (preferably 90% or more light transmittance) and excellent transparency (preferably 1% or less haze value), and examples thereof include the transparent plastic film substrates described in JP-A-2008-90263. As the transparent plastic film substrate, one having optically low birefringence is preferably used. The antiglare hard coat film of the present invention can be used, for example, as a protective film for a polarizing plate, and in this case, the transparent plastic film substrate is preferably a film formed from triacetyl cellulose (TAC), polycarbonate, an acrylic polymer, a polyolefin having a cyclic or norbornene structure, or the like. In addition, in the present invention, as described later, the transparent plastic film substrate may be a polarizer itself. With such a configuration, a protective layer made of TAC or the like is not required, and the structure of the polarizing plate can be simplified, so that the number of manufacturing steps for the polarizing plate or image display device can be reduced, and production efficiency can be improved. In addition, such a configuration allows the polarizing plate to be made thinner. When the transparent plastic film substrate is a polarizer, the antiglare hard coat layer (B) and the antireflection layer (C) play the role of a protective layer. In addition, such a configuration allows the antiglare hard coat film to also function as a cover plate when it is attached to the surface of a liquid crystal cell, for example.
[0032] In the present invention, the thickness of the light-transmitting substrate (A) is not particularly limited, but considering the strength, workability such as handleability, and thin layer property, it is, for example, in the range of 10 to 500 μm, 20 to 300 μm, or 30 to 200 μm. The refractive index of the light-transmitting substrate (A) is not particularly limited. The refractive index is, for example, in the range of 1.30 to 1.80 or 1.40 to 1.70.
[0033] In the hard-coated antiglare film of the present invention, for example, the resin contained in the light-transmitting substrate (A) may contain an acrylic resin.
[0034] In the hard-coated antiglare film of the present invention, for example, the light-transmitting substrate (A) may be an acrylic film.
[0035] In addition, as described above, the antiglare hard-coated film of the present invention has unevenness formed on the outermost surface on the antiglare hard-coat layer (B) side, and the maximum height Ry of the unevenness is 1.0 μm or more and 7.0 μm or less. The maximum height Ry may be, for example, 1.5 μm or more, 2.0 μm or more, 2.5 μm or more, or 3.0 μm or more, and may be, for example, 6.5 μm or less, 6.0 μm or less, 5.5 μm or less, or 5.0 μm or less. From the viewpoint of suppressing reflection, it is preferable that Ry is large. On the other hand, from the viewpoint of preventing the display from becoming unclear due to the haze value becoming too large, it is preferable that Ry is not too large. In the present invention, the maximum height Ry is a value based on JIS B 0601 (1994 edition). The method for measuring Ry is not particularly limited, but it can be measured, for example, by the measurement method described in the examples described later.
[0036] The value of Ry can be controlled by, for example, the thickness of the antiglare hard coat layer (B), the weight average particle diameter of the first particles, and the content of the first particles in the antiglare hard coat layer (B). For example, if the thickness of the antiglare hard coat layer (B) is the same, the larger the weight average particle diameter of the first particles, the larger the Ry tends to be. Also, for example, if the thickness of the antiglare hard coat layer (B) and the weight average particle diameter of the first particles are the same, the smaller the content of the first particles in the antiglare hard coat layer (B) (i.e., the larger the average distance between the first particles), the larger the Ry tends to be.
[0037] In addition, as described above, the antiglare hard-coated film of the present invention has an average inclination angle θa of 1.0° or more and 7.5° or less in the uneven shape of the outermost surface on the antiglare hard-coat layer (B) side. The average inclination angle θa may be, for example, 1.5° or more, 2.0° or more, 2.5° or more, or 3.0° or more, and may be, for example, 6.5° or less, 6.0° or less, 5.5° or less, or 5.0° or less. From the viewpoint of suppressing reflection, it is preferable that θa is large. On the other hand, from the viewpoint of preventing the display from becoming unclear due to the haze value becoming too large, it is preferable that θa is not too large. Here, the average inclination angle θa is a value defined by the following mathematical formula (5). The average inclination angle θa can be measured, for example, by the method described in the examples described later. Average inclination angle θa=tan -1 Δa (5)
[0038] In the above formula (5), Δa is the value obtained by dividing the sum (h1+h2+h3···+hn) of the differences (heights h) between the peaks of adjacent peaks and the lowest points of adjacent valleys in the reference length L of the roughness curve defined in JIS B 0601 (1994 edition) as shown in the following formula (6). The roughness curve is a curve obtained by removing surface waviness components longer than a predetermined wavelength from a profile curve using a phase difference compensation high-pass filter. The profile curve is the outline that appears at the cut surface when the target surface is cut by a plane perpendicular to the target surface. Δa=(h1+h2+h3···+hn) / L (6)
[0039] The antiglare hard-coated film of the present invention may have an external haze value of 5% or more due to the unevenness of the outermost surface on the antiglare hard-coated layer (B) side, as described above. In a highly antiglare film, the overall appearance may be blurred and black and white shading patterns (for example, the above-mentioned streaks, horizontal dimples, etc.) may easily occur. From the viewpoint of suppressing or preventing this and suppressing reflection, it is preferable that the external haze value is as large as possible. On the other hand, from the viewpoint of suppressing or preventing deterioration of display characteristics (for example, image becomes unclear, contrast in a dark place decreases, etc.), it is preferable that the external haze value is not too large. The external haze value is not particularly limited, but may be, for example, 5% or more, 10% or more, 15% or more, or 20% or more, and may be, for example, 50% or less, 45% or less, 40% or less, or 35% or less. In the present invention, the method for measuring the external haze value is not particularly limited, but may be, for example, the following measurement methods (1) to (3). (1) The total haze value of the hard-coated antiglare film of the present invention is measured based on the method in accordance with JIS K 7136. (2) A light-transmitting adhesive is laminated on the surface of the anti-glare hard-coated film (1) opposite to the light-transmitting substrate (A) in the anti-glare hard-coated layer (B), and a COP film (ZEONOR film, product name, manufactured by Zeon Corporation) is attached thereon to produce a laminate. This laminate is measured using the same method as the total haze measurement method in accordance with JIS K 7136 (i.e., the measurement method in (1) above), to obtain the internal haze value of the anti-glare hard-coated film (1). This internal haze value is the haze value obtained by excluding the influence of the unevenness of the outermost surface on the side of the anti-glare hard-coated layer (B) from the total haze value in (1) above. (3) The value obtained by subtracting the internal haze value measured in (2) above from the total haze value measured in (1) above is defined as the external haze value of the hard-coated antiglare film of (1) above.
[0040] In the hard-coated antiglare film of the present invention, for example, the resin contained in the hard-coated antiglare layer (B) may contain an acrylate resin (also called an acrylic resin).
[0041] In the hard-coated antiglare film of the present invention, for example, the resin contained in the hard-coated antiglare layer (B) may contain a urethane acrylate resin.
[0042] In the hard-coated antiglare film of the present invention, for example, the resin contained in the hard-coated antiglare layer (B) may be a copolymer of a curable urethane acrylate resin and a polyfunctional acrylate.
[0043] In the antiglare hard-coated film of the present invention, for example, the antiglare hard-coated layer (B) is formed using an antiglare hard-coated layer forming material containing a resin and a filler, and the antiglare hard-coated layer (B) may have an aggregate portion in which the filler aggregates to form a convex portion on the surface of the antiglare hard-coated layer (B). In the aggregate portion forming the convex portion, the filler may be present in a state in which a plurality of fillers are gathered in one direction in the surface direction of the antiglare hard-coated layer (B). In the image display device of the present invention, for example, the antiglare hard-coated film of the present invention may be arranged so that the one direction in which a plurality of fillers are gathered coincides with the long side direction of the black matrix pattern. Examples of the filler include the first particles, the second particles, and the thixotropy-imparting agent.
[0044] As described above, the antiglare hard coat layer (B) contains the first particles and the second particles. The first particles and the second particles, for example, impart antiglare properties by making the surface of the antiglare hard coat layer (B) uneven, and further function to control the external haze value of the antiglare hard coat layer (B). As described above, the first particles have a larger weight average particle diameter than the second particles. The reason why streaks and horizontal dents can be suppressed or prevented by using both the first particles and the second particles in this way is considered to be, for example, as follows. First, the first particles can exhibit high antiglare properties. However, when only the first particles are used, there is a risk that unevenness in the black and white shading of the display (for example, the above-mentioned streaks, horizontal dents, etc.) may occur due to the uneven distribution of the first particles. Here, by further adding the second particles, the scattering degree of the low scattering part corresponding to the "black" part of the black and white that causes defects in the display can be increased. This reduces the scattering difference between the "black" parts and normal parts, and makes it possible to maintain the appearance quality even when the coating liquid (antiglare hard coat layer (B) forming material) is continuously coated. Alternatively, it is believed that the addition of the second particles makes the distribution of the first particles themselves more uniform, which makes it possible to suppress or prevent streaks and horizontal bumps. However, these are merely examples of possible mechanisms and do not limit the present invention in any way.
[0045] In the present invention, the weight average particle diameter d1 of the first particles is more than 3.0 μm and not more than 8.5 μm as described above. The weight average particle diameter d1 of the first particles may be, for example, 3.5 μm or more, 4.0 μm or more, 4.5 μm or more, or 5.0 μm or more, and may be, for example, 8.0 μm or less, 7.5 μm or less, 7.0 μm or less, or 6.5 μm or less.
[0046] In the present invention, the weight average particle diameter d2 of the second particles is 1.0 μm or more and 3.0 μm or less, as described above. The weight average particle diameter d2 of the second particles may be, for example, 1.2 μm or more, 1.4 μm or more, 1.6 μm or more, or 1.8 μm or more, and may be, for example, 2.8 μm or less, 2.5 μm or less, 2.2 μm or less, or 2.0 μm or less.
[0047] In the present invention, the weight average particle diameter of the first particle, the second particle, etc. can be measured, for example, by the Coulter counting method. For example, a particle size distribution measuring device using a pore electrical resistance method (product name: Coulter Multisizer, manufactured by Beckman Coulter, Inc.) is used to measure the number and volume of the particles by measuring the electrical resistance of the electrolyte equivalent to the volume of the particles when the particles pass through the pores, and the weight average particle diameter is calculated.
[0048] The shape of the first and second particles is not particularly limited, and may be, for example, approximately spherical like a bead, or may be amorphous like a powder, but is preferably approximately spherical. The shape of the first and second particles is more preferably approximately spherical with an aspect ratio of 1.5 or less, and most preferably spherical.
[0049] In the antiglare hard-coated film of the present invention, the content of the first particles may be, for example, 1.0 mass% or more, 1.5 mass% or more, 2.0 mass% or more, or 2.5 mass% or more, and may be, for example, 20.0 mass% or less, 18.0 mass% or less, 16.0 mass% or less, or 14.0 mass% or less, based on the total mass of the resin forming the resin layer of the antiglare hard-coat layer (B). The content of the first particles may be appropriately set, for example, from the viewpoint of adjusting the above-mentioned Ry and θa, or from the viewpoint of adjusting other surface shape parameters to a desired range. From the viewpoint of ensuring that antiglare properties are not insufficient, it is preferable that the content of the first particles is not too low, and from the viewpoint of preventing excessive white blur, it is preferable that the content of the first particles is not too high.
[0050] In the antiglare hard-coated film of the present invention, the content of the second particles may be, for example, 1.0 mass% or more, 1.5 mass% or more, 2.0 mass% or more, or 2.5 mass% or more, and may be, for example, 15.0 mass% or less, 12.0 mass% or less, 10.0 mass% or less, or 7.0 mass% or less, based on the total mass of the resin forming the resin layer of the antiglare hard-coated layer (B). From the viewpoint of avoiding the risk of MD streaks and horizontal dents, it is preferable that the content of the second particles is not too low, and from the viewpoint of preventing excessive white blur and avoiding the risk of spot defects due to excessive aggregation, it is preferable that the content of the second particles is not too high.
[0051] The total mass of the first particles and the second particles may be, for example, 3.5% by mass or more, 4.0% by mass or more, 4.5% by mass or more, 5% by mass or more, 5.5% by mass or more, 6.0% by mass or more, or 6.5% by mass or more, and may be, for example, 25.0% by mass or less, 23.0% by mass or less, 22% by mass or less, 21% by mass or less, 20% by mass or less, 18.0% by mass or less, 16.0% by mass or less, 14.0% by mass or less, or 12.0% by mass or less, with respect to the total mass of the resin forming the resin layer. From the viewpoint of ensuring that antiglare properties are not insufficient, it is preferable that the total mass (content) of the first particles and the second particles is not too low. On the other hand, from the viewpoint of preventing excessive white blur and avoiding the risk of spot defects caused by excessive aggregation, it is preferable that the total mass (content) of the first particles and the second particles is not too high.
[0052] In addition, because it is easy to design desired Ry and θa by using particles of a certain size or more, as described above, it is preferable that the total mass of the first particles is 2 / 3 or more of the total mass of the second particles. On the other hand, in order to avoid the unevenness formed depending on the particle size of the second particles, it is preferable that the total mass of the first particles is 10 times or less of the total mass of the second particles. The total mass of the first particles may be, for example, 1 time or more, 2 times or more, 3 times or more, or 4 times or more of the total mass of the second particles, and may be, for example, 9 times or less, 8 times or less, 7 times or less, or 6 times or less.
[0053] The materials of the first particles and the second particles are not particularly limited, and may be, for example, inorganic particles or organic particles, or inorganic particles and organic particles may be used in combination. The inorganic particles are not particularly limited, and examples thereof include silicon oxide particles, titanium oxide particles, aluminum oxide particles, zinc oxide particles, tin oxide particles, calcium carbonate particles, barium sulfate particles, talc particles, kaolin particles, calcium sulfate particles, and the like. The organic particles are not particularly limited, and examples thereof include polymethyl methacrylate resin powder (PMMA particles), silicone resin powder, polystyrene resin powder, polycarbonate resin powder, acrylic styrene resin powder, benzoguanamine resin powder, melamine resin powder, polyolefin resin powder, polyester resin powder, polyamide resin powder, polyimide resin powder, polyethylene fluoride resin powder, and the like. These inorganic particles and organic particles may be used alone or in combination. The first particles may be used alone or in combination. The second particles may be one type of particle used alone, or two or more types of particles may be used in combination.
[0054] The refractive index of the first particle and the second particle is not particularly limited, and may be, for example, 1.3 or more, 1.4 or more, 1.5 or more, or 1.6 or more, and may be, for example, 2.0 or less, 1.9 or less, 1.8 or less, or 1.7 or less.
[0055] The antiglare hard coat layer (B) is formed, for example, as described below, by applying a coating liquid containing the resin, the first particles, the second particles, and a solvent onto the surface of the light-transmitting substrate (A) to form a coating film, and then removing the solvent from the coating film. Examples of the resin include a thermosetting resin and an ionizing radiation curable resin that is cured by ultraviolet light or light. As the resin, a commercially available thermosetting resin, ultraviolet curable resin, etc. can also be used.
[0056] As the thermosetting resin or ultraviolet curing resin, for example, a curable compound having at least one of an acrylate group and a methacrylate group that is cured by heat, light (ultraviolet light, etc.), electron beam, etc. can be used, and examples thereof include oligomers or prepolymers of acrylates and methacrylates of polyfunctional compounds such as silicone resins, polyester resins, polyether resins, epoxy resins, urethane resins, alkyd resins, spiroacetal resins, polybutadiene resins, polythiolpolyene resins, polyhydric alcohols, etc. These may be used alone or in combination of two or more types.
[0057] The resin may be, for example, a reactive diluent having at least one of an acrylate group and a methacrylate group. The reactive diluent may be, for example, a reactive diluent described in JP-A-2008-88309, and may include, for example, a monofunctional acrylate, a monofunctional methacrylate, a polyfunctional acrylate, and a polyfunctional methacrylate. The reactive diluent is preferably a trifunctional or higher acrylate or a trifunctional or higher methacrylate. This is because the hardness of the antiglare hard coat layer (B) can be excellent. The reactive diluent may be, for example, butanediol glycerin ether diacrylate, an acrylate of isocyanuric acid, a methacrylate of isocyanuric acid, and the like. These may be used alone or in combination of two or more.
[0058] As described above, the antiglare hard coat layer (B) may or may not contain a thixotropy-imparting agent. By containing the thixotropy-imparting agent, for example, it is possible to easily control the aggregation state of the first particles and the second particles. The thixotropy-imparting agent may be, for example, at least one selected from the group consisting of organic clay, oxidized polyolefin, and modified urea. The thixotropy-imparting agent may also be, for example, a thickener.
[0059] The organoclay is preferably a layered clay that has been subjected to an organification treatment in order to improve its affinity with the resin. The organoclay may be prepared at home or may be a commercially available product. Examples of the commercially available products include Lucentite SAN, Lucentite STN, Lucentite SEN, Lucentite SPN, Somasif ME-100, Somasif MAE, Somasif MTE, Somasif MEE, and Somasif MPE (trade names, all manufactured by Co-op Chemical Co., Ltd.); Esben, Esben C, Esben E, Esben W, Esben P, Esben WX, Esben N-400, Esben NX, Esben NX80, Esben NO12S, Esben NEZ, Esben NO12, Esben NE, Esben NZ, Esben NZ70, Organite, Organite D, and Organite T (trade names, all manufactured by Hojun Co., Ltd.); Kunipia F, Kunipia G, and Kunipia G4 (trade names, all manufactured by Kunimine Kogyo Co., Ltd.); Thixogel VZ, Clayton HT, and Clayton 40 (trade names, all manufactured by Rockwood Additives).
[0060] The oxidized polyolefin may be prepared in-house or may be a commercially available product, such as Disparlon 4200-20 (trade name, manufactured by Kusumoto Chemical Industries, Ltd.) or Flonone SA300 (trade name, manufactured by Kyoeisha Chemical Industries, Ltd.).
[0061] The modified urea is a reaction product of an isocyanate monomer or its adduct with an organic amine. The modified urea may be prepared in-house or may be a commercially available product. Examples of the commercially available product include BYK410 (manufactured by BYK-Chemie).
[0062] The thixotropy-imparting agents may be used alone or in combination of two or more kinds.
[0063] In the hard-coated antiglare film of the present invention, the thixotropy-imparting agent may be contained in an amount of, for example, 0.2 to 5 mass % or 0.4 to 4 mass % relative to the total mass of the resin forming the resin layer of the hard-coated antiglare layer (B).
[0064] The maximum thickness of the antiglare hard coat layer (B) (D B ) is not particularly limited, and may be, for example, 2 μm or more, 3 μm or more, 4 μm or more, or 5 μm or more, and may be, for example, 20 μm or less, 18 μm or less, 16 μm or less, or 14 μm or less.
[0065] The maximum thickness of the antiglare hard coat layer (B) (D B ) to the weight average particle diameter (d1) of the first particles, d1 / D B is not particularly limited, and may be, for example, 0.2 or more, 0.4 or more, 0.6 or more, or 0.8 or more, and may be, for example, 2.0 or less, 1.8 or less, 1.6 or less, or 1.4 or less. For example, d1 / D B As described above, when is large, Ry and θa tend to become large.
[0066] In the antiglare hard-coated film of the present invention, for example, the antiglare hard-coated layer (B) has an aggregated portion in which the filler aggregates to form a convex portion on the surface of the antiglare hard-coated layer (B), and in the aggregated portion forming the convex portion, the filler may be present in a state of being gathered in a plurality of pieces in one direction in the surface direction of the antiglare hard-coated layer (B). This can prevent, for example, the reflection of a fluorescent lamp. However, the antiglare hard-coated film of the present invention is not limited thereto.
[0067] In addition, the antiglare hard-coated film of the present invention may have, for example, an intermediate layer between the light-transmitting substrate (A) and the antiglare hard-coat layer (B), which contains a resin derived from the light-transmitting substrate (A) and a resin derived from the antiglare hard-coat layer (B). By controlling the thickness of this intermediate layer, the surface shape of the antiglare hard-coat layer (B) can be controlled. For example, when the thickness of the intermediate layer is increased, the Ry and θa tend to increase, and when the thickness of the intermediate layer is decreased, the Ry and θa tend to decrease.
[0068] In the present invention, the mechanism by which the intermediate layer (also referred to as a permeation layer or a compatible layer) is formed is not particularly limited, but for example, it is formed in the drying step in the method for producing an antiglare hard-coated film by the present inventor. Specifically, for example, in the drying step, the coating liquid for forming the antiglare hard-coat layer (B) permeates the light-transmitting substrate (A), and the intermediate layer containing the resin derived from the light-transmitting substrate (A) and the resin derived from the antiglare hard-coat layer (B) is formed. The resin contained in the intermediate layer is not particularly limited, and may be, for example, a simple mixture (compatible) of the resin contained in the light-transmitting substrate (A) and the resin contained in the antiglare hard-coat layer (B). In addition, the resin contained in the intermediate layer may be, for example, at least one of the resin contained in the light-transmitting substrate (A) and the resin contained in the antiglare hard-coat layer (B) that has undergone a chemical change due to heating, light irradiation, or the like.
[0069] The thickness ratio R of the intermediate layer defined by the following mathematical formula (7) is not particularly limited, and may be, for example, 0.10 to 0.80, and may be, for example, 0.15 or more, 0.20 or more, 0.25 or more, 0.30 or more, 0.40 or more, or 0.45 or more, and may be, for example, 0.75 or less, 0.70 or less, 0.65 or less, 0.60 or less, 0.50 or less, 0.40 or less, 0.45 or less, or 0.30 or less. The thickness ratio R of the intermediate layer may be, for example, 0.15 to 0.75, 0.20 to 0.70, 0.25 to 0.65, 0.30 to 0.60, 0.40 to 0.50, 0.45 to 0.50, 0.15 to 0.45, 0.15 to 0.40, 0.15 to 0.30, or 0.20 to 0.30. The intermediate layer can be confirmed and the thickness can be measured, for example, by observing a cross section of the hard-coated antiglare film with a transmission electron microscope (TEM). R=[D C / (D C +D B )] (7) In the formula (7), D B is the thickness [μm] of the antiglare hard coat layer (B), and D Cis the thickness of the intermediate layer [μm].
[0070] The surface shape of the antiglare hard coat layer (B) can also be designed by controlling the aggregation state of the filler contained in the antiglare hard coat layer forming material. The aggregation state of the filler can be controlled, for example, by the material of the filler (e.g., the chemical modification state of the particle surface, the affinity to the solvent or resin, etc.), the type and combination of the resin (binder) or the solvent, etc. The aggregation state of the fine particles can also be precisely controlled by the thixotropy-imparting agent.
[0071] In addition, the antiglare hard-coated film of the present invention may have a gently sloping convex portion, which can prevent the occurrence of protrusions on the surface of the antiglare hard-coated layer (B), which is a defect in appearance, but is not limited thereto. In addition, the antiglare hard-coated film of the present invention may have a certain amount of the fine particles present, for example, at a position where the fine particles directly or indirectly overlap the antiglare hard-coated layer (B) in the thickness direction.
[0072] The other layer is not particularly limited, and may be, for example, a low refractive index layer, an anti-reflection layer, a high refractive index layer, a hard coat layer, an adhesive layer, etc., as described above. The other layer may be one layer or multiple layers, and when multiple layers are present, they may be one type or multiple types. For example, the other layer may be an optical thin film whose thickness and refractive index are strictly controlled, or a laminate of two or more layers of the optical thin film.
[0073] [2. Manufacturing method of anti-glare hard coat film] The method for producing the hard-coated antiglare film of the present invention is not particularly limited, and the film may be produced by any method, but it is preferably produced by the method for producing the hard-coated antiglare film of the present invention described above.
[0074] The hard-coated antiglare film can be produced, for example, as follows.
[0075] First, the antiglare hard coat layer (B) is formed on the light-transmitting substrate (A) so as to satisfy the formulas (1) to (4) (antiglare hard coat layer (B) forming step). This produces a laminate of the light-transmitting substrate (A) and the antiglare hard coat layer (B). As described above, the antiglare hard coat layer (B) forming step includes a coating step of coating a coating liquid (antiglare hard coat layer (B) forming material) on the light-transmitting substrate (A) and a coating film forming step of drying the applied coating liquid to form a coating film. Also, for example, as described above, the antiglare hard coat layer (B) forming step may further include a curing step of curing the coating film. The curing may be performed, for example, after the drying, but is not limited thereto. The curing may be performed, for example, by heating, light irradiation, or the like. The light is not particularly limited, but may be, for example, ultraviolet light, or the like. The light source for the light irradiation is not particularly limited, and may be, for example, a high-pressure mercury lamp.
[0076] As described above, the coating liquid includes the resin, the first particles, the second particles, and a solvent. The coating liquid may be, for example, an antiglare hard coat layer forming material (coating liquid) including the resin, the first particles, the second particles, the thixotropy-imparting agent, and the solvent.
[0077] The coating fluid preferably exhibits thixotropy, and the Ti value defined by the following formula is preferably in the range of 1.3 to 3.5, more preferably in the range of 1.4 to 3.2, and even more preferably in the range of 1.5 to 3. Ti value = β1 / β2 In the above formula, β1 is the viscosity measured using a Rheostress RS6000 manufactured by HAAKE at a shear rate of 20 (1 / s), and β2 is the viscosity measured using a Rheostress RS6000 manufactured by HAAKE at a shear rate of 200 (1 / s).
[0078] If the Ti value is 1.3 or more, problems such as appearance defects and deterioration of antiglare properties and white blur are unlikely to occur, and if the Ti value is 3.5 or less, problems such as the particles not agglomerating but remaining in a dispersed state are unlikely to occur.
[0079] In addition, the coating liquid may or may not contain a thixotropy-imparting agent, but it is preferable to contain a thixotropy-imparting agent because it is easier to exhibit thixotropy. As described above, the coating liquid contains the thixotropy-imparting agent, which provides an effect of preventing the particles from settling (thixotropic effect). Furthermore, the shear aggregation of the thixotropy-imparting agent itself makes it possible to freely control the surface shape of the antiglare hard coat film over a wider range.
[0080] The solvent is not particularly limited, and various solvents can be used, and one type may be used alone, or two or more types may be used in combination. In order to obtain the antiglare hard coat film of the present invention, the optimal solvent type and solvent ratio may be appropriately selected according to the composition of the resin, the type and content of the particles and the thixotropy-imparting agent, etc. The solvent is not particularly limited, and examples thereof include alcohols such as methanol, ethanol, isopropyl alcohol (IPA), butanol, t-butyl alcohol (TBA), and 2-methoxyethanol; ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, and cyclopentanone; esters such as methyl acetate, ethyl acetate, and butyl acetate; ethers such as diisopropyl ether and propylene glycol monomethyl ether; glycols such as ethylene glycol and propylene glycol; cellosolves such as ethyl cellosolve and butyl cellosolve; aliphatic hydrocarbons such as hexane, heptane, and octane; and aromatic hydrocarbons such as benzene, toluene, and xylene. In addition, for example, the solvent may include a hydrocarbon solvent and a ketone solvent. The hydrocarbon solvent may be, for example, an aromatic hydrocarbon. The aromatic hydrocarbon may be, for example, at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, ethylbenzene, and benzene. The ketone solvent may be, for example, at least one selected from the group consisting of cyclopentanone, acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, cyclohexanone, isophorone, and acetophenone. The solvent preferably contains the hydrocarbon solvent (for example, toluene) in order to dissolve a thixotropy-imparting agent (for example, a thickener). The solvent may be, for example, a solvent in which the hydrocarbon solvent and the ketone solvent are mixed in a mass ratio of 90:10 to 10:90. The mass ratio of the hydrocarbon solvent and the ketone solvent may be, for example, 80:20 to 20:80, 70:30 to 30:70, or 40:60 to 60:40, etc. In this case, for example, the hydrocarbon solvent may be toluene and the ketone solvent may be methyl ethyl ketone.The solvent may include, for example, toluene and may further include at least one selected from the group consisting of ethyl acetate, butyl acetate, IPA, methyl isobutyl ketone, methyl ethyl ketone, methanol, ethanol, and TBA.
[0081] When an acrylic film is used as the light-transmitting substrate (A) to form an intermediate layer (permeation layer), a good solvent for the acrylic film (acrylic resin) can be suitably used. The solvent may be, for example, a solvent containing a hydrocarbon solvent and a ketone solvent, as described above. The hydrocarbon solvent may be, for example, an aromatic hydrocarbon. The aromatic hydrocarbon may be, for example, at least one selected from the group consisting of toluene, o-xylene, m-xylene, p-xylene, ethylbenzene, and benzene. The ketone solvent may be, for example, at least one selected from the group consisting of cyclopentanone, acetone, methyl ethyl ketone, methyl isobutyl ketone, diethyl ketone, cyclohexanone, isophorone, and acetophenone. The solvent may be, for example, a solvent obtained by mixing the hydrocarbon solvent and the ketone solvent in a mass ratio of 90:10 to 10:90. The mass ratio of the hydrocarbon solvent to the ketone solvent may be, for example, 80:20 to 20:80, 70:30 to 30:70, or 40:60 to 60:40, etc. In this case, for example, the hydrocarbon solvent may be toluene, and the ketone solvent may be methyl ethyl ketone.
[0082] When triacetyl cellulose (TAC) is used as the light-transmitting substrate (A) to form an intermediate layer (permeation layer), a good solvent for TAC can be suitably used, such as ethyl acetate, methyl ethyl ketone, and cyclopentanone.
[0083] In addition, by appropriately selecting solvent, when containing thixotropy-imparting agent, it is possible to well express the thixotropy in antiglare hard coat layer forming material (coating liquid).For example, when using organic clay, toluene and xylene can be preferably used alone or in combination; for example, when using oxidized polyolefin, methyl ethyl ketone, ethyl acetate, propylene glycol monomethyl ester can be preferably used alone or in combination; for example, when using modified urea, butyl acetate and methyl isobutyl ketone can be preferably used alone or in combination.
[0084] Various leveling agents can be added to the antiglare hard coat layer forming material. As the leveling agent, for example, a fluorine-based or silicone-based leveling agent can be used for the purpose of preventing coating unevenness (uniformity of the coating surface). In the present invention, a leveling agent can be appropriately selected depending on the case where antifouling is required on the surface of the antiglare hard coat layer (B) or the case where an antireflection layer (low refractive index layer) or a layer containing an interlayer filler is formed on the antiglare hard coat layer (B) as described later. In the present invention, for example, the thixotropy-imparting agent can be included to cause the coating liquid to exhibit thixotropy, so that coating unevenness is unlikely to occur. In this case, for example, the leveling agent has an advantage of being able to have a wider selection of options.
[0085] The amount of the leveling agent added is, for example, 5 parts by weight or less, and preferably in the range of 0.01 to 5 parts by weight, relative to 100 parts by weight of the resin.
[0086] The antiglare hard coat layer forming material may contain, if necessary, pigments, fillers, dispersants, plasticizers, ultraviolet absorbers, surfactants, antifouling agents, antioxidants, etc., within the scope of not impairing the performance. These additives may be used alone or in combination of two or more.
[0087] For the antiglare hard coat layer forming material, a conventionally known photopolymerization initiator such as that described in JP-A-2008-88309 can be used.
[0088] Examples of a method for applying the coating liquid onto the light-transmitting substrate (A) to form a coating film include coating methods such as fountain coating, die coating, spray coating, gravure coating, roll coating, and bar coating.
[0089] Next, as described above, the coating film is dried and cured to form the antiglare hard coat layer (B). The drying may be, for example, natural drying, air drying by blowing air, heat drying, or a combination of these methods.
[0090] The drying temperature of the coating liquid for forming the antiglare hard coat layer (B) may be, for example, in the range of 30 to 200° C. The drying temperature may be, for example, 40° C. or more, 50° C. or more, 60° C. or more, 70° C. or more, 80° C. or more, 90° C. or more, or 100° C. or more, and may be 190° C. or less, 180° C. or less, 170° C. or less, 160° C. or less, 150° C. or less, 140° C. or less, 135° C. or less, 130° C. or less, 120° C. or less, or 110° C. or less. The drying time is not particularly limited, and may be, for example, 30 seconds or more, 40 seconds or more, 50 seconds or more, or 60 seconds or more, and may be 150 seconds or less, 130 seconds or less, 110 seconds or less, or 90 seconds or less.
[0091] The method for curing the coating film is not particularly limited, but ultraviolet curing is preferred. The radiation dose of the energy ray source is 50 to 500 mJ / cm2 as the cumulative exposure dose at an ultraviolet wavelength of 365 nm. 2 The irradiation dose is preferably 50 mJ / cm. 2 If the curing rate is 500 mJ / cm or more, the curing is likely to proceed sufficiently, and the hardness of the antiglare hard coat layer (B) formed is likely to be high. 2 If it is equal to or less than this, coloring of the antiglare hard coat layer (B) to be formed can be prevented.
[0092] In the manner described above, a laminate of the light-transmitting substrate (A) and the antiglare hard coat layer (B) can be produced. This laminate may be used as the antiglare hard coat film of the present invention as it is, or may be used as the antiglare hard coat film of the present invention by forming the other layer on the antiglare hard coat layer (B). The method of forming the other layer is not particularly limited, and may be the same as or similar to the method of forming a general low refractive index layer, antireflection layer, high refractive index layer, hard coat layer, pressure-sensitive adhesive layer, etc.
[0093] [3. Optical components and image display devices] The optical member of the present invention is not particularly limited, but may be, for example, a polarizing plate. The polarizing plate is also not particularly limited, but may include, for example, the antiglare hard coat film of the present invention and a polarizer, and may further include other components. Each component of the polarizing plate may be bonded together, for example, with an adhesive or a pressure sensitive adhesive.
[0094] The image display device of the present invention is not particularly limited, and any image display device may be used, and examples thereof include a liquid crystal display device and an organic EL display device.
[0095] The image display device of the present invention is, for example, an image display device having the hard-coated antiglare film of the present invention on the viewing side surface, and the image display device may have a black matrix pattern.
[0096] The antiglare hard-coated film of the present invention can be laminated, for example, on the light-transmitting substrate (A) side to an optical member used in an LCD via a pressure-sensitive adhesive or adhesive. In addition, in this lamination, the surface of the light-transmitting substrate (A) may be subjected to various surface treatments as described above. As described above, according to the manufacturing method of the antiglare hard-coated film of the present invention, the surface shape of the antiglare hard-coated film can be freely controlled in a wide range. Therefore, the optical properties that can be obtained by laminating the antiglare hard-coated film with another optical member using an adhesive or pressure-sensitive adhesive are in a wide range corresponding to the surface shape of the antiglare hard-coated film.
[0097] The optical member may be, for example, a polarizer or a polarizing plate. A polarizing plate is generally configured to have a transparent protective film on one or both sides of a polarizer. When transparent protective films are provided on both sides of a polarizer, the transparent protective films on the front and back may be made of the same material or different materials. The polarizing plates are usually disposed on both sides of a liquid crystal cell. Moreover, the polarizing plates are disposed so that the absorption axes of the two polarizing plates are approximately perpendicular to each other.
[0098] The configuration of the polarizing plate having the anti-glare hard-coated film laminated thereon is not particularly limited, and may be, for example, a configuration in which a transparent protective film, the polarizer, and the transparent protective film are laminated in this order on the anti-glare hard-coated film, or a configuration in which the polarizer and the transparent protective film are laminated in this order on the anti-glare hard-coated film.
[0099] The image display device of the present invention has the same structure as a conventional image display device, except that the antiglare hard-coated film is arranged in a specific direction. For example, in the case of an LCD, it can be manufactured by appropriately assembling each component such as a liquid crystal cell, optical members such as a polarizing plate, and an illumination system (backlight, etc.) as necessary, and incorporating a driving circuit.
[0100] According to the antiglare hard coat film of the present invention, for example, strong external light can be scattered and reflection can be suppressed, so that reflection can be suppressed even outdoors. Therefore, the image display device of the present invention can be suitably used, for example, as an outdoor public information display. However, the image display device of the present invention is not limited to this use and can be used for any other use. Examples of the use include office automation equipment such as personal computer monitors, notebook computers, and copy machines, portable devices such as mobile phones, watches, digital cameras, personal digital assistants (PDAs), and portable game consoles, home electric appliances such as video cameras, televisions, and microwave ovens, in-vehicle devices such as back monitors, monitors for car navigation systems, and car audio, exhibition devices such as information monitors for commercial stores, security equipment such as surveillance monitors, and nursing and medical equipment such as nursing monitors and medical monitors. EXAMPLES
[0101] Next, examples of the present invention will be described together with comparative examples, although the present invention is not limited to the following examples and comparative examples.
[0102] In the following examples and comparative examples, the number of parts of a substance is by mass (parts by weight) unless otherwise specified.
[0103] [Example 1] A hard-coated antiglare film was produced as follows.
[0104] (Preparation of antiglare hard coat layer forming material) As the resin contained in the antiglare hard coat layer forming material, 40 parts by weight of an ultraviolet-curing urethane acrylate resin (manufactured by Shin-Nakamura Chemical Co., Ltd., product name "UA53H-80MB", solid content 80%) and 60 parts by weight of a multifunctional acrylate whose main component is pentaerythritol triacrylate (manufactured by Osaka Organic Chemical Industry Co., Ltd., product name "Viscoat #300", solid content 100%) were prepared. Per 100 parts by weight of the resin solid content of the resin, 5 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer SSX1055QXE", weight average particle diameter: 5.0 μm, refractive index 1.515) as the first particles, 1 part by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer SSX103DXE", weight average particle diameter: 3.0 μm, refractive index 1.525) as the second particles, a total of 6 parts by weight, 1.5 parts by weight of synthetic smectite (manufactured by Kunimine Kogyo Co., Ltd., trade name "Sumecton SAN") which is an organic viscosity as a thixotropy imparting agent, 3 parts by weight of a photopolymerization initiator (manufactured by BASF, trade name "OMNIRAD907"), and 1.0 part by weight of a leveling agent (manufactured by DIC Corporation, trade name "GRANDIC PC4100", solid content 10%) were mixed. This mixture was diluted with a mixed solvent of toluene / ethyl acetate (weight ratio 50 / 50) so that the solid content concentration was 30%, to prepare an antiglare hard coat layer forming material (coating liquid).
[0105] (Transparent base material (A)) As the light-transmitting substrate (A), a transparent plastic film substrate (acrylic film, manufactured by Toyo Kohan Co., Ltd., product name "HX40UC", thickness: 40 μm, film width: 1330 mm, refractive index: 1.49) was prepared.
[0106] (Manufacture of anti-glare hard coat film) On one side of the transparent plastic film substrate (light-transmitting substrate (A)), the antiglare hard coat layer (B) forming material (coating liquid) was continuously applied (coated) for 500 m using a die coater to form an undried coating film (coating step). Then, the transparent plastic film substrate with the undried coating film formed thereon was conveyed to the next drying step (coating film forming step). In the drying step (coating film forming step), the undried coating film was dried by heating at 100°C for 1 minute to form a coating film. Thereafter, ultraviolet rays with an integrated light quantity of 300 mJ / cm 2 were irradiated using a high-pressure mercury lamp, and the coating film was cured to form an antiglare hard coat layer (B) with a thickness (maximum thickness) of 3.0 μm, obtaining the antiglare hard coat film of Example 1. Regarding the central portion in the width direction of the obtained antiglare hard coat film, the surface shape profile was measured using a contact-type surface shape measuring instrument, and the surface shape parameters Ry and θa were measured. As a result, Ry = 6.62 μm and θa = 4.46°. Note that Ry and θa were measured by the following measuring method. The same applies to each of the following Examples and Comparative Examples. Also, the above thickness (maximum thickness) and surface shape parameters are all values measured by cutting out the central portion in the width direction from the film at the 500 m point when continuous coating of 500 m or more was performed. The same applies to each of the following Examples and Comparative Examples.
[0107] <Measuring method for Ry and θa> A glass plate (thickness 1.3 mm) manufactured by Matsunami Glass Industrial Co., Ltd. was attached to the surface of the antiglare hard-coat film on which the antiglare hard-coat layer (B) was not formed with an adhesive, and the surface shape of the antiglare hard-coat layer (B) was measured using a high-precision fine shape measuring instrument (product name: Surfcorder ET4000, manufactured by Kosaka Laboratory Co., Ltd.) under the condition of a cut-off value of 0.8 mm, and the maximum height and average tilt angle were calculated. Furthermore, the maximum height and average tilt angle were measured at any 10 points, and the average values were taken as the maximum height Ry and the average tilt angle θa, respectively. The high-precision fine shape measuring instrument automatically calculates the maximum height Ry and the average tilt angle θa. The measurement method and calculation method of the maximum height Ry and the average tilt angle θa are based on JIS B 0601 (1994 edition).
[0108] [Example 2] Except for forming the antiglare hard coat layer (B) to have a thickness (maximum thickness) of 7.0 μm, the antiglare hard coat film of Example 2 was produced by the same production method as in Example 1. The surface shape parameters were Ry=1.45 μm and θa=1.15°.
[0109] [Example 3] The antiglare hard coat film of Example 3 was produced by the same production method as in Example 1, except that 8 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX1055QXE", weight average particle size: 5.0 μm, refractive index 1.515) was used as the first particles, and the thickness (maximum thickness) of the antiglare hard coat layer (B) was formed to be 5.0 μm. The surface shape parameters were Ry = 2.97 μm and θa = 3.12°.
[0110] [Example 4] The antiglare hard coat film of Example 4 was produced by the same production method as in Example 3, except that 6 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX103DXE", weight average particle diameter: 3.0 μm, refractive index 1.525) were used as the second particles. The surface shape parameters were Ry = 3.03 μm and θa = 3.33°.
[0111] [Example 5] The antiglare hard coat film of Example 5 was produced by the same production method as in Example 4, except that 12 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX1055QXE", weight average particle diameter: 5.0 μm, refractive index 1.515) were used as the first particles, and 8 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX103DXE", weight average particle diameter: 3.0 μm, refractive index 1.525) were used as the second particles. The surface shape parameters were Ry = 3.23 μm and θa = 4.03 °.
[0112] [Example 6] The antiglare hard coat film of Example 6 was produced by the same production method as in Example 5, except that 8 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer SSX1055QXE", weight average particle diameter: 5.0 μm, refractive index 1.515) was used as the first particles, and 1 part by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer XX145AA", weight average particle diameter: 1.5 μm, refractive index 1.495) was used as the second particles. The surface shape parameters were Ry = 3.29 μm and θa = 3.61 °.
[0113] [Example 7] The antiglare hard-coated film of Example 7 was produced by the same production method as in Example 6, except that the antiglare hard-coated layer (B) was formed to have a thickness (maximum thickness) of 9.0 μm. The surface shape parameters were Ry=1.57 μm and θa=1.36°.
[0114] [Example 8] The antiglare hard coat film of Example 8 was produced by the same production method as in Example 1, except that 10 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer XX140AA", weight average particle diameter: 3.5 μm, refractive index 1.535) was used as the first particles, and 2 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer XX145AA", weight average particle diameter: 1.5 μm, refractive index 1.495) was used as the second particles, and the antiglare hard coat layer (B) was formed to have a thickness (maximum thickness) of 3.0 μm. The surface shape parameters were Ry = 3.81 μm and θa = 4.81 °.
[0115] [Example 9] The antiglare hard-coated film of Example 9 was produced by the same production method as in Example 8, except that the antiglare hard-coated layer (B) was formed to have a thickness (maximum thickness) of 5.0 μm. The surface shape parameters were Ry=1.59 μm and θa=1.61°.
[0116] [Example 10] The antiglare hard coat film of Example 10 was produced by the same production method as in Example 9, except that 2 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer XX42AA", weight average particle diameter: 8.0 μm, refractive index 1.515) were used as the first particles, and 3 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., trade name "Techpolymer SSX103DXE", weight average particle diameter: 3.0 μm, refractive index 1.525) were used as the second particles. The surface shape parameters were Ry = 4.40 μm and θa = 2.28 °.
[0117] [Example 11] The antiglare hard-coated film of Example 11 was produced by the same production method as in Example 10, except that the antiglare hard-coated layer (B) was formed to have a thickness (maximum thickness) of 9.0 μm. The surface shape parameters were Ry=1.70 μm and θa=1.18°.
[0118] [Comparative Example 1] Except for forming the antiglare hard coat layer (B) to have a thickness (maximum thickness) of 14.0 μm, the antiglare hard coat film of Comparative Example 1 was produced by the same production method as in Example 1. The surface shape parameters were Ry=1.40 μm and θa=0.88°.
[0119] [Comparative Example 2] The antiglare hard coat film of Comparative Example 2 was produced by the same production method as in Example 1, except that 8 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX1055QXE", weight average particle size: 5.5 μm, refractive index 1.515) were used as the first particles, and the antiglare hard coat layer (B) was formed to have a thickness (maximum thickness) of 3.0 μm. The surface shape parameters were Ry = 7.41 μm and θa = 5.90°.
[0120] [Comparative Example 3] The antiglare hard coat film of Comparative Example 3 was produced by the same production method as in Comparative Example 2, except that 6 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX103DXE", weight average particle size: 3.0 μm, refractive index 1.525) were used as the second particles. The surface shape parameters were Ry = 7.68 μm and θa = 7.83°.
[0121] [Comparative Example 4] The antiglare hard coat film of Comparative Example 4 was produced by the same production method as in Comparative Example 3, except that 1.5 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer XX140AA", weight average particle diameter: 3.5 μm, refractive index 1.535) were used as the first particles and no second particles were added. The surface shape parameters were Ry=2.32 μm and θa=1.44°.
[0122] [Comparative Example 5] The antiglare hard coat film of Comparative Example 5 was produced by the same production method as in Comparative Example 4, except that 8.0 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX1055QXE", weight average particle diameter: 5.5 μm, refractive index 1.515) were used as the first particles, no second particles were added, and the antiglare hard coat layer (B) was formed to have a thickness (maximum thickness) of 5.0 μm. The surface shape parameters were Ry = 3.58 μm and θa = 3.59 °.
[0123] [Comparative Example 6] Except for forming the antiglare hard coat layer (B) to have a thickness (maximum thickness) of 9.0 μm, the antiglare hard coat film of Comparative Example 6 was produced by the same production method as in Comparative Example 5. The surface shape parameters were Ry=1.74 μm and θa=1.42°.
[0124] [Comparative Example 7] The antiglare hard coat film of Comparative Example 7 was produced by the same production method as in Comparative Example 5, except that 12.0 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX1055QXE", weight average particle size: 5.5 μm, refractive index 1.515) was used as the first particles. The surface shape parameters were Ry = 3.74 μm and θa = 4.38°.
[0125] [Comparative Example 8] The antiglare hard-coated film of Comparative Example 8 was produced by the same production method as in Comparative Example 7, except that the antiglare hard-coated layer (B) was formed to have a thickness (maximum thickness) of 9.0 μm. The surface shape parameters were Ry=1.96 μm and θa=1.62°.
[0126] [Comparative Example 9] An antiglare hard coat film of Comparative Example 9 was produced by the same production method as in Example 1, except that the first particles were not added and 6 parts by weight of copolymer particles of acrylic and styrene (manufactured by Sekisui Chemical Co., Ltd., product name "Techpolymer SSX103DXE", weight average particle size: 3.0 μm, refractive index 1.525) were used as the second particles. The surface shape parameters were Ry=2.94 μm and θa=2.63°.
[0127] [Comparative Example 10] The antiglare hard-coated film of Comparative Example 10 was produced by the same production method as in Comparative Example 9, except that the antiglare hard-coated layer (B) was formed to have a thickness (maximum thickness) of 9.0 μm. The surface shape parameters were Ry=0.92 μm and θa=0.70°.
[0128] [Comparative Example 11] An antiglare hard coat film of Comparative Example 11 was produced by the same production method as in Example 3, except that 10 parts by weight of silica particles (manufactured by Nissan Chemical Industries, Ltd., product name "MIBK-ST", average particle size 10 nm, solid content 30%) was used as the second particles. The surface shape parameters were Ry = 3.21 μm and θa = 2.67°.
[0129] For each of the anti-glare hard-coated films of the Examples and Comparative Examples produced as described above, the external haze value was measured by the measurement method described above, and the streaks and horizontal dents at a distance of 500 m and the anti-glare properties were evaluated by the following method.
[0130] [Evaluation method for streaks and horizontal dents at the 500m point] In the film roll (antiglare hard-coated film) after 500 m coating, a sheet with a width of 1330 mm and a length of 1000 mm in the film running direction was cut out from the roll at any point after 500 m. Next, a black PET film with adhesive was attached to the opposite side of the antiglare hard-coated layer (B) of the cut-out sheet (antiglare hard-coated film). After that, an LED light source was projected onto the antiglare hard-coated layer (B) in a darkroom environment, and the boundary between the reflected LED light and the non-reflected LED light was visually judged, and the presence or absence of unevenness in the white blurred areas and the black, tight appearance was evaluated according to the following criteria. - Clear contrast between black and white: × There is some variation in color, but it is within the acceptable range: 〇
[0131] [How to assess anti-glare properties] In the film roll (antiglare hard-coated film) after 500 m coating, a sheet having a width of 1330 mm and a length of 1000 mm in the film running direction was cut out from the roll at any point after 500 m. Next, a black PET film with adhesive was attached to the opposite side of the antiglare hard-coated layer (B) of the cut-out sheet (antiglare hard-coated film). After that, an LED light source was projected onto the antiglare hard-coated layer (B) in a darkroom environment, and the degree of blurring of the projected LED light was visually judged and evaluated according to the following criteria. Fluorescent lights are moderately blurred (while still providing sharp blacks): Yes - White blur is too strong or the light source is too reflected: ×
[0132] The following Tables 1 and 2 show the weight average particle diameter d1 of the first particles, the weight average particle diameter d2 of the second particles, the content (parts) of the first particles and the second particles, the external haze value, Ry, θa, the evaluation results of streaks and horizontal dents at a point of 500 m, and the evaluation results of antiglare properties for the antiglare hard coat films of the respective Examples and Comparative Examples. In addition, in the following Tables 1 and 2, "parts" represents the number of parts by weight (parts by mass) of the first particles or the second particles relative to 100 parts by weight (parts by mass) of the resin forming the resin layer in the antiglare hard coat layer (B). In other words, this "parts" is equal to the content (% by mass) of the first particles or the second particles relative to the total mass of the resin forming the resin layer. In addition, in the following Tables 1 and 2, "total parts by weight" represents the total parts by weight (parts by mass) of the first particles and the second particles relative to 100 parts by weight (parts by mass) of the resin forming the resin layer in the antiglare hard coat layer (B). In other words, this "total parts by weight" is equal to the total content (% by mass) of the first particles and the second particles relative to the total mass of the resin forming the resin layer.
[0133] [Table 1]
[0134] [Table 2]
[0135] As shown in Tables 1 and 2, the anti-glare hard-coated films of the examples that satisfied all the requirements of the present invention had good anti-glare properties and did not show any streaks or horizontal dents. That is, the anti-glare hard-coated films of these examples suppressed reflections and suppressed or prevented streaks and horizontal dents. In contrast, the anti-glare hard-coated films of the comparative examples that did not satisfy any of the requirements of the present invention did not have good anti-glare properties or showed any streaks or horizontal dents. That is, the anti-glare hard-coated films of these comparative examples could not simultaneously suppress reflections and suppress streaks and horizontal dents. [Industrial Applicability]
[0136] As described above, according to the present invention, it is possible to provide an antiglare hard-coated film, a manufacturing method for an antiglare hard-coated film, an optical member, and an image display device in which reflection is suppressed and streaks and horizontal dents are suppressed or prevented. According to the antiglare film of the present invention, for example, strong external light can be scattered and reflection can be suppressed, so that reflection can be suppressed even outdoors. Therefore, the present invention can be suitably used for image display devices such as outdoor public information displays. However, the present invention is not limited to this use and can be used for a wide range of uses. [Explanation of symbols]
[0137] 10 Anti-glare film 11 Light-transparent base material (A) 12 Anti-glare layer (B) 12a Resin layer 12b1 1st particle 12b2 2nd particle Ry Maximum height of the convex part of the outermost surface θa Average inclination angle of the outermost surface irregularities
Claims
1. An antiglare hard-coated film comprising an antiglare hard-coat layer (B) laminated on a light-transmitting substrate (A), an intermediate layer is provided between the light-transmitting substrate (A) and the antiglare hard coat layer (B), the intermediate layer containing a resin derived from the light-transmitting substrate (A) and a resin derived from the antiglare hard coat layer (B); the antiglare hard coat layer (B) is formed of a resin layer, and contains first particles and second particles inside the resin layer, a total mass of the first particles and the second particles is 2 to 25% by mass with respect to a total mass of a resin forming the resin layer, the first particles and the second particles are each made of an organic material; The antiglare hard coat film has an outermost surface on the side of the antiglare hard coat layer (B) formed with irregularities, The weight average particle diameter of the first particles satisfies the following mathematical formula (1), The weight average particle diameter of the second particles satisfies the following formula (2), The uneven shape of the outermost surface of the hard-coated antiglare film satisfies the following formulas (3) and (4): 3.0<d1≦8.5 [μm] (1) 1.0≦d2≦3.0 [μm] (2) Ry: 1.0≦Ry≦7.0 [μm] (3) θa: 1.0≦θa≦7.5 [°] (4) In the formula (1), d1 is the weight average particle diameter [μm] of the first particles, In the formula (2), d2 is the weight average particle diameter [μm] of the second particles, In the formula (3), Ry is the maximum height [μm] of the convex portions of the concaves and convexes, In the formula (4), θa is the average inclination angle [°] of the irregularities.
2. 2. The hard-coated antiglare film according to claim 1, wherein the total mass of the second particles is 1 mass % or more based on the total mass of the resin forming the resin layer.
3. 3. The hard-coated antiglare film according to claim 1, wherein the external haze value caused by the unevenness is 5% or more.
4. 4. The hard-coated antiglare film according to claim 1, wherein the total mass of the first particles is at least 2 / 3 of the total mass of the second particles.
5. The method includes forming the antiglare hard coat layer (B) on the light-transmitting substrate (A) so as to satisfy the formulas (1) to (4), the antiglare hard coat layer (B) forming step includes a coating step of coating a coating liquid on the light-transmitting substrate (A), and a coating film forming step of drying the applied coating liquid to form a coating film, 5. The method for producing an antiglare hard-coated film according to claim 1, wherein the coating liquid contains the resin, the first particles, the second particles, and a solvent.
6. The method according to claim 5, wherein in the coating step, the coating liquid is continuously applied over a width of 1000 mm or more and a length of 500 m or more.
7. The method according to claim 5 or 6, wherein the step of forming the antiglare hard coat layer (B) further comprises a curing step of curing the coating film.
8. An optical member comprising the hard-coated antiglare film according to claim 1 .
9. 9. The optical member according to claim 8, which is a polarizing plate.
10. An image display device comprising the antiglare hard-coated film according to claim 1 , or the optical member according to claim 8 or 9 .
11. 11. The image display device according to claim 10, which is a public information display.
Citation Information
Patent Citations
Information sharing server and program
JP2004110461A
Light diffusion film, Anti-reflection film, polarizing plate and image display device using the light diffusion film or the Anti-reflection film
JP2006330705A
Antiglare laminate
JP2009175725A
Method of manufacturing antiglare film, antiglare film, polarizing plate and transmissive liquid crystal display device
JP2010102291A
Management method of antiglare film and roll body
JP2016050950A