Manufacturing method of resin sintered body
The immersion of resin sintered bodies in a sulfuric acid and chromic anhydride solution addresses uneven coloring and surface roughness in MJF-produced resin sintered bodies, resulting in uniformly colored and smooth surfaces with enhanced appearance and efficiency.
Patent Information
- Application Number
- JP2021045304
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-03-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2041-03-18
AI Technical Summary
The MJF method for producing resin sintered bodies results in uneven coloring and poor surface smoothness due to uncolored resin powder incorporation at the boundary of the coalescing agent and modifier, leading to non-uniform surfaces.
A method involving immersion of the intermediate resin sintered body in a treatment liquid containing sulfuric acid and chromic anhydride, with specific concentrations and temperatures, to etch the surface and remove non-uniformly colored areas, ensuring uniform coloring and smoothness.
Achieves uniformly colored and smooth resin sintered bodies with improved appearance and manufacturing efficiency by effectively removing uncolored resin powder residues.
Smart Images

Figure 0007575312000003 
Figure 0007575312000004 
Figure 0007575312000005
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing a resin sintered body by sintering a resin powder of a thermoplastic resin to form a resin sintered body. [Background technology]
[0002] Conventionally, as a technology for sintering thermoplastic resin powder to form a resin sintered body, the MJF method (multi-jet fusion method) is known, which sinters resin powder using additive manufacturing with a 3D printer. In this MJF method, a layer of polyamide resin powder such as polyamide 12 is formed, and a fusing agent that promotes fusion, including ink such as a light-absorbing ink, and a fusion modifier that prevents fusion by the action of vaporization heat are applied to the layer of resin powder at desired locations. Then, each layer of resin powder to which the fusing agent and fusion modifier are applied is fused by exposure to light or heating to form a resin sintered body (see Patent Document 1). [Prior art documents] [Patent documents]
[0003] [Patent Document 1] JP 2019-89348 A Summary of the Invention [Problem to be solved by the invention]
[0004] By the way, when forming a resin sintered body by repeating the process of applying ink to a layer of resin powder and sintering it by the MJF method, although the inside can be well colored by the ink, the outer surface near the boundary between the fusing agent and the fusion modifier has a problem that the surface of the outermost layer formed near the boundary between the fusing agent and the fusion modifier cannot be uniformly colored because the uncolored resin powder is taken into the sintered part of each layer. In addition, there is also a problem that the surface of the outermost sintered layer has poor smoothness because the unevenness of the resin powder remains on the surface.
[0005] The present invention has been proposed in consideration of the above-mentioned problems, and aims to provide a method for producing a resin sintered body, which, when producing a resin sintered body by sintering resin powder of a thermoplastic resin, can eliminate uneven colored areas on the surface, can provide a state in which the surface of the resin sintered body is uniformly and sufficiently colored as required, and can provide a surface of the resin sintered body in an attractive, smooth state. [Means for solving the problem]
[0006] The method for producing a resin sintered body of the present invention is a method for producing a resin sintered body by applying an ink to a resin powder of a thermoplastic resin and sintering the resin powder, and is characterized by comprising a step of immersing an intermediate resin sintered body, which has been entirely sintered and has an uneven colored region on its surface, in a treatment liquid containing sulfuric acid and chromic anhydride. In the step of immersing in the treatment liquid, it is preferable that the concentration of the chromic anhydride in the treatment liquid is 300 g / L or more, and the immersion time is 5 minutes or more. According to this, the surface of the intermediate resin sintered body can be reliably etched in a required range, and the surface portion of the intermediate resin sintered body that is not uniformly colored with ink can be removed, so that the surface of the resin sintered body can be uniformly and sufficiently colored as required, and the surface of the resin sintered body can be made smooth and attractive. In addition, the treatment of immersion in the surface treatment liquid allows uniform etching to be performed without being restricted by the shape of the intermediate resin sintered body or the resin sintered body, and is therefore highly versatile.
[0007] The method for producing a resin sintered body of the present invention is characterized by carrying out a step of immersing the intermediate resin sintered body in the surface treatment liquid while maintaining the temperature of the surface treatment liquid at 70° C. or higher. This makes it possible to reliably obtain a resin sintered body that is uniformly and sufficiently colored, has a good-looking smooth surface, and is excellent in appearance. In addition, a resin sintered body that is uniformly and sufficiently colored, has a good-looking smooth surface, and is obtained in a shorter time, thereby improving production efficiency.
[0008] The method for producing a resin sintered body of the present invention is characterized by carrying out a step of immersing the surface in the surface treatment liquid, the concentration of the sulfuric acid being 184 g / L to 368 g / L and the concentration of the chromic anhydride being 300 g / L to 500 g / L. This makes it possible to reliably obtain a resin sintered body that is uniformly and sufficiently colored, has a good-looking, smooth surface, and is excellent in appearance.
[0009] The method for producing a resin sintered body of the present invention is characterized in that the thermoplastic resin is polyamide 12. This makes it possible to reliably obtain a polyamide 12 resin sintered body that is uniformly and sufficiently colored, has a good-looking smooth surface, and is excellent in appearance.
[0010] The method for producing a resin sintered body of the present invention is characterized in that the intermediate resin sintered body is formed by applying ink to a layer of resin powder of a thermoplastic resin and sintering it using additive manufacturing based on a multi-jet fusion method. According to this, when ink is applied to a layer of thermoplastic resin powder and sintered using additive manufacturing with the multi-jet fusion method, it is possible to reliably obtain a resin sintered body that is uniformly and sufficiently colored and has a smooth, attractive surface. Effect of the Invention
[0011] According to the method for producing a resin sintered body of the present invention, the surface of the resin sintered body can be uniformly and sufficiently colored as required, and the surface of the resin sintered body can be made smooth and attractive. [Brief description of the drawings]
[0012] [Figure 1] 3(a) to 3(c) are schematic process explanatory views showing a manufacturing process for forming an intermediate resin sintered body of a resin sintered body according to an embodiment of the present invention. [Diagram 2] 5A and 5B are schematic process explanatory views showing a manufacturing process for forming a resin sintered body from an intermediate resin sintered body in an embodiment. [Diagram 3] 4 is a graph showing the relationship between the concentration of chromic anhydride in the surface treatment solution and brightness in the examples and comparative examples. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0013] [Method for producing resin sintered body according to embodiment] The method for producing a resin sintered body according to an embodiment of the present invention is a method for producing a resin sintered body using additive manufacturing of a 3D printer of the MJF method (multi-jet fusion method), in which a layer of resin powder of a thermoplastic resin is formed, and a fusing agent that promotes fusion, including an ink that colors the resin powder layer, and a fusion modifier that prevents fusion by the action of vaporization heat are applied to the desired location. Then, the resin powder layer to which the fusing agent and fusion modifier are applied is heated, or the resin powder layer is fused and sintered by exposure to light from an infrared or near-infrared light source or a halogen light source, and the resin powder layer is applied with ink and sintered, and a resin sintered body composed of multiple layers of resin powder is formed by repeating the process. The material of the resin powder of the thermoplastic resin used is appropriate within the applicable range, and for example, polyamide 11, polyamide 12, and polypropylene are suitable, and in particular, polyamide 12 is more suitable.
[0014] For example, as shown in FIG. 1(a), a layer of resin powder 2 of a thermoplastic resin is formed, a fusing agent and a fusing modifier containing ink 3 are applied to the layer of resin powder 2 to color the resin powder 2 with the ink 3, and the colored layer is fused and sintered by heating or exposure to light to form a sintered layer 41m. At this time, the resin powder 2 can be colored with the ink 3 inside the sintered layer 41m, but on the outer surface (the inclined surface in the figure) of the sintered layer 41m corresponding to the vicinity of the boundary between the fusing agent and the fusing modifier, the uncolored resin powder 2 is taken into the colored part of the sintered layer 41m by the heat of the sintered layer 41m, resulting in an area where the coloring is not uniform. Note that in FIG. 1 and FIG. 2 described later, the shape of the resin powder 2 is shown as a sphere, and the shape of the resin powder 2 is partially retained even after sintering, but in reality, the colored and sintered resin powder 2 melts and adheres tightly to each other without any gaps.
[0015] 1(b), a layer of resin powder 2 of thermoplastic resin is formed so as to be laminated on the upper side of the sintered layer 41m, a fusing agent and a fusing modifier containing ink 3 are applied to the layer of resin powder 2 to color the resin powder 2 with the ink 3, and the colored layer is fused and sintered by heating or exposure to light to form a sintered layer 42m. In this case as well, on the outer surface (the inclined surface in the figure) of the sintered layer 42m corresponding to the vicinity of the boundary between the fusing agent and the fusing modifier, the uncolored resin powder 2 is taken into the colored part of the sintered layer 42m by the heat of the sintered layer 42m, resulting in an area where the coloring is not uniform.
[0016] Similarly, when the sintered layer 43m is formed by stacking it on the upper side of the sintered layer 42m, the uncolored resin powder 2 is taken into the colored part of the sintered layer 43m on the outer surface (the inclined surface in the figure) of the sintered layer 43m corresponding to the boundary between the fusion agent and the fusion modifier, resulting in an area with uneven coloring (see FIG. 1(c)). That is, in the intermediate resin sintered body 1m, which is an intermediate product composed of the sintered layers 41m, 42m, and 43m and is entirely sintered, an uneven colored area is formed over the entire outer surface corresponding to the inclined surface shown in the figure due to the incorporation and remaining of the uncolored resin powder 2. In addition, the outer surface corresponding to the inclined surface shown in the figure of the intermediate resin sintered body 1m has the unevenness of the sintered resin powder 2 remaining as it is, and is in a state of poor smoothness. In addition, in the MJF type 3D printer, the temperature of the powder surface when melting the resin powder such as polyamide 12, and the amount of the fusion agent and the fusion modifier sprayed require complex control, so it is assumed that they are automatically controlled to improve the convenience of the user. Therefore, it is difficult for a user to intentionally improve the condition of the resin sintered body.
[0017] Furthermore, the region in which the uncolored resin powder 2 is incorporated and the unevenness of the sintered resin powder 2 remains as it is, occurs throughout the region near the boundary between the fusion agent and the fusion modifier, and occurs on the entire surface of the resin sintered body product, not limited to the inclined surface of the example in Figure 1. That is, in additive manufacturing using the MJF method, when molding a resin sintered body, the boundary between the resin powder 2 in the bottom layer and the resin powder 2 in the layer immediately above it becomes the boundary between the fusion agent and the fusion modifier, and the boundary between the resin powder 2 in the top layer and the resin powder 2 in the layer immediately below it becomes the boundary between the fusion agent and the fusion modifier, so that the bottom and top surfaces of the resin sintered body product also have regions in which the unevenness of the sintered resin powder 2 remains as it is with uneven coloring. Furthermore, in additive manufacturing using the MJF method, even when multiple resin sintered bodies are formed in multiple stages by stacking them on top of each other for work efficiency, the boundary between the resin powder 2 in the bottom layer of the product in the middle stage and the resin powder 2 in the layer immediately above it, and between the resin powder 2 in the top layer and the resin powder 2 in the layer immediately below it, are respectively the boundaries between the fusion agent and the fusion modifier, and this results in areas on the bottom and top surfaces of the resin sintered body product in the middle stage where the unevenness of the sintered resin powder 2 with uneven coloring remains as it is.
[0018] In the method for producing a resin sintered body of this embodiment, the intermediate resin sintered body 1m thus formed is immersed in an etching bath of a surface treatment liquid containing sulfuric acid and chromic anhydride, the concentration of which is 300 g / L or more. In this immersion step, from the viewpoint of shortening the treatment time and improving the production efficiency, it is preferable to maintain the temperature of the surface treatment liquid at 70°C or more, and from the viewpoint of further shortening the treatment time and further improving the production efficiency, it is more preferable to maintain the temperature at 80°C or more. In addition, from the viewpoint of increasing the certainty of the effect of sufficient coloring and smoothness of the surface 10 of the resin sintered body 1, it is preferable that the concentration of sulfuric acid in the surface treatment liquid to be immersed is 184 g / L to 368 g / L, and that the concentration of chromic anhydride is 300 g / L to 500 g / L.
[0019] In addition, a certain level of effect can be obtained if the immersion time in the surface treatment liquid is 5 minutes or more. However, from the viewpoint of further improving the appearance, if the surface treatment liquid is 70° C. or higher, immersion for 20 minutes or more can reliably obtain a high level of effect, and if the surface treatment liquid is 80° C. or higher, immersion for 10 minutes or more can reliably obtain a high level of effect, and is therefore preferable.
[0020] When the intermediate resin sintered body 1m is immersed in the above-mentioned surface treatment liquid and then pulled out of the etching bath, it becomes the finished resin sintered body 1 (see FIG. 2). In this resin sintered body 1, the uncolored resin powder 2 that has been incorporated into the sintered layers 41m, 42m, and 43m, for example, is removed, and the surface 10 is free of unevenly colored regions and is uniformly and sufficiently colored as required. Furthermore, the surface 10 of the resin sintered body 1 is made smooth and attractive by the etching.
[0021] According to the method for producing a resin sintered body of this embodiment, the surface of the intermediate resin sintered body 1m of the resin sintered body 1, which is produced by applying ink 3 to a layer of resin powder 2 of a thermoplastic resin and sintering the layer by additive manufacturing using the multi-jet fusion method, is reliably etched within a required range, and the surface portion of the intermediate resin sintered body 1m that is not uniformly colored with the ink 3 is removed. Then, the surface 10 of the resin sintered body 1 can be uniformly and sufficiently colored as required, and the surface 10 of the resin sintered body 1 can be made to have a good-looking smooth state, thereby obtaining a resin sintered body 1 with excellent appearance. In addition, by the treatment of immersion in the surface treatment liquid, uniform etching can be performed without being restricted by the shapes of the intermediate resin sintered body 1m and the resin sintered body 1, and the method is highly versatile.
[0022] [Scope of the invention disclosed herein] The inventions disclosed in this specification include, in addition to the inventions and embodiments listed as inventions, those specified by changing partial contents of these to other contents disclosed in this specification, those specified by adding other contents disclosed in this specification to these contents, or those specified by deleting partial contents of these to the extent that partial effects can be obtained, and specifying them as a higher-level concept. The inventions disclosed in this specification also include the following modified examples and added contents.
[0023] For example, the application of the method for producing a resin sintered body of the present invention is not limited to a resin sintered body formed by applying ink to a layer of resin powder of a thermoplastic resin and sintering it by additive manufacturing using the multi-jet fusion method, but can be applied to any resin sintered body formed by applying ink to resin powder of a thermoplastic resin and sintering it. In addition, the shape of the resin sintered body to which the present invention is applied is appropriate, and it can be applied to a resin sintered body having a substantially plate-like shape or a resin sintered body having various three-dimensional shapes. In addition, even when the temperature of the surface treatment liquid is less than 70°C or the concentration of sulfuric acid in the surface treatment liquid is less than 184 g / L, it is included in the present invention as long as the effect of improving the uniformity and smoothness of coloring on the surface of the resin sintered body can be obtained.
[0024] [Examples and Comparative Examples] Next, examples and comparative examples of resin sintered bodies manufactured by the method for manufacturing a resin sintered body of the present invention will be described. Table 1 shows Examples 1-8, and Table 2 shows Examples 9-13 and Comparative Examples 1-3.
[0025] Each substrate of Examples 1-13 and Comparative Examples 1-3 was created using a 3D printer (HP Development Company, LP) of the MJF method (multi-jet fusion method), polyamide 12 powder as the resin powder of the thermoplastic resin, and carbon black-containing ink as the ink. The composition of the carbon black-containing ink, which is the fusion agent, was water: 70-80 mass%, 2-pyrrolidone: less than 20 mass%, and carbon black: less than 7.5 mass%. In addition, each substrate was created using a fusion modifier (water: 80-90 mass%, triethylene glycol: less than 15 mass%, 2-pyrrolidone: less than 5 mass%) in combination with the fusion agent.
[0026] In the creation of a resin sintered body using the MJF method, a layer of polyamide 12 powder was formed, and a fusion agent and fusion modifier equivalent to a carbon black-containing ink were applied to the formed layer, and the process of fusing and sintering by heating or exposure was repeated to form a base material for an intermediate resin sintered body composed of multiple layers. The creation conditions were as follows: a surface layer of polyamide 12 powder spread to a thickness of 80 μm was irradiated with a movable light source consisting of six halogen lamps of 2000 W or more at a moving speed of 300 mm per second or more. It was assumed that the temperature of the powder surface was automatically controlled by the MJF 3D printer to keep it above the crystallization temperature of polyamide 12, approximately 150 °C, but the exact temperature was unknown. In addition, the exact amount of fusion agent and fusion modifier sprayed by the MJF 3D printer's automatic control was unknown, but based on the actual usage amount, it was estimated that the maximum application amount of each was 0.3 g / mm 3 It was confirmed that the polyamide 12 powder was sprayed onto the substrate. The substrates were all of the same structure, shape, and size, and the polyamide 12 powder was in the form of crushed particles with an average particle size of 60 μm. The specific gravity of the fusing agent was 1.1 g / cm 3 The black liquid, fusion modifier, has a specific gravity of 1.0g / cm 3 It is a colorless, transparent liquid.
[0027] Then, each of the substrates of Examples 1-13 and Comparative Examples 1 and 2 was immersed in an etching bath of a surface treatment liquid containing chromic anhydride as an oxidizing agent and sulfuric acid as a strong acid. The concentrations of chromic anhydride (oxidizing agent concentration) and sulfuric acid (strong acid concentration) of Examples 1-13 and Comparative Examples 1 and 2 are as shown in Tables 1 and 2. The substrate of Comparative Example 3 was immersed in an etching bath of a surface treatment liquid containing sulfuric acid at the concentration shown in Table 2 but not containing chromic anhydride. The temperatures and immersion times of the etching baths of the surface treatment liquids of Examples 1-13 and Comparative Examples 1-3 are as shown in Tables 1 and 2.
[0028] After completion of immersion in each surface treatment solution, for each of the substrates in Examples 1-13 and Comparative Examples 1-3, in order to confirm whether the surface (outer surface) of the substrate was colored in a black state with excellent design, the lightness (L*) of an area with a diameter of 8 mm on the surface (outer surface) of each substrate was measured with a spectrophotometer (CM-5: manufactured by Konica Minolta, Inc.). The lightness (L*) of Examples 1-13 and Comparative Examples 1-3 is shown in Tables 1 and 2. The experimental results were judged by setting a lightness (L*) of 40 or less as the acceptable standard for a black state with excellent design, and a lightness (L*) of 30 or less as the standard for a more desirable black state.
[0029] In Comparative Example 3 in Table 2, in which the plate was immersed in an etching bath of a surface treatment liquid that did not contain chromic anhydride, the lightness (L*) was 57.53, which was far from the acceptable coloring standard. In addition, when Example 1 (chromic anhydride concentration: 400 g / L), Example 2 (chromic anhydride concentration: 300 g / L), Example 3 (chromic anhydride concentration: 500 g / L), Comparative Example 1 (chromic anhydride concentration: 100 g / L), and Comparative Example 2 (chromic anhydride concentration: 200 g / L) were compared under the same conditions of sulfuric acid concentration: 368 g / L, etching bath temperature of the surface treatment liquid: 80° C., and immersion time in the etching bath: 20 minutes, in which only the concentration of chromic anhydride was changed, as shown in Tables 1 and 2 and FIG. 2, the chromic anhydride concentration of 300 g / L or more cleared the more desirable black state standard of lightness (L*): 30 or less, while Comparative Examples 1 and 2, in which the chromic anhydride concentration was less than 300 g / L, did not clear the black state pass standard of lightness (L*): 40 or less.
[0030] Furthermore, from the results of Examples 6 and 9, which are the same conditions (chromic anhydride concentration: 400 g / L, sulfuric acid concentration: 368 g / L) but have different etching bath temperatures and immersion times in the etching bath, it was found that when the etching bath temperature of the surface treatment liquid was 70° C., immersion for 20 minutes or more was sufficient to meet the criterion for a more desirable black state, brightness (L*): 30 or less, and when the etching bath temperature of the surface treatment liquid was 80° C., immersion for 10 minutes or more was sufficient to meet the criterion for a more desirable black state, brightness (L*): 30 or less. From the viewpoint of shortening the manufacturing time, it is found that the etching bath temperature of the surface treatment liquid is preferably 80° C. or higher.
[0031] [Table 1]
[0032] [Table 2] [Industrial Applicability]
[0033] The present invention can be utilized when producing a resin sintered body by sintering a resin powder of a thermoplastic resin. [Explanation of symbols]
[0034] 1... Resin sintered body 10... Surface 1m... Intermediate resin sintered body 2... Resin powder 3... Ink 41m, 42m, 43m... Sintered layer
Claims
1. A method for producing a resin sintered body by applying ink to a resin powder of a thermoplastic resin and sintering the ink, comprising the steps of: A method for producing a resin sintered body, comprising the step of immersing an entirely sintered intermediate resin sintered body having a non-uniformly colored region on its surface in a treatment liquid containing sulfuric acid and chromic anhydride.
2. 2. The method for producing a resin sintered body according to claim 1, wherein in the step of immersing in the treatment liquid, the concentration of the chromic anhydride in the treatment liquid is 300 g / L or more, and the immersion time is 5 minutes or more.
3. 3. The method for producing a resin sintered body according to claim 1, further comprising the step of immersing the intermediate resin sintered body in the surface treatment liquid while maintaining the temperature of the surface treatment liquid at 70° C. or higher.
4. The method for producing a resin sintered body according to any one of claims 1 to 3, characterized in that a step of immersing the resin sintered body in the surface treatment liquid is performed with the sulfuric acid concentration being 184 g / L to 368 g / L and the chromic anhydride concentration being 300 g / L to 500 g / L.
5. 5. The method for producing a resin sintered body according to claim 1, wherein the thermoplastic resin is polyamide 12.
6. The method for producing a resin sintered body according to any one of claims 1 to 5, characterized in that the intermediate resin sintered body is formed by applying ink to a layer of resin powder of a thermoplastic resin and sintering it by additive manufacturing using a multi-jet fusion method.
Citation Information
Patent Citations
Electrostrictive effect device
JP1991283683A
Additive manufacturing
JP2019089348A
Colored powders prepared by a combination of two thermal, chemical or irradiation processes
US5908499A
Sintered molded body, production method therefor, article provided with sintered molded body, sintered molded body material, and pre-sintering molded body and production method therefor
WO2016208671A1