Diamines and polymers

A liquid crystal alignment film using specific diamines and polymers addresses the issue of voltage retention under harsh conditions, ensuring stable display performance in liquid crystal elements.

JP7575729B2Active Publication Date: 2024-10-30NISSAN CHEM CORP
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
JP2023123504
Authority / Receiving Office
JP · JP
Patent Type
Patents
Current Assignee / Owner
Priority Date
2018-06-19
Filing Date
2023-07-28
Publication Date
2024-10-30
Estimated Expiration
2039-06-19

AI Technical Summary

Technical Problem

Conventional liquid crystal alignment films struggle to maintain high voltage retention rates under high temperature and high humidity conditions, leading to decreased display contrast and flickering in liquid crystal display elements.

Method used

A liquid crystal alignment agent containing specific diamines and polymers, such as polyimides, is used to form a film that ensures high voltage retention even under harsh conditions.

Benefits of technology

The solution provides a liquid crystal alignment film and display element with improved voltage retention rates, maintaining performance in high temperature and high humidity environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 0007575729000001
    Figure 0007575729000001
  • Figure 0007575729000002
    Figure 0007575729000002
  • Figure 0007575729000003
    Figure 0007575729000003
Patent Text Reader

Abstract

To provide a liquid crystal alignment agent capable of sustaining a high voltage retention rate even at high temperature and high humidity.SOLUTION: This liquid crystal alignment agent comprises: a diamine component containing a diamine having a structure represented by formula (1) and a diamine (v) having at least one selected from the group consisting of structures represented by formulas (S1)-(S3); and at least one polymer (P) selected from the group consisting of polyimides and polyimide precursors obtained from a tetracarboxylic acid component.SELECTED DRAWING: None
Need to check novelty before this filing date? Find Prior Art

Description

[Technical field]

[0001] The present invention relates to a liquid crystal alignment agent, a liquid crystal alignment film, a liquid crystal display element using the same, and a method for manufacturing the same. In particular, the present invention relates to a liquid crystal alignment agent, a liquid crystal alignment film, and the same liquid crystal display element using the same, which are suitable for VA mode liquid crystal display elements in which liquid crystal molecules aligned perpendicular to a substrate are made to respond to an electric field, and a method for manufacturing the same. [Background technology]

[0002] Liquid crystal display elements are widely used in personal computers, mobile phones, smartphones, televisions, etc. In recent years, there are more and more opportunities for liquid crystal display elements to be used under high temperature and high humidity conditions, such as in car navigation systems installed in vehicles and in the display units of industrial equipment and measuring instruments installed outdoors.

[0003] This type of liquid crystal display element generally comprises a liquid crystal layer sandwiched between an element substrate and a color filter substrate, pixel electrodes and a common electrode that apply an electric field to the liquid crystal layer, a liquid crystal alignment film that controls the orientation of the liquid crystal molecules in the liquid crystal layer, and thin film transistors (TFTs) that switch the electrical signals supplied to the pixel electrodes.

[0004] In liquid crystal display elements, a liquid crystal layer sandwiched between pixel electrodes and a common electrode functions as a liquid crystal cell. If the voltage holding ratio (VHR) of a liquid crystal cell is low, it is difficult to apply a sufficient voltage to the liquid crystal molecules even when a voltage is applied. As a result, when used in high temperature and humidity conditions or for a long period of time, the display contrast decreases and flicker occurs in the display, making it difficult to see the display.

[0005] One of the driving methods for such liquid crystal display elements is a method in which liquid crystal molecules aligned vertically to the substrate are made to respond by an electric field (also called a vertical alignment (VA) method). In a vertical alignment type liquid crystal display element, a technology is known in which a photopolymerizable compound is added to the liquid crystal composition in advance, a vertical alignment film such as a polyimide film is used, and ultraviolet light is irradiated while a voltage is applied to the liquid crystal cell, thereby increasing the response speed of the liquid crystal (a PSA (Polymer Sustained Alignment) type element, see, for example, Patent Document 1 and Non-Patent Document 1). [Prior art documents] [Patent documents]

[0006] [Patent Document 1] JP 2003-307720 A [Non-patent literature]

[0007] [Non-Patent Document 1] K.Hanaoka,SID 04DIGEST, P1200-1202 Summary of the Invention [Problem to be solved by the invention]

[0008] However, in recent years, as liquid crystal display elements have become more sophisticated, the characteristics expected of liquid crystal alignment films have become more stringent. Therefore, it has been difficult for conventional techniques to meet the expectations for the characteristics of liquid crystal alignment films and liquid crystal display elements that accompany the recent improvements in performance.

[0009] The present invention has been made in view of the above, and aims to provide a liquid crystal alignment agent capable of obtaining a liquid crystal alignment film that can maintain a high voltage retention rate for a long period of time even under high temperature and high humidity conditions, the liquid crystal alignment film, a liquid crystal display element using the same, and a method for manufacturing the liquid crystal display element. [Means for solving the problem]

[0010] 1. A liquid crystal aligning agent comprising a diamine component containing a diamine (v) having at least one selected from the group consisting of a diamine having a structure of the following formula (1) (hereinafter also referred to as a specific diamine) and structures represented by the following formulae (S1) to (S3), and at least one polymer (P) selected from the group consisting of a polyimide precursor and a polyimide obtained from a tetracarboxylic acid component.

[0011] [ka]

[0012] In the formula, A is a single bond or a divalent organic group, and R1, R2, and R3 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms. Effect of the Invention

[0013] According to the liquid crystal aligning agent of the present invention, it is possible to provide a liquid crystal alignment film capable of ensuring a high voltage retention rate for a long period of time even under high temperature and high humidity conditions, and a liquid crystal display element using the liquid crystal alignment film. DETAILED DESCRIPTION OF THE PREFERRED EMBODIMENTS

[0014] The liquid crystal aligning agent of the present invention contains a diamine component containing a specific diamine having a structure of formula (1) and at least one diamine (v) having a side chain structure represented by formulas (S1) to (S3), and at least one polymer (P) selected from the group consisting of a polyimide precursor and a polyimide obtained from a tetracarboxylic acid component.

[0015] <Specific diamine> The specific diamine used in the liquid crystal aligning agent of the present invention has a structure represented by the following formula (1).

[0016] [ka]

[0017] In the formula, A is a single bond or a divalent organic group, and R1, R2, and R3 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms.

[0018] In the formula (1), A is a single bond or a divalent organic group. The structure of the divalent organic group is, for example, represented by the following formula (12).

[0019] [ka]

[0020] In the formula, B is a divalent linking group, and R5 and R6 are each independently a single bond or a divalent hydrocarbon group having 1 to 20 carbon atoms, preferably 1 to 10. Specific examples of B include -CH2-, -CHR7-, -CR7R8-, -CR7=CR8-, -C≡C-, -O-, -S-, -NR9-, -C(=O)O-, -OC(=O)-, and -C(=O)NR 10 -, -NR 10 C(=O)-, -NR 10 C(=O)NR 11 - but are not limited to these.

[0021] Above R7, R8, R9, R 10 , and R 11 are each independently a hydrogen atom or a monovalent hydrocarbon group having 1 to 20 carbon atoms. Examples of the monovalent hydrocarbon group include alkyl groups such as methyl, ethyl, propyl, butyl, t-butyl, hexyl, octyl, and decyl groups; cycloalkyl groups such as cyclopentyl and cyclohexyl groups; bicycloalkyl groups such as bicyclohexyl groups; alkenyl groups such as vinyl, 1-propenyl, 2-propenyl, isopropenyl, and hexenyl groups; aryl groups such as phenyl, xylyl, biphenyl, and naphthyl groups; and aralkyl groups such as benzyl, phenylethyl, and phenylcyclohexyl groups.

[0022] Some or all of the hydrogen atoms of these monovalent hydrocarbon groups may be substituted with halogen atoms, hydroxyl groups, thiol groups, carboxyl groups, thioester groups, amide groups, alkyl groups, cycloalkyl groups, bicycloalkyl groups, alkenyl groups, aryl groups, aralkyl groups, etc.

[0023] R7, R8, R9, R 10 , and R 11 When the alkyl group has a bulky structure such as an aromatic ring or an alicyclic structure, the solubility of the polymer may be reduced, and therefore the alkyl group is preferably a methyl group, an ethyl group, a propyl group, a butyl group, or a hydrogen atom, and more preferably a hydrogen atom.

[0024] In formula (1), R1, R2, and R3 are each independently a hydrogen atom or a monovalent organic group having 1 to 20 carbon atoms, preferably 1 to 10, and more preferably 1 to 6 carbon atoms. Examples of the monovalent organic group include a monovalent hydrocarbon group, a hydroxyl group, a thiol group, an ester group, a carboxyl group, a thioester group, an amide group, an organooxy group, an organosilyl group, an organothio group, and an acyl group. From the viewpoint of high resistance to high temperature and high humidity, the monovalent organic group is preferably a monovalent hydrocarbon group. Specific examples of the monovalent hydrocarbon group include the examples of the monovalent hydrocarbons described above, and some or all of the hydrogen atoms of these monovalent hydrocarbon groups can be selected from the group consisting of R7, R8, R9, R 10 In addition to the substitutable groups exemplified above, it may be substituted with a group such as a pyrrole group, an imidazole group, or a pyrazole group.

[0025] From the viewpoint of high resistance to high temperature and high humidity, R1 and R2 are preferably an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group, or a hydrogen atom, and more preferably a hydrogen atom.

[0026] From the viewpoint of high resistance to high temperature and humidity, R3 is preferably an alkyl group such as a methyl group, an ethyl group, a propyl group, or a butyl group, or a hydrogen atom, and more preferably a hydrogen atom.

[0027] As specific examples of the structure represented by formula (1), structures of the following formulae (H-1) to (H-6) are particularly preferred.

[0028] [ka]

[0029] n1, n2, n3, n4, n5, and n6 each independently represent an integer of 1 to 10.

[0030] The specific diamine is preferably a diamine represented by the following formula (M1) from the viewpoint of high resistance to high temperature and high humidity of the liquid crystal alignment film: The specific diamine may be used alone or in combination of two or more kinds.

[0031] [ka]

[0032] Z1 is a substituent having a structure represented by the above formula (1), and n is an integer of 1 to 4. Y1 is a (n+2)-valent organic group having 5 to 40 carbon atoms.

[0033] Examples of the (n+2)-valent organic group having 5 to 40 carbon atoms in Y1 include hydrocarbon groups such as chain hydrocarbon groups, alicyclic hydrocarbon groups, and aromatic hydrocarbon groups, groups in which a functional group such as -O-, -COO-, -OCO-, -CO-, -NHCO-, -S-, -NH-, a divalent heterocycle, or a divalent group containing a steroid skeleton is introduced between the carbon-carbon bonds in the hydrocarbon group, and (n+2)-valent heterocycles. Each of these groups may have a substituent such as a halogen atom (e.g., a fluorine atom, a chlorine atom, a bromine atom, an iodine atom, etc.), an alkoxy group, etc.

[0034] Here, the (n+2)-valent chain hydrocarbon group is R7, R8, R9, R 10 , and R 11Examples of the (n+2)-valent alicyclic hydrocarbon group include R7, R8, R9, and R10. 10 , and R 11 Examples of the (n+2)-valent aromatic hydrocarbon group include R7, R8, R9, and R10. 10 , and R 11 and groups in which (n+1) hydrogen atoms have been removed from the monovalent aryl group and groups in which (n+1) hydrogen atoms have been removed from the monovalent aralkyl group.

[0035] Examples of the divalent heterocycle include a divalent pyrrole ring, a divalent thiophene ring, a divalent furan ring, a 5-membered heterocycle such as a pyrrolidinylene group, and a 6-membered heterocycle such as a piperidinylene group, a piperazinylene group, a pyridinylene group, a pyridazinylene group, and a pyrimidinylene group.

[0036] The steroid skeleton has a skeleton represented by the following formula (st) in which three six-membered rings and one five-membered ring are bonded.

[0037] [ka]

[0038] From the viewpoint of providing a liquid crystal alignment film with high resistance to high temperature and high humidity, Y1 is preferably a (n+2)-valent organic group having 5 to 40 carbon atoms and an aromatic ring, and specifically is preferably a (n+2)-valent aromatic hydrocarbon group having 5 to 40 carbon atoms, a group in which a functional group such as -O-, -COO-, -OCO-, -CO-, -NHCO-, -S-, -NH-, a divalent heterocycle, or a divalent group containing a steroid skeleton is introduced between the carbon-carbon bonds in the hydrocarbon group, or a (n+2)-valent group having an aromatic heterocycle.

[0039] In the (n+2)-valent group having an aromatic heterocycle in Y1, the aromatic heterocycle is preferably a nitrogen-containing aromatic heterocycle having a nitrogen atom in the ring portion.Specific examples thereof include a pyridine ring, a pyrimidine ring, a pyrazine ring, a pyridazine ring, and a triazine ring, and more preferably a pyridine ring, a pyrimidine ring, or a triazine ring.

[0040] From the viewpoint of achieving a high voltage holding ratio, Y1 is preferably a (n+2)-valent aromatic hydrocarbon group having 5 to 40 carbon atoms, and is preferably a (n+2)-valent group having 5 to 40 carbon atoms and having a structure represented by the following formula (Ar1).

[0041] [ka]

[0042] A1 represents a single bond or a divalent organic group having an aromatic ring.

[0043] More preferred specific examples of the formula (M1) include the following formulae (M1-1) to (M1-13).

[0044] [ka]

[0045] Z1 is a structure represented by the above formula (1), c is an integer of 1 to 4, d and e are integers of 1 to 2, and n is an integer of 2 to 6.

[0046] From the viewpoint of improving vertical alignment, the specific diamine is preferably at least one selected from the group consisting of diamines represented by the following formulas (M-1) to (M-6).

[0047] [ka]

[0048] n1, n2, n3, n4, n5, and n6 each independently represent an integer of 1 to 10.

[0049] From the viewpoint of imparting liquid crystal alignment properties, the content of the specific diamine is preferably 5 to 95 mol %, more preferably 5 to 85 mol %, and still more preferably 5 to 70 mol %, based on the total diamine components.

[0050] <Diamine (v)> The diamine (v) of the present invention has at least one structure selected from the group consisting of structures represented by the following formulas (S1) to (S3).

[0051] [ka]

[0052] [ka]

[0053] [ka]

[0054] In formula (S1), X 1 and X 2 are each independently a single bond, -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -COO-, -OCO- or -((CH2) a1 -A1) m1 In this, each of the multiple a1's is independently an integer of 1 to 15, each of the multiple A1's is independently an oxygen atom or -COO-, and m1 is 1 to 2. From the viewpoint of availability of raw materials and ease of synthesis, each of X1 and X2 is independently a single bond, -(CH2) a -(a is an integer of 1 to 15), -O-, -CH2O- or -COO- is preferred, and a single bond, -(CH2) a-(a is an integer of 1 to 10), -O-, -CH2O- or -COO- is more preferred.

[0055] G1 and G2 each independently represent a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms or a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with an alkyl group having 1 to 3 carbon atoms, an alkoxy group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxy group having 1 to 3 carbon atoms, or a fluorine atom. m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 4.

[0056] R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. 1 Any hydrogen atom forming the group may be substituted with fluorine. Examples of the divalent aromatic group having 6 to 12 carbon atoms include phenylene, biphenylene, and naphthalene. Examples of the divalent alicyclic group having 3 to 8 carbon atoms include cyclopropylene and cyclohexylene.

[0057] Accordingly, preferred specific examples of the above formula (S1) include the following formulae (S1-x1) to (S1-x7), but are not limited thereto.

[0058] [ka]

[0059] In the formula, R 1 is an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms; p is -(CH2) a A1 represents an oxygen atom or -COO-* (wherein the bond marked with "*" is (CH2)), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -CHOCO-, -COO-, or -OCO-; A1 represents an oxygen atom or -COO-* (wherein the bond marked with "*" is (CH2) a2A2 is an oxygen atom or *-COO- (where the bond marked with "*" is (CH2) a2 wherein a1 and a3 each independently represent an integer of 0 or 1, a2 represents an integer of 1 to 10, and Cy represents a 1,4-cyclohexylene group or a 1,4-phenylene group.

[0060] In formula (S2), X 3 represents a single bond, -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -COO- or -OCO-. Among these, -CONH-, -NHCO-, -O-, -CHO-, -COO- or -OCO- is preferred from the viewpoint of liquid crystal alignment.

[0061] R 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen atom in the group may be substituted with fluorine. Among these, from the viewpoint of liquid crystal alignment, alkyl having 3 to 20 carbon atoms or alkoxyalkyl having 2 to 20 carbon atoms is preferred.

[0062] In formula (S3), X 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-.

[0063] R 3 represents a structure having a steroid skeleton, and a specific example thereof can be a structure having a skeleton represented by the above formula (st).

[0064] An example of the above formula (S3) is the following formula (S3-x), but is not limited thereto.

[0065] [ka]

[0066] X represents the above formula (X1) or (X2). Col represents at least one selected from the group consisting of the above formulas (Col1) to (Col4), and G represents the above formula (G1) or (G2). * represents a site for bonding to another group.

[0067] More preferred structures of formula (S3) include structures represented by the following formulae (S3-1) to (S3-6).

[0068] [ka]

[0069] In the formula, * indicates the bond position.

[0070] From the viewpoint of high polymerization reactivity, the diamine (v) is preferably a diamine represented by the following formula (v1): The diamine (v) can be used alone or in combination of two or more kinds.

[0071] [ka]

[0072] Y2 is a structure represented by the following formula (Ar2), and Z2 is a substituent having a group selected from the group consisting of the formulas (S-1) to (S-3), and n is an integer of 1 to 2.

[0073] [ka]

[0074] A2 represents a divalent organic group having a single bond or an aromatic group.

[0075] Examples of the divalent organic group having an aromatic group in Ar2 include a structure of the following formula (R).

[0076] [ka]

[0077] X is a single bond, -O-, -C(CH3)2-, -NH-, -CO-, -NHCO-, -COO-, -(CH2) m -, -SO2-, -O-(CH2) m -O-, -OC(CH3)2-, -CO-(CH2) m -, -NH-(CH2) m -, -SO2-(CH2) m -, -CONH-(CH2) m -, -CONH-(CH2) m -NHCO-, -COO-(CH2) m Examples of Q include, but are not limited to, aromatic hydrocarbon groups having 6 to 20 carbon atoms, such as a benzene ring and a naphthyl ring. m is an integer of 1 to 8.

[0078] More preferred specific examples of the diamine (v) include structures represented by the following formulae (1-S1) to (1-S3) or (2-S1) to (2-S3).

[0079] [ka]

[0080] In the above formula (1-S1) or (2-S1), X 1 , X 2 , G 1 , G 2 , R 1 In the above formula (1-S2) or (2-S2), X 3 and R 2 is the same as in the above formula (S2). In the above formula (1-S3) or (2-S3), X 4 and R 3 is the same as in the above formula (S3). X has the same meaning as X in the above formula (R).

[0081] Specific examples of the diamine (v) include diamines of the following formulas (V-1) to (V-13).

[0082] [ka] [ka]

[0083] In the formula, X v1 ~X v4 , X p1 ~X p8 Each of is independently -(CH2) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH3)-, -NH-, -O-, -CHO-, -CHOCO-, -COO-, or -OCO-; X v5 represents -O-, -CH2O-, -CH2OCO-, -COO-, or -OCO-; X V6 ~X V7 , X s1 ~X s4 Each independently represents -O-, -COO- or -OCO-. X a ~X f is a single bond, -O-, -NH-, -O-(CH2) m -O-, R v1 ~R v4 , R 1a ~R 1h each independently represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms. m represents an integer of 1 to 8.

[0084] From the viewpoint of imparting liquid crystal alignment properties, the content of the diamine (v) is preferably 5 to 95 mol %, more preferably 5 to 90 mol %, and still more preferably 5 to 80 mol %, based on the total diamine components.

[0085] <Other diamines: diamines other than those mentioned above> Other diamines that can be used as the diamine component in this embodiment include diamines that have the function of polymerizing or generating radicals upon irradiation with light, diamines described in paragraph

[0169] of International Publication WO2015 / 046374, diamines having a carboxyl group or a hydroxyl group described in paragraphs

[0171] to

[0172] , diamines having a nitrogen-containing heterocycle described in paragraphs

[0173] to

[0188] , diamines having a nitrogen-containing structure described in paragraph

[0050] of JP2016-218149A, and organosiloxane-containing diamines such as 1,3-bis(3-aminopropyl)-1,1,3,3-tetramethyldisiloxane and 1,3-bis(4-aminobutyl)-1,1,3,3-tetramethyldisiloxane. Among these, in the case of producing a PSA (Polymer Sustained Alignment) type liquid crystal display element, it is preferable to use a diamine having a function of polymerizing or generating radicals by light irradiation, from the viewpoint of increasing the response speed. Specific preferred examples of other diamines include m-phenylenediamine, p-phenylenediamine, 4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminobiphenyl, 3,3'-difluoro-4,4'-diaminobiphenyl, 4,4'-diaminodiphenylmethane, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylamine, N-methyl(4,4'-diaminodiphenyl)amine, 4,4'-diaminobenzophenone, 1,4-diaminonaphthalene, 2,6-diaminonaphthalene, 1,2-bis(4-aminofuran), 1,3-bis(4-aminophenyl)ethane, 1,3-bis(4-aminophenyl)propane, 1,4-bis(4-aminophenyl)butane, 1,4-bis(4-aminophenoxy)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(4-aminobenzyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 4,4'-[1,4-phenylenebis(methylene)]dianiline, 1,4-phenylenebis[(4-aminophenyl)methanone], 1,4-phenylenebis(4-aminobenzoate), bis (4-aminophenyl)terephthalate, bis(4-aminophenyl)isophthalate, N,N'-(1,4-phenylene)bis(4-aminobenzamide), N,N'-bis(4-aminophenyl)terephthalamide, N,N'-bis(4-aminophenyl)isophthalamide, 9,10-bis(4-aminophenyl)anthracene, 2,2'-bis[4-(4-aminophenoxy)phenyl]propane, 2,2'-bis(4-aminophenyl)propane, 1,3-bis(4-aminophenoxy)propane, 1,4-bis(4-aminophenoxy)buta 1,5-bis(4-aminophenoxy)pentane, 1,6-bis(4-aminophenoxy)hexane, 1,7-bis(4-aminophenoxy)heptane, 1,8-bis(4-aminophenoxy)octane, 1,9-bis(4-aminophenoxy)nonane, 1,10-(4-aminophenoxy)decane, bis(4-aminocyclohexyl)methane, 1,3-diaminopropane, 1,4-diaminobutane, 1,5-diaminopentane, 1,6-diaminohexane, 2,4-diaminobenzoic acid, 2,5-diaminobenzoic acid, 3,5-diaminobenzoic acid, 4,4'-Diaminobiphenyl-3-carboxylic acid, 4,4'-diaminodiphenylmethane-3-carboxylic acid, 4,4'-diaminodiphenylethane-3-carboxylic acid, 4,4'-diaminobiphenyl-3,3'-dicarboxylic acid, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 3,3'-diaminobiphenyl-4,4'-dicarboxylic acid, 3,3'-diaminobiphenyl-2,4'-dicarboxylic acid, 4,4'-diaminodiphenylmethane-3,3'-dicarboxylic acid, 4,4'-diaminodiphenylethane-3,3'-dicarboxylic acid, 4,4'-diaminodiphenylether-3 ,3'-dicarboxylic acid, 2,6-diaminopyridine, 3,4-diaminopyridine, 2,4-diaminopyrimidine, 3,6-diaminocarbazole, N-methyl-3,6-diaminocarbazole, 1,4-bis-(4-aminophenyl)-piperazine, 3,6-diaminoacridine, N-ethyl-3,6-diaminocarbazole, N-phenyl-3,6-diaminocarbazole, N,N'-bis(4-aminophenyl)-benzidine, N,N'-bis(4-aminophenyl)-N,N'-dimethylbenzidine, compounds represented by each of the following formulas (D-2-1) to (D-2-8),

[0086] [ka]

[0087] Further examples include diamine compounds in which the amino group is a secondary amino group.

[0088] Examples of diamines capable of being polymerized by irradiation with light include diamines in which structures represented by the following formulas [p1] to [p7] are bonded directly or via a linking group to an aromatic ring such as a benzene ring.

[0089] [ka]

[0090] Specific examples include diamines represented by the following formulas [Pa] and [Pb].

[0091] [ka]

[0092] The bonding positions of the two amino groups (-NH2) in the formula [Pa] and the formula [Pb] are not limited, but from the viewpoint of the reactivity of the diamine, the 2,4-positions, the 2,5-positions, or the 3,5-positions are preferable. Taking into consideration the ease of synthesizing the diamine, the 2,4-positions, or the 3,5-positions are more preferable.

[0093] In the formula [Pa], R 8 represents a single bond, -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH)-, -CON(CH)-, or -N(CH)CO-, and is preferably a single bond, -O-, -COO-, -NHCO-, or -CONH- from the viewpoint of ease of synthesis.

[0094] R 9 represents a single bond, an alkylene group having 1 to 20 carbon atoms which may be substituted with a fluorine atom, a divalent group selected from aromatic rings having 6 to 12 carbon atoms such as a benzene ring or a naphthalene ring, a divalent alicyclic group having 3 to 8 carbon atoms such as a cyclohexane ring, or a divalent cyclic group selected from heterocycles having 5 or more members such as pyrrole, imidazole, pyridine, pyrimidine, pyrazine, pyridazine, triazine, indole, quinoline, carbazole, thiazole, purine, tetrahydrofuran, and thiophene. Here, -CH2- of the alkylene group may be optionally substituted with -CF2- or -CH=CH-. From the viewpoint of ease of synthesis, a single bond or an alkylene group having 1 to 12 carbon atoms is preferred. k represents an integer of 0 to 4. R 10 represents a structure selected from the above formulas [p1] to [p7]. From the viewpoint of photoreactivity, [p1], [p2] and [p4] are preferred.

[0095] In the formula [Pb], Y1 and Y3 each independently represent -CH2-, -O-, -CONH-, -NHCO-, -COO-, -OCO-, -NH-, or -CO-. Y2 and Y5 each independently represent the same as R9 in the above [Pa]. Y4 represents a cinnamoyl group. Y6 represents a structure selected from the above formulas [p1] to [p7]. From the viewpoint of photoreactivity, [p1], [p2], and [p4] are preferred. m represents 0 or 1.

[0096] The diamine having the function of being polymerized by irradiation with light can be used alone or in combination of two or more kinds depending on the liquid crystal alignment properties, pretilt angle, voltage retention characteristics, stored charge characteristics, etc. when used as a liquid crystal alignment film, and the response speed of the liquid crystal when used as a liquid crystal display element.

[0097] The content of the diamine capable of being polymerized by irradiation with light is preferably 5 to 70 mol %, more preferably 5 to 60 mol %, and particularly preferably 5 to 50 mol %, based on the total diamine components. Examples of diamines having the function of generating radicals upon irradiation with light include diamines having a moiety on the side chain that has a radical generating structure that decomposes upon irradiation with ultraviolet light to generate radicals, such as the diamine represented by the following formula (R).

[0098] [ka]

[0099] In the above formula (R), Ar, R1, R2, T1, T2, S and Q have the following definitions. That is, Ar represents an aromatic hydrocarbon group selected from phenylene, naphthylene and biphenylene, which may be substituted with an organic group, and the hydrogen atom may be substituted with a halogen atom. R1 and R2 are each independently an alkyl group or an alkoxy group having 1 to 10 carbon atoms. T1 and T2 are each independently a single bond or a bonding group such as -O-, -COO-, -OCO-, -NHCO-, -CONH-, -NH-, -CHO-, -N(CH3)-, -CON(CH3)- or -N(CH3)CO-. S represents the R group in the above [Pa].9 Q represents a structure selected from the following formulas [q-1] to [q-4] (in the structural formula, R represents a hydrogen atom or an alkyl group having 1 to 4 carbon atoms, and R3 represents -CH2-, -NR-, -O-, or -S-).

[0100] [ka]

[0101] In the formula, * indicates the bond position.

[0102] In the above formula (R), from the viewpoint of efficient absorption of ultraviolet light, Ar to which carbonyl is bonded is preferably a structure with a long conjugation length such as naphthylene or biphenylene. In addition, Ar may be substituted with a substituent, and such a substituent is preferably an electron-donating organic group such as an alkyl group, a hydroxyl group, an alkoxy group, or an amino group. If the wavelength of ultraviolet light is in the range of 250 nm to 380 nm, a phenyl group can provide sufficient characteristics, so a phenyl group is most preferred.

[0103] Furthermore, R1 and R2 are each independently an alkyl group, an alkoxy group, a benzyl group, or a phenethyl group having 1 to 10 carbon atoms, and in the case of an alkyl group or an alkoxy group, R1 and R2 may form a ring.

[0104] From the viewpoint of ease of production of the specific polymer, Q is more preferably a hydroxyl group or an alkoxyl group.

[0105] The diaminobenzene in formula (R) may have any structure of o-phenylenediamine, m-phenylenediamine, or p-phenylenediamine, but is preferably m-phenylenediamine or p-phenylenediamine in terms of high reactivity with the tetracarboxylic acid component.

[0106] Specifically, structures represented by the following formulae [R-1] to [R-4] are most preferred in terms of ease of synthesis, versatility, properties, etc. In the formulae, n is an integer of 2 to 8.

[0107] [ka]

[0108] The content of the diamine having the function of generating radicals upon irradiation with light is preferably 5 to 70 mol % based on the total diamine component, more preferably 5 to 60 mol %, and particularly preferably 5 to 50 mol %, from the viewpoint of increasing the voltage holding ratio.

[0109] <Tetracarboxylic acid component> Examples of the tetracarboxylic acid component for obtaining the polymer (P) include tetracarboxylic acid, tetracarboxylic dianhydride, tetracarboxylic acid dihalide, tetracarboxylic acid dialkyl ester, and tetracarboxylic acid dialkyl ester dihalide, and in the present invention, these are also collectively referred to as tetracarboxylic acid component.

[0110] As the tetracarboxylic acid component, tetracarboxylic acid dianhydride or its derivatives, such as tetracarboxylic acid, tetracarboxylic acid dihalide, tetracarboxylic acid dialkyl ester, or tetracarboxylic acid dialkyl ester dihalide (collectively referred to as a first tetracarboxylic acid component) can also be used.

[0111] Specific examples of tetracarboxylic dianhydrides include 1,2,5,6-naphthalenetetracarboxylic acid, 1,4,5,8-naphthalenetetracarboxylic acid, 1,2,5,6-anthracenetetracarboxylic acid, 3,3',4,4'-biphenyltetracarboxylic acid, 2,3,3',4-biphenyltetracarboxylic acid, bis(3,4-dicarboxyphenyl)ether, 3,3',4,4'-benzophenonetetracarboxylic acid, bis(3,4-dicarboxyphenyl)sulfone, bis(3,4-dicarboxyphenyl)methane, 2,2-bis(3,4-dicarboxyphenyl)propane, 1,1,1,3,3,3-hexafluoro-2,2-bis(3,4-dicarboxyphenyl)propane, bis(3,4-dicarboxyphenyl)methane, ... Examples of the tetracarboxylic acid dianhydride include tetracarboxylic acid dianhydrides such as bis(3,4-dicarboxyphenyl)dimethylsilane, bis(3,4-dicarboxyphenyl)diphenylsilane, 2,3,4,5-pyridinetetracarboxylic acid, 2,6-bis(3,4-dicarboxyphenyl)pyridine, 3,3',4,4'-diphenylsulfonetetracarboxylic acid, 3,4,9,10-perylenetetracarboxylic acid, and 1,3-diphenyl-1,2,3,4-cyclobutanetetracarboxylic acid, tetracarboxylic acid dianhydrides represented by the following formula [4], and tetracarboxylic acid dihalide compounds, tetracarboxylic acid dialkyl ester compounds, and tetracarboxylic acid dialkyl ester dihalide compounds which are derivatives thereof. Among these, from the viewpoint of high resistance to high temperature and high humidity of the liquid crystal alignment film, it is preferable that the tetracarboxylic acid component contains tetracarboxylic acid dianhydride (T) represented by the following formula (4).

[0112] [ka]

[0113] X represents a structure selected from the following (x-1) to (x-11).

[0114] [ka]

[0115] In the formula, *1 is a bond bonded to one acid anhydride group, and *2 is a bond bonded to the other acid anhydride group.

[0116] In formula (x-1), R 1 ~R 4 represents a hydrogen atom, a methyl group, an ethyl group, a propyl group, a chlorine atom or a benzene ring, and may be the same or different. Preferred specific examples of (x-1) include structures of the following formula (x1-1) or (x1-2).

[0117] [ka]

[0118] In the formula, *1 is a bond bonded to one acid anhydride group, and *2 is a bond bonded to the other acid anhydride group.

[0119] In formula (x-7), Z 5 and Z 6 represents a hydrogen atom or a methyl group, and may be the same or different.

[0120] Among Z in formula (4), tetracarboxylic dianhydrides and tetracarboxylic acid derivatives thereof having a structure represented by formula (x-1), formula (x-3) to formula (x-7), or formula (x-11) are preferred from the viewpoints of ease of synthesis and ease of polymerization reactivity in producing a polymer.

[0121] The content of the tetracarboxylic dianhydride represented by formula (4) in the polymer of the present invention is preferably 10 mol % or more based on the total tetracarboxylic acid components in order to enhance the solubility of the polymer, more preferably 15 mol % or more, and more preferably 20 mol % or more.

[0122] The tetracarboxylic acid compound of the present invention can be used alone or in combination of two or more kinds depending on the solubility of the polymer of the present invention in a solvent, the coatability of the liquid crystal alignment agent, and properties such as the alignment of the liquid crystal when formed into a liquid crystal alignment film, the voltage holding ratio, and the stored charge.

[0123] The polyimide precursor used in the present invention may be a polyamic acid or a polyamic acid ester. All of the constituent units of the polyamic acid ester may have an amic acid ester structure, or may partially contain an amic acid structure.

[0124] <Polyamic acid> The polyamic acid used in the present invention can be obtained by reacting the diamine component with the tetracarboxylic dianhydride, but this method is not limited. In general, the polyamic acid can be obtained by mixing in a solvent to cause the reaction, and the solvent used in this case is not particularly limited as long as the generated polyimide precursor can be dissolved in the solvent. Examples of the solvent include N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, γ-butyrolactone, N,N-dimethylformamide, N,N-dimethylacetamide, dimethylsulfoxide, 1,3-dimethyl-imidazolidinone, etc. Furthermore, when the polyimide precursor has high solvent solubility, a solvent represented by methyl ethyl ketone, cyclohexanone, cyclopentanone, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monomethyl ether, ethylene glycol monoethyl ether, ethylene glycol monopropyl ether, propylene glycol monomethyl ether, propylene glycol monoethyl ether, propylene glycol monopropyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, or diethylene glycol monopropyl ether can be used.

[0125] <Polyamic acid ester> Specific methods for producing the polyamic acid ester of the present invention include the following three methods: (1) a method of polycondensing a tetracarboxylic acid in which the carboxylic acid group has been dialkyl-esterified with a primary or secondary diamine, (2) a method of polycondensing a tetracarboxylic acid dialkyl dihalide in which the carboxylic acid group has been dialkyl-esterified or dihalogenated with a primary or secondary diamine, and (3) a method of converting the carboxy group of a polyamic acid into an ester. The polyamic acid alkyl ester is preferably produced by the above method (2) or (3).

[0126] <Polyimide> The polyimide used in the present invention can be obtained by dehydrating and ring-closing the polyimide precursor. The polyimide referred to here does not necessarily have to have a ring-closing rate (also called imidization rate) of the amic acid group or amic acid ester group of 100%, and can be arbitrarily adjusted according to the application or purpose. Methods for imidizing the polyimide precursor include thermal imidization in which the solution of the polyimide precursor is heated as it is, and catalytic imidization in which a catalyst is added to the solution of the polyimide precursor.

[0127] <Liquid crystal alignment agent> The liquid crystal aligning agent of the present invention contains one or more of the above polymers (P). It may also contain other polymers other than the polymer (P). Examples of the polymer include polyamic acid, polyimide, polyamic acid ester, polyester, polyamide, polyurea, polyorganosiloxane, cellulose derivatives, polyacetal, polystyrene or its derivatives, poly(styrene-phenylmaleimide) derivatives, and poly(meth)acrylates. When the liquid crystal aligning agent of the present invention contains other polymers, the ratio of the specific polymer to the total polymer components is preferably 5% by mass or more, and may be, for example, 5 to 95% by mass.

[0128] The liquid crystal aligning agent generally takes the form of a coating liquid in order to form a uniform thin film. The liquid crystal aligning agent of the present invention is also preferably a coating liquid containing the above-mentioned polymer component and an organic solvent that dissolves the polymer component. In this case, the concentration of the polymer in the liquid crystal aligning agent can be appropriately changed depending on the thickness of the coating film to be formed. In order to form a uniform and defect-free coating film, the concentration is preferably 1% by mass or more, and in order to ensure the storage stability of the solution, the concentration is preferably 10% by mass or less. A particularly preferred concentration of the polymer is 2 to 8% by mass.

[0129] The organic solvent contained in the liquid crystal aligning agent is not particularly limited as long as the polymer component can be uniformly dissolved therein. Specific examples include N,N-dimethylformamide, N,N-dimethylacetamide, N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, dimethyl sulfoxide, γ-butyrolactone, γ-valerolactone, 1,3-dimethyl-2-imidazolidinone, methyl ethyl ketone, cyclohexanone, cyclopentanone, 3-methoxy-N,N-dimethylpropanamide, 3-butoxy-N,N-dimethylpropanamide, 4-hydroxy-4-methyl-2-pentanone, ethylene glycol monomethyl ether, butyl lactate, butyl acetate, methyl-3-methoxypropionate, ethyl-3-ethoxypropionate, ethylene glycol methyl ether, ethylene glycol ethyl ether, ethylene glycol-n-propyl ether, ethylene glycol-i-propyl ether, ethylene glycol monobutyl ether (butyl cellosolve), ethyl Examples of specific solvents include ethylene glycol dimethyl ether, ethylene glycol monobutyl ether acetate, propylene glycol monomethyl ether, propylene glycol monobutyl ether, propylene glycol diacetate, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol monomethyl ether, diethylene glycol monoethyl ether, diethylene glycol monomethyl ether acetate, diethylene glycol monoethyl ether acetate, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, ethylene carbonate, and propylene carbonate (hereinafter, these are also referred to as "specific solvents"). In addition, specific solvents include those described in paragraphs

[0105] to

[0107] of International Publication WO2014 / 171493.

[0130] The organic solvent used in the liquid crystal aligning agent of the present invention preferably contains at least one selected from the group consisting of the above-mentioned specific solvents from the viewpoint of improving printability, and more preferably contains at least one selected from the group consisting of N-methyl-2-pyrrolidone, N-ethyl-2-pyrrolidone, N-butyl-2-pyrrolidone, γ-butyrolactone, γ-valerolactone, cyclohexanone, cyclopentanone, ethylene carbonate, propylene carbonate, and 1,3-dimethyl-2-imidazoline (hereinafter referred to as "specific organic solvent (1)") and butyl cellosolve, ethylene It is preferable that the specific organic solvent (2) is at least one selected from the group consisting of glycol monobutyl ether acetate, propylene glycol monomethyl ether, propylene glycol monobutyl ether, diacetone alcohol, propylene carbonate, diethylene glycol diethyl ether, dipropylene glycol monomethyl ether, dipropylene glycol dimethyl ether, diisobutyl ketone, isoamyl propionate, isoamyl isobutyrate, diisopentyl ether, and ethyl 3-ethoxypropionate (hereinafter referred to as "specific organic solvent (2)").

[0131] The organic solvent used in the liquid crystal aligning agent of the present invention preferably contains the specific organic solvent (1) in an amount of 5 to 95% by weight, more preferably 10 to 95% by weight, based on the total amount of the organic solvent. The organic solvent used in the liquid crystal aligning agent of the present invention preferably contains the specific organic solvent (2) in an amount of 5 to 95% by weight, more preferably 5 to 90% by weight, based on the total amount of the organic solvent.

[0132] The liquid crystal alignment agent of the present invention may additionally contain components other than the polymer component and the organic solvent. Such additional components include a crosslinking compound that crosslinks the polymer (P), a compound (B) for adjusting the dielectric constant or electrical resistance of the liquid crystal alignment film, and an adhesion assistant for improving the adhesion between the liquid crystal alignment film and the substrate or between the liquid crystal alignment film and the sealant.

[0133] (Crosslinkable compound) As the crosslinkable compound, it is preferable to introduce at least one compound selected from the group consisting of crosslinkable compounds having at least one substituent selected from epoxy group, isocyanate group, oxetane group, cyclocarbonate group, blocked isocyanate group, hydroxyl group and alkoxyl group, and crosslinkable compounds having polymerizable unsaturated group. Note that, it is preferable that the crosslinkable compound has two or more of these substituents or polymerizable unsaturated bonds from the viewpoint of enhancing crosslinkability. Specific examples of the crosslinkable compound include compounds having an epoxy group or an isocyanate group described in paragraphs

[0169] to

[0190] of WO 2011 / 132751, compounds having an oxetane group, amino resins having a hydroxyl group, an alkoxyl group or a lower alkoxyalkyl group, benzene or phenolic compounds having a hydroxyl group or an alkoxyl group, compounds having a cyclocarbonate group described in paragraphs

[0103] to

[0112] of WO 2012 / 014898, compounds having a hydroxyalkylamide group described in WO 2015 / 072554, and compounds having a blocked isocyanate group described in WO 2015 / 141598.

[0134] More preferred specific examples of the crosslinkable compound include the compounds represented by the following formulas (CL-1) to (CL-11).

[0135] [ka]

[0136] The content of the above-mentioned crosslinkable compound is preferably 0.1 to 100 parts by weight based on 100 parts by weight of all the polymers of the present invention, and from the viewpoint of improving the alignment of the liquid crystal, it is more preferably 0.1 to 50 parts by weight, and even more preferably 1 to 50 parts by weight.

[0137] (Compound (B)) From the viewpoint of obtaining vertical alignment and high voltage retention characteristics, the compound (B) is preferably an amine compound having one amino group (-NH2) and a nitrogen-containing aromatic heterocycle in the molecule, and the amino group is bonded to an aliphatic hydrocarbon group or a non-aromatic cyclic hydrocarbon group. Specifically, the amine compound can be represented by the following formula (B-1).

[0138] [ka]

[0139] X1 is a divalent organic group having an aliphatic hydrocarbon group or a non-aromatic cyclic hydrocarbon group, and X2 is a nitrogen-containing aromatic heterocycle.

[0140] Examples of the aliphatic hydrocarbon group of X1 include a linear alkyl group having 1 to 20 carbon atoms, an alkyl group having a branched structure, and a hydrocarbon group having an unsaturated bond. Examples of the non-aromatic cyclic hydrocarbon group include a non-aromatic cyclic hydrocarbon group having 3 to 20 carbon atoms, such as a cyclopropane ring, a cyclobutane ring, a cyclopentane ring, and a cyclohexane ring. In addition, -CH2- in any aliphatic hydrocarbon group or non-aromatic cyclic hydrocarbon group not adjacent to an amino group may be replaced with -O-, -NH-, -CO-O-, -O-CO-, -CO-NH-, -NH-CO-, -CO-, -S-, -S(O)2-, -CF2-, -C(CF3)2-, -C(CH3)2-, -Si(CH3)2-, -O-Si(CH3)2-, -Si(CH3)2-O-, -O-Si(CH3)2-O-, a cyclic hydrocarbon group, and a nitrogen-containing heterocycle. In addition, a hydrogen atom bonded to any carbon atom may be replaced with a linear or branched alkyl group having 1 to 20 carbon atoms, a cyclic hydrocarbon group, a fluorine-containing alkyl group having 1 to 10 carbon atoms, a nitrogen-containing heterocycle, a fluorine atom, or a hydroxyl group.

[0141] Specific examples of the nitrogen-containing heterocycle include a pyrrole ring, an imidazole ring, a pyrazole ring, a pyridine ring, a pyrimidine ring, a pyridazine ring, a triazine ring, a triazole ring, a pyrazine ring, a benzimidazole ring, a benzimidazole ring, a quinoxaline ring, an azepine ring, a diazepine ring, a naphthyridine ring, a phenazine ring, and a phthalazine ring.

[0142] Preferred specific examples of the compound (B) include the compounds described in paragraphs

[0194] to

[0200] of International Publication No. 2011 / 132751. More preferred specific examples include structures represented by the following formulae (B-1) to (B-41).

[0143] [ka]

[0144] The content of the above compound (B) is preferably 0.1 to 50 parts by weight based on 100 parts by weight of all the polymers of the present invention, and from the viewpoint of improving the alignment of the liquid crystal, it is more preferably 0.1 to 40 parts by weight, and even more preferably 1 to 30 parts by weight.

[0145] <Liquid crystal alignment film> The liquid crystal alignment film of the present invention is obtained from the liquid crystal alignment agent. The liquid crystal alignment film obtained from the liquid crystal alignment agent of the present invention can be used as a horizontal alignment type or vertical alignment type liquid crystal alignment film, but is particularly suitable for vertical alignment type liquid crystal display elements such as VA mode or PSA mode, and can ensure a high voltage retention rate for a long period of time even under high temperature and high humidity. In particular, it is suitable as a liquid crystal alignment film used for PSA mode liquid crystal display elements in that it can suppress the decrease in voltage retention rate caused by impurities contained in the liquid crystal composition.

[0146] <Liquid crystal display element and its manufacturing method> The liquid crystal display element of the present invention includes the above-mentioned liquid crystal alignment film. The liquid crystal display element of the present invention can be produced, for example, by a method including the following steps (1) to (3) or steps (1) to (4).

[0147] (1) A process of applying a liquid crystal alignment agent onto a substrate The liquid crystal alignment agent of the present invention is applied to one side of a substrate on which a patterned transparent conductive film is provided by an appropriate application method such as a roll coater method, a spin coat method, a printing method, an inkjet method, etc. The substrate is not particularly limited as long as it is a highly transparent substrate, and plastic substrates such as acrylic substrates and polycarbonate substrates can be used in addition to glass substrates and silicon nitride substrates. In addition, in a reflective liquid crystal display element, an opaque material such as a silicon wafer can be used for only one substrate, and in this case, a light-reflecting material such as aluminum can be used for the electrode.

[0148] (2) The coating is baked After applying the liquid crystal alignment agent, preliminary heating (pre-baking) is preferably performed first for the purpose of preventing dripping of the applied alignment agent. The pre-baking temperature is preferably 30 to 200°C, more preferably 40 to 150°C, and particularly preferably 40 to 100°C. The pre-baking time is preferably 0.25 to 10 minutes, more preferably 0.5 to 5 minutes. After the solvent is completely removed, a heating (post-baking) step is preferably performed. The post-baking temperature is preferably 80 to 300°C, more preferably 120 to 250°C. The post-baking time is preferably 5 to 200 minutes, more preferably 10 to 100 minutes. The film thickness of the film thus formed is preferably 5 to 300 nm, more preferably 10 to 200 nm.

[0149] The coating film formed in the above step (1) can be used as a liquid crystal alignment film as it is, but the coating film may be subjected to an alignment ability imparting treatment, such as a rubbing treatment in which the coating film is rubbed in a certain direction with a roll wrapped with a cloth made of fibers such as nylon, rayon, or cotton, or a photoalignment treatment in which the coating film is irradiated with polarized or non-polarized radiation.

[0150] In the photo-alignment treatment, the radiation to be irradiated to the coating film may be, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm. When the radiation is polarized, it may be linearly polarized or partially polarized. When the radiation used is linearly polarized or partially polarized, the radiation may be applied from a direction perpendicular to the substrate surface, from an oblique direction, or a combination of these. When non-polarized radiation is applied, the radiation is applied in an oblique direction.

[0151] (3) Forming the liquid crystal layer (3-1) VA type LCD element Two substrates on which a liquid crystal alignment film is formed are prepared as described above, and liquid crystal is placed between the two substrates arranged opposite each other. Specifically, the following two methods can be mentioned. The first method is a conventionally known method. First, the two substrates are arranged opposite each other with a gap (cell gap) between them so that the liquid crystal alignment films face each other. Next, the peripheries of the two substrates are bonded together using a sealant, and a liquid crystal composition is injected and filled into the substrate surfaces and the cell gap partitioned by the sealant to come into contact with the film surface, and then the injection hole is sealed.

[0152] The second method is a method called ODF (One Drop Fill) method. For example, a UV-curable sealant is applied to a predetermined location on one of the two substrates on which a liquid crystal alignment film is formed, and a liquid crystal composition is dropped at a predetermined number of locations on the liquid crystal alignment film surface. Thereafter, the other substrate is bonded so that the liquid crystal alignment film faces the other substrate, and the liquid crystal composition is spread over the entire surface of the substrate and contacted with the film surface. Next, the entire surface of the substrate is irradiated with UV light to cure the sealant. In either method, it is preferable to further remove the flow alignment during liquid crystal filling by heating to a temperature at which the liquid crystal composition used has an isotropic phase and then slowly cooling to room temperature.

[0153] (3-2) Manufacturing of PSA type liquid crystal display elements The procedure is the same as in (3-1) above, except that a liquid crystal composition containing a polymerizable compound is injected or dropped.

[0154] (4) UV irradiation process The liquid crystal cell is irradiated with light while a voltage is applied between the conductive films of the pair of substrates obtained in (3-2) above. The voltage applied here can be, for example, 5 to 50 V DC or AC. The light to be irradiated can be, for example, ultraviolet light and visible light containing light with a wavelength of 150 to 800 nm, but ultraviolet light containing light with a wavelength of 300 to 400 nm is preferred. The light source for the irradiation light can be, for example, a low-pressure mercury lamp, a high-pressure mercury lamp, a deuterium lamp, a metal halide lamp, an argon resonance lamp, a xenon lamp, an excimer laser, or the like. The light irradiation dose is preferably 1,000 to 200,000 J / m 2 and more preferably 1,000 to 100,000 J / m 2 It is.

[0155] When a coating film is formed on a substrate using a liquid crystal alignment agent containing a compound (polymer or additive) having a photopolymerizable group, a method of manufacturing a liquid crystal display element may be adopted in which, after the same procedure as in (3-1) above, a step of irradiating the liquid crystal cell with light while applying a voltage between the conductive films of a pair of substrates is carried out. With this method, the advantages of the PSA mode can be realized with a small amount of light irradiation.

[0156] A liquid crystal display element can be obtained by attaching a polarizing plate to the outer surface of the liquid crystal cell. Examples of the polarizing plate to be attached to the outer surface of the liquid crystal cell include a polarizing film called an "H film" made by absorbing iodine while stretching and aligning polyvinyl alcohol, sandwiched between cellulose acetate protective films, and a polarizing plate made of the H film itself.

[0157] The liquid crystal display element of the present invention can be effectively applied to various devices, and can be used in various display devices such as watches, portable games, word processors, notebook computers, car navigation systems, camcorders, PDAs, digital cameras, mobile phones, smartphones, various monitors, liquid crystal televisions, and information displays. EXAMPLES

[0158] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to these examples. The compounds used are as follows. (Diamine component) Compounds represented by the following formulas [DA-1] to [DA-11] DA-1: A compound represented by the formula [DA-1] DA-2: A compound represented by the formula [DA-2] DA-3: A compound represented by the formula [DA-3] DA-4: Compound represented by the formula [DA-4] DA-5: A compound represented by the formula [DA-5] DA-6: Compound represented by the formula [DA-6] DA-7: A compound represented by the formula [DA-7] (specific diamine) DA-8: A compound represented by the formula [DA-8] (specific diamine) DA-9: A compound represented by the formula [DA-9] (specific diamine) DA-10: A compound represented by the formula [DA-10] (specific diamine) DA-11: A compound represented by the formula [DA-11] (specific diamine)

[0159] [ka]

[0160] (New diamine component) Synthesis examples of the compounds [W-A1] to [W-A3] represented by the following formulae [DA-9] to [DA-11] will be described in detail. The products described in the following Synthesis Examples 1 to 7 are 1 The product was identified by H-NMR analysis (analysis conditions are as follows). Equipment: Varian NMR System 400 NB (400 MHz) Measurement solvent: CDCl 3、 DMSO-d6 Reference material: Tetramethylsilane (TMS) (δ0.0 ppm for 1 H) In the following, the abbreviations have the following meanings: THF: tetrahydrofuran DMAc: N,N-dimethylacetamide

[0161] [ka]

[0162] <<Compound synthesis example 1: Synthesis of DA-9>>

[0163] [ka]

[0164] <Synthesis of compound [1]> 2-Aminoethanol (40.0 g, 655 mmol) was added to tetrahydrofuran (160 g) and stirred under ice-cooled conditions in a nitrogen atmosphere. Di-tert-butyl dicarbonate (150 g, 687 mmol) dissolved in tetrahydrofuran (150 g) was added dropwise over 1 hour while paying attention to heat generation, and when heat generation ceased, the mixture was stirred at room temperature for 2 hours. After stopping the stirring and leaving it for 16 hours, the generated white precipitate was separated by filtration, and the filtrate was concentrated and dried to obtain a crude product of compound [1] (yield: 117 g). The obtained compound was used as it was in the next step. 1 H-NMR(400MHz) in CDCl3:5.04ppm(br,1H), 3.72-3.68ppm(m,2H), 3.31-3.27ppm(m,2H), 2.78ppm(br,1H), 1.45ppm(s,9H)

[0165] <Synthesis of compound [2]> In tetrahydrofuran (190 g), crude compound [1] (60.4 g) and triethylamine (42.5 g, 420 mmol) were charged. 2,4-Dinitrofluorobenzene (60.4 g, 325 mmol) dissolved in tetrahydrofuran (59.2 g) was added dropwise under a nitrogen atmosphere at 50 °C, and the mixture was stirred for 25 hours. Then, crude compound [1] (26.0 g) and triethylamine (16.3 g, 161 mmol) dissolved in tetrahydrofuran (30.0 g) were additionally added and reacted for 3 hours. Thereafter, crude compound [1] (30.0 g) dissolved in tetrahydrofuran (30.0 g) was further added and reacted for 16 hours to complete the reaction. Ethyl acetate (208 g) was added to the reaction solution, and it was separated and washed with pure water (153 g × 3 times). After recovering the organic phase, it was concentrated under reduced pressure. The precipitated crystals were slurried and washed with methanol (180 g), filtered, and the obtained crystals were cake-washed with methanol (60.0 g × 3 times) and dried to obtain compound [2] (yield: 52.8 g, 161 mmol). 1 1H-NMR (400 MHz) in CDCl3: 8.80 ppm (d, 1H, J = 2.8 Hz), 8.45 ppm (dd, 1H, J = 9.2 Hz, 2.8 Hz), 7.23 ppm (d, 1H, J = 9.2 Hz), 5.06 ppm (br, 1H), 4.31 ppm (t, 2H, J = 5.0 Hz), 3.63 ppm (dd, 2H, J = 11.2 Hz, 4.8 Hz), 1.45 ppm (s, 9H)

[0166] <Synthesis of DA-9> In tetrahydrofuran (264 g) and methanol (106 g), compound [2] (52.8 g, 162 mmol) and 5% palladium carbon (hydrous product) (4.23 g) were charged and stirred under a hydrogen atmosphere at room temperature for about 5 days. After completion of the reaction, palladium carbon was removed by filtration and concentrated under reduced pressure. Ethyl acetate (398 g) was added to the concentrated crude product to dissolve it, hexane (367 g) was added to precipitate crystals, and after stirring at room temperature, it was filtered. The obtained crystals were cake-washed with hexane (106 g × 2 times) and dried to obtain DA-9 (yield: 37.3 g, 140 mmol). 1H-NMR(400MHz) in CDCl3:6.60ppm(d,1H,J=8.4Hz), 6.14ppm(d,1H,J=2.8Hz), 6.05ppm(dd,1H,J=8.4Hz,2.8Hz), 5.07ppm(br,1H), 3.97ppm(t,2H,J=5.0Hz), 3.76ppm(br,2H), 3.49ppm(m,2H), 3.38ppm(br,2H), 1.44ppm(s,9H)

[0167] <<Compound synthesis example 2: Synthesis of DA-10>>

[0168] [ka]

[0169] <Synthesis of compound [3]> 2-Chloroethylamine hydrochloride (51.9g, 447mmol) and triethylamine (49.6g, 490mmol) were added to methanol (204g) and stirred under ice-cooled conditions in a nitrogen atmosphere. Di-tert-butyl dicarbonate (117g, 536mmol) dissolved in methanol (102g) was added dropwise over 1 hour while paying attention to heat generation, and when heat generation ceased, the mixture was stirred at room temperature for 15 hours. After the reaction was completed, 4-dimethylaminopyridine (0.543g, 4.44mmol) was added and stirred at 60°C for 1 hour. Excess di-tert-butyl dicarbonate was reacted with methanol to remove it, and the reaction solution was concentrated under reduced pressure. Ethyl acetate (300g) was added to the concentrated crude product, which was washed with pure water (300g x 3 times), and the organic phase was concentrated under reduced pressure and dried to obtain crude compound [3] (yield: 77.8g). The obtained compound [3] was used as it was in the next step. 1 H-NMR(400MHz) in DMSO-d6:7.08ppm(br,1H), 3.57-3.54ppm(m,2H), 3.25-3.20ppm(m,2H), 1.38ppm(s,9H)

[0170] <Synthesis of compound [4]> In N,N-dimethylacetamide (210 g), 2-amino-5-nitrophenol (54.8 g, 356 mmol), potassium carbonate (54.9 g, 397 mmol), and potassium iodide (5.90 g, 35.5 mmol) were charged and the temperature was raised to 100 °C. Then, a crude product of compound [3] (70.0 g) dissolved in N,N-dimethylacetamide (70.0 g) was added dropwise and stirred for 4 hours. Thereafter, potassium carbonate (6.85 g, 49.6 mmol) and a crude product of compound [3] (7.78 g) were further added and stirred for 17 hours to complete the reaction. Ethyl acetate (280 g) and pure water (280 g) were added to the reaction solution, and the precipitated crystals were separated by filtration to obtain a crude product of compound [4]. Further, the filtrate was concentrated, ethyl acetate (90.0 g) and methanol (340 g) were added and stirred to precipitate crystals, which were then filtered. The obtained crystals were cake-washed with methanol (140 g) to obtain a crude product of compound [4]. The crude products obtained in the above two ways were combined, crystallized with ethyl acetate (480 g) and toluene (480 g), filtered, and the obtained crystals were dried to obtain compound [4] (yield: 63.3 g, 213 mmol). 1 H-NMR (400 MHz) in DMSO-d6: 7.74 ppm (dd, 1H, J = 8.8 Hz, 2.4 Hz), 7.53 ppm (d, 1H, J = 2.4 Hz), 6.64 ppm (d, 1H, J = 8.8 Hz), 7.20 ppm (t, 1H, J = 6.0 Hz), 4.00 - 3.97 ppm (m, 2H), 6.54 ppm (br, 2H), 3.39 - 3.34 ppm (m, 2H), 1.93 ppm (s, 9H)

[0171] <Synthesis of DA-10> Compound [4] (60.0g, 202mmol) and 5% palladium carbon (wet product) (2.40g) were added to tetrahydrofuran (240g) and methanol (60.0g) and stirred at room temperature under a hydrogen atmosphere for 30 hours. After the reaction was completed, the palladium carbon was removed by filtration, and the filtrate was concentrated under reduced pressure to obtain a crude red-purple liquid. Ethyl acetate (120g) and hexane (360g) were added to the crude product and stirred to precipitate crystals, which were then filtered and dried to obtain DA-10 (yield: 16.5g, 61.7mmol). 1 H-NMR(400MHz) in DMSO-d6:7.11ppm(t,1H,J=6.0Hz), 6.35ppm(d,1H,J=8.0Hz), 6.13ppm(d,1H,J=2.4Hz), 5.97ppm(dd,1H,J=8.0Hz,2.0Hz), 4.24(br,2H), 4.00(br,2H), 3.76ppm(t,2H,J=5.2Hz), 3.35-3.27ppm(m,2H), 1.39ppm(s,9H)

[0172] <<Compound Synthesis Example 3: Synthesis of DA-11>>

[0173] [ka]

[0174] <Synthesis of compound [5]> 6-Amino-1-hexanol (66.0g, 563mmol) was added to toluene (325g), and thionyl chloride (79.8g, 671mmol) dissolved in toluene (90.0g) was added under ice cooling, and the mixture was heated and stirred at 70°C for 5 hours. After the reaction was completed, the reaction solution was concentrated under reduced pressure to obtain crude compound [5] (yield: 98.9g). The obtained compound was used as it was in the next step. 1 H-NMR(400MHz) in CDCl3:5.58ppm(br,3H), 3.56-3.53ppm(m,2H), 3.01-2.98ppm(m,2H), 1.83-1.76ppm(m,4H), 1.53-1.40ppm(m,4H)

[0175] <Synthesis of compound [6]> Crude compound [5] (98.9 g) and triethylamine (64.0 g, 632 mmol) were added to methanol (310 g) and stirred under ice-cooled conditions in a nitrogen atmosphere. Di-tert-butyl dicarbonate (151 g, 692 mmol) dissolved in methanol (60.7 g) was added dropwise over 1 hour while paying attention to heat generation, and when heat generation ceased, the mixture was stirred at room temperature for 24 hours. After the reaction was completed, 4-dimethylaminopyridine (0.700 g, 5.73 mmol) was added and the mixture was stirred at 60°C for 1 hour to remove excess di-tert-butyl dicarbonate by reacting it with methanol. Ethyl acetate (328 g) was added to the reaction solution, which was then washed with pure water (300 g x 2 times), and the organic phase was concentrated under reduced pressure and dried to obtain crude compound [6]. Ethyl acetate (320 g) was added to the separated aqueous phase, and the mixture was washed with pure water (300 g x 2 times). The organic phase was concentrated under reduced pressure and dried to obtain crude compound [6]. The compound obtained by combining the crude compound [6] from the above two methods (yield: 129 g) was used as it was in the next step. 1 H-NMR(400MHz) in CDCl3:4.54ppm(br,1H), 3.55-3.52ppm(m,2H), 3.16-3.09ppm(m,2H), 1.81-1.74ppm(m,2H), 1.53-1.37ppm(m,13H), 1.37-1.30ppm(m,2H)

[0176] <Synthesis of compound [7]> In N,N-dimethylacetamide (270 g), 2-amino-5-nitrophenol (67.2 g, 436 mmol), potassium carbonate (72.3 g, 523 mmol), and potassium iodide (7.26 g, 43.7 mmol) were charged. After heating to 100 °C, compound [6] (crude, 90.7 g) dissolved in N,N-dimethylacetamide (90.0 g) was added dropwise, followed by stirring for 4 hours. Further, potassium carbonate (25.9 g, 187 mmol) and compound [6] (crude, 22.5 g) were added, and the reaction was stirred for 18 hours to completion. Ethyl acetate (450 g) was added to the reaction solution, and it was washed by liquid separation with pure water (300 g × 6 times). The organic phase was concentrated under reduced pressure. The obtained concentrated crude product was purified by silica gel column chromatography (developing solvent: ethyl acetate / hexane = 1 / 2 mixed solvent), concentrated under reduced pressure, and dried to obtain compound [7] (yield: 146 g, 413 mmol). 1 H-NMR (400 MHz) in DMSO-d6: 7.73 ppm (dd, 1H, J = 8.8 Hz, 2.4 Hz), 7.55 - 7.54 ppm (d, 1H, J = 2.4 Hz), 6.79 ppm (t, 1H, J = 6.0 Hz), 6.67 ppm (d, 1H, J = 8.8 Hz), 6.37 ppm (br, 2H), 2.94 - 2.90 ppm (m, 2H), 1.77 - 1.73 ppm (m, 2H), 1.47 - 1.40 ppm (m, 6H), 1.37 ppm (s, 9H), 1.36 - 1.28 ppm (m, 2H)

[0177] <Synthesis of DA-11> Compound [7] (82.0 g, 232 mmol), 10 wt% ammonium chloride aqueous solution (372 g), and reduced iron (powder) (64.8 g, 1.16 mol) were added to ethyl acetate (658 g) and stirred at 70 ° C for 24 hours. After that, 10 wt% ammonium chloride aqueous solution (248 g) and reduced iron (powder) (51.8 g, 927 mmol) were added and stirred for 3 days to complete the reaction. After the reaction was completed, the iron powder was removed by filtration, and the filtrate to which ethyl acetate (200 g) was added was washed with saturated sodium bicarbonate aqueous solution (328 g x 3 times), and the organic phase was concentrated under reduced pressure. Tetrahydrofuran (174 g) and special Shirasagi activated carbon (4.10 g) were added to the obtained concentrated crude product and stirred at 60 ° C for 2 hours, the activated carbon was removed by filtration, and the filtrate was concentrated under reduced pressure. The resulting concentrated crude product was purified by silica gel column chromatography (developing solvent: ethyl acetate), concentrated under reduced pressure, and dried to obtain DA-11 (yield: 39.2 g, 121 mmol). 1 H-NMR(400MHz) in DMSO-d6:6.79ppm(t,1H,J=6.0Hz), 6.38ppm(d,1H,J=8.0Hz), 6.17ppm(d,1H,J=2.4Hz), 5.97ppm(dd,1H,J=8.4Hz,2.0Hz), 4.24(br,2H), 3.82(br,2H), 3.82(m,2H), 2.93-2.88ppm(m,2H), 1.70-1.67ppm(m,2H), 1.42-1.37ppm(m,4H), 1.37ppm(s,9H), 1.32-1.27ppm(m,2H)

[0178] (Tetracarboxylic acid component) Compounds represented by the following formulas [D1] to [D2] D1: 1,2,3,4-cyclobutanetetracarboxylic dianhydride D2: Bicyclo[3,3,0]octane-2,4,6,8-tetracarboxylic dianhydride D3: 2,3,5-tricarboxycyclopentylacetic dianhydride

[0179] [ka]

[0180] (solvent) NMP: N-methyl-2-pyrrolidone BCS: Ethylene glycol monobutyl ether

[0181] <Measurement of molecular weight of polyimide> The molecular weight of the polyimide in the synthesis examples was measured as follows using a room temperature gel permeation chromatography (GPC) apparatus (SSC-7200) manufactured by Senshu Scientific Co., Ltd. and columns (KD-803, KD-805) manufactured by Shodex Co., Ltd. Column temperature: 50℃ Eluent: N,N'-dimethylformamide (additives: lithium bromide hydrate (LiBr·H2O) 30mmol / L, phosphoric acid anhydrous crystal (o-phosphoric acid) 30mmol / L, tetrahydrofuran (THF) 10ml / L) Flow rate: 1.0ml / min Standard samples for creating calibration curves: TSK standard polyethylene oxide (molecular weights: approximately 9,000,000, 150,000, 100,000, and 30,000) manufactured by Tosoh Corporation, and polyethylene glycol (molecular weights: approximately 12,000, 4,000, and 1,000) manufactured by Polymer Laboratory.

[0182] <Measurement of imidization rate> The imidization rate of the polyimide in the synthesis examples was measured as follows: 20 mg of polyimide powder was placed in an NMR sample tube (Kusano Scientific NMR Sampling Tube Standard φ5), 0.53 ml of deuterated dimethyl sulfoxide (DMSO-d6, 0.05% TMS mixture) was added, and the mixture was sonicated to completely dissolve it.

[0183] This solution was subjected to 500 MHz proton NMR measurement using an NMR measuring instrument (JNW-ECA500) manufactured by JEOL Datum Co., Ltd. The imidization rate was calculated by the following formula using a proton derived from a structure that does not change before and after imidization as a reference proton and the peak integrated value of this proton and the proton peak integrated value derived from the NH group of the amic acid that appears in the vicinity of 9.5 to 10.0 ppm.

[0184] Imidization rate (%) = (1-α·x / y) × 100

[0185] <Synthesis of polyimide polymer> <Synthesis Example 1> Tetracarboxylic dianhydride D2 (5.00 g, molar ratio to all diamines: 0.5 mol), diamine components DA-1 (4.57 g, molar ratio to all diamines: 0.3 mol), and DA-7 (6.64 g, molar ratio to all diamines: 0.7 mol) were mixed in a solvent NMP (N1 in Table 1: 64.86 g) and reacted at 60°C for 3 hours, after which D1 (3.84 g, molar ratio to all diamines: 0.49 mol) and NMP (N2 in Table 1: 15.37 g) were added and reacted at 40°C for 6 hours to obtain a polyamic acid solution.

[0186] NMP (41.54 g) was added to this polyamic acid solution (20.0 g) and diluted to 6.5% by mass, and then acetic anhydride (4.06 g) and pyridine (1.26 g) were added as imidization catalysts and reacted at 80° C. for 3 hours. This reaction solution was poured into methanol (233.98 g), and the resulting precipitate was filtered off. This precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain polyimide powder (A) of Synthesis Example 1. The imidization rate of this polyimide was 83%, the number average molecular weight was 11,600, and the weight average molecular weight was 32,200.

[0187] <Synthesis Examples 2 to 7> Following the procedure of Synthesis Example 1, the materials and ratios were changed as shown in Tables 1 and 2 to obtain polyimide powders (B to G) of Synthesis Examples 2 to 7.

[0188] <Synthesis Example 8> Tetracarboxylic dianhydride D3 (7.63 g, molar ratio to all diamines: 0.99 mol), diamine components DA-2 (5.21 g, molar ratio to all diamines: 0.2 mol), DA-3 (2.84 g, molar ratio to all diamines: 0.25 mol), and DA-7 (4.49 g, molar ratio to all diamines: 0.55 mol) were mixed in a solvent NMP (N1 in Table 1: 80.70 g) and reacted at 60°C for 6 hours to obtain a polyamic acid solution.

[0189] NMP (41.54 g) was added to this polyamic acid solution (20.0 g) and diluted to 6.5 mass %, and then acetic anhydride (3.48 g) and pyridine (1.08 g) were added as imidization catalysts and reacted at 100 ° C for 3 hours. This reaction solution was poured into methanol (231.35 g), and the resulting precipitate was filtered off. This precipitate was washed with methanol and dried under reduced pressure at 60 ° C to obtain polyimide powder (H) of Synthesis Example 8. The imidization rate of this polyimide was 75%, the number average molecular weight was 11,100, and the weight average molecular weight was 40,600.

[0190] <Synthesis Example 9> Polyimide powder (I) of Synthesis Example 9 was obtained by following the procedure of Synthesis Example 8, but changing the materials and ratios as shown in Tables 1 and 2.

[0191] <Comparative Synthesis Example 1> Tetracarboxylic dianhydride D2 (6.13 g, molar ratio to all diamines: 0.5 mol), diamine components DA-1 (5.59 g, molar ratio to all diamines: 0.3 mol), and DA-5 (3.71 g, molar ratio to all diamines: 0.7 mol) were mixed in 61.73 g of NMP and reacted at 60°C for 3 hours, after which D1 (4.71 g, molar ratio to all diamines: 0.49 mol) and 18.83 g of NMP were added and reacted at 40°C for 6 hours to obtain a polyamic acid solution.

[0192] 41.54g of NMP was added to 20.0g of this polyamic acid solution, and the solution was diluted to 6.5% by mass. Then, acetic anhydride (4.94g) and pyridine (1.53g) were added as imidization catalysts, and the mixture was reacted at 50°C for 3 hours. The reaction solution was poured into methanol (238.05g), and the resulting precipitate was filtered off. The precipitate was washed with methanol and dried under reduced pressure at 60°C to obtain polyimide powder (J) of Comparative Synthesis Example 1. The imidization rate of this polyimide was 54%, the number average molecular weight was 7,700, and the weight average molecular weight was 17,900.

[0193] <Comparative Synthesis Example 2> Tetracarboxylic dianhydride D2 (6.01 g, molar ratio to all diamines: 0.5 mol), diamine components DA-1 (5.48 g, molar ratio to all diamines: 0.3 mol), DA-4 (2.39 g, molar ratio to all diamines: 0.2 mol), and DA-5 (2.60 g, molar ratio to all diamines: 0.5 mol) were mixed in NMP (65.90 g) and reacted at 60°C for 3 hours, after which D1 (4.47 g, molar ratio to all diamines: 0.475 mol) and NMP (17.88 g) were added and reacted at 40°C for 6 hours to obtain a polyamic acid solution.

[0194] NMP (41.54 g) was added to this polyamic acid solution (20.0 g) and diluted to 6.5% by mass, and then acetic anhydride (4.63 g) and pyridine (1.43 g) were added as imidization catalysts and reacted at 80° C. for 3 hours. This reaction solution was poured into methanol (236.60 g) and the resulting precipitate was filtered off. This precipitate was washed with methanol and dried under reduced pressure at 60° C. to obtain polyimide powder (K) of Comparative Synthesis Example 1. The imidization rate of this polyimide was 73%, the number average molecular weight was 11,100, and the weight average molecular weight was 29,100.

[0195] [Table 1]

[0196] [Table 2]

[0197] <Example 1> NMP (54.0 g) was added to the polyimide powder (A) (6.0 g) obtained in Synthesis Example 1, and the mixture was stirred at 70° C. for 40 hours to dissolve. BCS (40.0 g) was added to this solution, and the mixture was stirred for 5 hours to obtain a liquid crystal alignment agent [1] of Example 1. No abnormalities such as turbidity or precipitation were observed in this liquid crystal alignment agent, and it was confirmed that the resin component was uniformly dissolved.

[0198] <Examples 2 to 5> Following the procedure of Example 1, the polyimide material was changed as shown in Table 3 to obtain alignment treatment agents [2] to [5] of Examples 2 to 5. No abnormalities such as turbidity or precipitation were observed in these liquid crystal alignment agents, and it was confirmed that the resin components were uniformly dissolved.

[0199] <Comparative Examples 1 and 2> Following the method of Example 1, the polyimide material was changed as shown in Table 3 to obtain the alignment treatment agent [6] of Comparative Example 1 and the alignment treatment agent [7] of Comparative Example 2. No abnormalities such as turbidity or precipitation were observed in these liquid crystal alignment agents, and it was confirmed that the resin components were uniformly dissolved.

[0200] <Preparation of liquid crystal cell> The liquid crystal alignment agents of Examples 1 to 5 and Comparative Example 1 obtained above were spin-coated on the ITO surface of a 3×4 cm ITO-coated glass substrate, baked on a hot plate at 70° C. for 1 minute and 30 seconds, and then baked in an infrared heating furnace at 230° C. for 20 minutes to prepare a polyimide-coated substrate with a thickness of 100 nm.

[0201] Two polyimide-coated substrates were prepared by the above method, and 4 μm bead spacers were sprayed on the liquid crystal alignment film surface of one substrate, and then a thermosetting sealant (XN-1500T manufactured by Kyoritsu Chemical Co., Ltd.) was printed on top of the bead spacers. Next, the other substrate was attached to the previous substrate with the side on which the liquid crystal alignment film was formed facing inward, and the sealant was cured to prepare an empty cell. PSA polymerizable compound-containing liquid crystal MLC-3023 (Merck product name) was injected into this empty cell by the reduced pressure injection method to prepare a liquid crystal cell. The voltage retention rate of this liquid crystal cell was measured.

[0202] Next, with a DC voltage of 15 V applied to the liquid crystal cell, UV was irradiated from the outside of the liquid crystal cell at 10 J / cm through a 325 nm cut filter. 2 The UV illuminance was measured using a UV-MO3A manufactured by ORC.

[0203] Thereafter, in order to inactivate the unreacted polymerizable compound remaining in the liquid crystal cell, the cell was irradiated with UV (UV lamp: FLR40SUV32 / A-1) for 30 minutes without applying voltage using a UV-FL irradiation device manufactured by Toshiba Lighting & Technology Corp. (referred to as secondary PSA treatment). Then, the voltage retention rate was measured.

[0204] <Evaluation of voltage holding ratio> Using the liquid crystal cell prepared above, a voltage of 1V was applied for 60μs in a hot air circulating oven at 60℃, and the voltage was measured 1667msec later, and the voltage retention rate was calculated to determine how long the voltage was retained. A VHR-1 manufactured by Toyo Corporation was used to measure the voltage retention rate.

[0205] <Evaluation of high temperature and humidity resistance> The liquid crystal cell prepared above was left to stand for 7 days in a thermohygrostat (PR-2KP manufactured by Espec Corp.) at a temperature of 85°C and a humidity of 85%, after which the voltage holding ratio was measured. The difference between the voltage holding ratio measured here and the voltage holding ratio after the secondary PSA treatment was taken as the amount of change in VHR.

[0206] [Table 3]

[0207] As shown in Table 3, in Comparative Example 1, by placing the liquid crystal cell under high temperature and high humidity, the VHR change amount changed significantly by 59%, whereas in Examples 1 to 5, it was confirmed that the VHR change amount could be reduced to a small amount of 40% or less.

[0208] From the above, it can be said that the liquid crystal alignment film formed using the liquid crystal alignment agents [1] to [5] of Examples 1 to 5, and the liquid crystal display element obtained by using the liquid crystal alignment film, can maintain a high voltage retention rate for a long period of time even when used under high temperature and high humidity conditions, for example, in car navigation systems and meters installed in vehicles, and display units of industrial equipment and measuring instruments installed outdoors.

[0209] Of course, the liquid crystal alignment film formed using the liquid crystal alignment agents [1] to [5] of Examples 1 to 5 and the liquid crystal display element obtained using the liquid crystal alignment film can ensure a high voltage retention rate for a long period of time even when not under high temperature and high humidity conditions. As described above, the liquid crystal alignment film formed using the liquid crystal alignment agents [1] to [5] of Examples 1 to 5 and the liquid crystal display element obtained using the liquid crystal alignment film have a higher initial voltage retention rate than those of the comparative example, that is, it is found that high driving reliability can be ensured. [Industrial Applicability]

[0210] The present invention provides a liquid crystal alignment agent capable of obtaining a liquid crystal alignment film that can maintain a high voltage retention rate for a long period of time even under high temperature and high humidity conditions, the liquid crystal alignment film, a liquid crystal display element using the same, and a method for manufacturing the liquid crystal display element. The liquid crystal display element can be used in personal computers, mobile phones, smartphones, televisions, car navigation systems installed in vehicles, and display units of industrial equipment and measuring instruments installed outdoors, etc.

Claims

1. Diamines represented by the following formulas [W-A1], [W-A2], or [W-A3]. 【Chemistry 1】

2. A diamine component containing at least one selected from the group consisting of diamines represented by the formulas [W-A1], [W-A2] and [W-A3] according to claim 1, and at least one polymer selected from the group consisting of polyimide precursors and polyimides obtained from a tetracarboxylic acid component.

3. A diamine component containing at least one selected from the group consisting of diamines represented by the formulae [W-A1], [W-A2] and [W-A3] according to claim 1 and diamine (v) having at least one side chain structure selected from the group consisting of diamines represented by the formulae (S1), (S2) and (S3), and at least one polymer selected from the group consisting of polyimide precursors and polyimides obtained from a tetracarboxylic acid component. 【Chemistry 2】 X 1 and X 2 are each independently a single bond, -(CH 2 ) a -(a is an integer of 1 to 15), -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -COO-, -OCO- or -((CH 2 ) a1 -A 1 ) m1 In this case, each of the multiple a1's is independently an integer of 1 to 15, and the multiple A's are each independently an integer of 1 to 15. 1 each independently represents an oxygen atom or -COO-; m 1 is 1 to 2. 1 and G 2 each independently represents a divalent cyclic group selected from a divalent aromatic group having 6 to 12 carbon atoms and a divalent alicyclic group having 3 to 8 carbon atoms. Any hydrogen atom on the cyclic group may be substituted with at least one selected from the group consisting of an alkyl group having 1 to 3 carbon atoms, an alkoxyl group having 1 to 3 carbon atoms, a fluorine-containing alkyl group having 1 to 3 carbon atoms, a fluorine-containing alkoxyl group having 1 to 3 carbon atoms, and a fluorine atom. m and n each independently represent an integer of 0 to 3, and the sum of m and n is 1 to 4. R 1 represents an alkyl group having 1 to 20 carbon atoms, an alkoxy group having 1 to 20 carbon atoms, or an alkoxyalkyl group having 2 to 20 carbon atoms; R 1 Any hydrogen in the formula may be replaced by fluorine. 【Chemistry 3】 X 3 is a single bond, -CONH-, -NHCO-, -CON(CH 3 )-, -NH-, -O-, -CH 2 represents -O-, -COO- or -OCO-. 2 represents an alkyl group having 1 to 20 carbon atoms or an alkoxyalkyl group having 2 to 20 carbon atoms; R 2 Any hydrogen in the formula may be replaced by fluorine. 【Chemistry 4】 X 4 represents -CONH-, -NHCO-, -O-, -COO- or -OCO-. 3 represents a structure having a steroid skeleton.

Citation Information

Patent Citations

  • Liquid crystal display device

    JP2003307720A

  • pyridinonyl pdk1 inhibitor

    JP2009542684A

  • JPP7401853B

  • Imaging gastrointestinal volumes and motility

    WO2011005609A2

  • Liquid crystal alignment agent, liquid crystal alignment film, and liquid crystal display device

    WO2018062353A1