Soft magnetic powder, dust core, magnetic element and electronic device
The formulation of Fe x Cu a Nb b (Si 1-y B y ) 100-x-a-b soft magnetic powder with specific atomic percentages and crystal grain characteristics addresses the challenge of high-current saturation, achieving low coercive force and high saturation magnetic flux density for efficient and compact magnetic elements.
Patent Information
- Application Number
- JP2021018523
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-02-08
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-02-08
AI Technical Summary
Existing soft magnetic powders, as described in Patent Document 1, face challenges in stably achieving excellent soft magnetism under high current conditions, particularly in terms of reducing coercive force and increasing saturation magnetic flux density to prevent saturation at high currents.
The soft magnetic powder composition Fe x Cu a Nb b (Si 1-y B y ) 100-x-a-b is formulated with specific atomic percentages (0.3≦a≦2.0, 2.0≦b≦4.0, 73.0≦x≦79.5, f(x)≦y≦0.99) and includes crystal grains of 1.0 nm to 30.0 nm, with a Cu segregation area deeper than 30 nm and a maximum Cu concentration of over 6.0 atomic %.
This configuration results in a soft magnetic powder with low coercive force and high saturation magnetic flux density, enabling a powder magnetic core that withstands high currents with minimal iron loss and allows for miniaturized, high-efficiency magnetic elements.
Smart Images

Figure 0007574681000003 
Figure 0007574681000004 
Figure 0007574681000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a soft magnetic powder, a dust core, a magnetic element, and an electronic device. [Background technology]
[0002] In various mobile devices equipped with magnetic elements containing powder magnetic cores, in order to reduce size and increase output, the switching power supply must be compatible with high frequencies and high currents in conversion frequency, which requires that the soft magnetic powder contained in the powder magnetic cores must also be compatible with high frequencies and high currents.
[0003] In Patent Document 1, Fe x Cu a Nb b (Si 1-y B y ) 100-x-a-b [where a, b, and x are each in atomic percent and are numbers that satisfy 0.3≦a≦2.0, 2.0≦b≦4.0, and 73.0≦x≦79.5. Also, y is a number that satisfies f(x)≦y<0.99. Note that f(x)=(4×10 -34 )x 17.56 The present invention discloses a soft magnetic powder having a composition represented by the formula: and containing 30% by volume or more of a crystal structure having a grain size of 1.0 nm to 30.0 nm. Such soft magnetic powder contains minute crystals, which allows for low iron loss at high frequencies. [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2019-189928 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, the soft magnetic powder described in Patent Document 1 still has room for improvement in terms of stably achieving excellent soft magnetism even under high current. Specifically, the soft magnetic powder has to have a further reduced coercive force and a further increased saturation magnetic flux density so that the green compact does not become saturated even under high current. [Means for solving the problem]
[0006] The soft magnetic powder according to the application example of the present invention is Fe x Cu a Nb b (Si 1-y B y ) 100-x-a-b [where a, b, and x are numbers in atomic percent, and satisfy 0.3≦a≦2.0, 2.0≦b≦4.0, and 73.0≦x≦79.5. Also, y is a number that satisfies f(x)≦y≦0.99, and f(x)=(4×10 -34 )x 17.56 It is.] The particles have a composition represented by The particles contain crystal grains having a particle size of 1.0 nm or more and 30.0 nm or less, The content ratio of the crystal grains in the particles is 30% by volume or more, The Cu segregation area includes a Cu segregation area. the Cu segregation portion is present at a depth of 30 nm or more from the surface of the particle, The maximum Cu concentration in the Cu segregation portion is characterized by exceeding 6.0 atomic %.
[0007] The powder magnetic core according to the application example of the present invention is The soft magnetic powder according to the application example of the present invention is included.
[0008] The magnetic element according to the application example of the present invention includes: The present invention is characterized by including a powder magnetic core according to an application example of the present invention.
[0009] The electronic device according to the application example of the present invention includes: The present invention is characterized by including a magnetic element according to an application example of the present invention. [Brief description of the drawings]
[0010] [Figure 1] FIG. 2 is a diagram showing a region where the range of x and the range of y in the composition formula of the soft magnetic powder according to the embodiment overlap in a two-axis orthogonal coordinate system with x being the horizontal axis and y being the vertical axis. [Diagram 2] FIG. 1 is a vertical cross-sectional view showing an example of an apparatus for producing soft magnetic powder by a rotating water jet atomization method. [Diagram 3] FIG. 2 is a plan view illustrating a schematic diagram of a toroidal type coil component. [Figure 4] FIG. 2 is a see-through perspective view that typically illustrates a closed magnetic circuit type coil component. [Diagram 5] FIG. 1 is a perspective view showing a configuration of a mobile personal computer, which is an electronic device including a magnetic element according to an embodiment. [Figure 6] FIG. 1 is a plan view showing a configuration of a smartphone, which is an electronic device including a magnetic element according to an embodiment. [Figure 7] FIG. 1 is a perspective view showing a configuration of a digital still camera, which is an electronic device including a magnetic element according to an embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0011] The soft magnetic powder, the dust core, the magnetic element, and the electronic device of the present invention will be described in detail below with reference to preferred embodiments shown in the accompanying drawings.
[0012] 1. Soft magnetic powder The soft magnetic powder according to the embodiment is a metal powder exhibiting soft magnetism. Such soft magnetic powder can be used for any purpose, but for example, the particles are bound together via a binder and used to manufacture various types of compacts such as dust cores and electromagnetic wave absorbing materials.
[0013] The soft magnetic powder according to the embodiment is Fe x Cu a Nb b (Si1-y B y ) 100-x-a-b The particles include particles having a composition represented by the formula:
[0014] a, b, and x are each a number whose unit is atomic %, and a satisfies 0.3≦a≦2.0, b satisfies 2.0≦b≦4.0, and x satisfies 73.0≦x≦79.5.
[0015] Also, y satisfies f(x)≦y≦0.99. And, f(x)=(4×10 -34 )x 17.56 It is.
[0016] Furthermore, the particles contained in the soft magnetic powder according to the embodiment contain crystal grains with a grain size of 1.0 nm to 30.0 nm, and also contain a Cu segregation portion in which Cu is segregated. The Cu segregation portion is present at a position deeper than 30 nm from the surface of the particle. The maximum Cu concentration of the Cu segregation portion is more than 6.0 atomic %.
[0017] Such soft magnetic powders have both low coercivity and high saturation magnetic flux density. This makes it possible to realize a powder magnetic core that has low iron loss and is not easily saturated even at high currents. This makes it possible to realize a magnetic element that can handle high currents, can be miniaturized, and can achieve high efficiency and high output.
[0018] The composition of the particles of the soft magnetic powder according to the embodiment will be described below. 1.1. Composition Fe (iron) has a significant effect on the basic magnetic properties and mechanical properties of the soft magnetic powder according to the embodiment.
[0019] The Fe content x is 73.0 atomic % or more and 79.5 atomic % or less, preferably 75.0 atomic % or more and 78.5 atomic % or less, more preferably 75.5 atomic % or more and 78.0 atomic % or less. If the Fe content x is below the lower limit, the saturation magnetic flux density of the soft magnetic powder may decrease. On the other hand, if the Fe content x is above the upper limit, it may be difficult to form an amorphous structure stably during the production of the soft magnetic powder, and therefore it may be difficult to form crystal grains having a fine grain size as described above.
[0020] When the soft magnetic powder according to the embodiment is manufactured from raw materials, Cu (copper) tends to separate from Fe. Therefore, the inclusion of Cu causes fluctuations in the composition, and regions that are easily crystallized are generated in the particles. As a result, the precipitation of the body-centered cubic lattice Fe phase, which is relatively easy to crystallize, is promoted, and it is possible to easily form crystal grains having a small grain size as described above.
[0021] The Cu content a is 0.3 atomic % or more and 2.0 atomic % or less, preferably 0.5 atomic % or more and 1.5 atomic % or less, more preferably 0.7 atomic % or more and 1.3 atomic % or less. If the Cu content a is below the lower limit, the crystal grains may not be finely divided, and it may be impossible to form crystal grains having a particle size within the above-mentioned range. On the other hand, if the Cu content a is above the upper limit, the mechanical properties of the soft magnetic powder may be reduced and the powder may become brittle.
[0022] When powder containing a large amount of amorphous structure is heat-treated, Nb (niobium) contributes to the refinement of crystal grains together with Cu, which makes it easier to form crystal grains having a fine grain size as described above.
[0023] The Nb content b is 2.0 atomic % or more and 4.0 atomic % or less, preferably 2.5 atomic % or more and 3.5 atomic % or less, more preferably 2.7 atomic % or more and 3.3 atomic % or less. If the Nb content b is below the lower limit, the crystal grains may not be finely divided, and crystal grains having a particle size within the above-mentioned range may not be formed. On the other hand, if the Nb content b is above the upper limit, the mechanical properties of the soft magnetic powder may be deteriorated and the soft magnetic powder may become brittle. In addition, the magnetic permeability of the soft magnetic powder may be reduced.
[0024] Si (silicon) promotes amorphization when the soft magnetic powder according to the embodiment is manufactured from raw materials. Therefore, when manufacturing the soft magnetic powder according to the embodiment, a homogeneous amorphous structure is first formed, and then, by crystallizing it, crystal grains with a more uniform grain size are easily formed. And, the uniform grain size contributes to averaging the crystalline magnetic anisotropy in each crystal grain, so that the coercive force can be reduced and the magnetic permeability can be increased, thereby improving the soft magnetic property.
[0025] B (boron) promotes amorphization when the soft magnetic powder according to the embodiment is manufactured from raw materials. Therefore, when manufacturing the soft magnetic powder according to the embodiment, a homogeneous amorphous structure is formed once, and then, by crystallizing it, crystal grains with a more uniform grain size are easily formed. And, since the uniform grain size contributes to averaging the magnetocrystalline anisotropy in each crystal grain, the coercive force can be reduced and the magnetic permeability can be increased, and the soft magnetic property can be improved. In addition, by using Si and B in combination, amorphization can be promoted synergistically based on the difference in the atomic radii of the two.
[0026] Here, when the sum of the contents of Si and B is 1 and the ratio of the content of B to this total is y, the ratio of the content of Si to the total is (1-y).
[0027] Here, y is a number that satisfies f(x)≦y≦0.99. And, f(x), which is a function of x, is f(x)=(4×10 -34 )x 17.56It is.
[0028] FIG. 1 is a diagram showing a region where the range of x and the range of y in the composition formula of the soft magnetic powder according to the embodiment overlap in a two-axis orthogonal coordinate system with x being the horizontal axis and y being the vertical axis.
[0029] In FIG. 1, area A where the x range and the y range overlap is inside the solid line drawn on the Cartesian coordinate system.
[0030] Specifically, region A is a closed region surrounded by three straight lines and one curve when the (x, y) coordinates that satisfy the four equations x = 73.0, x = 79.5, y = f(x), and y = 0.99 are plotted on a Cartesian coordinate system.
[0031] In addition, y is preferably a number that satisfies f'(x)≦y≦0.97. And, f'(x), which is a function of x, is expressed as f'(x)=(4×10 -29 )x 14.93 It is.
[0032] The dashed line in FIG. 1 indicates a region B where the above-mentioned preferable range of x and the above-mentioned preferable range of y overlap.
[0033] Specifically, region B is a closed region surrounded by three straight lines and one curve when the (x, y) coordinates that satisfy the four equations x = 75.0, x = 78.5, y = f'(x), and y = 0.97 are plotted on a Cartesian coordinate system.
[0034] Furthermore, y is more preferably a number that satisfies f"(x)≦y≦0.95. And, f"(x), which is a function of x, is expressed as f"(x)=(4×10 -29 )x 14.93 It is +0.05.
[0035] The dashed dotted line in FIG. 1 indicates a region C where the above-mentioned more preferable range of x and the above-mentioned more preferable range of y overlap.
[0036] Specifically, region C corresponds to a closed region enclosed by three straight lines and one curve when the (x, y) coordinates that satisfy the four equations x = 75.5, x = 78.0, y = f"(x), and y = 0.95 are plotted on a Cartesian coordinate system.
[0037] When soft magnetic powder in which x and y are at least included in region A is manufactured, it is highly likely to form a homogeneous amorphous structure. Therefore, by crystallizing it, crystal grains of particularly uniform grain size can be formed. This results in a soft magnetic powder with a sufficiently reduced coercive force. In addition, by using this soft magnetic powder, the iron loss of the powder magnetic core can be sufficiently reduced.
[0038] In addition, soft magnetic powders in which x and y are at least in region A can form uniform crystal grains even when the Fe content is sufficiently increased. This allows soft magnetic powders with sufficiently increased saturation magnetic flux density to be obtained. As a result, a powder magnetic core can be obtained that has a high saturation magnetic flux density while sufficiently reducing iron loss.
[0039] If the value of y is smaller than that of region A, the balance between the content of Si and the content of B is lost, making it difficult to form a homogeneous amorphous structure when the soft magnetic powder is produced. As a result, crystal grains with a small grain size cannot be formed, and the coercive force cannot be sufficiently reduced.
[0040] On the other hand, when the value of y is larger than that of region A, the balance between the content of Si and the content of B is lost, so that it becomes difficult to form a homogeneous amorphous structure when the soft magnetic powder is produced. As a result, crystal grains with a small grain size cannot be formed, and the coercive force cannot be sufficiently reduced.
[0041] The lower limit of y is determined by the function of x as described above, but is preferably 0.30 or more, more preferably 0.45 or more, and even more preferably 0.55 or more, which allows the soft magnetic powder to have a higher saturation magnetic flux density.
[0042] In particular, in regions B and C, the value of x is large even in region A, and therefore the Fe content is high. This makes it easier to increase the saturation magnetic flux density of the soft magnetic powder. Therefore, by using soft magnetic powder in which x and y are at least included in region B, it is possible to reduce the size and increase the output of powder cores and magnetic elements.
[0043] In addition, the sum of the Si content and the B content, (100-xab), is not particularly limited, but is preferably 15.0 atomic % or more and 24.0 atomic % or less, more preferably 16.0 atomic % or more and 23.0 atomic % or less, and even more preferably 16.0 atomic % or more and 22.0 atomic % or less. By having (100-xab) within the above range, crystal grains with a particularly uniform grain size can be formed in the soft magnetic powder.
[0044] Considering the above, y(100-xab) corresponds to the content of B in the soft magnetic powder. y(100-xab) is appropriately set in consideration of the coercive force and saturation magnetic flux density as described above, and preferably satisfies 5.0≦y(100-xab)≦17.0, more preferably satisfies 7.0≦y(100-xab)≦16.0, and even more preferably satisfies 8.0≦y(100-xab)≦15.0.
[0045] This results in a soft magnetic powder containing a relatively high concentration of B (boron). Even if the soft magnetic powder has a high Fe content, it is possible to form a homogeneous amorphous structure during production. Therefore, by subsequent heat treatment, crystal grains with small and relatively uniform grain sizes can be formed, and the coercive force can be sufficiently reduced while achieving a high magnetic flux density.
[0046] If y(100-xab) is below the lower limit, the content of B is small, and depending on the overall composition, it may be difficult to make the soft magnetic powder amorphous when it is produced. On the other hand, if y(100-xab) is above the upper limit, the content of B is large and the content of Si is relatively low, and therefore the magnetic permeability of the soft magnetic powder may decrease, and the saturation magnetic flux density may decrease.
[0047] In addition, the soft magnetic powder according to the embodiment contains the above-mentioned Fe x Cu a Nb b (Si 1-y B y ) 100-x-a-b In addition to the composition represented by the formula (1), impurities may be included. The impurities may include any elements other than those mentioned above, but it is preferable that the total content of the impurities is 0.50 atomic % or less. Within this range, the impurities are not likely to impair the effects of the present invention, so the inclusion of the impurities is permitted.
[0048] The content of each of the impurity elements is preferably 0.05 atomic % or less. Within this range, the impurities are not likely to impair the effects of the present invention, and therefore their inclusion is permitted.
[0049] The sum of the Si content and the B content, (100-xab), is uniquely determined according to the values of x, a, and b. However, due to manufacturing errors and the effects of impurities, a deviation of ±0.50 atomic % or less from the center value of (100-xab) is allowed.
[0050] The composition of the soft magnetic powder according to the embodiment has been described above, but the composition and impurities are identified by the following analytical method.
[0051] Examples of analytical methods include iron and steel-atomic absorption spectrometry specified in JIS G 1257:2000, iron and steel-inductively coupled plasma atomic emission spectrometry specified in JIS G 1258:2007, iron and steel-spark discharge atomic emission spectrometry specified in JIS G 1253:2002, iron and steel-fluorescent X-ray analysis specified in JIS G 1256:1997, and gravimetry, titration, and absorptiometry specified in JIS G 1211 to G 1237.
[0052] Specific examples include a solid-state optical emission spectrometer manufactured by SPECTRO, in particular a spark discharge optical emission spectrometer, model: SPECTROLAB, type: LAVMB08A, and an ICP device, CIROS120 type manufactured by Rigaku Corporation.
[0053] In particular, when identifying C (carbon) and S (sulfur), the oxygen flow combustion (high-frequency induction heating furnace combustion)-infrared absorption method specified in JIS G 1211:2011 is also used. Specifically, the LECO carbon / sulfur analyzer, CS-200, can be used.
[0054] In particular, when specifying N (nitrogen) and O (oxygen), the nitrogen determination method for iron and steel specified in JIS G 1228:1997 and the general method for oxygen determination for metallic materials specified in JIS Z 2613:2006 are also used. Specifically, the LECO oxygen / nitrogen analyzer, TC-300 / EF-300, can be mentioned.
[0055] 1.2. Grains The particles of the soft magnetic powder according to the embodiment contain crystal grains with a crystal grain size of 1.0 nm or more and 30.0 nm or less. Since the crystal grains with such a grain size are small, the crystal magnetic anisotropy in each crystal grain is easily averaged. Therefore, the coercive force can be reduced, and a particularly magnetically soft powder can be obtained. In addition, when a certain amount of crystal grains are contained in such a grain size, the magnetic permeability of the soft magnetic powder is increased. As a result, a powder rich in soft magnetism, with low coercive force and high magnetic permeability, can be obtained. In addition, the high magnetic permeability makes it difficult to saturate even under high current, so that the saturation magnetic flux density of the soft magnetic powder can be increased.
[0056] In the particles, the content ratio of the crystal grains in the above particle size range is preferably 30% by volume or more, more preferably 40% by volume or more and 99% by volume or less, and even more preferably 55% by volume or more and 95% by volume or less. If the content ratio of the crystal grains in the above particle size range is below the lower limit, the ratio of crystal grains with small particle size decreases, so that the averaging of the crystal magnetic anisotropy becomes insufficient, and the magnetic permeability of the soft magnetic powder may decrease or the coercive force of the soft magnetic powder may increase. On the other hand, the content ratio of the crystal grains in the above particle size range may exceed the upper limit, but the effect of the coexistence of amorphous structure may be insufficient as described later.
[0057] In addition, the soft magnetic powder according to the embodiment may contain crystal grains having a particle size outside the above-mentioned range, that is, a particle size less than 1.0 nm or a particle size greater than 30.0 nm. In this case, the crystal grains having a particle size outside the range are preferably suppressed to 10% by volume or less, and more preferably suppressed to 5% by volume or less. This makes it possible to suppress the above-mentioned effect from being reduced by the crystal grains having a particle size outside the range.
[0058] The grain size of the crystal grains of the soft magnetic powder can be determined, for example, by observing a cut surface of the soft magnetic powder particle with an electron microscope and reading the observed image. In this method, a perfect circle having the same area as the crystal grain is assumed, and the diameter of the perfect circle, i.e., the equivalent circle diameter, can be regarded as the grain size of the crystal grain.
[0059] The volume ratio of the crystal grains is considered to be approximately equal to the area ratio that the crystal grains occupy with respect to the area of the cut surface, so the area ratio may be regarded as the content ratio.
[0060] In addition, the soft magnetic powder according to the embodiment preferably has an average crystal grain size of 2.0 nm to 25.0 nm, more preferably 5.0 nm to 20.0 nm, which makes the above-mentioned effect, i.e., the effect of low coercivity and high magnetic permeability, more pronounced.
[0061] The average particle size of the crystal grains of the soft magnetic powder can be determined, for example, by determining the particle size of the crystal grains as described above and averaging them, or by determining the width of the peak derived from Fe in the X-ray diffraction pattern of the soft magnetic powder and calculating from that value using the Halder-Wagner method.
[0062] The particles of the soft magnetic powder according to the embodiment may further contain an amorphous structure. The coexistence of the crystal grains and the amorphous structure in the above particle size range cancels out the magnetostriction of each other, so that the magnetostriction of the soft magnetic powder can be made smaller. As a result, a soft magnetic powder with a particularly high magnetic permeability is obtained. In addition, a soft magnetic powder with easy-to-control magnetization is obtained. Furthermore, the inclusion of the amorphous structure makes it easier to maintain the grain size of the crystal grains finer and more uniform.
[0063] The content ratio of the amorphous structure in the particles is preferably 5.0 times or less, more preferably 0.02 times or more and 2.0 times or less, and even more preferably 0.10 times or more and less than 1.0 times, of the content ratio of the crystal grains in the above particle size range, in terms of volume ratio. This optimizes the balance between the crystal grains and the amorphous structure, and the effect of the coexistence of the crystal grains and the amorphous structure becomes more pronounced.
[0064] 1.3. Cu segregation area The particles of the soft magnetic powder according to the embodiment include a Cu segregation portion in which Cu is locally segregated relative to the surroundings. The Cu segregation portion exists at a position deeper than 30 nm from the surface of the particle. The maximum Cu concentration of the Cu segregation portion is more than 6.0 atomic %.
[0065] By including Cu segregation in the particles, it is possible to suppress the coarsening of crystal grains during heat treatment. This makes it possible to form uniform crystal grains by heat treatment. As a result, a soft magnetic powder is obtained that has both low coercivity and high saturation magnetic flux density.
[0066] The Cu segregation portion exists at a position deeper than 30 nm from the surface of the particle. The presence of the Cu segregation portion at such a deep position allows the above-mentioned action of the Cu segregation portion to occur from the surface of the particle to a deep position. In other words, the action of suppressing the coarsening of crystal grains during heat treatment occurs to a deep position. This allows the grain size to be refined and uniform in more parts of the particle, and allows both low coercivity and high saturation magnetic flux density to be achieved.
[0067] The depth of the Cu segregation portion from the particle surface can be identified from an area analysis image obtained by analyzing the particle cross section by EDX (energy dispersive X-ray spectroscopy) using a STEM (scanning transmission electron microscope). Specifically, an image of a 250 nm square range including the particle surface is taken of the particle cross section, and Cu segregation is identified by elemental analysis. The depth of the Cu segregation portion from the particle surface is determined as the distance from the particle surface to the Cu segregation portion with the highest Cu concentration in the area analysis image. At this time, it is preferable that the image shows a range of 200 nm or more deep from the particle surface.
[0068] The depth of the Cu segregation portion is set to more than 30 nm as described above, but is preferably set to 40 nm or more and 500 nm or less, and more preferably set to 50 nm or more and 400 nm or less.
[0069] The maximum value of the Cu concentration in the Cu segregation portion is more than 6.0 atomic %. By including the Cu segregation portion in which Cu is segregated at a high concentration, the Cu segregation portion acts as a nucleation site during heat treatment, facilitating the growth of Fe-based crystal grains. This allows crystal grains of uniform grain size to be generated from the surface to the deep position of the particle. As a result, it is possible to achieve both the averaging of the magnetocrystalline anisotropy and an increase in the ratio of crystal grains of uniform grain size, and it is possible to achieve both low coercivity and high saturation magnetic flux density in an even better manner.
[0070] The maximum Cu concentration in the Cu segregation area was determined as the maximum value of the Cu concentration measured in the area shown in the image by elemental analysis using EDX.
[0071] The maximum value of the Cu concentration in the Cu segregation portion is set to be more than 6.0 atomic % as described above, but is preferably set to be 10.0 atomic % or more, and more preferably set to be 16.0 atomic % or more. This particularly promotes the growth of crystal grains with the Cu segregation portion as a nucleation site. As a result, crystal grains with a more uniform grain size can be generated, especially up to a deep position. The upper limit of the maximum value of the Cu concentration is not particularly limited, but from the viewpoint of avoiding uneven distribution of the Cu segregation portion, it is preferably 70.0 atomic % or less, and more preferably 60.0 atomic % or less.
[0072] In addition, the Cu concentration in the Cu segregation portion is preferably at least twice that of the parent phase, and more preferably at least three times that of the parent phase. This makes the Cu concentration in the Cu segregation portion sufficiently higher than that of the parent phase, and more reliably suppresses the coarsening of crystal grains during heat treatment. The parent phase refers to a portion at a depth of 500 nm from the surface of the particle.
[0073] In addition, by counting the number of Cu segregation parts by diameter in a 200 nm square range that includes the Cu segregation parts in the above-mentioned area analysis image, the average grain size of the Cu segregation parts can be calculated. Specifically, first, a binarized image analysis is performed on the area analysis image to extract the area occupied by the Cu segregation parts. Next, the circle equivalent diameter of the extracted area, that is, the grain size of the Cu segregation parts, is calculated. Then, the number of Cu segregation parts by grain size is counted, and the average grain size is calculated from the counting results.
[0074] The average grain size of the Cu segregation portion calculated in this manner is preferably 3 nm or more and 20 nm or less, more preferably 5 nm or more and 15 nm or less, and even more preferably 5 nm or more and 12 nm or less. If the average grain size of the Cu segregation portion is within the above range, sufficiently fine and more uniform crystal grains can be formed by heat treatment. As a result, the coercive force of the soft magnetic powder can be further reduced.
[0075] As described above, the soft magnetic powder according to this embodiment contains Fe x Cu a Nb b (Si 1-y B y ) 100-x-a-b where a, b, and x are numbers in atomic percent. a satisfies 0.3≦a≦2.0, b satisfies 2.0≦b≦4.0, and x satisfies 73.0≦x≦79.5. y satisfies f(x)≦y≦0.99. f(x)=(4×10 -34 )x 17.56 It is.
[0076] The particles contained in the soft magnetic powder according to the embodiment contain crystal grains with a particle size of 1.0 nm to 30.0 nm, and also contain a Cu segregation portion in which Cu is segregated. The Cu segregation portion is present at a position deeper than 30 nm from the surface of the particle. The maximum Cu concentration of the Cu segregation portion is more than 6.0 atomic %.
[0077] According to this configuration, a soft magnetic powder having both low coercivity and high saturation magnetic flux density can be obtained. This makes it possible to realize a powder magnetic core having low iron loss and being less likely to saturate even at high current. This makes it possible to realize a magnetic element that can handle high current, can be miniaturized, and can achieve high efficiency and high output.
[0078] 1.4.Si segregation area The particles of the soft magnetic powder according to the embodiment include a Si segregation portion in which Si is segregated. This Si segregation portion exists between the Cu segregation portion and the surface of the particle. By including the Si segregation portion existing at such a position, the insulation property of the particle is improved. This makes it possible to suppress the generation of eddy currents that run through the paths between the particles.
[0079] The depth of the Si segregation portion from the particle surface can be determined from an area analysis image obtained by analyzing the particle cross section by EDX (energy dispersive X-ray spectroscopy) using a STEM (scanning transmission electron microscope). Specifically, an image of a 250 nm square area including the particle surface is taken of the particle cross section, and the Si segregation is identified by elemental analysis, and the depth is determined as the distance from the particle surface to the shallowest Si segregation portion. At this time, it is preferable that the image shows a range of 200 nm or more deep from the particle surface.
[0080] The maximum value of the Si concentration in the Si segregation portion is preferably 10.0 atomic % or more, more preferably 15.0 atomic % to 60.0 atomic % or less, and further preferably 20.0 atomic % to 50.0 atomic % or less. If the maximum value of the Si concentration exceeds the upper limit, the amount of Si distributed in the crystal grains is relatively reduced, and there is a risk that the high saturation magnetic flux density derived from the crystal grains will be impaired.
[0081] Such Si segregation portions are likely to be formed when the soft magnetic powder has the composition described above, particularly when the relationship between x and y is within the region shown in FIG.
[0082] 1.5.Fe concentration distribution In the soft magnetic powder particles according to the embodiment, the Fe concentration at a position 12 nm from the surface of the particle is preferably higher than the O concentration in atomic concentration ratio. This makes it possible to realize particles that prevent the oxide film, which is mainly composed of oxides such as SiO2, from becoming thicker than necessary. In other words, by minimizing the thickness of the oxide film and suppressing the concentration of Si segregated as the oxide film, the amount of Si distributed in the crystal grains can be secured, and the volume ratio occupied by the crystal grains can be secured. As a result, a soft magnetic powder having a higher saturation magnetic flux density can be obtained.
[0083] The Fe concentration and O concentration can be determined from the results of area analysis (mapping) and line analysis (line scan) obtained by analyzing the cross section of a particle using EDX (energy dispersive X-ray spectroscopy) with a STEM (scanning transmission electron microscope).
[0084] The difference between the Fe concentration and the O concentration is not particularly limited, but is preferably 10 atomic % or more, and more preferably 30 atomic % or more. The upper limit of the difference between the Fe concentration and the O concentration is not particularly limited, but is preferably 80 atomic % or less, and more preferably 60 atomic % or less.
[0085] In addition, it is not necessary for all particles in the soft magnetic powder according to the embodiment to have the above-mentioned configuration, and the powder may contain particles that do not have the above-mentioned configuration, but it is preferable that 95% by mass or more of the particles have the above-mentioned configuration.
[0086] Furthermore, the soft magnetic powder according to the embodiment may be mixed with other soft magnetic powders or non-soft magnetic powders, and the mixed powder may be used for producing a powder core or the like.
[0087] 1.6.Various characteristics The soft magnetic powder according to the embodiment has a particle Vickers hardness of preferably 1000 to 3000, more preferably 1200 to 2500. When the soft magnetic powder containing particles with such hardness is compressed to form a powder core, deformation at the contact points between the particles is minimized. This keeps the contact area small, and improves the insulation between the particles in the powder core.
[0088] If the Vickers hardness is below the lower limit, depending on the average particle size of the soft magnetic powder, the particles may be easily crushed at the contact points between the particles when the soft magnetic powder is compression molded. This may increase the contact area and reduce the insulation between the particles in the powder core. On the other hand, if the Vickers hardness is above the upper limit, depending on the average particle size of the soft magnetic powder, the powder compactibility may decrease, and the density when the powder core is formed may decrease, resulting in a decrease in the saturation magnetic flux density of the powder core.
[0089] The Vickers hardness of the soft magnetic powder particles is measured at the center of the particle's cross section using a micro Vickers hardness tester. The center of the particle's cross section is the part that corresponds to the midpoint of the long axis on the cut surface when the particle is cut. The pressing load of the indenter during the test is 1.96 N.
[0090] The average particle size D50 of the soft magnetic powder according to the embodiment is not particularly limited, but is preferably 1.0 μm to 50 μm, more preferably 10 μm to 45 μm, and even more preferably 20 μm to 40 μm. By using soft magnetic powder with such an average particle size, the path through which eddy currents flow can be shortened, and therefore a dust core can be manufactured that can sufficiently suppress eddy current loss generated in the particles of the soft magnetic powder.
[0091] Furthermore, when the average particle size of the soft magnetic powder is 10 μm or more, by mixing it with a soft magnetic powder having a smaller average particle size, a mixed powder capable of realizing a high green compaction density can be produced. This mixed powder is also one embodiment of the soft magnetic powder according to the present invention. Such a mixed powder can increase the packing density of the powder core, and increase the magnetic flux density and magnetic permeability of the powder core.
[0092] The average particle size D50 of the soft magnetic powder is determined as the particle size at which the cumulative 50% from the small diameter side is reached in the mass-based particle size distribution obtained by laser diffraction method.
[0093] If the average particle size of the soft magnetic powder is below the lower limit, the soft magnetic powder may become too fine, and the packing property of the soft magnetic powder may be easily reduced. As a result, the compaction density of the powder core, which is an example of a powder compact, decreases, and depending on the material composition and mechanical properties of the soft magnetic powder, the magnetic flux density and magnetic permeability of the powder core may decrease. On the other hand, if the average particle size of the soft magnetic powder is above the upper limit, depending on the material composition and mechanical properties of the soft magnetic powder, the eddy current loss generated within the particles may not be sufficiently suppressed, and the iron loss of the powder core may increase.
[0094] Regarding the soft magnetic powder according to the embodiment, in the mass-based particle size distribution obtained by the laser diffraction method, when the particle size at 10% cumulative from the small diameter side is D10 and the particle size at 90% cumulative from the small diameter side is D90, (D90-D10) / D50 is preferably about 1.0 to 2.5, more preferably about 1.2 to 2.3. (D90-D10) / D50 is an index showing the degree of spread of the particle size distribution, and by this index being within the above range, the filling property of the soft magnetic powder is improved. Therefore, a green compact having particularly high magnetic properties such as magnetic permeability and magnetic flux density can be obtained.
[0095] The coercive force of the soft magnetic powder according to the embodiment is not particularly limited, but is preferably less than 2.0 [Oe] (less than 160 [A / m]), and more preferably 0.1 [Oe] to 1.5 [Oe] (39.9 [A / m] to 120 [A / m]). By using such a soft magnetic powder with a small coercive force, it is possible to manufacture a powder magnetic core that can sufficiently suppress hysteresis loss even under high frequency.
[0096] The coercive force of the soft magnetic powder can be measured, for example, by a vibrating sample magnetometer such as TM-VSM1230-MHHL manufactured by Tamagawa Seisakusho Co., Ltd.
[0097] The soft magnetic powder according to the embodiment preferably has a magnetic permeability of 15 or more at a measurement frequency of 100 MHz when compacted, and more preferably 18 to 50. Such a soft magnetic powder contributes to the realization of a powder magnetic core having excellent magnetic properties such as saturation magnetic flux density.
[0098] The magnetic permeability of the green compact is, for example, the relative magnetic permeability obtained by forming the green compact into a toroidal shape and calculating the self-inductance of the closed magnetic core coil, that is, the effective magnetic permeability. The magnetic permeability is measured using an impedance analyzer such as Agilent Technologies 4194A, with a measurement frequency of 100 MHz. The number of turns of the winding is 7, and the wire diameter of the winding is 0.6 mm.
[0099] The saturation magnetic flux density of the soft magnetic powder according to the embodiment is preferably 1.00 [T] or more, and more preferably 1.10 [T] or more.
[0100] The saturation magnetic flux density of the soft magnetic powder is measured, for example, by the following method. First, the true specific gravity ρ of the soft magnetic powder is measured using a fully automatic gas displacement density meter, AccuPyc1330, manufactured by Micromeritics. Next, the maximum magnetization Mm of the soft magnetic powder is measured using a vibration sample magnetometer, VSM system, TM-VSM1230-MHHL, manufactured by Tamagawa Seisakusho Co., Ltd. Then, the saturation magnetic flux density Bs is calculated using the following formula. Bs = 4π / 10000 × ρ × Mm
[0101] The soft magnetic powder according to the embodiment is a cylindrical compact having an inner diameter of 8 mm and a mass of 0.7 g. When the compact is compressed in the axial direction with a load of 20 kgf, the resistance value of the compact in the axial direction is preferably 0.3 kΩ or more, more preferably 1.0 kΩ or more. A soft magnetic powder capable of realizing a compact having such a resistance value has sufficient insulation between particles. Therefore, such a soft magnetic powder contributes to the realization of a magnetic element capable of suppressing eddy current loss.
[0102] The upper limit of the resistance value is not particularly limited, but in consideration of suppressing variations, it is preferably 30.0 kΩ or less, and more preferably 9.0 kΩ or less.
[0103] 2. Manufacturing method of soft magnetic powder Next, a method for producing the soft magnetic powder according to the embodiment will be described.
[0104] The soft magnetic powder may be produced by any method, for example, by various powdering methods such as atomization methods such as water atomization, gas atomization, and rotary water flow atomization, reduction methods, carbonyl methods, and pulverization methods.
[0105] The atomization method includes water atomization, gas atomization, and rotating water atomization, etc., depending on the type of cooling medium and the device configuration. Of these, the soft magnetic powder is preferably manufactured by the atomization method, more preferably by the water atomization method or the rotating water atomization method, and even more preferably by the rotating water atomization method. The atomization method is a method of manufacturing powder by colliding molten metal with a fluid such as a liquid or gas sprayed at high speed, thereby pulverizing and cooling it. By using such an atomization method, a high cooling rate can be obtained, so that amorphization can be promoted. As a result, crystal grains with a more uniform grain size can be formed by heat treatment.
[0106] In this specification, the term "water atomization method" refers to a method in which a liquid such as water or oil is used as a coolant, which is sprayed in an inverted cone shape that converges to one point, and molten metal is made to flow toward this convergence point and collide with it, thereby pulverizing the molten metal to produce metal powder.
[0107] In addition, the rotary water flow atomization method can cool the molten metal extremely quickly, so that the disordered atomic arrangement of the molten metal can be maintained to a high degree during solidification. Therefore, by carrying out a crystallization treatment after that, it is possible to efficiently produce soft magnetic powder having crystal grains with a uniform grain size.
[0108] The method for producing soft magnetic powder by the rotary water jet atomization method will be further described below. In the rotary water flow atomization method, a cooling liquid is jetted along the inner circumferential surface of a cooling cylinder and rotated along the inner circumferential surface of the cooling cylinder to form a cooling liquid layer on the inner circumferential surface. Meanwhile, the raw material of the soft magnetic powder is melted, and the resulting molten metal is allowed to fall naturally while a jet of liquid or gas is sprayed onto it. This causes the molten metal to splash and be captured in the cooling liquid layer. As a result, the molten metal that has been splashed and turned into fine powder is rapidly cooled and solidified, and soft magnetic powder is obtained.
[0109] FIG. 2 is a vertical cross-sectional view showing an example of an apparatus for producing soft magnetic powder by the rotary water jet atomization method.
[0110] The powder manufacturing apparatus 30 shown in FIG. 2 includes a cooling cylinder 1, a crucible 15, a pump 7, and a jet nozzle 24. The cooling cylinder 1 is a cylinder for forming a cooling liquid layer 9 on its inner circumferential surface. The crucible 15 is a supply container for supplying molten metal 25 to flow down into a space 23 inside the cooling liquid layer 9. The pump 7 supplies the cooling liquid to the cooling cylinder 1. The jet nozzle 24 ejects a gas jet 26 that breaks the molten metal 25 in the form of a thin stream that flows down into droplets. The molten metal 25 is prepared according to the composition of the soft magnetic powder.
[0111] The cooling cylinder 1 has a cylindrical shape and is installed so that the axis of the cylinder is aligned vertically or inclined at an angle of 30° or less with respect to the vertical.
[0112] The upper end opening of the cooling cylinder 1 is closed by a lid 2. The lid 2 is formed with an opening 3 for supplying the flowing molten metal 25 to the space 23 of the cooling cylinder 1.
[0113] A cooling liquid ejection pipe 4 is provided at the upper part of the cooling cylinder 1 to eject a cooling liquid onto the inner peripheral surface of the cooling cylinder 1. A plurality of ejection ports 5 of the cooling liquid ejection pipe 4 are provided at equal intervals along the circumferential direction of the cooling cylinder 1.
[0114] The cooling liquid ejection pipe 4 is connected to the tank 8 through a pipe connected to the pump 7, and the cooling liquid in the tank 8 sucked up by the pump 7 is ejected and supplied into the cooling cylinder 1 through the cooling liquid ejection pipe 4. As a result, the cooling liquid gradually flows down while rotating along the inner circumferential surface of the cooling cylinder 1, and a cooling liquid layer 9 is formed along the inner circumferential surface. In addition, a cooler may be interposed in the tank 8 or in the middle of the circulation flow path as necessary. As the cooling liquid, in addition to water, oil such as silicone oil is used, and various additives may be added. In addition, by removing the dissolved oxygen in the cooling liquid in advance, oxidation of the powder produced due to cooling can be suppressed.
[0115] In addition, a layer thickness adjusting ring 16 for adjusting the thickness of the coolant layer 9 is detachably provided on the lower part of the inner circumferential surface of the cooling cylinder 1. By providing this layer thickness adjusting ring 16, the flow rate of the coolant is reduced, and the thickness of the coolant layer 9 is ensured and made uniform.
[0116] Furthermore, a cylindrical draining net 17 is connected to the lower part of the cooling cylinder 1, and a funnel-shaped powder recovery container 18 is provided below this draining net 17. A cooling liquid recovery cover 13 is provided around the draining net 17 so as to cover it, and a drain port 14 formed at the bottom of this cooling liquid recovery cover 13 is connected to the tank 8 via a pipe.
[0117] The jet nozzle 24 is provided in the space 23. The jet nozzle 24 is attached to the tip of a gas supply pipe 27 inserted through the opening 3 of the lid 2, and is disposed so that its nozzle is directed toward the molten metal 25 in the form of a thin stream.
[0118] To produce soft magnetic powder in such powder production apparatus 30, first, pump 7 is operated to form a cooling liquid layer 9 on the inner peripheral surface of cooling cylinder 1. Next, molten metal 25 in crucible 15 is caused to flow down into space 23. When gas jet 26 is blown onto the flowing molten metal 25, molten metal 25 is scattered, and the finely powdered molten metal 25 is caught up in cooling liquid layer 9. As a result, the finely powdered molten metal 25 is cooled and solidified, and soft magnetic powder is obtained.
[0119] In the rotary water flow atomization method, a very high cooling rate can be stably maintained by continuously supplying a cooling liquid, so that the amorphous state of the soft magnetic powder produced before the heat treatment is stabilized. As a result, by carrying out the heat treatment after that, it is possible to efficiently produce soft magnetic powder having crystal grains with a uniform grain size.
[0120] In addition, the molten metal 25 atomized to a certain size by the gas jet 26 falls with inertia until it is caught in the cooling liquid layer 9, at which point the droplets become spherical. As a result, soft magnetic powder can be produced.
[0121] For example, the amount of molten metal 25 flowing down from crucible 15 varies depending on the size of the device and is not particularly limited, but is preferably kept to 1 kg or less per minute. As a result, when molten metal 25 scatters, it scatters as droplets of appropriate size, so that soft magnetic powder with the average particle size as described above can be obtained. In addition, by suppressing the amount of molten metal 25 supplied in a certain period of time to a certain degree, a sufficient cooling rate can be obtained. Note that, for example, by reducing the amount of molten metal 25 flowing down within the above range, adjustments can be made to reduce the average particle size.
[0122] On the other hand, the outer diameter of the thin stream of molten metal 25 flowing down from crucible 15, i.e., the inner diameter of the flow outlet of crucible 15, is not particularly limited, but is preferably 1 mm or less. This makes it easier to uniformly hit the thin stream of molten metal 25 with gas jet 26, making it easier to uniformly scatter droplets of appropriate size. As a result, soft magnetic powder with the average particle size described above is obtained. Also, since the amount of molten metal 25 supplied in a certain period of time is suppressed, a sufficient cooling rate is obtained.
[0123] The flow rate of the gas jet 26 is not particularly limited, but is preferably set to 100 m / s or more and 1000 m / s or less. This also allows the molten metal 25 to be scattered as droplets of a suitable size, so that soft magnetic powder with the average particle size described above can be obtained. In addition, since the gas jet 26 has a sufficient speed, the scattered droplets are also given a sufficient speed, so that the droplets become finer and the time until they are caught in the cooling liquid layer 9 is shortened. As a result, the droplets can be made spherical in a short time and are cooled in a short time. For example, the flow rate of the gas jet 26 can be adjusted to be increased within the above range, so that the average particle size can be reduced.
[0124] As other conditions, for example, it is preferable to set the pressure of the cooling liquid supplied to the cooling cylinder 1 at the time of ejection to about 50 MPa or more and 200 MPa or less, and the liquid temperature to about -10° C. or more and 40° C. or less. This optimizes the flow rate of the cooling liquid layer 9, and allows the pulverized molten metal 25 to be cooled appropriately and evenly.
[0125] Moreover, the temperature of the molten metal 25 is preferably set to about Tm+20° C. or more and Tm+200° C. or less, and more preferably set to about Tm+50° C. or more and Tm+150° C. or less, relative to the melting point Tm of the soft magnetic powder to be manufactured. This makes it possible to particularly reduce the variation in properties between particles when the molten metal 25 is pulverized by the gas jet 26, and also to more reliably make the manufactured soft magnetic powder amorphous before the heat treatment. The gas jet 26 can be replaced by a liquid jet if necessary.
[0126] In addition, the cooling rate of the molten metal 25 in the atomization method is 1×10 4 °C / s or more, and preferably 1×10 5 °C / s or more is more preferable, and 1×10 6 It is more preferable that the cooling rate is ℃ / s or more. By such rapid cooling, particularly stable amorphousization can be achieved, and soft magnetic powder having crystal grains with uniform grain size can be finally obtained. In addition, the variation in the composition ratio between the particles of the soft magnetic powder can be suppressed. In addition, by increasing the cooling rate, the Fe concentration can be made higher than the O concentration.
[0127] The soft magnetic powder produced as described above is subjected to a crystallization treatment, whereby at least a part of the amorphous structure is crystallized to form crystal grains.
[0128] The crystallization treatment can be performed by subjecting the soft magnetic powder containing an amorphous structure to a heat treatment. The temperature of the heat treatment is not particularly limited, but is preferably 520°C to 640°C, more preferably 530°C to 630°C, and even more preferably 540°C to 620°C. The time of the heat treatment is preferably 1 minute to 180 minutes, more preferably 3 minutes to 120 minutes, and even more preferably 5 minutes to 60 minutes, during which the temperature is maintained at the temperature. By setting the temperature and time of the heat treatment within the above ranges, crystal grains with a more uniform grain size can be generated.
[0129] If the heat treatment temperature or time is below the lower limit, depending on the composition of the soft magnetic powder, crystallization may be insufficient and the uniformity of the particle size may be poor. On the other hand, if the heat treatment temperature or time is above the upper limit, crystallization may proceed too far and the uniformity of the particle size may be poor, depending on the composition of the soft magnetic powder.
[0130] The heating and cooling rates in the crystallization treatment affect the grain size and uniformity of the grain size of the crystal grains generated by the heat treatment, as well as the distribution, grain size, and Cu concentration of the Cu segregated portions.
[0131] The heating rate is preferably 10°C / min to 35°C / min, more preferably 10°C / min to 30°C / min, and even more preferably 15°C / min to 25°C / min. By setting the heating rate within the above range, the grain size of the crystal grains, the distribution and grain size of the Cu segregation portion, and the Cu concentration can be kept within the above range. If the heating rate is below the lower limit, the time of exposure to high temperature is extended accordingly, and the grain size of the crystal grains may become too large. If the heating rate exceeds the upper limit, the grain size of the crystal grains may become too small, the distribution of the Cu segregation portion may become too shallow, the grain size of the Cu segregation portion may become too small, or the Cu concentration may become too low.
[0132] The cooling rate is preferably 40°C / min to 80°C / min, more preferably 50°C / min to 70°C / min, and even more preferably 55°C / min to 65°C / min. By setting the cooling rate within the above range, the grain size of the crystal grains, the distribution and grain size of the Cu segregation portion, and the Cu concentration can be kept within the above range. If the cooling rate is below the lower limit, the time of exposure to high temperature is extended accordingly, and the grain size of the crystal grains may become too large. If the cooling rate exceeds the upper limit, the grain size of the crystal grains may become too small, the distribution of the Cu segregation portion may become too shallow, the grain size of the Cu segregation portion may become too small, or the Cu concentration may become too low.
[0133] The atmosphere for the crystallization treatment is not particularly limited, but is preferably an inert gas atmosphere such as nitrogen or argon, a reducing gas atmosphere such as hydrogen or ammonia decomposition gas, or a reduced pressure atmosphere thereof, which allows crystallization while suppressing oxidation of the metal, and produces a soft magnetic powder with excellent magnetic properties. In this manner, the soft magnetic powder according to this embodiment can be manufactured.
[0134] The soft magnetic powder thus obtained may be classified as necessary. Examples of the classification method include dry classification such as sieving classification, inertial classification, centrifugal classification, and air classification, and wet classification such as sedimentation classification.
[0135] If necessary, an insulating film may be formed on the surface of each particle of the obtained soft magnetic powder. Examples of materials constituting this insulating film include inorganic materials such as phosphates such as magnesium phosphate, calcium phosphate, zinc phosphate, manganese phosphate, and cadmium phosphate, and silicates such as sodium silicate. In addition, it may be appropriately selected from the organic materials listed as the materials constituting the binder described later.
[0136] 3. Powder cores and magnetic components Next, the powder magnetic core and the magnetic element according to the embodiment will be described.
[0137] The magnetic element according to the embodiment can be applied to various magnetic elements having a magnetic core, such as a choke coil, an inductor, a noise filter, a reactor, a transformer, a motor, an actuator, an electromagnetic valve, a generator, etc. Furthermore, the powder magnetic core according to the embodiment can be applied to the magnetic cores included in these magnetic elements.
[0138] Two types of coil components will be described below as representative examples of the magnetic element. 3.1.Toroidal type First, a toroidal type coil component, which is an example of a magnetic element according to the embodiment, will be described. FIG. 3 is a plan view that illustrates a schematic diagram of a toroidal type coil component.
[0139] 3 has a ring-shaped powder core 11 and a conductive wire 12 wound around this powder core 11. Such a coil component 10 is generally called a toroidal coil.
[0140] The powder magnetic core 11 is obtained by mixing the soft magnetic powder according to the embodiment with a binder, supplying the mixture to a molding die, and pressing and molding it. That is, the powder magnetic core 11 is a compact containing the soft magnetic powder according to the embodiment. Such a powder magnetic core 11 has a high saturation magnetic flux density and a small iron loss. As a result, when the powder magnetic core 11 is mounted in an electronic device or the like, it is possible to reduce the power consumption of the electronic device or the like and improve its performance, thereby contributing to improving the reliability of the electronic device or the like. The binder may be added as necessary, or may be omitted.
[0141] Furthermore, the coil component 10 including such a powder magnetic core 11 achieves low iron loss and high performance.
[0142] Examples of the binder material used to manufacture the powder magnetic core 11 include organic materials such as silicone resins, epoxy resins, phenol resins, polyamide resins, polyimide resins, and polyphenylene sulfide resins, and inorganic materials such as phosphates such as magnesium phosphate, calcium phosphate, zinc phosphate, manganese phosphate, and cadmium phosphate, and silicates such as sodium silicate. Thermosetting polyimide or epoxy resins are particularly preferred. These resin materials are easily cured by heating and have excellent heat resistance. This makes it possible to improve the ease of manufacture and heat resistance of the powder magnetic core 11.
[0143] The ratio of binder to soft magnetic powder varies slightly depending on the desired magnetic flux density, mechanical properties, allowable eddy current loss, etc. of the powder core 11 to be produced, but is preferably about 0.5% by mass to 5% by mass, and more preferably about 1% by mass to 3% by mass. This makes it possible to obtain powder core 11 with excellent magnetic properties such as magnetic flux density and magnetic permeability while sufficiently binding the individual particles of the soft magnetic powder to each other. If necessary, various additives may be added to the mixture for any purpose.
[0144] The conductive wire 12 may be made of a highly conductive material, such as a metal material containing Cu, Al, Ag, Au, Ni, etc. An insulating film may be provided on the surface of the conductive wire 12 as necessary.
[0145] The shape of the powder magnetic core 11 is not limited to the ring shape shown in FIG. 3, but may be, for example, a ring shape with a part missing, or a shape with a linear shape in the longitudinal direction.
[0146] Furthermore, the powder magnetic core 11 may contain soft magnetic powder other than the soft magnetic powder according to the embodiment described above or non-magnetic powder, as necessary.
[0147] 3.2.Closed magnetic circuit type Next, a closed magnetic circuit type coil component, which is an example of a magnetic element according to the embodiment, will be described. FIG. 4 is a see-through perspective view that typically shows a closed magnetic circuit type coil component.
[0148] The closed magnetic circuit type coil component will be described below, but in the following description, the differences from the toroidal type coil component will be mainly described, and a description of similar points will be omitted.
[0149] 4, the coil component 20 according to this embodiment is formed by embedding a conductor wire 22 formed into a coil shape inside a powder magnetic core 21. That is, the coil component 20 is formed by molding the conductor wire 22 with the powder magnetic core 21. This powder magnetic core 21 has a similar configuration to the powder magnetic core 11 described above.
[0150] It is easy to obtain a relatively small coil component 20 having this configuration. In manufacturing such a small coil component 20, by using a powder magnetic core 21 having high magnetic flux density and magnetic permeability and low loss, it is possible to obtain a coil component 20 that is small in size but has low loss and low heat and is capable of handling a large current.
[0151] Furthermore, because the conductive wire 22 is embedded inside the powder core 21, a gap is unlikely to occur between the conductive wire 22 and the powder core 21. This makes it possible to suppress vibrations caused by magnetostriction of the powder core 21, and also to suppress the generation of noise associated with this vibration.
[0152] When manufacturing the coil component 20 according to the present embodiment as described above, first, the conductive wire 22 is placed in the cavity of a molding die, and the cavity is filled with granulated powder containing the soft magnetic powder according to the embodiment. That is, the granulated powder is filled so as to surround the conductive wire 22.
[0153] Next, the granulated powder is pressed together with the conductive wire 22 to obtain a compact. Next, similarly to the above embodiment, the compact is subjected to a heat treatment, whereby the binder is hardened and the dust core 21 and the coil component 20 are obtained.
[0154] The dust core 21 may contain soft magnetic powder other than the soft magnetic powder according to the embodiment described above or non-magnetic powder, as necessary.
[0155] 4.Electronic equipment Next, an electronic device including the magnetic element according to the embodiment will be described with reference to FIGS.
[0156] Fig. 5 is a perspective view showing a mobile personal computer, which is an electronic device including a magnetic element according to an embodiment. The personal computer 1100 shown in Fig. 5 includes a main body 1104 including a keyboard 1102, and a display unit 1106 including a display unit 100. The display unit 1106 is rotatably supported by the main body 1104 via a hinge structure. Such a personal computer 1100 includes a magnetic element 1000, such as a choke coil or inductor for a switching power supply, or a motor.
[0157] Fig. 6 is a plan view showing a smartphone, which is an electronic device including the magnetic element according to the embodiment. The smartphone 1200 shown in Fig. 6 includes a plurality of operation buttons 1202, an earpiece 1204, and a mouthpiece 1206. A display unit 100 is disposed between the operation buttons 1202 and the earpiece 1204. Such a smartphone 1200 includes a magnetic element 1000, such as an inductor, a noise filter, or a motor.
[0158] Fig. 7 is a perspective view showing a digital still camera, which is an electronic device equipped with a magnetic element according to the embodiment. Fig. 7 also shows a simplified view of connections to external devices. The digital still camera 1300 photoelectrically converts an optical image of a subject using an imaging element such as a CCD (Charge Coupled Device) to generate an imaging signal.
[0159] 7 includes a display unit 100 provided on the back of a case 1302. The display unit 100 functions as a viewfinder that displays a subject as an electronic image. In addition, a light receiving unit 1304 including an optical lens, a CCD, etc. is provided on the front side of the case 1302, i.e., on the back side in the figure.
[0160] When the photographer checks the subject image displayed on the display unit 100 and presses the shutter button 1306, the image signal of the CCD at that time is transferred to and stored in memory 1308. Such a digital still camera 1300 also has a built-in magnetic element 1000, such as an inductor or a noise filter.
[0161] Examples of electronic devices according to the embodiments include the personal computer of FIG. 5, the smartphone of FIG. 6, and the digital still camera of FIG. 7, as well as mobile phones, tablet terminals, watches, inkjet discharge devices such as inkjet printers, laptop personal computers, televisions, video cameras, video tape recorders, car navigation devices, pagers, electronic organizers, electronic dictionaries, calculators, electronic game devices, word processors, workstations, videophones, security television monitors, electronic binoculars, POS terminals, medical devices such as electronic thermometers, blood pressure monitors, blood glucose meters, electrocardiogram measuring devices, ultrasonic diagnostic devices, and electronic endoscopes, fish finders, various measuring devices, instruments for vehicles, aircraft, and ships, mobile object control devices such as automobile control devices, aircraft control devices, railway vehicle control devices, and ship control devices, and flight simulators.
[0162] As described above, such electronic devices include the magnetic element according to the embodiment, and can enjoy the effects of the magnetic element, such as low coercive force and high saturation magnetic flux density, to thereby achieve miniaturization and high output of the electronic devices.
[0163] The soft magnetic powder, the dust core, the magnetic element, and the electronic device of the present invention have been described above based on the preferred embodiments, but the present invention is not limited thereto.
[0164] For example, in the above embodiment, a powder compact such as a powder core was given as an example of an application of the soft magnetic powder of the present invention, but the application examples are not limited to this and may also be, for example, magnetic fluids, magnetic devices such as magnetic heads, etc.
[0165] Furthermore, the shapes of the dust core and the magnetic element are not limited to those shown in the drawings, and may be any shape. EXAMPLES
[0166] Next, specific examples of the present invention will be described. 5. Manufacturing of powder magnetic cores 5.1. Sample No. 1 First, the raw materials were melted in a high-frequency induction furnace and pulverized by a rotary water flow atomization method to obtain soft magnetic powder. At this time, the flow rate of the molten metal flowing down from the crucible was 0.5 kg / min, the inner diameter of the flow outlet of the crucible was 1 mm, and the flow rate of the gas jet was 900 m / s. Next, classification was performed using a wind classifier. The composition of the obtained soft magnetic powder is shown in Table 1. The composition was specified using a solid-state optical emission spectrometer manufactured by SPECTRO, model: SPECTROLAB, type: LAVMB08A. As a result, the total content of impurities was 0.50 atomic % or less.
[0167] Next, the particle size distribution of the obtained soft magnetic powder was measured. This measurement was performed using a laser diffraction type particle size distribution measuring device, Microtrack HRA9320-X100 manufactured by Nikkiso Co., Ltd. Then, the average particle size D50 of the soft magnetic powder was obtained from the particle size distribution and found to be 20 μm. In addition, the obtained soft magnetic powder was evaluated by an X-ray diffractometer to see whether the structure before heat treatment was amorphous or not.
[0168] The obtained soft magnetic powder was then heated in a nitrogen atmosphere under the heating conditions shown in Table 1.
[0169] Next, the obtained soft magnetic powder was mixed with an epoxy resin as a binder to obtain a mixture. The amount of the epoxy resin added was 2 parts by mass per 100 parts by mass of the soft magnetic powder.
[0170] Next, the mixture was stirred and then dried for a short time to obtain a lump-shaped dried body. The dried body was then sieved through a sieve with a mesh size of 400 μm, and the dried body was pulverized to obtain a granulated powder. The obtained granulated powder was dried at 50° C. for 1 hour.
[0171] Next, the obtained granulated powder was filled into a molding die, and a molded body was obtained based on the following molding conditions.
[0172] <Molding conditions> Molding method: Press molding Shape of molded body: Ring-shaped -Dimensions of molded body: Outer diameter 14mm, inner diameter 8mm, thickness 3mm ·Molding pressure: 3t / cm 2 (294MPa)
[0173] Next, the compact was heated in an air atmosphere at a temperature of 150° C. for 0.5 hours to harden the binder, thereby obtaining a powder magnetic core.
[0174] 5.2. Samples No. 2 to 21 Powder cores were obtained in the same manner as Sample No. 1, except that the manufacturing conditions of the soft magnetic powder and the manufacturing conditions of the powder core were changed as shown in Table 1. The average particle size D50 of each sample was within the range of 10 μm or more and 30 μm or less.
[0175] [Table 1]
[0176] In Table 1, among the soft magnetic powders of each sample number, those which correspond to the present invention are indicated as "Examples", and those which do not correspond to the present invention are indicated as "Comparative Examples".
[0177] In addition, when x and y in the alloy composition of the soft magnetic powder of each sample number are located inside region C, "C" is entered in the region column, when they are located outside region C but inside region B, "B" is entered in the region column, and when they are located outside region B but inside region A, "A" is entered in the region column. When they are located outside region A, "-" is entered in the region column.
[0178] 6. Evaluation of soft magnetic powders and dust cores 6.1.Evaluation of the particle structure of soft magnetic powder The soft magnetic powder obtained in each of the examples and comparative examples was processed into thin pieces by a focused ion beam device to obtain test pieces.
[0179] Next, the obtained test piece was observed using a scanning transmission electron microscope, and an elemental analysis was carried out to obtain an area analysis image.
[0180] Next, the grain size of the crystal grains was measured from the observed image, and the area ratio of the crystal grains falling within a specific range of 1.0 nm to 30.0 nm was calculated, and this was regarded as the volume ratio of the crystal grains of the specified grain size. The measurement results are shown in Table 2.
[0181] In addition, by analyzing the surface analysis images, various indices shown in Table 2 were obtained for the Cu segregation areas, the Si segregation areas, the Fe concentration distribution, and the O concentration distribution.
[0182] Specifically, the Cu segregation area with the highest Cu concentration was identified, and the depth from the particle surface of the Cu segregation area and the maximum Cu concentration were measured.The grain size of the Cu segregation area was also measured, and the average grain size was calculated.
[0183] In addition, the Fe concentration and O concentration at a position 12 nm from the particle surface were compared, and if the Fe concentration was higher, it was recorded as "Fe>O", and if the O concentration was higher, it was recorded as "O>Fe", as shown in Table 2. Furthermore, the presence or absence of Si segregation was evaluated.
[0184] 6.2.Resistance Value of Compacted Soft Magnetic Powder For the compacts of the soft magnetic powders obtained in each of the Examples and Comparative Examples, the electrical resistance values were measured by the method described below.
[0185] First, a lower punch electrode was set at the lower end of a cylindrical mold cavity with an inner diameter of 8 mm. Next, 0.7 g of soft magnetic powder was filled into the cavity. Next, an upper punch electrode was set at the upper end of the cavity. Then, the mold, lower punch electrode, and upper punch electrode were set on a load application device. Next, using a digital force gauge, a load of 20 kgf was applied in the direction in which the lower punch electrode and upper punch electrode were brought closer together. Then, the electrical resistance value between the lower punch electrode and upper punch electrode was measured while the load was applied. The measured resistance values were then evaluated according to the following evaluation criteria.
[0186] A: Resistance value is 5.0kΩ or more B: Resistance value is 3.0kΩ or more and less than 5.0kΩ C: Resistance value is 0.3kΩ or more and less than 3.0kΩ D: Resistance is less than 0.3kΩ The evaluation results are shown in Table 2.
[0187] 6.3. Measurement of coercive force of soft magnetic powder The coercive force of each of the soft magnetic powders obtained in the respective Examples and Comparative Examples was measured using the following measuring device.
[0188] Measurement equipment: Vibrating sample magnetometer, Tamagawa Manufacturing Co., Ltd. VSM system, TM-VSM1230-MHHL The measured coercive force was evaluated according to the following criteria.
[0189] A: Coercive force is less than 0.90 Oe B: Coercive force is 0.90 Oe or more and less than 1.33 Oe C: Coercive force is 1.33 Oe or more and less than 1.67 Oe D: Coercive force is 1.67 Oe or more and less than 2.00 Oe E: Coercive force is 2.00 Oe or more and less than 2.33 Oe F: Coercive force is 2.33 Oe or more The evaluation results are shown in Table 2.
[0190] 6.4. Calculation of Saturation Magnetic Flux Density of Soft Magnetic Powder The saturation magnetic flux density of each of the soft magnetic powders obtained in the respective Examples and Comparative Examples was calculated as follows.
[0191] First, the true specific gravity ρ of the soft magnetic powder was measured using a fully automatic gas displacement densitometer, AccuPyc1330, manufactured by Micromeritics.
[0192] Next, the maximum magnetization Mm of the soft magnetic powder was measured using the above-mentioned vibrating sample magnetometer. Next, the saturation magnetic flux density Bs was calculated using the following formula.
[0193] Bs = 4π / 10000 × ρ × Mm The calculation results are shown in Table 2.
[0194] 6.5.Measuring the magnetic permeability of powder cores The magnetic permeability of each of the powder magnetic cores obtained in the examples and comparative examples was measured under the following measurement conditions.
[0195] Measurement equipment: Impedance analyzer, Agilent Technologies 4194A Measurement frequency: 100MHz Number of turns of winding: 7 Winding wire diameter: 0.6mm The measurement results are shown in Table 2.
[0196] 6.6.Measuring Iron Loss in Powder Cores For each of the dust cores obtained in the examples and comparative examples, the iron loss was measured under the following measurement conditions.
[0197] Measurement equipment: BH analyzer, Iwasaki Electric Co., Ltd. SY-8258 Measurement frequency: 900kHz Number of turns of winding: 36 turns on the primary side, 36 turns on the secondary side Winding wire diameter: 0.5mm Maximum magnetic flux density: 50mT The measurement results are shown in Table 2.
[0198] [Table 2]
[0199] As is clear from Table 2, the soft magnetic powders obtained in each Example had both low coercivity and high saturation magnetic flux density. In addition, the powder cores containing the soft magnetic powders obtained in each Example had high magnetic permeability and low iron loss. In contrast, the soft magnetic powders obtained in each Comparative Example had high coercivity and low saturation magnetic flux density. [Explanation of symbols]
[0200] Reference Signs List 1...cooling cylinder, 2...lid, 3...opening, 4...cooling liquid ejection tube, 5...discharge port, 7...pump, 8...tank, 9...cooling liquid layer, 10...coil part, 11...powder core, 12...conductor, 13...cooling liquid recovery cover, 14...drain port, 15...crucible, 16...layer thickness adjustment ring, 17...liquid draining mesh, 18...powder recovery container, 20...coil part, 21...powder core, 22...conductor, 23...space, 24...jet nozzle, 25...molten metal, 26...gas jet, 27...gas supply tube , 30...powder manufacturing apparatus, 100...display section, 1000...magnetic element, 1100...personal computer, 1102...keyboard, 1104...main body, 1106...display unit, 1200...smartphone, 1202...operation button, 1204...earpiece, 1206...mouthpiece, 1300...digital still camera, 1302...case, 1304...light receiving unit, 1306...shutter button, 1308...memory, A...area A, B...area B, C...area C
Claims
1. Fe x Cổ a Nコ b (Yes) 1-y B y ) 100-x-a-b [wherein a, b, and x are numbers in atomic percent, and satisfy 0.3≦a≦2.0, 2.0≦b≦4.0, and 73.0≦x≦79.
5. Also, y is a number that satisfies f(x)≦y≦0.99, and f(x)=(4×10 -34 ) x 17.56 It is.] The particles have a composition represented by The particles contain crystal grains having a particle size of 1.0 nm or more and 30.0 nm or less, The content ratio of the crystal grains in the particles is 30% by volume or more, The steel sheet includes a Cu segregation portion in which Cu is segregated, the Cu segregation portion is present at a position deeper than 30 nm from the surface of the particle, A soft magnetic powder characterized in that the maximum Cu concentration in the Cu segregation portion exceeds 6.0 atomic %.
2. The soft magnetic powder according to claim 1 , wherein the Fe concentration at a position 12 nm from the surface of the particle is higher than the O concentration.
3. 3. The soft magnetic powder according to claim 1, wherein the maximum Cu concentration in the Cu segregation portion is 10.0 atomic % or more.
4. The silicon-segregated portion includes a silicon-segregated portion, The soft magnetic powder according to claim 1 , wherein the Si segregated portion is present between the Cu segregated portion and the surface of the particle.
5. 5. The soft magnetic powder according to claim 1, which is a cylindrical compact having an inner diameter of 8 mm and a mass of 0.7 g, and when the compact is compressed in the axial direction under a load of 20 kgf, the resistance value of the compact in the axial direction is 0.3 kΩ or more.
6. A dust core comprising the soft magnetic powder according to claim 1 .
7. A magnetic element comprising the powder magnetic core according to claim 6.
8. An electronic device comprising the magnetic element according to claim 7.
Citation Information
Patent Citations
Constantly-magnetic magnetic core and manufacture method and functions of constantly-magnetic magnetic core
CN103258623A
Production of iron-base fine crystal soft magnetic alloy
JP1995258728A
Soft magnetic powder, dust core, magnetic element and electronic device
JP2019189928A
CRYSTALLINE Fe-BASED ALLOY POWDER, MANUFACTURING METHOD THEREFOR, AND MAGNETIC CORE
JP2020056107A