Plasma treatment method

By monitoring and adjusting plasma conditions in real-time, the plasma processing method addresses shape abnormalities in high aspect ratio patterns, ensuring precise and uniform film deposition, thereby stabilizing the film formation process.

JP7575201B2Active Publication Date: 2024-10-29TOKYO ELECTRON LTD
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2020092244
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-05-27
Publication Date
2024-10-29
Estimated Expiration
2040-05-27

AI Technical Summary

Technical Problem

The challenge of stabilizing the performance of film formation processes in plasma processing, particularly in forming high aspect ratio patterns with high precision, is exacerbated by shape abnormalities such as bowing in deep holes, which traditional methods struggle to address effectively.

Method used

A plasma processing method involving monitoring the plasma state during film formation, adjusting processing conditions based on real-time plasma monitoring, and determining whether to re-execute the process to ensure accurate and uniform film deposition, using a plasma processing apparatus with integrated sensors and control units to manage plasma generation and film formation.

Benefits of technology

This approach stabilizes the film formation process, enabling precise and uniform film deposition even in high aspect ratio patterns, improving in-plane uniformity and accuracy of plasma processing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575201000001
    Figure 0007575201000001
  • Figure 0007575201000002
    Figure 0007575201000002
  • Figure 0007575201000003
    Figure 0007575201000003
Patent Text Reader

Abstract

To stabilize the performance of film formation processing using plasma.SOLUTION: A plasma processing method includes a step a), a step b), and a step c). In the step a), a substrate having a recess is provided in a processing container. In the step b), plasma is generated in the processing container to form a film on the recess. In the step c), the state of the plasma generated in the step b) is monitored. on the basis of the monitored plasma state, the necessity of re-execution of the step b) and the processing condition at the time of re-execution are determined.SELECTED DRAWING: Figure 6
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The following disclosure relates to a plasma processing method. By law Regarding. [Background technology]

[0002] As semiconductor device integration progresses not only horizontally but also vertically, the aspect ratio of the patterns formed during the semiconductor device manufacturing process is also increasing. For example, in the manufacture of 3D NAND, channel holes are formed in a direction that penetrates multiple metal wiring layers. When forming 64-layer memory cells, the aspect ratio of the channel hole is as high as 45.

[0003] Various methods have been proposed to form high aspect ratio patterns with high accuracy. For example, a method has been proposed in which etching and film deposition are repeatedly performed in an opening formed in a dielectric material of a substrate to suppress lateral etching (Patent Document 1). Also, a method has been proposed in which etching and film deposition are combined to form a protective film to prevent lateral etching of a dielectric layer (Patent Document 2). [Prior art documents] [Patent documents]

[0004] [Patent Document 1] US Patent Application Publication No. 2016 / 0343580 [Patent Document 2] US Patent Application Publication No. 2018 / 0174858 Summary of the Invention [Problem to be solved by the invention]

[0005] The present disclosure provides a technique capable of stabilizing the performance of a film formation process using plasma. [Means for solving the problem]

[0006] A plasma processing method realized by a plasma processing apparatus according to an embodiment of the present disclosure includes steps a), b), and c). In step a), a substrate having a recess is provided in a processing vessel. In step b), plasma is generated in the processing vessel to form a film on the recess. In step c), a state of the plasma generated in step b) is monitored. Based on the monitored state of the plasma, it is determined whether step b) needs to be performed again and the processing conditions for re-performing step b). Effect of the Invention

[0007] According to the present disclosure, it is possible to stabilize the performance of a film formation process using plasma. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a diagram illustrating an example of a configuration of a plasma processing system according to an embodiment. [Diagram 2] FIG. 2 is a diagram illustrating an example of a configuration of a plasma processing apparatus according to an embodiment. [Diagram 3] FIG. 3 is a flowchart showing an outline of the flow of plasma processing according to an embodiment. [Figure 4] FIG. 4 is a diagram for explaining an example of a flow of subconformal atomic layer deposition (ALD). [Diagram 5] FIG. 5 is a diagram for explaining another example of the flow of the sub-conformal ALD. [Figure 6] FIG. 6 is a flow chart further illustrating a plasma process according to one embodiment. [Figure 7] FIG. 7 is a flowchart illustrating the monitoring process and the determination process according to an embodiment. [Figure 8] FIG. 8 is a diagram for explaining a monitoring result obtained in the monitoring process according to an embodiment. [Figure 9A]FIG. 9A is a diagram for explaining a second method example for detecting a physical quantity in a monitor process according to an embodiment. [Figure 9B] FIG. 9B is a diagram showing an example of digitalization of the image obtained by the method example 2 in FIG. 9A. [Figure 10] FIG. 10 is a flowchart showing an example of the flow of the monitor process based on the example technique 2 of FIGS. 9A and 9B. [Figure 11] FIG. 11 is a diagram illustrating an example of information stored in the storage unit in the plasma processing according to the embodiment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] The disclosed embodiments will be described in detail below with reference to the drawings. Note that the present embodiments are not limiting. In addition, each embodiment can be appropriately combined as long as the processing contents are not contradictory. Note that the same reference numerals are used for the same or corresponding parts in each drawing.

[0010] In the following description, the term "pattern" refers to a shape formed on a substrate in general. The pattern refers to the entirety of a plurality of shapes formed on a substrate, such as holes, trenches, and lines and spaces. The term "recess" refers to a portion of a pattern formed on a substrate that is recessed in the thickness direction of the substrate. The recess has a "sidewall" which is the inner peripheral surface of the recessed shape, a "bottom" which is the bottom part of the recessed shape, and a "top" which is the substrate surface adjacent to the sidewall and is continuous with the sidewall. The space surrounded by the top is called an "opening". The term "opening" is also used to refer to the entire space surrounded by the bottom and sidewall of the recess, or any position in the space.

[0011] It is known that shape abnormalities are likely to occur when forming deep holes with high aspect ratios, such as HARC (High Aspect Ratio Contact). For example, a shape abnormality called bowing is known. Bowing is a shape abnormality in which the inner peripheral surface of an opening bulges horizontally into a barrel shape when an opening is formed in the vertical direction. In this embodiment, a film is formed on the side wall of the opening to suppress the occurrence of shape abnormalities such as bowing. Examples of film formation techniques include atomic layer deposition (ALD), plasma-enhanced ALD (PEALD), chemical vapor deposition (CVD), plasma-enhanced CVD (PECVD), plasma-enhanced annular chemical vapor deposition (PECCVD), and the like.

[0012] (Configuration Example of Plasma Processing System According to the Embodiment) FIG. 1 is a diagram illustrating an example of a plasma processing system that can be used to perform plasma processing according to an embodiment of the present invention.

[0013] 1 includes a control unit Cnt, a stage 1122a, a stage 1122b, a stage 1122c, a stage 1122d, a container 1124a, a container 1124b, a container 1124c, a container 1124d, a loader module LM, a load lock chamber LL1, a load lock chamber LL2, a transfer chamber 1121, and a plasma processing device 1010. The plasma processing device 1010 may be, for example, the plasma processing device 1 shown in FIG.

[0014] The control unit Cnt is a computer equipped with a processor, a storage unit, an input device, a display device, etc., and controls each unit (to be described later) of the plasma processing system 1000. The control unit Cnt is connected to the transfer robot Rb1, the transfer robot Rb2, the observation device OC, the plasma processing device 1010, etc. The control unit Cnt may also function as the control unit 100 of the plasma processing device 1 shown in FIG.

[0015] The control unit Cnt operates according to a computer program (a program based on an input recipe) for controlling each part of the plasma processing system 1000, and sends out a control signal. The control signal from the control unit Cnt controls each part of the plasma processing system 1000, such as the transfer robots Rb1 and Rb2, the observation device OC, and each part of the plasma processing device 1010. In the plasma processing device 1010, the control signal from the control unit Cnt can control the selection and flow rate of the gas supplied from the gas supply source 15, the exhaust of the exhaust device 65, the power supply from the high frequency power sources 32 and 34, the coolant flow rate, and the coolant temperature. Each step of the substrate processing method according to the first and second embodiments can be executed by operating each part of the plasma processing system 1000 under the control of the control unit Cnt. The storage unit of the control unit Cnt readably stores a computer program for executing the plasma processing method according to the embodiment, and various data used for the execution.

[0016] The stages 1122a to 1122d are arranged along one edge of the loader module LM. The storage containers 1124a to 1124d are provided on the stages 1122a to 1122d, respectively. The storage containers 1124a to 1124d can store wafers W therein.

[0017] A transfer robot Rb1 is provided in the loader module LM. The transfer robot Rb1 takes out a wafer W accommodated in any one of the accommodation containers 1124a to 1124d, and transfers the wafer W to a load lock chamber LL1 or LL2.

[0018] The load lock chambers LL1 and LL2 are provided along another edge of the loader module LM and are connected to the loader module LM. The load lock chambers LL1 and LL2 constitute preliminary decompression chambers. The load lock chambers LL1 and LL2 are each connected to a transfer chamber 1121.

[0019] The transfer chamber 1121 is a chamber that can be depressurized, and a transfer robot Rb2 is provided in the transfer chamber 1121. The plasma processing apparatus 1010 is connected to the transfer chamber 1121. The transfer robot Rb2 takes out a wafer W from the load lock chamber LL1 or the load lock chamber LL2, and transfers the wafer W to the plasma processing apparatus 1010.

[0020] The plasma processing system 1000 includes an observation device OC. The observation device OC can be installed at any location in the plasma processing system 1000. In one example, the observation device OC is installed in an observation module OM adjacent to the loader module LM. The wafer W can be moved between the observation module OM and the plasma processing device 1010 by a transfer robot Rb1 and a transfer robot Rb2. After the wafer W is accommodated in the observation module OM by the transfer robot Rb1 and the wafer W is aligned in the observation module OM, the observation device OC measures the groove width of a pattern such as a mask on the wafer W and transmits the measurement result to the controller Cnt. The observation device OC can measure the groove width of a pattern such as a mask formed in a plurality of regions on the surface of the wafer W. The measurement result by the observation device OC is used, for example, as a "detection result" (see FIG. 11) in the embodiment described later. For example, an optical observation device, a weight scale, an ultrasonic microscope, etc. can be used as the observation device OC.

[0021] (Configuration Example of Plasma Processing Apparatus According to the Embodiment) A plasma processing apparatus 1 according to an embodiment of the present invention will be described with reference to FIG. 2. FIG. 2 shows a vertical cross section of an example of the configuration of the plasma processing apparatus 1 according to this embodiment. The plasma processing apparatus 1 according to this embodiment is a parallel plate type plasma processing apparatus (capacitively coupled plasma processing apparatus) in which a mounting table 20 and a gas shower head 25 are arranged opposite each other in a processing vessel 10. The mounting table 20 has a function of holding a semiconductor substrate (hereinafter simply referred to as "wafer W") and also functions as a lower electrode. The gas shower head 25 has a function of supplying gas into the processing vessel 10 in a shower-like manner and also functions as an upper electrode.

[0022] The processing vessel 10 is made of, for example, aluminum whose surface has been anodized (anodized), and has a cylindrical shape. The processing vessel 10 is electrically grounded. The mounting table 20 is installed at the bottom of the processing vessel 10, and a wafer W is mounted thereon. The wafer W is an example of a substrate to be subjected to plasma processing.

[0023] The mounting table 20 is made of, for example, aluminum (Al), titanium (Ti), silicon carbide (SiC), etc. An electrostatic chuck 106 for electrostatically attracting a substrate is provided on the upper surface of the mounting table 20. The electrostatic chuck 106 has a structure in which a chuck electrode 106a is sandwiched between insulators 106b.

[0024] A DC voltage source 112 is connected to the chuck electrode 106a, and a DC current is supplied to the chuck electrode 106a from the DC voltage source 112. As a result, the wafer W is attracted to the electrostatic chuck 106 by Coulomb force.

[0025] An annular focus ring 103 is placed on the electrostatic chuck 106 so as to surround the peripheral portion of the wafer W. The focus ring 103 is made of a conductive material such as silicon, and focuses plasma inside the processing vessel 10 toward the surface of the wafer W, thereby improving the efficiency of etching.

[0026] The mounting table 20 is supported by a support 104. A coolant flow path 104a is formed inside the support 104. A coolant inlet pipe 104b and a coolant outlet pipe 104c are connected to the coolant flow path 104a. A cooling medium such as cooling water or brine output from a chiller 107 circulates through the coolant inlet pipe 104b, the coolant flow path 104a, and the coolant outlet pipe 104c. As a result, the mounting table 20 and the electrostatic chuck 106 are cooled.

[0027] The heat transfer gas supply source 85 supplies a heat transfer gas such as helium gas (He) or argon gas (Ar) to the backside of the wafer W on the electrostatic chuck 106 through a gas supply line 130. With this configuration, the temperature of the electrostatic chuck 106 is controlled by the cooling medium circulated through the refrigerant flow passage 104a and the heat transfer gas supplied to the backside of the wafer W. As a result, the substrate can be controlled to a predetermined temperature.

[0028] The first high frequency power supply 34 is electrically connected to the gas shower head 25 via a matching unit 35. The first high frequency power supply 34 applies, for example, a high frequency power HF of 60 MHz for plasma excitation to the mounting table 20. In this embodiment, the high frequency power HF is applied to the gas shower head 25, but it may be applied to the mounting table 20. The second high frequency power supply 32 is electrically connected to the mounting table 20 via a matching unit 33. The second high frequency power supply 32 applies, for example, a high frequency power LF of 13.56 MHz for bias to the mounting table 20.

[0029] The matching box 35 matches the load impedance to the internal (or output) impedance of the first high frequency power supply 34. The matching box 33 matches the load impedance to the internal (or output) impedance of the second high frequency power supply 32. The matching box 35 and the matching box 33 function so that the internal impedance and the load impedance of the first high frequency power supply 34 and the second high frequency power supply 32 appear to match each other when plasma is generated in the processing vessel 10.

[0030] The gas shower head 25 includes a ceiling electrode plate 41 having a number of gas supply holes 55, and a cooling plate 42 that detachably supports the ceiling electrode plate 41. The gas shower head 25 is attached to close an opening in the ceiling of the processing vessel 10 via a shield ring 40 that covers the periphery of the gas shower head 25. The gas shower head 25 is formed with a gas inlet 45 for introducing gas. Inside the gas shower head 25, a center-side diffusion chamber 50a and an edge-side diffusion chamber 50b that are branched from the gas inlet 45 are provided. The gas output from the gas supply source 15 is supplied to the diffusion chambers 50a and 50b via the gas inlet 45, diffused in the diffusion chambers 50a and 50b, and introduced toward the mounting table 20 through the multiple gas supply holes 55.

[0031] An exhaust port 60 is formed in the bottom surface of the processing vessel 10, and the inside of the processing vessel 10 is evacuated by an exhaust device 65 connected to the exhaust port 60. This makes it possible to maintain the inside of the processing vessel 10 at a predetermined vacuum level. A gate valve G is provided on the side wall of the processing vessel 10. A wafer W is loaded and unloaded from the processing vessel 10 by opening and closing the gate valve G.

[0032] The plasma processing apparatus 1 is equipped with an optical sensor 108 capable of measuring the intensity of light of each wavelength in the plasma in the processing vessel 10 through a quartz window 109. The optical sensor 108 includes a first sensor 108a and a second sensor 108b. The first sensor 108a detects the state of the plasma generated in the processing vessel 10. The detection result of the first sensor 108a is used in a monitoring process and a determination process, which will be described later. The second sensor 108b detects the pattern shape of the surface of the wafer W placed on the placement table 20. The detection result of the second sensor 108b is used in first to third detection processes, which will be described later.

[0033] The plasma processing apparatus 1 is provided with a control unit 100 that controls the operation of the entire apparatus. The control unit 100 has a CPU (Central Processing Unit) 105, a ROM (Read Only Memory) 110, and a RAM (Random Access Memory) 115. The CPU 105 executes desired processes such as a film forming process, a monitoring process, a determination process, an etching process, and first to third detection processes, which will be described later, according to various recipes stored in these storage areas. The recipes include process time, pressure (gas exhaust), high frequency power and voltage, various gas flow rates, temperature inside the processing vessel 10 (upper electrode temperature, sidewall temperature of the processing vessel, electrostatic chuck temperature, etc.), and temperature of the chiller 107, which are control information for the apparatus with respect to process conditions. Note that these programs and recipes indicating the processing conditions may be stored in a hard disk or a semiconductor memory. Also, the recipes may be set in a predetermined position in the storage area while being stored in a portable computer-readable storage medium such as a CD-ROM or DVD.

[0034] The control unit 100 executes a monitor process (described later) for making the first sensor 108a monitor the state of plasma in the processing vessel 10. The control unit 100 also executes a determination process (described later) for determining whether or not the film forming process needs to be re-executed based on the detection result of the first sensor 108a and for determining the processing conditions for the re-execution. The control unit 100 also detects the pattern shape of the wafer W based on the detection result of the second sensor 108b and executes first to third detection processes (described later).

[0035] During plasma processing, the opening and closing of the gate valve G is controlled, and the wafer W is loaded into the processing vessel 10 and placed on the mounting table 20. A direct current is supplied from a direct current voltage source 112 to the chuck electrode 106a, whereby the wafer W is attracted to and held by the electrostatic chuck 106 by Coulomb force.

[0036] Next, a gas for plasma processing, a high frequency power HF for plasma excitation, and a high frequency power LF for bias are supplied into the processing chamber 10 to generate plasma. The generated plasma performs plasma processing (e.g., film formation, etching) on ​​the wafer W.

[0037] After the plasma processing, a DC voltage HV having a polarity opposite to that during the attraction of the wafer W is applied from the DC voltage source 112 to the chuck electrode 106a to remove the charge on the wafer W, and the wafer W is peeled off from the electrostatic chuck 106. The opening and closing of the gate valve G is controlled, and the wafer W is unloaded from the processing vessel 10.

[0038] (ALD and subconformal ALD) In this embodiment, a process using plasma is performed as the film formation process. The film formation process is not particularly limited as long as it is a process using plasma. For example, the above-mentioned PEALD, PECVD, PECCVD, etc. can be used.

[0039] First, ALD and sub-conformal ALD will be described with reference to Figs. 3 to 5. Fig. 3 is a flowchart showing an outline of a plasma processing flow according to an embodiment. The processing flow shown in Fig. 3 is common to both ALD and sub-conformal ALD. Fig. 4 is a diagram for explaining an example of a flow of sub-conformal ALD. Fig. 5 is a diagram for explaining another example of a flow of sub-conformal ALD.

[0040] First, a wafer W having a pattern formed thereon is provided in the processing vessel 10 (step S11). The wafer W is automatically loaded into the processing vessel 10 through the gate valve G by the transfer robot Rb2. Then, a first gas (also called a precursor) is introduced from the gas supply source 15 into the processing vessel 10 in which the wafer W is placed (step S12). A first component contained in the first gas is adsorbed on the surface of the wafer W. Then, the inside of the processing vessel 10 is evacuated (purged) by the exhaust device 65 (step S13). Next, a second gas (also called a reactive gas) containing a second component that reacts with the first component is introduced from the gas supply source 15 into the processing vessel 10, and plasma of the second gas is generated (step S14). The second component reacts with the first component on the wafer W to form a film. Then, the inside of the processing vessel 10 is evacuated again by the exhaust device 65 (step S15). After the film formation in steps S12 to S15, the control unit 100 causes each unit to further execute a process such as etching (step S16). Then, the control unit 100 causes each unit of the plasma processing apparatus 1 to finish the processing.

[0041] In the above description, each process is performed in one plasma processing device 1. However, if the plasma processing system 1000 has multiple plasma processing devices 1010, the film formation process and the etching process may be performed in different plasma processing devices 1010.

[0042] In ALD, a film is formed by self-regulating adsorption and reaction of a specific component with a substance that is already present on the substrate surface. For this reason, ALD usually achieves conformal film formation by providing a sufficient processing time. In the case of FIG. 3, the processing time of steps S12 and S14 is made sufficiently long. In other words, the processing conditions of steps S12 and S14 are set to saturation conditions. As a result, the adsorption of the first gas component to the wafer W and the reaction between the first gas component and the second gas component reach saturation on the wafer W surface, forming a conformal film. A conformal film is a film that has a uniform thickness regardless of the position on the wafer W (e.g., the vertical position).

[0043] In contrast, subconformal ALD uses a process procedure similar to ALD, but controls at least one of the adsorption and reaction of the film-forming components so that they do not reach saturation. In other words, subconformal ALD uses a process procedure similar to ALD, but forms a subconformal film by not completing the self-limiting adsorption or reaction on the surface of the wafer W. A subconformal film is a film whose thickness varies depending on the position on the wafer W (e.g., the vertical position).

[0044] There are at least two types of processing modes for sub-conformal ALD: (1) The precursor is adsorbed onto the entire surface of the wafer W. The reaction gas introduced thereafter is controlled so as not to permeate the entire surface of the wafer W. (2) The precursor is adsorbed only to a portion of the surface of the wafer W. The reactive gas that is then introduced forms a film only on the surface portion where the precursor is adsorbed. By using the above method (1) or (2), a film whose thickness gradually decreases from top to bottom can be formed on the sidewall of the pattern formed on the wafer W.

[0045] 4 includes an etching target film EL1 and a mask MA. A recess having an opening OP is formed in the laminate of the etching target film EL1 and the mask MA.

[0046] First, a wafer W is provided in a processing vessel 10 (step S11 in FIG. 3). Then, a precursor P is introduced into the processing vessel 10 in which the wafer W is placed ((A) in FIG. 4, step S12 in FIG. 3). By providing a sufficient processing time for the precursor P to be adsorbed, the precursor P is adsorbed on the entire surface of the wafer W ((B) in FIG. 4). When the adsorption of the precursor P is completed, the processing vessel 10 is purged. Next, a reaction gas R is introduced into the processing vessel 10 ((C) in FIG. 4, step S14 in FIG. 3). The introduced reaction gas R reacts with the precursor P on the wafer W to gradually form a film F from above the mask MA. Here, before the formation of the film F reaches below the etching target film EL1, the reaction gas R is purged. By processing in this manner, while using the ALD technique, the film F can be formed only on the mask MA and the upper part of the etching target film EL1, rather than on the entire sidewall of the recess ((D) in FIG. 4). In FIG. 4D, film F is formed on the upper sidewalls and top of the recess, but not on the lower sidewalls and bottom.

[0047] Next, the second method will be described with reference to Fig. 5. The wafer W shown in Fig. 5 has the same shape as the wafer W in Fig. 4.

[0048] In the example of Fig. 5, the precursor P is adsorbed only to the upper part of the wafer W (Fig. 5(A)). After the precursor P is purged, the reactive gas R is introduced into the processing vessel 10 (Fig. 5(B)). At this time, the reactive gas R reacts and forms a film only at the position where the precursor P is adsorbed, so that a film F is formed only above the pattern on the wafer W (Fig. 5(C)).

[0049] (Processing conditions for selective adsorption and reaction) Fig. 4 shows a case where step S14 in Fig. 3 is executed under a non-saturated condition, and Fig. 5 shows a case where step S12 in Fig. 3 is executed under a non-saturated condition.

[0050] If the processing times of steps S12 and S14 are made long enough, the film formed will be conformal rather than subconformal. For this reason, in subconformal ALD, the processing conditions are set so that at least one of the adsorption and reaction of the film-forming components does not reach saturation.

[0051] The process parameters adjusted to realize subconformal ALD include, for example, the temperature of the mounting table 20 on which the wafer W is placed, the pressure in the process chamber 10, the flow rate and introduction time of the precursor to be introduced, the flow rate and introduction time of the reactive gas to be introduced, the process time, etc. In addition, in the case of a process using plasma, the film formation position can also be adjusted by adjusting the value of the radio frequency (RF) power applied to generate plasma. In the process of Fig. 3, the second gas is turned into plasma in step S14, but the first gas in step S12 may also be turned into plasma.

[0052] (Example of flow of plasma processing method according to one embodiment) 6 is a flow chart for further illustrating the plasma processing method according to one embodiment. The plasma processing method according to this embodiment monitors the state of plasma generated during the film formation process (steps S12 to S15 in FIG. 3) to realize highly accurate determination of the end timing of the film formation process.

[0053] First, a wafer W is provided in the processing vessel 10 (step S61). A pattern is formed on the wafer W in advance. For example, recesses similar to those shown in FIGS. 4 and 5 are formed. Note that, if both etching and film formation can be performed in the plasma processing apparatus 1, the formation of the recesses may also be performed in the plasma processing apparatus 1.

[0054] Next, the plasma processing apparatus 1 executes a first detection process (step S62). In the first detection process, the second sensor 108b or the observation device OC detects the pattern shape on the wafer W, and the control unit 100 determines the process conditions for the subsequent film formation process (step S63) based on the detection result. The pattern shape includes the aspect ratio of the recess and the surface profile. The first detection process may be performed before or after the step of providing the wafer W (step S61), as long as it is performed before the film formation process (step S63). The process conditions for the film formation process (step S63) include, for example, the amount of the first gas introduced, the amount of the second gas introduced, the reaction time between the first gas and the second gas, the purge time, and the number of cycles. The first detection process will be described later.

[0055] The control unit 100 sends instructions to each unit of the plasma processing apparatus 1 based on the processing conditions determined by the first detection process, and starts the film formation process (step S63). First, the control unit 100 introduces a first gas from the gas supply source 15 into the processing vessel 10 (step S631). When the processing time determined by the processing conditions has elapsed, the control unit 100 stops the introduction of the first gas. The first gas is adsorbed onto the surface of the wafer W on the mounting table 20.

[0056] Next, the control unit 100 controls the exhaust device 65 to purge the gas inside the processing chamber 10 (step S632).

[0057] Next, the control unit 100 introduces the second gas from the gas supply source 15 into the processing vessel 10 (step S633). The control unit 100 also controls the first high frequency power supply 34 to apply high frequency power HF for plasma excitation to the gas shower head 25. The control unit 100 also controls the second high frequency power supply 32 to apply high frequency power LF to the mounting table 20. The high frequency power HF may also be applied to the mounting table 20. By applying the high frequency powers LF and HF, plasma of the second gas is generated in the processing vessel 10. Then, when the processing time based on the processing conditions determined by the first detection process has elapsed, the control unit 100 ends the introduction of the second gas and the generation of the plasma. The components contained in the plasma of the second gas react with the components of the first gas on the surface of the wafer W to form a film on the surface of the wafer W.

[0058] During the introduction of the second gas, the control unit 100 executes a monitoring process in parallel (step S64A). In the monitoring process, the first sensor 108a monitors the state of plasma in the processing vessel 10, and transmits and stores the monitoring result to the control unit 100. The details of the monitoring process will be described later.

[0059] Next, the control unit 100 controls the exhaust device 65 to purge the gas inside the processing chamber 10 (step S634). This completes one cycle of the film forming process (step S63).

[0060] The control unit 100 then executes a determination process (step S64B) based on the monitoring results of the monitoring process (step S64A). The determination process is a process in which the control unit 100 determines the subsequent process and the process conditions based on the monitoring results transmitted from the first sensor 108a. The determination process may be executed for each cycle of the film formation process (step S63), or may be executed after the film formation process (step S63) has been executed a predetermined number of cycles.

[0061] In the determination process, the control unit 100 determines whether or not to re-execute the film formation process. If the control unit 100 determines to re-execute the film formation process, it determines whether to repeat the process from the introduction of the first gas (step S631) or from the introduction of the second gas (step S633). If the control unit 100 determines to re-execute the film formation process, it selects the process conditions for the film formation process (step S63).

[0062] In FIG. 6, the determination process (step S64B) is executed after the purging (step S634), but the determination process (step S64B) may be executed before the purging or in parallel with the purging.

[0063] The control unit 100 continues the process based on the determination result in the determination process. If it is determined to repeat from step S631 (step S64B, repeat S631), the control unit 100 repeats the above-mentioned processes of steps S631 to S634. On the other hand, if it is determined to repeat from step S633 (step S64B, repeat S633), the control unit 100 repeats the above-mentioned processes of steps S633 to S634. Also, if it is determined not to re-execute the film forming process (step S64B, no re-execution), the control unit 100 proceeds to the second detection process (step S65).

[0064] In the second detection process, similarly to the first detection process, the second sensor 108b or the observation device OC detects the pattern shape on the wafer W, and the control unit 100 determines the subsequent process (film formation process (step S63) or etching (step S66)) and the process conditions based on the detection result. The process conditions for etching (step S66) include the amount of etching gas introduced, the high frequency power, the substrate temperature, etc. The second detection process will be described later.

[0065] If it is determined in the second detection process that the film formation process is to be re-executed (step S65, re-execution), the control unit 100 returns to step S63 and repeats the process. On the other hand, if it is determined in the second detection process that the film formation process is not to be re-executed (step S65, no re-execution), the control unit 100 causes etching to be performed under the determined processing conditions (step S66). At this time, the control unit 100 may perform a monitor process in parallel, as in the case of introducing the second gas.

[0066] When etching is completed, the control unit 100 executes a third detection process (step S67). In the third detection process, similar to the first and second detection processes, the second sensor 108b or the observation device OC detects the pattern shape on the wafer W, and the control unit 100 determines the subsequent process and the process conditions based on the detection result. The third detection process will be described later.

[0067] If it is determined in the third detection process that the film formation process is to be re-executed (step S67, re-execute film formation), the control unit 100 returns to step S63 and repeats the process. Also, if it is determined in the third detection process that the etching process is to be re-executed (step S67, re-execute etching), the control unit 100 returns to step S66 and repeats the process. On the other hand, if it is determined in the third detection process that the film formation process and the etching process are not to be re-executed (step S67, not to be re-executed), the control unit 100 ends the process. This ends the plasma processing of this embodiment.

[0068] (Monitoring / Decision-making) Next, the monitoring process in step S64A and the determination process in step S64B will be described. FIG. 7 is a flowchart for describing the monitoring process and the determination process according to an embodiment. In the plasma process according to this embodiment, the control unit 100 monitors the state of the plasma generated during the film formation process by the monitoring process. Then, the control unit 100 executes a determination process for determining the timing to end the film formation process based on the result of the monitoring process.

[0069] As described above, the monitor process (step S64A) is performed in parallel with the process of introducing the second gas into the processing vessel 10 and generating plasma in the film forming process (step S63). Here, the monitor process is assumed to start when the processing of one wafer W starts.

[0070] When the control unit 100 starts processing the wafer W, it causes the first sensor 108a to start a monitoring process. When the second gas is introduced into the processing vessel 10 and step S633 starts, the first sensor 108a detects the state of plasma in the processing vessel 10 (step S71). The timing at which the first sensor 108a starts its operation is not particularly limited, and the control unit 100 may control the first sensor 108a to start processing based on the processing recipe for the wafer W. In the monitoring process, the first sensor 108a monitors, for example, the amount of radicals generated by plasma generation of the second gas.

[0071] Incidentally, the coverage of the film formed on the pattern in the film formation process is determined by the temperature in the processing vessel 10, the aspect ratio of the pattern to be processed, and the dose of radicals generated in the processing vessel 10. In the film formation process of the embodiment, the temperature in the processing vessel 10 is controlled by predetermined processing conditions, and the aspect ratio of the pattern can be derived in advance from a design value. Therefore, if the dose of radicals during the film formation process is known, the coverage of the film formed by the film formation process can be estimated. Note that the coverage here refers to the state of the film, including the thickness and position of the film to be formed. For example, the coverage means the change in film thickness according to the aspect ratio.

[0072] The amount of radicals contained in plasma can be estimated from the plasma's electron density, ion density, etc. Therefore, instead of directly monitoring the amount of radicals, it is sufficient to monitor other physical quantities that indicate the plasma state. Physical quantities that indicate the plasma state include electron density, ion density, molecular and radical density, and atomic and molecular ion masses.

[0073] These physical quantities that indicate the state of plasma can be measured by spectroscopy (including those using lasers), interference and reflection methods, etc. Spectroscopy can be performed using emission spectroscopy, which measures radiant flux, emission spectrum intensity, continuous spectrum intensity, etc. Absorption spectroscopy can also be performed, such as total absorption, self-absorption, and hook method. Spectroscopy using lasers can also be used. For example, laser organic fluorescence, laser absorption spectroscopy, and laser scattering methods can be used. Microwave interference / reflection, laser interferometry / polarization, and Schlieren / shadowgraphy can also be used.

[0074] The first sensor 108a is a detection device capable of monitoring a physical quantity indicating the state of the plasma. As long as the physical quantity indicating the state of the plasma can be monitored, the specific configuration of the first sensor 108a is not particularly limited. For example, an optical emission spectroscopy (OES) sensor may be used as the first sensor 108a. Also, a super-high resolution image sensor may be used as the first sensor 108a. Then, the control unit 100 may analyze information acquired by the first sensor 108a, such as an image, to calculate the physical quantity.

[0075] The first sensor 108a monitors a physical quantity indicating the state of the plasma generated during the process of step S633, and transmits the monitoring result to the control unit 100. The control unit 100 stores the received monitoring result in association with the timing.

[0076] The control unit 100 determines whether the film formation process (steps S631 to S634) has ended (step S72). If it has been determined that the film formation process has not ended (step S72, No), the control unit 100 returns to step S71 and continues the monitoring process by the first sensor 108a. On the other hand, if it has been determined that the film formation process has ended (step S72, Yes), the control unit 100 proceeds to step S73 and executes the determination process.

[0077] (Decision making process) In the determination process, the control unit 100 calculates an integral value of the physical quantity at each timing obtained by the monitoring process. The physical quantity obtained by the monitoring process is stored in the control unit 100 in association with the timing. FIG. 8 is a diagram for explaining the monitoring result obtained in the monitoring process according to an embodiment. In the example of FIG. 8, the first sensor 108a monitors the amount of radicals in the plasma at every predetermined time (t1, t2, t3, . . .) and sends the amount of radicals to the control unit 100 as a numerical value. Here, the monitored amount of radicals changes along the curve of FIG. 8. The control unit 100 calculates the integral value of the monitoring result from the start of the processing of the wafer W to that time point. In the example of FIG. 8, the control unit 100 calculates a value obtained by adding up S1, S2, S3, . . .

[0078] Next, the control unit 100 determines whether the calculated integral value is equal to or greater than a predetermined value (step S73). Here, the "predetermined value" is calculated in advance as the amount of radicals required to reach a desired coverage based on the aspect ratio of the pattern on the wafer W, the temperature inside the processing vessel 10, and the desired coverage.

[0079] When the control unit 100 determines that the calculated integral value is equal to or greater than the predetermined value (Yes in step S73), it ends the film forming process (step S74). That is, the control unit 100 proceeds to the "No re-execution" branch in step S64B of FIG. 6, and then executes step S65.

[0080] On the other hand, when the control unit 100 determines that the calculated integral value is less than the predetermined value (step S73, No), it determines the processing conditions when re-executing the film forming process (step S75). The determined processing conditions may include the processing time when steps S631 and S633 are re-executed. For example, if the processing time of steps S631 and S633 to be executed next is set to the same length as the previous time based on the integral value calculated in step S73, and the desired coverage is exceeded, the control unit 100 sets the processing time of steps S631 and S633 to be shorter. The determined processing conditions may also include a determination of whether to start the re-execution from step S631 or from step S633. Then, the control unit 100 re-executes the film forming process under the determined processing conditions (step S76). Then, the control unit 100 proceeds to step S631 or step S633 depending on the determined processing conditions.

[0081] In addition, since the control unit 100 determines the progress of the film formation process on the wafer W using the above-mentioned integral value, it can determine the processing conditions after the plasma processing device 1 is restored if the plasma processing device 1 is forcibly terminated during processing, for example.

[0082] (Monitoring method example 1 of first sensor 108a) Incidentally, the first sensor 108a may monitor the state of plasma at a point, on a surface, or three-dimensionally. Next, an example of a monitoring method in the monitoring process will be described.

[0083] 2, a first example of a method for detecting a physical quantity in a monitor process according to an embodiment uses an image obtained by disposing a first sensor 108a on a side surface of the processing vessel 10 and monitoring the state of plasma from the side surface of the processing vessel 10. The first sensor 108a is, for example, a super-high resolution image sensor.

[0084] In the first method example, the plasma is displayed in the obtained image as a whitish object that gradually spreads in the processing space over time. The spread and intensity of the plasma correspond to the saturation and brightness of the white parts in the image. Therefore, the control unit 100 can obtain a value indicating the state of the plasma by analyzing the brightness and saturation of the white parts in the obtained image.

[0085] The first sensor 108a transmits the acquired image to the control unit 100. The control unit 100 analyzes the received image and converts the plasma state into a numerical value based on the saturation, brightness, etc. of the image. Then, the control unit 100 compares the integral value of the calculated numerical value with a predetermined threshold value ("predetermined value" in FIG. 7). By performing this processing, the control unit 100 can estimate the film formation state on the wafer W based on the plasma state near the wafer W placed in the processing vessel 10 and determine the end timing of the film formation process.

[0086] (Monitoring method example 2 of first sensor 108a) 2, the first sensor 108a may be disposed to monitor the processing space near the wafer W from above and below the processing vessel 10. FIG 9A is a diagram for explaining a second example method for detecting a physical quantity in a monitor process according to an embodiment.

[0087] As shown in Fig. 9A, in the second technique example, the first sensor 108a monitors the entire surface of the wafer W from above. In the image shown in Fig. 9A, a portion R1 having a relatively large amount of radicals is displayed with a dark pattern, and a portion R2 having a relatively small amount of radicals is displayed with a light pattern. The first sensor 108a acquires such an image at predetermined time intervals (e.g., every 50 nanoseconds). Then, the first sensor 108a transmits the acquired image to the control unit 100.

[0088] The control unit 100 analyzes the image received from the first sensor 108a and digitizes the color shading corresponding to the amount of radicals. FIG. 9B is a diagram showing an example of digitizing the image obtained by the method example 2 of FIG. 9A. In the example shown in FIG. 9B, values ​​1, 2, and 3 obtained by digitizing the color shading are displayed at positions corresponding to the areas R1 and R2 of FIG. 9A. The control unit 100 first divides the area including the surface of the wafer W into multiple areas of uniform size. Then, the control unit 100 analyzes and digitizes the image corresponding to each area. This allows the control unit 100 to obtain the integral value of the value representing the state of plasma for each area of ​​each image.

[0089] 9A and 9B, when the wafer W surface is divided into a plurality of areas and a numerical value representing the plasma state in each area is obtained, the control unit 100 can determine the film formation state for each position in the wafer W surface. Therefore, the control unit 100 can use the results of the monitoring process to improve the in-surface uniformity of the plasma processing. For example, depending on the results of the monitoring process, the control unit 100 can adjust the high-frequency power applied to the mounting table 20 and the gas shower head, which are processing conditions for the subsequent processing, to different values ​​depending on the position in the surface.

[0090] Fig. 10 is a flowchart showing an example of the flow of the monitoring process based on the technique example 2 of Fig. 9A and Fig. 9B. In the example of Fig. 10, first, when the monitoring process starts, the first sensor 108a starts monitoring the plasma state, and transmits the acquired information to the control unit 100 for storage (step S1101). At this time, the first sensor 108a monitors the entire surface of the wafer W.

[0091] The control unit 100 analyzes the received information, e.g., an image, and calculates a value indicating the state of plasma for each of the multiple areas set in advance (step S1102).The control unit 100 then calculates an integral value for the film formation process performed up to that point for each of the multiple areas based on the calculated value (step S1103).Furthermore, the control unit 100 calculates the difference between the calculated integral values ​​for the multiple areas (step S1104).

[0092] Next, the control unit 100 judges whether the integral value calculated in step S1103 is equal to or greater than a predetermined value (step S1105). If it is judged to be equal to or greater than the predetermined value (step S1105, Yes), the control unit 100 judges whether the difference calculated in step S1104 is equal to or less than a predetermined value (step S1106). If it is judged to be equal to or less than the predetermined value (step S1106, Yes), the control unit 100 ends the film forming process (step S1107). Then, the control unit 100 proceeds to step S65.

[0093] On the other hand, when the control unit 100 determines that the integral value calculated in step S1103 is less than the predetermined value (step S1105, No), it determines the process conditions for re-executing the film formation process (step S1108). Then, it causes the film formation process to be executed based on the determined process conditions (step S1109). In this case, the film formation process is re-executed based on the process conditions determined in step S1108 and the process step to be re-executed (S631 or S633).

[0094] On the other hand, when the control unit 100 determines that the difference calculated in step S1104 is greater than the predetermined value (step S1106, No), it determines processing conditions for offsetting the difference in order to improve the in-plane uniformity (step S1110). Then, the control unit 100 causes the film formation process to be executed again based on the determined processing conditions (step s1109). After this, the process proceeds to step S631 or S633. This ends the monitoring process of the second method example.

[0095] In this manner, according to the plasma processing of this embodiment, by monitoring the state of plasma in the processing vessel 10, it is possible to estimate the film formation state without inspecting the pattern itself on the wafer W. Therefore, the plasma processing apparatus 1 according to this embodiment can accurately and simply determine the timing to end the film formation process.

[0096] Next, the first to third detection processes will be described. Here, the detection in the first to third detection processes will be described as being performed by the second sensor 108b. However, the detection in the first to third detection processes may be performed by the observation device OC by transporting the wafer W to the observation module OM shown in FIG.

[0097] (First detection process) The first detection process includes a process in which the second sensor 108b detects the shape and dimensions of a pattern on the wafer W, and a process in which the control unit 100 determines processing conditions for a subsequent process based on the detection result of the second sensor 108b.

[0098] The second sensor 108b optically detects the shape and dimensions of the pattern on the wafer W. There is no particular limitation on the detection method used by the second sensor 108b. The detection result by the second sensor 108b is transmitted to the control unit 100 and stored in a storage unit such as the ROM 110 or the RAM 115.

[0099] When the control unit 100 receives the detection result, it compares the detection result with a predetermined pattern dimension. Then, it calculates the difference between the predetermined pattern dimension and the detected dimension. Based on the calculated difference, the control unit 100 adjusts the processing conditions for the subsequent processing. Then, the control unit 100 determines the processing conditions to be used in the subsequent processing.

[0100] If the pattern formed on the wafer W deviates from the design value when the wafer W is placed in the processing vessel 10, there is a high possibility that the state of the film finally formed will deviate from the design value if the subsequent processing is performed under the designed processing conditions. Therefore, in this embodiment, in the first detection process, the processing conditions are adjusted based on the difference between the design value and the actual measurement value.

[0101] (Second detection process) The second detection process includes a process in which the second sensor 108b detects the shape and dimensions of a pattern on the wafer W, and a process in which the control unit 100 determines a subsequent process and process conditions based on the detection result of the second sensor 108b.

[0102] The detection process of the second sensor 108b in the second detection process is the same as the detection process in the first detection process. However, when the second detection process is performed, the film formation process is completed, so the pattern shape formed on the wafer W is different from that in the first detection process. Furthermore, in the process of the control unit 100, the predetermined pattern dimensions to be compared with the detection result are also different from those in the first detection process.

[0103] When the control unit 100 receives the detection result, it compares the detection result with a predetermined pattern dimension. Then, it calculates the difference between the predetermined pattern dimension and the detected dimension. Based on the calculated difference, the control unit 100 determines whether or not to re-execute the film formation process (step S63). For example, if the calculated difference is equal to or greater than a threshold value, the control unit 100 determines to re-execute the film formation process. On the other hand, if the calculated difference is less than the threshold value, the control unit 100 determines not to re-execute the film formation process.

[0104] If it is determined that the film formation process is not to be performed again, the control unit 100 then determines the process conditions for the subsequent etching (step S66). For example, if the numerical value of the film thickness formed on the pattern obtained from the detection result is greater than a set value, the process conditions are adjusted so that the effect of etching is enhanced. Then, the control unit 100 determines the adjusted process conditions as the process conditions for etching (step S66).

[0105] If the second sensor 108b used in the second detection process is an infrared sensor or the like, the second sensor 108b can directly measure the thickness of the film formed on the pattern. In this case, the control unit 100 compares the detection result by the second sensor 108b with a predetermined film thickness and calculates the difference. Then, based on the calculated difference, the control unit 100 determines whether or not to re-execute the film forming process (step S63). Then, the control unit 100 determines the subsequent process and the process conditions.

[0106] (Third detection process) The third detection process includes a process in which the second sensor 108b detects the shape and dimensions of a pattern on the wafer W, and a process in which the control unit 100 determines a subsequent process and processing conditions based on the detection result of the second sensor 108b.

[0107] The detection process of the second sensor 108b in the third detection process is the same as the detection process in the first and second detection processes. However, when the third detection process is performed, the film formation process and the etching process are completed, so the pattern shape formed on the wafer W is different from that in the first and second detection processes. Furthermore, in the process of the control unit 100, the predetermined pattern dimensions to be compared with the detection result are also different from those in the first and second detection processes.

[0108] When the control unit 100 receives the detection result, it compares the detection result with a predetermined pattern dimension. Then, it calculates the difference between the predetermined pattern dimension and the detected dimension. The control unit 100 determines whether or not to re-execute the film formation process (step S63) based on the calculated difference. For example, if the calculated difference is equal to or greater than a threshold value and the detected dimension is smaller than the predetermined pattern dimension, the control unit 100 determines to re-execute the film formation process. On the other hand, if the calculated difference is less than the threshold value, the control unit 100 determines not to re-execute the film formation process. In addition, the control unit 100 determines whether or not to re-execute the etching process (step S66) based on the calculated difference. For example, if the calculated difference is equal to or greater than a threshold value and the detected dimension is larger than the predetermined pattern dimension, the control unit 100 determines to re-execute the etching process.

[0109] When it is determined that the film formation process is to be re-executed, the control unit 100 then determines the process conditions for the film formation process. For example, the process conditions are determined so that the difference between the pattern shape obtained from the detection result and the predetermined pattern dimensions is small. Then, the control unit 100 executes the film formation process using the determined process conditions (FIG. 6, step S67, "Re-execute film formation").

[0110] Furthermore, when it is determined that the etching process is to be re-executed, the control unit 100 then determines the process conditions for the etching process. For example, the process conditions are determined so that the difference between the pattern shape obtained from the detection result and the predetermined pattern dimensions is small. Then, the control unit 100 executes the etching process using the determined process conditions (FIG. 6, step S67, "re-execute etching"). When it is determined that neither the film formation process nor the etching process is to be re-executed (FIG. 6, step S67, "no re-execution"), the control unit 100 ends the process.

[0111] The first, second and third detection processes may be performed using the same detection unit, such as the second sensor 108b or the observation device OC, or a different detection unit may be used for each process. The determination process may be performed by the control unit 100, or the first sensor 108a may be provided with a determination function and transmit a numerical value and a timestamp to the control unit 100.

[0112] FIG. 11 is a diagram showing an example of information stored in a storage unit in a plasma process according to an embodiment. In the example shown in FIG. 11(A), the results detected in the first detection process, the second detection process, and the third detection process are stored in association with a "time stamp." Here, the detection results may be specific dimensions. Also, shape abnormalities may be categorized into a plurality of types in advance, and the type to which the detection result corresponds may be stored. In FIG. 11(A), the detection results are categorized and stored as "dimension A," "dimension B," and the like. Also, the results of the monitoring process may be associated with a time stamp and a numerical value associated with a plurality of time stamps may be stored each time step S633 is executed once. Also, if the first sensor 108a is an image sensor, a plurality of images themselves may be stored. In FIG. 11(A), a value "V1" obtained by digitizing and integrating a plurality of images acquired in step S633 is stored as the monitoring result. Also, in FIG. 11(A), the results of the first to third detection processes and the judgment process are stored as the "judgment result." For example, in the first detection process, the process condition "X" of the subsequent process is stored. Also, for example, in the second detection process, "rerun" indicating rerun of the film formation process and the process condition "Y" at the time of rerun are stored. "Y" also includes information specifying the step at which the process is to be performed. Also, in the third detection process, "no rerun" indicating that neither etching nor film formation is to be rerun is stored. Also, since there is no rerun, the process condition column is stored as "NA" (not applicable). Also, "rerun" and "condition X" are stored in association with the monitor process "V1". This indicates that in the determination process, the film formation process is to be rerun and the process condition is "X".

[0113] Also, (B) of Fig. 11 is an example of a configuration when dimensions and threshold values ​​to be compared with the detection result in each process are stored in the storage unit. For example, in the first detection process, the detection result is compared with "dimension AA" to determine the processing conditions for the subsequent process. Note that Fig. 11 is only an example, and the configuration of information stored in the storage unit for executing the first to third detection processes, the monitor process, and the determination process is not particularly limited.

[0114] (Modification) In the above embodiment, the detection result of the first detection process (step S62), the monitor result of the monitor process (step S64), the detection result of the second detection process (step S65), and the detection result of the third detection process (step S67) are used to adjust the processing conditions for the wafer W on which the processing has been performed and to determine whether each processing needs to be performed again. However, these detection results and monitor results can be applied to the wafer W' to be processed after the wafer W, in addition to the wafer W on which the processing has been performed. That is, a series of processes (steps S61 to S67) are performed on the wafer W, and data on the shape of the recess before the film formation process, the state of the plasma in the film formation process, the state of the film formed by the film formation process, the state of the film after etching, the shape of the pattern, etc. are obtained, and the correlations between these are obtained. In one example, the correlation between the shape of the recess before the film formation process, the state of the plasma in the film formation process, and the state of the film formed by the film formation process is obtained. In another example, the correlation between the state of the plasma in the film formation process, the state of the film formed by the film formation process, and the state of the film after etching and the shape of the pattern is obtained. These correlations can be stored as physical models in a memory unit in the control unit Cnt. Then, based on these physical models, the conditions for the film formation process (step S63) or etching (step S66) are modified, and the modified conditions are applied to the processing of the substrate W'. In one example, the physical model is constructed by repeating a cycle including execution of the processing, acquisition of the correlations, and modification of the conditions. The construction of the physical model may be performed by machine learning. According to such a modified example, the processing of the wafer W' can be performed in a shorter time and with higher accuracy than the processing of the wafer W.

[0115] (Effects of the embodiment) The plasma processing method according to the embodiment includes steps a), b), c), and d). In step a), a substrate having a recess is provided in a processing vessel. In step b), plasma is generated in the processing vessel to form a film on the recess. In step c), the state of the plasma generated in step b) is monitored. In step d), whether or not step b) needs to be re-executed and the processing conditions at the time of re-execution are determined based on the monitored state of the plasma. Therefore, according to the plasma processing method according to the embodiment, it is possible to estimate the film formation state and determine whether or not the film formation process needs to be re-executed and the processing conditions suitable for re-execution without the need to check the pattern on the substrate itself. In addition, according to the present plasma processing method, since the state of the plasma during the film formation process is monitored, the film formation state can be estimated without carrying the substrate out of the processing vessel. Therefore, according to the present plasma processing method, the end timing of the film formation process can be easily determined with high accuracy. Therefore, according to the present plasma processing method, the performance of the film formation process using plasma can be stabilized.

[0116] Moreover, in the plasma processing method according to the above embodiment, step b) may include steps b-1) and b-2). In step b-1), a first gas may be introduced into the processing vessel and adsorbed onto the recesses. In step b-2), a second gas may be introduced into the processing vessel, and plasma of the second gas may be generated to react with the components of the first gas adsorbed onto the recesses to form a film. Then, step c) may monitor the state of the plasma generated in step b-2). In this way, the plasma processing method according to the embodiment can be applied to a film formation process, such as ALD, which is realized in two steps, adsorption of the first gas and reaction of the second gas.

[0117] In addition, in the plasma processing method according to the above embodiment, the step b) may be terminated before the reaction between the components of the first gas and the components of the second gas on the entire surface of the recessed portion becomes saturated. In this manner, the plasma processing method according to the above embodiment can be used to determine the end timing of the film formation process in sub-conformal ALD. Therefore, according to the plasma processing method according to the embodiment, the end timing of the film formation process can be estimated with high accuracy, and the film formation process can be terminated before the film formed in sub-conformal ALD reaches a saturated state.

[0118] In the plasma processing method according to the above embodiment, step c) may monitor a physical quantity indicating the state of the plasma. Then, step d) may determine to re-execute step b) when the integral value of the physical quantity obtained by the monitor is less than a predetermined value. Therefore, according to the plasma processing method according to the above embodiment, the state of the film formed from the start of the process to that point in time can be estimated with high accuracy based on the integral value of the physical quantity obtained by the monitor during the film formation process. Therefore, according to the embodiment, even if the film formation process is interrupted for some reason, the film formation state at that point in time can be estimated based on the monitor result, and the film formation process can be resumed to make up for the deficiency.

[0119] In the plasma processing method according to the above embodiment, the step c) may monitor the amount of radicals in the plasma generated in the step b). The amount of radicals can be calculated based on, for example, electron density, ion density, etc. In addition, when the temperature in the processing vessel and the pattern shape on the substrate to be processed are known, the film formation state can be estimated based on the amount of radicals. Therefore, according to the above embodiment, the film formation state on the substrate can be easily estimated using physical quantities that can be obtained by an optical emission spectroscopic sensor, etc.

[0120] In the plasma processing method according to the above embodiment, step c) may monitor the state of plasma in each of a plurality of areas set in the substrate placement surface. Step d) may determine to re-execute step b) when an integral value of a physical quantity indicating the state of plasma in each of the plurality of areas is less than a predetermined value. Therefore, according to the above embodiment, the film formation state in each area in the substrate surface can be estimated to determine whether or not to re-execute the film formation process.

[0121] In the plasma processing method according to the above embodiment, step c) may monitor the state of plasma in each of a plurality of areas set in the substrate placement surface. Then, step d) may compare physical quantities indicating the state of plasma in each of the plurality of areas, and determine to re-execute step b) when the difference is greater than a predetermined value. Therefore, according to the above embodiment, the film formation process can be re-executed so that the film formation state is uniform for each area in the substrate surface. Therefore, the plasma processing method according to the above embodiment can improve the in-surface uniformity of the film formation process.

[0122] Moreover, the plasma processing method according to the above embodiment may further include a step e) and a step f). In the step e), the state of the film on the recess is detected after the execution of the step b). In the step f), the step b) is executed again according to the detection result of the step e). Therefore, according to the plasma processing method according to the embodiment, not only the state of the plasma is monitored, but also the state of the film is detected to determine whether or not to execute the film formation process again. Therefore, according to the embodiment, the performance of the film formation process using plasma can be stabilized, and highly accurate film formation can be achieved.

[0123] Moreover, the plasma processing method according to the above embodiment may further include steps e), f), and g). In step e), a state of the film on the recess is detected after step b) is performed. In step f), processing conditions are determined according to the detection result of step e). In step g), an underlying layer of the layer on which the film is formed on the recess is etched using the layer on which the film is formed as a mask under the processing conditions determined in step f). Therefore, according to the embodiment, processing conditions for the subsequent etching can be adjusted according to the film formation result, and highly accurate pattern formation can be realized.

[0124] Moreover, the plasma processing method according to the above embodiment may further include step h). Step h) detects the shape of the pattern formed by etching after step g) is performed and / or the state of the film on the recess, and if the degree of coincidence between the detected shape and the predetermined shape is equal to or less than a predetermined value, step b) or step g) is performed again. Therefore, according to the embodiment, it is possible to determine whether or not to perform further etching depending on the shape after etching. Therefore, according to the embodiment, it is possible to realize highly accurate pattern formation.

[0125] Moreover, the plasma processing method according to the above embodiment may further include a step i) and a step j). In the step i), the shape of the recess is detected before the execution of the step b). In the step j), the processing conditions of the step b) are determined according to the detection result of the step i). Therefore, according to the embodiment, the processing conditions can be determined according to the state of the pattern on the substrate before the film formation or etching is performed. Therefore, according to the embodiment, the pattern formation with high accuracy can be realized.

[0126] The plasma processing method according to the embodiment may further include steps k), l), and m). In step k), a correlation between the shape of the recess before film formation, the state of plasma, and the state of the film formed in step b) is obtained based on the shape of the recess of the substrate before the execution of step b), the state of plasma monitored in step c), and the state of the recess of the substrate after the execution of step b). In step l), a processing condition in step b) is modified based on the obtained correlation. In step m), the modified processing condition is applied to a substrate (substrate to be processed next to the substrate) different from the substrate on which steps k), l), and m) are executed, and a plasma processing is performed. Therefore, according to the embodiment, the film formation conditions can be optimized every time a film formation process is executed on a substrate.

[0127] Moreover, the plasma processing method according to the embodiment may include a step n), a step o), a step p), and a step q). In the step n), the shape of the pattern formed by etching and / or the state of the film on the recessed portion are detected after the execution of the step g). In the step o), the correlation between the state of the film before and after the step g), the state of the plasma, and the shape of the pattern after the step g) is obtained based on the state of the film detected in the step e), the state of the plasma monitored in the step n), and the shape of the pattern and / or the state of the film on the recessed portion detected in the step o). In the step p), the processing conditions in the step g) are modified based on the obtained correlation. In the step q), a substrate different from the substrate on which the steps n), o), and p) are performed is etched under the modified processing conditions. Therefore, according to the embodiment, the etching conditions can be optimized every time a substrate is etched.

[0128] The plasma processing apparatus according to the embodiment includes one or more processing vessels and a control unit. At least one of the one or more processing vessels is configured to perform etching. At least one of the one or more processing vessels is configured to perform film formation. One processing vessel may be configured to perform etching and film formation. The processing vessel has a gas supply unit for supplying a processing gas therein. The control unit causes each unit to execute a plasma processing method including steps a), b), c), and d). The step a) provides a substrate having a recess in the processing vessel. The step b) generates plasma in the processing vessel to form a film on the recess. The step c) monitors the state of the plasma generated in the step b). The step d) determines whether or not to re-execute the step b) and the processing conditions at the time of re-execution based on the monitored state of the plasma. Therefore, the plasma processing apparatus according to the embodiment can stabilize the performance of the film formation process using plasma and realize high-precision pattern formation.

[0129] The application of the plasma processing method according to the above embodiment is not particularly limited as long as it is a substrate processing using plasma. The plasma processing method according to the above embodiment can be used in the manufacturing process of 3D NAND and DRAM. The plasma processing method according to the above embodiment can be used when processing high AR (aspect ratio) organic films, when processing masks for logic, etc.

[0130] The embodiments disclosed herein should be considered to be illustrative and not restrictive in all respects. The above-described embodiments may be omitted, substituted, or modified in various forms without departing from the scope and spirit of the appended claims. [Explanation of symbols]

[0131] 1. Plasma processing equipment 10 Processing vessel 15 Gas supply source 20 Placement table 25 Gas shower head 32 2nd high frequency power supply 34 1st high frequency power supply 100 Control section 103 Focus Ring 106 Electrostatic Chuck 108 Optical Sensor 108a First sensor 108b Second sensor 1000 Plasma Processing System OC Observation Device EL1 Etching target film F membrane MA Mask OP Opening P Precursor R Reactive gas W wafer

Claims

1. (a) providing a plurality of plasma processing apparatuses and an observation apparatus, At least one of the plasma processing apparatuses includes: A chamber including a mounting table and a plasma generator facing the mounting table, a chamber in which a substrate having a recess is placed on the mounting table within the chamber; a first sensor for monitoring a state of a plasma generated in the chamber; Control unit and Equipped with the observation device includes at least one second sensor provided outside the plasma processing device; (b) detecting a pattern shape on the substrate using the second sensor; (c) generating plasma in the chamber under first process conditions determined based on the results of (b), thereby forming a film that is formed on an upper side of a sidewall of the recess and on an outer upper surface of the recess adjacent to the recess, and that is not formed on an underside of the sidewall of the recess and on a bottom surface of the recess; (d) monitoring a state of the plasma generated in (c) using the first sensor; (e) determining the necessity of re-executing (c) and second processing conditions for re-executing (c) based on the state of the plasma monitored in (d); (f) detecting a pattern shape of the substrate on which the film is formed, using the second sensor, when it is determined in (e) that the process of (c) is not to be performed again; (g) etching the underlayer using a layer formed on the film as a mask under third processing conditions determined based on the result of (f); Including, The (c) is (c-1) introducing a first gas into the chamber and allowing the first gas to be adsorbed in the recess; (c-2) purging the chamber; (c-3) supplying a second gas into the chamber, generating plasma from the second gas, and reacting a component of the second gas with a component of the first gas adsorbed in the recess to form the film; (c-4) purging the chamber; and (c-5) repeating the steps (c-1), (c-2), (c-3), and (c-4); At least one of the following (1) and (2) is carried out: In the above (1), in the above (c-1), the first gas is adsorbed only in a part of the recess, In the process (2), the process (c-3) is terminated before the reaction between the first gas component and the second gas component is saturated over the entire surface of the recessed portion, In the step (c), the film is formed on the side wall such that the thickness of the film gradually decreases from an upper side of the side wall toward a bottom of the recess; The step (d) includes monitoring a state of plasma in each of a plurality of regions in which the substrate is placed; In the step (e), it is determined that the step (c) is executed again when an integral value of a physical quantity indicating a state of the plasma in each of the plurality of regions obtained in the step (d) is less than a predetermined value, and the physical quantity includes at least one parameter selected from a parameter group consisting of an electron density, an ion density, a molecular radical density, and an atomic / molecular ion mass; (e) is carried out before (c-4), after (c-4), or in parallel with (c-4); (g) is performed in a plasma processing apparatus different from (c); the first process condition includes at least one selected from a group of parameters consisting of a temperature of a mounting table on which the substrate is placed, a pressure of the chamber, a flow rate of the first gas, a supply time of the first gas, and a process time; the second processing condition includes at least one of a processing time for re-executing (c-1), a processing time for re-executing (c-3), starting re-execution of (c) from (c-1), and starting re-execution of (c) from (c-3); The plasma processing method, wherein the third processing condition includes at least one of an etching gas supply amount, a high frequency power, and a substrate temperature.

2. The plasma processing method according to claim 1 , wherein a subconformal film is formed in the recess.

3. 2. The plasma processing method according to claim 1, wherein in the step (c-3), a position at which the film is formed on the recess is controlled by adjusting at least one parameter selected from a group of parameters consisting of a temperature of a mounting table on which the substrate is placed, a pressure of the chamber, a flow rate of the second gas, an introduction time of the second gas, a processing time, and a high-frequency power for plasma generation.

4. 2. The plasma processing method according to claim 1, wherein in (d), an amount of radicals in the plasma generated in (c) is monitored.

5. 2. The plasma processing method of claim 1, wherein in (e), physical quantities indicating plasma states in the respective regions are compared, and if a difference therebetween is greater than a predetermined value, second processing conditions that offset the difference are determined, and (c) is re-performed under the determined second processing conditions.

6. The (f) is (f-1) detecting a state of the film on the recess after (c); (f-2) re-executing (c) according to the detection result of (f-1); The plasma processing method of claim 1 , comprising:

7. (i) detecting the shape of the recess before (c); (j) determining the processing conditions of (c) according to the detection result of (i); The plasma processing method of claim 6 , further comprising:

8. (k) determining a correlation between the shape of the recess before deposition, the state of the plasma, and the state of the film formed in (c) based on the shape of the recess detected in (i), the state of the plasma monitored in (d), and the pattern shape of the substrate detected in (f); (l) correcting the process conditions of (c) based on the correlation; (m) forming a film in a recess of a substrate different from the substrate under the processing conditions corrected in (l); The plasma processing method of claim 7 , comprising:

9. The (f) is (f-1) detecting a state of the film on the recess after (c); (f-2) determining processing conditions according to the detection results of (f-1); Including, 2. The plasma processing method according to claim 1, wherein the step (g) etches the underlayer under the processing conditions determined in the step (f-2).

10. (h) after (g), detecting the shape of the pattern formed by the etching and / or the state of the film on the recess, and if the degree of agreement between the shape detected in (h) and a predetermined shape is equal to or less than a predetermined value, re-executing (c) or (g). The plasma processing method of claim 9 , further comprising:

11. (i) detecting the shape of the recess before (c); (n) detecting the shape of a pattern formed by the etching and / or the state of the film on the recess after (g); (o) determining a correlation between the state of the film, the state of the plasma, and the shape of the pattern after (g) based on the state of the film detected in (f), the state of the plasma monitored in (d), and the shape of the pattern of the film on the recess detected in (n) and / or the state of the film; (p) correcting the process conditions of (g) based on the correlation; (q) etching a substrate different from the substrate under the processing conditions corrected in (p); The plasma processing method of claim 9 , further comprising:

12. The first sensor monitors a physical quantity indicative of a state of the plasma; The plasma processing method of claim 1 , wherein the second sensor optically determines a quantity related to a pattern shape on the substrate.

13. 13. The plasma processing method according to claim 12, wherein the physical quantity indicating the state of the plasma is a quantity by which an amount of radicals in the plasma can be estimated.

14. 2. The plasma processing method of claim 1 , further comprising: determining, in step (e), a variation in in-wafer uniformity based on the state of the plasma monitored in step (d); and changing the second processing condition when re-executing step (c) based on the determined variation in in-wafer uniformity.

15. providing a plasma processing apparatus having a chamber in which a substrate having a recess is received; forming a film on the recess by generating plasma in the chamber, the film being formed on an upper side of a sidewall of the recess and on an outer upper surface of the recess adjacent to the recess, but not on an underside of the sidewall of the recess or on a bottom surface of the recess; monitoring a state of the plasma generated in the generating step using a first sensor; detecting a pattern shape on the substrate using a second sensor; determining whether or not it is necessary to retry generating the plasma; detecting a pattern shape of the substrate on which the film is formed using the second sensor when the plasma generation is not performed again; Etching the underlayer using a layer formed on the film as a mask; Including, In the step of generating plasma, supplying a first gas into the chamber and allowing the first gas to be adsorbed only in a portion of the recess; supplying a second gas into the chamber and reacting a component of the second gas with a component of the first gas adsorbed in the recess to form the film; Including, In the step of generating the plasma, generation of the plasma is stopped before a reaction between a component of the first gas and a component of the second gas is saturated over an entire surface of the recess, The plasma processing method, wherein the film is formed on the side wall such that the film thickness gradually decreases from an upper side of the side wall toward a bottom of the recess.

16. the first sensor monitors a physical quantity from which an amount of radicals in the plasma can be estimated; The plasma processing method of claim 15 , wherein the second sensor optically determines a quantity related to the pattern shape.

17. Based on the results of the monitoring, a variation in within-wafer uniformity is determined; and The plasma processing method of claim 15 , wherein when the plasma generation is re-performed, at least one plasma condition is changed based on the determined change in the within-wafer uniformity.

18. a determination is made as to whether or not to re-attempt generating the plasma based on the detection using the second sensor; and In response to a decision to reactivate the generation of the plasma, the generation of the plasma is reactivated with at least one modified process condition compared to an immediately ongoing generation of the plasma; The plasma processing method of claim 15 , wherein, in response to a decision not to regenerate the plasma, an etch is performed.

Citation Information

Patent Citations

  • Plasma measurement procedure

    JP1990230698A

  • Plasma device

    JP1993175165A

  • Plasma process apparatus, method for controlling the same and method for determining defective product

    JP2001284322A

  • Plasma treating apparatus

    JP2006216605A

  • Pattern formation method and substrate processing system

    JP2014017438A