Printing ink composition for detachment and detachment method
The release printing ink composition addresses inefficiencies in existing methods by providing quick and balanced adhesion and release properties, enabling efficient film removal and simplifying recycling processes.
Patent Information
- Application Number
- JP2020191948
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2020-11-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-18
AI Technical Summary
Existing methods for removing printed layers from packaging materials are inefficient and complex, requiring prolonged infiltration of sodium hydroxide solutions and causing complications in waste treatment.
A release printing ink composition containing specific pigments, binder resins, and solvents, which allows for quick and balanced adhesion and release properties, utilizing an aqueous alkaline solution for film removal.
Enables rapid and effective peeling of printed films from substrates, simplifying the removal process and facilitating recycling of materials.
Smart Images

Figure 0007574506000001
Abstract
Description
[Technical field]
[0001] The present invention relates to a detachable printing ink composition and a method for detaching an ink composition film from a printed matter printed with the ink composition. [Background technology]
[0002] Packaging materials using various plastic films are used for food, confectionery, household goods, pet food, etc., from the viewpoints of design, economy, content protection, transportability, etc. Furthermore, gravure printing or flexographic printing is applied to many packaging materials with the intention of adding designs and messages that will appeal to consumers. To obtain these packaging materials, printing is performed on the front or back surface of the base film of the packaging material, or an adhesive or anchor agent is applied to the printed surface of the base film of the packaging material as necessary, and the film is then laminated. In printing, colored inks and white ink are printed in sequence on various films such as polyester, nylon, and aluminum foil, and then a polyethylene film or polypropylene film for heat sealing is laminated on the white ink printed layer by dry lamination using an adhesive or extrusion lamination using an anchor coating agent (see Patent Document 1).
[0003] In order to remove the printed layer, a method is known in which a removable primer layer is formed on a polyester substrate in advance, and a printed layer is further formed thereon (see Patent Document 2). However, in this method, even if the printed matter in which the removable primer layer has been cut into pieces is immersed in an aqueous sodium hydroxide solution, the removable primer comes into contact with the aqueous sodium hydroxide solution only at the cross section of the cut-out printed matter. Therefore, the removable primer layer exhibits the property of being removed only when the aqueous sodium hydroxide solution penetrates through the cross section. At this time, the penetration takes time, so the printed layer cannot be removed quickly. In addition, the removable primer layer dissolves in the aqueous sodium hydroxide solution, so that the disposal of the aqueous sodium hydroxide solution after use may become complicated. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] Japanese Patent Application Publication No. 5-97959 [Patent Document 2] Patent No. 6388131 Summary of the Invention [Problem to be solved by the invention]
[0005] An object of the present invention is to provide a detachable printing ink composition that enables a printing coating of the ink composition on the front or back surface of a printed matter to be quickly and arbitrarily peeled off after the printed matter has been used, and a method for detaching the ink composition coating from a printed matter printed with the ink composition. [Means for solving the problem]
[0006] Means for Solving the Problems The present inventors have conducted extensive research to solve the above problems and have invented the following detachment printing ink composition. 1. A printing ink composition for detachment comprising a pigment, a binder resin substantially having no acid groups, and a rosin-based resin having an acid value of 100 to 350 mgKOH / g in an amount of 0.1 to 5.0 mass %, and an organic solvent. 2. The detachable printing ink composition according to 1, wherein the rosin-based resin is a rosin-modified maleic acid resin and / or a polymerized rosin resin. 3. The binder resin is (A) a binder resin containing at least one resin selected from a polyurethane resin, a polyamide resin, and an acrylic resin, and a cellulose derivative; or (B) a binder resin containing a polyurethane resin and a vinyl chloride-vinyl acetate copolymer resin, the solid content ratio of which is polyurethane resin / vinyl chloride-vinyl acetate copolymer resin=100 / 0 to 70 / 30; 3. The detachable printing ink composition according to 1 or 2, 4. A detachable printing ink composition, wherein the polyurethane resin according to 3 is a polyester polyether type polyurethane resin. 5. A method for removing a printing ink composition for detachment, comprising removing a coating of the surface printing ink composition for detachment from a printed matter formed by printing the printing ink composition for detachment according to any one of 1 to 4 on a substrate in a removing liquid consisting of an alkaline aqueous solution. Effect of the Invention
[0007] The detachable printing ink composition of the present invention provides a printed coating with good adhesion to a resin film and also exhibits a well-balanced releasability. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0008] The detachable printing ink composition of the present invention will be described in more detail below. <Pigments> As the pigment that can be used in the present invention, various inorganic pigments and / or organic pigments that are generally used in printing inks can be used. Examples of inorganic pigments include color pigments such as titanium oxide, red iron oxide, antimony red, cadmium yellow, cobalt blue, Prussian blue, ultramarine, carbon black, and graphite, and extender pigments such as silica, calcium carbonate, kaolin, clay, barium sulfate, aluminum hydroxide, and talc. Examples of the organic pigment include soluble azo pigments, insoluble azo pigments, azo lake pigments, condensed azo pigments, copper phthalocyanine pigments, and condensed polycyclic pigments. The content of the pigment in the detachable printing ink composition in the present invention is preferably 0.5 to 50.0% by mass. If the content of the pigment in the detachable printing ink composition is less than the above range, the coloring power of the detachable printing ink composition decreases, and if it is more than the above range, the viscosity of the detachable printing ink composition increases, making the printed matter more susceptible to smudging.
[0009] <Binder resin> As the binder resin, it is preferable to use (A) a binder resin containing at least one selected from polyurethane resin, polyamide resin and acrylic resin, and a cellulose derivative, or (B) a binder resin containing polyurethane resin and vinyl chloride-vinyl acetate copolymer resin, with a solid content ratio of polyurethane resin / vinyl chloride-vinyl acetate copolymer resin=100 / 0 to 70 / 30. In the case of either (A) or (B) above, there is an additional effect that the adhesiveness to various substrates is particularly excellent and the releasability is also excellent. Furthermore, the content of (A) in the solid content of the ink composition is preferably 30.0 mass % or more, more preferably 40.0 mass % or more, even more preferably 50.0 mass % or more, and most preferably 55.0 mass % or more. The content of (B) in the solid content of the ink composition is preferably 25.0% by mass or more, more preferably 40.0% by mass or more, even more preferably 50.0% by mass or more, and most preferably 60.0% by mass or more. The binder resin is substantially free of acid groups. The term "substantially free of acid groups" used herein means that the binder resin does not have acid groups derived from the constituent monomers themselves or acid groups intentionally generated during polymerization. In addition, acid groups that naturally occur during storage, etc. are not intended.
[0010] (Polyurethane resin) As the polyurethane resin in the present invention, a polyurethane resin obtained by reacting a polyisocyanate compound, a diol compound, and, if necessary, a chain extender, a reaction terminator, etc. can be used. Examples of the polyisocyanate compound that can be used herein include aliphatic diisocyanate compounds such as hexamethylene diisocyanate and 2,2,4-trimethylhexamethylene diisocyanate; alicyclic diisocyanate compounds such as isophorone diisocyanate, hydrogenated xylylene diisocyanate and 4,4-cyclohexylmethane diisocyanate; aromatic aliphatic diisocyanate compounds such as xylylene diisocyanate and α,α,α',α'-tetramethylxylylene diisocyanate; and aromatic diisocyanate compounds such as toluylene diisocyanate and diphenylmethane diisocyanate.
[0011] Among the diol compounds, preferred are polymeric diol compounds having a number average molecular weight of more than 500 and not more than 3000, more preferably 500 to 2000, and may be composed of one type of diol compound or may be a combination of multiple diol compounds. When the number average molecular weight of the diol compound is 500 or less, the adhesiveness tends to decrease, while when the number average molecular weight exceeds 3000, the oil resistance tends to decrease. Specific examples of such diol compounds include alkylene glycol compounds having a molecular weight of 100 or more, polyalkylene glycol compounds such as polyethylene glycol and polypropylene glycol, and polyether diol compounds obtained by polyaddition of oxyalkylenes such as ethylene oxide and propylene oxide, tetrahydrofuran, or the like to diol compounds such as low-molecular-weight alkylene glycols and bisphenols. Further examples include polyester diol compounds obtained by polycondensation of low molecular weight diol compounds such as linear glycols such as ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,6-hexanediol; branched glycols such as 1,2-propanediol, neopentyl glycol, 3-methyl-1,5-pentanediol, 2,4-diethyl-1,5-pentanediol, and ethylbutylpropanediol; and ether-based diols such as diethylene glycol and triethylene glycol, with dicarboxylic acid compounds such as saturated and unsaturated aliphatic dicarboxylic acids such as succinic acid, adipic acid, azelaic acid, sebacic acid, and maleic acid, and aromatic dicarboxylic acids such as phthalic acid; and polyester diol compounds obtained by ring-opening reaction of cyclic ester compounds such as lactones.
[0012] Furthermore, linear or side chain polycarbonate compounds, polybutadiene glycol compounds, etc. can also be used in combination. In addition, in consideration of the environment, it is preferable to use a polyether diol compound as the polyol compound in order to obtain good printability in a system that does not contain aromatic hydrocarbon organic solvents (toluene, etc.) and contains a large proportion of highly polar organic solvents such as alcohols and esters. When other solvents are used, it may be preferable to use a polyester diol compound.
[0013] Furthermore, in the present invention, it is also possible to utilize a polyurethane resin obtained by using a chain extender or a reaction terminator. Examples of chain extenders include aliphatic diamines such as ethylenediamine, propylenediamine, tetramethylenediamine, and hexamethylenediamine; alicyclic diamines such as isophoronediamine and 4,4'-dicyclohexylmethanediamine; polyamines such as diethylenetriamine and triethylenetetratriamine; aromatic diamines such as toluylenediamine; aromatic aliphatic diamines such as xylenediamine; diamines having a hydroxyl group such as N-(2-hydroxyethyl)ethylenediamine, N-(2-hydroxyethyl)propylenediamine, and N,N'-di(2-hydroxyethyl)ethylenediamine; and diol compounds such as ethylene glycol, propylene glycol, 1,4-butanediol, neopentyl glycol, diethylene glycol, and triethylene glycol.
[0014] Examples of the reaction terminator include monoalcohols such as methanol and ethanol, alkylamines such as n-propylamine, n-butylamine, and di-n-butylamine, alkanolamines such as monoethanolamine and diethanolamine, aliphatic diamines such as ethylenediamine, propylenediamine, tetramethylenediamine, and hexamethylenediamine, alicyclic diamines such as isophoronediamine, 1,4-butanediamine, and 4,4'-dicyclohexylmethanediamine, polyamines such as diethylenetriamine and triethylenetetratriamine, aromatic diamines such as toluylenediamine, aromatic aliphatic diamines such as xylylenediamine, diamines having a hydroxyl group such as N-(2-hydroxyethyl)ethylenediamine, N-(2-hydroxyethyl)propylenediamine, and N,N'-di(2-hydroxyethyl)ethylenediamine, and aminoethylethanolamine.
[0015] In order to obtain the polyurethane resin used in the present invention using the above synthesis components, first, the NCO of the polyisocyanate compound and the OH of the diol compound are reacted so that the molar equivalent ratio (molar equivalent of NCO of the polyisocyanate compound / molar equivalent of OH of the diol compound) is 0.5 or more and 3.0 or less, preferably 1.2 or more and 1.5 or less, and then, if necessary, a chain extender and a reaction terminator are reacted. If the molar equivalent of NCO of the polyisocyanate compound / the molar equivalent of OH of the diol compound is less than 0.5, the heat resistance and oil resistance tend to decrease, whereas if the molar equivalent of NCO of the polyisocyanate compound / the molar equivalent of OH of the diol compound is more than 3, the stretchability tends to decrease.
[0016] (Biomass polyurethane) In consideration of environmental aspects, a part or all of the diol compounds constituting the polyurethane may be diol compounds obtained using biomass components derived from plant components. As such a diol compound, a polyester polyol compound is preferable, and as this polyester polyol compound, a biopolyester polyol (biomass polyester polyol) obtained by reacting a short-chain diol compound having 2 to 4 carbon atoms with a carboxylic acid compound can be used. As for the biopolyol component, it is more preferable that at least one of the short-chain diol compound and the carboxylic acid compound is derived from a plant, and it is even more preferable that both are derived from a plant. The plant-derived short-chain diol compound having 2 to 4 carbon atoms is not particularly limited. For example, the short-chain diol compound may be 1,3-propanediol, 1,4-butanediol, ethylene glycol, etc., which are obtained from plant raw materials by the following method. These may be used in combination. 1,3-propanediol can be produced from glycerol via 3-hydroxypropylaldehyde (HPA) by a fermentation method in which glucose is obtained by decomposing plant resources (such as corn, etc.). The 1,3-propanediol component produced by a biomethod such as the fermentation method is safer than the 1,3-propanediol component of the EO production method, and useful by-products such as lactic acid can be obtained, and the production cost can be kept low. 1,4-butanediol can be produced by producing glycol from plant resources, fermenting it to obtain succinic acid, and hydrogenating it. Ethylene glycol can also be produced from bioethanol obtained by a conventional method via ethylene.
[0017] The carboxylic acid compound derived from a plant is not particularly limited. For example, the carboxylic acid compound is sebacic acid, succinic acid, lactic acid, glutaric acid, dimer acid, etc. These may be used in combination. Among these, the carboxylic acid compound preferably contains at least one selected from the group consisting of sebacic acid, succinic acid, and dimer acid. In addition, 0.05 to 0.5 parts by mass of malic acid may be contained per 100 parts by mass of sebacic acid. The biopolyester polyol compound is produced as a 100% plant-derived biopolyester polyol by appropriately condensing a plant-derived short-chain diol compound and a plant-derived carboxylic acid. Specifically, polytrimethylene sebacate polyol is obtained by directly dehydrating and condensing plant-derived sebacic acid and plant-derived 1,3-propanediol. Also, polybutylene succinate polyol is obtained by directly dehydrating and condensing plant-derived succinic acid and plant-derived 1,4-butanediol. One or more of these biopolyester polyol compounds may be used. The urethane prepolymer obtained from these plant-derived components may be contained in an amount of 10% by mass or more, or 40% by mass or more, calculated as a solid content, in the total urethane prepolymer. Even when a plant-derived component is used in this way, the same chain extenders and reaction terminators as described above can be used.
[0018] (Polyamide resin) The polyamide resin is obtained by reacting an acid component, which may mainly contain polymerized fatty acid, and further may contain aliphatic, alicyclic, and aromatic dicarboxylic acids and aliphatic monocarboxylic acids, with an amine component, which may mainly contain aliphatic, alicyclic, araliphatic, and aromatic polyamines alone or in mixtures, and further may contain primary and secondary monoamines. Here, the polymerized fatty acid is generally obtained by polymerization of unsaturated fatty acids having 16 to 22 carbon atoms or their esters, and includes monobasic fatty acids, dimerized polymerized fatty acids, trimerized polymerized fatty acids, etc. Examples of aliphatic dicarboxylic acids include succinic acid, adipic acid, azelaic acid, maleic acid, etc. Examples of alicyclic dicarboxylic acids include cyclohexanedicarboxylic acid, etc. Examples of aromatic dicarboxylic acids include isophthalic acid, terephthalic acid, etc. Examples of aliphatic monocarboxylic acids include acetic acid, stearic acid, oleic acid, linoleic acid, etc.
[0019] On the other hand, the aliphatic polyamines among the amine components include aliphatic diamines such as ethylenediamine, propylenediamine, hexamethylenediamine, and methylaminopropylamine, and aliphatic polyamines such as diethylenetriamine and triethylenetetramine, and the alicyclic polyamines include cyclohexylenediamine and isophoronediamine. The aromatic aliphatic polyamines include xylylenediamine, and the aromatic polyamines include phenylenediamine and diaminodiphenylmethane. Furthermore, the primary and secondary monoamines include butylamine, octylamine, diethylamine, monoethanolamine, monopropanolamine, diethanolamine, and dipropanolamine. From the viewpoint of the oil resistance, heat resistance and PVC blocking resistance of the ink composition, it is preferable to use a polyamide resin which uses an alkanolamine as the primary or secondary monoamine component and has a hydroxyl group in the molecule. In the method for synthesizing a polyamide resin from the above acid components and amine components, it is desirable to set the ratio of carboxyl groups / amino groups in the reaction components to 0.9 / 1.0 to 1.0 / 0.9, preferably 1.0 / 1.0, at a reaction temperature of 160 to 280°C, preferably 180 to 230°C, and to carry out the reaction under reduced pressure of about 100 torr in the final stage.
[0020] (Thermoplastic polyamide resin using vegetable oil fatty acid as a reaction raw material) Among the above polyamide resins, the thermoplastic polyamide resins using vegetable oil fatty acids as reaction raw materials are not particularly limited. For example, the thermoplastic polyamide resins using vegetable oil fatty acids as reaction raw materials include polyamide resins using vegetable oil fatty acids such as tall oil, rice bran oil, palm oil, coconut oil, soybean oil, etc. as reaction raw materials. By using vegetable oil fatty acids as reaction raw materials, the load on the environment when using such thermoplastic polyamide resins can be reduced. The thermoplastic polyamide resin using vegetable oil fatty acid as a reaction raw material is a polycondensation product of polycarboxylic acid containing vegetable oil fatty acid and polyamine. The polyamine is not particularly limited. For example, the polyamine is an aliphatic polyamine, an alicyclic polyamine, an aromatic polyamine, etc. The aliphatic polyamine is ethylenediamine, diethylenetriamine, triethylenetetramine, tetraethylenepentamine, pentaethylenehexane, piperazine, N-aminoethylpiperazine, etc. The alicyclic polyamine is isophoronediamine, bisaminomethylcyclohexane, etc. The aromatic polyamine is metaxylenediamine, etc. The thermoplastic polyamide resin may be used in combination. The number average molecular weight (Mn) of the thermoplastic polyamide resin is not particularly limited. For example, the Mn of the thermoplastic polyamide resin is preferably 1000 or more. Also, the Mn is preferably 30000 or less. When the Mn of the thermoplastic polyamide resin is less than 1000, the ink composition tends to have reduced blocking resistance and heat resistance. On the other hand, when the Mn exceeds 30000, the ink composition tends to have reduced crumping resistance. The acid value and amine value of the thermoplastic polyamide resin are not particularly limited. For example, the acid value and amine value of the thermoplastic polyamide resin are preferably 10 or less and 5 or less, respectively. The softening point of the thermoplastic polyamide resin is more preferably 90 to 150°C. The content of the thermoplastic polyamide resin is not particularly limited. For example, the content of the thermoplastic polyamide resin is preferably 20% by mass or more and 70% by mass or less based on the total solid content in the ink composition.
[0021] (Acrylic resin) The acrylic resin can be produced by a conventionally known method, and the production method is not particularly limited. The acrylic resin is obtained by polymerizing a monomer having a carbon-carbon unsaturated double bond in one molecule in a solvent in the presence of a polymerization initiator. Examples of the monomer having a carbon-carbon unsaturated double bond in one molecule include (i) (meth)acrylic acid derivatives, (ii) aromatic vinyls, (iii) olefinic hydrocarbons, (iv) vinyl esters, (v) vinyl halides, and (vi) vinyl ethers.
[0022] (i) Examples of (meth)acrylic acid derivatives include (meth)acrylonitrile, (meth)acrylate salts, alkyl (meth)acrylates such as methyl (meth)acrylate, butyl (meth)acrylate, ethylhexyl (meth)acrylate, and stearyl (meth)acrylate, and benzyl (meth)acrylate. (ii) Examples of aromatic vinyls include styrenes in which some hydrogen atoms have been substituted with fluorine, such as styrene, methylstyrene, ethylstyrene, chlorostyrene, monofluoromethylstyrene, difluoromethylstyrene, and trifluoromethylstyrene. (iii) Examples of olefinic hydrocarbons include ethylene, propylene, butadiene, isobutylene, isoprene, and 1,4-pentadiene. (iv) Vinyl esters include vinyl acetate, etc. (v) Vinyl halides include vinyl chloride, vinylidene chloride, and the like. (vi) Examples of vinyl ethers include vinyl methyl ether. In addition, as the monomer having a carbon-carbon unsaturated double bond in one molecule, a monomer having a crosslinkable functional group can be used. Examples of the monomer having a functional group include (vii) a monomer having a hydroxyl group, (viii) a monomer having an isocyano group, and (ix) a monomer having an epoxy group.
[0023] (vii) Examples of monomers having a hydroxyl group include hydroxyalkyl (meth)acrylates such as 2-hydroxyethyl (meth)acrylate, 1-hydroxypropyl (meth)acrylate, 2-hydroxypropyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 8-hydroxyoctyl (meth)acrylate, etc.; glycol mono(meth)acrylates such as polyethylene glycol mono(meth)acrylate, polypropylene glycol mono(meth)acrylate, polytetramethylene glycol mono(meth)acrylate, etc.; and hydroxystyrene. (viii) Examples of monomers having an isocyano group include (meth)acryloyloxyethyl isocyanate, (meth)acryloyloxypropyl isocyanate, and the like, as well as those obtained by reacting a hydroxyalkyl (meth)acrylate, such as 2-hydroxyethyl (meth)acrylate or 4-hydroxybutyl (meth)acrylate, with a polyisocyanate, such as toluene diisocyanate or isophorone diisocyanate. (ix) Examples of monomers having an epoxy group include glycidyl methacrylate, glycidyl cinnamate, glycidyl allyl ether, glycidyl vinyl ether, vinylcyclohexane monoepoxide, and 1,3-butadiene monoepoxide. If necessary, one or more of these monomers having a carbon-carbon unsaturated double bond in one molecule can be used, and it is preferable to set the acid value to 100 to 200. Outside this range, phase separation, an increase in viscosity, and gelation of the ink occur, resulting in problems with storage stability. As a polymerization initiator used in synthesizing the acrylic resin, a typical peroxide or azo compound, such as benzoyl peroxide, azoisobutylvalenonitrile, azobisisobutyronitrile, di-t-butyl peroxide, t-butyl perbenzoate, t-butyl peroctoate, or cumene hydroxyperoxide, is used, and the polymerization temperature is 50 to 140°C, preferably 70 to 140°C. The weight average molecular weight of the resulting polymer is preferably 5,000 to 100,000. The non-aromatic solvent used in the above production method may be ketones such as acetone, methyl ethyl ketone, methyl isobutyl ketone, cyclohexanone, etc., ethers such as tetrahydrofuran, dioxane, ethylene glycol dimethyl ether, diethylene glycol dimethyl ether, etc., esters such as ethyl acetate, butyl acetate, etc. The solvent may be a mixture of two or more kinds.
[0024] (Cellulose derivatives) The cellulose derivative may be any cellulose derivative that has been used in printing ink compositions. Examples of such cellulose derivatives include nitrocellulose (nitro group-substituted), lower acyl group-substituted cellulose derivatives such as cellulose acetate, cellulose acetate propionate, and cellulose acetate butyrate, and lower alkyl group-substituted cellulose derivatives such as methyl cellulose and ethyl cellulose. The molecular weight and degree of substitution of the hydroxyl group of these cellulose derivatives may be within the ranges used in ordinary ink compositions and paints, and may be used without any problems in the present invention.
[0025] The degree of substitution of hydroxyl groups is preferably about 1.3 to 2.7. In addition, from the viewpoint of heat resistance, the use of nitro group-substituted products is advantageous, and from the viewpoint of adhesion, lower acyl group-substituted products and lower alkyl group-substituted products are advantageous, so it is preferable to select and use them appropriately according to the purpose. When a cellulose derivative is contained, the content ratio of the polyurethane resin and the cellulose derivative is preferably, in mass terms, polyurethane resin:cellulose derivative=5:95 to 95:5. The content ratio of the polyamide resin and the cellulose derivative is preferably, polyamide resin:cellulose derivative=95:5 to 70:30. The content ratio of the acrylic resin and the cellulose derivative is preferably, acrylic resin:cellulose derivative=95:5 to 30:70.
[0026] (Vinyl chloride / vinyl acetate copolymer resin) Vinyl chloride-vinyl acetate copolymer resins can be produced by known methods using the vinyl chloride monomer and vinyl acetate monomer that have been conventionally used in gravure printing ink compositions as essential components, and, if necessary, fatty acid vinyl monomers such as vinyl propionate, vinyl monochloroacetate, vinyl versatate, vinyl laurate, vinyl stearate, vinyl benzoate, and monomers having functional groups such as hydroxyl groups as copolymerization components. Such vinyl chloride-vinyl acetate copolymer resins having hydroxyl groups can be obtained by partially saponifying the acetate moieties and by introducing (meth)acrylic monomers having hydroxyl groups. In the case of vinyl chloride-vinyl acetate copolymer resins with hydroxyl groups obtained by partially saponifying the acetate ester moieties, the film properties and dissolution behavior of the resin are determined by the ratio of the structural units based on the reactive sites of vinyl chloride (formula 1 below), the structural units based on the reactive sites of vinyl acetate (formula 2 below), and the structural units based on the saponification of the reactive sites of vinyl acetate (formula 3 below) in the molecule. In other words, the structural units based on the reactive sites of vinyl chloride give the resin film its toughness and hardness, the structural units based on the reactive sites of vinyl acetate give it adhesion and flexibility, and the structural units based on the saponification of the reactive sites of vinyl acetate give it good solubility in organic solvent systems for environmentally friendly inks. Formula 1 -CH2-CHCl- Formula 2 -CH2-CH(OCOCH3)- Formula 3 -CH2-CH(OH)- From the viewpoints of solubility in organic solvents described below and printability used in the detachment printing ink composition of the present invention, the above vinyl chloride-vinyl acetate copolymer resin may have various functional groups in the molecule. When an environmentally friendly solvent is used as the organic solvent, the vinyl chloride-vinyl acetate copolymer preferably has a hydroxyl group concentration of 50 to 200 mg KOH / g. Commercially available vinyl chloride-vinyl acetate copolymer resins such as Solvin A, AL, TA5R, TA2, TA3, TAO, and TAOL are preferably used. When a cellulose derivative is contained, the content ratio of the vinyl chloride / vinyl acetate copolymer resin to the cellulose derivative is preferably, in mass terms, vinyl chloride / vinyl acetate copolymer resin:cellulose derivative=5:95 to 30:70.
[0027] (rosin resin) Examples of rosin include gum rosin, tall oil rosin, wood rosin, etc. Generally, rosin is an amber-colored, amorphous resin obtained from pine trees, and since it is obtained naturally, it is a mixture, but it may be used after being isolated into its constituent components, namely abietic acid, neoabietic acid, palustric acid, pimaric acid, isopimaric acid, sandaracopimaric acid, and dehydroabietic acid, and these are also defined as rosin in the present invention. The rosin derivatives are compounds obtained by modifying the above-mentioned rosins, and specific examples thereof are listed below. (1) Hydrogenated rosin: A rosin whose weather resistance has been improved by adding hydrogen to the conjugated double bonds (hydrogenation). (2) Disproportionated rosin: Disproportionation is a process in which two molecules of rosin react with each other, and two molecules of abietic acid with conjugated double bonds are modified, one to an aromatic molecule and the other to a molecule with a single double bond. In general, disproportionated rosin is less weather resistant than hydrogenated rosin, but its weather resistance is better than that of untreated rosin. (3) Rosin-modified phenolic resin: Rosin-modified phenolic resin is often used as the main binder in offset printing inks. Rosin-modified phenolic resin can be obtained by known manufacturing methods. (4) Rosin ester: An ester resin derived from rosin, which has long been used as a tackifier in adhesives and adhesives. (5) Rosin-modified maleic acid resin: This is obtained by adding maleic anhydride to rosin, and may also include those in which a hydroxyl-containing compound such as glycerin is esterified with the anhydride group and grafted, if necessary. (6) Polymerized rosin: A derivative containing dimerized resin acid derived from the natural resin rosin. In addition, known rosins and rosin derivatives can also be used, and these can be used alone or in combination. From the viewpoint of releasability, the rosin resin has an acid value of 100 to 350 mgKOH / g, more preferably 200 to 350 mgKOH / g, and further preferably 250 to 350 mgKOH / g. Among the rosin resins, rosin maleic acid resin and / or polymerized rosin are preferred. The content of the rosin resin in the ink composition is 0.1 to 5.0% by mass, preferably 0.5% by mass or more, more preferably 1.0% by mass or more, and even more preferably 1.5% by mass or more, and is preferably 4.0% by mass or less, more preferably 3.0% by mass or less, and even more preferably 2.5% by mass or less. The content of the rosin resin in the solid content of the ink composition is preferably 0.3 to 10.0% by mass, more preferably 1.0% by mass or more, even more preferably 2.0% by mass or more, and most preferably 2.5% by mass or more, more preferably 6.0% by mass or less, even more preferably 5.0% by mass or less, and most preferably 4.0% by mass or less.
[0028] (Other resins) Other resins that may be used as necessary in the ink composition of the present invention include dimer acid resins, maleic acid resins, petroleum resins, terpene resins, ketone resins, dammar resins, copal resins, chlorinated polypropylene, and oxidized polypropylene. By using these hard resins, it is expected that the adhesion will be improved, especially for resin films that have not been surface-treated. The content of the hard resin in the detachment printing ink composition of the present invention is preferably less than 5.0% by mass.
[0029] (Chelating Crosslinker) As the chelate crosslinking agent, a metal chelate crosslinking agent such as a titanium chelate or a zirconium chelate can be used. Examples of titanium chelates include titanium alkoxides such as tetraisopropyl titanate, tetra-n-butyl titanate, butyl titanate dimer, tetra(2-ethylhexyl) titanate, a reaction product of tetraisopropoxytitanium with 2-ethylhexanoic acid, tetramethyl titanate, and tetrastearyl titanate, triethanolamine titanate, titanium acetylacetate, titanium ethylacetoacetate, titanium lactate, octylene glycol titanate, titanium tetraacetylacetonate, n-butyl phosphate titanium, and propanedioxytitanium bis(ethyl acetylacetate). Examples of zirconium chelates include zirconium propionate and zirconium acetylacetate. From the environmental viewpoint, among the chelating crosslinking agents, a chelating crosslinking agent that does not have acetylacetonate as a ligand is preferred so as not to generate acetylacetone after the crosslinking reaction.
[0030] (Fatty acid amide) From the viewpoint of blocking resistance, fatty acid amide is used. Examples of fatty acid amide include saturated fatty acid amide, unsaturated fatty acid amide, modified fatty acid amide, etc., and it is particularly preferable to use modified fatty acid amide in order to improve blocking resistance to soft polyvinyl chloride sheets used for tablecloths. The content of fatty acid amide when it is contained is preferably 0.1 to 3.0 mass %, more preferably 0.5 to 2.0 mass %, in the detachment printing ink composition. If the content is less than 0.1% by mass, blocking resistance may decrease, whereas if it exceeds 3.0% by mass, oil resistance may decrease.
[0031] (Organic solvent) As the organic solvent, it is preferable to use an organic solvent that does not contain an aromatic hydrocarbon organic solvent in consideration of the environment. As the organic solvent that does not contain an aromatic hydrocarbon organic solvent, mainly, alcohol organic solvents such as methanol, ethanol, n-propanol, isopropanol, butanol, ketone organic solvents such as acetone, methyl ethyl ketone, methyl isobutyl ketone, ester organic solvents such as methyl acetate, ethyl acetate, propyl acetate, butyl acetate, aliphatic hydrocarbon organic solvents such as n-hexane, n-heptane, n-octane, and alicyclic hydrocarbon organic solvents such as cyclohexane, methylcyclohexane, ethylcyclohexane, cycloheptane, cyclooctane can be mentioned, and they can be used in a mixture in consideration of the solubility and drying property of the binder resin. However, in consideration of the environmental aspect, it is preferable to suppress ketone organic solvents as much as possible among the above organic solvents. The amount of these organic solvents used is 15.0% by mass or more in the detachment printing ink composition of the present invention, taking printability into consideration. From the viewpoint of printability, it is preferable to contain 5.0% by mass or more, more preferably 10.0% by mass or more, of propyl acetate in the ink composition. In order to improve printability, it is preferable to contain 0.1 to 10% by mass of water in the organic solvent.
[0032] (Additives that can be added as needed) For the purpose of improving the abrasion resistance, wax can be added within a range that does not deteriorate the performance. As the wax, various known waxes such as polyolefin wax and paraffin wax can be used. Furthermore, various ink additives such as pigment dispersants, leveling agents, surfactants, plasticizers, etc. may be added as desired.
[0033] (Method of manufacturing ink composition) The method for producing an ink composition using these materials involves first stirring and mixing the pigment, binder resin, organic solvent, and, if necessary, a pigment dispersant, surfactant, etc., and then grinding using various grinding machines, such as a bead mill, ball mill, sand mill, attritor, roll mill, pearl mill, etc., and then adding and mixing the fatty acid amide, chelating crosslinker, and remaining materials. The ink composition obtained from the above materials and production method can be printed using a conventional gravure printing method.
[0034] (Printed material) Next, the printed matter using the ink composition will be specifically described. The substrate to be printed may be either paper or plastic, but resin film is preferred. Examples of such resin films include stretched and unstretched polyolefin films such as polyethylene and polypropylene, polyester, nylon, cellophane, vinylon, and other films. Furthermore, these resin films are films obtained by processing the resin film in advance, such as coating or kneading an anti-fogging agent, or surface coating or kneading a matting agent. The printed matter of the present invention can be obtained, for example, by printing the ink composition in a single color or by overprinting each color on the resin film by gravure printing and drying it with a dryer. The ink film formed by printing has a dry film thickness of 0.1 to 2.0 g / m. 2 The appropriate application amount is 100%.
[0035] (Method for removing ink composition film from printed matter) As a method for removing the ink composition coating from a printed matter printed on the front or back side with the printing ink composition for detachment of the present invention and separating the substrate from the ink composition, a method can be adopted in which the printed matter is cut into small pieces by any means, immersed in an alkaline aqueous solution in which a basic compound such as sodium hydroxide or potassium hydroxide is dissolved as the detachment liquid, and stirred as necessary. In this case, the concentration of sodium hydroxide or potassium hydroxide is preferably 0.5 to 15 mass%, more preferably 1.0 mass% or more, and even more preferably 1.5 mass% or more. In addition, 5.0 mass% or less is preferable when treating waste liquid after use, and 3.0 mass% or less is more preferable.
[0036] The alkaline aqueous solution used for desorption may be at room temperature, about 25° C., or may be heated to 25 to 90° C. Furthermore, it may be at 30° C. or higher. The immersion time is preferably 1 minute to 12 hours, more preferably 1 hour or less, further preferably 30 minutes or less, and most preferably 10 minutes or less. At the same time, it is preferable to treat the divided printed matter with a sufficiently large amount of alkaline aqueous solution, that is, 1 to 1,000,000 times the mass of the printed matter, in order to achieve smooth desorption. If the substrate of the printed matter is, for example, polyester, this removal method can be used to remove the ink composition coating in an alkaline aqueous solution, and the separated polyester can be washed with water and dried to obtain a recycled polyester substrate. The recycled polyester substrate can also be recycled into pellets using an extruder for reuse.
[0037] For example, the following two types of release liquid 1 or 2 can be used. [Removal solution 1] An alkaline aqueous solution can be used in which an alkali metal hydroxide such as sodium hydroxide or potassium hydroxide is dissolved in water. The concentration of the alkaline aqueous solution is preferably 0.5 to 15 mass%, and more preferably 1 to 5 mass%. When the concentration is within the above range, the alkaline aqueous solution can maintain sufficient alkalinity for desorption. From the viewpoint of environmental friendliness and handling of waste liquid in the recycling process, the concentration of the alkaline aqueous solution is preferably 5% or less.
[0038] [Removal solution 2] An alkaline aqueous solution containing water, a basic compound, and a polyoxyalkylene alkyl derivative can be used. As the basic compound, an alkaline metal hydroxide such as sodium hydroxide or potassium hydroxide can be used, and the concentration of the alkaline aqueous solution in the alkaline aqueous solution is preferably 0.5 to 15 mass%, more preferably 1 to 5 mass%. By having the concentration within the above range, the alkaline aqueous solution can maintain sufficient alkalinity for desorption. From the viewpoint of environmental friendliness and handling of waste liquid in the recycling process, it is preferable that the concentration of the alkaline aqueous solution is 5% or less. As the polyoxyalkylene alkyl derivative, polyoxyalkylene alkyl phenyl ether, specifically, polyethylene glycol (10) octyl phenyl ether, poly(oxyethylene) nonyl phenyl ether, etc. can be used. The amount of the polyoxyalkylene alkyl derivative used in the aqueous alkaline solution is preferably in the range of 0.05 to 3% by mass. EXAMPLES
[0039] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. Unless otherwise specified, "%" means "% by mass" and "parts" means "parts by mass."
[0040] <Removal printing ink composition> Pigment: Carbon black Polyamide resin: Thermoplastic polyamide resin made from tall oil fatty acid (Mn 8000, acid value 2, softening point 110℃) Thermoplastic polyamide resin (Mn 6000, acid value 1.6, softening point 112℃) made from rice bran oil fatty acid as a reaction raw material
[0041] Polyurethane resin (30% solids varnish) A four-neck flask equipped with a stirrer, a cooling tube, and a nitrogen gas inlet tube was charged with 100 parts by mass of 3-methyl-1,5-pentylene adipate diol having an average molecular weight of 2000, 100 parts by mass of polypropylene glycol having an average molecular weight of 2000, and 44.4 parts by mass of isophorone diisocyanate, and reacted for 6 hours at 100 to 105°C while introducing nitrogen gas. The mixture was allowed to cool to near room temperature, and 521 parts by mass of ethyl acetate and 92 parts by mass of isopropyl alcohol were added, followed by adding 15.6 parts by mass of isophorone diamine to extend the chain, and then adding 0.31 parts by mass of monoethanolamine to react, and then adding 2.18 parts by mass of isophorone diamine and 0.17 parts by mass of diethylene triamine to stop the reaction, to obtain a polyurethane resin varnish (solid content 30% by mass).
[0042] Biomass polyurethane resin (30% solids varnish) A four-neck flask equipped with a stirrer, a cooling tube, and a nitrogen gas inlet tube was charged with 200 parts by mass of polyester diol with an average molecular weight of 2000 obtained from sebacic acid (derived from castor oil) / succinic acid (derived from plant) = 70 / 30 (mass ratio) and 1,3-propanediol (derived from plant), 17.6 parts by mass of isophorone diisocyanate, and 21.0 parts by mass of hydrogenated MDI, and reacted for 6 hours at 100-105 ° C while introducing nitrogen gas. The mixture was allowed to cool to near room temperature, and 400 parts by mass of ethyl acetate and 171 parts by mass of isopropyl alcohol were added, followed by adding 8.2 parts by mass of isophorone diamine to extend the chain, and then adding 0.35 parts by mass of monoethanolamine to react, and then adding 1.3 parts by mass of isophorone diamine and 0.6 parts by mass of diethylene triamine to stop the reaction, to obtain a polyurethane resin varnish (solid content 30 mass %).
[0043] Cellulose Derivatives Nitrocellulose solution (20% solids) 20 parts by mass of nitrocellulose (NC RS-2 KCNC, manufactured by KOREA CNC LTD.) was dissolved in a mixed solvent consisting of 35 parts by mass of propyl acetate and 45 parts by mass of isopropyl alcohol to obtain a nitrocellulose solution with a solid content of 20%.
[0044] Vinyl chloride / vinyl acetate copolymer solution (25% solids) 25 parts of vinyl chloride / vinyl acetate copolymer (product name: Solvine TA5R, manufactured by Nissin Chemical Industry Co., Ltd.) was dissolved in a mixed organic solvent consisting of 37.5 parts of methyl ethyl ketone, 18.75 parts of ethyl acetate, and 18.75 parts of propyl acetate to obtain a vinyl chloride / vinyl acetate copolymer solution with a solid content of 25%.
[0045] Rosin Resin Rosin maleic acid resin: acid value 290-320mgKOH / mg Polymerized rosin resin: acid value 145mgKOH / mg Chelating Crosslinker Titanium acetylacetonate · Chlorinated PP (chlorinated propylene (solids 20%)) 40 parts by mass of chlorinated polypropylene (solid content 50%) having a chlorination degree of 40% and a number average molecular weight of 10,000 and 60 parts by mass of methylcyclohexane were mixed and stirred to obtain a chlorinated propylene varnish having a solid content of 20%.
[0046] (Ink composition preparation, printing and evaluation) Ink compositions were prepared by kneading the materials in a paint conditioner according to the mass ratios (mass%) in Table 1 below. The resulting ink compositions were subjected to gravure printing under the following conditions to obtain printed matter. The resulting printed matter was evaluated for adhesion and releasability according to the following evaluation methods. Base Film Low density polyethylene (LLDPE, film thickness 50μm) Non-oriented polypropylene (CPP, film thickness 25μm) - Oriented polypropylene (OPP, film thickness 25μm) Nylon film (NY, thickness 12μm) Polyethylene terephthalate (PET, film thickness 12μm)
[0047] <Creating printed matter> The ink composition shown in Table 1 was further diluted with a mixed solvent of n-propyl acetate / isopropyl alcohol = 80 / 20 using a Rigo Zahn Cup No. 3 to a viscosity of 16 seconds. This diluted ink composition was applied onto the above film using a bar coater with a line diameter of 0.15 mm to obtain a printed matter.
[0048] <Evaluation of Adhesion> Adhesion was evaluated according to the following criteria based on the degree to which the printed film peeled off when cellophane tape was applied to the printed surface of each printed matter and then quickly peeled off. (Evaluation Criteria) A: The area ratio of the printed coating that peeled off from the film was less than 5%. B: 5% or more and less than 30% of the area of the printed coating peeled off from the film. C: 30% or more of the area of the printed coating peeled off from the film.
[0049] <Evaluation of ink release properties> 1.5 g of the above printed matter was cut into small pieces of approximately 15 mm MD×25 mm TD to obtain samples for the ink release property test. (Preparation of the release solution consisting of an alkaline aqueous solution) 2 parts by mass of sodium hydroxide was added to 98.0 parts by mass of water, and the mixture was stirred and dissolved to obtain a release liquid consisting of an alkaline aqueous solution. (Preheating of the desorption solution) 100 g of the above-mentioned elution liquid was placed in a 200 cc HDPE (high density polyethylene) container and heated in a hot water bath until the liquid temperature reached 70°C. (Detachment) After the release liquid reached 70°C, the ink release test sample was placed in the release liquid and stirred for 20 minutes using a stainless steel stirring blade with a blade diameter of 25 mm. After stirring, the HDPE (high density polyethylene) container was removed from the hot water bath and allowed to stand at room temperature for 5 minutes. The release liquid and the various film pieces were separated using a stainless steel mesh with mesh openings of approximately 2 mm. (rinse) After the detachment, the various films were transferred to a 200cc HDPE container and 100g of water was added. The mixture was stirred for 5 minutes using a stainless steel stirring blade. After leaving the mixture to stand for 5 minutes, the various film pieces were separated from the water using a stainless steel mesh. After drying the various film pieces, the peelability of the ink from the various films was visually evaluated. The ink coating was completely peeled off from the film as coating pieces, and the results were: Those that were about half peeled off were marked △, Those that did not peel at all were marked with "X".
[0050] [Table 1]
[0051] The ink compositions of the Examples and Comparative Examples all exhibited excellent adhesion to various substrates. However, while the releasability was excellent in each of the Examples, the releasability was insufficient in each of the Comparative Examples which did not contain a rosin-based resin.
Claims
1. A printing ink composition for detachment comprising a pigment, a binder resin containing a polyurethane resin substantially having no acid groups and / or a polyamide resin, and a rosin-based resin having an acid value of 100 to 350 mgKOH / g in an amount of 0.1 to 5.0 mass% in the ink composition, and an organic solvent. (However, the packaging material includes at least a first substrate, a primer layer for removing the first substrate and recycling the first substrate, and a printed layer in this order, The primer composition used to form the primer layer is a printing ink composition used in a printing layer of a packaging material, which contains, as a binder resin, a resin (A) having a weight average molecular weight (Mw) of 70% or less (Mw before immersion is taken as 100%) after immersion in a 1 mass % sodium hydroxide aqueous solution at 60°C for 12 hours. (Excluding
2. 2. The detachable printing ink composition according to claim 1, wherein the rosin-based resin is a rosin-modified maleic acid resin and / or a polymerized rosin resin.
3. The binder resin is (A) a binder resin containing a polyurethane resin and / or a polyamide resin and a cellulose derivative; or (B) a binder resin containing a polyurethane resin and a vinyl chloride-vinyl acetate copolymer resin, the solid content ratio of which is polyurethane resin / vinyl chloride-vinyl acetate copolymer resin=100 / 0 to 70 / 30; The detachable printing ink composition according to claim 1 or 2,
4. The detachable printing ink composition according to claim 3, wherein the polyurethane resin is a polyester polyether type polyurethane resin.
5. A method for removing a detachable printing ink composition, comprising removing a coating of the detachable surface printing ink composition from a printed matter formed by printing the detachable printing ink composition according to any one of claims 1 to 4 on a substrate in a removing liquid comprising an alkaline aqueous solution.
Citation Information
Patent Citations
JP1988088131A
Resin for printing ink
JP1993097959A
Ink composition having elimination performance and method for eliminating ink composition from print
JP1999209677A
Easily separable ink composition for laminate printing
JP2000313833A
Releasable ink composition and method for releasing the ink composition from printed substrate
JP2001031899A