METHOD AND APPARATUS FOR WELDING METAL STRIP

The described method addresses the hardness difference issue in metal strip welding by incorporating a cooling process before post-heating, ensuring tempered welds and preventing plate breakage, thereby improving productivity.

JP7574818B2Active Publication Date: 2024-10-29JFE STEEL CORP
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
JP2022031531
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2022-03-02
Publication Date
2024-10-29
Estimated Expiration
2042-03-02

AI Technical Summary

Technical Problem

Existing metal strip welding methods fail to effectively reduce the hardness difference between the base metal and the welded part in high-strength steel sheets, leading to potential plate breakage and reduced productivity due to martensitic transformation during welding.

Method used

A method involving mash seam welding with a cooling process before post-heating to temper the welded part, using cooling media, rolling speed reduction, or standby time to ensure the welded part undergoes martensitic transformation before post-heating, thereby reducing hardness differences.

Benefits of technology

The method reliably tempers the welded part, preventing plate breakage and ensuring continuous processing by effectively reducing the hardness difference between the base metal and the weld, thus enhancing productivity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007574818000002
    Figure 0007574818000002
  • Figure 0007574818000003
    Figure 0007574818000003
  • Figure 0007574818000004
    Figure 0007574818000004
Patent Text Reader

Abstract

To provide a welding method of a metal strip and a welding apparatus in which tempering of a weld zone after mash seam weld of the metal strip is surely performed to decrease hardness difference between a base material part and the weld zone to be capable of preventing sheet fracture in a continuous processing line.SOLUTION: A welding method of a metal strip in a metal strip continuous processing line comprises: a welding process where a tail end of a preceding metal strip 1 is superimposed on a fore-end of a succeeding metal strip 2, and mash seam weld of the superimposed portion is performed by rotating a top and bottom pair of electrode rings 4; a rolling process where a weld zone 20 welded in the welding process is rolled by a top and bottom pressure rollers 5; a post-heating process where heating treatment of the weld zone rolled in the rolling process is performed; and a cooling process where the weld zone is cooled before the post-heating process. A method of the cooling process is preferably selected from at least one of: a method where cooling medium is blown out over the weld zone; a method where rolling speed is decreased in the rolling process; and a method where a prescribed standby time is set before the post-heating process.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method and apparatus for welding metal strips in a continuous metal strip processing line, and in particular to a method and apparatus for welding metal strips of high tensile steel plates, in which the tail end of a leading metal strip and the front end of a trailing metal strip are welded by mash seam welding and the welded portion is tempered by post-heating to reliably reduce the hardness of the welded portion while preventing plate breakage and achieving high productivity. [Background technology]

[0002] In continuous processing lines for metal strips such as steel strips, continuous processing is made possible by joining the preceding metal strip (hereinafter also referred to as the "preceding material") and the following metal strip (hereinafter also referred to as the "following material") by welding at the line entry side. There are various welding methods such as butt resistance welding, lap resistance welding (called "mash seam welding", hereinafter also referred to as "MSW"), and laser welding, but generally, butt resistance welding and laser welding are used for thick materials with a thickness of 2 to 3 mm or more, and lap resistance welding (MSW) is used for thin materials of 2 mm or less.

[0003] In recent years, the demand for high-tensile steel plates has been increasing. However, because high-tensile steel plates contain a lot of carbon (C), there is a problem in that the hardness of the welded parts increases significantly when the steel undergoes martensite transformation through heat treatment.

[0004] In MSW, the weld is heated to a temperature in the austenite region exceeding 1000℃, which is higher than the A3 transformation point, and then, during the natural cooling process, it is rapidly cooled (quenched) to the martensite start point (Ms point), and the weld transforms into martensite and hardens. The base metal part, which does not receive welding heat input, is not affected by heat hardening, so there is a hardness difference between the base metal part and the weld, and there is a risk of the plate breaking when it is repeatedly bent in a continuous processing line. If it breaks in the annealing furnace, it will cause a major problem, such as a decrease in productivity due to the maintenance of the furnace due to damage inside the furnace and the shutdown of operations required to remove the broken plate. In order to eliminate the hardness difference between the base metal part and the weld, which causes such trouble, it is necessary to reduce the hardness difference by tempering the martensite-transformed weld by heat treatment.

[0005] Patent Document 1 discloses a method for welding metal strips in a continuous metal strip processing line, which aims to improve the mechanical properties of a joint formed by mash seam welding (MSW) on overlapping portions of multiple thin steel plates, by welding with a disk electrode (electrode wheel) made of the same type of copper alloy, and then retracting and reciprocating the electrode wheel of the MSW device again to perform MSW and post-heat treatment (tempering of the welded portion that has been hardened by heating with MSW) using the same electrode wheel, and further performing processing (swaging) to reduce the thickness of the overlapping portion at the same time as the post-heat treatment.

[0006] Furthermore, Patent Document 2 discloses a mash seam welding method different from Patent Document 1, in which the ends of two metal sheets are overlapped, the overlapped portion is pressed with a pair of upper and lower electrode wheels, the overlapped portion is continuously welded while a welding current is applied, the two metal sheets are joined, and then the joint portion of the metal sheets is rolled with a pair of upper and lower pressure rollers.

[0007] Furthermore, Patent Document 3 discloses a method for improving the performance of seam welded joints by using post-weld heat treatment in seam welding of steel structures such as automobile bodies, in which after seam welding, heat treatment is performed to cool the seam weld below the martensite start temperature (Ms point), and then the seam weld is tempered, in which the tempering is performed by heating the seam weld above the martensite start temperature but not above the lower critical temperature.

[0008] Incidentally, Patent Document 4 discloses a welding machine that, in order to realize a labor-saving mash seam welding machine, applies a cooling medium immediately after welding to rapidly cool the metal plates so that the overlap can be made smaller, thereby preventing changes in the overlap that can cause welding defects. [Prior art documents] [Patent documents]

[0009] [Patent Document 1] JP 2015-136725 A [Patent Document 2] International Publication No. WO2012 / 039060 [Patent Document 3] Special Publication No. 2010-516471 [Patent Document 4] Japanese Patent Application Publication No. 8-71762 Summary of the Invention [Problem to be solved by the invention]

[0010] The method of joining welded joints described in Patent Document 1 uses the same electrode wheels during mash seam welding and post-heat treatment, and reverses the relative movement directions of the upper and lower electrode wheels while applying pressure and current to the overlapping steel plates, thereby sharing the equipment for mash seam welding and the equipment for post-heat treatment. However, the method described in Patent Document 1 requires the upper and lower electrode wheels to be moved back and forth relative to the intended joining points of the overlapping steel plates, which poses the problem of reduced productivity.

[0011] In contrast, the mash seam welding method disclosed in Patent Document 2 shows a method in which the ends of two metal sheets are overlapped and continuously welded, and then rolled with a pressure roller. In addition, it is described that productivity can be improved by further arranging a post-heating treatment device behind the pressure roller and subsequently performing heat treatment, but while this improves productivity more than the mash seam welding method disclosed in Patent Document 1, the distance between the pressure roller and the post-heating treatment device is narrow, making it difficult to ensure the same amount of time between the end of mash seam welding and the start of heat treatment (post-heating) as in Patent Document 1, and there are cases in which the welded part cannot be reliably tempered, and the difference in hardness between the base material part and the welded part is not reduced, resulting in a problem that the hardness of the welded part remains high.

[0012] Furthermore, Patent Document 3 is directed to seam welding of steel structures such as automobile bodies, and does not describe or suggest a method for seam welding the ends of a metal strip in a continuous metal strip processing line, which can stably achieve both improved productivity and tempering of the welded portion.

[0013] Furthermore, Patent Document 4 only shows an apparatus for performing mash seam welding, and does not mention anything about rolling after welding or heat treatment thereafter. The rapid cooling process after welding is also for the purpose of securing the overlap, and the hardness difference between the base material and the welded part is not reduced, and the problem of the high hardness of the welded part remains.

[0014] The present invention has been made in consideration of the above-mentioned problems, and has an object to provide a metal strip welding method and welding apparatus that can reliably temper the welded portion after mash seam welding of a metal strip, reduce the hardness difference between the base material portion and the welded portion, and prevent plate breakage in a continuous processing line. [Means for solving the problem]

[0015] The present inventors have thoroughly investigated the cause of the phenomenon in which, in a metal strip welding method using MSW in a metal strip continuous processing line, even if the weld is rolled with a pressure roller after MSW and then tempered using a post-heating device, the tempering treatment is not effective and the difference in hardness between the base material and the weld is not reduced, leaving the weld with a martensitic structure that has high hardness.

[0016] As a result, it was found that there is variation in the temperature of the weld immediately after MSW, and when the temperature is higher than a specified temperature, the weld remains in a martensitic structure with high hardness.

[0017] MSW is a joining method in which the leading and trailing metal strips are overlapped by clamping the tail end of the leading metal strip and the tip end of the trailing metal strip, respectively, and then the overlapped portion is sandwiched between a pair of upper and lower electrode rings. An appropriate pressure is applied and an electric current is passed through the overlapped portion, causing the overlapped portions to melt and bond together using Joule heat generated by the contact resistance. The amount of heat generated in MSW is determined by the welding current, the overlap between the metal strips, and the current resistance, which is affected by the pressure.

[0018] However, the overlap between the tail end of the leading metal strip and the tip end of the trailing metal strip may vary by a few percent due to the mechanical precision of the clamp frames that clamp the respective metal strips. In addition, wear and deterioration of the electrode wheels may also cause variation in the pressing force. Furthermore, voltage pulsation due to fluctuations in the power supply load in the factory causes variation in the actual welding current relative to the welding current setting. It was found that due to these causes, the temperature of the weld immediately after MSW varies in the range of 1000 to 1100°C.

[0019] Furthermore, if the temperature of the weld immediately after MSW is higher than a specified temperature, the temperature of the weld does not drop below the martensite start temperature (Ms point) before the weld is tempered by the post-heating device, so martensite transformation does not occur, and the metal structure remains austenitic, and is not tempered even if the weld is tempered by the post-heating device. Also, in high-tensile steel plates with a strength of 1470 MPa or more that contain a lot of carbon, even if they are not rapidly cooled to below the Ms point during the subsequent standby air cooling, the weld transforms into a martensite structure with high hardness as it is slowly cooled to room temperature. For this reason, it was found that the weld remains a martensite structure with high hardness even after heat treatment by the post-heating device.

[0020] The present invention has been made based on the findings obtained from the above-mentioned studies and further studies, and has the following configuration. [1] A method for welding a metal strip in a continuous metal strip processing line, comprising the steps of: a welding process in which the tail end of the preceding metal strip and the front end of the following metal strip are overlapped with each other, and the overlapped portion is mash seam welded by rotating a pair of upper and lower electrode wheels; a rolling step of rolling the welded portion welded in the welding step with a pair of upper and lower pressure rollers; a post-heating process for performing heat treatment on the welded portion rolled in the rolling process; having Furthermore, a cooling step of cooling the welded portion is performed before the post-heating step. 1. A method for welding metal strips, comprising: [2] The method for welding metal strips according to [1], characterized in that the cooling step is at least one of a method of spraying a cooling medium onto the welded portion, a method of reducing the rolling speed in the rolling step, and a method of waiting for a predetermined time before the post-heating step. [3] The method for welding metal strips according to [1] or [2], characterized in that the cooling step is carried out based on the temperature of the weld immediately after the welding step. [4] The method for welding metal strips according to any one of [1] to [3] above, wherein the metal strip is a high-tensile steel plate having a thickness of 2 mm or less and a strength of 1470 MPa or more. [5] A welding device for a metal strip in a metal strip continuous processing line, comprising: a welding means for overlapping the tail end of the preceding metal strip with the front end of the following metal strip, and mash seam welding the overlapped portion by rotating a pair of upper and lower electrode wheels; a rolling means for rolling the welded portion welded by the welding means with a pair of upper and lower pressure rollers; a post-heating means for performing heat treatment on the welded portion rolled by the rolling means; Equipped with Furthermore, a cooling means for cooling the welded portion is provided upstream of the post-heating means. 1. A metal strip welding apparatus comprising: [6] The metal strip welding apparatus according to [5], characterized in that the cooling means is a cooling medium injection device that sprays a cooling medium onto the welded portion. [7] The metal strip welding apparatus according to [6], characterized in that the cooling medium injection device is a high-pressure air injection device. [8] The metal strip welding apparatus according to any one of [5] to [7], characterized in that the post-heating means is an induction heating device. [9] In any one of [5] to [8] above, the metal strip welding apparatus is characterized in that the metal strip is a high-tensile steel plate having a thickness of 2 mm or less and a strength of 1470 MPa or more. Effect of the Invention

[0021] According to the present invention, by providing a cooling step for cooling the welded portion before the post-heating step, even if there is a variation in temperature of the welded portion immediately after mash seam welding before the post-heating step, the temperature of the welded portion can be lowered and martensitic transformation can occur before the post-heating step. This ensures that the welded portion is tempered in the post-heating step, reduces the hardness difference between the base material portion and the welded portion, and prevents plate breakage when the metal strip is repeatedly bent in a continuous processing line. [Brief description of the drawings]

[0022] [Figure 1] 1 is a schematic side view showing an example of a basic device configuration of a mash seam welding device according to the present invention. FIG. [Diagram 2] 1A is a schematic side view showing an example of a mash seam welding apparatus according to the present invention, the apparatus being equipped with a cooling medium injection device, (a) being a side view of the entire apparatus, (b) being a partially enlarged view, and (c) being a front view of the entire apparatus. [Diagram 3] FIG. 2 is a schematic explanatory diagram showing an example of a waiting method before post-heating in the cooling step in the mash seam welding method according to the present invention. [Figure 4] 13 is a graph showing the difference in temperature change of the welded portion when waiting to cool and when a cooling medium injection method is combined. [Diagram 5] 1A is a schematic diagram illustrating a temperature change (heat cycle) of a welded portion due to differences in the cooling process in the welding method according to the present invention, (a) a conventional example, (b) an example 1 of the invention, (c) an example 2 of the invention, and (d) an example 3 of the invention. [Figure 6] FIG. 4 is a schematic cross-sectional view illustrating a state of a welded portion during welding. [Figure 7] 1 is a graph showing the measurement results of Vickers hardness distribution around a welded portion. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0023] [Mash seam welding equipment] A specific embodiment of the mash seam welding apparatus according to the present invention will be described with reference to the drawings. FIG. 1 is a schematic diagram showing a schematic configuration of one embodiment of a mash seam welding device according to the present invention. The system is equipped with a leading metal strip 1 and a trailing metal strip 2, a pair of upper and lower electrode wheels 4, a pair of upper and lower pressure rollers (also called "swaging rolls") 5, a post-heating device 6, a post-welding thermometer 7, a post-rolling thermometer 8, and a post-heating thermometer 9, all of which are mounted on a carriage 3 for transporting the electrode wheels 4 and other components together.

[0024] With the leading metal strip 1 and the trailing metal strip 2 overlapping, the carriage 3 moves in the direction of the arrow.

[0025] The pair of upper and lower electrode wheels 4 can be driven vertically, for example, by a hydraulic or pneumatic cylinder device (not shown), which applies pressure to the overlapping portion of the leading metal strip 1 and the trailing metal strip 2 and continuously welds the entire width of the metal strips from one end to the other while passing a welding current.

[0026] A pair of upper and lower pressure rollers 5 are arranged downstream of the electrode wheel 4 and can be driven vertically by, for example, a hydraulic or pneumatic cylinder device (not shown) to continuously roll and crush the welded portion and flatten the steps of the welded portion. The pressure rollers 5 are structured so that the temperature rise of the roller surface is suppressed by internal water cooling. The rotational surfaces of the upper and lower rolls may cross at an angle of, for example, 5° or less.

[0027] The heating method of the post-heating device 6 can be a direct heating method using a burner, a heating method using an induction heating device, or a heating method using an electrode wheel as in Patent Document 1. In this case, however, it is preferable to use an induction heating device which has a fast temperature rise rate and can heat from one side from the viewpoint of installation space.

[0028] Furthermore, in order to measure the temperature of the welded portion in each of the welding, rolling and post-heating steps constituting the welding method for metal strips according to the present invention, which will be described later, it is preferable to arrange thermometers as follows. The temperature of the welded portion after the welding step is measured by a post-welding thermometer 7 installed immediately after the pair of upper and lower electrode wheels 4. The temperature of the welded portion after the rolling step is measured by a post-rolling thermometer 8 installed immediately after the pair of upper and lower pressure rollers 5. Note that this post-rolling thermometer 8 also indicates the temperature when a waiting time is provided after the rolling step (=the temperature before the post-heating step), as when a waiting method before post-heating is performed in the cooling step, which will be described later. Furthermore, the temperature of the welded portion during the post-heating step is measured by a post-heating thermometer 9 installed on the top of the post-heating device 6. It is preferable to use non-contact infrared radiation thermometers for all of these thermometers.

[0029] Here, the welded portion is a portion where the parent metal strips 1 and 2 are joined by welding, as shown in Fig. 6, and is made up of a molten portion 21 (also called a "nugget") at the center where the initial overlapping portion is pressurized and heated to melt, a solid-phase welded portion 22 where the end faces of both parent metals are deformed and diffusion-bonded, and a heat-affected zone 23 (also called a "HAZ") deformed by the welding heat. A welded step 24 is formed at a point-symmetrical position with respect to the center of the welded portion. The temperature of the welded portion is measured at a position S on the surface of the metal strips directly above the molten portion (nugget) 21 at the center of the welded portion 20 shown in Fig. 6.

[0030] In one embodiment of the mash seam welding apparatus according to the present invention described above, by moving the carriage 3 in the direction of the arrow, the welding process, rolling process, and post-heating process that constitute the metal strip welding method according to the present invention described below can be performed continuously, thereby increasing productivity.

[0031] [Metal strip welding method] Next, the method for welding metal strips according to the present invention comprises a welding step, a rolling step, a post-heating step, and a cooling step.

[0032] In other words, the present invention is characterized in that a cooling process is provided to cool the welded part either in the welding process or the rolling process before the post-heating process, or after the welding process.As a result, even if there is a temperature variation in the welded part immediately after mash seam welding, the temperature of the welded part can be lowered and martensitic transformation can be caused by the time the welded part enters the post-heating device 6, and the welded part can be reliably tempered and the hardness difference between the base material and the welded part can be reduced. Each of the above steps will now be described in more detail.

[0033] [Welding process] As described above, the mash seam welding process involves clamping and overlapping the tail end of the leading metal strip 1 and the front end of the trailing metal strip 2, respectively, and then sandwiching the overlapped portion between a pair of upper and lower electrode wheels 4. Pressure is applied while rotating the overlapped portion, and a welding current is passed through the overlapped portion to continuously weld the entire width of the metal strip from one end to the other in the width direction.

[0034] The metal strip to be processed is the above-mentioned thin material having a thickness of 2 mm or less, but the thickness can also be 5 mm or less, and more preferably in the range of 0.5 to 2.5 mm.

[0035] The overlap, which is the length (width) of the overlapping portion in the transport direction, is preferably in the range of 0.5 to 1.5 mm from one end of the plate width to the other end, but it is more preferable to determine the length depending on the specifications such as the type, plate thickness, and plate width of the metal strip. It is preferable to make the overlap larger for thicker plates and higher strength materials.

[0036] The electrode wheels 4 are placed on a carriage 3 that moves in the width direction of the plate in order to weld the overlapping portion over the entire width from one end of the plate to the other end in the width direction. A pressure device (not shown) is provided above the upper electrode wheel 4 to press the electrode wheel 4 and apply pressure to the overlapping portion of the metal strip. The lower electrode wheel 4 is structured to support pressure from above. An electrode wheel drive motor (not shown) is provided for each of the upper and lower electrode wheels 4 to rotate them.

[0037] Other welding conditions than the welding overlap include the welding current value, electrode pressure, and welding speed. The greater the electrode pressure, the larger the current carrying area, and therefore the greater the required welding current. If the welding current is too large, the molten part (nugget) in the center of the weld will break through the surface layer of the metal band and cause dust to be ejected to the outside, while if the welding current is too small, it will cause weld peeling. Therefore, the welding current value and electrode pressure are appropriately determined based on the results of a welding test, a cross-sectional macro-structure photograph of the weld and the strength of the weld, such as an Erichsen test. For example, the welding current value is about 10 to 25 kA, and the electrode pressure is about 5 to 40 kN.

[0038] Furthermore, the welding speed (carriage movement speed) is preferably as fast as possible within the range in which insufficient heat input to the weld occurs under the conditions of the welding current value and electrode pressure determined by welding tests, and is preferably in the range of 5.0 to 20.0 mpm.

[0039] [Rolling process] The rolling step is a step in which the welded portion is continuously rolled by a pair of upper and lower pressure rollers 5 . The pressure roller 5 is mounted on the carriage 3 in the same manner as the electrode wheel 4, and is disposed downstream of the electrode wheel 4. A pressure device (not shown) is provided above the pressure roller 5 to press the pressure roller 5 and apply pressure to the welded portion of the metal strip. The lower pressure roller 5 is structured to support pressure from above. The upper and lower pressure rollers 5 are each provided with a pressure roller drive motor (not shown) for rotating them.

[0040] The pressure of the pressure roller 5 is a pressure applied to the pressure roller, similar to the electrode pressure. This pressure is determined based on the results of a rolling test of the welded portion and a cross-sectional macro-structure photograph of the welded portion, so that the welded portion step 24 (FIG. 6) of the welded portion can be smoothed and flattened. For example, the pressure of the pressure roller is about 10 to 30 kN.

[0041] [Post-heating process] The post-heating step is a step in which the rolled welded portion is subjected to heat treatment by a post-heating device 6. As the post-heating device (also called a "post-annealer"), as described above, an induction heating device that has a fast temperature rise rate and is capable of heating from one side is preferable.

[0042] The post-heating temperature is preferably set in a range in which the temperature of the weld does not exceed the austenite start point (Ac1 point) so as to obtain the tempering effect of the martensite structure of the weld, as described later. The Ac1 point can be calculated using the following formula (1).

[0043] Ac1=750.8-26.6C+17.6Si-11.6Mn-22.9Cu-23Ni+24.1Cr+22.5Mo-39.7V-5.7Ti+232.4Nb-169.4Al-894.7B... (1) Here, the symbol of an element indicates the content (mass%) of the element in the metal band composition. An element that is not contained is represented as 0.

[0044] For example, when the material type of the target metal strip is the same as above, with C: 0.1-0.2%, Si: 0.5-1.5%, and Mn: 1-5%, the Ac1 point range is 696-763° C. As an example, when the above-mentioned steel type is C: 0.20 mass%, Si: 1.50 mass%, Mn: 4.60 mass%, and the balance is Fe and unavoidable impurities, the Ac1 point is approximately 720° C.

[0045] The temperature variation of the weld immediately after the above-mentioned MSW is about 100°C (1000 to 1100°C) in the range, so the post-heating temperature is determined taking into consideration the variation in the post-heating temperature caused by this variation. For example, a margin of 20°C is added to the temperature variation (about 100°C in the range), and the target post-heating temperature is set to a temperature 120°C lower than the Ac1 point. If the C, Si, and Mn contents (mass%) of the material type of the target metal strip are in the above-mentioned range, the post-heating temperature is 576 to 643°C. As an example, for the above-mentioned steel type, C: 0.20 mass%, Si: 1.50 mass%, Mn: 4.60 mass%, and the balance: Fe and unavoidable impurities, the post-heating temperature is about 600°C.

[0046] [Cooling process] The cooling step is a step of cooling the welded portion before the above-mentioned post-heating step, i.e., after the welding step and / or after the rolling step before entering the post-heating step.

[0047] Specific methods for cooling the welded portion include (1) spraying a cooling medium onto the welded portion (hereinafter also referred to as the "cooling medium injection method"); (2) reducing the rolling speed in the rolling process (hereinafter also referred to as the "rolling speed reduction method"); and (3) waiting for the metal strip to stand by for a predetermined time before the post-heating process (hereinafter also referred to as the "waiting before post-heating method"). The above methods (1), (2), and (3) may be carried out separately or in any suitable combination. The cooling method to be adopted may be selected depending on the working conditions of the welding process.

[0048] Furthermore, the cooling methods may be selected and combined based on the temperature of the welded portion immediately after the welding process. The reason for selecting and combining the cooling methods based on the temperature of the welded portion immediately after the welding process is as follows. In the mash seam welding device shown in FIG. 1, the carriage 3 is moved in the direction of the arrow to continuously perform the welding process, the rolling process, and the post-heating process, and the time from immediately after the welding process to immediately before the post-heating process is short, at 10 s or less. For this reason, when the temperature of the welded portion immediately after the mash seam welding is high, for example, the method (1) alone cannot cause martensitic transformation before the entry side of the post-heating device 6, and it may be appropriate to select a combination of (1) and (2). That is, by selecting and combining appropriate cooling methods according to the variation in the temperature of the welded portion immediately after the mash seam welding, it is possible to reliably cause martensitic transformation before the entry side of the post-heating device even in the short time from immediately after the welding process to immediately before the post-heating process.

[0049] [(1) Coolant injection method] One embodiment of the cooling medium injection method is shown in Fig. 2. As shown in the enlarged view of Fig. 2, for example, a cooling medium of 3 to 4 kg / cm is injected by a compressor or the like (not shown) between the electrode wheel 4 and the pressure roller 5, and further between the pressure roller 5 and the post-heating device 6. 2 Headers 10, 11 are provided to inject high-pressure air at a pressure of about 1000 psi, and the high-pressure air is discharged toward the welded portion after mash seam welding and the welded portion after rolling by the pressure roller. The higher the temperature of the welded portion, the greater the heat removal effect of the high-pressure air, so it is particularly preferable to provide the header 10 between the electrode wheel 4 and the pressure roller 5. Air that is -40 to -80°C lower than room temperature may be used as the cooling medium via a vortex tube that utilizes the vortex effect to separate the high-pressure air (compressed air) into warm air and cold air. For example, in the case of a 1.6 mm steel plate, the cooling rate when using the cooling medium injection method is 0.89°C / s when natural cooling is performed by radiant heat at room temperature of 20°C, whereas it is 3 to 4 kg / cm when using a compressor or the like. 2In the case of high-pressure air jet cooling at a pressure of about 100°C, the cooling rate is 2.63°C / s, which is 2.3 times that of natural cooling, and in the case of low-temperature air jet cooling at -30°C through a vortex tube, the cooling rate is 2.93°C / s, which is 2.9 times that of natural cooling.

[0050] Furthermore, in addition to the above-mentioned air, it is also possible to compress and spray an inert gas such as argon gas or helium gas, although this is not practical (in terms of cost) as a cooling medium.

[0051] [(2) Rolling speed reduction method] In contrast to the above-mentioned cooling medium injection method, this rolling speed reduction method does not require any special cooling means. This method involves reducing the rolling speed of the pressure roller in the rolling process, and increasing the contact time between the pressure roller, whose surface is kept low by internal water cooling, and the weld, thereby removing heat by contact.

[0052] Here, the rolling speed in the rolling process refers to the speed at which the welded portion of the leading metal strip 1 and the trailing metal strip 2 is rolled by the pressure roller 5 in the welding device shown in Fig. 1, and refers to the speed at which the carriage 3 is moved relative to the metal strips in the direction of the arrow, also called the carriage moving speed, and is equal to the above-mentioned welding speed. This rolling speed is preferably in the range of 5 to 20 mpm.

[0053] The average cooling rate during the rolling process from the pressure roller 5 to the post-heating device 6 (distance of about 60 mm) is extremely high at 140 to 160 ° C / s for a 1.6 mm steel plate, so by lowering the carriage movement speed and lengthening this period, the amount of heat removed by contact with the welded part during pressure by the pressure roller 5 and by cooling (natural cooling) during movement before and after pressure can be increased. This narrows the temperature variation range on the entry side of the post-heating device 6 to the low temperature side, so that the temperature can be reliably kept below the Ms point. For example, if the distance between the electrode wheel 4 and the post-heating device 6 is 500 mm, the rolling speed is 10 mpm, and the average cooling rate from after welding to after rolling is 140 ° C / s, if the temperature is to be reduced by minus 20 ° C on the entry side of the post-heating device 6, the rolling speed should be 9.54 mpm (minus 5%) and the residence time should be increased by 0.14 s from 3 s.

[0054] In addition, by carrying out the cooling medium injection method in which a cooling medium is injected into the welded portion to cool it in combination with the rolling speed reduction method in the rolling process, the amount of heat removed by forced convection can be increased in addition to the natural cooling during movement before and after pressurization, and the welded portion can be cooled more efficiently in a short period of time, which is preferable.

[0055] [(3) Standby method before post-heating] As another cooling method, there is a method in which the metal strip is allowed to stand and cool for a predetermined period of time before the post-heating step.

[0056] One embodiment of the post-heating waiting method will be described with reference to FIG. FIG. 3(a) shows the state during welding in the mash seam welding method. While the carriage 3 moves from right to left, the overlapping portion of the leading metal strip 1 and the trailing metal strip 2 is welded by a pair of upper and lower electrode wheels 4, and the welded metal strip is then rolled by the pressure roller 5. In this state, the post-heating device 6 is not in operation and is in the OFF state. Normally, the post-heating device 6 is operated, that is, the post-heating process is performed in the ON state, but in the case of this post-heating waiting method, the post-heating device 6 remains in the OFF state, resulting in the state shown in FIG. 3(b). That is, the welding and rolling are completed, and the carriage 3 has reached the left end. Here, only the upper roll of the electrode wheel 4 and the pressure roller 5 is raised to open a gap (gap) between the top and bottom. Then, as shown in FIG. 3(c), the carriage 3 is moved to the right. At this time, the gap remains open. Then, when the carriage 3 returns to its initial position (the carriage 3 is at the right end), as shown in FIG. 3(d), the post-heating device 6 is turned on, the carriage 3 is moved to the left, and the welded metal strip is passed through to perform post-heating treatment on the metal strip.

[0057] This method allows the welded metal strip to wait for the time it takes for the carriage 3 to go back and forth between the rolling process and the post-heating process, during which the temperature of the welded part drops due to natural cooling. In this case, the waiting time is preferably 40 to 80 seconds.

[0058] Furthermore, in addition to the post-heating waiting method, the above-mentioned cooling medium injection method may be combined. In this case, the waiting may be performed until the temperature of the welded portion falls below a predetermined temperature (e.g., Ms point), or the waiting may be performed for a predetermined time depending on the temperature of the welded portion immediately after the welding process.

[0059] Figure 4 shows the difference in temperature change in a weld when the plate thickness is 1.6 mm and the temperature of the weld is 335°C, between leaving the weld to cool naturally and when the cooling medium injection method is combined. This shows that when the Ms point is 305°C, it takes about 40 seconds to lower the temperature of the weld to the Ms point by simply leaving it to wait, but this is reduced to about 10 seconds when the cooling medium injection method is combined.

[0060] [Temperature change in welded part (heat cycle)] The temperature change (heat cycle) of the welded part due to the difference in the cooling process in the welding method according to the present invention will be explained with reference to Fig. 5(a) to (d). Here, Fig. 5(a) is a conventional example without a cooling process. Fig. 5(b) is an example of cooling by the cooling medium injection method (1) in the above-mentioned cooling method in Example 1 of the invention, Fig. 5(c) is an example of cooling by the rolling speed reduction method (2) in Example 2 of the invention, and Fig. 5(d) is an example of cooling by the waiting before post-heating method (3) in Example 3 of the invention.

[0061] In addition, the symbols [A] to [F] in Figures 5(a) to (d) indicate periods, and their contents are as follows. [A] Duration of the welding process (from start to finish) [B] Period from after welding to before rolling (the transition period from the end of welding to before rolling by the pressure roller) [C] Period of rolling process (period of rolling by pressure roller 5) [D] Period from after rolling to before post-heating (period from after rolling to before post-heating) [E] Period of post-heating process (period of heat treatment by post-heating device) [F] The period from post-heating to cooling

[0062] First, the transition of temperature change in the conventional example of FIG. 5(a) will be described. The period [A] in Figure 5(a) is very short, within 0.5 seconds. During this period, the weld is heated to 1000°C or higher, for example 1033°C, which exceeds the austenite transformation point (hereinafter also referred to as the "Ac3 point"), causing austenite transformation (hereinafter also referred to as the "γ transformation"). This Ac3 point can be calculated using the following formula (2):

[0063] Ac3 points=937.2-436.5C+56Si-19.7Mn-16.3Cu-26.6Ni-4.9Cr+38.1Mo+124.8V+136.3Ti-19.1Nb+198.4Al+3315B... (2) Here, the symbol of an element indicates the content (mass%) of the element in the metal band composition. An element that is not contained is represented as 0.

[0064] For example, when the steel composition of the target metal strip is 0.1-0.2 mass% C, 0.5-1.5 mass% Si, and 1-5 mass% Mn, the Ac3 point ranges from 779 to 958° C. As an example, when the steel composition is 0.20 mass% C, 1.50 mass% Si, 4.60 mass% Mn, and the balance is Fe and unavoidable impurities, the Ac3 point is approximately 850° C.

[0065] Next, the period [B] in Fig. 5(a) is within 3 s, during which the weld is naturally cooled. The cooling rate of natural cooling is about 0.7 to 3.0°C / s when the plate thickness is in the range of 0.5 to 2.0 mm.

[0066] 5(a), the period [C] is within 0.5 seconds, similar to the above [A]. Here, the heat of the welded portion is largely removed by contact with the pressure roller 5. In the next period [D] in Figure 5(a), the material is allowed to cool further naturally.

[0067] Here, when the temperature drops below the martensitic transformation starting point (hereinafter also referred to as the "Ms point") and martensitic transformation (hereinafter also referred to as the "M transformation") occurs, a hard martensitic structure is generated. However, if there is no cooling and the temperature drop is small, there is no martensitic transformation and a hard martensitic structure is not generated.

[0068] This Ms point can be calculated using the following formula (3). Ms point=521-353C-22Si-24.3Mn-7.7Cu-17.3Ni-17.7Cr-25.8Mo... (3) Here, the symbol of an element indicates the content (mass%) of the element in the metal band composition. An element that is not contained is represented as 0.

[0069] For example, when the material type of the target metal strip is the same as above, with C: 0.1-0.2%, Si: 0.5-1.5%, and Mn: 1-5%, the Ms point ranges from 296 to 450° C. As an example, when the above-mentioned steel type is C: 0.20 mass%, Si: 1.50 mass%, Mn: 4.60 mass%, and the balance is Fe and unavoidable impurities, the Ms point is approximately 305° C. When the temperature of the weld falls below this Ms point, martensite transformation occurs, and a hard martensite structure is formed.

[0070] Next, the period [E] in Fig. 5(a) is within 2 s. If the temperature of the weld exceeds the Ms point before entering the post-heating process, in other words, if martensitic transformation has not occurred before entering the post-heating process, the weld will not be tempered even if heat treatment is performed, so the hardness difference between the base material (leading metal strip and trailing metal strip) and the weld will not be reduced, and the hardness of the weld will remain high.

[0071] After that, the weld is naturally cooled during the period [F] in Fig. 5(a). In this conventional example, the weld is not tempered even after the post-heating process [E], and the hardness of the weld remains high.

[0072] Next, the first embodiment of the present invention shown in FIG. 5(b) will be described. In this invention example 1, cooling was performed by injecting a cooling medium during periods [B] and [D] in Fig. 5(b). In this case, the temperature of the welded part drops significantly during period [B], and after the subsequent rolling process [C], the temperature of the welded part falls below the Ms point, martensitic transformation occurs, and a hard martensite structure is formed. Therefore, even if tempering is performed in the subsequent post-heating process [E], the Ac1 point is not reached, and tempered martensite is formed, reducing the hardness difference between the base material and the welded part.

[0073] Next, a second embodiment of the present invention shown in FIG. 5(c) will be described. This invention example 2 is an example using a rolling speed reduction method in which the rolling speed (carriage movement speed) of the rolling process is reduced during the period [C] in Fig. 5(c). In this case, by reducing the carriage movement speed, it is possible to gain time for the rolling time [C] and for the cooling (natural cooling) times [B] and [C], so that the temperature of the welded part drops below the Ms point. As a result, as with the above invention example 1, the temperature of the welded part does not reach the Ac1 point even after the subsequent post-heating process, so that tempered martensite is generated and the hardness difference between the base material and the welded part is reduced.

[0074] Finally, Example 3 of the invention shown in FIG. 5(d) will be described. This example 3 of the invention is an example using a method of lowering the temperature of the weld by providing a waiting time before post-heating in the period [D] in Fig. 5(d). In this case, by extending the period [D], the temperature of the weld falls below the Ms point, and similarly to the above-mentioned examples 1 and 2 of the invention, the temperature of the weld does not reach the Ac1 point even by the subsequent post-heating process, so that tempered martensite is generated and the hardness difference between the base material and the weld is reduced.

[0075] [Cooling control by temperature measurement] Furthermore, it is preferable (from an economic point of view) to carry out this cooling step by measuring the temperature of the weld immediately after the welding step and, if the temperature of the weld exceeds a predetermined value, carrying out a subsequent cooling step.

[0076] Specifically, for example, in the case of the cooling medium injection method shown in FIG. 2, the temperature of the welded part immediately after the electrode wheel 4 is measured by a thermometer 7 after welding, and when the temperature exceeds a predetermined value, it is preferable to control so that high-pressure air is ejected from a header 10 that is provided between the electrode wheel 4 and the pressure roller 5 and that injects high-pressure air, and from a header 11 that is provided after the pressure roller 5 and that injects high-pressure air.

[0077] This predetermined value may be determined in advance based on the measurement data of the post-welding thermometer 7 and the post-rolling thermometer 8, as a temperature value at which the temperature of the welded portion at the entry side of the post-heating device 6 is surely below the Ms point. For example, if the temperature of the welded portion immediately after MSW varies in the range of 1000 to 1100°C, the temperature of the welded portion at the entry side of the post-heating device 6 is in the range of 281 to 309°C, and the Ms point is 305°C, then if the predetermined value is set to 1070°C, the variation range at the entry side of the post-heating device 6 can be narrowed to 281 to 300°C, and the temperature can be surely below the Ms point. Therefore, when the temperature of the welded portion immediately after welding is 1070°C or lower, the high-pressure air can be controlled to stop its injection, thereby preventing unnecessary discharge of high-pressure air, and thus reducing running costs.

[0078] Also, even when the cooling method is the rolling speed reduction method or the waiting method before post-heating, the temperature of the welded portion may be measured immediately after the welding process, and the cooling method may be carried out if the temperature of the welded portion exceeds a predetermined value. EXAMPLES

[0079] In this example, the mash seam welding equipment shown in FIG. 1 or FIG. 2 was used, and a 1470 MPa class high tensile steel plate (the composition of the steel type was the same as the above-mentioned steel type example, C: 0.20 mass %, Si: 1.50 mass %, Mn: 4.60 mass %, the balance: Fe and unavoidable impurities) and a cold-rolled coil (metal strip) having a sheet thickness of 1.6 mm were overlapped with an overlap of 1.2 mm as a leading metal strip 1 and a trailing metal strip 2, and continuously welded with an electrode wheel 4, subsequently rolled with a pressure roller 5, and further subsequently subjected to heat treatment with a post-heating device 6. The temperatures of the welded portion after the welding process and the welded portion after the rolling process were measured with a post-welding thermometer 7 and a post-rolling thermometer 8, respectively.

[0080] Regarding the temperature of the thermometer 8 after rolling, if it did not exceed the Ms point (305° C. for the above steel sheet), it was judged as good (◯), and if it did exceed it, it was judged as bad (×).

[0081] We then checked whether the hardness of the welds had been softened by tempering to a level equivalent to the hardness of the base metal strip (400HV or less). Hardness was measured in accordance with JIS Z 2244 "Vickers hardness test method," measuring the Vickers hardness (HV) in the conveying direction of the welds at measurement intervals of 0.2mm with a measurement load (test force) of 200g. If the average Vickers hardness (HV) was 400 or less (HV≦400), it was deemed to have been softened by tempering (good: ◯).

[0082] In the post-heating step using the post-heating device 6, the welded portion was heated to a target temperature of 600° C., and then allowed to cool naturally.

[0083] Table 1 shows a list of the results of Inventive Examples 1 to 14 and Comparative Examples 1 to 3.

[0084] [Table 1]

[0085] Among Inventive Examples 1 to 14, Inventive Examples 1 to 7 are examples in which the cooling step was carried out and the post-heating step was carried out without any particular temperature control.

[0086] Examples 8 to 14 of the present invention are examples of the invention that use a cooling control method based on temperature measurement, in which the predetermined value for the temperature after welding is set to 1070°C, the temperature immediately after welding is measured using the post-welding thermometer 7 shown in FIG. 1, and when the measured value exceeds the above-mentioned predetermined value, control is performed to carry out a cooling process.

[0087] First, in Example 1 of the present invention, as shown in Fig. 2, headers 10 and 11 for spraying high-pressure air as a cooling medium are provided between the electrode wheel 4 and the pressure roller 5, and between the pressure roller 5 and the post-heating device 6, and high-pressure air is sprayed toward the welded part after mash seam welding and after rolling by the pressure roller 5. The pressure of the high-pressure air is 4 kg / cm 2 The temperature after rolling was 255℃, which was below the Ms point (305℃), and the average Vickers hardness was 328HV, which was below the target of 400HV.

[0088] In Example 2 of the present invention, the rolling speed was reduced during the rolling process. In this case, the rolling speed was reduced by 0.5 mpm from the normal 9.5 mpm to 9.0 mpm. As a result, the temperature after rolling was 273°C, which was below the Ms point, and the average Vickers hardness was 344HV.

[0089] In Example 3 of the present invention, as explained in the procedure shown in Fig. 3, after the rolling process, the gap between the electrode wheel 4 and the pressure roller 5 was opened before the post-heating process, and the material was left to stand by for a predetermined time (40 s) to cool naturally before the post-heating process. As a result, the temperature after rolling (= temperature before post-heating) was 302°C, which was below the Ms point, and the average Vickers hardness was 358 HV.

[0090] Inventive Example 4 is a case where cooling was performed by combining the cooling medium injection method of Inventive Example 1 and the rolling speed reduction method of Inventive Example 2. As a result, the temperature after rolling was 241°C, which was below the Ms point, and the average Vickers hardness was 320HV.

[0091] Inventive Example 5, cooling was performed by combining the cooling medium injection method of Inventive Example 1 and the waiting method before post-heating of Inventive Example 3. As a result, the temperature after rolling was 247°C, which was below the Ms point, and the average Vickers hardness was 336HV.

[0092] Inventive Example 6 is a case where cooling was performed by combining the rolling speed reduction method of Inventive Example 2 and the waiting method before post-heating of Inventive Example 3. As a result, the temperature after rolling was 262°C, which was below the Ms point, and the average Vickers hardness was 350HV.

[0093] Inventive Example 7 is a case where cooling was performed by combining all three methods: the cooling medium injection method of Inventive Example 1, the rolling speed reduction method of Inventive Example 2, and the waiting method before post-heating of Inventive Example 3. As a result, the temperature after rolling was 238°C, which was below the Ms point, and the average Vickers hardness was 312HV.

[0094] Next, in Examples 8 to 14 of the present invention, a cooling process was carried out when the post-welding temperature exceeded a predetermined value (1070°C), and the content of the cooling process was carried out in accordance with each of the methods of Examples 1 to 7 of the present invention described above.

[0095] As a result, in Example 8 of the present invention, which is an example in which the cooling medium injection method was used, the temperature after rolling was 285° C., which was below the Ms point, and the average Vickers hardness was 320 HV.

[0096] Inventive Example 9 is an example in which the rolling speed reduction method was used, in which the temperature after rolling was 282° C., which was below the Ms point, and the average Vickers hardness was 333 HV.

[0097] Inventive Example 10 is an example in which the waiting before post-heating method was used, in which the temperature after rolling was 303° C., which was below the Ms point, and the average Vickers hardness was 350 HV.

[0098] Inventive Example 11 is an example in which cooling was performed by combining the cooling medium injection method and the rolling speed reduction method, whereby the temperature after rolling was 271°C, which was below the Ms point, and the average Vickers hardness was 318HV.

[0099] Inventive Example 12 is an example in which cooling was performed by combining the cooling medium injection method and the waiting method before post-heating. As a result, the temperature after rolling was 280°C, which was below the Ms point, and the average Vickers hardness was 330HV.

[0100] Inventive Example 13 is an example in which cooling was performed by combining the rolling speed reduction method and the waiting method before post-heating. As a result, the temperature after rolling was 303°C, which was below the Ms point, and the average Vickers hardness was 345HV.

[0101] Inventive Example 14 is an example in which cooling was performed by combining the cooling medium injection method, the rolling speed reduction method, and the waiting before post-heating method. As a result, the temperature after rolling was 270°C, which was below the Ms point, and the average Vickers hardness was 310HV.

[0102] Comparative Examples 1 and 2 are cases where the post-heating step using the post-heating device 6 shown in Fig. 1 was not performed, and in Comparative Example 1, the temperature after rolling was 286°C, which was below the Ms point, but since no post-heating treatment was performed, the average Vickers hardness was 501HV, which significantly exceeded the target of 400HV. In Comparative Example 2, the temperature after rolling was 315°C, which was above the Ms point, and no post-heating treatment was performed, and the average Vickers hardness was 520HV, which significantly exceeded the target of 400HV.

[0103] Comparative Example 3 is an example in which post-heat treatment was performed. However, since the temperature after the rolling prior to the post-heat treatment was high at 325°C and there was no cooling process, even after the subsequent post-heat treatment, the average Vickers hardness was 482 HV, which significantly exceeded the target of 400 HV.

[0104] Furthermore, the Vickers hardness distribution around the welds in the invention examples and comparative examples was measured. The measurement results are shown in Figure 7. Comparative Example 1 "without post-heating process" and Comparative Example 3 "without cooling process and with post-heating process" did not show any reduction in Vickers hardness, but the invention example 4 "with cooling process and with post-heating process" showed a reduction in Vickers hardness.

[0105] From the above, the effectiveness of the present invention was demonstrated. [Explanation of symbols]

[0106] 1 Lead metal strip (lead material) 2 Trailing metal strip (trailing material) 3 Carriage 4 electrode ring 5 Pressure roller (swaging roll) 6 Post-heating device 7. Post-weld thermometer 8 Thermometer after rolling 9 Post-heating thermometer 10, 11 Header (cooling device) 12 Inlet clamp 13 Output clamp 20 Welding 21 Welded part (nugget) 22 Solid phase junction 23 HAZ (heat affected zone) 24 Welding step

Claims

1. 1. A method for welding a metal strip in a continuous metal strip processing line, comprising the steps of: a welding process in which the tail end of the preceding metal strip and the front end of the following metal strip are overlapped with each other, and the overlapped portion is mash seam welded by rotating a pair of upper and lower electrode wheels; a rolling step of rolling the welded portion welded in the welding step with a pair of upper and lower pressure rollers; a post-heating process for performing heat treatment on the welded portion rolled in the rolling process; having Furthermore, a cooling step of cooling the welded portion is performed before the post-heating step. Has the cooling step is at least one of a method of spraying a cooling medium on the welded portion, a method of reducing a rolling speed in the rolling step, and a method of waiting for a predetermined time before the post-heating step; The metal strip is a high-tensile steel plate having a plate thickness of 2 mm or less and a strength of 1470 MPa or more, and the Vickers hardness (HV) of the welded portion is 400 or less.

2. A method for welding metal strips comprising the steps of:

2. The method for welding a metal strip as described in claim 1, characterized in that the cooling medium is high-pressure air at a pressure of 3 to 4 kg / cm2, the rolling speed is 5.0 to 20.0 mpm, or the predetermined waiting time before the post-heating step is 40 to 80 s.

3. 3. The method of claim 1, wherein the cooling step is performed based on the temperature of the weld immediately after the welding step.

4. 1. An apparatus for welding a metal strip in a continuous metal strip processing line, comprising: a welding means for overlapping the tail end of the preceding metal strip with the front end of the following metal strip, and mash seam welding the overlapped portion by rotating a pair of upper and lower electrode wheels; a rolling means for rolling the welded portion welded by the welding means with a pair of upper and lower pressure rollers; a post-heating means for performing heat treatment on the welded portion rolled by the rolling means; Equipped with Further, a cooling means for cooling the welded portion is provided upstream of the post-heating means, the cooling means is a cooling medium injection device that sprays a cooling medium onto the welded portion, The metal strip is a high-tensile steel plate having a plate thickness of 2 mm or less and a strength of 1470 MPa or more, and the Vickers hardness (HV) of the welded portion is 400 or less.

1. An apparatus for welding metal strips, comprising:

5. 5. The metal strip welding apparatus according to claim 4, wherein the cooling medium jetting device is a high-pressure air jetting device with a pressure of 3 to 4 kg / cm 2 .

6. 6. An apparatus for welding metal strips according to claim 4 or 5, characterized in that the post-heating means is an induction heating device.

Citation Information

Patent Citations

  • Mash seam welding machine

    JP1996071762A

  • A method for improving the performance of seam welded joints using post-weld heat treatment.

    JP2010516471A

  • Method of forming weld joint

    JP2015136725A

  • Dual-pass, dual-anneal welding process for joining high-strength steels

    JP2022513080A

  • Mash seam welding method and device

    WO2012039060A1