Method and apparatus for synthesizing diamond by CVD

By employing plasma compression, DC/RF hybridization, and magnetic fields, the method enhances diamond deposition rates, addressing inefficiencies in existing CVD methods and enabling cost-effective large-scale diamond synthesis.

JP7575376B2Active Publication Date: 2024-10-29DIAROTECH
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2021521888
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-07-05
Filing Date
2019-06-18
Publication Date
2024-10-29
Estimated Expiration
2039-06-18

AI Technical Summary

Technical Problem

Existing methods for diamond synthesis by chemical vapor deposition (CVD) are limited by slow deposition rates, contamination, and equipment inefficiencies, making large-scale industrial application economically unviable.

Method used

A method involving plasma compression, hybridization of direct current (DC) and radio frequency (RF) energy sources, and application of a magnetic field near the substrate to enhance the concentration and collision probability of reactive carbon atoms, thereby increasing deposition rates.

Benefits of technology

Significantly accelerates diamond deposition rates, allowing for thicker and more uniform diamond layers with improved efficiency and reduced production costs, applicable to various technological applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575376000002
    Figure 0007575376000002
  • Figure 0007575376000003
    Figure 0007575376000003
  • Figure 0007575376000004
    Figure 0007575376000004
Patent Text Reader

Abstract

The present invention relates to improvements in chemical vapor deposition synthesis, particularly diamond synthesis, and proposes to reduce the time required for diamond layer deposition by compressing the plasma in the vicinity of the deposition substrate in order to increase the chance of collisions between activated species.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to the synthesis of diamond, or any other allotrope of carbon, by chemical vapour deposition. [Background technology]

[0002] Carbon is a substance that occurs naturally in the solid state on Earth in several allotropes, namely amorphous carbon and three crystallized forms: graphite, diamond, and lonsdaleite. Diamond is primarily a sp 3 composed of hybridized carbon atoms, whereas graphite is composed mainly of sp 2 It is composed of hybridized carbon. Other allotropes exist in synthetic forms, for example DLC.

[0003] Diamond is a material that has a unique combination of properties, e.g. wear resistance, thermal conductivity or electrical insulation, that make it extremely useful for many technical applications. Natural diamond cannot be used on a large scale due to its rarity and price, and is restricted to its use as a fine jewel. However, in the last decades, methods have been developed to synthesize diamond, with the aim of utilizing this material on a larger scale for technical applications.

[0004] DLC, or "Diamond-Like Carbon," is also a useful material. 3 sp in hybridized carbon 2 It differs from diamond in its hybridized carbon (up to 60% content).

[0005] The preferred method for synthesizing thin layers of diamond or DLC on a substrate is low pressure chemical vapor deposition, or CVD, in which a carbon atom-containing carrier gas is introduced into a chamber, and when the gas is converted into a plasma by an energy source, diamond is deposited in crystalline form on a substrate placed in the chamber.

[0006] Several technologies can be used to create the plasma, such as direct current, arc, hot filament or microwave, and several other methods. The devices currently dominating the market use microwave or hot filament.

[0007] The main drawback of these methods is the extremely slow rate of diamond deposition. Hot filament techniques can produce diamond layers of about 1 μm in one hour. These diamond layers are also often contaminated by components of the filament. Microwaves improve the deposition rate to about 45 μm per hour, but the wavelength of microwaves limits the deposition diameter technically to about 16 mm. Thus, significantly long reaction times are required to produce extremely thin diamond layers. This makes these methods industrially unusable in terms of energy costs, equipment working time efficiency, and therefore manufacturing costs. These limitations of existing methods are provided in detail by A. Tallaire in CR Physique 14 (2013), pp. 169-184. Thus, synthetically thinned diamond remains limited for the time being to applications in the mining or oil drilling sectors. Summary of the Invention [Problem to be solved by the invention]

[0008] In order to make diamond technically and economically viable for many technical applications, the Applicant considered it necessary to propose a method for the synthesis of diamond with improved deposition rates, a problem which led to the present invention of the present application. [Means for solving the problem]

[0009] To this end, the present invention relates first to a method for synthesizing diamond on a synthesis substrate between two plasma-generating electrodes in a vapor deposition chamber, the method comprising the steps of: A carbon atom-containing carrier gas is introduced into the chamber; - a method in which a plasma is created in the vicinity of a substrate to generate reactive carbon atoms, The method is characterized in that the plasma is compressed to increase the volume density of reactive carbon atoms near the substrate, thereby increasing the deposition rate.

[0010] The invention also relates to a method for synthesizing diamond on a synthesis substrate (5) between two plasma generating electrodes (4, 5) in a vapor deposition chamber (1), comprising the steps of: A carbon atom-containing carrier gas is introduced into the chamber (1); - a method in which a plasma (28) is created in the vicinity of a substrate to generate reactive carbon atoms, The method is characterized in that a plasma is created by applying a direct current (DC) (6) and a radio frequency (RF) (46) alternating current between two electrodes.

[0011] Finally, the invention also relates to a method for synthesizing diamond on a synthesis substrate (5) between two plasma-generating electrodes (4, 5) in a vapor deposition chamber (1), comprising the steps of: A carbon atom-containing carrier gas is introduced into the chamber (1); - a method in which a plasma (28) is created in the vicinity of a substrate to generate reactive carbon atoms, The method is characterized in that a magnetic field (51) is applied in the vicinity of the substrate.

[0012] The term diamond is used throughout this specification as sp 3 It refers to any allotrope containing hybridized carbon, in particular diamond, or DLC, in any crystalline form.

[0013] In the context of the first implementation of the present invention, a reactive carbon atom is usually a carbon atom in "activated" form, i.e., a radical or an ion. In the present specification, this expression also refers to a carbon-containing molecule in activated form, i.e., a radical or an ion.

[0014] Plasma compression consists of directing or concentrating reactive plasma species, such as radicals and ions, created between the two electrodes into a confined area between the two electrodes in order to increase the density of the plasma and thereby the probability of reactive collisions occurring between the radicals. The increased number of collisions also produces UVC or even infrared photons, which themselves produce more reactive atoms. The combination of these effects significantly increases the rate of diamond deposition on the substrate.

[0015] For the second implementation of the invention, the electrodes at which the plasma is generated are typically supplied by a direct current (DC) source. This energy source is effective in initiating diamond deposition. However, as the layer formed becomes thicker, e.g., 25-30 μm, at typical chamber temperatures, e.g., 300-1600° C., the diamond layer becomes a sufficient electrical insulator to significantly reduce the flow of energy between the electrodes, thereby slowing down the rate of diamond synthesis.

[0016] To compensate for this effect, the applicant proposes a hybrid energy generation, further combining a radio frequency (RF) power source with a direct current (DC) source, thus creating a plasma by applying a direct current and an alternating radio frequency (RF) current between two electrodes. The direct current (DC) source can be continuous or intermittent.

[0017] During synthesis, the DC / RF ratio can be adjusted to keep the diamond deposition rate constant, depending in particular on the thickness of diamond already synthesized.

[0018] It has also been unexpectedly found that the DC / RF ratio affects the crystal structure of the diamond formed (single crystal, polycrystalline with variable and tunable grain size).

[0019] Regarding the third implementation of the present invention, a magnetic field can be applied near the substrate to homogenize the distribution of reactive carbon atoms in the plasma. Instead of following a direct path between the two electrodes, the reactive atoms further acquire a loop or spiral motion. In this way, the reactive atoms travel a longer path and acquire a higher speed. This increases the collision probability of the atoms, which creates sp3 hybridized C-C bonds, which are characteristic of diamond, and therefore increases the synthesis rate. The application of a magnetic field further helps to avoid arcs and voids in the formed diamond layer or film.

[0020] The application of a magnetic field alone can enhance the rate of diamond deposition, but can be advantageously combined with plasma compression and / or hybridization of DC / RF energy sources.

[0021] It is therefore also demonstrated that the first to third implementations of the method of the present invention aim to solve the same, but unique, problem: increasing the synthesis rate for economic reasons. In other words, the present invention of the present application is an invention of a problem solved in three different ways, which can be further combined.

[0022] Therefore, the uniqueness requirement of the invention as filed for patent is fully met.

[0023] In fact, the applicant does not intend to limit the scope of the application to diamond synthesis.The method of the present invention may be effective for any other material that can be synthesized by chemical vapor deposition, such as, for example, Si-Ge-based semiconductors made from silicon and germanium-carrier gases, or silicon nitride or silicon oxide-containing carrier gases.Therefore, the present invention relates firstly to the method of claims 1-3.

[0024] Regarding diamond, the invention herein is not limited to pure diamond, but can also be applied to doping diamond. For example, diamond can be doped with boron. In addition to the carbon-containing carrier gas, a boron-carrier gas, such as trimethylborane, boron trichloride or diborane, is then introduced into the chamber. Diamond can also be doped with nitrogen. Thus, in addition to the carbon-containing carrier gas, a nitrogen carrier gas, such as dinitrogen, ammonia or methylamine, is introduced into the chamber.

[0025] For the implementation of the above-mentioned method, the present invention also relates to a vapor deposition chamber equipped with a gas inlet and an exhaust outlet, in which are installed two plasma generating electrodes connected to a direct current (DC) source, characterized in that means are provided for compressing the plasma between the two electrodes.

[0026] According to a particular embodiment, the two electrodes are also connected to a source of radio frequency (RF) alternating current.

[0027] Preferably, the two electrodes should be an anode and a cathode, the cathode forming the substrate for diamond deposition.

[0028] It is also possible to provide means for generating a magnetic field within the chamber and adjacent the substrate.

[0029] The present invention will be better understood by reference to the following specification of preferred embodiments of the invention and by reference to the accompanying drawings, in which: [Brief description of the drawings]

[0030] [Figure 1] 1 is a schematic diagram of a prior art vapor deposition chamber. [Diagram 2] 1 is a schematic diagram of a vapor deposition chamber according to the present invention. [Diagram 3] FIG. 3 is a perspective view of the electrode and grill of FIG. 2. [Figure 4]1 is a schematic diagram of a vapor deposition chamber according to the present invention. [Diagram 5] 1 is a schematic diagram of a vapor deposition chamber according to the present invention. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0031] With reference to FIG. 1, a chemical vapor deposition (CVD) chamber 1 includes a gas inlet 2, an exhaust outlet 3 for reducing the pressure, and a substrate 5 forming electrodes, i.e. an anode 4 and a cathode, connected to the terminals of a direct current power supply 6, the circuit being connected to ground 7.

[0032] Diamond synthesis is carried out by introducing a carbon-containing carrier gas, such as methane or ethane, through inlet 2, applying a vacuum to outlet 3 to reduce pressure in chamber 1, and applying a voltage between electrodes 4 and 5. Under the influence of the voltage between the electrodes, the molecules of the carbon-containing carrier gas are activated to form a plasma of a large volume 8. The plasma volume 8 extends beyond the area between the electrodes.

[0033] Energy applied between the electrodes specifically breaks certain bonds, such as C-H bonds, thereby generating reactive species such as carbon and hydrogen radicals. These radicals can then recombine with hydrogen radicals or with other carbon radicals, resulting in C-C bonds. The hydrogen radicals can also combine with each other to form hydrogen gas, which can be exhausted from the chamber through exhaust port 3.

[0034] Since the energy of CC bonds is weaker than that of CH bonds, the equilibrium of the reaction shifts towards replacement of all CH bonds by CC bonds (i.e., formation of diamond). The larger the CC bonds, the less volatile the species is, and the molecules formed will deposit on the substrate under the influence of gravity. The substrate may also contain species that can initiate the formation of CC bonds on contact. Free radicals are unstable species with extremely long lifetimes in gaseous media. The formation of molecular bonds from pendant bonds of radicals is highly favorable from an energy point of view, but requires three molecular collisions to allow for the conservation of momentum. It is therefore a very rare phenomenon. On surfaces, it is quite different: gaseous radicals easily combine with surface radical centers, since phonons ensure the conservation of momentum.

[0035] Alternatively, a sample tray can be placed over the substrate to deposit to specific dimensions or to avoid depositing directly onto the electrodes.

[0036] The probability of collisions between reactive carbon atoms is directly proportional to the atomic volume density of these reactive carbon atoms in the zone 8 , which is related to the energy applied between the two electrodes 4 and 5 .

[0037] 2 and 3, reusing the numbering of Figure 1 for identical elements, electrodes 4 and 5 are now parallel disks whose centres are aligned along axis AA'. Grill 20 is placed between electrodes 4 and 5 within the chamber, with the periphery of the cylinder aligned with axis AA'. Grill 20 is connected to a source of direct current.

[0038] The electrode 4 may have other shapes. For example, the electrode 4 may consist of a single or pair of tips with spherical ends oriented along the AA' axis. The electrode 4 may have a concave, convex or flat shape.

[0039] To carry out the synthesis of diamond, the chamber 1 is placed under low pressure (lower than atmospheric pressure) containing a carbon atom-containing carrier gas by opening the gas inlet 2 and applying a negative pressure through the exhaust 3. A direct current is applied between the electrodes 4 and 5, generating a reactive carbon atom plasma between the two electrodes. At the same time, a direct current is applied to the grill 20 in order to generate an electric field around the cylinder defined by the grill 20. This has the effect of positioning the reactive carbon atoms of the plasma within a zone 28 defined between the electrodes 4 and 5 and limited in width inside the cylinder formed by the grill 20. Diamond is gradually deposited on the substrate 5 in the form of a homogeneous layer.

[0040] 1 and 2, since the same energy is applied between electrodes 4 and 5, i.e. the same amount of reactive carbon atoms is assumed, the plasma expansion zone becomes smaller in the presence of grill 20 and the plasma is compressed, thereby increasing the volume density of reactive carbon atoms. In this way, the probability of collisions between reactive carbon atoms and with surfaces increases, and the subsequent diamond formation and deposition rate on the substrate or on a sample tray placed on the substrate increases.

[0041] Preferably, the grill should be made of one or more materials with high electron emissivity. It is advantageous to use refractory materials for the grill, such as molybdenum or tungsten, to obtain a longer service life of the grill and to limit deformation due to the temperatures the grill may reach. These refractory materials can be doped, for example with thorium, to increase their electron emissivity. Due to the peak effect generated on the entire surface of the grill and by each of the components, the grill is a structure with a larger electron emitting surface.

[0042] The grill 20 shown here is of circular cross section, but any other cross section may be considered. In particular, the shape of the grill can be selected depending on the shape of diamonds that one wishes to obtain. The mesh and / or height of the grill can also be varied depending on the dimensions and / or properties of the chamber, the electrodes and / or the chamber. The height of the grill can be the same around the entire circumference of the cross section, or can be varied, such as at corners, to compensate for electronic effects that may lead to non-uniform diamond deposition.

[0043] Similarly, instead of a grille, it is also possible to use one or more rings, which may have the same or different diameters and whose centres would be aligned on the AA' axis, or a tube.

[0044] The grill, ring or tube thus defined is the means of plasma compression and has the following functions: - Homogenizing the plasma around the substrate or around a specific zone where diamond needs to be deposited. - Increasing the volume density of reactive carbon atoms in this zone. - It produces UVC or even IR photons and possibly releases electrons, providing additional energy to increase the density of the plasma.

[0045] Since diamond is an insulator, as the layer of diamond deposited on the substrate becomes thicker, especially when the diamond layer is 25-30 μm thick, a barrier is formed for the direct current passing between electrodes 4 and 5. Thus, for the same applied voltage, the volume density of reactive carbon atoms in the plasma decreases with the thickness of the diamond layer. The rate of diamond deposition decreases with increasing thickness of the already formed layer.

[0046] In order to be able to form layers thicker than a few tens of microns, the applicant proposes combining a direct current (DC) source with a radio frequency (RF) current source, thereby creating a plasma by applying a direct current and a radio frequency (RF) alternating current.

[0047] Referring to FIG. 4, using the numbering of the previous figure for common components, electrode 4 and electrode 5 are connected in parallel to a circuit including a high frequency AC source 46 and ground 47, and a DC source 6.

[0048] The high frequency AC source 46 should preferably have a filter at its outlet to prevent the DC of source 6 from flowing back into source 46. The high frequency AC source 6 should preferably have a filter at its outlet to prevent the DC of source 46 from flowing back into source 6.

[0049] During synthesis, in this configuration, a direct current and a high frequency alternating current are applied between electrodes 4 and 5 .

[0050] The ratio of the two currents, i.e. the DC / RF ratio, can be constant during the synthesis. However, it has been unexpectedly observed that the DC / RF ratio influences the crystal morphology of the diamond deposited on the substrate. For example, in a configuration where the application of only DC current allows the formation of ultrananocrystalline diamond on the substrate, the application of RF current with a ratio of RF / DC power supply of 0.05-0.3 helps to obtain a deposit formed of larger crystals, i.e. submicron sized crystals of tens of microns.

[0051] During synthesis, the ratio between the two currents, i.e. the DC / RF ratio, can also be varied to optimize the synthesis rate. For example, one can switch from direct current to RF current in stages as the diamond layer being deposited gets thicker. The DC / RF ratio can also be selected depending on, for example, the properties desired for the deposition.

[0052] The hybrid power supply for the plasma generating electrodes thus enhances the rate of diamond deposition by compensating for the electrical insulating effect of the already deposited diamond, and also allows modification of the properties, e.g. structure and nature, of the deposit.

[0053] Additionally, an RF power source can be connected to the grill 20 in parallel with the DC power source. These sources can be the same as the electrode sources or can be separate sources. Alternatively, each of these sources can be connected through a power regulator to control the ratio of DC / RF power delivered to the grill, which enhances the emission of electrons from the grill.

[0054] A magnetic field can be applied to the plasma, preferably near the substrate, to homogenize the distribution of positive and negative charges in the plasma, which can reduce or even prevent the presence of voids in the formed diamond layer / film.

[0055] Alternatively or additionally, a magnet may be placed adjacent to the anode 4 .

[0056] Referring to Figure 5, using the numbering of the previous figures for common parts, a permanent magnet 50 generating a magnetic field 51 (represented by a dotted line) is placed below the substrate electrode 5. The magnet (or electromagnet) is selected or placed so as to maximize the radial or longitudinal component of the magnetic field, or both components. The electrodes 4 and 5 illustrated herein are supplied with direct current only. It is also possible herein to combine direct current and RF current.

[0057] Here, a single magnet is shown below the substrate 5, but a magnet could also be placed adjacent to the anode 4. Also, multiple magnets could be placed, specifically one adjacent to the substrate 5 and one adjacent to the anode 4.

[0058] During synthesis, the charged atoms of the plasma 28 move between the anode 4 and the cathode 5 under the influence of the electric field created between them and are further exposed to the magnetic field 51 in the vicinity of the substrate 5. The paths of the charged atoms are thus deviated under the action of the Lorentz force, and the effect of the two fields is additive for each charged / reactive atom. The charged atoms will then tend to follow longer spiral paths than they would follow in the presence of a single field, forming loops around the magnetic field lines. The additive effect of the two fields, the electric field and the magnetic field, will also accelerate the movement of the reactive atoms.

[0059] Reactive atoms traveling faster over longer paths have a higher probability of subsequent collisions, resulting in an increased concentration of activated carbon and ultimately an increased rate of diamond formation and deposition onto the substrate.

[0060] Although permanent magnets are described herein, any shape of magnet, permanent or not, may be used that generates an appropriate magnetic field adjacent to the substrate.

[0061] The distance between the anode and the substrate / cathode can be adjusted to optimize the deposition.

[0062] Thus, each of the three elements of the present invention, the means of plasma compression, the hybridization of the power supply, and the application of a magnetic field near the substrate, have a positive effect on the diamond formation and deposition rates individually, and the unique inventive concept combines these three elements. This effect is stronger when the three means are used in combination, as shown in the following example, than when these two means are used in combination.

[0063] As mentioned above, UVC generated in situ in the plasma helps to increase the efficiency of the reaction by promoting the dissociation of reagents as the plasma is formed. In addition, UVC can be applied in the vicinity of the substrate where the plasma is formed to achieve the same in situ effect. UVC lamps can also be placed in the chemical vapor deposition chamber.

[0064] Likewise, in order to further increase the efficiency of the synthesis reaction, and in particular the specificity of this reaction, the principles described in WO2017121892 can be applied: in particular, photons of specific frequencies and / or energies, corresponding to the absorption frequencies of the substance to be synthesized and / or of the reagents, can be delivered to the substrate to increase the rate of substance formation.

[0065] example The CVD chamber, 260 mm in diameter and 160 mm in height, accommodates a 3.2 mm diameter tungsten anode placed approximately 35 mm above a 15 mm by 15 mm silicon substrate that forms the cathode.

[0066] If a grill is used, it is made from molybdenum and has a diameter of 5 cm, a height of approximately 1 cm and a mesh of 1 mm.

[0067] When magnets are used, an orthogonal magnetic field of 0.02 T is generated by the electromagnets.

[0068] When a DC / RF hybrid energy source is used, the two sources are applied simultaneously for the entire duration of the deposition.

[0069] The carbon carrier gas introduced into the chamber consists of a mixture of 97% hydrogen and 3% methane. To ensure plasma stability, the pressure is brought to and stabilized at approximately 300 mbar.

[0070] The temperature in the chamber during synthesis is about 950° C., which corresponds to the optimum temperature for deposition on a silicon substrate.

[0071] The applied DC is 735V DC with a power of approximately 1200W (±100W).

[0072] Several diamond deposits were prepared in 1 hour by applying direct current or hybrid DC / RF current with or without a grill, with or without a magnet placed under the substrate, the results are shown in the table below. [Table 1]

[0073] The presence of the grill alone doubles the deposition rate and homogenizes the film quality. The combination of the grill and hybrid DC / RF power supply accelerates the deposition rate by more than six times.

[0074] The magnetic field applied herein prevents discharges that result in occasional arcing and lead to voids in the diamond deposition, and also nearly doubles the deposition rate.

[0075] Similar results have been observed with molybdenum substrates.

[0076] The above description describes diamond synthesis, and has concerned both pure diamond and diamond doped with nitrogen atoms to obtain diamond with specific properties, such as semiconducting properties, for which suitable gases may be introduced in appropriate amounts into the vapor deposition chamber.

[0077] It has also been unexpectedly observed that the quality of the substrate affects the crystal morphology of the diamond, depending on whether the substrate is made of, for example, silicon, molybdenum, tungsten, titanium or quartz.

[0078] Although the advantages of the method herein are shown for diamond synthesis, the means of plasma compression can be applied to any other type of synthesis by chemical vapor deposition at atmospheric or low pressure to enhance the deposition rate. The same is true for DC / RF hybridization and / or application of a magnetic field near the substrate.

Claims

1. A method for synthesizing allotropes of carbon substances on a synthesis substrate between two plasma-generating electrodes in a chemical vapor deposition chamber, the two electrodes being an anode (4) and a cathode (5), The method comprises: introducing a carrier gas containing atoms of the substance to be synthesized into said chamber; 1. A method for generating a plasma in the vicinity of the substrate to activate atoms of the carrier gas containing atoms of the substance to be synthesized, comprising: A method according to any one of claims 1 to 5, characterized in that the plasma is compressed by a cylindrical means formed by a refractory material of a grill, one or more rings, or a tube, so as to increase the volume density of activated atoms near the substrate and thereby increase the deposition rate of the synthesized material, the refractory material of the grill, one or more rings, or the tube further homogenizing the plasma near the substrate.

2. A method as described in claim 1, wherein the two electrodes are an anode (4) and a cathode (5), the cathode forming a substrate (5) for diamond (45) deposition.

3. A method as described in claim 1 or 2, wherein the plasma is created by applying direct current (DC) and radio frequency (RF) alternating current between the two electrodes.

4. A magnetic field is applied adjacent to the substrate. The method according to any one of claims 1 to 3.

5. The substance to be synthesized is diamond, and the carrier gas containing atoms of the substance to be synthesized is a carbon atom-containing carrier gas; and A plasma (28) is created adjacent the substrate to generate reactive carbon atoms. The method according to any one of claims 1 to 4.

6. The method of claim 3 , wherein the DC / RF ratio is adjustable during synthesis.

7. A chemical vapor deposition chamber (1) for carrying out the method according to claim 1, comprising a gas inlet (2) and an exhaust (3), inside which are placed two plasma (28) generating electrodes (4, 5) connected to a direct current (DC) supply (6), characterized in that means (20) for compressing the plasma between the two electrodes (4, 5) are provided, said means (20) being cylindrical in shape formed by the refractory material of the one or more rings or tubes.

8. The chamber of claim 7, wherein the two electrodes (4, 5) are further connected to a source (46) of radio frequency (RF) alternating current.

9. A chamber according to claim 7 or 8, wherein the two electrodes are an anode (4) and a cathode (5), i.e. the cathode forming the substrate (5) for diamond (45) deposition.

10. A chamber according to any one of claims 7 to 9, comprising means (50) for generating a magnetic field in the vicinity of the substrate (5).

Citation Information

Patent Citations

  • Hard carbon film

    JP1987157602A

  • Synthesis of diamond

    JP1997040493A

  • Plasma CVD apparatus and film deposition method using the same

    JP2004339570A

  • Plasma-assisted chemical gas separation method having increased plasma density and device for implementing the method

    US20150170902A1