Method for producing nanocrystalline magnetic material, nanocrystalline magnetic material, and compact for nanocrystalline magnetic material
The production method for nanocrystalline magnetic materials addresses the issue of increased coercive force in flat metal crystal materials by crystallizing FeSiBNbCu alloy powders within a matrix, resulting in a magnetic material with high saturation flux and low coercive force for high-frequency applications.
Patent Information
- Application Number
- JP2021130828
- Authority / Receiving Office
- JP · JP
- Patent Type
- Patents
- Current Assignee / Owner
- Filing Date
- 2021-08-10
- Publication Date
- 2024-10-30
- Estimated Expiration
- 2041-08-10
AI Technical Summary
Magnetic core materials using flat metal crystals suffer from strain-induced increased coercive force, leading to higher hysteresis loss and reduced magnetic permeability, necessitating a solution to reduce coercive force while maintaining high saturation magnetic flux density.
A method involving the preparation of a mixture containing non-heat-treated FeSiBNbCu amorphous alloy powder and a matrix material, followed by molding and crystallization through heating to produce a nanocrystalline magnetic material, which includes steps like coating, pressurizing, and crystallization heat treatment to remove internal distortion.
The resulting magnetic material achieves high saturation magnetic flux density with low coercive force, suitable for high-frequency applications in reactors and transformers, with improved magnetic permeability and reduced hysteresis loss.
Smart Images

Figure 0007575649000001 
Figure 0007575649000002 
Figure 0007575649000003
Abstract
Description
[Technical field]
[0001] The present invention relates to a method for producing nanocrystalline magnetic materials. , nanocrystalline magnetic materials and nanocrystalline magnetic materials Molded body for Regarding. [Background technology]
[0002] In recent years, magnetic components have become a bottleneck in the miniaturization and efficiency improvement of switching power supplies. Ni-Zn ferrite is used as a magnetic core material for high-frequency switching power supplies of MHz or more that employ power semiconductors such as GaN and SiC (for example, Patent Documents 1 and 2).
[0003] While Ni-Zn ferrite has the advantage of high electrical resistivity, it has the disadvantages of the risk of thermal runaway and low saturation magnetic flux density. In response to this, there is a technology that uses a pressed powder material of flat metal crystals as a magnetic core material that has a high saturation magnetic flux density and can operate at high temperatures (for example, Patent Document 3). [Prior art documents] [Patent documents]
[0004] [Patent Document 1] JP 2013-155055 A [Patent Document 2] JP 2017-073447 A [Patent Document 3] JP 2017-59816 A Summary of the Invention [Problem to be solved by the invention]
[0005] However, in magnetic core materials using flat metal crystals, distortion remains inside the powder during the flattening and powder compaction processes in the manufacturing process, which increases the coercive force. Since an increase in coercive force leads to an increase in hysteresis loss and a decrease in magnetic permeability, it is necessary to reduce the coercive force.
[0006] An object of the present invention is to provide a magnetic material having a high saturation magnetic flux density and a low coercive force. [Means for solving the problem]
[0007] A method for producing a nanocrystalline magnetic material according to one aspect of the present invention includes the steps of: Crystallization The method includes a preparation step of preparing a mixture containing a powder of an amorphous alloy of FeSiBNbCu that has not been heat-treated and a matrix material, a molding step of molding the mixture to produce a molded body of the mixture, and a crystallization step of heating the molded body to crystallize the amorphous alloy powder. Effect of the Invention
[0008] According to one aspect of the present invention, a magnetic material having a high saturation magnetic flux density and a low coercive force can be provided. [Brief description of the drawings]
[0009] [Figure 1] 1A to 1C are process diagrams illustrating a method for manufacturing a magnetic material according to a first embodiment. [Diagram 2] 1 is a list of specific examples of iron-based amorphous alloys. [Diagram 3] FIG. 2 is a process diagram for producing iron-based amorphous alloy powder. [Figure 4] This is an SEM image of iron-based amorphous alloy powder. [Diagram 5] 1 is a graph showing the relationship between heating time and heating temperature in a crystallization heat treatment. [Figure 6] 5A to 5C are process diagrams showing a method for manufacturing a magnetic material according to a second embodiment. [Figure 7] FIG. 2 is a process diagram for impregnating a resin into a sheet molded body after crystallization heat treatment. [Figure 8] 1 is a graph showing the relationship between heating time and coercive force of a magnetic material. [Figure 9] 1 is a table showing saturation magnetization, volume filling factor, coercive force, and magnetic permeability of examples and reference examples. [Figure 10]1 is a graph showing the magnetic permeability of an example and a reference example. [Figure 11] X-ray diffraction intensity before and after crystallization heat treatment. [Figure 12] 1 is a SEM image of a sheet molding after crystallization heat treatment in an example. [Figure 13] 13 is an enlarged SEM image of the matrix material portion of FIG. 12. [Figure 14] 1 is an SEM image of a sheet molding of a reference example. [Figure 15] 14 is an enlarged SEM image of the matrix material portion of FIG. 13. [Figure 16] The chemical structure of silicone rubber. [Figure 17] 1 is a mass spectrum of silicone rubber before and after baking. [Figure 18] 1 is a mass spectrum of silicone rubber after baking. [Figure 19] 1 is a mass spectrum of a molded body after crystallization heat treatment. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS
[0010] Hereinafter, an embodiment of the present invention will be described with reference to the drawings. In addition, common parts in the drawings may be denoted by the same or corresponding reference numerals, and the description thereof may be omitted.
[0011] 1 is a process diagram showing a method for producing a magnetic material according to the first embodiment. The method for producing a magnetic material according to the present embodiment includes a preparation step of preparing a mixture containing an iron-based amorphous alloy powder and a matrix material.
[0012] In this specification, the term "iron-based amorphous alloy" refers to an amorphous alloy (a disordered property with no regularity in the arrangement of elements) that contains iron (Fe) as the main component in the alloy composition. The term "matrix material" refers to a resin component that forms a continuous phase (matrix) for the dispersed phase.
[0013] In the preparation step, as shown in Fig. 1(A), iron-based amorphous alloy powder 10, matrix material 20, and solvent 30 are placed in a container C and stirred (or kneaded) to prepare a mixture 40. The form of the mixture is not particularly limited, and may be, for example, a powder state in which the powder is impregnated with the matrix material, or a slurry (paste) state in which the powder is dispersed in the matrix material.
[0014] The elements other than iron (Fe) contained in the iron-based amorphous alloy include Cr, Co, Ni, Zr, Nb, Hf, Pd, Cu, rare earth elements, and alloys thereof. Among these, Pd, Co, Ni, rare earth elements, and alloys thereof are preferred in terms of easily inducing uniaxial magnetic anisotropy. Also, Si, B, and P are preferred in terms of forming an amorphous phase.
[0015] These elements other than iron (Fe) may be contained alone or in combination of two or more.
[0016] FIG. 2 is a list of specific examples of iron-based amorphous alloys. In this embodiment, the Fe 73.5 S 13.5 Iron-based amorphous alloys such as B9Nb3Cu1 are preferably used because they have low coercive force.
[0017] There is no particular limitation on the mode of producing the iron-based amorphous alloy powder 10. The iron-based amorphous alloy powder 10 can be produced, for example, by the process shown in FIG.
[0018] 3, first, an iron-based amorphous alloy ribbon 11 is prepared (FIG. 3(A)). The iron-based amorphous alloy ribbon 11 has, for example, a composition of Fe-Si-B-Nb-Cu and a thickness of 5 μm to 30 μm (18 μm in this embodiment).
[0019] The ribbon 11 is heated at about 400°C for 3 hours to embrittle the ribbon 11, thereby obtaining flakes 12 of an iron-based amorphous alloy (FIG. 3(B)). Next, the flakes 12 are pulverized into powder 13 of less than 150 μm (about 18 μm in this embodiment) (FIG. 3(C)). The iron-based amorphous alloy powder 13 is an example of the iron-based amorphous alloy powder in this embodiment.
[0020] The powder 13 is preferably further flattened to form a flat powder 14 of an iron-based amorphous alloy (FIG. 3(D)). The flat powder 14 has a thickness of about 2 to 3 μm. As shown in the SEM image of FIG. 4, the flat powder 14 is flattened into a thin plate shape with a thickness of submicrons. The flat powder 14 is another example of a powder of an iron-based amorphous alloy.
[0021] The thickness of the flat powder 14 can be adjusted by the conditions when the powder 13 is flattened using a ball mill, a vibration mill, or the like. Flattening conditions include, for example, the pot rotation speed and processing time in the case of a ball mill, and the vibration frequency, vibration displacement, processing time, and the like in the case of a vibration mill. Note that, since the thinner the flat powder is, the smaller the eddy current loss can be, the thickness of the flat powder can be appropriately selected depending on the frequency at which the final dust core is used.
[0022] In addition, the flat powder 14 can reduce the demagnetizing field effect in the in-plane direction and has high magnetic permeability, so it can be used in high frequency bands such as 10 MHz to several hundred MHz and 1 GHz. Therefore, it is preferable to use the powder of the iron-based amorphous alloy in this embodiment after flattening (flat powder 14), since it can provide a magnetic material (magnetic core material) for reactors and transformers that can be used in high frequency ranges.
[0023] The amount of the iron-based amorphous alloy powder 10 (flat powder 14) is not particularly limited and is determined according to the application. In this embodiment, the amount of the iron-based amorphous alloy is, for example, 60 to 90 mass%, preferably 65 to 85 mass%, and more preferably 70 to 80 mass%.
[0024] The components of the matrix material 20 are not particularly limited, but may be, for example, resin materials such as silicone and epoxy, or inorganic materials such as water glass. Among these, from the viewpoint of improving mechanical strength, resin materials are preferred, silicone is more preferred, and two-liquid silicone rubber in which a base agent and a curing agent are mixed is even more preferred.
[0025] The amount of the matrix material 20 is not particularly limited as long as a mixture containing the iron-based amorphous alloy powder 10 and the matrix material can be prepared. The amount of the matrix material can be, for example, 10 to 40 mass%, more preferably 15 to 35 mass%, and even more preferably 20 to 30 mass%.
[0026] The solvent 30 is added as desired depending on the purpose. In this embodiment, the solvent 30 is added as a diluent for the matrix material 20. The components of the solvent 30 are not particularly limited, and may be, for example, an organic solvent. Preferably, toluene or the like that is compatible with the matrix material 20 is used.
[0027] The amount of the solvent 30 added is not particularly limited, and is, for example, 5 to 15 times the amount of the matrix material, preferably 7 to 13 times, and more preferably 9 to 11 times.
[0028] In this embodiment, a liquid silicone rubber base material and a curing agent were mixed in a 1:1 ratio as the matrix material 20, and stirred in a vacuum at 1000 rpm for 2 minutes. To this was added toluene as a solvent (diluent) 30. While stirring, iron-based amorphous alloy powder 10 was added, and the mixture 40 was produced by stirring at 1000 rpm for 2 minutes.
[0029] The method for producing a magnetic material according to this embodiment includes a molding step of molding a mixture containing an iron-based amorphous alloy powder and a matrix material to produce a compact of the mixture.
[0030] In the forming step, as shown in FIG. 1(B), the mixture 40 is formed into a sheet. Specifically, the forming step includes a coating step in which the mixture is coated. In the coating step, a printer 51 is used to print the mixture 40 into a sheet on a metal mask 52 to produce a sheet 50. In this embodiment, a sheet 50 measuring approximately 6 cm in length and approximately 7 cm in width was produced. The produced sheet 50 is dried at approximately 40° C. for 20 minutes to volatilize excess solvent 30 contained in the sheet 50.
[0031] The molding step also includes a pressurizing step of pressing the molded body in the thickness direction, as shown in Fig. 1(C). In the pressurizing step, the sheet 50 is pressed in the thickness direction using a press machine 61 to obtain a sheet-like molded body 60. In this embodiment, the sheet 50 is sandwiched between the press machine 61, and the pressure is increased to 15t at 40°C and 2t / min, and the pressure is maintained at 40°C and 15t for 10 minutes, and then the temperature is increased to 100°C and the temperature is maintained at 80°C and 15t for 2 hours to obtain a sheet-like molded body 60.
[0032] Furthermore, the molding step preferably includes a lamination step of laminating a plurality of molded bodies. In the lamination step, a laminate obtained by laminating a plurality of sheets 50 is pressed in the lamination direction of the laminate using a press machine 61 to obtain a laminate of molded bodies 60.
[0033] A plurality of sheets 50 can be obtained by repeating the coating process shown in FIG. 1(B).
[0034] The laminate of the molded body 60 may be a laminate of a plurality of sheet-like molded bodies 60 and pressurized. In this case, the plurality of sheet-like molded bodies 60 are obtained by repeating the coating step shown in Fig. 1(B) and the pressurizing step shown in Fig. 1(C).
[0035] The manufacturing method of the magnetic material according to the present embodiment includes a crystallization step of heating the compact to crystallize the iron-based amorphous alloy powder contained in the compact. In this specification, crystallization refers to the change of the iron-based amorphous alloy powder contained in the compact into nanocrystals. Here, nanocrystals refer to crystals with a grain size of about several nm to several tens of nm, in which the volume of the grain boundary occupies at least 10% of the entire crystal.
[0036] In the crystallization process, as shown in FIG. 1(D), the sheet-like compact 60 (or a stack of sheet-like compacts 60) is heated in a heating furnace (not shown) such as a muffle furnace until the iron-based amorphous alloy powder 10 contained in the sheet-like compact 60 is crystallized.
[0037] The heating temperature in the crystallization step is not particularly limited as long as it is a temperature at which the iron-based amorphous alloy powder 10 contained in the sheet-like compact 60 is crystallized. The heating temperature in the crystallization step is, for example, preferably 450°C or more and 600°C or less, more preferably 480°C or more and 570°C or less, and even more preferably 500°C or more and 550°C or less.
[0038] In this embodiment, the sheet-like molded body 60 (or a stack of the sheet-like molded bodies 60) is placed in the above-mentioned heating furnace. As shown in Fig. 5, the temperature inside the heating furnace is raised from room temperature to 500 to 575°C (515°C in this embodiment) at 5°C / min, and after being held at 515°C for 45 minutes, the furnace is cooled (cooled) to room temperature. As a result, a crystallized molded body 70 in which the iron-based amorphous alloy powder 10 contained in the sheet-like molded body 60 is crystallized is obtained (see Fig. 1(D)).
[0039] The heating in the crystallization step may be a magnetic field heat treatment. This is because by selecting an alloy composition that can impart uniaxial magnetic anisotropy to the iron-based amorphous alloy powder and applying a magnetic field in the direction of the hard magnetization axis, it is possible to obtain even higher magnetic permeability at high frequencies. The strength of the magnetic field applied during heating should be at least five times the coercive force of the iron-based amorphous alloy powder.
[0040] In addition, the iron-based amorphous alloy powder is preferably flat powder as described above, but is not limited to being flat powder. Any shape may be used as long as it can be heated and crystallized. For example, a spherical iron-based amorphous alloy powder produced by an atomization method or the like may be used.
[0041] The crystallized molded body 70 thus obtained is an example of the magnetic material of this embodiment. That is, the magnetic material of this embodiment is obtained by the manufacturing method of the first embodiment described above, and is a magnetic material obtained by crystallizing the iron-based amorphous alloy powder in a molded body containing the iron-based amorphous alloy powder and a matrix material.
[0042] In other words, the magnetic material according to the present embodiment is a crystalline magnetic material formed by molding a mixture containing iron-based amorphous alloy powder and a matrix material. The magnetic material crystallized in this way (crystalline magnetic material) has a coercive force of 2 Oe or less.
[0043] A similar method can also be applied to a powder magnetic core produced by die pressing flat or spherical Fe-based amorphous powder that has been kneaded with a resin binder and a lubricant and surface-treated. Fig. 6 is a process diagram showing a method for producing a magnetic material according to a second embodiment. In Fig. 6, parts common to Fig. 1 may be given reference numbers that are 100 larger than the reference numbers in Fig. 1, and descriptions thereof may be omitted.
[0044] In the manufacturing method of the magnetic material according to the second embodiment, as shown in Fig. 6(A), a mixture 140 is prepared by kneading iron-based amorphous alloy powder 110, a matrix material 120, and a solvent 130. An epoxy resin is used as the matrix material 120. The amount of the epoxy resin is 0.05 to 10 mass %, preferably 0.1 to 6 mass %, relative to 100 mass % of the iron-based amorphous alloy powder. A lubricant is used as the solvent 130.
[0045] The obtained mixture 140 is press-molded using a press molding die 150, as shown in Fig. 6(B). Specifically, the mixture 140 filled in a molding container 152 of the die 150 is pressed with a presser 151 (Fig. 6(B)).
[0046] The obtained press molded body is heated (fired) at 80°C for 2 hours to obtain a doughnut-shaped molded body 160 (Fig. 6(C)). The obtained molded body 160 is heated in a heating furnace (not shown) such as a muffle furnace until the iron-based amorphous alloy powder 110 contained in the molded body 160 is crystallized, thereby obtaining a crystallized molded body 170 in which the iron-based amorphous alloy powder 110 contained in the molded body 160 is crystallized (see Fig. 6(D)).
[0047] The crystallized molded body 170 thus obtained is another example of the magnetic material of this embodiment. That is, the magnetic material according to this embodiment is obtained by the manufacturing method according to the second embodiment described above, and is a magnetic material obtained by crystallizing the iron-based amorphous alloy powder in a molded body containing the iron-based amorphous alloy powder and a matrix material. The magnetic material thus obtained is also a crystalline magnetic material obtained by molding a mixture containing the iron-based amorphous alloy powder and a matrix material, and has a coercive force of 2 Oe or less.
[0048] The manufacturing method of the magnetic material according to the present embodiment preferably includes an impregnation step of impregnating the crystallized molded body of the iron-based amorphous alloy powder with an impregnation resin after the crystallization step. The impregnation step will be described below in the case of using the magnetic material (crystallized molded body 70) obtained by the manufacturing method according to the first embodiment shown in FIG.
[0049] In the impregnation step, as shown in Figures 7(A) and (B), the crystallized molded body 70 that has been subjected to the crystallization heat treatment in the crystallization step is immersed in the impregnation resin 80 for 60 minutes in a container T whose pressure has been reduced to 1 / 3 atmospheric pressure, so that the crystallized molded body 70 is impregnated with the impregnation resin 80. The crystallized molded body 70 impregnated with the impregnation resin 80 is placed in a heating furnace (not shown) such as a muffle furnace and baked at 80°C for 2 hours, to obtain a resin-impregnated molded body 90 as shown in Figure 7(C).
[0050] The components of the impregnated resin are not particularly limited, but for example, resin materials such as silicone and epoxy, and inorganic materials such as water glass can be used. Among these, from the viewpoint of improving mechanical strength, resin materials are preferred, silicone is more preferred, and two-liquid silicone rubber consisting of a base agent and a hardener is even more preferred. The resin-impregnated molded body 90 obtained in this manner is another example of the magnetic material of this embodiment.
[0051] The magnetic material used in the impregnation step is not limited to the magnetic material (crystallized molded body 70) obtained by the manufacturing method of the first embodiment, and may be a magnetic material (crystallized molded body 170) obtained by the manufacturing method of the second embodiment shown in Fig. 6. When the magnetic material (crystallized molded body 170) obtained by the manufacturing method of the second embodiment is used as the magnetic material used in the impregnation step, the crystallized molded body 170 impregnated with the impregnation resin 80 is heated (fired) at 60°C for 5 hours, for example.
[0052] The relationship between the heating temperature and the coercive force of the crystallized compact 70, which is a magnetic material obtained by the manufacturing method of this embodiment, was confirmed. As shown in Fig. 8, when the heating temperature in the crystallization step was 500°C to 545°C, the coercive force of the obtained crystallized compact 70 was 1.0 Oe (80 A / m) to 1.3 Oe.
[0053] This coercive force was at the same level as the coercive force (0.7 Oe) of the nanocrystalline alloy flat powder obtained by heating the above-mentioned iron-based amorphous alloy powder 10 (flat powder 14) at the same temperature (515°C) as the heating temperature of the crystallization heat treatment in this embodiment.
[0054] In the manufacturing method of the magnetic material according to the present embodiment, as described above, the mixture containing the iron-based amorphous alloy powder and the matrix material is molded into a compact, and the iron-based amorphous alloy powder is crystallized by heating the compact, so that the strain inside the iron-based amorphous alloy powder during molding can be removed by the final crystallization heat treatment. As a result, the hysteresis loss of the obtained magnetic material can be reduced, and the coercive force can be reduced.
[0055] Therefore, according to the manufacturing method of the present embodiment, the coercive force of the obtained magnetic material can be reduced even if the obtained magnetic material has a high saturation magnetic flux density, and thus the obtained magnetic material can be used for reactors and transformers.
[0056] In addition, in the manufacturing method of the magnetic material according to the present embodiment, as described above, the heating temperature in the crystallization step is set to 450° C. or more and 600° C. or less, so that the iron-based amorphous alloy powder contained in the compact is sufficiently crystallized. Therefore, according to the present embodiment, the coercive force of the obtained magnetic material can be reduced with high accuracy.
[0057] In the manufacturing method of the magnetic material according to the present embodiment, as described above, the mixture is molded into a sheet in the molding step, so that the magnetic poles generated on the end surfaces of the magnetic material molded into a sheet cancel out the opposing magnetic poles of the adjacent magnetic powders, thereby reducing the demagnetizing field. Therefore, in the obtained magnetic material, the effective permeability of the magnetic powder in the aggregated state becomes higher than that of the magnetic powder in the single state due to the reduction in the demagnetizing field, and the coercive force can be reduced.
[0058] In the manufacturing method of the magnetic material according to this embodiment, as described above, the molding process includes a coating process for coating the mixture, which makes it easy to form the mixture of iron-based amorphous alloy powder and matrix material into a sheet shape.
[0059] In addition, during the coating process, distortion may occur within the iron-based amorphous alloy powder contained in the mixture, which may increase the coercive force of the resulting magnetic material. However, the above-mentioned crystallization process eliminates this distortion and makes it possible to suppress the increase in coercive force.
[0060] In the manufacturing method of the magnetic material according to the present embodiment, as described above, the molding process includes a pressing process for pressing the molded body in the thickness direction, so that the molded body containing the iron-based amorphous alloy powder densely can be molded. In addition, the crystallization heat treatment after the molding process including the pressing process can remove the distortion inside the iron-based amorphous alloy powder caused by the pressing process. Therefore, the saturation magnetic flux density can be increased while reducing the coercive force.
[0061] In the manufacturing method of the magnetic material according to the present embodiment, as described above, the molding step includes a lamination step of laminating a plurality of molded bodies, so that the thickness of the magnetic material molded into a sheet shape can be increased. This makes it possible to increase the saturation magnetic flux density while reducing the coercive force. In addition, since the thickness of the magnetic material molded into a sheet shape can be adjusted, the magnetic material can be easily mounted.
[0062] In the manufacturing method of the magnetic material according to this embodiment, as described above, the crystallization step is followed by an impregnation step in which an impregnating resin is impregnated into the compact in which the iron-based amorphous alloy powder has been crystallized, thereby making it possible to increase the mechanical strength of the magnetic material obtained as a compact.
[0063] In the manufacturing method of the magnetic material according to the embodiment, a magnetic field is applied during the heat treatment for nanocrystallization of iron-based amorphous alloy powder having an element composition effective for inducing uniaxial magnetic anisotropy, thereby imparting uniaxial magnetic anisotropy to the obtained magnetic material. In the magnetic material imparted with uniaxial magnetic anisotropy, the direction parallel to the applied magnetic field during the nanocrystallization heat treatment is the easy axis direction, and the direction perpendicular to the easy axis direction is the hard axis direction.
[0064] In such a magnetic material having uniaxial magnetic anisotropy, the magnetic permeability is not easily deteriorated even in a high frequency band (for example, 10 MHz to several hundreds of MHz) by applying a magnetic field in the direction of the hard axis of magnetization. Therefore, the magnetic material obtained by the manufacturing method of the embodiment can be used in a high frequency band of MHz or more with a high saturation magnetic flux density while reducing the coercive force.
[0065] As described above, the magnetic material of the present embodiment is a magnetic material obtained by crystallizing the iron-based amorphous alloy powder contained in a compact formed into a sheet-like shape from a matrix material mixed with iron-based amorphous alloy powder, and since it is obtained by the above-mentioned manufacturing method, the effects obtained by the above-mentioned manufacturing method for magnetic materials can be obtained directly.
[0066] That is, the magnetic material of this embodiment is a crystallized magnetic material (crystalline magnetic material), and even if it has a high saturation magnetic flux density, the hysteresis loss is low and the magnetic permeability is high, so that the coercive force is low at 2 Oe or less. Therefore, the magnetic material of this embodiment can be suitably used for reactors and transformers. EXAMPLES
[0067] The present embodiment will be further described below with reference to examples. Various tests and evaluations were carried out according to the following methods.
[0068] [Example] Two-component silicone rubber (KE-1031, manufactured by Shin-Etsu Chemical Co., Ltd., a 1:1 ratio of base agent and curing agent) was mixed as a matrix material, and stirred in a vacuum at 1000 rpm for 2 minutes. Toluene was added as a solvent (diluent) 30, and the mixture was stirred while being flattened into iron-based amorphous alloy powder. 73.5 S 13.5 B9Nb3Cu1 powder was added and kneaded to prepare a mixture.
[0069] The prepared mixture was printed into a sheet using a printer (Mitani Micronics, MEC-2400E15A) to produce multiple sheets. The produced multiple sheets were stacked (laminated) in the thickness direction. This was sandwiched between a press (As One, 1t-15t HC300-15), the pressure was increased to 15t at 40°C and 2t / min, and the temperature was held at 40°C and 15t for 10 minutes, and then the temperature was raised to 100°C and the temperature was held at 80°C and 15t for 2 hours to obtain a sheet molded body.
[0070] The sheet molded body was placed in a muffle furnace (Digital Hydental, KDF-009G), the temperature inside the furnace was raised from room temperature to 515°C at 5°C / min, and then held at 515°C for 45 minutes. After that, the furnace was cooled (cooled) to room temperature to obtain a molded body.
[0071] [Reference example] The same flattened iron-based amorphous alloy powder as in the example was placed in a muffle furnace (Digital Hydental, KDF-009G), the temperature inside the furnace was raised from room temperature to 515°C at a rate of 5°C / min, and the temperature was held at 515°C for 45 minutes. The furnace was then cooled (cooled) to room temperature to obtain a flattened iron-based crystalline alloy powder.
[0072] A mixture was prepared by mixing this powder with a two-component silicone rubber (KE-1031, manufactured by Shin-Etsu Chemical Co., Ltd., a 1:1 ratio of base agent and curing agent) as a matrix material. The mixture was printed onto a film in the form of a sheet using a printer (MEC-2400E15A, manufactured by Mitani Micronics Co., Ltd.) to produce multiple sheets.
[0073] Several sheets were stacked and clamped in a press (As One Corporation, 1t-15t HC300-15), the pressure was increased to 15t at 40°C and 2t / min, held at 40°C and 15t for 10 minutes, then the temperature was increased to 100°C and held at 80°C and 15t for 2 hours to obtain a molded body.
[0074] <Saturation magnetization Ms> A vibrating sample magnetometer (Riken Denshi Co., Ltd., BHV-55) was used to apply a magnetic field of 10 kOe and measure the saturation magnetization (saturation magnetic flux density) Ms as the static magnetization characteristics. Both the working example and the reference example showed a saturation magnetization of 0.45 T or more (see FIG. 9).
[0075] <Volume filling rate> The volumetric filling rate (vol.%) of the iron-based amorphous alloy powder in the compact was confirmed, and was about 40 volume % in both the working example and the reference example.
[0076] <Coercive force Hc> Using a coercive force meter (manufactured by Denshi Jiki Kogyo Co., Ltd., HC-1031), a 3 kOe magnetic field was applied, and the coercive force Hc in the in-plane direction of the sheet was measured as the static magnetization characteristic. The coercive force Hc is the value of the magnetic field in the negative direction when the magnetization becomes zero after applying a sufficiently large magnetic field for magnetic saturation and then gradually (quasi-statically) reducing the magnetic field. The coercive force of the reference example was 5.8 Oe, while the coercive force of the example was as low as 1.0 Oe (see Fig. 9).
[0077] <Permeability μ'> The permeability μ' was measured using an impedance analyzer (manufactured by Agilent Technologies, Precision Impedance Analyzer 4294A).
[0078] Fig. 10 is a graph showing the permeability of the example and the reference example. In Fig. 10, A represents the real part μ' of the permeability of the example, B represents the real part μ' of the permeability of the reference example, C represents the imaginary part μ" of the permeability of the example, and D represents the imaginary part μ" of the permeability of the reference example. When comparing the permeability μ' per 1 MHz, the permeability of the reference example was 59, while the permeability of the example was as high as 209 (see Figs. 9 and 10).
[0079] <X-ray diffraction intensity> Using an X-ray diffractometer (manufactured by Rigaku Corporation, RINT (registered trademark)), the X-ray diffraction (XRD) intensities of the molded body before crystallization heat treatment and the molded body after crystallization heat treatment in the example were measured.
[0080] From Fig. 11, no peak was confirmed on the 110 plane of α-iron in the molded body before crystallization heat treatment (lower part of Fig. 11). On the other hand, a peak was confirmed on the 110 plane of α-iron in the molded body after crystallization heat treatment (upper part of Fig. 11). That is, it was confirmed that the molded body of the example was a molded body in which the powder of the iron-based amorphous alloy was crystallized by heat treatment.
[0081] <SEM image> SEM images were taken using a field emission scanning electron microscope (SU8000, manufactured by Hitachi High-Technologies Corporation). Figure 12 is an SEM image of the molded body of the example, Figure 13 is an SEM image of the molded body of the example (matrix material part), Figure 14 is an SEM image of the molded body of the reference example, and Figure 15 is an SEM image of the molded body of the reference example (matrix material part).
[0082] In both the Examples and the Reference Examples, the iron-based amorphous alloy powder is crystallized, but in the Reference Examples, the matrix material is in an amorphous state, whereas in the Examples, it was confirmed that the matrix material is crystallized.
[0083] <Mass spectrometry> Mass spectrometry was performed using a time-of-flight secondary ion mass spectrometer (ION-TOF, 5-ADSD-100). Figure 16 shows the chemical structure (coiled helix structure) of the silicone rubber used as the standard sample. Figure 17 shows the spectrum of the standard sample in Figure 16 after curing (before baking), Figure 18 shows the spectrum of the standard sample in Figure 17 after baking at 515°C for 45 minutes, and Figure 19 shows the spectrum of the example.
[0084] As shown in Figures 17 and 18, in the standard sample after baking, most of the cyclic siloxanes are cleaved, low molecular weight cyclic siloxanes are generated, and some of the cyclic siloxanes before baking remain. Also, as shown in Figures 18 and 19, it was confirmed that the composition of the standard sample after baking is included in the composition of the example. Note that, although the spectrum of the reference example is not shown, the composition of the reference example includes the composition of the standard sample before baking in Figure 17.
[0085] From these results, it can be seen that in the examples, by heating a compact made by molding a mixture of iron-based amorphous alloy powder and a matrix material to crystallize the iron-based amorphous alloy powder, the coercive force of the resulting magnetic material can be reduced even if it has a high saturation magnetic flux density.
[0086] In addition, in the examples, the iron-based amorphous alloy powder is flattened, and the resulting magnetic material has a high saturation magnetic flux density while reducing the coercive force, and can be used in high frequency bands of MHz or more.
[0087] Although an embodiment of the present invention has been described above, the present invention is not limited to a specific embodiment, and various modifications and changes are possible within the scope of the invention described in the claims. [Explanation of symbols]
[0088] 10, 110 Iron-based amorphous alloy powder 11 Thin ribbon 12 flakes 13 powder 14 Flat powder 20, 120 Matrix material 30, 130 Solvent 40, 140 mixture C container 50 sheets 51 Printing machine 52 Metal Mask 60, 160 Molded body 61 Press Machine 70, 170 Crystallized compact T container 80 Impregnating Resin 90 Resin-impregnated molding 150 Molds 151 Presser 152 Molded containers
Claims
1. A method for producing a mixture comprising: preparing a powder of an amorphous alloy of FeSiBNbCu that has not been heat-treated for crystallization; and preparing a mixture containing a matrix material. a molding step of molding the mixture to produce a molded body of the mixture; A crystallization process for crystallizing the amorphous alloy powder by heating the molded body. Methods for producing nanocrystalline magnetic materials.
2. The heating temperature in the crystallization step is 450° C. or higher and 600° C. or lower. A method for producing the nanocrystalline magnetic material of claim 1.
3. In the forming step, the mixture is formed into a sheet. A method for producing the nanocrystalline magnetic material according to claim 1 or 2.
4. The molding step includes a coating step of coating the mixture. A method for producing a nanocrystalline magnetic material according to any one of claims 1 to 3.
5. The molding step includes a pressurizing step of pressing the molded body in a thickness direction. A method for producing a nanocrystalline magnetic material according to any one of claims 1 to 4.
6. The molding step includes a lamination step of laminating a plurality of the molded bodies. A method for producing a nanocrystalline magnetic material according to any one of claims 1 to 5.
7. After the crystallization step, an impregnation step is performed in which the crystallized molded body is impregnated with an impregnation resin. A method for producing a nanocrystalline magnetic material according to any one of claims 1 to 6.
8. The powder is flattened. A method for producing a nanocrystalline magnetic material according to any one of claims 1 to 7.
9. A molded body comprising a powder of an amorphous alloy of FeSiBNbCu that has not been heat-treated for crystallization and a matrix material, which is crystallized. Nanocrystalline magnetic materials.
10. The coercive force is 2 Oe or less.
10. The nanocrystalline magnetic material of claim 9.
11. A nanocrystalline magnetic material molding for use in a nanocrystalline magnetic material, comprising: A mixture containing powder of an amorphous alloy of FeSiBNbCu that has not been heat-treated for crystallization and a matrix material is molded. Nanocrystalline magnetic material compacts.
12. The coercive force of the nanocrystalline magnetic material is 2 Oe or less.
12. The nanocrystalline magnetic material compact according to claim 11.
Citation Information
Patent Citations
Ferrite composition, ferrite core and electronic part
JP2013155055A
Soft magnetic material, rotary electric machine, motor and electric power generator
JP2017059816A
Powder-compact magnetic core material, powder-compact magnetic core, and manufacturing method therefor
JP2017073447A