Method for manufacturing the mold

The method of impregnating mold precursors with colloidal silica and water glass enhances mold heat resistance, addressing the issue of insufficient heat resistance in conventional molds, ensuring durability and reducing casting defects.

JP7575327B2Active Publication Date: 2024-10-29GUN EI CHEM IND
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2021054923
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2021-03-29
Publication Date
2024-10-29
Estimated Expiration
2041-03-29

AI Technical Summary

Technical Problem

Conventional mold manufacturing methods result in molds with insufficient heat resistance, leading to issues such as seizure and flashing when exposed to high temperatures during metal casting.

Method used

A method involving the impregnation of a mold precursor with colloidal silica and water glass, followed by curing and optional firing, to enhance the mold's heat resistance.

Benefits of technology

The method produces molds with excellent heat resistance, maintaining shape and strength even at high temperatures, reducing casting defects and improving environmental safety by minimizing thermal decomposition gases.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575327000007
    Figure 0007575327000007
  • Figure 0007575327000008
    Figure 0007575327000008
  • Figure 0007575327000009
    Figure 0007575327000009
Patent Text Reader

Abstract

To provide a mold production method capable of producing a mold having excellent heat resistance.SOLUTION: A mold production method comprises: an impregnation step in which a mold precursor as a hardened material comprising a refractory granular material and an organic binder is separately impregnated with colloidal silica and water glass; and a hardening step in which the water glass impregnated into the mold precursor is hardened.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for manufacturing a mold. [Background technology]

[0002] Conventionally, casting molds (hereinafter simply referred to as "molds") are classified into normal molds and special molds, and normal molds are classified into green molds and dry molds. On the other hand, special molds are classified into heat-hardening molds, self-hardening molds, and gas-hardening molds. Refractory granular materials such as silica sand are used as mold materials, but because the refractory granular materials alone tend to crumble when dried, a binder is added to make them less likely to crumble. Ordinary molds use clay such as bentonite as a binder, while special molds use organic binders such as phenolic resin, furan resin, and urethane resin, or inorganic binders such as water glass.

[0003] For example, Patent Documents 1 and 2 disclose a method for manufacturing a mold in which a mold made with an organic binder is impregnated with water glass in a specific molar ratio (molar ratio of SiO2 and Na2O) as an inorganic binder and then fired. Patent Document 3 discloses a method for producing a mold in which a mold made with an organic binder is impregnated with a water-soluble inorganic salt such as sodium chloride and then fired. Patent Document 4 discloses a method for producing a mold by three-dimensional additive manufacturing, which repeats a step of forming a thin layer of a fire-resistant molding base material and a step of printing water glass and a binder in a predetermined location on the thin layer. [Prior art documents] [Patent documents]

[0004] [Patent Document 1] Japanese Patent Application Publication No. 3-248740 [Patent Document 2] JP 2018-158377 A [Patent Document 3] JP 2020-22981 A [Patent Document 4] Special Publication No. 2017-538585 Summary of the Invention [Problem to be solved by the invention]

[0005] However, in the methods described in Patent Documents 1 to 4, the heat resistance of the mold may be insufficient. Since the mold is exposed to high temperatures when a liquid (molten metal) made by melting metals such as iron, copper, and aluminum at high temperatures is poured into it, casting defects such as seizure and glare may occur, or the mold may be deformed if the mold has low heat resistance. Therefore, the mold is required to have heat resistance that allows it to exhibit sufficient strength even when exposed to high temperatures. An object of the present invention is to provide a method for producing a mold that is capable of producing a mold having excellent heat resistance. [Means for solving the problem]

[0006] The present invention has the following aspects. [1] An impregnation step of separately impregnating a mold precursor, which is a hardened mixture containing a refractory granular material and an organic binder, with colloidal silica and water glass; a hardening step of hardening the water glass impregnated into the template precursor; A method for manufacturing a mold, comprising: [2] The method for producing a mold according to [1] above, further comprising a firing step after the hardening step. [3] The method for producing a template according to [1] or [2] above, wherein the template precursor is produced by three-dimensional additive manufacturing. Effect of the Invention

[0007] According to the present invention, a method for manufacturing a mold capable of manufacturing a mold having excellent heat resistance can be provided. [Brief description of the drawings]

[0008] [Figure 1] FIG. 1 is a schematic diagram of the template precursor produced in Example 17, where (a) is a perspective view and (b) is a side view. [Diagram 2]1 is a photograph of a test piece (fired body) obtained in Example 17. [Diagram 3] 1 is a photograph of a test piece (fired body) obtained in Comparative Example 11. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0009] [Mold manufacturing method] Hereinafter, one embodiment of the method for producing a mold of the present invention will be described. In the method for producing a template of this embodiment, the template precursor is impregnated with colloidal silica and water glass separately (impregnation step), and then the water glass is hardened (hardening step) to obtain the template. The method for producing a mold of this embodiment may further include a firing step described below after the hardening step. In this specification, in order to distinguish between a mold obtained by the hardening process and a mold obtained by the firing process, the mold obtained by the hardening process is also called a "hardened body" and the mold obtained by the firing process is also called a "fired body."

[0010] <Template precursor> The mold precursor is a cured mixture that includes a refractory particulate material and an organic binder. In producing the template precursor, it is preferred to use a hardener in addition to the refractory granular material and the organic binder. The template precursor may contain components (optional components) other than the refractory granular material, the organic binder and the hardener, as necessary.

[0011] (Fire-resistant granular material) As the refractory granular material, conventionally known materials such as natural sands, such as silica sand, chromite sand, zircon sand, olivine sand, amorphous silica, alumina sand, and mullite sand, and artificial sand can be used. In addition, used refractory granular materials that have been recovered (recovered sand) or regenerated (recycled sand) can also be used. These refractory granular materials may be used alone or in combination of two or more types.

[0012] The average particle size of the refractory granular material is preferably 50 to 600 μm, more preferably 60 to 550 μm, and even more preferably 75 to 500 μm. If the average particle size of the refractory granular material is equal to or greater than the lower limit, a mold with high strength can be obtained. If the average particle size of the refractory granular material is equal to or less than the upper limit, the surface properties of the castings cast using the mold are also excellent. In particular, if the average particle size of the refractory granular material is equal to or less than 300 μm, it is suitable for producing a mold precursor by three-dimensional additive manufacturing, and a mold with excellent surface properties can be obtained. The average particle size of the refractory granular material is the median size of 50% of the total volume of the refractory granular material measured by dynamic light scattering.

[0013] (Organic binder) Examples of the organic binder include binders used in producing molds by the shell mold method, binders used in producing molds by the amine cold box method, alkaline phenol resins, acid-hardening binders, etc. These organic binders may be used alone or in combination of two or more. Among these, acid-setting binders are preferred.

[0014] Examples of binders used in producing a mold by the shell molding method include novolac-type phenolic resins and resol-type phenolic resins. Novolak-type phenolic resins are obtained by reacting phenols with aldehydes in the presence of an acid catalyst, and are usually solid. Examples of phenols include phenol, o-cresol, m-cresol, p-cresol, 2,3-xylenol, 3,5-xylenol, m-ethylphenol, m-propylphenol, m-butylphenol, p-butylphenol, o-butylphenol, resorcinol, hydroquinone, catechol, 3-methoxyphenol, 4-methoxyphenol, 3-methylcatechol, 4-methylcatechol, methylhydroquinone, 2-methylresorcinol, 2,3-dimethylhydroquinone, 2,5-dimethylresorcinol, 2-ethoxyphenol, 4-ethoxyphenol, 4-ethylresorcinol, 3-ethoxy-4-methoxyphenol, 2-propenylphenol, 2-isopropylphenol, 3-isopropylphenol, 4-isopropylphenol, 3,4,5-trimethylphenol, 2-isopropoxyphenol, 4-propoxyphenol, 2-allylphenol, 3,4,5-trimethoxyphenol, phenol, 4-isopropyl-3-methylphenol, pyrogallol, phloroglucinol, 1,2,4-benzenetriol, 5-isopropyl-3-methylphenol, 4-butoxyphenol, 4-t-butylcatechol, t-butylhydroquinone, 4-t-pentylphenol, 2-t-butyl-5-methylphenol, 2-phenylphenol, 3-phenylphenol, 4-phenylphenol, 3-phenoxyphenol, 4-phenoxyphenol, 4-hexyloxyphenol, 4-hexanoylresorcinol, 3,5-diisopropylcatechol, 4-hexylresorcinol, 4-heptyloxyphenol, 3,5-di-t-butylphenol, 3,5-di-t-butylcatechol, 2,5-di-t-butylhydroquinone, di-sec-butylphenol, 4-cumylphenol, nonylphenol, 2-cyclopentylphenol, 4-cyclopentylphenol, bisphenol A, bisphenol F, and the like. These phenols may be used alone or in combination of two or more.

[0015] Examples of aldehydes include formaldehyde, trioxane, furfural, paraformaldehyde, benzaldehyde, methylhemiformal, ethylhemiformal, propylhemiformal, salicylaldehyde, glyoxal, butylhemiformal, phenylhemiformal, acetaldehyde, propylaldehyde, phenylacetaldehyde, α-phenylpropylaldehyde, β-phenylpropylaldehyde, and the like. Examples of the aldehydes include aldehyde, o-hydroxybenzaldehyde, m-hydroxybenzaldehyde, p-hydroxybenzaldehyde, o-chlorobenzaldehyde, o-nitrobenzaldehyde, m-nitrobenzaldehyde, p-nitrobenzaldehyde, o-methylbenzaldehyde, m-methylbenzaldehyde, p-methylbenzaldehyde, p-ethylbenzaldehyde, pn-butylbenzaldehyde, etc. These aldehydes may be used alone or in combination of two or more. Examples of the acid catalyst include hydrochloric acid, sulfuric acid, phosphoric acid, formic acid, acetic acid, oxalic acid, butyric acid, lactic acid, benzenesulfonic acid, p-toluenesulfonic acid, and boric acid. These acid catalysts may be used alone or in combination of two or more. Metal salts such as zinc chloride or zinc acetate may also be used, or may be used in combination with an acid catalyst.

[0016] In addition, a silane coupling agent may be added to the novolac phenolic resin during the manufacturing process in order to improve mold strength. If a silane coupling agent is not added during the manufacturing process, the novolac phenolic resin may be used in combination with a silane coupling agent. Examples of the silane coupling agent include the silane coupling agents exemplified in the description of the acid-curable resin described below.

[0017] The resol type phenolic resin is obtained by reacting a phenol with an aldehyde in the presence of a basic catalyst. Examples of the phenols and aldehydes include the phenols and aldehydes exemplified above in the description of the novolac type phenolic resin. Examples of the basic catalyst include sodium hydroxide, potassium hydroxide, ammonia, hexamine, amines, etc. These basic catalysts may be used alone or in combination of two or more.

[0018] The resol type phenolic resin is usually obtained in a state of being dispersed in a solvent such as water (hereinafter, the resol type phenolic resin in this state will be referred to as "liquid resol type phenolic resin"). The resol type phenolic resin may be used in a liquid state, or the liquid resol type phenolic resin may be subjected to a dehydration treatment or the like to remove the solvent, and then dried at room temperature to be used in a solid state. In addition, a silane coupling agent may be added to the resol type phenolic resin during the manufacturing process in order to improve the mold strength. If a silane coupling agent is not added during the manufacturing process, the resol type phenolic resin may be used in combination with a silane coupling agent.

[0019] An example of a binder used in producing a mold by the amine cold box method is a two-component binder composed of a phenol resin solution and a polyisocyanate solution, both of which are dissolved in an organic solvent.

[0020] The alkaline phenol resin can be obtained by reacting one or more compounds selected from the group consisting of phenols and bisphenols (hereinafter referred to as "phenolic compounds") with aldehydes in an aqueous system in the presence of an alkali metal hydroxide by a conventional method. Examples of the phenols and aldehydes include the phenols and aldehydes exemplified above in the description of the novolac type phenolic resin. Examples of bisphenols include bisphenol A, bisphenol F, bisphenol C, bisphenol S, and bisphenol Z. As the phenol-based compound, either one of phenols and bisphenols may be used alone, or a mixture of phenols and bisphenols may be used.

[0021] Examples of the hydroxides of alkali metals include sodium hydroxide, potassium hydroxide, and lithium hydroxide. Among these, sodium hydroxide and potassium hydroxide are preferred. These hydroxides of alkali metals may be used alone or in combination of two or more.

[0022] Examples of the acid-hardening resin include furfuryl alcohol, furan resin, etc. Also, the resol type phenolic resin exemplified above may be used as the acid-hardening resin. Among these, furfuryl alcohol and furan resin are preferred, and furfuryl alcohol is more preferred.

[0023] Furan resin is a resin whose main raw materials are furfuryl alcohol, urea, formaldehyde, etc., and hardens through polycondensation while undergoing a dehydration reaction in the presence of an acid catalyst. The furan resin to be used preferably contains, as a main component, one or more condensates or co-condensates of either furfuryl alcohol or furfuryl alcohol and urea with aldehydes, and a mixture with furfuryl alcohol, and optionally contains at least one of a phenol and a bisphenol. Examples of the phenols and aldehydes include the phenols and aldehydes exemplified above in the description of the novolac type phenolic resin.

[0024] Particularly preferred embodiments of the furan resin include the following two: In the following, the (co)condensate means at least one of a condensate and a co-condensate. i) A mixture of a (co)condensate (a) obtained by condensing urea, furfuryl alcohol, and an aldehyde, furfuryl alcohol, and, if necessary, at least one of a phenol and a bisphenol. ii) A mixture of a condensation product of urea and an aldehyde, furfuryl alcohol, and, if necessary, at least one of a phenol and a bisphenol.

[0025] In addition to the above, the furan resin may also be, for example, a mixture of furfuryl alcohol and one or more selected from the group consisting of 2,5-bis(hydroxymethyl)furan, phenols, and bisphenols; or a mixture of a condensate of urea and aldehydes, furfuryl alcohol, and 2,5-bis(hydroxymethyl)furan.

[0026] The acid-curable resin may contain a silane coupling agent for the purpose of increasing the strength of the mold. Examples of the silane coupling agent include N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane, γ-aminopropyltriethoxysilane, γ-(2-aminoethyl)aminopropyltrimethoxysilane, and γ-glycidoxypropyltrimethoxysilane.

[0027] When the acid-curable resin contains a silane coupling agent, the content of the silane coupling agent is preferably 0.01 to 3 mass% based on the total mass of the solid content of the acid-curable resin, and more preferably 0.1 to 2 mass%. If the content of the silane coupling agent is equal to or greater than the lower limit, the effect of improving the strength of the mold can be sufficiently obtained. The effect of improving the strength of the mold tends to be more easily obtained as the content of the silane coupling agent increases, but if the content increases too much, the effect will simply plateau. Therefore, the content of the silane coupling agent is preferably 3 mass% or less. The solid content of the acid-curable resin refers to the non-volatile content at 100°C.

[0028] The acid-curable resin may contain a curing accelerator for the purpose of accelerating the curing rate. Examples of the hardening accelerator include resorcinol, formalin, furfural, etc. Among these, resorcinol is preferred because it also has the effect of reducing formaldehyde generated during mold making. When the acid-curable resin contains a curing accelerator, the content of the curing accelerator is preferably 1 to 20 mass %, more preferably 2 to 15 mass %, based on the total mass of the solid content of the acid-curable resin. If the content of the curing accelerator is equal to or greater than the lower limit, the curing speed is sufficiently increased. The curing speed tends to be increased as the content of the curing accelerator increases, but if the content is too high, the effect will simply plateau. Therefore, the content of the curing accelerator is preferably 20 mass % or less. From the viewpoint of reducing formaldehyde, urea, gallic acid, and pyrogallol may be used in addition to resorcinol.

[0029] (hardening agent) The hardener may be selected from known hardeners depending on the type of organic binder and the hardening method. For example, when a binder used in producing a mold by the shell molding method is used as the organic binder, hexamethylenetetramine is preferred as the hardener. When using a binder used in producing a mold by the amine cold box method as an organic binder, the hardener is preferably an amine gas such as triethylamine or diethylamine. These hardeners may be used alone or in combination of two or more. When an alkaline phenol resin is used as an organic binder, the curing agent is preferably methyl formate, ethyl formate, triacetin, diacetin, monoacetin, ethylene glycol diacetate, ethylene glycol monoacetate, γ-butyrolactone, propiolactone, ε-caprolactone, etc. in the self-hardening mold-making method, while highly volatile esters are preferred, with methyl formate, etc. being more preferred in the gas-hardening mold-making method. When an acid-curing resin is used as the organic binder, the curing agent is preferably an inorganic acid such as sulfuric acid, phosphoric acid, or hydrochloric acid; or an organic acid such as an organic sulfonic acid (e.g., xylenesulfonic acid, paratoluenesulfonic acid, benzenesulfonic acid, or methanesulfonic acid), or a carboxylic acid (e.g., formic acid, acetic acid, oxalic acid, lactic acid, maleic acid, malic acid, citric acid, tartaric acid, malonic acid, succinic acid, or benzoic acid). These curing agents may be used alone or in combination of two or more.

[0030] The hardener can be used in the form of an aqueous solution, that is, as an aqueous hardener solution. The content of the curing agent relative to the total mass of the aqueous curing agent solution is preferably from 20 to 75% by mass, and more preferably from 30 to 70% by mass. The content of water relative to the total mass of the aqueous hardener solution is preferably from 25 to 80 mass %, more preferably from 30 to 70 mass %. The aqueous hardener solution may contain a solvent other than water (another solvent), and examples of the other solvent include alcohols such as methanol, ethanol, and butanol.

[0031] (optional ingredient) Examples of the optional components include a silane coupling agent, a lubricant, a disintegrant, and a hardening accelerator. Examples of the silane coupling agent include the silane coupling agents exemplified above in the description of the acid-curable resin. The lubricant may, for example, be fatty acid amide or calcium stearate. Disintegrants include, for example, nitrates. Examples of the hardening accelerator include benzoic acid and salicylic acid.

[0032] (Method of Producing Template Precursor) The template precursor can be obtained, for example, by the following method (I) or method (II). Method (I): A method of producing a mold precursor by filling a mixture (hereinafter also referred to as "mixture (A)") containing a refractory granular material, an organic binder, and optional components as necessary, into a casting mold, and hardening the organic binder. Method (II): A method for producing a template precursor by three-dimensional additive manufacturing.

[0033] <<Method(I)>> In the method (I), the mixture (A) can be prepared by mixing, for example, a refractory granular material, an organic binder, and optionally optional components. The mixture (A) thus obtained is also called "mixed sand". The content of the organic binder in the mixture (A) is preferably 0.1 to 5 parts by mass, more preferably 0.5 to 3.5 parts by mass, based on 100 parts by mass of the refractory granular material. If the content of the organic binder is equal to or more than the lower limit, sufficient strength can be maintained until the hardening step described below. If the content of the organic binder is equal to or less than the upper limit, the mold after pouring can be easily dismantled. In addition, the amount of gas generated by thermal decomposition of the acid-hardening binder during pouring can be reduced.

[0034] Methods for hardening the organic binder include heat hardening, room temperature hardening, gas hardening, etc. Here, "room temperature hardening" means hardening at room temperature without external heating or gas ventilation. When the organic binder is cured by heat curing or room temperature curing, that is, when a mold is manufactured by a heat curing mold making method or a self-hardening mold making method, the mixture (A) preferably contains a curing agent. Hereinafter, the mixture (A) containing a curing agent is also referred to as "mixture (A1)". The content of the hardener in the mixture (A1) is preferably 0.1 to 0.5 parts by mass, more preferably 0.2 to 0.4 parts by mass, based on 100 parts by mass of the refractory granular material. If the content of the hardener is within the above range, a mold having higher strength is likely to be obtained.

[0035] The mixture (A1) can be prepared, for example, by mixing a refractory granular material, an organic binder, an aqueous hardener solution, and, if necessary, optional components. Alternatively, for example, the refractory granular material may be heated to a predetermined temperature, an aqueous hardener solution may be added to the heated refractory granular material to produce coated sand, and the resulting coated sand may be mixed with an organic binder and, if necessary, optional components to produce the mixture (A1). The heating temperature of the refractory granular material is preferably a temperature higher than the boiling point of the solvent contained in the aqueous hardener solution, and is usually 100 to 150°C.

[0036] When the organic binder is hardened by gas hardening, i.e., when a mold is produced by a gas hardening casting molding method, the mixture (A) is filled into a mold for casting, and the organic binder is hardened by passing a gaseous hardener through it. The flow rate and time of the gaseous hardener are not particularly limited as long as they are within the range of flow rate and time used in a typical gas-hardening mold-making process.

[0037] The organic binder is cured by a method such as heat curing, room temperature curing, or gas curing, to obtain a mold precursor made of a cured product of the mixture (A). The obtained mold precursor is removed from the mold. The mold precursor is able to maintain its shape due to the hardened organic binder, so it is not easily crumbled even when removed from the mold.

[0038] <<Method (II)>> In the case of method (II), a mold precursor is produced by repeating the steps of: laying out a layer of a mixture (hereinafter also referred to as "mixture (B)") containing a refractory granular material, a hardener, and, as necessary, optional components; and selectively injecting and hardening an organic binder into the layered covering sand so as to bond the layered mixture (B) in accordance with the desired three-dimensional additive object (hereinafter also referred to as "step (b)"). The organic binder used in the method (II) is preferably an acid-curing resin.

[0039] The mixture (B) can be prepared, for example, by mixing a refractory granular material, a hardener, and, if necessary, optional components. In addition, for example, the refractory granular material may be heated to a predetermined temperature and an aqueous hardener solution may be added to the heated refractory granular material to produce coated sand, which may then be used as mixture (B). Alternatively, the coated sand may be mixed with optional components as necessary and used as mixture (B).

[0040] The steps (a) and (b) are carried out as follows, for example, using a three-dimensional lamination device using a printing molding method. The three-dimensional lamination device preferably includes a blade mechanism, a print nozzle head mechanism, and a modeling table mechanism, and further includes a control unit that controls the operation of each mechanism using three-dimensional data of the object to be modeled. The blade mechanism includes a recoater, which applies a predetermined thickness of coated sand to the bottom surface of the metal case or to the top layer of the model that has already been bound with an organic binder. The printing nozzle head mechanism prints the stacked coated sand with an organic binder, binding the coated sand together to create a shape layer by layer. The modeling table mechanism lowers the distance of one layer when modeling of one layer is completed, achieving layered modeling with a specified thickness.

[0041] First, a three-dimensional lamination device using a printing molding method is used, and the mixture (B) is laminated on the bottom surface of a metal case installed in the three-dimensional lamination device by a blade mechanism having a recoater (step (a)). Next, on the laminated mixture (B), the print nozzle head is scanned by the print nozzle head mechanism based on the data obtained by designing the shape of the target three-dimensional laminated object (three-dimensional laminated mold) using 3D CAD, and an organic binder is printed (ejected) (step (b)). The bottom surface of the metal case is a modeling table, which can be moved up and down. After printing the organic binder, the bottom surface (modeling table) of the metal case is lowered by one layer, and the mixture (B) is laminated in the same manner as before (step (a)), and an organic binder is printed on it (step (b)). These lamination and printing operations are repeated until the target three-dimensional laminated object is formed. The thickness of one layer is preferably 100 to 500 μm, more preferably 200 to 300 μm.

[0042] The amount of the organic binder applied when printing is, in terms of solid content, preferably 0.4 parts by mass or more, more preferably 0.4 to 4.6 parts by mass, even more preferably 0.5 to 4 parts by mass, particularly preferably 0.6 to 3 parts by mass, and most preferably 0.7 to 2 parts by mass, per 100 parts by mass of the fire-resistant granular material in the mixture (B) for one layer in the printing area.

[0043] The mold precursor obtained by method (II) is shaped while being embedded in the powder of mixture (B). Therefore, the mixture (B) in the area where the organic binder is not printed (non-printed area) is removed with a brush or vacuum cleaner to extract the mold precursor. The mold precursor can maintain its shape due to the hardened organic binder, so it is not easily crumbled even when it is removed. In this specification, the template precursor obtained by method (II) is also referred to as a "three-dimensional additive manufacturing object."

[0044] <Impregnation process> The impregnation step is a step in which the template precursor is impregnated with colloidal silica and water glass separately. Colloidal silica is a dispersion of silica particles (SiO2) in water or an organic solvent. The colloidal silica is not particularly limited, and any conventionally known colloidal silica can be used. Examples of colloidal silica include aqueous colloidal silica that exhibits acidity, aqueous colloidal silica that exhibits alkalinity, and cationic colloidal silica.

[0045] Examples of acidic aqueous colloidal silica include products manufactured by Nissan Chemical Industries, Ltd. under the trade names SNOWTEX OXS (SiO2 solid content 10 mass%), SNOWTEX OS (SiO2 solid content 20 mass%), SNOWTEX O (SiO2 solid content 20 mass%), SNOWTEX O-40 (SiO2 solid content 40 mass%), SNOWTEX OL (SiO2 solid content 20 mass%), SNOWTEX OYL (SiO2 solid content 20 mass%) and SNOWTEX OUP (SiO2 solid content 15 mass%). Examples of aqueous colloidal silica exhibiting alkalinity include product names manufactured by Nissan Chemical Industries, Ltd.: SNOWTEX XS (SiO2 solid content 20% by mass), SNOWTEX 30 (SiO2 solid content 30% by mass), SNOWTEX 50-T (SiO2 solid content 48% by mass), SNOWTEX 30L (SiO2 solid content 30% by mass), SNOWTEX UP (SiO2 solid content 20% by mass), SNOWTEX NXS (SiO2 solid content 15% by mass), SNOWTEX NS (SiO2 solid content 20% by mass), SNOWTEX N (SiO2 solid content 20% by mass), SNOWTEX N-40 (SiO2 solid content 40% by mass), and the like. Examples of cationic colloidal silica include products manufactured by Nissan Chemical Industries, Ltd. under the trade names Snowtex AK (SiO2 solid content 20% by mass), Snowtex AK-L (SiO2 solid content 20% by mass), and Snowtex AK-YL (SiO2 solid content 30% by mass). Examples of colloidal silica dispersed in an organic solvent include Nissan Chemical Co., Ltd.'s product names: Organosilica sol IPA-ST (SiO2 solid content 30 mass%, solvent isopropyl alcohol) and Methanol silica sol (SiO2 solid content 30 mass%, solvent methyl alcohol). These colloidal silicas may be used alone or in combination of two or more kinds.

[0046] The method for impregnating the colloidal silica is not particularly limited, and examples thereof include a method of immersing the template precursor in colloidal silica (dipping method); a method of applying colloidal silica to the template precursor by flow coating (spraying) method, spraying method, brush coating method, etc.

[0047] The impregnated amount of colloidal silica is preferably 1 to 10% by mass, more preferably 2 to 8% by mass, and even more preferably 3 to 7% by mass. If the impregnated amount of colloidal silica is equal to or greater than the lower limit, the molar ratio (SiO2 / M) of SiO2 to M (M=K2O or Na2O) of the entire mold is sufficiently increased, and the heat resistance of the mold is further improved. If the impregnated amount of colloidal silica is equal to or less than the upper limit, the strength of the mold can be maintained without increasing the molar ratio too much. Hereinafter, in this specification, the molar ratio (SiO2 / M) of SiO2 to M (M=K2O or Na2O) in the entire template is also referred to as the "molar ratio of the template." The method for determining the impregnated amount of colloidal silica will be described in detail in the Examples below.

[0048] The water glass is not particularly limited, and any known water glass can be used, such as sodium silicate (specifically, No. 1, No. 2, No. 3 and sodium metasilicate (Type 1 and Type 2) described in JIS K 1408:1966), potassium silicate, or a mixture thereof. The molar ratio (SiO2 / M) of SiO2 to M (M=K2O or Na2O) in the water glass is preferably 1.9 to 4.0, more preferably 2.0 to 3.5, even more preferably 2.0 to 3.2, particularly preferably 2.0 or more and less than 3.1, and most preferably 2.1 to 3.0. When the molar ratio of water glass is equal to or more than the lower limit, a sufficient hardening speed can be obtained. When the molar ratio of water glass is equal to or less than the upper limit, the water glass is unlikely to precipitate, and the water glass is sufficiently impregnated into the template precursor.

[0049] The method for impregnating with water glass is not particularly limited, but may be the same as the method for impregnating with colloidal silica. The amount of water glass impregnated is preferably 1 to 10% by mass, more preferably 2 to 8% by mass, and even more preferably 3 to 7% by mass. If the amount of water glass impregnated is equal to or more than the lower limit, the molar ratio of the mold is sufficiently increased, and the heat resistance of the mold is further improved. If the amount of water glass impregnated is equal to or less than the upper limit, the amount of alkali metal in the mold can be suppressed, and a decrease in the molar ratio of the mold can be prevented. The method for determining the amount of impregnation of water glass will be described in detail in the Examples below.

[0050] The order in which the colloidal silica and water glass are impregnated into the template precursor is not particularly limited. When the step of impregnating the template precursor with colloidal silica is designated as "step (α)" and the step of impregnating the template precursor with water glass is designated as "step (β)", step (β) may be performed after step (α), or step (α) may be performed after step (β). Furthermore, step (α) and step (β) may be performed repeatedly. From the viewpoint of increasing the molar ratio of the template and further improving the heat resistance of the template, it is preferable to carry out the step (β) after the step (α).

[0051] A drying step may be carried out between step (α) and step (β), or between step (β) and step (α). In particular, when step (β) is carried out after step (α), it is preferable to carry out a drying step between step (α) and step (β) from the viewpoints of making it easier for colloidal silica to adhere sufficiently to the refractory granular material and suppressing precipitation of water glass on the mold surface. When a drying step is performed between step (α) and step (β), the drying temperature is preferably 100 to 200°C, more preferably 110 to 150°C, and even more preferably 120 to 130°C. When the drying temperature is equal to or higher than the lower limit, the removal of the solvent contained in the colloidal silica and the hardening of the binder in the mold can be further enhanced. When the drying temperature is equal to or lower than the upper limit, the decomposition of the binder in the mold can be suppressed. The drying time is not particularly limited and may be appropriately determined depending on the shape and size of the mold. When a drying step is carried out between step (β) and step (α), the drying temperature is preferably 100 to 200°C, more preferably 110 to 150°C, and even more preferably 120 to 130°C. When the drying temperature is equal to or higher than the lower limit, the removal of the solvent contained in the water glass and the hardening of the binder in the mold can be enhanced. When the drying temperature is equal to or lower than the upper limit, the decomposition of the binder in the mold can be suppressed. The drying time is not particularly limited and may be appropriately determined depending on the shape and size of the mold. When a drying step is carried out, it is preferable to cool the template precursor to room temperature (25° C.) after the drying step, and then carry out step (α) or step (β).

[0052] <Curing process> The hardening step is a step of hardening the water glass impregnated into the template precursor. The curing temperature is preferably 100 to 300°C, more preferably 100 to 250°C, and even more preferably 100 to 200°C. If the curing temperature is equal to or higher than the lower limit, the water glass will be sufficiently cured in a short time. If the drying temperature is equal to or lower than the upper limit, decomposition of the binder in the mold can be suppressed, and the strength at room temperature is excellent. When the above-mentioned drying step is performed, the curing temperature is preferably higher than the drying temperature. The curing time is not particularly limited and may be appropriately determined depending on the shape and size of the mold.

[0053] The molar ratio of the mold after the curing step is preferably 4 to 10, more preferably 5 to 9, and even more preferably 6 to 8. If the molar ratio of the mold is equal to or greater than the lower limit, the heat resistance of the mold is improved. As a result, the mold can maintain its shape well while maintaining a strength sufficient to withstand exposure to high temperatures. In particular, even if the mold has a complex shape, the shape can be well maintained. The higher the molar ratio of the mold, the higher the heat resistance tends to be, but if the molar ratio is too high, the adhesive strength as an inorganic binder may decrease, and the strength may decrease. If the molar ratio of the mold is within the above range, the mold has an excellent balance between heat resistance and strength. In particular, when the precursor template is produced by the method (ii), the molar ratio of the template after the curing step is preferably 5-9, and more preferably 5.5-7. The method for determining the molar ratio of the template will be described in detail in the Examples below.

[0054] After the water glass has hardened, it is cooled to room temperature (25°C) (cooling step) to obtain a mold (hardened body). As the cooling method, a known method can be used, for example, a method of natural cooling at room temperature, a method of forced cooling using a blower, etc.

[0055] The mold (hardened body) obtained in the hardening process contains hardened organic binders and hardened inorganic binders (mainly hardened water glass), but the organic binders and their hardened products may thermally decompose when pouring. When the organic binders and their hardened products thermally decompose, gas (pyrolysis gas) is generated, which may cause defects in the casting or worsen the working environment due to odors. Therefore, when it is desired to remove the organic binder and its hardened material from the mold, it is preferable to carry out the firing step described below. When the baking step is carried out after the hardening step, it is not necessary to provide a cooling step between the hardening step and the baking step.

[0056] <Firing process> The firing step is a step of firing the mold (hardened body) obtained in the hardening step. By carrying out the firing step, the organic binder contained in the hardened body and the hardened material thereof are thermally decomposed and gasified, and are removed from the mold as pyrolysis gas. The mold (fired body) obtained in the firing step contains a hardened inorganic binder (mainly hardened water glass).

[0057] The firing temperature may be determined depending on the type of organic binder contained in the hardened body, but is preferably equal to or higher than the decomposition temperature of the organic binder and lower than the decomposition temperatures of colloidal silica and water glass. Specifically, the firing temperature is preferably 350 to 1000° C., and more preferably 400 to 800° C. If the firing temperature is equal to or higher than the lower limit, the organic binder and its hardened material are sufficiently thermally decomposed. If the firing temperature is equal to or lower than the upper limit, colloidal silica and water glass, and hardened materials such as water glass are unlikely to be thermally decomposed. The baking time is not particularly limited as long as it is a time that allows the organic binder contained in the hardened body and the hardened product thereof to be sufficiently thermally decomposed, and may be appropriately determined depending on the shape and size of the mold. The cured product can be baked by any known method, such as a method using an electric furnace or an oven.

[0058] After firing the hardened body, it is cooled to room temperature (25°C) (cooling step) to obtain a mold (fired body). As the cooling method, a known method can be used, for example, a method of natural cooling at room temperature, a method of forced cooling using a blower, etc.

[0059] <Action and effect> As described above, conventionally, there are known methods for producing a mold by impregnating a mold (mold precursor) made with an organic binder with water glass, or for producing a mold by three-dimensional additive manufacturing using water glass. Since a high molar ratio of water glass causes precipitation and tends to reduce the impregnation ability of the water glass, it is common to use water glass with a low molar ratio. However, because low-molar ratio water glass has a low melting point, a mold made using low-molar ratio water glass has low heat resistance and is not suitable for casting products that require high pouring temperatures. If the mold has low heat resistance, casting defects such as seizure and glare, or deformation, may occur.

[0060] According to the method for producing a mold of the present embodiment, the mold precursor made of an organic binder is impregnated with colloidal silica and water glass separately, so that the molar ratio of the mold is increased, a mold with excellent heat resistance can be produced, and the mold shape can be well maintained while maintaining a strength sufficient to withstand exposure to high temperatures. In addition, since there is no need to use water glass with a high molar ratio, the mold precursor can be sufficiently impregnated with water glass.

[0061] In addition, if the method involves mixing the refractory granular material with a binder and filling the resulting mixed sand into a mold for casting, water glass with a high molar ratio can also be used as the binder, but this method is not suitable for producing molds with complex shapes. However, with the method for producing a template of the present embodiment, it is also possible to produce a template precursor by three-dimensional additive manufacturing, and even templates with complex shapes can be easily produced.

[0062] Furthermore, in the mold manufacturing method of this embodiment, it is not necessary to increase the curing temperature in the curing step more than necessary, and the water glass is sufficiently cured at a relatively low temperature, for example, about 100 to 300° C. Therefore, the organic binder and its cured product in the mold precursor are not easily thermally decomposed during the curing step, and the binding power of the water glass, which is an inorganic binder, is fully exerted before the organic binder and its cured product are thermally decomposed, so that even molds with complex shapes are not easily deformed, and molds with good dimensional accuracy can be easily obtained. Moreover, if the firing step is carried out after the hardening step, the organic binder and its hardened material are sufficiently removed from the mold, so that the organic binder and its hardened material are less likely to generate pyrolysis gas during casting, which makes it possible to improve the working environment during casting and to suppress defects in the casting caused by pyrolysis gas. EXAMPLES

[0063] The present invention will be described in detail below with reference to examples, but the present invention is not limited to these. The materials used in each example are shown below. Various measurement methods are also shown below.

[0064] [Materials used] As the refractory granular material, artificial sand obtained by a sintering method (containing 95 mass% of Al2O3-SiO2, product name "CB-X#1450" manufactured by Itochu Ceratec Corporation, particle size 53 to 150 μm) was used.

[0065] As the organic binder, the following was used. Organic binder (i): A furan-based binder which is a mixture of 87.8 parts by mass of furfuryl alcohol, 10.0 parts by mass of bisphenol A, 2.0 parts by mass of resorcinol, and 0.2 parts by mass of N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane. Organic binder (ii): A furan-based binder which is a mixture of 89.8 parts by mass of furfuryl alcohol, 10.0 parts by mass of resorcinol, and 0.2 parts by mass of N-β(aminoethyl)γ-aminopropylmethyldimethoxysilane.

[0066] The following hardeners were used. Hardener (iii): An aqueous hardener solution which is a mixture of 55 parts by mass of xylene sulfonic acid, 10 parts by mass of sulfuric acid, and 35 parts by mass of water. · Hardener (iv): A hardener aqueous solution which is a mixture of 60 parts by mass of xylene sulfonic acid and 40 parts by mass of water.

[0067] As the colloidal silica, a dispersion liquid in which silica particles having an average particle size of 9 nm were dispersed in water (manufactured by Nissan Chemical Industries, Ltd., product name "Snowtex OS", SiO2 solid content 20 mass %) was used.

[0068] The water glass used was as follows: Water glass (v): An aqueous solution of sodium silicate (molar ratio (SiO2 / Na2O): 2.1) manufactured by Fuji Chemical Industry Co., Ltd., to which water has been added, and the specific gravity at 25°C is adjusted to 1.242. Water glass (vi): An aqueous solution of sodium silicate (molar ratio (SiO2 / Na2O): 2.3) manufactured by Fuji Chemical Industry Co., Ltd., to which water has been added, and the specific gravity at 25°C is adjusted to 1.214. Water glass (vii): An aqueous solution of sodium silicate (molar ratio (SiO2 / Na2O): 2.5) manufactured by Fuji Chemical Industry Co., Ltd., to which water has been added, and the specific gravity at 25°C is adjusted to 1.210. Water glass (viii): An aqueous solution of sodium silicate (molar ratio (SiO2 / Na2O): 2.7) manufactured by Fuji Chemical Industry Co., Ltd., to which water has been added, and the specific gravity at 25°C is adjusted to 1.206. Water glass (ix): An aqueous solution of sodium silicate (molar ratio (SiO2 / Na2O): 3.2) manufactured by Fuji Chemical Industry Co., Ltd., to which water has been added, and the specific gravity at 25°C is adjusted to 1.174.

[0069] [Calculation method] <Calculation of impregnated amount of colloidal silica> The mass of the template precursor just before impregnation with colloidal silica (W A The mass (W BThe impregnated amount of colloidal silica (S) was calculated from the following formula (1). Impregnated amount of colloidal silica [mass%] = (W B -W A ) / W A ×100 ···(1)

[0070] <Calculation of the amount of water glass impregnated> The mass of the direct casting precursor before impregnation with water glass (W C The mass (W D The impregnated amount of water glass (G) was calculated from the following formula (2). Water glass impregnation amount [mass%] = (W D -W C ) / W C ×100 ···(2)

[0071] <Calculation of the total impregnated amount of colloidal silica and water glass> When the mold was produced without performing a drying step between the step (α) and the step (β), or between the step (β) and the step (α), the total impregnated amount of colloidal silica and water glass was calculated as follows. The mass (W E The mass (W F The impregnated amount of colloidal silica was calculated from the following formula (3). Total impregnation amount [mass%] = (W F -W E ) / W E ×100 (3)

[0072] <Calculation of template molar ratio> The molar ratio (SiO2 / Na2O) of the mold (test piece) was calculated from the following formula (4). Note that M1 in the following formula (4) was calculated from the following formula (5), and M2 in the following formula (4) was calculated from the following formula (6). SiO2 / Na2O=M2 / M1 (4) M1[mol]=(G / 100) / (60.1×N+62.0) ···(5) M2[mol]=(M1×N)+{(S / 100) / 60.1} ···(6) In addition, in the formulas (5) and (6), "N" is the molar ratio of the water glass impregnated into the template precursor, "G" is the impregnated amount of the water glass, and "S" is the impregnated amount of the colloidal silica.

[0073] [Measurement method] <Measurement of bending strength> The bending strength of the test pieces obtained in each of the Examples and Comparative Examples was measured using the measurement method described in JACT Test Method SM-1.

[0074] <Gas generation rate measurement> The mold was heat-treated in an atmosphere of 1000°C for 5 minutes, exposing the mold to the same atmosphere as when the casting was produced. The amount of gas generated during the heat treatment was measured according to JACT test method M-5 "Gas generation amount measurement method".

[0075] [Example 1] <Preparation of template precursor> 100 parts by mass of the refractory granular material and 0.3 parts by mass of the hardener (iii) were added to a mixer and stirred for 1 minute. Then, 1.5 parts by mass of the organic binder (i) was added and stirred for another minute to obtain a mixture (A1-1). The obtained mixture (A1-1) was immediately poured into a wooden mold for preparing a mold precursor, which had a rectangular shape of 10 mm in length, 60 mm in width, and 10 mm in height, under conditions of a temperature of 25°C and a humidity of 50%, and allowed to harden. Three hours after the start of hardening, a rectangular mold precursor of 10 mm in length, 60 mm in width, and 10 mm in height was removed from the wooden mold (mold removal time: 3 hours) and left for 24 hours from the start of hardening under conditions of a temperature of 25°C and a humidity of 50%.

[0076] <Test piece manufacturing> The mold precursor after standing was impregnated with colloidal silica at room temperature (25°C) for 60 seconds (step (α)), and then heat-treated at 120°C for 1 hour (drying step). The mold precursor after the drying step was cooled to room temperature (25°C), impregnated with water glass (v) at room temperature (25°C) for 60 seconds (step (β)), and then heat-treated at 200°C for 1 hour (hardening step). The mold precursor after the hardening step was cooled to room temperature (25°C) to obtain a test piece (hardened body). The step (α) was carried out by immersing the template precursor in colloidal silica, and the step (β) was carried out by immersing the template precursor in water glass. The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (hardened body) as a mold were calculated. The results are shown in Table 1. The bending strength and gas generation rate of the obtained test pieces (cured bodies) were measured. The results are shown in Table 1. Separately, a test piece (cured body) was heat-treated for 5 minutes in an electric furnace set at 800° C. The bending strength of the test piece was measured immediately after it was taken out of the electric furnace. The results are shown in Table 1.

[0077] [Examples 2 to 5] Test pieces (hardened bodies) were produced and various measurements were carried out in the same manner as in Example 1, except that the types of water glass shown in Table 1 were used. The results are shown in Table 1.

[0078] [Comparative Example 1] A template precursor was produced in the same manner as in Example 1. The template precursor after standing was heat-treated at 120° C. for 1 hour and used as a test piece for various measurements, etc. The results are shown in Table 2.

[0079] [Comparative Example 2] Except for not carrying out the step (β) and the curing step, a test piece was produced in the same manner as in Example 1, and various measurements were carried out. The results are shown in Table 2.

[0080] [Comparative Examples 3 to 7] Test pieces were produced in the same manner as in Example 1, except that the types of water glass shown in Table 1 were used and the step (α) and the drying step were not performed, and various measurements were carried out. The results are shown in Table 2.

[0081] [Table 1]

[0082] [Table 2]

[0083] From the results in Table 1, the test pieces (cured bodies) obtained in Examples 1 to 5 had high bending strength even when heat-treated at a high temperature of 800° C., and had heat resistance sufficient to withstand exposure to high temperatures. In addition, no change in shape was observed even when heat-treated at a high temperature of 800° C. In contrast, the results in Table 2 show that the test pieces obtained in Comparative Examples 1 and 2 collapsed when they were removed from the electric furnace after being heat-treated at a high temperature of 800°C, and therefore the bending strength could not be measured, indicating that they had poor heat resistance. The test pieces obtained in Comparative Examples 3 to 7 were deformed when they were heat-treated at a high temperature of 800° C. and removed from the electric furnace, so that the bending strength could not be measured and they were poor in heat resistance.

[0084] [Examples 6 to 10] Test pieces (hardened bodies) were produced in the same manner as in Example 1, except that the types of water glass shown in Table 3 were used. The obtained test piece (hardened body) was heat-treated for 1 hour in an electric furnace set at 800°C (firing process). The temperature inside the electric furnace was allowed to cool until it reached 32°C, during which time the mold precursor after the firing process was left in the electric furnace, and then removed from the electric furnace and further cooled to room temperature (25°C) to obtain a test piece (firing body). The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (fired body) as a template were calculated. The results are shown in Table 3. The bending strength and gas generation rate of the obtained test pieces (fired bodies) were measured. The results are shown in Table 3. Separately, the test piece (sintered body) was heat-treated for 5 minutes in an electric furnace set at 800° C. The bending strength of the test piece was measured immediately after it was taken out of the electric furnace. The results are shown in Table 3.

[0085] [Comparative Example 8] Test pieces (hardened bodies) were produced in the same manner as in Example 1, except that the types of water glass shown in Table 3 were used and the step (α) and the drying step were not carried out. The obtained test piece (hardened body) was heat-treated for 1 hour in an electric furnace set at 800°C (firing process). The temperature inside the electric furnace was allowed to cool until it reached 32°C, during which time the mold precursor after the firing process was left in the electric furnace, and then removed from the electric furnace and further cooled to room temperature (25°C) to obtain a test piece (firing body). The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (fired body) as a template were calculated. The results are shown in Table 3. The bending strength and gas generation rate of the obtained test pieces (fired bodies) were measured. The results are shown in Table 3. Separately, the test piece (sintered body) was heat-treated for 5 minutes in an electric furnace set at 800° C. The bending strength of the test piece was measured immediately after it was taken out of the electric furnace. The results are shown in Table 3.

[0086] [Table 3]

[0087] From the results in Table 3, the test pieces (sintered bodies) obtained in Examples 6 to 10 had high bending strength even when heat-treated at a high temperature of 800° C., and had heat resistance sufficient to withstand exposure to high temperatures. Furthermore, no change in shape was observed even when heat-treated at a high temperature of 800° C. In addition, the test pieces (sintered bodies) obtained in Examples 6 to 10 generated a small amount of gas. In contrast, the test piece obtained in Comparative Example 8 had a lower bending strength after heat treatment at a high temperature of 800° C. than the test pieces obtained in Examples 6 to 10, and was inferior in heat resistance.

[0088] [Example 11] Test pieces (hardened bodies) were produced and various measurements were carried out in the same manner as in Example 1, except that the types of water glass shown in Table 4 were used. The results are shown in Table 4.

[0089] [Example 12] Test pieces (hardened bodies) were produced in the same manner as in Example 1, except that the types of water glass shown in Table 4 were used and the order of steps (α) and (β) was reversed, and various measurements were performed. The results are shown in Table 4.

[0090] [Example 13] Test pieces (hardened bodies) were produced in the same manner as in Example 1, except that the types of water glass shown in Table 4 were used and the drying step between step (α) and step (β) was not performed, and various measurements were performed. The results are shown in Table 4.

[0091] [Example 14] Test pieces (hardened bodies) were produced in the same manner as in Example 1, except that the types of water glass shown in Table 4 were used, the order of steps (α) and (β) was reversed, and the drying step between steps (β) and (α) was not performed, and various measurements were performed. The results are shown in Table 4.

[0092] [Table 4]

[0093] The results in Table 4 show that the test pieces (cured bodies) obtained in Examples 11 to 14 had high bending strength even when heat-treated at a high temperature of 800° C., and had sufficient heat resistance to withstand exposure to high temperatures. In particular, the test pieces (cured bodies) obtained in Examples 11 and 13 did not show any change in shape even when they were heat-treated at a high temperature of 800°C. The test pieces (cured bodies) obtained in Examples 12 and 14 were found to have undergone slight changes in shape when heat-treated at a high temperature of 800° C., but this was not of any practical concern. Further, the test piece (cured product) obtained in Example 13 had slight deposits on the surface, but these were not of any practical concern.

[0094] [Example 15] <Preparation of template precursor> 100 parts by mass of the refractory granular material was heated to 120° C. Next, 0.5 parts by mass of the hardener (iv) was added to the heated refractory granular material, and the mixture was stirred for 3 minutes to obtain a mixture (B-1). Using a three-dimensional additive manufacturing device using a printing method (product name "Sand Mold Additive Manufacturing Device SCM-800" manufactured by CMET Co., Ltd.), the mixture (B-1) was laminated on the bottom surface of a metal case installed in the three-dimensional additive manufacturing device by a blade mechanism having a recoater (step (a)). At this time, the shutter opening angle of the recoater was set to 49.5°. Next, the print nozzle head was scanned on the laminated mixture (B-1) based on the data obtained by designing the shape of the mold precursor using 3D CAD, and the organic binder (ii) was printed at a discharge amount of 2.0 parts by mass per 100 parts by mass of the refractory granular material in the mixture (B-1) for one layer (step (b)). After printing the organic binder (ii), the bottom surface (modeling table) of the metal case was lowered by one layer (280 μm), and the mixture (B-1) was laminated in the same manner as above (step (a)), and the organic binder (ii) was printed thereon at a discharge amount of 2.0 parts by mass per 100 parts by mass of the refractory granular material in the mixture (B-1) for one layer (step (b)). After repeating these steps (a) and (b), the mixture (B-1) in the non-printed portion of the organic binder (ii) was removed with a brush to obtain a rectangular parallelepiped mold precursor with a length of 10 mm, a width of 60 mm, and a height of 10 mm.

[0095] <Test piece manufacturing> The template precursor was impregnated with colloidal silica at room temperature (25°C) for 60 seconds (step (α)), and then heated at 120°C for 1 hour (drying step). The template precursor after the drying step was cooled to room temperature (25°C), impregnated with water glass (v) at room temperature (25°C) for 60 seconds (step (β)), and then heated at 200°C for 1 hour (hardening step). The template precursor after the hardening step was cooled to room temperature (25°C) to obtain a test piece (hardened body). The step (α) was carried out by immersing the template precursor in colloidal silica, and the step (β) was carried out by immersing the template precursor in water glass. The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (hardened body) as a mold were calculated. The results are shown in Table 5. The bending strength and gas generation rate of the obtained test pieces (cured bodies) were measured. The results are shown in Table 5. Separately, the test piece (cured body) was heat-treated for 5 minutes in an electric furnace set at 800° C. The bending strength of the test piece was measured immediately after it was taken out of the electric furnace. The results are shown in Table 5.

[0096] [Example 16] A test piece (cured product) was produced in the same manner as in Example 15. The obtained test piece (hardened body) was heat-treated for 1 hour in an electric furnace set at 800°C (firing process). The temperature inside the electric furnace was allowed to cool until it reached 32°C, during which time the mold precursor after the firing process was left in the electric furnace, and then removed from the electric furnace and further cooled to room temperature (25°C) to obtain a test piece (firing body). The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (fired body) as a template were calculated. The results are shown in Table 5. The bending strength and gas generation rate of the obtained test pieces (fired bodies) were measured. The results are shown in Table 5. Separately, the test piece (sintered body) was heat-treated for 5 minutes in an electric furnace set at 800° C. The bending strength of the test piece was measured immediately after it was taken out of the electric furnace. The results are shown in Table 5.

[0097] [Comparative Example 9] A template precursor was prepared in the same manner as in Example 15. The template precursor was heat-treated at 120° C. for 1 hour and used as a test piece for various measurements. The results are shown in Table 5.

[0098] [Comparative Example 10] Test pieces were produced in the same manner as in Example 15, except that the step (α) and the drying step were not performed, and various measurements were carried out. The results are shown in Table 5.

[0099] [Table 5]

[0100] From the results of Table 5, the test piece (hardened body) obtained in Example 15 and the test piece (sintered body) obtained in Example 16 had high bending strength even when heat-treated at a high temperature of 800°C, and had heat resistance to a degree that could withstand exposure to high temperatures. In addition, no change in shape was observed even when heat-treated at a high temperature of 800°C. In particular, the test piece (sintered body) obtained in Example 16 also generated a small amount of gas. In contrast, the test piece obtained in Comparative Example 9 was heat-treated at a high temperature of 800° C. and collapsed when removed from the electric furnace, so that the bending strength could not be measured and the heat resistance was poor. The test piece obtained in Comparative Example 10 was deformed when it was heat-treated at a high temperature of 800° C. and removed from the electric furnace, so that the bending strength could not be measured and the heat resistance was poor.

[0101] [Example 17] A template precursor was produced in the same manner as in Example 15, except that the shape of the template precursor was designed using 3D CAD so as to have the shape shown in FIG. Using the obtained mold precursor, a test piece (cured body) was produced in the same manner as in Example 15, except that the drying time in the drying step was changed to 3.5 hours and the curing time in the curing step was changed to 2.5 hours. The obtained test piece (hardened body) was heat-treated for 1 hour in an electric furnace set at 800°C (firing process). The temperature inside the electric furnace was allowed to cool until it reached 32°C, during which time the mold precursor after the firing process was left in the electric furnace, and then removed from the electric furnace and further cooled to room temperature (25°C) to obtain a test piece (firing body). The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (fired body) as a template were calculated. The results are shown in Table 6. A photograph of the obtained test piece (fired body) is shown in Figure 2. The distance R2 in Figure 2 was measured and found to be 18.39 mm. The difference (R1-R2) between the distance R1 (20 mm) in Figure 1 and the distance R2 (18.39 mm) in Figure 2 was 1.61 mm, which was determined as the amount of deformation.

[0102] [Comparative Example 11] A template precursor was produced in the same manner as in Example 15, except that the shape of the template precursor was designed using 3D CAD so as to have the shape shown in FIG. Using the obtained mold precursor, a test piece (cured product) was produced in the same manner as in Example 15, except that the curing time in the curing step was changed to 2.5 hours and the step (α) and the drying step were not performed. The obtained test piece (hardened body) was heat-treated for 1 hour in an electric furnace set at 800°C (firing process). The temperature inside the electric furnace was allowed to cool until it reached 32°C, during which time the mold precursor after the firing process was left in the electric furnace, and then removed from the electric furnace and further cooled to room temperature (25°C) to obtain a test piece (firing body). The impregnated amounts of colloidal silica and water glass and the molar ratio of the test piece (fired body) as a template were calculated. The results are shown in Table 6. FIG. 3 shows a photograph of the obtained test piece (fired body).

[0103] [Table 6]

[0104] As shown in FIG. 2, the test piece (hardened body) obtained in Example 17 had a complex shape, but even when heat-treated at a high temperature of 800°C, the deformation amount at the most deformed point was 1.61 mm, and it was difficult to deform. In contrast, as shown in FIG. 3, the test piece (hardened body) obtained in Comparative Example 11 was significantly deformed when heat-treated at a high temperature of 800° C., and was poor in heat resistance.

Claims

1. an impregnation step of separately impregnating a mold precursor, which is a hardened mixture containing a refractory granular material and an organic binder, with colloidal silica and water glass; a hardening step of hardening the water glass impregnated into the template precursor; A method for producing a mold, comprising:

2. The method for producing a mold according to claim 1 , further comprising a baking step after the curing step.

3. The method for producing a template according to claim 1 or 2, wherein the template precursor is produced by three-dimensional additive manufacturing.

Citation Information

Patent Citations

  • Method of making core

    JP1977011127A

  • Mould molding method

    JP1991248740A

  • Casting mold and its manufacture

    JP1996174144A

  • Method for manufacturing casting mold for precision casting