Method for producing precursor of positive electrode active material for lithium ion secondary battery, and method for producing positive electrode active material for lithium ion secondary battery

By controlling the atmosphere and introducing gas simultaneously into the reaction solution and gas phase during the production of nickel-cobalt-manganese composite hydroxide, the method addresses the challenges of achieving high oil absorption and output characteristics in lithium ion secondary batteries, resulting in a positive electrode active material with enhanced performance.

JP7575721B2Active Publication Date: 2024-10-30SUMITOMO METAL MINING CO LTD
View PDF 11 Cites 0 Cited by

Patent Information

Application Number
JP2020154655
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Filing Date
2020-09-15
Publication Date
2024-10-30
Estimated Expiration
2040-09-15

AI Technical Summary

Technical Problem

Existing methods for producing lithium nickel cobalt manganese composite oxide as a positive electrode active material for lithium ion secondary batteries face challenges in achieving high oil absorption and output characteristics due to difficulties in controlling the atmosphere during the production process, leading to reduced productivity and inconsistent particle size distribution.

Method used

A method involving a controlled switching of oxidizing and non-oxidizing atmospheres during the seed particle generation and growth processes, combined with simultaneous gas introduction into both the reaction aqueous solution and gas phase, to produce a nickel-cobalt-manganese composite hydroxide with a hollow structure, enhancing oil absorption and output characteristics.

Benefits of technology

The method results in a positive electrode active material with high oil absorption and improved output characteristics, achieving a controlled particle size distribution and structure that enhances the performance of lithium ion secondary batteries.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575721000002
    Figure 0007575721000002
  • Figure 0007575721000003
    Figure 0007575721000003
  • Figure 0007575721000001
    Figure 0007575721000001
Patent Text Reader

Abstract

To provide a method of manufacturing a precursor of a positive electrode active material for lithium ion secondary battery, the precursor being nickel-cobalt-manganese composite hydroxide particles, capable of increasing the oil absorption of the positive electrode active material for lithium ion secondary batteries to improve output capabilities of a battery.SOLUTION: A method of producing nickel-cobalt-manganese composite hydroxide particles by crystallization reaction after mixing a raw material water containing at least nickel, cobalt, and manganese and a water solution containing ammonium ion supply body to form reaction aqueous solution, includes a particle generation process conducted at pH controlled to 12.0-14.0 in an oxidizing atmosphere, a seed particle growth process conducted at pH controlled to 10.0-12.0 while the oxidizing atmosphere is maintained, and a particle growth process in which the oxidizing atmosphere is switched to a non-oxidizing atmosphere, where in the seed particle generation process and the seed particle growth process, an oxidizing gas is synchronously introduced to both of the reaction aqueous solution and the gas phase thereof.SELECTED DRAWING: Figure 1
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, and a method for producing a positive electrode active material for a lithium ion secondary battery. [Background technology]

[0002] Regarding the increasingly serious environmental problems on a global scale, exhaust gases emitted from vehicles that use fossil fuels, such as gasoline and diesel vehicles, remain one of the main causes of air pollution. In response to this, in order to rapidly transition to environmentally friendly hybrid and electric vehicles, worldwide research and development into lithium-ion secondary batteries with excellent characteristics such as high output and high capacity is still being conducted in many countries. In addition, with the rapid increase in demand for mobile devices such as smartphones, tablet terminals, and mobile PCs, lithium-ion secondary batteries, which have many advantages as an energy source for these devices, such as high energy density and working potential, long cycle life, and low self-discharge rate, are attracting even more attention.

[0003] Such lithium ion secondary batteries using lithium metal composite oxides having a layered or spinel type crystal structure as the positive electrode active material can obtain a high voltage of about 4 V, and therefore are being put into practical use as secondary batteries exhibiting high energy density.

[0004] Examples of lithium metal composite oxides include lithium cobalt composite oxide (LiCoO2), which is relatively easy to synthesize, lithium nickel composite oxide (LiNiO2), which uses nickel, which is cheaper than cobalt, and lithium nickel cobalt manganese composite oxide (e.g., LiNi 1 / 3 Co 1 / 3 Mn 1 / 3 O2), lithium manganese composite oxide (LiMn2O4), lithium nickel manganese composite oxide (LiNi 0.5 Mn 0.5O2), lithium nickel cobalt aluminum composite oxide (e.g., LiNi 0.75 Co 0.15 Al 0.10 O2) have been proposed.

[0005] Among these lithium metal composite oxides, a ternary positive electrode active material made of lithium nickel cobalt manganese composite oxide (also known as NCM), which contains at least nickel, cobalt, and manganese, has attracted much attention as a material that has excellent thermal stability, high capacity, good cycle characteristics, and can provide high output with low resistance. This lithium nickel cobalt manganese composite oxide is a compound having a layered crystal structure, similar to lithium cobalt composite oxide and lithium nickel composite oxide.

[0006] Regarding lithium metal composite oxides, the focus of their development has been on increasing output by reducing their internal resistance, and while lithium nickel cobalt aluminum-containing composite oxides (NCA), which have improved properties of lithium nickel composite oxides, have also attracted attention, lithium nickel cobalt manganese composite oxides are considered to be of the utmost importance in the development of lithium metal composite oxides because they are more weather resistant and easier to handle than lithium nickel cobalt aluminum-containing composite oxides. Therefore, there is a high demand for ternary positive electrode active materials made of lithium nickel cobalt manganese composite oxides to increase output by further reducing internal resistance, particularly in applications as power sources for electric vehicles.

[0007] Incidentally, in order to obtain a lithium-ion secondary battery having excellent cycle characteristics, output characteristics, and the like, it is necessary that the positive electrode active material, which is the positive electrode material of the lithium-ion secondary battery, is composed of particles with a small particle size and a narrow particle size distribution. This is because particles with a small particle size have a large specific surface area, and when used as a positive electrode active material, not only can the reaction area with the electrolyte be sufficiently secured, but also the positive electrode can be made thin, shortening the distance that lithium ions travel between the positive and negative electrodes, thereby reducing the positive electrode resistance.In addition, particles with a narrow particle size distribution can uniformize the voltage applied to the particles in the electrode, making it possible to suppress the decrease in battery capacity caused by selective deterioration of fine particles.

[0008] Therefore, in order to further improve the output characteristics, it is effective to form a space inside the positive electrode active material into which the electrolyte can enter. Such a positive electrode active material can increase the reaction area with the electrolyte compared to a positive electrode active material with a solid structure having the same particle size, so that it is possible to significantly reduce the positive electrode resistance. It is known that the positive electrode active material inherits the particle properties of the metal composite hydroxide that is its precursor. That is, in order to obtain the above-mentioned positive electrode active material, it is necessary to appropriately control the particle size, particle size distribution, and particle structure of the particles in the metal composite hydroxide that is its precursor.

[0009] For example, Patent Documents 1 to 4 disclose methods for producing a metal composite hydroxide, which is a precursor of a positive electrode active material, by a crystallization reaction that is clearly separated into two stages: a "nucleation step" in which nucleation is mainly performed, and a "particle growth step" in which particle growth is mainly performed. In these methods, by appropriately adjusting the pH and reaction atmosphere in the nucleation step and the particle growth step, a metal composite hydroxide is obtained that has a small particle size and a narrow particle size distribution, and is composed of a low-density central part made of fine primary particles and a high-density outer shell made of plate-like or needle-like primary particles.

[0010] The positive electrode active material obtained by the above-mentioned method, which is composed of a low-density core and a high-density outer shell and has a metal composite hydroxide as a precursor, has a small particle size, a narrow particle size distribution, and a hollow structure or a structure having spaces, and thus has an increased contact area with the electrolyte, which facilitates the movement of lithium ions, and allows the production of a positive electrode active material with excellent cycle characteristics and output characteristics.

[0011] Here, it is important to be able to evaluate the state of contact with the electrolyte. As described in Patent Document 5, the "oil absorption amount" is an index for evaluating the contact area with the electrolyte in the obtained positive electrode active material, and a high oil absorption amount is one evidence that the positive electrode active material has excellent cycle characteristics and output characteristics. In view of this, as a method for improving the oil absorption of a positive electrode active material, Patent Document 6 reports a method for obtaining a metal composite hydroxide in which low-density regions and high-density regions are alternately laminated by switching the atmosphere of the crystallization reaction between an oxidizing atmosphere and a non-oxidizing atmosphere multiple times during the production of a precursor. By using this metal composite hydroxide as a precursor, a positive electrode active material having a porous structure can be obtained. However, although this method is effective in improving the oil absorption when used as a positive electrode active material, there are concerns that it takes time to switch between an oxidizing atmosphere and a non-oxidizing atmosphere during the production of the metal composite hydroxide, which leads to a decrease in productivity and that it is difficult to control the atmosphere during the switching. [Prior art documents] [Patent documents]

[0012] [Patent Document 1] JP 2012-246199 A [Patent Document 2] JP 2013-147416 A [Patent Document 3] WO2012 / 131881 publication [Patent Document 4] WO2014 / 181891 publication [Patent Document 5] JP 2018-022568 A [Patent Document 6] JP 2018-104273 A Summary of the Invention [Problem to be solved by the invention]

[0013] In view of the above-mentioned problems, the present invention has an object to provide a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, which is a nickel-cobalt-manganese composite hydroxide that has a high oil absorption and can improve output characteristics, by a method easier than conventional methods, and a method for producing a positive electrode active material for a lithium ion secondary battery. [Means for solving the problem]

[0014] The present inventors have focused on a method for producing a nickel-cobalt-manganese composite hydroxide, which is a precursor of a positive electrode active material having a hollow structure, in which switching between an oxidizing atmosphere and a non-oxidizing atmosphere is only required once, and have found that changing the method of introducing (hereinafter also referred to as "injecting") an oxidizing gas in the seed particle generation process and the seed particle growth process is a more effective means than the conventional method of injecting an oxidizing gas by bubbling the aqueous reaction solution in a reaction tank using an air diffuser. In the present invention, however, it has been found that a more effective means is to simultaneously inject the gas into the gas phase in the reaction tank (the space above the liquid level of the aqueous reaction solution) in addition to bubbling the gas into the aqueous reaction solution in the reaction tank. As a result, a precursor with a controlled density of seed particles can be obtained, and the positive electrode active material produced using this precursor has a high oil absorption capacity and can improve output characteristics, which led to the completion of the present invention.

[0015] A first aspect of the present invention is a method for producing nickel-cobalt-manganese composite hydroxide particles by a crystallization reaction in a reaction tank configured with a reaction aqueous solution formed by introducing and mixing a raw material aqueous solution containing at least nickel, cobalt, and manganese, an aqueous solution containing an ammonium ion donor, and an alkaline aqueous solution into a reaction tank, and a gas phase portion occupying the reaction tank other than the reaction aqueous solution, the method comprising: a seed particle generation step in which the gas phase portion is adjusted to an oxidizing atmosphere and the pH is controlled to 12.0 to 14.0 in the oxidizing atmosphere; a seed particle growth step in which the pH is controlled to 10.0 to 12.0 while maintaining the oxidizing atmosphere; and a particle growth step in which the gas phase portion is switched from an oxidizing atmosphere to a non-oxidizing atmosphere, the method being characterized in that in the seed particle generation step and the seed particle growth step, an oxidizing gas is introduced synchronously into both the reaction aqueous solution and the gas phase portion.

[0016] A second aspect of the present invention is a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, characterized in that the oxidizing atmosphere in the invention described in the first aspect is an atmosphere in which the oxygen concentration in the gas phase part in the reaction vessel exceeds 1 volume %, the non-oxidizing atmosphere is an atmosphere in which the oxygen concentration in the gas phase part in the reaction vessel is 1 volume % or less, and the oxidizing gas is a gas in which the oxygen concentration exceeds 1 volume %.

[0017] A third aspect of the present invention is a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, characterized in that the introduction of the oxidizing gas in the inventions described in the first and second aspects is performed by using an air diffuser from just below the center of the stirring blade.

[0018] A fourth aspect of the present invention is a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, characterized in that in the seed particle generation step and the seed particle growth step in the inventions described in the first to third aspects, when the oxidizing gas is introduced synchronously into both the aqueous reaction solution and the gas phase in the reaction tank, the introduction flow rates of the oxidizing gas per minute are both 1 / 100 or more of the capacity of the reaction tank.

[0019] A fifth aspect of the present invention is a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, characterized in that in the seed particle generation step and the seed particle growth step in the inventions described in the first to fourth aspects, a crystallization reaction is continued in a state in which a temperature in the reaction tank is maintained at 40° C. or higher.

[0020] A sixth aspect of the present invention is the positive electrode active material for a lithium ion secondary battery according to any one of the first to fifth aspects of the present invention. Precursor of But the general formula: Ni X Co Y Mn Z M T (OH) 2+α The present invention relates to a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, the precursor having a composition represented by the formula (X+Y+Z+T=1, 0.3≦X≦0.7, 0≦Y≦0.4, 0.1≦Z≦0.55, 0≦T≦0.1, 0≦α≦0.5, and M is one or more additive elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W).

[0021] A seventh aspect of the present invention is a compound represented by the general formula: Li 1+U Ni X Co Y Mn Z M T O 2+α(-0.05≦U≦0.50, X+Y+Z+T=1, 0.3≦X≦0.7, 0≦Y≦0.4, 0.1≦Z≦0.55, 0≦T≦0.1, 0≦α≦0.5, M is one or more additive elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W), and the lithium-nickel-cobalt-manganese composite oxide has a layered structure, a hexagonal crystal structure, and a hollow structure, and the method for producing a positive electrode active material for a lithium ion secondary battery is the first to sixth aspects. This method for producing a positive electrode active material for a lithium ion secondary battery includes a mixing step of mixing a precursor of the positive electrode active material for a lithium ion secondary battery obtained by the above-described method with a lithium compound to form a lithium mixture, and a firing step of firing the lithium mixture formed in the mixing step at a temperature of 800°C to 1000°C in a furnace atmosphere having an oxygen concentration of 10 to 100% by volume, and is characterized in that the oil absorption of the positive electrode active material for a lithium ion secondary battery can be controlled to 37.5 ml / 100 g or more. Effect of the Invention

[0022] According to the manufacturing method of the present invention, a precursor for a positive electrode active material for a lithium ion secondary battery can be obtained, in which the density of seed particles is controlled. Furthermore, a positive electrode active material for a lithium ion secondary battery produced using this precursor has a high oil absorption amount and can improve output characteristics. [Brief description of the drawings]

[0023] [Figure 1] FIG. 1 is a schematic flow chart showing the steps of producing a precursor of a positive electrode active material for a lithium ion secondary battery according to the present invention. [Diagram 2] FIG. 2 is a schematic diagram of a method for introducing (also referred to as driving) an oxidizing gas in the present invention, where (a) is a diagram illustrating the method of the present invention and (b) is a diagram illustrating a conventional method. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0024] The present invention relates to a method for producing a precursor of a positive electrode active material for a lithium ion secondary battery, and a method for producing a positive electrode active material for a lithium ion secondary battery. The positive electrode active material used in the positive electrode has a large impact on improving the performance of lithium-ion secondary batteries (hereinafter also referred to as "secondary batteries" or "batteries"). In order to obtain secondary batteries with excellent output characteristics, it is necessary to develop a positive electrode active material with high oil absorption.

[0025] The nickel-cobalt-manganese composite hydroxide (hereinafter also referred to as "composite hydroxide") obtained by the production method of the present invention is composed of secondary particles formed by aggregation of primary particles, and has an aggregate of fine and sparse primary particles present at the center of the secondary particle (hereinafter also referred to as "core") and a dense aggregate of primary particles (hereinafter also referred to as "shell") surrounding it. In the firing step of the manufacturing process of the positive electrode active material, firing of this composite hydroxide proceeds at a lower temperature in the center than in the outer shell, and the primary particles in the center shrink from the center of the secondary particles toward the outer shell where firing proceeds more slowly. In addition, since the central portion has a low density, the shrinkage rate is also large, and the central portion becomes a space having a sufficient size, forming a hollow portion inside the positive electrode active material.

[0026] The seed particles generated in the seed particle generation step described later constitute the aforementioned center portion, and by controlling the centrifugal sedimentation density of the seed particles to be low, the center portion has a structure in which there are more gaps between sufficiently fine primary particles, and the center portion shows a large amount of shrinkage in the aforementioned firing step, and the resulting positive electrode active material has a sufficiently large hollow portion. In addition, since the center portion has a large number of fine primary particles, the size of the primary particles in the outer shell portion also becomes small, and the outer shell portion of the positive electrode active material becomes thin. As a result, the oil absorption of the positive electrode active material becomes large, and when used in a battery, it shows excellent output characteristics.

[0027] In the present invention, the "oil absorption" is determined by the procedure described in "JIS_K_6217-4 (Carbon black for rubber-Fundamental properties-Part 4: Determination of oil absorption (including compressed samples))". However, since the operation process is complicated, the oil absorption is generally measured using an oil absorption (absorption) measuring device (e.g., "S-500" manufactured by Asahi Research Institute Co., Ltd.) that is commercially available in accordance with the above JIS. Typically, di-n-butyl phthalate (DBP) is used as the oil used for measurement, and the measurement results are calculated as the oil absorption per 100 g of sample, so the unit is "ml / 100 g."

[0028] Preferred embodiments of the present invention will be described in detail below in the following order. 1. Positive electrode active material for lithium-ion secondary batteries of Method for producing the precursor 2. Manufacturing method of positive electrode active material for lithium-ion secondary batteries The present embodiment described below does not unduly limit the contents of the present invention described in the claims, and can be modified without departing from the gist of the present invention. Furthermore, not all of the configurations described in the present embodiment are necessarily essential as the means for solving the problems of the present invention.

[0029] 1. Method for producing a precursor of a positive electrode active material for lithium-ion secondary batteries 〔overview〕 The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery of the present invention comprises the steps of: X Co Y Mn Z M T (OH) 2+αA method for producing a nickel-cobalt-manganese composite hydroxide, characterized in that the nickel-cobalt-manganese composite hydroxide has a composition represented by the formula (X+Y+Z+T=1, 0.3≦X≦0.7, 0≦Y≦0.4, 0.1≦Z≦0.55, 0≦T≦0.1, 0≦α≦0.5, M is one or more additive elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W), the method comprising the steps of: a "seed particle production step" of supplying a raw material aqueous solution in which at least a metal compound containing nickel, a metal compound containing cobalt, and a metal compound containing manganese are dissolved, an aqueous solution containing an ammonium ion donor, and an alkaline aqueous solution, and generating seed particles in an oxidizing atmosphere having an oxygen concentration of more than 1% by volume while controlling the pH to be 12.0 to 14.0 at a liquid temperature of 25° C.; and adding at least a metal compound containing nickel, and The crystallization reaction is characterized by including: a "seed particle growth step" in which a raw material aqueous solution in which a cobalt-containing metal compound and a manganese-containing metal compound are dissolved, an aqueous solution containing an ammonium ion donor, and an alkaline aqueous solution are supplied, and an oxidizing atmosphere with an oxygen concentration exceeding 1% by volume is maintained while controlling the pH to be 10.0 to 12.0 (a pH range lower than the pH range of the seed particle generation step) at a liquid temperature of 25°C; and a "particle growth step" in which a raw material aqueous solution in which at least a nickel-containing metal compound, a cobalt-containing metal compound, and a manganese-containing metal compound are dissolved, an aqueous solution containing an ammonium ion donor, and an alkaline aqueous solution are supplied to a reaction aqueous solution containing the seed particles grown in the seed particle growth step, and the atmosphere is switched from the previous oxidizing atmosphere to a non-oxidizing atmosphere with an oxygen concentration of 1% by volume or less, thereby growing the seed particles into particles.

[0030] [Crystallization reaction] The method for producing a composite hydroxide of the present invention is a method for producing a nickel-cobalt-manganese composite hydroxide by a crystallization reaction, and is composed of (A) a seed particle generation step, (B) a seed particle growth step, and (C) a particle growth step. As shown in FIG. 1, the method is characterized in that an oxidizing gas is injected in (A) and (B), which is different from conventional production methods.

[0031] (A) Seed particle generation process First, a plurality of metal compounds containing nickel, cobalt, and manganese are dissolved in water in a predetermined ratio to prepare a raw aqueous solution. In the method for producing a composite hydroxide of the present invention, the composition ratio of each metal in the obtained composite hydroxide is the same as the composition ratio of each metal in the raw aqueous solution. Therefore, the raw aqueous solution is prepared by controlling the ratio of metal compounds dissolved in water so that the composition ratio of each metal in the raw aqueous solution is within the same composition ratio range as the composition ratio range of each metal in the composite hydroxide in the present invention.

[0032] On the other hand, water, an aqueous solution containing an ammonium ion donor (such as an aqueous ammonia solution), and an aqueous alkali solution (such as an aqueous sodium hydroxide solution) are supplied to the reaction tank, and then the raw material aqueous solution is further supplied and mixed to prepare an aqueous reaction solution. The pH of the aqueous reaction solution is adjusted to 12.0 to 14.0, preferably 12.3 to 13.5, and more preferably 12.5 to 13.0 at a liquid temperature of 25°C by controlling the supply amount of the aqueous alkali solution. The ammonium ion concentration in the aqueous reaction solution is adjusted to 3 to 25 g / L, preferably 5 to 20 g / L, and more preferably 10 to 15 g / L by controlling the supply amount of the aqueous solution containing an ammonium ion donor.

[0033] The temperature in the reaction vessel is preferably 40° C. or higher, and the higher the temperature, the more preferable. However, if the temperature exceeds 60° C., ammonium ions will volatilize, so it is better to control the temperature to 40 to 60° C., and more preferably to control the temperature to 40 to 50° C. In this case, the atmosphere in the space (gas phase) in the reaction vessel is controlled to an oxidizing atmosphere using an oxidizing gas with an oxygen concentration of more than 1% by volume, and the oxygen concentration is set to more than 1% by volume, preferably more than 10% by volume, and more preferably more than 20% by volume.

[0034] The structure of the reaction vessel used to control the oxidizing atmosphere is shown in Figure 2. Fig. 2 is a schematic diagram of a method for introducing (also called "driving") an oxidizing gas, (a) is a diagram explaining the method of the present invention, and (b) is a diagram explaining a conventional method. In Fig. 2, 1 is a reaction vessel, 2 and 3 are aeration tubes for introducing gas, 4 is a stirring blade, 5 is a reaction aqueous solution, 6 is a stirrer, and A is a gas phase part in the reaction vessel.

[0035] 2(a), it is preferable to use diffusers 2 and 3 to introduce the oxidizing gas into the aqueous reaction solution 5 in the reaction vessel 1 and simultaneously inject (using diffuser 2) the gas into the gas phase A (space above the liquid level of the aqueous reaction solution) in the reaction vessel 1 in addition to bubbling (using diffuser 3) into the aqueous reaction solution 5. Furthermore, in bubbling into the aqueous reaction solution 5 in the reaction vessel 1, it is preferable to introduce the oxidizing gas from just below the center of the stirring blade 4 using diffuser 3. As a result, the bubbles of oxidizing gas bubbled through the air diffuser 3 are sheared by the rotation of the stirring blade 4, and in this state, finer bubbles can be diffused into the reaction aqueous solution 5. The pH and ammonium ion concentration of the reaction aqueous solution 5 in the reaction tank 1, and the oxygen concentration of the gas phase A in the reaction tank 1 can be measured using a general pH meter, ion meter, and oxygen concentration meter, respectively.

[0036] By the above-mentioned operation, fine seed particles of composite hydroxide are generated in the reaction aqueous solution. At this time, since the pH of the reaction aqueous solution is within the range of 12.0 to 14.0 based on a liquid temperature of 25°C, the generated seed particles hardly grow, and the generation of seed particles is preferentially performed. In order to prevent the pH and ammonium ion concentration of the reaction aqueous solution from changing, an aqueous solution containing an ammonium ion donor and an alkaline aqueous solution are continuously supplied together with the raw material aqueous solution, and the pH of the reaction aqueous solution is controlled so as to be maintained within the range of 12.0 to 14.0 based on a liquid temperature of 25°C, and the ammonium ion concentration is maintained within the range of 3 to 25 g / L, respectively.

[0037] By continuously supplying the aqueous solution containing an ammonium ion donor, the alkaline aqueous solution, and the raw material aqueous solution to the aqueous reaction solution, new seed particles are continuously generated in the aqueous reaction solution. When a predetermined amount of seed particles is generated in the aqueous reaction solution, the seed particle generation process is terminated. Whether or not the predetermined amount of seed particles has been generated is determined from the amount of metal salt added to the aqueous reaction solution.

[0038] (B) Seed particle growth process After the seed particle production process is completed, while maintaining the oxidizing atmosphere, the supply amount of the aqueous alkaline solution is controlled so that the pH of the aqueous reaction solution is adjusted to 10.0 to 12.0, preferably 10.5 to 12.0, and more preferably 11.0 to 12.0, based on a liquid temperature of 25°C.

[0039] Similarly to the seed particle production step, it is particularly preferable to control the temperature in the reaction tank to 40 to 50°C, and to maintain the atmosphere in the reaction tank as an oxidizing atmosphere by using an oxidizing gas. To introduce the oxidizing gas, an aeration tube is used similar to the previous step, and it is preferable to simultaneously use bubbling of the oxidizing gas into the aqueous reaction solution in the reaction tank and injection of the oxidizing gas into the gas phase (the space above the liquid surface of the aqueous reaction solution) in the reaction tank. Furthermore, in bubbling the oxidizing gas into the aqueous reaction solution in the reaction vessel, it is preferable to introduce the oxidizing gas from a diffuser tube directly below the center of the stirring blade.

[0040] By setting the pH of the reaction aqueous solution in the above range, seed particle growth takes precedence over seed particle generation, and the growth of seed particles is promoted with almost no new seed particles being generated. Similarly, an aqueous solution containing an ammonium ion donor is supplied and controlled so that the ammonium ion concentration can be maintained in the range of 3 to 25 g / L. Thereafter, when the seed particles grow to a predetermined particle size, the seed particle growth process is terminated.

[0041] (C) Particle growth process After the seed particle growth step is completed, the pH of the reaction aqueous solution is maintained at 10.0 to 12.0, preferably 10.5 to 12.0, and more preferably 11.0 to 12.0, based on a liquid temperature of 25°C, while the ammonium ion concentration is maintained at 3 to 25 g / L, preferably 5 to 20 g / L, and more preferably 10 to 15 g / L, and the atmosphere in the reaction tank is switched from an oxidizing atmosphere to a non-oxidizing atmosphere. The non-oxidizing atmosphere uses an inert gas such as nitrogen gas and has an oxygen concentration of 1% by volume or less, preferably 0.5% by volume or less, and more preferably 0.1% by volume or less.

[0042] By switching this atmosphere, the above-mentioned particle structure can be formed, in which the seed particles, i.e., the fine primary particles are in a coarse state, and the outside of the core of the composite hydroxide particles is an outer shell formed of plate-like primary particles that are larger than the primary particles and are in a dense state. Even in the particle growth step, new seed particles are hardly generated in the reaction aqueous solution, and the seed particles continue to grow (particle growth) to form a composite hydroxide having a predetermined particle size.

[0043] Thereafter, when the composite hydroxide grows to a predetermined particle size, the particle growth step is terminated. The particle size of the composite hydroxide can be easily determined from the amount of metal salt added in each step by determining the relationship between the amount of metal salt added to the reaction aqueous solution at each step of the seed particle generation step, the seed particle growth step, and the particle growth step and the particle size of the resulting particles in a preliminary test.

[0044] As explained above in (A), (B), and (C), in the method for producing a composite hydroxide, in the seed particle generating step, seed particle generation takes precedence, so seed particle growth hardly occurs, whereas in the seed particle growing step and particle growing step, particle growth takes precedence, so new seed particles are hardly generated. Therefore, in the seed particle generating step, uniform seed particles with a narrow particle size distribution can be formed, and in the seed particle growing step and particle growing step, seed particles can be grown uniformly.

[0045] Furthermore, as described above, by switching the atmosphere, it is possible to obtain a particle structure consisting of a central portion formed of fine primary particles in a coarse state and an outer portion formed of primary particles larger than the fine primary particles in a dense state. The pH of the reaction solution can be controlled by adding, in addition to the alkaline aqueous solution, an inorganic acid of the same type as the acid constituting the metal compound, for example, sulfuric acid in the case of sulfate, to the reaction solution.

[0046] The common manufacturing factors in each process are described in detail below. [Reaction atmosphere] The particle structure of the composite hydroxide of the present invention is formed by controlling the atmosphere in the reaction tank in the seed particle generation step, seed particle growth step, and particle growth step, and these steps are therefore of great significance. In an oxidizing atmosphere in the reaction tank during the crystallization reaction, the primary particles of the composite hydroxide do not grow, and the fine primary particles form coarse, low-density particles with many voids, whereas in a non-oxidizing atmosphere, the primary particles are large and dense, high-density particles are formed.

[0047] That is, by carrying out the seed particle generation process and the seed particle growth process in an oxidizing atmosphere, a central portion in which fine primary particles are in a coarse state is formed, and by switching from the oxidizing atmosphere to a non-oxidizing atmosphere in the subsequent particle growth process, a particle structure can be formed in which the outer side of the central portion has an outer shell portion in which plate-like primary particles larger than the fine primary particles are in a dense state.

[0048] In the crystallization reaction controlled by this atmosphere, the primary particles in the center are usually fine plate-like and / or needle-like, and the primary particles in the outer shell are plate-like, but depending on the composition, they may have a rectangular parallelepiped, elliptical, prismatic or other shape.

[0049] The oxidizing atmosphere for forming the central portion is defined as "an atmosphere in which the oxygen concentration in the reaction vessel exceeds 1% by volume." In addition, an oxidizing atmosphere in which the oxygen concentration exceeds 10% by volume is preferable, and an oxidizing atmosphere in which the oxygen concentration exceeds 20% by volume is more preferable. By using an atmosphere in which the oxygen concentration exceeds 1% by volume, the average particle size of the primary particles in the central portion can be set to 0.01 to 0.3 μm. If the oxygen concentration is 1% by volume or less, the average particle size of the primary particles in the central portion may exceed 0.3 μm. The upper limit of the oxygen concentration is not particularly limited, but if it exceeds 30% by volume, the average particle size of the primary particles in the central portion may be less than 0.01 μm, which is not preferable.

[0050] On the other hand, the non-oxidizing atmosphere for forming the outer shell is defined as "an atmosphere in which the oxygen concentration in the reaction vessel is 1% by volume or less." Preferably, the oxygen concentration is controlled to be 0.5% by volume or less, more preferably 0.1% by volume or less, so that the atmosphere is a mixture of oxygen and inert gas. By making the oxygen concentration in the space in the reaction vessel 1% by volume or less and growing the particles, unnecessary oxidation of the particles is suppressed, the growth of the primary particles is promoted, and secondary particles having a dense and high-density outer shell with an average particle size of 0.30 to 3.0 μm, a primary particle size larger than that of the center, and uniform particle size can be obtained.

[0051] As a means for maintaining such an atmosphere inside the reaction tank, it is known to introduce an oxidizing gas such as air into the space (gas phase) inside the reaction tank in order to create an oxidizing atmosphere, or an inert gas such as nitrogen into the space (gas phase) inside the reaction tank in order to create a non-oxidizing atmosphere. In a conventional method, it is known that bubbling of gas into the aqueous reaction solution is effective.

[0052] Therefore, the present invention is characterized in that "bubbling into the liquid" and "injection of the gas phase" are performed simultaneously, as shown in Fig. 2(a). In addition, in "bubbling into the liquid", it is preferable to introduce the above-mentioned gas from an air diffuser 3 directly below the center of the stirring blade 4. This allows the gas bubbles bubbled by the air diffuser 3 to be sheared by the rotation of the stirring blade 4, and diffused in the reaction aqueous solution 5 in a finer bubble state.

[0053] The timing of switching the atmosphere in the particle growth process is determined taking into consideration the size of the central part of the composite hydroxide particle so that the final positive electrode active material has a hollow portion that is large enough not to cause the generation of fine particles and deteriorate the cycle characteristics. For example, the switching is performed for 0 to 40%, preferably 0 to 30%, and more preferably 0 to 25% of the total time of the particle growth process from the start of the particle growth process. If the switching is performed at a time exceeding 40% of the total time of the particle growth process, the central part formed may become large, and the thickness of the outer shell in the particle diameter of the secondary particles may become too thin. On the other hand, if the switching is performed before the start of the particle growth process, i.e., during the seed particle growth process, the central part may become too small, or secondary particles having the above structure may not be formed.

[0054] [pH control] In the seed particle generating step, it is necessary to control the pH of the reaction aqueous solution to be in the range of 12.0 to 14.0, preferably 12.3 to 13.5, based on a liquid temperature of 25°C. If the pH exceeds 14.0, the seed particles generated will be too fine, and the reaction aqueous solution will gel. If the pH is less than 12.0, the seed particle formation and the seed particle growth reaction will occur simultaneously, and the particle size distribution of the formed seed particles will be broad and the particles will be heterogeneous. That is, by controlling the pH of the reaction aqueous solution in the above range in the seed particle generating step, the seed particle growth can be suppressed and only the seed particle generation can occur, and the formed seed particles can be homogeneous and have a narrow particle size distribution.

[0055] On the other hand, in the seed particle growth step and the particle growth step, it is necessary to control the pH of the reaction aqueous solution to be in the range of 10.5 to 12.0, preferably 11.0 to 12.0, based on a liquid temperature of 25°C. If the pH exceeds 12.0, the number of newly generated seed particles increases, and fine secondary particles are generated, so that a hydroxide with a good particle size distribution cannot be obtained. If the pH is less than 10.5, the solubility of ammonia ions is high, and the number of metal ions that remain in the liquid without being precipitated increases, resulting in a deterioration in production efficiency. That is, by controlling the pH of the reaction aqueous solution in the above range in the particle growth step, it is possible to preferentially cause the growth of only the seed particles generated in the seed particle generation step, suppress the formation of new seed particles, and make the obtained composite hydroxide homogeneous and have a narrow particle size distribution.

[0056] In any of the seed particle generation step, the seed particle growth step, and the particle growth step, the pH fluctuation range is preferably within ±0.2 of the set value. If the pH fluctuation range is large, the seed particle generation, seed particle growth, and particle growth may not be constant, and a uniform composite hydroxide with a narrow particle size distribution may not be obtained. In addition, since a pH of 12.0 is the boundary condition between seed particle generation and seed particle growth, the conditions can be set to either the seed particle generation process or the seed particle growth process depending on the presence or absence of seed particles in the reaction aqueous solution.

[0057] That is, if the pH in the seed particle generation step is made higher than 12.0 to generate a large amount of seed particles, and then the pH is made 12.0 in the seed particle growth step, the large amount of seed particles present in the reaction aqueous solution causes seed particle growth to occur preferentially, resulting in a hydroxide with a narrow particle size distribution and a relatively large particle size. On the other hand, if no seed particles are present in the reaction aqueous solution, that is, if the pH in the seed particle generation step is made 12.0, there are no seed particles to grow, so seed particle generation occurs preferentially, and by making the pH in the particle growth step lower than 12.0, the generated seed particles grow, resulting in a good hydroxide.

[0058] In either case, the pH of the seed particle growth process and the particle growth process may be controlled to a lower value than the pH of the seed particle generation process. In order to clearly separate seed particle generation and seed particle growth, it is preferable to set the pH of the seed particle growth process and the particle growth process to be 0.5 or more lower than the pH of the seed particle generation process, and it is particularly preferable to set the pH of the seed particle growth process to be 1.0 or more lower.

[0059] [Amount of seed particles produced] The amount of seed particles produced in the seed particle production step is not particularly limited, but in order to obtain a composite hydroxide having a good particle size distribution, the amount is preferably 0.1 to 2% of the total amount, i.e., of all metal salts supplied to obtain the composite hydroxide, and more preferably 1.5% or less.

[0060] [Control of particle size of composite hydroxide] The particle size of the composite hydroxide can be controlled by the total time of the seed particle generation step, the seed particle growth step, and the particle growth step, and by continuing the particle growth step until the desired particle size is reached, composite hydroxide particles having a desired particle size can be obtained. The particle size of the composite hydroxide can be controlled not only by the seed particle generation step, the seed particle growth step, and the particle growth step, but also by the pH of the seed particle generation step and the amount of raw material input for seed particle generation. That is, by setting the pH of the seed particle generation step to a high pH side or by extending the time of the seed particle generation step, the amount of raw material input can be increased, and the amount of seed particles generated can be increased. As a result, even if the seed particle growth step and the particle growth step are carried out under the same conditions, the particle size of the composite hydroxide can be made small. On the other hand, by controlling the amount of seed particles produced to be small, the particle size of the obtained composite hydroxide can be made large.

[0061] Next, various conditions such as the metal compound, the ammonia concentration in the reaction aqueous solution, and the reaction temperature will be described. The differences between the seed particle generation process, the seed particle growth process, and the particle growth process are the control of the pH of the reaction aqueous solution and the atmosphere in the reaction tank, and the conditions such as the metal compound, the ammonia concentration in the reaction aqueous solution, and the reaction temperature are substantially the same in each process.

[0062] [Metal compound] The metal compound used is a compound containing the target metal, and is preferably a water-soluble compound, such as sulfate, chloride, or nitrate, more preferably nickel sulfate, manganese sulfate, or cobalt sulfate.

[0063] [Additional element (M)] The additive element (M) (one or more elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W) is preferably a water-soluble compound, and examples of the additive element that can be used include titanium sulfate, ammonium peroxotitanate, potassium titanium oxalate, vanadium sulfate, ammonium vanadate, chromium sulfate, potassium chromate, zirconium sulfate, zirconium nitrate, niobium oxalate, ammonium molybdate, sodium tungstate, and ammonium tungstate. When the additive element is to be uniformly dispersed inside the composite hydroxide, an additive containing the additive element may be added to the raw material aqueous solution, and the additive element can be coprecipitated in a state where it is uniformly dispersed inside the composite hydroxide.

[0064] In addition, when the surface of the composite hydroxide is coated with an additive element, for example, the composite hydroxide is slurried in an aqueous solution containing the additive element, and while controlling the pH to a predetermined level, an aqueous solution containing one or more additive elements is added to precipitate the additive element on the particle surface of the composite hydroxide by a crystallization reaction, whereby the surface can be uniformly coated with the additive element. In this case, an alkoxide solution of the additive element may be used instead of the aqueous solution containing the additive element. Furthermore, the particle surface of the composite hydroxide can be coated with the additive element by spraying an aqueous solution or slurry containing the additive element onto the composite hydroxide and drying it. Also, the composite hydroxide can be coated by spray drying a slurry in which the composite hydroxide and one or more salts containing the additive element are suspended, or by mixing the composite hydroxide and one or more salts containing the additive element by a solid phase method.

[0065] In addition, when the surface is coated with an additive element, the atomic ratio of the additive element ions present in the raw material aqueous solution can be made to coincide with the atomic ratio of the metal ions in the obtained composite hydroxide by reducing the atomic ratio of the additive element ions present in the raw material aqueous solution by the amount to be coated. In addition, the step of coating the particle surface with the additive element may be performed on the particles after the composite hydroxide is heated.

[0066] [Concentration of raw material aqueous solution] The concentration of the raw aqueous solution is adjusted to 1.0 to 2.6 mol / L, preferably 1.5 to 2.2 mol / L, in terms of the total amount of metal compounds. If the concentration of the raw aqueous solution is less than 1.0 mol / L, the amount of crystallized material per reaction tank decreases, which is undesirable since it reduces productivity. On the other hand, if the salt concentration of the raw aqueous solution exceeds 2.6 mol / L, it exceeds the saturation concentration at room temperature, so there is a risk of crystals re-precipitating and clogging the equipment piping.

[0067] In addition, the metal compounds do not necessarily need to be supplied to the reaction tank as a raw material aqueous solution in which all of them are mixed. For example, when using metal compounds that react when mixed to produce another compound, the aqueous solutions of the metal compounds may be prepared individually so that the total concentration of the aqueous solutions of all the metal compounds is within the above range, and each may be supplied to the reaction tank at a predetermined ratio at the same time. Furthermore, the amount of the raw material aqueous solution and the aqueous solutions of the individual metal compounds to be supplied to the reaction tank is adjusted so that the crystallization concentration at the time when the crystallization reaction is completed is approximately 30 to 200 g / L, preferably 80 to 150 g / L. If the crystallization concentration is less than 30 g / L, the aggregation of primary particles may be insufficient, and if it exceeds 200 g / L, the diffusion of the raw material aqueous solution added in the reaction tank may be insufficient, causing uneven particle growth.

[0068] [Ammonia concentration] The ammonia concentration in the reaction aqueous solution is controlled to be preferably 3 to 25 g / L, more preferably 5 to 20 g / L, in order to avoid the following problems. Ammonia acts as a complexing agent, so if the ammonia concentration is less than 3 g / L, the solubility of metal ions cannot be kept constant, and plate-like hydroxide primary particles with uniform shape and particle size are difficult to form, and gel-like seed particles are likely to be generated, resulting in a broader particle size distribution. On the other hand, if the ammonia concentration exceeds 25 g / L, the solubility of metal ions becomes too high, and the amount of metal ions remaining in the reaction aqueous solution increases, causing deviations in the composition, etc.

[0069] In addition, when the ammonia concentration fluctuates, the solubility of metal ions also fluctuates, and a uniform hydroxide is not formed, so it is preferable to maintain the ammonia concentration at a constant value, and it is more preferable to maintain the ammonia concentration at a desired concentration, for example, with the upper and lower limits set to about 5 g / L. The ammonium ion donor is not particularly limited, and examples of the ammonium ion donor that can be used include ammonia, ammonium sulfate, ammonium carbonate, ammonium chloride, and ammonium fluoride.

[0070] [Temperature of reaction aqueous solution] In the reaction tank, the temperature of the aqueous reaction solution is preferably set to 20° C. or higher, more preferably 20 to 60° C., and particularly preferably 40 to 50° C. If the temperature of the aqueous reaction solution is less than 20° C., the solubility is low, so that seed particle generation is likely to occur and control becomes difficult. On the other hand, if the temperature exceeds 60° C., the volatilization of ammonia is promoted, and in order to maintain a predetermined ammonia concentration, an excess of ammonium ion donor must be added, which increases costs.

[0071] [Temperature inside the reactor] The temperature in the reaction vessel is also an important factor for the formation of the composite hydroxide. The temperature in the reaction vessel is preferably set to 40 to 60°C, more preferably 40 to 50°C. In particular, in the seed particle generation process and the seed particle growth process, the higher the temperature is, the more likely it is that a precursor that will become a positive electrode active material with a high oil absorption can be produced. However, a temperature higher than 60°C is not preferable because it promotes the volatilization of ammonia.

[0072] [Alkaline aqueous solution] The alkaline aqueous solution used to adjust the pH of the reaction aqueous solution is not particularly limited, but for example, an aqueous solution in which an alkali metal hydroxide, such as sodium hydroxide or potassium hydroxide, is dissolved can be used. In the case of an alkali metal hydroxide, it may be directly supplied to the reaction aqueous solution, but it is preferable to add it as an aqueous solution because it is easy to control the pH of the reaction aqueous solution in the reaction tank. In addition, the method of adding the alkaline aqueous solution to the reaction tank is also not particularly limited, but it may be added while thoroughly stirring the reaction aqueous solution, using equipment capable of controlling the flow rate, such as a metering pump, so that the pH of the reaction aqueous solution is maintained within a predetermined range.

[0073] [Manufacturing equipment] In the method for producing a composite hydroxide of the present invention, equipment is used that does not recover the product until the reaction is completed. For example, a batch reaction tank 1 equipped with an agitator 6 having an agitating blade 4 as shown in Fig. 2 is used. When such equipment is used, unlike a continuous crystallizer that recovers the product by overflow, the problem of growing particles being recovered together with the overflow liquid does not occur, and it is possible to obtain particles with a narrow particle size distribution and a uniform particle size. In addition, it is necessary to control the reaction atmosphere, and therefore equipment capable of controlling the atmosphere, such as a sealed equipment, is used. By using such equipment, the composite hydroxide can be made to have the above-mentioned structure, and the seed particle generation reaction, seed particle growth reaction, and particle growth reaction can be made to proceed almost uniformly, so that particles with an excellent particle size distribution, i.e., particles with a narrow particle size distribution, can be obtained.

[0074] The composition of the nickel-cobalt-manganese composite hydroxide obtained by the above-mentioned production method is controlled to be expressed by the following general formula: If a lithium-nickel-cobalt-manganese composite oxide is produced using a composite hydroxide having such a composition as a precursor, when an electrode having the obtained lithium-nickel-cobalt-manganese composite oxide as a positive electrode active material is used in a battery, the positive electrode resistance can be reduced, excellent output characteristics can be exhibited, and the battery performance can be improved.

[0075] General formula: Ni X Co Y MnZ M T (OH) 2+α (X+Y+Z+T=1, 0.3≦X≦0.7, 0≦Y≦0.4, 0.1≦Z≦0.55, 0≦T≦0.1, 0≦α≦0.5, M is one or more additive elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W)

[0076] In the present invention, when a hollow-structured positive electrode active material is to be obtained, the nickel content, cobalt content, and manganese content of the precursor nickel-cobalt-manganese composite hydroxide are controlled to be 0.3≦X≦0.7, 0≦Y≦0.4, and 0.1≦Z≦0.55 in the above general formula, respectively, and the manganese content is set to be high, thereby making it possible to obtain a nickel-cobalt-manganese composite hydroxide consisting of secondary particles that are easy to obtain a hollow structure. When a positive electrode active material is obtained using this composite hydroxide as a precursor, the composition ratio (Ni:Mn:Co) of the composite hydroxide is maintained in the obtained positive electrode active material. Therefore, the composition ratio of the composite hydroxide in the present invention is controlled to be similar to the composition ratio required for the positive electrode active material to be obtained.

[0077] [Average particle size] The average particle size of the composite hydroxide of the present invention is controlled to be in the range of 1 to 15 μm, preferably 3 to 10 μm. This allows the cathode active material obtained using the composite hydroxide as a precursor to be controlled to a predetermined average particle size (1 to 15 μm). As described above, the particle size of the composite hydroxide correlates with the particle size of the obtained cathode active material, and therefore affects the characteristics of the battery using this cathode active material as a cathode material. When the average particle size of the composite hydroxide is less than 1 μm, the average particle size of the obtained cathode active material also becomes small, and the surface area increases, so that high output can be obtained, but the packing density of the cathode decreases and the battery capacity per volume decreases. In addition, when the electrode paste is mixed, the dispersibility with the conductive assistant deteriorates, and the voltage applied to the particles in the electrode becomes uneven, so that the particles deteriorate when repeatedly charged and discharged, and the battery capacity decreases. Conversely, when the average particle size of the composite hydroxide exceeds 15 μm, the specific surface area of ​​the obtained cathode active material decreases, and the interface with the electrolyte decreases, so that the cathode resistance increases and the output characteristics of the battery decrease.

[0078] [Particle size distribution] The composite hydroxide of the present invention is controlled so that [(d90-d10) / average particle size], which is an index showing the breadth of the particle size distribution, is 1.0 or less, preferably 0.5 or less. The particle size distribution of the positive electrode active material is strongly influenced by the composite hydroxide, which is the precursor. For example, if fine particles or coarse particles are present in the composite hydroxide, fine particles or coarse particles are also present in the positive electrode active material. In other words, if [(d90-d10) / average particle size] exceeds 1.0 and the particle size distribution is wide, fine particles or coarse particles are present in the positive electrode active material.

[0079] When a positive electrode is formed using a positive electrode active material containing many fine particles, local reactions of the fine particles may cause heat generation, which reduces the safety of the battery, and the fine particles may selectively deteriorate, resulting in poor cycle characteristics of the battery. On the other hand, when a positive electrode is formed using a positive electrode active material containing many coarse particles, the reaction area between the electrolyte and the positive electrode active material is insufficient, and the reaction resistance increases, resulting in a decrease in battery output.

[0080] The average particle size, d90, and d10 can be calculated from the volume accumulated value measured by a particle size analyzer using a laser diffraction / scattering method. In the index [(d90-d10) / average particle size] that indicates the spread of particle size distribution, d10 means the particle size at which the cumulative volume, calculated by accumulating the number of particles at each particle size from the smallest particle size side, is 10% of the total volume of all particles. Similarly, d90 means the particle size at which the cumulative volume, calculated by accumulating the number of particles in the same way, is 90% of the total volume of all particles. For the average particle size, the volume average particle size MV can be used.

[0081] [Particle structure] The composite hydroxide of the present invention is composed of secondary particles formed by agglomeration of a plurality of primary particles. The primary particles constituting the secondary particles have various shapes, such as plate-like, needle-like, rectangular, elliptical, and rhombohedral. The agglomeration state may be such that the particles are agglomerated in a random direction, or may be agglomerated in a radial manner from the center in the long diameter direction. However, in the present invention, it is preferable that the plate-like and / or needle-like primary particles are agglomerated in a random direction to form the secondary particles. In the case of such a structure, voids are generated almost uniformly between the primary particles, and when mixed with a lithium compound and sintered, the molten lithium compound spreads throughout the secondary particles, and lithium is diffused sufficiently.

[0082] The average particle size of the primary particles constituting the secondary particles is preferably controlled to a range of 0.3 to 3 μm. By controlling the size of the primary particles in this manner, appropriate voids are obtained between the primary particles, and lithium is sufficiently and easily diffused into the secondary particles during firing. The average particle size of the primary particles is more preferably 0.4 to 1.5 μm. If the average particle size of the primary particles is less than 0.3 μm, the firing temperature during firing becomes low, sintering between secondary particles increases, and the resulting positive electrode active material contains many coarse particles. On the other hand, if the average particle size of the primary particles exceeds 3 μm, the firing temperature must be increased in order to ensure sufficient crystallinity of the resulting positive electrode active material, and high-temperature firing causes sintering between secondary particles, resulting in the particle size distribution of the positive electrode active material falling outside the appropriate range.

[0083] In the present invention, a hollow structure having a dense and thin outer shell and a hollow interior is obtained as the secondary particle structure of the positive electrode active material. On the other hand, as a precursor of the hollow structure positive electrode active material, a composite hydroxide has a center part which is an aggregate of fine and sparse primary particles forming a hollow space, and an outer part which is an aggregate of dense primary particles surrounding the center part. In such a particle structure, the properties of the primary particles have an influence. That is, it is preferable that the fine primary particles are randomly aggregated in the center and the larger primary particles are randomly aggregated in the outer shell. Such randomly oriented aggregation causes uniform shrinkage in the center, and allows the positive electrode active material to form a sufficiently large space.

[0084] In this case, the average particle size of the fine primary particles is preferably 0.01 to 0.3 μm, more preferably 0.1 to 0.3 μm. If the average particle size of the fine primary particles is less than 0.01 μm, a center portion of sufficient size may not be formed in the composite hydroxide, and if it exceeds 0.3 μm, the shrinkage may be insufficient, and a space of sufficient size may not be obtained in the positive electrode active material after firing. The properties of the primary particles of the outer shell may be the same as those described above.

[0085] The secondary particles constituting the positive electrode active material obtained using such composite hydroxide as a precursor have a hollow structure, and the ratio of the thickness of the outer shell to the secondary particle diameter is roughly maintained as that of the composite hydroxide. Therefore, by setting the ratio of the thickness of the outer shell to the secondary particle diameter in the composite hydroxide to the above-mentioned range of the primary particles, sufficient hollow portions can be formed in the lithium metal composite oxide.

[0086] The particle size of the fine primary particle in the center and the larger primary particle in the outer shell, as well as the thickness of the outer shell, can be observed by measuring the cross section of the composite hydroxide with a scanning electron microscope (SEM). For example, multiple composite hydroxides (secondary particles) are embedded in a resin and processed with a cross-section polisher (CP) to enable cross-section observation of the particles. The particle size of the fine primary particle in the center and the larger primary particle in the outer shell can be determined by measuring the maximum diameter of the cross section of preferably 10 or more primary particles among the secondary particles as the particle size and calculating the average value.

[0087] The ratio of the thickness of the outer shell to the secondary particle diameter can be determined as follows. First, from the secondary particles in the resin, particles that allow cross-sectional observation of the particle center are selected, and the distance between two points on the outer circumference of the outer shell and the inner circumference of the center side is measured at three or more arbitrary points to obtain the average thickness of the outer shell for each particle. Next, the distance between two arbitrary points on the outer circumference of the secondary particle that is the maximum distance is taken as the secondary particle diameter, and the ratio of the outer shell thickness for each particle is obtained by dividing the average thickness by this secondary particle diameter. Furthermore, the ratios for each particle obtained for 10 or more particles are averaged, so that the ratio of the outer shell thickness to the secondary particle diameter in the composite hydroxide can be obtained.

[0088] [Method of manufacturing positive electrode active material for lithium ion secondary batteries] The method for producing a positive electrode active material in the present invention mainly comprises two steps: a "mixing step" in which the nickel-cobalt-manganese composite hydroxide obtained by the above-mentioned method for producing a precursor is mixed with a lithium compound to form a lithium mixture, and a "calcination step" in which the lithium mixture formed in the mixing step is calcined. However, a "heat treatment step" in which the composite hydroxide is heat-treated and converted into a "composite oxide" may be added before the mixing step. That is, the production method can include three steps: (a) a heat treatment step in which the nickel-cobalt-manganese composite hydroxide, which is a precursor of the positive electrode active material, is heat-treated; (b) a mixing step in which a lithium compound is mixed with the particles after the heat treatment to form a lithium mixture; and (c) a calcination step in which the lithium mixture formed in the mixing step is calcined. Each step will be described below.

[0089] (a) Heat treatment process The heat treatment step is a step of heating the composite hydroxide obtained by the above-mentioned method for producing a precursor to a temperature of 105 to 750°C, preferably 105 to 400°C, and performing a heat treatment. By performing this heat treatment step, it is possible to remove the moisture contained in the composite hydroxide, and it is possible to prevent the ratio of the number of metal atoms and the number of lithium atoms from varying in the obtained positive electrode active material. Here, it is sufficient to remove the moisture to such an extent that the ratio of the number of metal atoms and the number of lithium atoms in the positive electrode active material does not vary, and it is not necessary to convert all of the composite hydroxide into a "composite oxide".

[0090] Therefore, heat treatment at a temperature below 400°C is sufficient, but to further reduce variation, the heat treatment temperature should be 400°C or higher to convert all of the complex hydroxides to "complex oxides." In the subsequent firing process, the complex hydroxides are also converted to "complex oxides" during heating, but by carrying out heat treatment in advance, variation can be further reduced.

[0091] In the heat treatment step, if the heat treatment temperature is less than 105°C, the moisture in the composite hydroxide cannot be removed, and the variation may not be sufficiently prevented. On the other hand, if the heat treatment temperature exceeds 750°C, the particles may be sintered by the heat treatment, and a composite oxide with a uniform particle size may not be obtained. In addition, the variation can be prevented by determining the metal components contained in the composite hydroxide in advance by analysis and determining the ratio with the lithium compound.

[0092] The atmosphere in the heat treatment is not particularly limited, but it is sufficient to use an oxidizing atmosphere, and it is preferable to use an air stream, which is easy to use. The heat treatment time is not particularly limited, but if it is less than 1 hour, the moisture of the composite hydroxide may not be sufficiently removed, so it is preferable to use at least 1 hour, and more preferably 5 to 15 hours. The equipment used for the heat treatment is not particularly limited, but it is sufficient to use an electric furnace that does not generate gas, so long as it can heat the composite hydroxide in an oxidizing atmosphere, preferably in an air stream.

[0093] (b) Mixing process The mixing step is a step of mixing a composite hydroxide or a composite oxide heat-treated in a heat treatment step (hereinafter also referred to as a "heat-treated product") with a lithium compound to obtain a lithium mixture. Here, the heat-treated product includes not only a composite hydroxide from which moisture has been removed to a certain extent in the heat treatment step, but also a composite oxide converted into an oxide, or a mixture thereof. The heat-treated product and the lithium compound are mixed so that the ratio (Li / Me) of the number of atoms of metals other than lithium in the lithium mixture, that is, the sum of the numbers of atoms of nickel, cobalt, manganese, and added elements (Me) to the number of lithium atoms (Li) is 0.95 to 1.5, preferably 1 to 1.35, and more preferably 1 to 1.20. That is, since Li / Me does not usually change before and after the baking step, the Li / Me in this mixing step becomes the Li / Me in the positive electrode active material, so the mixture is mixed so that the Li / Me of the lithium mixture becomes the same as the Li / Me of the positive electrode active material.

[0094] The lithium compound is not particularly limited, but for example, lithium hydroxide, lithium carbonate, lithium sulfate, lithium chloride, lithium nitrate, or a mixture thereof is preferable because it is easily available. In particular, in consideration of ease of handling and stability of quality, it is more preferable to use lithium hydroxide, lithium carbonate, or a mixture thereof.

[0095] In addition, it is preferable to thoroughly mix the lithium mixture before the firing step. If the mixture is not thoroughly mixed, the Li / Me ratio varies between individual particles, and problems such as insufficient battery characteristics may occur. For mixing, a general mixer can be used, such as a shaker mixer, a Lödige mixer, a Julia mixer, or a V blender, and it is sufficient to thoroughly mix the lithium compound with the heat-treated product to the extent that the shell of the heat-treated product is not destroyed.

[0096] (c) Firing process The calcination step is a step of calcining the lithium mixture obtained in the mixing step to form a lithium metal composite oxide. When the lithium mixture is calcined in the calcination step, lithium in the lithium compound is diffused into the heat-treated product, and a lithium metal composite oxide is formed.

[0097] [Firing temperature] The lithium mixture is sintered at 650 to 1000°C. If the sintering temperature is less than 650°C, the diffusion of lithium into the heat-treated material is insufficient, and excess lithium and unreacted heat-treated material are likely to remain, and problems such as difficulty in arranging the crystal structure occur, and sufficient characteristics cannot be obtained when used in a battery. If the sintering temperature exceeds 1000°C, intense sintering occurs between the lithium metal composite oxides and abnormal grain growth occurs, so that the particles become coarse and the shape of the spherical secondary particles cannot be maintained. In either case, not only does the battery capacity decrease, but the positive electrode resistance also increases. The sintering temperature is preferably 800 to 980°C, and more preferably 850 to 950°C.

[0098] [Baking time] During the firing time, the holding time at a predetermined temperature is preferably at least 1 hour, and more preferably 2 to 10 hours. If it is less than 1 hour, the production of the lithium metal composite oxide may not be sufficient.

[0099] [Pre-firing] In particular, when lithium hydroxide and lithium carbonate are used as the lithium compounds, it is preferable to hold the mixture at a temperature lower than the firing temperature, 350 to 800°C, preferably 450 to 780°C, for about 1 to 10 hours, more preferably 3 to 6 hours, prior to the firing step, for pre-firing. Alternatively, by slowing down the rate of temperature rise until the firing temperature is reached, it is possible to obtain substantially the same effect as in the case of pre-firing. That is, it is preferable to pre-firing at the reaction temperature of the lithium hydroxide and lithium carbonate with the heat-treated product. In this case, if the mixture is held at a temperature near the reaction temperature of the lithium hydroxide and lithium carbonate, lithium is sufficiently diffused into the heat-treated product, and a uniform lithium metal composite oxide can be obtained.

[0100] [Firing atmosphere] The firing atmosphere is preferably an oxidizing atmosphere, more preferably an atmosphere with an oxygen concentration of 10 to 100% by volume, and particularly preferably an atmosphere of a mixture of oxygen and an inert gas with an oxygen concentration. That is, it is preferable to carry out the oxidation in the air or in an oxygen stream. If the oxygen concentration is less than 10% by volume, the oxidation may be insufficient, and the crystallinity of the lithium metal composite oxide may be insufficient. The furnace used for firing is not particularly limited as long as it can heat in the air or in an oxygen stream. From the viewpoint of maintaining a uniform atmosphere in the furnace, an electric furnace that does not generate gas is preferable, and a batch or continuous furnace is used.

[0101] [Crushing] The lithium metal composite oxide obtained by firing may be aggregated or slightly sintered. In this case, the lithium metal composite oxide may be crushed to obtain the lithium metal composite oxide, i.e., the positive electrode active material of the present invention. The term "crushing" refers to an operation in which mechanical energy is applied to an aggregate of multiple secondary particles that is generated during firing due to sintering necking between secondary particles, and the secondary particles are separated without substantially destroying the secondary particles themselves, thereby breaking up the aggregates. The crushing method can be performed using a known means, such as a pin mill or a hammer mill. In addition, it is preferable to control the crushing force within an appropriate range so as not to destroy the secondary particles. EXAMPLES

[0102] Examples of the present invention and comparative examples will be described in detail below. EXAMPLES

[0103] <Production of nickel-cobalt-manganese composite hydroxide (precursor)> (1) Seed particle generation process First, water was poured into a 600 L reaction tank 1 (see FIG. 2 for reference symbols), half the volume of the tank was filled, and the crystallization temperature (temperature inside the tank, liquid temperature) was set to 42° C. while stirring, creating an oxidizing atmosphere (oxygen concentration: 21% by volume) inside the reaction tank (gas phase). Appropriate amounts of aqueous sodium hydroxide solution (20% by mass) and aqueous ammonia (25% by mass) were added to the water in the reaction tank, and the pH of the reaction solution in the tank was controlled to 13.0 (based on liquid temperature of 25° C.), while the ammonia concentration in the reaction solution was controlled to 10 g / L.

[0104] Next, nickel sulfate, manganese sulfate, and cobalt sulfate were dissolved in water to prepare a 2 mol / L raw material aqueous solution, and the element molar ratio of each metal was controlled to be Ni:Co:Mn=33:33:33. This raw material aqueous solution was supplied to the reaction aqueous solution in the reaction tank at a predetermined ratio, and simultaneously, sodium hydroxide aqueous solution (20 mass%) and ammonia water (25 mass%) were also added to the reaction aqueous solution at a constant rate, and seed particles were generated by crystallization for a predetermined time while controlling the ammonia concentration in the reaction aqueous solution to 10 g / L and the pH to 13.0 (based on a liquid temperature of 25° C.).

[0105] Furthermore, air was introduced (20 L / min) into the gas phase A through the air diffuser 2, and air was bubbled (40 L / min) into the reaction solution through the air diffuser 3 from just below the center of the stirring blade.

[0106] (2) Seed particle growth process After completion of the generation of seed particles, sulfuric acid was added until the pH of the reaction aqueous solution reached 11.6 (based on a liquid temperature of 25°C). After the pH of the reaction aqueous solution reached 11.6 (based on a liquid temperature of 25°C), the supply of an aqueous sodium hydroxide solution (20 mass%) to the reaction aqueous solution was resumed. While maintaining the pH at 11.6 (based on a liquid temperature of 25°C), crystallization was continued for 180 minutes to grow seed particles. Further, the introduction of air into the gas phase portion A through the air diffuser 2 and the air bubbling into the reaction aqueous solution through the air diffuser 3 were continued under the same conditions as above.

[0107] (3) Particle growth process All liquid supply was temporarily stopped, and air introduction into the gas phase and air bubbling into the reaction solution were terminated. Nitrogen gas was introduced at a flow rate of 100 L / min through an aeration tube (not shown) until the oxygen concentration in the reaction tank (gas phase) was 0.1% by volume or less. Then, all liquid supply was resumed and crystallization was carried out for 210 minutes. The product was then washed with water, filtered, and dried, and the product was named "Ni 0.33 Co 0.33 Mn 0.33 We obtained a complex hydroxide represented by the formula "(OH)2".

[0108] <Production of lithium nickel cobalt manganese composite oxide (positive electrode active material)> (1) Heat treatment and firing process The composite hydroxide thus obtained was heat-treated at 150°C for 12 hours, after which commercially available lithium carbonate was added so that the molar ratio of metal to lithium (Li / Me) was 1.15, and the mixture was thoroughly mixed using a shaker mixer (TURBULA_Type T2C, manufactured by Willy & Bachofen (WAB)) to obtain a lithium mixture. This lithium mixture was heated to 950°C at a heating rate of 2.5°C / min in an air stream (oxygen: 21% by volume), and calcined by holding at this temperature for 5 hours, and then cooled to room temperature at a cooling rate of approximately 4°C / min.

[0109] (2) Crushing The obtained sintered material had some agglomeration and slight sintering, so it was crushed using a pin mill and then separated into "Li 1.15 Ni 0.33 Co 0.33 Mn 0.33 O2”, that is, a positive electrode active material for lithium ion secondary batteries, was obtained. The evaluation results of the oil absorption amount of the finally obtained positive electrode active material for a lithium ion secondary battery are shown in Table 1. EXAMPLES

[0110] In the seed particle generating step and the seed particle growing step, the same operations as in Example 1 were carried out except that the air introduction into the gas phase was set to 30 L / min, thereby obtaining a positive electrode active material for a lithium ion secondary battery according to Example 2. The evaluation results are shown in Table 1. EXAMPLES

[0111] In the seed particle generating step and the seed particle growing step, the same operations as in Example 1 were carried out except that the air introduction into the gas phase was set to 40 L / min, thereby obtaining a positive electrode active material for a lithium ion secondary battery according to Example 3. The evaluation results are shown in Table 1. EXAMPLES

[0112] The same operations as in Example 1 were carried out except that the crystallization temperature was set to 44° C. in the seed particle generating step, the seed particle growing step, and the particle growing step, to obtain a positive electrode active material for a lithium ion secondary battery according to Example 4. The evaluation results are shown in Table 1. EXAMPLES

[0113] The same operations as in Example 1 were carried out except that the crystallization temperature was 46° C. in the seed particle generating step, the seed particle growing step, and the particle growing step, to obtain a positive electrode active material for a lithium ion secondary battery according to Example 5. The evaluation results are shown in Table 1.

[0114] Comparative Example 1 In the seed particle generating step and the seed particle growing step, air was not introduced into the gas phase, and air bubbling into the reaction aqueous solution was performed from above the center of the stirring blade, except that the same operations as in Example 1 were performed to obtain a positive electrode active material for a lithium ion secondary battery according to Comparative Example 1. The evaluation results are shown in Table 1.

[0115] Comparative Example 2 A positive electrode active material for a lithium ion secondary battery according to Comparative Example 2 was obtained by carrying out the same operations as in Example 1, except that air was not introduced into the gas phase in the seed particle generating step and the seed particle growing step. The evaluation results are shown in Table 1.

[0116] Comparative Example 3 A positive electrode active material for a lithium ion secondary battery according to Comparative Example 3 was obtained by carrying out the same operations as in Example 4, except that air was not introduced into the gas phase in the seed particle generating step and the seed particle growing step. The evaluation results are shown in Table 1.

[0117] Comparative Example 4 A positive electrode active material for a lithium ion secondary battery according to Comparative Example 4 was obtained by carrying out the same operations as in Example 5, except that air was not introduced into the gas phase in the seed particle generating step and the seed particle growing step. The evaluation results are shown in Table 1.

[0118] [Table 1]

[0119] (Conclusion) It was confirmed that in the manufacturing methods of Examples 1 to 5, which are within the scope of the present invention, the oil absorption of the finally obtained lithium metal composite oxide (positive electrode active material) was improved in all cases in comparison with Comparative Examples 1 to 4. As in the comparative example, the oxidizing gas has been injected into the reaction aqueous solution during crystallization by bubbling the gas using an aeration tube 3. However, as in the examples of the present invention, it has been found that the inside of the composite hydroxide (precursor) particles becomes more sparse by simultaneously injecting the gas into the reaction aqueous solution in addition to bubbling the gas into the reaction aqueous solution, thereby making it possible to more effectively improve the oil absorption.

[0120] Furthermore, these results support the following: by carrying out the present invention, a composite hydroxide (precursor) having a controlled density of seed particles can be obtained, and a lithium metal composite oxide (positive electrode active material) produced using this composite hydroxide (precursor) has a high oil absorption capacity and can improve output characteristics. [Explanation of symbols]

[0121] 1 Reactor 2, 3 Gas introduction pipe 4 Stirring blade 5. Reaction solution 6 Mixer A Gas phase in the reactor

Claims

1. A reaction aqueous solution is formed by introducing and mixing a raw material aqueous solution containing at least nickel, cobalt, and manganese, an aqueous solution containing an ammonium ion donor, and an alkaline aqueous solution into a reaction vessel; A method for producing nickel-cobalt-manganese composite hydroxide particles by a crystallization reaction in the reaction aqueous solution in a reaction tank configured with a gas phase portion occupying an aqueous reaction solution other than the reaction aqueous solution, a seed particle generating step of adjusting the gas phase to an oxidizing atmosphere and controlling the pH in the oxidizing atmosphere to 12.0 to 14.0; a seed particle growing step in which the pH is controlled to 10.0 to 12.0 while maintaining the oxidizing atmosphere; A particle growth process in which the gas phase is switched from an oxidizing atmosphere to a non-oxidizing atmosphere, The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery is characterized in that, in the seed particle generation process and the seed particle growth process, an oxidizing gas is introduced synchronously into both the reaction aqueous solution and the gas phase portion.

2. The oxidizing atmosphere is an atmosphere in which the oxygen concentration in the gas phase in the reaction vessel exceeds 1% by volume, The non-oxidizing atmosphere is an atmosphere in which the oxygen concentration in the gas phase in the reaction tank is 1% by volume or less, 2. The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the oxidizing gas has an oxygen concentration of more than 1% by volume.

3. 3. The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery according to claim 1, wherein the oxidizing gas is introduced from a diffuser tube directly below the center of an agitating blade.

4. The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 3, wherein in the seed particle generation step and the seed particle growth step, when the oxidizing gas is introduced synchronously into both the aqueous reaction solution and the gas phase part in the reaction tank, the introduction flow rates of the oxidizing gas per minute are both 1 / 100 or more of the capacity of the reaction tank.

5. The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 4, characterized in that in the seed particle generation step and the seed particle growth step, a crystallization reaction is continued in a state in which a temperature in the reaction tank is maintained at 40°C or higher.

6. The precursor of the positive electrode active material for a lithium ion secondary battery is represented by the general formula: Ni X Co Y Mn Z M T (OH) 2+α 6. The method for producing a precursor of a positive electrode active material for a lithium ion secondary battery according to any one of claims 1 to 5, characterized in that the precursor has a composition represented by the formula: (X+Y+Z+T=1, 0.3≦X≦0.7, 0≦Y≦0.4, 0.1≦Z≦0.55, 0≦T≦0.1, 0≦α≦0.5, and M is one or more additive elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W).

7. General formula: Li 1+U Ni X Co Y Mn Z M T A method for producing a positive electrode active material for a lithium ion secondary battery, comprising a lithium nickel cobalt manganese composite oxide having a layered structure, a hexagonal crystal structure, and a hollow structure, the method comprising the steps of: O 2 + α (-0.05≦U≦0.50, X+Y+Z+T=1, 0.3≦X≦0.7, 0≦Y≦0.4, 0.1≦Z≦0.55, 0≦T≦0.1, 0≦α≦0.5, M is one or more additive elements selected from Mg, Ca, Al, Ti, V, Cr, Zr, Nb, Mo, Hf, Ta, and W), A mixing step of mixing a precursor of a positive electrode active material for a lithium ion secondary battery obtained by the production method according to any one of claims 1 to 6 with a lithium compound to form a lithium mixture; and a calcination step of calcining the lithium mixture formed in the mixing step at a temperature of 800°C to 1000°C in a furnace atmosphere having an oxygen concentration of 10 to 100% by volume, wherein the oil absorption of the lithium ion secondary battery positive electrode active material can be controlled to 37.5 ml / 100 g or more.

Citation Information

Patent Citations

  • Manganese composite hydroxide particle, positive pole active material for nonaqueous electrolyte secondary battery, and nonaqueous electrolyte secondary battery, and method for producing them

    JP2012246199A

  • Nickel compound hydroxide and method for producing the same, positive pole active substance for nonaqueous electrolyte secondary cell and method for producing the same, and nonaqueous electrolyte secondary cell

    JP2013147416A

  • Method for manufacturing nickel manganese composite hydroxide particles, and method for manufacturing positive electrode active material for nonaqueous electrolyte secondary battery

    JP2018022568A

  • Method for producing nickel-manganese composite hydroxide and method for producing positive electrode active material for nonaqueous electrolyte secondary battery

    JP2018024570A

  • Transition metal-containing composite hydroxide particle and production method of the same, and positive electrode active substance for non-aqueous electrolyte secondary cell and production method of the same