Laminated body
The laminate structure, using a polyester base film from PET bottles and inorganic thin film layers, addresses the need for environmentally friendly packaging with gas barrier and transparency, achieving the necessary performance for packaging materials.
Patent Information
- Application Number
- JP2021562590
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Priority Date
- 2019-12-05
- Filing Date
- 2020-11-25
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2040-11-25
AI Technical Summary
Existing packaging materials fail to achieve a balance of being environmentally friendly, having gas barrier properties, and maintaining transparency and toughness, while also being suitable for microwave use.
A laminate structure composed of a polyester base film derived from PET bottles, an inorganic thin film layer, and a protective layer, with specific resin compositions and manufacturing processes to enhance gas barrier performance and maintain transparency.
The laminate achieves the required performance of gas barrier properties, sealing properties, and toughness while being environmentally friendly, suitable for microwave use, and recyclable.
Smart Images

Figure 0007574804000001 
Figure 0007574804000002 
Figure 0007574804000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a laminate for use in the fields of packaging food, medicine, industrial products, etc. More specifically, the present invention relates to an environmentally friendly laminate that is excellent in gas barrier properties, processability, and toughness, and further allows visualization of the contents and is convenient for use in a microwave oven. [Background technology]
[0002] In recent years, regulations aimed at reducing the use of disposable plastics have been strengthened in Europe and other countries around the world. Behind this lies the growing international awareness of resource circulation and the worsening waste problems in emerging countries. For this reason, there is a demand for environmentally friendly products from the perspective of the 3Rs (recycle, reuse, reduce) for plastic packaging materials required for food, medicines, etc.
[0003] The performance required for the aforementioned environmentally friendly packaging materials includes (1) being made from recycled materials, (2) having gas barrier performance that can block various gases and extend the shelf life, and (3) having a laminate structure that has a low environmental impact (for example, not using organic solvents, using only small amounts of materials, and being able to be made into a mono-material).
[0004] Regarding (1), polyester resin recycled from PET bottles is known as a representative recycled material, and a technology is known for producing polyester film for body wrap labels that has few problems caused by static electricity without impairing productivity or quality from polyester resin derived from PET bottles that has a low oligomer content (see, for example, Patent Document 1). With the stricter environmental regulations in the future, demand for such film applications is expected to expand.
[0005] Regarding (2) above, in food applications that require blocking various gases such as water vapor and oxygen, gas barrier laminates are generally used in which a thin metal film made of aluminum or the like, or an inorganic thin film made of an inorganic oxide such as silicon oxide or aluminum oxide, is formed on the surface of a plastic base film. Of these, those formed with a thin film (inorganic thin film layer) of an inorganic oxide such as silicon oxide, aluminum oxide, or a mixture of these are transparent, allowing the contents to be confirmed, and can be used in microwave ovens, and therefore demand is growing also from the environmental perspective of eliminating aluminum foil.
[0006] The gas barrier film, which is made of the aforementioned recycled materials and inorganic thin film, uses polyester resin recycled from PET bottles, and has low heat shrinkage and small thickness unevenness. A laminate film that exhibits good gas barrier properties when made into a gas barrier laminate film having an inorganic thin film layer and a sealant layer has been proposed (see, for example, Patent Document 2). However, in this conventional technology, the barrier performance is insufficient to replace aluminum foil.
[0007] Regarding (3) above, pouches that do not use aluminum foil are required to have barrier properties, heat resistance, toughness (resistance to bag rupture and pinholes), and high sealability all at the same time. Therefore, they generally have a structure of at least three layers, with a vapor-deposited polyester film on the outside, a polyamide film in the middle, and an olefin-based heat-sealable resin dry-laminated via an adhesive on the inside (contents side) of the bag.
[0008] In order to achieve mono-materialization from an environmental perspective in the above-mentioned retort pouch configuration, it is necessary to further improve the barrier performance of the bag (to the same level as aluminum foil), not use polyamide film and olefin-based sealant, or change to polyester-based materials, but this change was not easy with conventional technology. Also, when an olefin-based sealant is used, the transparency may be insufficient, which causes undesirable problems in terms of visual safety and appearance after printing.
[0009] As an alternative to polyamide film, the use of biaxially stretched polybutylene terephthalate (hereinafter sometimes abbreviated as PBT) film has been considered (see, for example, Patent Document 3). In Patent Document 3, it was known that a biaxially stretched PBT film obtained by simultaneously biaxially stretching a resin composition consisting of at least polybutylene terephthalate resin or a polyester resin composition in which polyethylene terephthalate (hereinafter sometimes abbreviated as PET) resin is blended in the range of 30% by weight or less with respect to polybutylene terephthalate resin, is used as a base film layer. According to this technology, a liquid-filled packaging material having bending pinhole resistance, impact resistance, and excellent aroma retention can be obtained. However, this document did not sufficiently consider the specific values and effects of barrier performance.
[0010] In addition, as an alternative to olefin-based sealants, polyester-based sealants with improved low adsorption and heat resistance have been disclosed (see, for example, Patent Document 4). The sealant in Patent Document 4 satisfies heat sealability and heat resistance by separating a layer having heat sealability from other layers and separately controlling the raw material composition of each of these layers. However, the sealant described in Patent Document 4 does not have the ability to block gases such as oxygen and water vapor (gas barrier properties), and therefore does not contribute to improving the barrier performance of the pouch. [Prior art documents] [Patent documents]
[0011] [Patent Document 1] JP 2012-91862 A [Patent Document 2] Patent No. 6500629 [Patent Document 3] JP 2017-094746 A [Patent Document 4] JP 2017-165059 A Summary of the Invention [Problem to be solved by the invention]
[0012] The above Patent Documents 1 to 4 describe the performance of each material, but they do not consider the three performance requirements for an environmentally friendly packaging material, namely (1) containing recycled materials as constituent materials, (2) having gas barrier performance capable of blocking various gases and extending the expiration date, and (3) having a laminate structure that is easy to recycle and has a low environmental impact (mono-material), nor the basic performance requirements as a pouch, such as compatibility between heat sealability, toughness, and transparency. There has not been a polyester-based packaging material that satisfies all of the above configurations and performance requirements.
[0013] The present invention has been made in view of the above problems in the prior art. In other words, an object of the present invention is to provide a laminated product which contains environmentally friendly recycled materials, has a laminate structure composed of almost a single resin type that has a low environmental impact, mainly consisting of polyester, and has the necessary performance properties required for packaging materials, such as gas barrier properties, sealability, toughness, transparency, etc. [Means for solving the problem]
[0014] The inventors have significantly improved the gas barrier performance by laminating and bonding an inorganic thin film layer, a coating layer, and a barrier protection layer onto each film (resin layer) in accordance with the required barrier performance, and have further achieved a mono-material structure while maintaining toughness, sealability, and transparency by laminating a substrate film made of polyester resin derived from PET bottles, which has a low environmental impact, and a sealant made of a polyester component.
[0015] That is, the present invention comprises the following: 1. A laminated product formed by laminating a polyester base film containing 50% by weight or more of polyester resin recycled from PET bottles and a heat-sealable resin in that order, the base film being a laminated film having an inorganic thin film layer (A) and a protective layer (a) made of a urethane resin on one side, the heat-sealable resin being made of a polyester-based component whose main component is ethylene terephthalate, and having a puncture strength of 10 N or more and a haze of 20% or less. 2. A laminated body as described in 1, characterized in that an intermediate layer film is disposed between the base film and the heat-sealable resin via an adhesive, and the intermediate layer film is made of a resin composition containing 70% by mass or more of PBT resin. 3. The laminate according to 1 or 2, wherein an inorganic thin film layer (B) is laminated on at least one surface of the heat-sealable resin. 4. The laminate according to any one of 1. to 3., wherein an inorganic thin film layer (C) is laminated on at least one surface of the intermediate layer film. 5. The laminate according to any one of 1. to 4., wherein a protective layer (b) having a urethane resin is laminated on the inorganic thin film layer (C) of the intermediate layer film. 6. The laminate according to any one of 1. to 5., further comprising a coating layer (Y) between the substrate film and the inorganic thin film layer (C). 7. The laminate according to any one of 4. to 6., further comprising a coating layer (Y) between the intermediate layer film and the inorganic thin film layer (C). 8. The laminate according to any one of 1 to 7, wherein the inorganic thin film layers (A) to (C) are layers made of aluminum oxide or a composite oxide of silicon oxide and aluminum oxide. Effect of the Invention
[0016] This technique has made it possible for the present inventors to provide a laminate that is environmentally friendly and has the necessary properties required for packaging materials, such as barrier properties, sealing properties, and toughness. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0017] The present invention will be described in detail below. The laminated product of the present invention is a laminated product formed by laminating in this order a polyester base film containing 50% by weight or more of polyester resin recycled from PET bottles, and a heat-sealable resin layer, the base film being a laminated film having on one side thereof an inorganic thin film layer (A) and a protective layer (a) containing a urethane resin, the heat-sealable resin layer being made of a polyester-based resin whose main component is ethylene terephthalate, and having a puncture strength of 10 N or more and a haze of 20% or less.
[0018] [Base film layer] In the present invention, as described later, a preferred embodiment is to use recycled polyester resin regenerated from PET bottles containing an isophthalic acid component as an acid component as a raw material for the substrate film. Therefore, the substrate film is a mixed resin of recycled polyester resin and virgin raw material, i.e., non-recycled resin, and the intrinsic viscosity of the resin constituting the film means a value obtained by measuring the intrinsic viscosity of the mixed resin constituting the film. The lower limit of the intrinsic viscosity of the resin constituting the film obtained by measuring the substrate film is preferably 0.58 dl / g, more preferably 0.60 dl / g. If it is less than 0.58 dl / g, many recycled resins made from PET bottles have an intrinsic viscosity exceeding 0.68 dl / g, and if the viscosity is reduced when using it to produce a film, it may cause thickness unevenness defects, which is not preferred. In addition, it is not preferred because the film may be colored. The upper limit is preferably 0.70 dl / g, more preferably 0.68 dl / g. If it exceeds 0.70 dl / g, it may be difficult to extrude the resin from the extruder, which may reduce productivity, which is not preferred.
[0019] The lower limit of the thickness of the base film is preferably 8 μm, more preferably 10 μm, and even more preferably 12 μm. If it is less than 8 μm, the strength of the film may be insufficient, which is not preferable. The upper limit is preferably 200 μm, more preferably 50 μm, and even more preferably 30 μm. If it exceeds 200 μm, it may become too thick and difficult to process. In addition, an increase in the thickness of the film is not preferable in terms of environmental load, and it is preferable to reduce the volume as much as possible.
[0020] The lower limit of the refractive index in the thickness direction of the base film is preferably 1.4930, more preferably 1.4940. If it is less than 1.4930, the orientation is insufficient, and the laminate strength may not be obtained. The upper limit is preferably 1.4995, more preferably 1.4980. If it exceeds 1.4995, the orientation of the surface may be lost, and the mechanical properties may be insufficient, which is not preferable.
[0021] The lower limit of the heat shrinkage rate of the base film in the longitudinal direction (sometimes referred to as MD) and transverse direction (sometimes referred to as TD) when treated at 150°C for 30 minutes is preferably 0.1%, more preferably 0.3%. If it is less than 0.1%, the improvement effect will saturate and the film may become mechanically brittle, which is not preferable. The upper limit is preferably 3.0%, more preferably 2.5%. If it exceeds 3.0%, pitch deviation may occur due to dimensional changes during processing such as printing, which is not preferable. Also, if it exceeds 3.0%, shrinkage in the width direction may occur due to dimensional changes during processing such as printing, which is not preferable.
[0022] As the raw material for the base film, it is preferable to use recycled polyester resin made from PET bottles containing an isophthalic acid component as an acid component. The crystallinity of the polyester used in PET bottles is controlled to improve the bottle appearance, and as a result, polyester containing 10 mol% or less of isophthalic acid may be used. In order to utilize recycled resin, a material containing an isophthalic acid component may be used.
[0023] The lower limit of the amount of the terephthalic acid component in the total dicarboxylic acid components constituting the polyester resin contained in the base film is preferably 95.0 mol%, more preferably 96.0 mol%, even more preferably 96.5 mol%, and particularly preferably 97.0 mol%. If it is less than 95.0 mol%, the crystallinity decreases, so the heat shrinkage rate may increase, which is not preferable. In addition, the upper limit of the amount of the terephthalic acid component of the polyester resin contained in the film is preferably 99.5 mol%, more preferably 99.0 mol%. Since many recycled polyester resins made from PET bottles have dicarboxylic acid components other than terephthalic acid, such as isophthalic acid, it is not preferable for the terephthalic acid component constituting the polyester resin in the film to exceed 99.5 mol%, as this makes it difficult to produce a polyester film with a high ratio of recycled resin.
[0024] The lower limit of the amount of isophthalic acid component in the total dicarboxylic acid components constituting the polyester resin contained in the base film is preferably 0.5 mol%, more preferably 0.7 mol%, even more preferably 0.9 mol%, and particularly preferably 1.0 mol%. Some recycled polyester resins made of PET bottles contain a large amount of isophthalic acid component, so if the isophthalic acid component constituting the polyester resin in the film is less than 0.5 mol%, it becomes difficult to manufacture a polyester film with a high ratio of recycled resin, which is not very preferable. The upper limit of the amount of isophthalic acid component in the total dicarboxylic acid components constituting the polyester resin contained in the film is preferably 5.0 mol%, more preferably 4.0 mol%, even more preferably 3.5 mol%, and particularly preferably 3.0 mol%. If it exceeds 5.0 mol%, the crystallinity decreases, so the heat shrinkage rate may increase, which is not very preferable. In addition, by setting the content of isophthalic acid component to the above range, it is easy to create a film with excellent lamination strength, shrinkage rate, and thickness unevenness, which is preferable.
[0025] The upper limit of the limiting viscosity of the recycled resin from PET bottles is preferably 0.90 dl / g, more preferably 0.80 dl / g, even more preferably 0.77 dl / g, and particularly preferably 0.75 dl / g. If it exceeds 0.9 dl / g, it becomes difficult to extrude the resin from the extruder, which may reduce productivity, and is not preferable.
[0026] The lower limit of the content of polyester resin recycled from PET bottles in the film is preferably 50% by weight, more preferably 65% by weight, and even more preferably 75% by weight. If it is less than 50% by weight, the content is poor and it is not very preferable in terms of contributing to environmental protection as a utilization of recycled resin. Since recycled resin is produced by solid-phase polymerization, the content of oligomers that can cause film whitening is low. Therefore, the higher the content of recycled resin, the more likely it is that film whitening after retort treatment will be improved. If the content of recycled resin is less than 50%, there is a concern that uneven whitening of the film after retort treatment will be promoted. On the other hand, the upper limit of the content of polyester resin recycled from PET bottles is not particularly limited, but is preferably 95% by weight, more preferably 90% by weight, and even more preferably 85% by weight. If it exceeds 95% by weight, it may not be possible to add lubricants such as inorganic particles or additives sufficiently to improve the function of the film, which is not very preferable. In addition, polyester resin recycled from PET bottles can also be used as a master batch (high-concentration resin) used when adding lubricants or additives such as inorganic particles to improve the functionality of the film.
[0027] As the lubricant type, in addition to inorganic lubricants such as silica, calcium carbonate, and alumina, organic lubricants are preferred, and silica and calcium carbonate are more preferred, as they can provide transparency and lubricity.
[0028] The lower limit of the lubricant content in the base film is preferably 0.01% by weight, more preferably 0.015% by weight, and even more preferably 0.02% by weight. If it is less than 0.01% by weight, the slipperiness may decrease. The upper limit is preferably 1% by weight, more preferably 0.2% by weight, and even more preferably 0.1% by weight. If it exceeds 1% by weight, the transparency may decrease, which is not preferable.
[0029] The method for producing the base film used in the laminate of the present invention is not particularly limited, but the following production method is recommended, for example. The temperature setting for melting and extruding the resin in the extruder is important. The basic idea is that (1) since the polyester resin used in PET bottles contains an isophthalic acid component, it is extruded at the lowest possible temperature to suppress deterioration, while (2) in order to melt the intrinsic viscosity and fine highly crystalline parts sufficiently and uniformly, it has a part that melts at high temperature or high pressure. The inclusion of an isophthalic acid component reduces the stereoregularity of the polyester, leading to a decrease in the melting point. Therefore, extrusion at a high temperature will result in a significant decrease or deterioration in the melt viscosity due to heat, resulting in a decrease in mechanical strength and an increase in deteriorated foreign matter. In addition, simply lowering the extrusion temperature may not be enough to perform melt kneading, and there may be problems with increased thickness unevenness and foreign matter such as fish eyes. From the above, the recommended production method includes, for example, using two extruders in tandem, increasing the pressure in the filter section, and using a screw with strong shear force as part of the screw configuration.
[0030] The lower limit of the set temperature in the resin melting section in the extruder (excluding the maximum set temperature in the compression section of the screw in the extruder) is preferably 270° C., and the upper limit is preferably 290° C. If the temperature is less than 270° C., extrusion is difficult, and if the temperature is more than 290° C., deterioration of the resin may occur, which is not preferable.
[0031] The lower limit of the maximum set temperature of the compression section of the screw in the extruder is preferably 295°C. In many cases, high melting point crystals (260°C to 290°C) are present in polyester resins used in PET bottles from the viewpoint of transparency. In addition, additives and crystallization nucleating agents are added, and there is variation in the fine melting behavior in the resin material. If the temperature is less than 295°C, it becomes difficult to melt them sufficiently, which is not preferable. The upper limit of the maximum set temperature of the compression section of the screw in the extruder is preferably 310°C. If the temperature exceeds 310°C, deterioration of the resin may occur, which is not preferable.
[0032] The lower limit of the time for the resin to pass through the region of the highest set temperature of the compression section of the screw in the extruder is preferably 10 seconds, more preferably 15 seconds. If it is less than 10 seconds, the polyester resin used in the PET bottle cannot be sufficiently melted, which is not preferable. The upper limit is preferably 60 seconds, more preferably 50 seconds. If it exceeds 60 seconds, the resin is likely to deteriorate, which is not preferable. By setting the extruder in this range, it is possible to obtain a film with little thickness unevenness, foreign matter such as fish eyes, and coloring, while using a large amount of polyester resin recycled from PET bottles.
[0033] The resin thus melted is extruded into a sheet on a cooling roll and then biaxially stretched. The stretching method may be a simultaneous biaxial stretching method, but a sequential biaxial stretching method is particularly preferred. This makes it easier to satisfy the productivity and quality required by the present invention.
[0034] In the present invention, the film stretching method is not particularly limited, but the following points are important. In order to stretch a resin having an intrinsic viscosity of 0.58 dl / g or more and containing an isophthalic acid component, the stretching ratio and temperature in the machine direction (MD) and transverse direction (TD) are important. If the MD stretching ratio and temperature are not appropriate, the stretching force is not applied uniformly, the orientation of the molecules is insufficient, and there are cases where the thickness unevenness increases and the mechanical properties are insufficient. In addition, the film may break in the next TD stretching step, or there may be an extreme increase in the thickness unevenness. If the TD stretching ratio and temperature are not appropriate, the film may not be stretched uniformly, the balance of the orientation in the machine and transverse directions may be poor, and the mechanical properties may be insufficient. In addition, if the film proceeds to the next heat setting step in a state of large thickness unevenness or insufficient orientation of the molecular chains, there may be problems such as the thickness unevenness not being uniformly relaxed, and the thickness unevenness further increasing and the mechanical properties being insufficient. Therefore, it is basically recommended that in MD stretching, the temperature is adjusted as described below to perform stretching stepwise, and in TD stretching, stretching is performed at an appropriate temperature so as not to cause the orientation balance to become extremely unbalanced. Although not limited to the following embodiment, an example will be described below.
[0035] As a method for stretching in the machine direction (MD), a roll stretching method or an IR heating method is preferred.
[0036] The lower limit of the MD stretching temperature is preferably 100°C, more preferably 110°C, and even more preferably 120°C. If it is less than 100°C, even if a polyester resin with an intrinsic viscosity of 0.58 dl / g or more is stretched and molecularly oriented in the machine direction, the film may break or have an extremely poor thickness in the subsequent transverse stretching step, which is not preferable. The upper limit is preferably 140°C, more preferably 135°C, and even more preferably 130°C. If it exceeds 140°C, the orientation of the molecular chains may be insufficient, and the mechanical properties may be insufficient, which is not preferable.
[0037] The lower limit of the MD stretching ratio is preferably 2.5 times, more preferably 3.5 times, and even more preferably 4 times. If it is less than 2.5 times, even if a polyester resin with an intrinsic viscosity of 0.58 dl / g or more is stretched and molecularly oriented in the machine direction, the film may break or have an extremely poor thickness in the next transverse stretching step, which is not very preferable. The upper limit is preferably 5 times, more preferably 4.8 times, and even more preferably 4.5 times. If it exceeds 5 times, the effects of improving the mechanical strength and thickness unevenness may become saturated, and there is little point in doing so.
[0038] The MD stretching method may be the one-stage stretching described above, but it is more preferable to divide the stretching into two or more stages, which allows the polyester resin made of recycled resin having a high intrinsic viscosity and containing isophthalic acid to be stretched well, and improves thickness unevenness, lamination strength, mechanical properties, etc.
[0039] The lower limit of the first stage MD stretching temperature is preferably 110°C, more preferably 115°C. If it is less than 110°C, the heat is insufficient, the longitudinal stretching cannot be performed sufficiently, and the flatness is poor, which is not preferable. The upper limit of the first stage MD stretching temperature is preferably 125°C, more preferably 120°C. If it exceeds 125°C, the orientation of the molecular chains becomes insufficient, and the mechanical properties may be deteriorated, which is not preferable.
[0040] The lower limit of the first-stage MD stretching ratio is preferably 1.1 times, more preferably 1.3 times. If the first-stage MD stretching ratio is 1.1 times or more, the polyester resin having an intrinsic viscosity of 0.58 dl / g or more can be fully stretched longitudinally by weak stretching in the first stage, and productivity can be improved. The upper limit of the first-stage MD stretching ratio is preferably 2 times, more preferably 1.6 times. If the first-stage MD stretching ratio exceeds 2 times, the orientation of the molecular chain in the longitudinal direction becomes too high, making it difficult to stretch in the second and subsequent stages or resulting in a film with poor thickness unevenness, which is not preferred.
[0041] The lower limit of the MD stretching temperature in the preferred second stage (or final stage) is preferably 110°C, more preferably 115°C. At 110°C or higher, the polyester resin having an intrinsic viscosity of 0.58 dl / g or more can be sufficiently stretched longitudinally, making it possible to stretch transversely in the next step, and improving thickness unevenness in the longitudinal and transverse directions. The upper limit is preferably 130°C, more preferably 125°C. At temperatures above 130°C, crystallization is promoted, making transverse stretching difficult or increasing thickness unevenness, which is not preferred.
[0042] The lower limit of the MD stretch ratio in the preferred second stage (or final stage) is preferably 2.1 times, more preferably 2.5 times. If it is less than 2.1 times, even if a polyester resin with an intrinsic viscosity of 0.58 dl / g or more is stretched and molecularly oriented in the longitudinal direction, the film may break or have extreme thickness defects in the subsequent transverse stretching step, which is not preferred. The upper limit is preferably 3.5 times, more preferably 3.1 times. If it exceeds 3.5 times, the longitudinal orientation becomes too high, making it impossible to perform stretching in the second stage or later, or the film may have large thickness unevenness, which is not preferred.
[0043] The lower limit of the TD stretching temperature is preferably 110°C, more preferably 120°C, and even more preferably 125°C. If it is less than 110°C, the stretching stress in the transverse direction increases, and the film may break or the thickness unevenness may become extremely large, which is not preferable. The upper limit is preferably 150°C, more preferably 145°C, and even more preferably 140°C. If it exceeds 150°C, the orientation of the molecular chains is not increased, and the mechanical properties may decrease, which is not preferable.
[0044] The lower limit of the transverse direction (TD) stretching ratio is preferably 3.5 times, more preferably 3.9 times. If it is less than 3.5 times, the molecular orientation may be weak and the mechanical strength may be insufficient, which is not preferable. In addition, the orientation of the molecular chains in the longitudinal direction is large, and the longitudinal and lateral balance is poor, which causes the thickness unevenness to increase, which is not preferable. The upper limit is preferably 5.5 times, more preferably 4.5 times. If it exceeds 5.5 times, it may break, which is not preferable.
[0045] In order to obtain a substrate film to be used in the laminated film of the present invention, it is desirable to appropriately set the conditions for heat setting in the tenter after the TD stretching and for cooling the film to room temperature thereafter. A polyester film containing recycled resin made of PET bottles containing isophthalic acid has lower crystallinity and is more likely to melt extremely finely than a normal polyethylene terephthalate film that does not contain isophthalic acid, and also has low mechanical strength. Therefore, if it is suddenly exposed to high temperatures under tension after the stretching is completed, or if it is suddenly cooled under tension after the high-temperature heat setting is completed, the unavoidable temperature difference in the width direction of the film will disrupt the tension balance in the width direction, resulting in uneven thickness and poor mechanical properties. On the other hand, if an attempt is made to deal with this phenomenon by lowering the heat setting temperature, sufficient laminate strength may not be obtained. In the present invention, it is recommended to perform a slightly low-temperature heat setting 1, a sufficiently high-temperature heat setting 2 (or heat setting 3 if necessary), and then a slow cooling process to cool the film to room temperature after the stretching is completed. However, this is not limited to this method, and examples thereof include a method of controlling the film tension in accordance with the hot air speed in the tenter and the temperature of each zone, a method of performing a heat treatment at a relatively low temperature in a furnace with a sufficient length after the completion of stretching, and a method of relaxing the film with a heated roll after the completion of heat setting.
[0046] As an example, a method of controlling the temperature of a tenter will be described below.
[0047] The lower limit of the temperature of heat setting 1 is preferably 160°C, more preferably 170°C. If it is less than 160°C, the final heat shrinkage rate will be large, and it may cause misalignment or shrinkage during processing, which is not preferable. The upper limit is preferably 215°C, more preferably 210°C. If it exceeds 215°C, the film will be suddenly exposed to high temperatures, which may cause thickness unevenness to increase or breakage, which is not preferable.
[0048] The lower limit of the time for heat fixation 1 is preferably 0.5 seconds, more preferably 2 seconds. If it is less than 0.5 seconds, the film temperature may not rise sufficiently. The upper limit is preferably 10 seconds, more preferably 8 seconds. If it exceeds 10 seconds, the productivity may decrease, which is not preferable.
[0049] The lower limit of the temperature for heat setting 2 is preferably 220°C, more preferably 227°C. If it is less than 220°C, the heat shrinkage rate increases, which may cause misalignment or shrinkage during processing, and is not preferred. The upper limit is preferably 240°C, more preferably 237°C. If it exceeds 240°C, the film may melt, or even if it does not melt, it may become brittle, which is not preferred.
[0050] The lower limit of the time for heat setting 2 is preferably 0.5 seconds, more preferably 3 seconds. If it is less than 0.5 seconds, breakage may occur easily during heat setting, which is not preferable. The upper limit is preferably 10 seconds, more preferably 8 seconds. If it exceeds 10 seconds, sagging may occur, which may cause thickness unevenness, which is not preferable.
[0051] If necessary, the lower limit of the temperature for providing heat fixation 3 is preferably 205°C, more preferably 220°C. If it is less than 205°C, the heat shrinkage rate increases, which may cause displacement or shrinkage during processing, and is not preferred. The upper limit is preferably 240°C, more preferably 237°C. If it exceeds 240°C, the film may melt, or even if it does not melt, it may become brittle, which is not preferred.
[0052] If necessary, the lower limit of the time for heat fixing 3 is preferably 0.5 seconds, more preferably 3 seconds. If it is less than 0.5 seconds, breakage may occur easily during heat fixing, which is not preferable. The upper limit is preferably 10 seconds, more preferably 8 seconds. If it exceeds 10 seconds, sagging may occur, resulting in uneven thickness, which is not preferable.
[0053] TD relaxation can be performed at any point during heat setting. The lower limit is preferably 0.5%, more preferably 3%. If it is less than 0.5%, the thermal shrinkage rate is particularly large in the lateral direction, which may cause misalignment or shrinkage during processing, which is not preferred. The upper limit is preferably 10%, more preferably 8%. If it exceeds 10%, sagging may occur, which may cause thickness unevenness, which is not preferred.
[0054] The lower limit of the annealing temperature after TD heat setting is preferably 90° C., more preferably 100° C. If it is less than 90° C., the film contains isophthalic acid, and thus the thickness unevenness may become large due to shrinkage caused by a sudden temperature change, or the film may break, which is not preferred. The upper limit of the annealing temperature is preferably 150° C., more preferably 140° C. If it exceeds 150° C., a sufficient cooling effect may not be obtained, which is not preferred.
[0055] The lower limit of the annealing time after heat setting is preferably 2 seconds, more preferably 4 seconds. If it is less than 2 seconds, sufficient annealing effect may not be obtained, which is not preferable. The upper limit is preferably 20 seconds, more preferably 15 seconds. If it exceeds 20 seconds, it is likely to be disadvantageous in terms of productivity, which is not preferable.
[0056] The upper limit of the haze per thickness of the base film layer in the present invention is preferably 0.66% / μm, more preferably 0.60% / μm, and even more preferably 0.53% / μm. When printing is performed on a base film layer having a haze of 0.66% / μm or less, the quality of the printed characters and images is improved.
[0057] In addition, the base film layer in the present invention may be subjected to corona discharge treatment, glow discharge treatment, flame treatment, or surface roughening treatment, and may also be subjected to known anchor coat treatment, printing, decoration, etc., as long as the object of the present invention is not impaired.
[0058] A layer of another material may be laminated on the base film layer in the present invention. As a method for this, the layer may be laminated after the base film layer is produced, or during film formation.
[0059] [Inorganic thin film layer] In the present invention, the inorganic thin film layer (A) is provided on the surface of the base film. The inorganic thin film layer (A) is a thin film made of a metal or an inorganic oxide. There is no particular limitation on the material for forming the inorganic thin film layer as long as it can be made into a thin film, but from the viewpoint of gas barrier properties, inorganic oxides such as silicon oxide (silica), aluminum oxide (alumina), and a mixture of silicon oxide and aluminum oxide are preferred. In particular, a composite oxide of silicon oxide and aluminum oxide is preferred from the viewpoint of achieving both flexibility and denseness of the thin film layer. In this composite oxide, the mixture ratio of silicon oxide and aluminum oxide is preferably in the range of 20 to 70 mass% Al in terms of the mass ratio of the metal content. If the Al concentration is less than 20 mass%, the water vapor barrier property may be reduced. On the other hand, if it exceeds 70 mass%, the inorganic thin film layer tends to become hard, and there is a risk that the film will be destroyed during secondary processing such as printing or lamination, resulting in a reduction in gas barrier property. Note that silicon oxide here refers to various silicon oxides such as SiO and SiO2 or a mixture thereof, and aluminum oxide refers to various aluminum oxides such as AlO and Al2O3 or a mixture thereof. It is an object.
[0060] The thickness of the inorganic thin film layer (A) is usually 1 to 100 nm, preferably 5 to 50 nm. If the thickness of the inorganic thin film layer (A) is less than 1 nm, it may be difficult to obtain satisfactory gas barrier properties, while if the thickness is excessively greater than 100 nm, the corresponding improvement in gas barrier properties cannot be obtained, and it is rather disadvantageous in terms of flex resistance and production costs.
[0061] The method for forming the inorganic thin film layer (A) is not particularly limited, and any known deposition method, such as physical deposition methods (PVD methods) such as vacuum deposition, sputtering, and ion plating, or chemical deposition (CVD), may be appropriately adopted. A typical method for forming the inorganic thin film layer (A) will be described below using a silicon oxide / aluminum oxide thin film as an example. For example, when the vacuum deposition method is adopted, a mixture of SiO2 and Al2O3, or a mixture of SiO2 and Al, is preferably used as the deposition raw material. Particles are usually used as these deposition raw materials, and in this case, it is desirable that the size of each particle is such that the pressure during deposition does not change, and the preferred particle diameter is 1 mm to 5 mm. For heating, methods such as resistance heating, high-frequency induction heating, electron beam heating, and laser heating can be adopted. In addition, it is also possible to adopt reactive deposition by introducing oxygen, nitrogen, hydrogen, argon, carbon dioxide gas, water vapor, etc. as a reactive gas, or by using means such as ozone addition and ion assist. Furthermore, the film formation conditions can be changed as desired by applying a bias to the deposition target (laminated film to be deposited), heating or cooling the deposition target, etc. The deposition material, reactive gas, bias, heating / cooling, etc. of the deposition target can be changed in the same way even when the sputtering method or CVD method is adopted.
[0062] [Coating layer] In the laminate of the present invention, a coating layer (X) can be provided between the base film layer and the inorganic thin film layer (A) in order to ensure stable gas barrier properties and laminate strength. Examples of the resin composition used for the coating layer (X) provided between the base film layer and the inorganic thin film layer (A) include resins such as urethane-based, polyester-based, acrylic-based, titanium-based, isocyanate-based, imine-based, and polybutadiene-based resins to which curing agents such as epoxy-based, isocyanate-based, melamine-based, oxazoline-based, and carbodiimide-based curing agents have been added. It is preferable that the resin composition used for these coating layers (X) contains a silane coupling agent having at least one type of organic functional group. Examples of the organic functional group include an alkoxy group, an amino group, an epoxy group, and an isocyanate group. The addition of the silane coupling agent further improves the laminate strength after retort treatment.
[0063] Among the resin compositions used for the coating layer (X), it is preferable to use a mixture of a resin containing an oxazoline group or a carbodiimide group with an acrylic resin and a urethane resin. These functional groups have high affinity with inorganic thin films, and can react with oxygen-deficient parts of inorganic oxides and metal hydroxides generated during the formation of the inorganic thin film layer, and show strong adhesion to the inorganic thin film layer. In addition, unreacted functional groups present in the coating layer can react with carboxylic acid terminals generated by hydrolysis of the base film layer and the coating layer to form crosslinks.
[0064] In the present invention, the coating weight of the coating layer (X) is 0.010 to 0.200 (g / m 2 ) is preferable. This allows the coating layer to be controlled uniformly, and as a result, the inorganic thin film layer can be densely deposited. In addition, the cohesive force inside the coating layer is improved, and the adhesion between the substrate film-coating layer (X)-inorganic thin film layer (A) is also increased, so that the water-resistant adhesion of the coating layer can be improved. The coating amount of the coating layer (X) is preferably 0.015 (g / m 2 ) or more, more preferably 0.020 (g / m 2 ) or more, more preferably 0.025 (g / m 2) or more, and preferably 0.190 (g / m 2 ) or less, more preferably 0.180 (g / m 2 ) or less, more preferably 0.170 (g / m 2 ) or less. The coating weight of the coating layer (X) is 0.200 (g / m 2 If the thickness of the coating layer (X) is more than 0.010 (g / m), the cohesive force inside the coating layer becomes insufficient, and good adhesion may not be achieved. In addition, the uniformity of the coating layer is reduced, which may cause defects in the inorganic thin film layer and reduce the gas barrier properties. Moreover, the manufacturing cost increases, which is economically disadvantageous. On the other hand, if the thickness of the coating layer (X) is more than 0.010 (g / m), 2 If the thickness is less than 100 nm, the substrate cannot be sufficiently covered, and sufficient gas barrier properties and interlayer adhesion may not be obtained.
[0065] The method for forming the coating layer (X) is not particularly limited, and a conventionally known method such as a coating method can be used. Among the coating methods, preferred methods include an offline coating method and an in-line coating method. For example, in the case of an in-line coating method carried out in the process of producing a base film layer, the conditions of drying and heat treatment during coating vary depending on the coating thickness and the device conditions, but it is preferable to feed the film immediately after coating into a stretching process in the perpendicular direction and dry it in the preheating zone or stretching zone of the stretching process, and in such a case, it is usually preferable to set the temperature at about 50 to 250°C. Examples of the solvent to be used when the coating method is used include aromatic solvents such as benzene and toluene; alcohol solvents such as methanol and ethanol; ketone solvents such as acetone and methyl ethyl ketone; ester solvents such as ethyl acetate and butyl acetate; and polyhydric alcohol derivatives such as ethylene glycol monomethyl ether.
[0066] [Protective layer] In the present invention, the protective layer (a) is provided on the inorganic thin film layer (A). The inorganic thin film layer made of a metal oxide layer is not a completely dense film, but has minute defects scattered therein. By forming the protective layer (a) by applying a specific resin composition for the protective layer described later onto the metal oxide layer, the resin in the resin composition for the protective layer penetrates into the defective parts of the metal oxide layer, resulting in an effect of stabilizing the gas barrier properties. In addition, by using a material having gas barrier properties for the protective layer (a) itself, the gas barrier performance of the laminated film is also greatly improved. Furthermore, the layer having barrier properties prevents hot water from penetrating the substrate, and as a result, the transparency of the film can be maintained.
[0067] In the present invention, the coating weight of the protective layer (a) is 0.10 to 0.40 (g / m 2 ) is preferable. This allows the protective layer to be uniformly controlled during coating, resulting in a film with fewer coating irregularities and defects. In addition, the cohesive strength of the protective layer itself is improved, and the adhesion between the inorganic thin film layer and the protective layer is also strengthened. Furthermore, the protective layer contributes to suppressing oligomer exposure, stabilizing the haze after retort. The coating weight of the protective layer (a) is preferably 0.13 (g / m 2 ) or more, more preferably 0.16 (g / m 2 ) or more, and more preferably 0.19 (g / m 2 ) or more, and preferably 0.37 (g / m 2 ) or less, more preferably 0.34 (g / m 2 ) or less, more preferably 0.31 (g / m 2 ) or less. The adhesion weight of the protective layer (a) is 0.400 (g / m 2 ), the gas barrier properties are improved, but the cohesive force inside the protective layer becomes insufficient and the uniformity of the protective layer also decreases, resulting in unevenness or defects in the coat appearance and inability to fully exhibit gas barrier properties and adhesiveness. On the other hand, if the thickness of the protective layer (a) exceeds 0.10 (g / m 2 ) there is a risk that sufficient gas barrier properties and interlayer adhesion cannot be obtained.
[0068] The resin composition used for the protective layer (a) formed on the surface of the inorganic thin film layer of the laminate of the present invention contains a urethane-based resin as an essential component, and other resins such as polyester-based, acrylic-based, titanium-based, isocyanate-based, imine-based, and polybutadiene-based resins can also be used, and epoxy-based, isocyanate-based, and melamine-based curing agents may also be added. In particular, the inclusion of a urethane resin is preferred because, in addition to the barrier performance due to the high cohesiveness of the urethane bond itself, the polar group interacts with the inorganic thin film layer, and the film also has flexibility due to the presence of amorphous parts, so that damage to the inorganic thin film layer can be suppressed even when a bending load is applied. Polyester resins are also preferred because they are expected to have the same effect.
[0069] (urethane resin) From the viewpoint of improving the barrier property by the cohesive force, the urethane resin used in the present invention preferably has a glass transition temperature (Tg) of 100°C or more, more preferably 110°C or more, and even more preferably 120°C or more. However, in order to develop adhesive force, a soft resin having excellent flexibility and a Tg of 100°C or less may be mixed and used. In that case, the addition ratio of the soft resin is preferably within the range of 0 to 80%, more preferably within the range of 10 to 70%, and even more preferably within the range of 20 to 60%. When the addition ratio is within the above range, it is possible to achieve both cohesive force and flexibility, and the barrier property and adhesive property are good. Note that, if the addition ratio exceeds 80%, the film becomes too soft, which may lead to a decrease in barrier performance.
[0070] From the viewpoint of improving gas barrier properties, it is more preferable to use a urethane resin containing an aromatic or araliphatic diisocyanate component as a main constituent component. Among these, it is particularly preferable to contain a metaxylylene diisocyanate component. By using the above resin, the cohesive strength of the urethane bond can be further increased due to the stacking effect between aromatic rings, and as a result, good gas barrier properties can be obtained.
[0071] In the present invention, the ratio of aromatic or araliphatic diisocyanate in the urethane resin is preferably in the range of 50 mol% or more (50 to 100 mol%) in 100 mol% of the polyisocyanate component (F). The total amount of aromatic or araliphatic diisocyanate is preferably 60 to 100 mol%, more preferably 70 to 100 mol%, and even more preferably 80 to 100 mol%. As such a resin, the "Takelac (registered trademark) WPB" series commercially available from Mitsui Chemicals, Inc. can be suitably used. If the total amount of aromatic or araliphatic diisocyanate is less than 50 mol%, good gas barrier properties may not be obtained.
[0072] In the urethane resin used in the present invention, various crosslinking agents (silicon-based crosslinking agents) may be blended in order to improve the cohesive strength of the film and the adhesion resistance to wet heat, as long as the gas barrier properties are not impaired. As a method for introducing silanol groups into the protective layer, a method of post-adding a silane coupling agent or the like is also known. However, in this method, there is a possibility that the work becomes complicated and the amount of the agent to be added may be measured incorrectly. On the other hand, by incorporating silanol groups into the polyurethane dispersion skeleton in advance, there is an advantage in that the above-mentioned complications and mistakes can be prevented.
[0073] If the amount of silanol groups in the polyurethane dispersion, expressed as the amount of Si element contained in the silanol groups, is less than 700 mg per 1 kg of the resin that constitutes the polyurethane dispersion, the formation of a crosslinked structure will be insufficient, and the resin itself will deteriorate when retort treatment is performed, which will cause a decrease in adhesion and gas barrier properties after retort treatment. In addition, if the amount of silanol groups contained exceeds 1700 mg per kg of resin constituting the polyurethane dispersion as the amount of Si element contained in the silanol groups, the cross-linked structure becomes too numerous, which impairs the flexibility of the protective layer, causing deterioration of the inorganic thin film during retort treatment and a decrease in bending resistance. Furthermore, the amount of unreacted silanol groups increases, weakening water resistance and possibly causing deterioration of the resin itself during retort treatment.
[0074] On the other hand, examples of the crosslinking agent that can be added later include silicon-based crosslinking agents, oxazoline compounds, carbodiimide compounds, epoxy compounds, etc. Among them, by blending a silicon-based crosslinking agent, it is possible to improve the water-resistant adhesion to the inorganic thin film layer in particular. From this viewpoint, silicon-based crosslinking agents are particularly preferred. Other crosslinking agents may be used in combination with oxazoline compounds, carbodiimide compounds, epoxy compounds, etc.
[0075] As the silicon-based crosslinking agent, a silane coupling agent is preferred from the viewpoint of crosslinking between an inorganic substance and an organic substance.Examples of the silane coupling agent include hydrolyzable alkoxysilane compounds, such as halogen-containing alkoxysilanes (chloro C2-4 alkyl tri C1-4 alkoxysilanes such as 2-chloroethyltrimethoxysilane, 2-chloroethyltriethoxysilane, 3-chloropropyltrimethoxysilane, and 3-chloropropyltriethoxysilane), alkoxysilanes having an epoxy group [2-glycidyloxyethyltrimethoxysilane, 2-glycidyloxyethyltriethoxysilane, 3-glycidyloxypropyltrimethoxysilane, 3-glycidyloxypropyltriethoxy ... -glycidyloxy C2-4 alkyl tri C1-4 alkoxy silanes such as glycidyloxypropyl triethoxy silane, glycidyloxy di C2-4 alkyl di C1-4 alkoxy silanes such as 3-glycidyloxypropyl methyl dimethoxy silane and 3-glycidyloxypropyl methyl diethoxy silane, (epoxy cyclohexyl) ethyl trimethoxy silane, 2-(3,4-epoxy cyclohexyl) ethyl triethoxy silane, 3-(3,4-epoxy cyclohexyl) propyl trimethoxy silane, etc. alkyl)C2-4 alkyltriC1-4 alkoxysilane, etc.], alkoxysilanes having an amino group [amino C2-4 alkyltriC1-4 alkoxysilanes such as 2-aminoethyltrimethoxysilane, 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, etc., amino diC2-4 alkyldiC1-4 alkoxysilanes such as 3-aminopropylmethyldimethoxysilane, 3-aminopropylmethyldiethoxysilane, etc., 2-[N-(2-aminoethyl)amino]ethyltrimethoxysilane, 3-[N-(2-aminoethyl (2-amino C2-4 alkyl) amino C2-4 alkyl tri C1-4 alkoxysilanes such as 3-[N-(2-aminoethyl)amino]propyltrimethoxysilane and 3-[N-(2-aminoethyl)amino]propyltriethoxysilane; (amino C2-4 alkyl) amino di C2-4 alkyl di C1-4 alkoxysilanes such as 3-[N-(2-aminoethyl)amino]propylmethyldimethoxysilane and 3-[N-(2-aminoethyl)amino]propylmethyldiethoxysilane; and alkoxysilanes having a mercapto group (2-mercaptoethyltrimethoxysilane). , mercapto C2-4 alkyl tri C1-4 alkoxy silanes such as 3-mercaptopropyl trimethoxy silane and 3-mercaptopropyl triethoxy silane, mercapto di C2-4 alkyl di C1-4 alkoxy silanes such as 3-mercaptopropyl methyl dimethoxy silane and 3-mercaptopropyl methyl diethoxy silane), alkoxy silanes having a vinyl group (vinyl tri C1-4 alkoxy silanes such as vinyl trimethoxy silane and vinyl triethoxy silane), alkoxy silanes having an ethylenically unsaturated bond group [(meth)acryloxy C2-4 alkyl tri C1-4 alkoxy silanes such as 2-(meth)acryloxyethyl trimethoxy silane, 2-(meth)acryloxyethyl triethoxy silane, 3-(meth)acryloxypropyl trimethoxy silane, and 3-(meth)acryloxypropyl triethoxy silane, (meth)acryloxy di C2-4 alkyl di C1-4 alkoxy silanes such as 3-(meth)acryloxypropyl methyl dimethoxy silane and 3-(meth)acryloxypropyl methyl diethoxy silane, etc.] and the like can be exemplified. These silane coupling agents can be used alone or in combination of two or more. Among these silane coupling agents, silane coupling agents having an amino group are preferred.
[0076] The silane coupling agent or silicon-based crosslinking agent is preferably added to the protective layer in an amount of 0.25 to 3.00% by mass, more preferably 0.5 to 2.75% by mass, and even more preferably 0.75 to 2.50% by mass. If the amount added exceeds 3.00% by mass, the film hardens and the cohesive strength improves, but some unreacted portions may be generated, and the adhesion between layers may decrease. On the other hand, if the amount added is less than 0.25% by mass, sufficient cohesive strength may not be obtained.
[0077] (polyester resin) The polyester resin used in the protective layer of the present invention is produced by polycondensation of a polyvalent carboxylic acid component and a polyhydric alcohol component. The molecular weight of the polyester is not particularly limited as long as it can provide sufficient film toughness, coating suitability, and solvent solubility as a coating material, but is preferably 1000 to 50000 in number average molecular weight, more preferably 1500 to 30000. The functional group at the polyester end is also not particularly limited, and may be an alcohol end, a carboxylic acid end, or both. However, when an isocyanate-based curing agent is used in combination, it is necessary to use a polyester polyol mainly composed of alcohol ends.
[0078] [Polyester glass transition temperature (Tg)] The Tg of the polyester used in the present invention must be 15°C or higher. If the temperature is lower than this, the resin will become tacky after the coating operation, and blocking will easily occur, making the winding operation after coating difficult. If the Tg is 15°C or lower, it will be difficult to prevent blocking even under conditions where the pressure near the winding core is high, even with the addition of an anti-blocking agent. The Tg temperature is more preferably 18°C or higher, and even more preferably 25°C or higher.
[0079] The polyester used in the present invention is prepared by polycondensing a polyvalent carboxylic acid component and a polyhydric alcohol component. [Polycarboxylic acid component] The polyvalent carboxylic acid component of the polyester used in the present invention is characterized by containing at least one of ortho-oriented aromatic dicarboxylic acid or anhydride thereof. Examples of aromatic polycarboxylic acids or anhydrides thereof in which a carboxylic acid is substituted at the ortho position include orthophthalic acid or anhydride, naphthalene 2,3-dicarboxylic acid or anhydride, naphthalene 1,2-dicarboxylic acid or anhydride, anthraquinone 2,3-dicarboxylic acid or anhydride, and 2,3-anthracene carboxylic acid or anhydride. These compounds may have a substituent at any carbon atom of the aromatic ring. Examples of the substituent include a chloro group, a bromo group, a methyl group, an ethyl group, an i-propyl group, a hydroxyl group, a methoxy group, an ethoxy group, a phenoxy group, a methylthio group, a phenylthio group, a cyano group, a nitro group, an amino group, a phthalimide group, a carboxyl group, a carbamoyl group, an N-ethylcarbamoyl group, a phenyl group, or a naphthyl group. In addition, polyester polyols having a usage rate of 70 to 100% by mass relative to the total amount of these polycarboxylic acid components are particularly preferred because they have a high effect of improving barrier properties and are excellent in solvent solubility, which is essential for a coating material.
[0080] The polyester used in the present invention may be copolymerized with other polyvalent carboxylic acid components within the range that does not impair the effects of the present invention. Specifically, examples of aliphatic polycarboxylic acids include succinic acid, adipic acid, azelaic acid, sebacic acid, and dodecanedicarboxylic acid; examples of unsaturated bond-containing polycarboxylic acids include maleic anhydride, maleic acid, and fumaric acid; examples of alicyclic polycarboxylic acids include 1,3-cyclopentanedicarboxylic acid and 1,4-cyclohexanedicarboxylic acid; examples of aromatic polycarboxylic acids include terephthalic acid, isophthalic acid, pyromellitic acid, trimellitic acid, 1,4-naphthalenedicarboxylic acid, 2,5-naphthalenedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, naphthalic acid, biphenyldicarboxylic acid, diphenic acid and its anhydride, 1,2-bis(phenoxy)ethane-p,p'-dicarboxylic acid, and anhydrides or ester-forming derivatives of these dicarboxylic acids; p-hydroxybenzoic acid, p-(2-hydroxyethoxy)benzoic acid, and ester-forming derivatives of these dihydroxycarboxylic acids; and the like, which can be used alone or in a mixture of two or more kinds. Among these, succinic acid, 1,3-cyclopentanedicarboxylic acid, isophthalic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalic acid, and diphenic acid are preferred from the viewpoints of solubility in organic solvents and gas barrier properties.
[0081] [Polyhydric alcohol component] The polyhydric alcohol component of the polyester used in the present invention is not particularly limited as long as it can synthesize a polyester that exhibits gas barrier compensation performance, but it is preferable to contain a polyhydric alcohol component containing at least one selected from the group consisting of ethylene glycol, propylene glycol, butylene glycol, neopentyl glycol, cyclohexanedimethanol, and 1,3-bishydroxyethylbenzene. Among them, it is most preferable to use ethylene glycol as the main component, since it is presumed that the smaller the number of carbon atoms between oxygen atoms, the less the molecular chain will be excessively flexible and the less oxygen will permeate.
[0082] The polyester used in the present invention preferably uses the above-mentioned polyhydric alcohol component, but other polyhydric alcohol components may be copolymerized within a range that does not impair the effects of the present invention. Specifically, the diols include 1,5-pentanediol, 3-methyl-1,5-pentanediol, 1,6-hexanediol, methylpentanediol, dimethylbutanediol, butylethylpropanediol, diethylene glycol, triethylene glycol, tetraethylene glycol, dipropylene glycol, and tripropylene glycol, and the trihydric or higher alcohols include glycerol, trimethylolpropane, trimethylolethane, tris(2-hydroxyethyl)isocyanurate, 1,2,4-butanetriol, pentaerythritol, and dipentaerythritol. In particular, polyesters using glycerol and tris(2-hydroxyethyl)isocyanurate in combination among trihydric alcohols are particularly preferably used because they have a moderately high crosslinking density due to their branched structure, have good solubility in organic solvents, and have excellent barrier function.
[0083] Examples of catalysts used in the reaction to obtain the polyester of the present invention include tin catalysts such as monobutyltin oxide and dibutyltin oxide, titanium catalysts such as tetra-isopropyl-titanate and tetra-butyl-titanate, and acid catalysts such as zirconia catalysts such as tetra-butyl-zirconate. It is preferable to use the titanium catalysts such as tetra-isopropyl-titanate and tetra-butyl-titanate, which have high activity in esterification reactions, in combination with the zirconia catalyst. The amount of the catalyst is 1 to 1000 ppm, more preferably 10 to 100 ppm, based on the total mass of the reaction raw materials used. If the amount is less than 1 ppm, it is difficult to obtain the effect of the catalyst, and if the amount is more than 1000 ppm, a problem of inhibiting the urethane reaction may occur when an isocyanate curing agent is used.
[0084] In the present invention, when a polyester resin is used as the main agent of the coating agent constituting the protective layer, it is necessary to use an isocyanate-based curing agent to make it into a urethane resin. In this case, the coating layer becomes a crosslinked system, which has the advantage of improving heat resistance, abrasion resistance, and rigidity. Therefore, it is easy to use for boiling and retort packaging. On the other hand, there is a problem that the liquid cannot be reused after mixing the curing agent, and a curing (aging) process is necessary after coating.
[0085] The polyisocyanate compound used in the protective layer (a) of the present invention is highly polar as a resin component by reacting at least a part of the polyester with a hydroxyl group to form a urethane structure. The gas barrier function can be further enhanced by crosslinking the resin of the coating material with a polyisocyanate having a valence of 3 or more, thereby causing aggregation between polymer chains. When the resin of the coating material is a straight-chain resin, heat resistance and abrasion resistance can be imparted by crosslinking with a polyisocyanate having a valence of 3 or more. The polyisocyanate compound used in the present invention may be any of diisocyanates, polyisocyanates having a valence of 3 or more, low molecular weight compounds, and high molecular weight compounds, but it is preferable to contain an aromatic ring or an aliphatic ring in a part of the skeleton from the viewpoint of improving the gas barrier function. For example, examples of isocyanates having an aromatic ring include toluene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, and naphthalene diisocyanate; examples of isocyanates having an aliphatic ring include hydrogenated xylylene diisocyanate, hydrogenated toluene diisocyanate, isophorone diisocyanate, norbornine diisocyanate, or trimers of these isocyanate compounds; and compounds containing terminal isocyanate groups obtained by reacting an excess amount of these isocyanate compounds with low molecular weight active hydrogen compounds such as ethylene glycol, propylene glycol, trimethylolpropane, glycerin, sorbitol, ethylenediamine, monoethanolamine, diethanolamine, and triethanolamine, or high molecular weight active hydrogen compounds such as various polyester polyols, polyether polyols, and polyamides.
[0086] The method of coating the resin composition for the protective layer is not particularly limited as long as it is a method that coats the film surface to form a layer. For example, a typical coating method such as gravure coating, reverse roll coating, wire bar coating, or die coating can be used.
[0087] When forming the protective layer (a), it is preferable to apply the resin composition for the protective layer and then heat-dry it. The drying temperature is preferably 110 to 190°C, more preferably 130 to 185°C, and even more preferably 150 to 180°C. If the drying temperature is less than 110°C, the protective layer may be insufficiently dried, or the film formation of the protective layer may not proceed, resulting in a decrease in cohesive strength and water-resistant adhesion, and as a result, the barrier properties and hand-tearability may decrease. On the other hand, if the drying temperature exceeds 190°C, the film may be too hot, making it brittle and reducing puncture strength, or shrinking and causing poor processability. In particular, by drying at 150°C or higher, preferably 160°C or higher, the film formation of the protective layer proceeds effectively, and the adhesive area between the resin of the protective layer and the inorganic thin film layer becomes larger, thereby improving the water-resistant adhesion. It is particularly preferable to first volatilize the solvent at a relatively low temperature of 90°C to 110°C immediately after application, and then dry at 150°C or higher, since a uniform and transparent film can be obtained. In addition to drying, additional heat treatment at a temperature as low as possible is also effective in accelerating the formation of the protective layer.
[0088] [Interlayer film] In the present invention, in order to ensure the toughness of the bag while enabling mono-materialization, a polyester film mainly composed of PBT can be used as the intermediate layer. The intermediate layer film used in the present invention is a biaxially stretched film made of a resin composition containing 70% by mass or more of PBT. The PBT content is more preferably 75% by mass or more. If the PBT content is less than 70% by mass, the puncture strength decreases and the film properties are no longer sufficient. PBT preferably contains 90 mol % or more, more preferably 95 mol % or more, even more preferably 98 mol % or more, and most preferably 100 mol % of terephthalic acid as a dicarboxylic acid component, and preferably contains 90 mol % or more, more preferably 95 mol % or more, even more preferably 97 mol % or more of 1,4-butanediol as a glycol component, and most preferably contains no by-products other than those generated by ether bonds of 1,4-butanediol during polymerization.
[0089] The resin composition used in the intermediate layer film of the present invention may contain a polyester other than PBT for the purpose of adjusting the film formability during biaxial stretching and the mechanical properties of the obtained film. Examples of polyesters other than PBT include at least one polyester selected from the group consisting of PET, polyethylene naphthalate, polybutylene naphthalate, and polypropylene terephthalate; PBT copolymerized with at least one dicarboxylic acid selected from the group consisting of isophthalic acid, orthophthalic acid, naphthalenedicarboxylic acid, biphenyl dicarboxylic acid, cyclohexane dicarboxylic acid, adipic acid, azelaic acid, and sebacic acid; and PBT copolymerized with at least one diol component selected from the group consisting of ethylene glycol, 1,3-propylene glycol, 1,2-propylene glycol, neopentyl glycol, 1,5-pentanediol, 1,6-hexanediol, diethylene glycol, cyclohexanediol, polyethylene glycol, polytetramethylene glycol, and polycarbonate diol.
[0090] The upper limit of the amount of the polyester resin other than PBT added is preferably 30% by mass or less, more preferably 25% by mass or less. If the amount of the polyester resin other than PBT added exceeds 30% by mass, the mechanical properties of polybutylene terephthalate are impaired, and the impact strength, pinhole resistance, or bag rupture resistance becomes insufficient, and in addition, problems such as reduced transparency and gas barrier properties may occur.
[0091] The lower limit of the intrinsic viscosity of the polybutylene terephthalate (PBT) used in the present invention is preferably 0.9 dl / g, more preferably 0.95 dl / g, and further preferably 1.0 dl / g. If the intrinsic viscosity of the raw material polybutylene terephthalate (PBT) is less than 0.9 dl / g, the intrinsic viscosity of the film obtained by film formation will be low, and the puncture strength, impact strength, pinhole resistance, bag rupture resistance, etc. may be reduced. The upper limit of the intrinsic viscosity of polybutylene terephthalate is preferably 1.4 dl / g. If it exceeds the upper limit, the stress during stretching becomes too high, and film formability may deteriorate. When polybutylene terephthalate with a high intrinsic viscosity is used, the melt viscosity of the resin becomes high, so the extrusion temperature needs to be high, but extruding polybutylene terephthalate at a higher temperature may easily produce decomposition products.
[0092] The polybutylene terephthalate (PBT) resin may contain conventionally known additives, such as a lubricant, a stabilizer, a colorant, an antistatic agent, and an ultraviolet absorbing agent, if necessary. As the lubricant type, inorganic lubricants such as silica, calcium carbonate, alumina, and organic lubricants are preferable, silica and calcium carbonate are more preferable, and silica is particularly preferable in terms of reducing haze. These lubricants can provide transparency and lubricity. The lower limit of the lubricant concentration is preferably 100 ppm, more preferably 500 ppm, and even more preferably 800 ppm. If it is less than the above, the slipperiness of the base film layer may decrease. The upper limit of the lubricant concentration is preferably 20000 ppm, more preferably 10000 ppm, and even more preferably 1800 ppm. If it exceeds the above, the transparency may decrease.
[0093] The upper limit of the heat shrinkage rate of the biaxially stretched polyester film constituting the intermediate layer film in the present invention after heating at 150°C for 15 minutes in the longitudinal stretching (machine direction) direction (MD) and transverse stretching (width) direction (TD) is preferably 4.0%, more preferably 3.0%, and even more preferably 2%. If the upper limit is exceeded, not only may cracks occur in the inorganic thin film layer due to dimensional changes in the intermediate layer film that occur during the process of forming the inorganic thin film layer / protective layer or during high-temperature treatment such as retort sterilization, resulting in a decrease in gas barrier properties, but also pitch deviation may occur due to dimensional changes during processing such as printing.
[0094] The lower limit of the heat shrinkage rate of the biaxially oriented polyester film constituting the intermediate layer film in the present invention after heating at 150° C. for 15 minutes in both the longitudinal stretching direction (MD) and the transverse stretching direction (TD) is preferably 0%. If it is below the lower limit, the improvement effect will not be further obtained (saturation will occur) and the film may become mechanically brittle.
[0095] The lower limit of the impact strength of the biaxially oriented polyester film constituting the intermediate layer film in the present invention is preferably 0.05 J / μm. If it is 0.05 J / μm or more, the strength is sufficient when used as a bag. The upper limit of the impact strength of the biaxially oriented polyester film constituting the intermediate layer film in the present invention is preferably 0.2 J / μm. Even if the upper limit is exceeded, the effect of improvement is not obtained any more (it becomes saturated).
[0096] The lower limit of the planar orientation degree (ΔP) of the PBT film which is the intermediate layer film of the present invention is preferably 0.144, more preferably 0.148, and further preferably 0.15. If it is less than the above, the orientation is weak, so not only is sufficient strength not obtained and the puncture strength may decrease, but also, when an inorganic thin film layer (C) is provided on the intermediate layer film to form a laminate film, the inorganic thin film layer is easily stretched by the tension and temperature applied during formation, and the inorganic thin film layer may crack, resulting in a decrease in gas barrier properties. The upper limit of the planar orientation degree (ΔP) of the intermediate layer film in the present invention is preferably 0.160, more preferably 0.158. If it exceeds the above, the orientation becomes too strong and the film is easily broken during film formation. In addition, the higher the orientation, the higher the heat setting temperature is required to reduce the heat shrinkage rate, and there is a risk that the strength of the film will be reduced due to crystallization.
[0097] The upper limit of the haze per thickness of the biaxially oriented polyester film constituting the intermediate layer film in the present invention is preferably 0.66% / μm, more preferably 0.60% / μm, and even more preferably 0.53% / μm. When printing is performed on a base layer having a haze of 0.66% / μm or less, the quality of the printed characters and images is improved.
[0098] The upper limit of the intrinsic viscosity (IV) of the biaxially stretched polyester film constituting the intermediate layer film in the present invention is preferably 1.20 dl / g, more preferably 1.15 dl / g, and even more preferably 1.10 dl / g. If it exceeds the upper limit, the strength of the film is improved, but the pressure load on the filter during extrusion becomes large, making production difficult. The lower limit is preferably 0.60 dl / g, more preferably 0.65 dl / g, and even more preferably 0.70 dl / g. If it is below the lower limit, the strength of the film may decrease.
[0099] In addition, the biaxially oriented polyester film constituting the intermediate layer film in the present invention may be subjected to corona discharge treatment, glow discharge treatment, flame treatment, or surface roughening treatment, and may also be subjected to known anchor coat treatment, printing, decoration, etc., as long as the object of the present invention is not impaired.
[0100] Next, a method for producing the biaxially oriented polyester film constituting the intermediate layer film of the present invention will be described in detail, although the method is not limited thereto. The manufacturing method for obtaining the biaxially oriented polyester film constituting the intermediate layer film of the present invention comprises the steps of melt-extruding a polyester raw material resin into a sheet form and cooling it on a casting drum to form an unstretched sheet, a longitudinal stretching step of stretching the formed unstretched sheet in the longitudinal direction, a preheating step of preheating to a temperature at which the unstretched sheet can be stretched laterally after the longitudinal stretching, a transverse stretching step of stretching the unstretched sheet in the width direction perpendicular to the longitudinal direction, a heat setting step of heating and crystallizing the film after the longitudinal and transverse stretching steps, a heat relaxation step of removing residual strain in the heat-set film, and a cooling step of cooling the film after heat relaxation.
[0101] [Unstretched sheet molding process] First, the film raw materials are dried or hot air dried, then the raw materials are weighed, mixed, and fed into an extruder, where they are heated and melted, and then melt-cast into a sheet. The molten resin sheet is then brought into contact with a cooling roll (casting roll) using an electrostatic application method, and cooled and solidified to obtain an unstretched sheet. The electrostatic application method is a method in which a voltage is applied to an electrode disposed near the surface of the resin sheet opposite to the surface that contacts the rotating metal roll near where the molten resin sheet contacts the rotating metal roll, thereby charging the resin sheet and bringing the resin sheet into close contact with the rotating cooling roll.
[0102] The lower limit of the resin heat melting temperature is preferably 200°C, more preferably 250°C, and even more preferably 260°C. If the temperature is lower than the above, extrusion may become unstable. The upper limit of the resin melting temperature is preferably 280°C, more preferably 270°C. If the temperature exceeds the above, decomposition of the resin proceeds, and the film becomes brittle.
[0103] It is preferable to reduce the difference in crystallinity in the width direction when the molten polyester resin is extruded and cast onto a cooling roll. Specific methods for this purpose include casting raw materials of the same composition in a multi-layered form when the molten polyester resin is extruded and cast onto a cooling roll, and further lowering the cooling roll temperature. PBT resin has a fast crystallization rate, so crystallization continues even during casting. In this case, if the film is cast in a single layer without being multi-layered, the crystals will grow into large spherulites because there is no barrier that can suppress the growth of the crystals. As a result, the yield stress of the obtained unstretched sheet will be high, and not only will it be easily broken during biaxial stretching, but the impact strength, pinhole resistance, or bag breakage resistance of the obtained biaxially stretched film will be insufficient. On the other hand, by laminating the same resin in multiple layers, the stretching stress of the unstretched sheet can be reduced, and the subsequent biaxial stretching can be stably performed.
[0104] The method of extruding molten polyester resin and casting raw materials of the same composition into multiple layers specifically includes at least a step (1) of melting a resin composition containing 70% by weight or more of PBT resin to form a molten fluid, a step (2) of forming a laminated fluid having 60 or more layers from the formed molten fluid, a step (3) of discharging the formed laminated fluid from a die and bringing it into contact with a cooling roll to solidify it to form a laminated unstretched sheet, and a step (4) of biaxially stretching the laminated unstretched sheet. Other steps may be inserted between step (1) and step (2) and between step (2) and step (3). For example, a filtration step, a temperature change step, etc. may be inserted between step (1) and step (2). Furthermore, a temperature change step, a charge application step, etc. may be inserted between step (2) and step (3). However, there must be no step between step (2) and step (3) that destroys the laminated structure formed in step (2).
[0105] In step (1), the method for melting the polyester resin composition to form a molten fluid is not particularly limited, but a suitable method is to heat and melt the composition using a single-screw extruder or a twin-screw extruder.
[0106] The method for forming the laminated fluid in step (2) is not particularly limited, but from the viewpoints of facility simplicity and maintainability, a static mixer and / or a multi-layer feed block is more preferred. From the viewpoint of uniformity in the sheet width direction, a device having a rectangular melt line is more preferred. It is further preferred to use a static mixer or a multi-layer feed block having a rectangular melt line. The resin composition consisting of multiple layers formed by joining multiple resin compositions may be passed through one or more of a static mixer, a multi-layer feed block, and a multi-layer manifold.
[0107] The theoretical number of layers in step (2) is preferably 60 or more. The lower limit of the theoretical number of layers is more preferably 500. If the theoretical number of layers is too small, or the distance between the layer interfaces is long and the crystal size becomes too large, the effect of the present invention tends not to be obtained. In addition, the crystallinity increases near both ends of the sheet, making film formation unstable and reducing transparency after molding. The upper limit of the theoretical number of layers in step (2) is not particularly limited, but is preferably 100,000, more preferably 10,000, and even more preferably 7,000. Even if the theoretical number of layers is extremely large, the effect may become saturated.
[0108] When the lamination in step (2) is performed using a static mixer, the theoretical number of layers can be adjusted by selecting the number of elements of the static mixer. A static mixer is generally known as a stationary mixer (line mixer) without a drive unit, and the fluid that enters the mixer is stirred and mixed sequentially by the elements. However, when a high-viscosity fluid is passed through a static mixer, the high-viscosity fluid is divided and layered, forming a layered fluid. Each time the high-viscosity fluid passes through one element of the static mixer, it is divided into two, which then merge and are layered. For this reason, when a high-viscosity fluid is passed through a static mixer with n elements, a layered fluid with a theoretical number of layers N = 2n is formed.
[0109] A typical static mixer element has a rectangular plate twisted 180 degrees, with right and left elements depending on the direction of twist, and the dimensions of each element are basically 1.5 times the length compared to the diameter. Static mixers that can be used in the present invention are not limited to this type.
[0110] When the lamination in step (2) is performed in a multi-layer feedblock, the theoretical number of layers can be adjusted by selecting the number of divisions and laminations of the multi-layer feedblock. Multiple multi-layer feedblocks can be installed in series. It is also possible for the high-viscosity fluid supplied to the multi-layer feedblock itself to be the lamination fluid. For example, if the number of layers of the high-viscosity fluid supplied to the multi-layer feedblock is p, the number of divisions and layers of the multi-layer feedblock is q, and the number of installed multi-layer feedblocks is r, the number of layers N of the lamination fluid is N = p × qr.
[0111] In step (3), the laminating fluid is discharged from the die and solidified by contacting it with a chill roll. The lower limit of the cooling roll temperature is preferably -10°C. If the temperature is lower than this, the effect of suppressing crystallization may become saturated. The upper limit of the cooling roll temperature is preferably 40°C. If the temperature exceeds this, the crystallinity may become too high, making stretching difficult. The upper limit of the cooling roll temperature is preferably 25°C. Furthermore, when the cooling roll temperature is in the above range, it is preferable to lower the humidity of the environment near the cooling roll to prevent condensation. It is preferable to reduce the temperature difference in the width direction of the cooling roll surface. In this case, the thickness of the unstretched sheet is preferably in the range of 15 to 2500 μm. The above-mentioned multi-layered unstretched sheet has at least 60 layers, preferably at least 250 layers, and more preferably at least 1000 layers. If the number of layers is too small, the effect of improving stretchability is lost.
[0112] [Longitudinal and transverse stretching processes] The stretching method can be either simultaneous biaxial stretching or sequential biaxial stretching, but in order to increase the piercing strength, it is necessary to increase the degree of planar orientation, and sequential biaxial stretching is most preferable in terms of high productivity and high film production speed.
[0113] The lower limit of the stretching temperature in the longitudinal stretching direction is preferably 55°C, more preferably 60°C. At 55°C or higher, breakage is unlikely to occur. In addition, since the longitudinal orientation of the film is not too strong, shrinkage stress during heat setting treatment can be suppressed, and a film with less distortion of molecular orientation in the width direction can be obtained. The upper limit of the stretching temperature in the longitudinal stretching direction is preferably 100°C, more preferably 95°C. If it is 100°C or lower, the orientation of the film is not too weak, so the mechanical properties of the film are not reduced.
[0114] The lower limit of the stretching ratio in the longitudinal stretching direction is preferably 2.8 times, and particularly preferably 3.0 times. If it is 2.8 times or more, the degree of planar orientation increases, and the puncture strength of the film improves. The upper limit of the stretching ratio in the longitudinal stretching direction is preferably 4.3 times, more preferably 4.0 times, and particularly preferably 3.8 times. If it is 4.3 times or less, the orientation degree in the transverse direction of the film is not too strong, the shrinkage stress during heat setting is not too large, and the distortion of the molecular orientation in the transverse direction of the film is small, resulting in improved linear tearability in the longitudinal direction. In addition, the effect of improving the mechanical strength and thickness unevenness is saturated within this range.
[0115] The lower limit of the stretching temperature in the transverse stretching direction is preferably 60° C., and if it is 60° C. or higher, breakage may be less likely to occur. The upper limit of the stretching temperature in the transverse stretching direction is preferably 100° C., and if it is 100° C. or lower, the degree of orientation in the transverse direction increases, improving the mechanical properties.
[0116] The lower limit of the stretching ratio in the transverse stretching direction is preferably 3.5 times, more preferably 3.6 times, and particularly preferably 3.7 times. If it is 3.5 times or more, the degree of orientation in the transverse direction is not too weak, and the mechanical properties and thickness unevenness are improved. The upper limit of the stretching ratio in the transverse stretching direction is preferably 5 times, more preferably 4.5 times, and particularly preferably 4.0 times. 5.0 times or less In this range, the effect of improving the mechanical strength and thickness unevenness is maximized (saturated).
[0117] [Heat setting process] The lower limit of the heat setting temperature in the heat setting step is preferably 195° C., more preferably 200° C. If the temperature is 195° C. or higher, the heat shrinkage rate of the film is small, and even after boiling treatment, the inorganic thin film layer is less likely to be damaged, improving the gas barrier property. The upper limit of the heat setting temperature is preferably 220° C., and if the temperature is 220° C. or lower, the base film layer does not melt and is less likely to become brittle.
[0118] [Thermal relaxation section process] The lower limit of the relaxation rate in the heat relaxation section is preferably 0.5%. If it is 0.5% or more, breakage may be less likely to occur during heat setting. The upper limit of the relaxation rate is preferably 10%. If it is 10% or less, shrinkage in the longitudinal direction during heat setting is reduced, resulting in less distortion of the molecular orientation at the film edge, and improved straight tearability. In addition, sagging of the film is less likely to occur, and thickness unevenness is less likely to occur.
[0119] [Cooling process] In the cooling step after the relaxation in the heat relaxing section, the temperature of the surface of the edge of the polyester film is preferably set to 80° C. or lower. If the temperature of the film ends after passing through the cooling process exceeds 80°C, the ends will be stretched by the tension applied when the film is wound up, resulting in a high thermal shrinkage rate in the longitudinal direction of the ends, and the distribution of thermal shrinkage rate in the width direction of the roll will be non-uniform. When such a roll is heated and transported for deposition processing, etc., streaky wrinkles will occur, and the physical properties of the final gas barrier film may be non-uniform in the width direction.
[0120] In the cooling process, methods for keeping the surface temperature of the film ends at 80°C or below can include adjusting the temperature and air volume in the cooling process, providing a shielding plate at the center in the width direction of the cooling zone to selectively cool the ends, or blowing cold air locally against the ends of the film.
[0121] In order to ensure sufficient barrier properties and lamination strength, the intermediate layer film of the present invention may be provided with a coating layer (Y), an inorganic thin film layer (C), and a protective layer (b) in the same manner as the substrate film. The coating layer (Y) may have the composition, adhesion amount, and method for forming the coating layer described above for the coating layer (X). The inorganic thin film layer (C) may have the composition, thickness, and method for forming the inorganic thin film layer described above for the inorganic thin film layer (A). The protective layer (b) may have the composition, adhesion amount, and method for forming the protective layer described above for the protective layer (a).
[0122] [Heat sealable resin layer] The laminate of the present invention has a heat-sealable resin layer containing polyester as a component, and when it is desired to further improve the barrier performance, an inorganic thin film layer (B) can be provided on the non-sealable surface of the heat-sealable resin layer, and a protective layer (c) can be provided on the inorganic thin film layer (B). In order to satisfy a predetermined heat-seal strength, the sealing surface (the surface opposite to the non-sealable surface) of the heat-sealable resin layer must be provided on one of the outermost layers in the laminate. The composition, thickness, and method of forming the inorganic thin film layer described above for the inorganic thin film layer (A) can be applied to the inorganic thin film layer (B). The composition, adhesion amount, and method of forming the protective layer described above for the protective layer (a) can be applied to the protective layer (c).
[0123] The layer structure of the heat-sealable resin layer of the present invention is preferably a two-layer structure including a heat-sealable layer constituting the sealing surface and a heat-resistant layer. The heat-resistant layer is disposed on the non-sealable surface side of the heat-sealable resin layer. The constituent requirements for each layer will be described later, but in the case of a structure including a heat-sealable layer and a heat-resistant layer, the layer having the highest ethylene terephthalate content is the heat-resistant layer. The layer structure of the laminate of the present invention is more preferably a three-layer structure including, in order from the outermost layer (sealable surface side) of either one, a heat-sealable layer / heat-resistant layer / inorganic thin film layer (B).
[0124] The heat sealable resin layer of the present invention may also have a protective layer on the outermost layer on the side opposite to the heat seal layer (non-sealed side). In this case, a structure in which four layers are laminated in the order of heat seal layer / heat-resistant layer / inorganic thin film layer (B) / protective layer (c) is preferable. By providing a protective layer, not only is the gas barrier property improved, but the laminate strength when laminated with other materials is improved, and the occurrence of cracks due to rubbing or bending can be suppressed, and other advantages are obtained.
[0125] The thickness of the heat-sealable resin layer is not particularly limited, but is preferably 3 μm or more and 200 μm or less. If the thickness of the heat-sealable resin layer is thinner than 3 μm, it is not preferable because there is a risk of insufficient heat seal strength and processing such as printing becoming difficult. In addition, the thickness of the laminate may be thicker than 200 μm, but it is not preferable because the weight of the laminate used increases and the cost increases. The thickness of the laminate is more preferably 5 μm or more and 160 μm or less, and even more preferably 7 μm or more and 120 μm or less. The layer ratio of the heat seal layer to the entire heat sealable resin layer is preferably 20% or more and 80% or less. If the layer ratio of the heat seal layer is less than 20%, the heat seal strength of the heat sealable resin layer decreases, which is not preferable. If the layer ratio of the heat seal layer is higher than 80%, the heat sealability of the heat sealable resin layer is improved, but the heat resistance decreases, which is not preferable. The layer ratio of the heat seal layer is more preferably 30% or more and 70% or less.
[0126] The layer ratio of the heat-resistant layer is preferably 20% or more and 80% or less. If the layer ratio of the heat-resistant layer is less than 20%, the heat resistance of the film is reduced, which is not preferable. If the layer ratio of the heat-resistant layer is higher than 80%, the ratio of the heat seal layer of the laminate is reduced accordingly, which is not preferable because the heat sealability is sacrificed. The layer ratio of the heat-resistant layer is more preferably 30% or more and 70% or less.
[0127] In addition, the outermost layer (including the heat seal layer) of the laminate of the present invention may be provided with a layer that has been subjected to corona treatment, coating treatment, flame treatment, or the like in order to improve the printability and slipperiness of the film surface, and may be provided as desired within the scope of the present invention. In the following description, layers made of polyester resins, such as the heat seal layer and the heat-resistant layer, are collectively referred to as "polyester resin layer" to distinguish them from inorganic thin film layers and protective layers.
[0128] (Characteristics of heat seal layer) The upper limit of the haze per thickness of the heat seal layer in the present invention is preferably 0.50% / μm, more preferably 0.40% / μm, and even more preferably 0.30% / μm. When printing is performed on a base film layer having a haze of 0.50% / μm or less, the quality of the printed characters and images is improved. The heat seal strength of the laminated body of the present invention is preferably 8N / 15mm or more and 30N / 15mm or less when the heat seal layers are heat sealed at a temperature of 200°C, a seal bar pressure of 0.2MPa, and a sealing time of 4 seconds. If the heat seal strength is less than 8N / 15mm, the sealed portion is easily peeled off, making it impossible to use the laminated body as a packaging bag. The heat seal strength is preferably 9N / 15mm or more, and more preferably 10N / 15mm or more. Although a high heat seal strength is preferable, the upper limit currently obtainable is about 30N / 15mm.
[0129] The laminated laminate of the present invention preferably has a hot water heat shrinkage rate in both the width direction and the length direction when treated in hot water at 98°C for 3 seconds of -5% or more and 5% or less. If the shrinkage rate exceeds 5%, not only will the deformation of the bag become large and the bag will not be able to maintain its original shape when the bag made using the laminate is subjected to a heat treatment such as a retort treatment, but also cracks will occur in the layer made of inorganic substances, resulting in a decrease in gas barrier properties, which is undesirable. The hot water heat shrinkage rate is more preferably 4% or less, and even more preferably 3% or less. On the other hand, if the hot water heat shrinkage rate is less than -5%, this means that the laminate stretches, and it is undesirable because the bag will be less able to maintain its original shape as in the case of a high shrinkage rate. The hot water heat shrinkage rate of the laminate is more preferably -4% or more and 4% or less, and even more preferably -3% or more and 3% or less.
[0130] The laminate of the present invention preferably has a folding angle of 20 degrees or more and 70 degrees or less, as measured by the method described below. If the folding angle exceeds 70 degrees, it is difficult to make a crease when the laminate is made into a bag, which is undesirable because it results in a poor appearance. On the other hand, the smaller the folding angle, the more preferable it is, but the range that can be covered by the present invention is 20 degrees as the lower limit, and even if the folding angle is 25 degrees or more, it can be said that it is practically preferable. The upper limit of the folding angle is more preferably 65 degrees, and even more preferably 60 degrees.
[0131] (Raw materials for polyester resin layer) The raw material type of the polyester-based resin layer constituting the laminate of the present invention is one that contains ethylene terephthalate units as a main component. Here, "containing ethylene terephthalate units as a main component" means that the content of ethylene terephthalate units is 50 mol % or more when the total amount of all components is 100 mol %. In addition, it is preferable that the polyester used in the polyester-based resin layer of the present invention contains at least one component other than ethylene terephthalate. This is because the presence of components other than ethylene terephthalate improves the heat seal strength of the heat seal layer. In the heat-resistant layer, it is preferable that the amount of components other than ethylene terephthalate is small, but by containing components other than ethylene terephthalate, the difference in shrinkage rate with the heat seal layer can be reduced, which leads to less curling of the laminate. The content of each component differs between the heat-seal layer and the heat-resistant layer, and will be described later. Examples of dicarboxylic acid monomers that can be components other than terephthalic acid that constitute ethylene terephthalate include aromatic dicarboxylic acids such as isophthalic acid, 1,4-cyclohexanedicarboxylic acid, 2,6-naphthalenedicarboxylic acid, and orthophthalic acid, aliphatic dicarboxylic acids such as adipic acid, azelaic acid, sebacic acid, and decanedicarboxylic acid, and alicyclic dicarboxylic acids. However, it is preferable that trivalent or higher polyvalent carboxylic acids (for example, trimellitic acid, pyromellitic acid, and anhydrides thereof) are not contained in the polyester.
[0132] Examples of diol monomers that can be components other than ethylene glycol constituting ethylene terephthalate include long-chain diols such as neopentyl glycol, 1,4-cyclohexanedimethanol, diethylene glycol, 2,2-diethyl-1,3-propanediol, 2-n-butyl-2-ethyl-1,3-propanediol, 2,2-isopropyl-1,3-propanediol, 2,2-di-n-butyl-1,3-propanediol, hexanediol, and 1,4-butanediol, aliphatic diols such as hexanediol, and aromatic diols such as bisphenol A. However, it is preferable that the polyester does not contain a diol having 8 or more carbon atoms (e.g., octanediol, etc.) or a polyhydric alcohol having a valence of 3 or more (e.g., trimethylolpropane, trimethylolethane, glycerin, diglycerin, etc.).
[0133] Furthermore, the polyester may contain a polyester elastomer containing ε-caprolactone, tetramethylene glycol, etc. The polyester elastomer has the effect of lowering the melting point of the polyester resin layer, and therefore can be suitably used in particular for the heat seal layer.
[0134] Among these, it is preferable to use one or more of neopentyl glycol, 1,4-cyclohexanedimethanol, 1,4-butanediol, and diethylene glycol, since this facilitates achieving a heat seal strength of 8 N / 15 mm or more between the heat seal layers. It is more preferable to use one or more of neopentyl glycol and 1,4-cyclohexanedimethanol, and it is particularly preferable to use neopentyl glycol.
[0135] In the polyester resin layer constituting the laminate of the present invention, various additives such as waxes, antioxidants, antistatic agents, crystal nucleating agents, viscosity reducing agents, heat stabilizers, coloring pigments, coloring inhibitors, ultraviolet absorbers, etc. can be added as necessary. In addition, it is preferable to add fine particles as a lubricant to improve the slipperiness of the film to at least the outermost layer of the film. As the fine particles, any particles can be selected. For example, inorganic fine particles can include silica, alumina, titanium dioxide, calcium carbonate, kaolin, barium sulfate, etc., and organic fine particles can include acrylic resin particles, melamine resin particles, silicone resin particles, crosslinked polystyrene particles, etc. The average particle size of the fine particles can be appropriately selected as necessary within the range of 0.05 to 3.0 μm when measured with a Coulter counter.
[0136] As a method of blending particles into the polyester resin layer constituting the laminate of the present invention, for example, they can be added at any stage of manufacturing the polyester resin, but it is preferable to add them as a slurry dispersed in ethylene glycol or the like at the stage of esterification or after the completion of the transesterification reaction and before the start of the polycondensation reaction, and proceed with the polycondensation reaction. In addition, there is also a method of blending a slurry of particles dispersed in ethylene glycol, water, or other solvents with a polyester resin raw material using a vented kneading extruder, or a method of blending dried particles with a polyester resin raw material using a kneading extruder. Preferred components contained in the heat seal layer and the heat resistant layer will now be described.
[0137] The polyester used in the heat seal layer constituting the laminate of the present invention preferably has a content of dicarboxylic acid monomers and / or diol monomers other than terephthalic acid and ethylene glycol constituting ethylene terephthalate of 30 mol% or more, more preferably 32 mol% or more, and particularly preferably 34 mol% or more. The upper limit of the content of monomers other than ethylene terephthalate is 50 mol%. If the content of monomers other than ethylene terephthalate contained in the heat seal layer is less than 30 mol%, even if the molten resin is rapidly cooled and solidified after extrusion from the die, it will crystallize in the subsequent stretching and heat setting steps, making it difficult to achieve a heat seal strength of 8 N / 15 mm or more, which is not preferable.
[0138] On the other hand, if the content of the monomer other than the ethylene terephthalate in the heat seal layer is 50 mol % or more, the heat seal strength of the film can be increased, but the heat resistance of the heat seal layer is extremely low, so that the periphery of the sealed portion is blocked during heat sealing (a phenomenon in which a wider area than the intended area is sealed due to heat conduction from the heating member), making it difficult to perform proper heat sealing. The content of the monomer other than the ethylene terephthalate is more preferably 48 mol % or less, and particularly preferably 46 mol % or less.
[0139] The polyester used in the heat-resistant layer that can constitute the laminate of the present invention preferably has a content of dicarboxylic acid monomers and / or diol monomers other than terephthalic acid and ethylene glycol that constitute ethylene terephthalate of 9 mol% or more, more preferably 10 mol% or more, and particularly preferably 11 mol% or more. The upper limit of the content of the monomer other than ethylene terephthalate is 20 mol%. If the content of the monomer other than ethylene terephthalate contained in the heat-resistant layer is lower than 9 mol%, the difference in heat shrinkage rate with the heat seal layer becomes large, and the curl of the laminate becomes large, which is not preferable. If the difference in the content of the monomer other than ethylene terephthalate contained in the heat-resistant layer and the heat seal layer becomes large, the difference in heat shrinkage rate between each layer during heat setting becomes large, and even if cooling after heat setting is strengthened, the shrinkage toward the heat seal layer side becomes large, and the curl becomes large.
[0140] On the other hand, if the content of the monomer other than the ethylene terephthalate in the heat-resistant layer is 20 mol% or more, the heat resistance of the sealant is reduced, such as holes being formed due to the heat applied during heat sealing, which is not preferable. The content of the monomer other than the ethylene terephthalate is more preferably 19 mol% or less, and particularly preferably 18% or less. In addition, the content of the monomer other than the ethylene terephthalate for controlling curl is more preferably 20 mol% or more and 35 mol% or less, and even more preferably 21 mol% or more and 34 mol% or less, in addition to the amount of each layer alone.
[0141] (Laminate manufacturing conditions) The polyester-based resin layer (hereinafter, sometimes simply referred to as a film) constituting the laminate of the present invention can be obtained by melt-extruding the polyester raw material described in 3.1. "Raw material type of polyester-based resin layer" above with an extruder to form an unstretched laminated film, and stretching it by a predetermined method described below. When the film includes a heat seal layer and a heat-resistant layer, or other layers, the timing of laminating each layer may be either before or after stretching. When laminating before stretching, it is preferable to adopt a method in which the resins that are the raw materials for each layer are melt-extruded by separate extruders and joined using a feed block or the like in the middle of the resin flow path. When laminating after stretching, it is preferable to adopt a lamination method in which films formed separately are bonded together with an adhesive, or an extrusion lamination method in which a molten polyester resin is poured on the surface layer of a single or laminated film to laminate it. Among these, the method in which each layer is laminated before stretching is preferable.
[0142] As described above, the polyester resin can be obtained by polycondensation of a dicarboxylic acid component and a diol component selected in type and amount so as to contain an appropriate amount of a monomer that can be a component other than ethylene terephthalate. In addition, two or more kinds of chip-like polyesters can be mixed and used as a raw material for the polyester-based resin layer. When the raw resin is melt-extruded, it is preferable to dry the polyester raw material of each layer using a dryer such as a hopper dryer or a paddle dryer, or a vacuum dryer. After drying the polyester raw material of each layer in this way, it is melted at a temperature of 200 to 300 ° C. using an extruder and extruded as a laminated film. For extrusion, any existing method such as a T-die method or a tubular method can be adopted. Thereafter, the film melted by extrusion is quenched to obtain an unstretched film. As a method for quenching the molten resin, a method in which the molten resin is cast from a die onto a rotating drum and quenched and solidified to obtain a substantially unoriented resin sheet can be suitably adopted.
[0143] The film may be produced by any of the following methods: no stretching, uniaxial stretching (stretching in at least one of the longitudinal (length) direction and transverse (width) direction), and biaxial stretching. From the viewpoint of the mechanical strength and productivity of the laminate of the present invention, uniaxial stretching is preferable, and biaxial stretching is more preferable. In the following, a sequential biaxial stretching method by longitudinal stretching-transverse stretching in which longitudinal stretching is carried out first and transverse stretching is then carried out will be described, but the order may be reversed (transverse stretching-longitudinal stretching) since only the main orientation direction is changed. A simultaneous biaxial stretching method may also be used.
[0144] For longitudinal stretching, the unstretched film may be introduced into a longitudinal stretching machine in which a plurality of roll groups are arranged in series. For longitudinal stretching, it is preferable to preheat the film with a preheating roll until the film temperature reaches 65°C to 90°C. If the film temperature is lower than 65°C, the film is difficult to stretch when stretched in the longitudinal direction and is prone to breakage, which is not preferable. If the film temperature is higher than 90°C, the film is prone to sticking to the roll, and the film is prone to wrapping around the roll and the roll is prone to becoming dirty during continuous production, which is not preferable. When the film temperature reaches 65°C to 90°C, the film is stretched longitudinally. The longitudinal stretching ratio should be between 1 and 5 times. Since 1 times means that no longitudinal stretching has been performed, the longitudinal stretching ratio should be 1 to obtain a uniaxially stretched film, and the longitudinal stretching ratio should be 1.1 times or more to obtain a biaxially stretched film. The upper limit of the longitudinal stretching ratio may be any number of times, but if the longitudinal stretching ratio is too high, it becomes difficult to stretch transversely and breaks are likely to occur, so it is preferably 5 times or less.
[0145] In addition, by relaxing the film in the longitudinal direction after the longitudinal stretching (relaxation in the longitudinal direction), the shrinkage rate in the longitudinal direction of the film caused by the longitudinal stretching can be reduced. Furthermore, by relaxing in the longitudinal direction, the bowing phenomenon (distortion) occurring in the tenter can be reduced. This is because in the later process of transverse stretching and final heat treatment, both ends in the width direction of the film are heated while being held, and only the center part of the film shrinks in the longitudinal direction. The relaxation rate in the longitudinal direction is preferably 0% or more and 70% or less (relaxation rate of 0% means that relaxation is not performed). The upper limit of the relaxation rate in the longitudinal direction is determined by the raw material used and the longitudinal stretching conditions, so relaxation cannot be performed beyond this limit. In the polyester-based sealant of the present invention, the relaxation rate in the longitudinal direction is an upper limit of 70%. Relaxation in the longitudinal direction can be performed by heating the film after the longitudinal stretching at a temperature of 65°C to 100°C or less and adjusting the speed difference of the rolls. Any of rolls, near infrared rays, far infrared rays, hot air heaters, etc. can be used as the heating means. In addition, the relaxation in the longitudinal direction does not have to be performed immediately after the longitudinal stretching, but can be performed, for example, during the transverse stretching (including the preheating zone) or the final heat treatment by narrowing the clip interval in the longitudinal direction (in this case, both ends in the width direction of the film are also relaxed in the longitudinal direction, so that the bowing distortion is reduced), and can be performed at any timing. After the relaxation in the longitudinal direction (longitudinal stretching if relaxation is not performed), it is preferable to cool the film once, and it is preferable to cool it with a cooling roll having a surface temperature of 20 to 40°C.
[0146] After the longitudinal stretching, the film is preferably transversely stretched at a stretch ratio of about 3 to 5 times at 65° C. to 110° C. in a tenter while both ends in the width direction of the film are held by clips. Before the transverse stretching, it is preferable to preheat the film, and the preheating is preferably performed until the film surface temperature reaches 75° C. to 120° C.
[0147] After the transverse stretching, it is preferable to pass the film through an intermediate zone where no active heating operation is performed. Since the temperature in the next final heat treatment zone is higher than that in the transverse stretching zone of the tenter, if an intermediate zone is not provided, the heat (hot air itself or radiant heat) from the final heat treatment zone will flow into the transverse stretching process. In this case, the temperature in the transverse stretching zone is not stable, and not only does the film thickness precision deteriorate, but physical properties such as heat seal strength and shrinkage rate also vary. Therefore, it is preferable to pass the film after the transverse stretching through the intermediate zone for a predetermined time and then perform the final heat treatment. In this intermediate zone, it is important to block the accompanying flow caused by the running of the film and the hot air from the transverse stretching zone and the final heat treatment zone so that when a strip of paper is hung down without the film passing through it, the paper hangs down almost completely in the vertical direction. The passing time through the intermediate zone is sufficient for about 1 to 5 seconds. If it is shorter than 1 second, the length of the intermediate zone is insufficient and the heat blocking effect is insufficient. On the other hand, it is preferable for the intermediate zone to be long, but if it is too long the equipment will become large, so about 5 seconds is sufficient.
[0148] After passing through the intermediate zone, it is preferable to perform heat treatment at a temperature between the transverse stretching temperature and 250°C in the final heat treatment zone. If the heat treatment temperature is not equal to or higher than the transverse stretching temperature, the heat treatment will not be effective. In this case, the 80°C hot water shrinkage rate of the film will be higher than 5%, which is not preferable. The higher the heat treatment temperature, the lower the film shrinkage rate, but if the heat treatment temperature is higher than 250°C, the haze of the film will be higher than 15% or the film will melt during the final heat treatment process and fall into the tenter, which is not preferable.
[0149] During the final heat treatment, the shrinkage rate in the width direction can be reduced by shortening the distance between the clips of the tenter by any ratio (relaxation in the width direction). Therefore, in the final heat treatment, it is preferable to perform relaxation in the width direction in the range of 0% to 10% (a relaxation rate of 0% means that no relaxation is performed). Although the higher the relaxation rate in the width direction, the lower the shrinkage rate in the width direction, the upper limit of the relaxation rate (shrinkage rate in the width direction of the film immediately after transverse stretching) is determined by the raw material used, the stretching conditions in the width direction, and the heat treatment temperature, so relaxation cannot be performed beyond this limit. In the polyester sealant of the present invention, the relaxation rate in the width direction is an upper limit of 10%.
[0150] In addition, the time for passing through the final heat treatment zone is preferably 2 to 20 seconds. If the time for passing through is less than 2 seconds, the film passes through the heat treatment zone before the surface temperature of the film reaches the set temperature, making the heat treatment meaningless. The longer the time for passing through, the more effective the heat treatment becomes, so a time of 2 seconds or more is preferable, and a time of 5 seconds or more is even more preferable. However, if the time for passing through is increased, the equipment will become larger, so for practical purposes, a time of 20 seconds or less is sufficient.
[0151] After passing through the final heat treatment, the film is preferably cooled in the cooling zone with cooling air at 10°C to 30°C. At this time, it is preferable to improve the cooling efficiency by lowering the temperature of the cooling air or increasing the wind speed so that the actual temperature of the film at the tenter outlet is lower than the glass transition temperature of either the heat seal layer or the heat resistant layer, whichever is lower. The actual temperature refers to the film surface temperature measured with a non-contact radiation thermometer. If the actual temperature of the film at the tenter outlet exceeds the glass transition temperature, the film will thermally shrink when both ends of the film held by the clips are released. At this time, the film curls toward the heat seal layer, which has a large thermal shrinkage rate, which is undesirable as it reduces the radius of curvature.
[0152] The time for passing through the cooling zone is preferably 2 to 20 seconds. If the time is 2 seconds or less, the film passes through the cooling zone before the surface temperature of the film reaches the glass transition temperature, resulting in a small radius of curvature. The longer the time for passing through, the greater the cooling effect, so a time of 2 seconds or more is preferable, and a time of 5 seconds or more is even more preferable. However, if the time for passing through is increased, the equipment will become larger, so for practical purposes, a time of 20 seconds or less is sufficient. After that, the film is wound up while cutting and removing both ends to obtain a film roll.
[0153] [Adhesive layer] The adhesive layer used in the present invention can be a general-purpose adhesive for lamination. For example, (non-)solvent type, water-based type, or hot melt type adhesives mainly composed of poly(ester)urethane, polyester, polyamide, epoxy, poly(meth)acrylic, polyethyleneimine, ethylene-(meth)acrylic acid, polyvinyl acetate, (modified) polyolefin, polybutadiene, wax, or casein can be used. Among these, urethane or polyester types are preferred in consideration of the moisture and heat resistance that can withstand retort treatment and the flexibility that can follow the dimensional changes of each substrate. The adhesive layer can be applied by, for example, direct gravure coating, reverse gravure coating, kiss coating, die coating, roll coating, dip coating, knife coating, spray coating, fountain coating, or other methods, and the coating amount after drying is 1 to 8 g / m in order to exhibit sufficient adhesion after retort. 2 More preferably, the thickness is 2 to 7 g / m 2 , and more preferably 3 to 6 g / m 2 The coating amount is 1g / m 2 If it is less than 8g / m, it becomes difficult to bond the entire surface, and the adhesive strength decreases. 2 If the temperature exceeds this range, it will take a long time for the film to completely cure, unreacted material will be likely to remain, and adhesive strength will decrease.
[0154] Furthermore, in the laminate of the present invention, at least one printed layer or other plastic substrate may be laminated between or on the outside of the inorganic thin film layer or substrate film layer and the heat-sealable resin layer, although from the viewpoint of mono-materialization, the laminate is limited to polyester-based materials.
[0155] As the printing ink for forming the printing layer, water-based and solvent-based resin-containing printing inks can be preferably used. Examples of the resin used in the printing ink include acrylic resins, urethane resins, polyester resins, vinyl chloride resins, vinyl acetate copolymer resins, and mixtures thereof. The printing ink may contain known additives such as antistatic agents, light blocking agents, ultraviolet absorbers, plasticizers, lubricants, fillers, colorants, stabilizers, lubricants, defoamers, crosslinking agents, anti-blocking agents, and antioxidants. The printing method for providing the printing layer is not particularly limited, and known printing methods such as offset printing, gravure printing, and screen printing can be used. To dry the solvent after printing, known drying methods such as hot air drying, hot roll drying, and infrared drying can be used.
[0156] [Characteristics of laminated bodies] The laminate of the present invention has an oxygen permeability of 5 ml / m under conditions of 23°C x 65% RH. 2 In order to achieve good gas barrier properties, it is preferable that the gas barrier strength is 4 ml / m or less. 2 ·d·MPa or less, more preferably 3ml / m 2 ·d·MPa or less. Oxygen permeability is 5ml / m 2 If the oxygen permeability exceeds 0.5 ml / m, it becomes difficult to use the material in applications that require high gas barrier properties, such as replacing aluminum foil. 2 If the oxygen permeability is less than 0.5 ml / m, the barrier performance is excellent, but the residual solvent is less likely to permeate to the outside of the bag, and the amount of the solvent that migrates to the contents is likely to increase. 2 ·d·MPa or more.
[0157] The laminate of the present invention has a water vapor permeability of 1.0 g / m under conditions of 40°C x 90% RH. 2 In order to achieve good gas barrier properties, it is preferable that the thickness of the barrier layer is 0.75 g / m or less. 2 d or less, preferably 0.5 g / m 2 ·d or less. The water vapor permeability is 1.0 g / m 2 If the water vapor permeability exceeds 0.1 g / m, it becomes difficult to meet the requirements for applications that require high gas barrier properties, such as aluminum foil replacement. 2 If the water vapor permeability is less than 0.1 g / m, the barrier performance is excellent, but the residual solvent is less likely to permeate to the outside of the bag, and the amount of the solvent that migrates to the contents may increase relatively, which is not preferable. 2 ·d or more.
[0158] The laminate of the present invention preferably has a puncture strength measured in accordance with JIS Z1707 of at least 10 N, more preferably at least 12 N, and even more preferably at least 14 N. If the puncture strength is less than 10 N, there is a risk that when used as a bag, the application of an external load will cause a hole to form, causing the contents to leak out.
[0159] The laminate of the present invention preferably has a haze of 20% or less, more preferably 18% or less, and even more preferably 16% or less, measured in accordance with JIS K 7136. If the haze is 20% or more, the transparency is poor when used as a bag, which is undesirable in terms of visibility of contents from the viewpoint of safety and appearance after printing.
[0160] The heat seal strength of the laminated body of the present invention is preferably 8N / 15mm or more and 30N / 15mm or less when the heat seal layers are heat sealed at a temperature of 200°C, a seal bar pressure of 0.2MPa, and a sealing time of 4 seconds. If the heat seal strength is less than 8N / 15mm, the sealed portion is easily peeled off, making it impossible to use the laminated body as a packaging bag. The heat seal strength is preferably 9N / 15mm or more, and more preferably 10N / 15mm or more. Although a high heat seal strength is preferable, the upper limit currently obtainable is about 30N / 15mm. EXAMPLES
[0161] The present invention will now be described in more detail with reference to examples, but the present invention is not limited to the following examples. Various evaluations were carried out by the following measurement methods.
[0162] (1) Thickness of various films The measurement was performed using a dial gauge in accordance with JIS K7130-1999 Method A.
[0163] (2) Composition and thickness of inorganic thin film layer The film thickness composition of the laminated films (after thin film lamination) obtained in the examples and comparative examples was measured using a fluorescent X-ray analyzer ("ZSX100e" manufactured by Rigaku Corporation) based on a calibration curve prepared in advance. The excitation X-ray tube conditions were 50 kV and 70 mA.
[0164] (3) Amount of protective layer attached In each Example and Comparative Example, each laminate film obtained at the stage of laminating a protective layer onto a base film was used as a sample, and a test piece of 100 mm x 100 mm was cut out from this sample, and the protective layer was wiped off with 1-methoxy-2-propanol or dimethylformamide. The amount of adhesion was calculated from the change in mass of the film before and after wiping.
[0165] [Preparation of laminated body] (4) Preparation of laminate for evaluation The substrate film, intermediate layer film, and heat seal resin described in the examples and comparative examples were bonded by dry lamination using a urethane-based two-component curing adhesive (Mitsui Chemicals' "Takelac (registered trademark) A525S" and "Takenate (registered trademark) A50" mixed in a ratio of 13.5:1 (mass ratio)) and aged at 40°C for 4 days to obtain a laminate gas barrier laminate for evaluation (hereinafter sometimes referred to as "laminate laminate A"). The thickness of the adhesive layer formed with the urethane-based two-component curing adhesive after drying was about 4 μm in each case.
[0166] (5) Evaluation method for oxygen permeability The laminate produced in (4) above was subjected to oxygen permeability measurement in accordance with JIS-K7126 Method B under an atmosphere of temperature 23° C. and humidity 65% RH using an oxygen permeability measurement device ("OX-TRAN (registered trademark) 2 / 22" manufactured by MOCON Co., Ltd.) The oxygen permeability measurement was performed in the direction in which oxygen permeates from the substrate film side of the laminate to the heat sealable resin layer side.
[0167] (6) Method for evaluating water vapor permeability The laminated body prepared in (4) above was subjected to measurement of water vapor permeability in an atmosphere of temperature 40° C. and humidity 90% RH using a water vapor permeability measuring device ("PERMATRAN-W 3 / 33MG" manufactured by MOCON) in accordance with JIS-K7129 Method B. The water vapor permeability was measured in the direction in which water vapor permeates from the heat sealable resin layer side of the laminated body toward the base film side.
[0168] (7) Evaluation method for heat seal strength The laminated body prepared in (4) above was subjected to heat seal strength measurement in accordance with JIS Z1707. The specific procedure is as follows. The heat seal surfaces of the samples were bonded together using a heat sealer. The heat seal conditions were upper bar temperature 200°C, lower bar temperature 30°C, pressure 0.2 MPa, and time 4 seconds. The bonded sample was cut out to have a seal width of 15 mm. The peel strength was measured using a universal tensile tester "DSS-100" (manufactured by Shimadzu Corporation) at a tensile speed of 200 mm / min. The peel strength is expressed as the strength per 15 mm (N / 15 mm).
[0169] (9) Evaluation method for puncture strength The laminated body prepared in (4) above was sampled into a 5 cm square, and the puncture strength of the film was measured in accordance with JIS Z1707 using a digital force gauge "ZTS-500N", a motorized test stand "MX2-500N", and a puncture jig "TKS-250N" manufactured by IMADA CORP.
[0170] (10) Haze of laminated body The haze of the laminates obtained in the examples and comparative examples was measured in accordance with JIS K7136 using a haze meter NDH-2000 (manufactured by Nippon Denshoku Industries Co., Ltd.). (11) Evaluation criteria for mono-materialization Regarding the laminate produced in (4) above, as a criterion for evaluating whether it was a mono-material, those in which the thickness of the polyester-based material relative to the total thickness was 90% or more were rated as ◯ (mono-material). (12) Visibility and range suitability Regarding the laminates produced in (4) above, those with a haze of 20% or less and not using aluminum foil were rated as ◯, those with a haze of 20% or more and not using aluminum foil were rated as △, and those using aluminum foil were rated as ×.
[0171] The coating fluids used in Examples 1 to 7 and Comparative Examples 1 to 7 are described in detail below.
[0172] [Carbodiimide crosslinking agent (A)] As a carbodiimide-based crosslinking agent, a commercially available product "Carbodilite (registered trademark) SV-02" (solid content 40%) manufactured by Nisshinbo Corporation was prepared. [Resin having oxazoline groups (B)] As a resin having an oxazoline group, a commercially available water-soluble acrylate containing an oxazoline group ("Epocross (registered trademark) WS-300" manufactured by Nippon Shokubai Co., Ltd.; solid content 10%) was prepared. The amount of oxazoline groups in this resin was 7.7 mmol / g.
[0173] [Acrylic resin (C)] As the acrylic resin, a 25% by mass emulsion of a commercially available acrylic acid ester copolymer ("Mowinyl (registered trademark) 7980" manufactured by Nichigo Mowinyl Co., Ltd.) was prepared. The acid value (theoretical value) of this acrylic resin was 4 mgKOH / g.
[0174] [Urethane resin (D)] As the urethane resin, a commercially available polyester urethane resin dispersion ("Takelac (registered trademark) W605" manufactured by Mitsui Chemicals, Inc.; solid content 30%) was prepared. The acid value of this urethane resin was 25 mgKOH / g, and the glass transition temperature (Tg) measured by DSC was 100°C. The ratio of aromatic or araliphatic diisocyanate to the entire polyisocyanate component measured by 1H-NMR was 55 mol%. [Silane coupling agent (E)] As a silane coupling agent, a commercially available product "KBM903 (registered trademark)" (solid content 100%) manufactured by Shin-Etsu Chemical Co., Ltd. was prepared. When used, it was diluted with water to give a 2% aqueous solution.
[0175] [Urethane resin (F)] In a four-neck flask equipped with a stirrer, a Dimroth condenser, a nitrogen inlet tube, a silica gel drying tube, and a thermometer, 143.95 parts by mass of metaxylylene diisocyanate, 25.09 parts by mass of 4,4'-methylenebis(cyclohexyl isocyanate), 28.61 parts by mass of ethylene glycol, 5.50 parts by mass of trimethylolpropane, 12.37 parts by mass of dimethylolpropionic acid, and 120.97 parts by mass of methyl ethyl ketone as a solvent were mixed, and the mixture was stirred at 70°C under a nitrogen atmosphere, and it was confirmed that the reaction solution reached a predetermined amine equivalent. Next, the reaction solution was cooled to 35°C, and then 9.14 parts by mass of triethylamine was added to obtain a polyurethane prepolymer solution. Next, 794.97 parts by mass of water was added to a reaction vessel equipped with a homodisperser capable of high-speed stirring, and the temperature was adjusted to 15°C. While stirring and mixing at 2000 min-1, a polyurethane prepolymer solution was added to disperse the mixture in water, and an amine aqueous solution obtained by mixing 22.96 parts by mass of 2-[(2-aminoethyl)amino]ethanol and 91.84 parts by mass of water was added, and then an amine aqueous solution obtained by mixing 2.38 parts by mass of N-2-(aminoethyl)-3-aminopropyltrimethoxysilane (trade name; KBM-603, manufactured by Shin-Etsu Chemical Co., Ltd.) and 9.50 parts by mass of water was added to carry out a chain extension reaction. Thereafter, a polyurethane dispersion (E) having a solid content of 25% by mass and an average particle size of 70 nm was obtained by removing a part of the methyl ethyl ketone and water under reduced pressure. The Si content (calculated by the charge) of the obtained polyurethane dispersion (D-1) was 1200 mg / 1 kg, and the metaxylylene group content (calculated by the charge) was 32% by mass.
[0176] [Polyester resin (G)] As the polyester component, polyester polyol (DIC Corporation's "DF-COAT GEC-004C": solid content 30%) was used.
[0177] [Polyisocyanate crosslinker (H)] As the polyisocyanate component, a trimethylolpropane adduct of metaxylylene diisocyanate ("Takenate D-110N" manufactured by Mitsui Chemicals, Inc.: solid content 75%) was used.
[0178] [Silane coupling agents (I)] As the silane coupling agent, N-2-(aminoethyl)-3-aminopropyltrimethoxysilane ("KBM-603" manufactured by Shin-Etsu Chemical Co., Ltd.) was used.
[0179] [Coating solution 1 used for coating layer] The materials were mixed in the following mixing ratio to prepare a coating liquid (resin composition for coating layer). Water 54.40% by mass Isopropanol 25.00% by mass Oxazoline group-containing resin (A) 15.00 mass% Acrylic resin (B) 3.60% by mass Urethane resin (C) 2.00% by mass
[0180] [Coating solution 2 used for coating layer] The materials were mixed in the following ratio to prepare a coating liquid (resin composition for coating layer). Water 57.80% by mass Isopropanol 25.00% by mass Carbodiimide crosslinking agent (A) 2.10% by mass Urethane resin (F) 8.00% by mass Silane coupling agent (E) 7.10% by mass
[0181] [Coating solution 3 used for coating protective layer] The following coating materials were mixed to prepare Coating Liquid 3. Here, the mass ratio calculated as the solid content of the urethane resin (E) is as shown in Table 1. Water 22.00% by mass Isopropanol 30.00% by mass Urethane resin (F) 48.00% by mass
[0182] [Coating solution 4 used for coating protective layer] A solution (15% by weight) of silane coupling agent (I) dissolved in acetone and isocyanate (G) were mixed in the following ratio and stirred for 10 minutes using a magnetic stirrer. The resulting mixture was diluted with methyl ethyl ketone, and polyester resin (G) was added to obtain a coating liquid. The mixing ratio is shown below. Polyester resin (G) 4.90% by mass Isocyanate (H) 1.87% by mass Silane coupling agent (I) *Acetone diluted solution 0.85% by mass Methyl ethyl ketone 92.39% by mass
[0183] The methods for producing the laminated films used in the respective Examples and Comparative Examples are described below. The films used in Examples 1 to 8 and Comparative Examples 1 to 7 are shown in Table 2.
[0184] 1. Base film (Preparation of polyester resin recycled from PET bottles) After washing out the remaining beverages and other foreign matter from the PET bottles, the flakes obtained by crushing them were melted in an extruder, and the finer foreign matter was filtered out twice using filters with successively smaller opening sizes, and the third time using a filter with the smallest opening size of 50 μm to obtain recycled polyester raw material. The composition of the obtained resin was terephthalic acid / isophthalic acid / ethylene glycol = 97.0 / 3.0 / / 100 (mol%), and the intrinsic viscosity of the resin was 0.70 dl / g. This was designated Polyester A.
[0185] (Production of base film) Polyester B was a polyethylene terephthalate resin with an intrinsic viscosity of 0.62 dl / g, composed of terephthalic acid / ethylene glycol = 100 / / 100 (mol%), and polyester C was a master batch containing 0.3% amorphous silica with an average particle size of 1.5 μm in polyester B. Each raw material was dried at 125 ° C for 8 hours under a reduced pressure of 33 Pa. They were mixed to A / B / C = 80 / 10 / 10 (weight ratio) and fed into a single-screw extruder. The temperature was set so that the resin temperature was 280 ° C from the extruder to the melt line, filter and T-die. However, the resin temperature was set to 305 ° C for 30 seconds from the start of the compression part of the extruder screw, and then it was set to 280 ° C again.
[0186] The molten material extruded from the T-die was brought into contact with a cooling roll to form an unstretched sheet, which was then stretched 1.41 times in the longitudinal direction by rolls heated to 118°C with different peripheral speeds (MD1), and further stretched 2.92 times in the longitudinal direction by rolls heated to 128°C with different peripheral speeds (MD2). The longitudinally stretched sheet was introduced into a tenter, and the above-mentioned coating liquid 1 was coated on one side of the film by the fountain bar coating method. The sheet was introduced into the tenter while drying, preheated at 121°C, and then stretched 4.3 times laterally at 131°C. The heat setting was then performed at 180°C, no relaxation (0%) for 2.5 seconds (TS1), followed by 231°C, 5% relaxation for 3.0 seconds (TS2), followed by 222°C, no relaxation for 2.5 seconds (TS3). Subsequently, the film was cooled at 120° C. for 6.0 seconds in the same tenter, and finally taken up by a winder to obtain a biaxially oriented polyester film having a thickness of 12 μm.
[0187] In preparing the base film layer described in each of the Examples and Comparative Examples, laminate films were produced in the same manner as above, except that the blending amounts of the resins A, B and C were changed, and evaluations were carried out.
[0188] 2. Interlayer film (Adjustment of PBT resin) 1) Polybutylene terephthalate (PBT) resin: The polybutylene terephthalate resin used in the production of the biaxially oriented polyester film described below was 1100-211XG (CHANG CHUN PLASTICS CO., LTD., intrinsic viscosity 1.28 dl / g). 2) Polyethylene terephthalate (PET) resin: The polyethylene terephthalate resin used in the production of the biaxially oriented polyester film described below was terephthalic acid / ethylene glycol=100 / / 100 (mol %) (manufactured by Toyobo Co., Ltd., intrinsic viscosity 0.62 dl / g).
[0189] (Film manufacturing) Using a single screw extruder, a mixture of 80% by mass of PBT resin and 20% by mass of PET resin was mixed with silica particles with an average particle size of 2.4 μm as inactive particles at a silica concentration of 900 ppm relative to the mixed resin. The mixture was then melted at 290°C, and the melt line was introduced into a 12-element static mixer. This allowed the polyester resin melt to be divided and laminated, resulting in a multi-layer melt made from the same raw materials. The mixture was cast from a T-die at 265°C and adhered to a cooling roll at 15°C by electrostatic adhesion to obtain an unstretched sheet. The film was then stretched 2.9 times in the machine direction at 60°C, and after the machine direction stretching, the adhesive layer resin composition (coating liquid 1) was applied by the fountain bar coating method. The film was then guided to a tenter while drying, and then passed through the tenter to stretch 4.0 times in the machine direction at 90°C. After performing a tension heat treatment at 200°C for 3 seconds and a 9% relaxation treatment for 1 second, the film was cooled at 50°C for 2 seconds. The surface temperature of the film end at this time was 75°C. Next, 9% of the gripped portions on both ends were cut and removed to obtain a laminated film in which a coating layer of 0.030 g / m2 was formed on a polyester film with a thickness of 15 μm. The physical properties of the obtained film are shown in Table 1.
[0190] 3.Heat-sealable resin layer (Preparation of polyester raw materials) [Synthesis Example 1] In a stainless steel autoclave equipped with a stirrer, a thermometer, and a partial reflux condenser, 100 mol % of dimethyl terephthalate (DMT) as a dicarboxylic acid component and 100 mol % of ethylene glycol (EG) as a polyhydric alcohol component were charged so that the molar ratio of ethylene glycol was 2.2 times that of dimethyl terephthalate, and 0.05 mol % (relative to the acid component) of zinc acetate was used as an ester exchange catalyst to carry out an ester exchange reaction while distilling off the produced methanol outside the system. Then, 0.225 mol % (relative to the acid component) of antimony trioxide was added as a polycondensation catalyst, and a polycondensation reaction was carried out at 280°C under reduced pressure of 26.7 Pa to obtain polyester (A) with an intrinsic viscosity of 0.75 dl / g. This polyester (A) is polyethylene terephthalate. The composition of the polyester is shown in Table 1. [Synthesis Example 2] Polyesters (B) to (E) were obtained by changing the monomers in the same manner as in Synthesis Example 1. The composition of each polyester is shown in Table 1. In Table 1, TPA is terephthalic acid, BD is 1,4-butanediol, NPG is neopentyl glycol, CHDM is 1,4-cyclohexanedimethanol, and DEG is diethylene glycol. When producing polyester (E), SiO2 (Silysia 266 manufactured by Fuji Silysia Ltd.) was added as a lubricant at a ratio of 7,000 ppm to the polyester. Each polyester was appropriately formed into chips.
[0191] [Table 1]
[0192] [Film Creation] The raw materials for the heat seal layer were polyester A, polyester B, polyester D, and polyester E mixed in a mass ratio of 10:60:24:6, and the raw materials for the heat resistant layer were polyester A, polyester B, polyester D, and polyester E mixed in a mass ratio of 57:31:6:6. The mixed raw materials for the heat seal layer and the heat resistant layer were fed into separate twin screw extruders, and both were melted at 270°C. The molten resins were joined by a feed block in the middle of the flow path, extruded from a T-die, and cooled on a chill roll set at a surface temperature of 30°C to obtain an unstretched laminated film. The flow path of the molten resin was set so that one side of the laminated film was a heat seal layer and the other side was a heat resistant layer (a two-layer structure of heat seal layer / heat resistant layer), and the extrusion amount was adjusted so that the thickness ratio of the heat seal layer and the heat resistant layer was 50 / 50.
[0193] The unstretched laminated film obtained by cooling and solidifying was introduced into a longitudinal stretching machine with multiple rolls arranged in series, preheated on the preheating roll until the film temperature reached 78°C, and then stretched 4.1 times. The film immediately after longitudinal stretching was passed through a heating furnace set at 100°C with a hot air heater, and a 20% relaxation treatment was performed in the longitudinal direction using the speed difference between the rolls at the entrance and exit of the heating furnace. The longitudinally stretched film was then forcibly cooled by a cooling roll set at a surface temperature of 25°C. The film after the relaxation treatment was introduced into a transverse stretching machine (tenter) and preheated for 5 seconds until the surface temperature reached 105°C, after which it was stretched 4.0 times in the width direction (transverse direction). The film after the transverse stretching was introduced directly into the intermediate zone and passed through in 1.0 second. In the intermediate zone of the tenter, the hot air from the final heat treatment zone and the hot air from the transverse stretching zone were blocked so that when a rectangular piece of paper was hung down without the film passing through, the piece of paper would hang down almost completely in the vertical direction.
[0194] The film then passed through the intermediate zone and was guided to the final heat treatment zone, where it was heat-treated at 190°C for 5 seconds. At this time, the clip interval in the film width direction was narrowed at the same time as the heat treatment, so that a 3% relaxation treatment was performed in the width direction. After passing through the final heat treatment zone, the film was cooled with 30°C cooling air for 5 seconds. At this time, the actual film temperature at the tenter outlet was 45°C. Both edges were cut and removed, and the film was wound into a roll with a width of 500 mm, to continuously produce a biaxially stretched film with a thickness of 30 μm over a predetermined length.
[0195] The method for producing the inorganic thin film layer used in each of the Examples and Comparative Examples will be described below. The method used in Examples 1 to 8 and Comparative Examples 1 to 7 is shown in Table 2. (Formation of inorganic thin film layer M-1) As the inorganic thin film layer M-1, the heat resistance of the base film layer, intermediate layer, or heat seal resin Aluminum oxide was vapor-deposited on the layer. The method of vapor-depositing aluminum oxide on the base film layer is to set the film on the unwinding side of a continuous vacuum deposition machine, run it over a cooled metal drum and wind the film. At this time, the continuous vacuum deposition machine is depressurized to 10-4 Torr or less, and 99.99% pure aluminum metal is loaded into an alumina crucible from the bottom of the cooling drum, and the aluminum metal is heated and evaporated. Oxygen is supplied to the vapor to cause an oxidation reaction, which causes it to adhere and deposit on the film, forming an aluminum oxide film with a thickness of 10 nm.
[0196] (Formation of inorganic thin film layer M-2) As the inorganic thin film layer M-2, a composite oxide layer of silicon dioxide and aluminum oxide was formed by electron beam deposition on the base film layer, intermediate layer, or heat-sealing resin heat-resistant layer. As the deposition source, granular SiO2 (purity 99.9%) and A12O3 (purity 99.9%) of about 3 mm to 5 mm were used. The film thickness of the inorganic thin film layer (SiO2 / A12O3 composite oxide layer) in the film thus obtained (film containing inorganic thin film layer / coating layer) was 13 nm. The composition of this composite oxide layer was SiO2 / A12O3 (mass ratio) = 60 / 40.
[0197] (Coating of coating solution 3 on vapor deposition film (lamination of protective layer)) The above prepared coating solution 3 was applied onto the inorganic thin film layer of the obtained deposition film by gravure roll coating, pre-dried at 110°C, and then fully dried at 160°C to obtain a protective layer of a predetermined coating amount. Then, a post-heat treatment was performed at 40°C for 2 days.
[0198] (Coating of coating solution 4 on vapor deposition film (lamination of protective layer)) The above prepared coating solution 4 was applied onto the inorganic thin film layer of the obtained deposition film by gravure roll coating, pre-dried at 110°C, and then dried at 190°C to obtain a protective layer of a predetermined coating amount. Then, a post-heat treatment was performed at 40°C for 4 days.
[0199] In this manner, film laminates 1 to 3 described in Table 2, each having a coating layer / inorganic thin film layer / protective layer on each film, were prepared. In each of the examples and comparative examples, films 1 to 3 were used and laminated by dry lamination using an adhesive to prepare laminates having the configurations described in Table 3. In addition, in the comparative examples, a polyamide film (N1100-15 μm, manufactured by Toyobo; referred to as NY) was used as the intermediate layer, and a linear low-density polyethylene film (L4102-40 μm, manufactured by Toyobo; referred to as LLDPE) or a non-oriented polypropylene film (P1146-70 μm, manufactured by Toyobo; referred to as CPP) was used as the heat seal resin. The configurations of the prepared laminates are shown in Table 3. In addition, various evaluations were performed on the obtained laminates. The results are shown in Table 3.
[0200] [Table 2]
[0201] [Table 3] [Industrial Applicability]
[0202] According to the present invention, the gas barrier performance is greatly improved by laminating and bonding an inorganic thin film layer, a coating layer, and a barrier protection layer onto each film, and further, by laminating a substrate film using a polyester resin derived from PET bottles, which has a low environmental impact, and a sealant made of a polyester component, a mono-material film is realized while maintaining toughness, sealability, and transparency. Moreover, since the laminated film of the present invention can be easily produced with few processing steps, it is excellent in both economy and production stability, and a gas barrier film with uniform properties can be provided.
Claims
1. A laminated laminate comprising a polyester base film containing 50% by weight or more of polyester resin recycled from PET bottles and a heat-sealable resin layer laminated in that order, the base film being a laminated film having on one side thereof an inorganic thin film layer (A) and a protective layer (a) containing a urethane resin, the heat-sealable resin layer being made of a polyester-based resin having ethylene terephthalate as its main component, the laminated laminate having a puncture strength of 10 N or more and a haze of 20% or less, and an inorganic thin film layer (B) laminated on the heat-sealable resin layer.
2. The laminate described in claim 1, characterized in that an intermediate layer film is provided between the base film and the heat-sealable resin layer via an adhesive, and the intermediate layer film is made of a resin composition containing 70% by mass or more of polybutylene terephthalate resin.
3. 3. The laminate according to claim 2, further comprising an inorganic thin film layer (C) laminated on the intermediate layer film.
4. 4. The laminate according to claim 2, further comprising a protective layer (b) containing a urethane resin laminated on the inorganic thin film layer (C) of the intermediate film.
5. 5. The laminate according to claim 1, further comprising a coating layer (X) between the substrate film and the inorganic thin film layer (A).
6. 5. The laminate according to claim 2, further comprising a coating layer (Y) between the intermediate layer film and the inorganic thin film layer (C).
7. 7. The laminate according to claim 1, wherein each of the inorganic thin film layers (A) to (C) is a layer made of aluminum oxide or a composite oxide of silicon oxide and aluminum oxide.
Citation Information
Patent Citations
Lift amount regulating device for solenoid valve
JP1997004746A
Laminated film, packaging bag and forming method of sealant layer
JP2006305975A
Thermoformable polyester-containing laminate
JP2007517685A
Biaxially-oriented polyester film for use as wrap-around container label, and wrap-around container label of container
JP2012091862A
Battery case packaging material for cold molding, including biaxially-stretched polybutylene terephthalate film
JP2012146636A